Positive electrode active material for magnesium secondary battery and magnesium secondary battery
By integrating magnesium, transition metals, and oxyborate anions into the positive electrode active material, the charge and discharge capacity of magnesium secondary batteries is enhanced, addressing the diffusion challenges faced by existing technologies.
Patent Information
- Application Number
- JP2020084734
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-05-13
AI Technical Summary
Existing magnesium secondary batteries face challenges with low charge and discharge capacity due to the strong interaction between magnesium ions and oxygen, making it difficult for magnesium ions to diffuse within the positive electrode active materials, particularly those using transition metal oxides.
Incorporating magnesium, transition metals, and oxyborate anions into the positive electrode active material, such as compounds like Mg x Fe y B.O. 4 or Mg x Mn y B.O. 5, which are synthesized through mixing and firing processes, to facilitate magnesium ion diffusion and reduce interfacial resistance.
The proposed active material enhances charge and discharge capacity by allowing easier movement of magnesium ions, resulting in improved charging and discharging efficiency.
Smart Images

Figure 0007595289000002 
Figure 0007595289000003 
Figure 0007595289000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode active material for a magnesium secondary battery and a magnesium secondary battery. [Background technology]
[0002] In recent years, research into magnesium secondary batteries has been attracting attention.
[0003] Patent Document 1 describes a positive electrode active material having a coating layer formed so as to cover the surface of the positive electrode active material and having a polyanion structure part exhibiting acidity. Patent Document 1 describes an all-solid-state battery having a positive electrode active material layer containing this positive electrode active material. An example of the all-solid-state battery is an all-solid-state magnesium battery. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-99323 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present disclosure provides a positive electrode active material for a magnesium secondary battery that can improve charge / discharge capacity, and a magnesium secondary battery using the same. [Means for solving the problem]
[0006] The present disclosure relates to containing magnesium, a transition metal, and an oxyborate anion; A positive electrode active material for a magnesium secondary battery is provided. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a positive electrode active material for a magnesium secondary battery capable of improving charge / discharge capacity, and a magnesium secondary battery using the same. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a diagram showing the results of powder X-ray diffraction measurement of the positive electrode active material according to Example 1, and a diagram showing the results of powder X-ray diffraction of MgFeBO4 and Fe2O3 obtained by simulation. [Diagram 2] FIG. 2 is a diagram showing the results of powder X-ray diffraction measurement of the positive electrode active material according to Example 2 and a diagram showing the results of powder X-ray diffraction of Mg1.71Mn1.29BO5 obtained by simulation. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a schematic configuration example of a magnesium secondary battery. [Figure 4] FIG. 4 is a schematic diagram showing a schematic configuration of a battery for charge / discharge evaluation according to the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Knowledge that formed the basis of this disclosure> The process by which the positive electrode active material of the present disclosure was obtained will be described below.
[0010] Currently, lithium secondary batteries are widely used as secondary batteries. In recent years, electric vehicles (EVs) have rapidly spread, and secondary batteries with a larger capacity than lithium secondary batteries have been actively researched. Magnesium secondary batteries are expected to be high-capacity secondary batteries because they can utilize the two-electron reaction of magnesium.
[0011] As a positive electrode active material for a magnesium secondary battery, the use of transition metal oxides such as vanadium oxide is considered. However, since the interaction between magnesium ions and oxygen is strong, it has been found that in the positive electrode active material using vanadium oxide, the activation barrier for the diffusion of magnesium ions is large. That is, it is difficult for magnesium ions to move within the active material, and the electrode reaction in the active material hardly proceeds. As a result, a magnesium secondary battery using a transition metal oxide as a positive electrode active material is difficult to charge and discharge.
[0012] On the other hand, Patent Document 1 describes, for example, a positive electrode active material in which a positive electrode active material is coated with a polyanion structure portion having an oxyborate anion. Since the surface of the positive electrode active material is coated with a coating layer including the polyanion structure portion, an increase over time in the interfacial resistance between the positive electrode active material and the solid electrolyte material can be suppressed. However, Patent Document 1 does not disclose using a polyanion having an oxyborate anion as a positive electrode active material.
[0013] As a result of intensive studies, the inventors have newly found that a positive electrode active material containing an oxyborate anion enables the occlusion and release of magnesium. Based on this new finding, the inventors have completed the present disclosure.
[0014] <Summary of one aspect according to the present disclosure> The positive electrode active material for a magnesium secondary battery according to the first aspect of the present disclosure is composed of magnesium, a transition metal, and an oxyborate anion.
[0015] According to the first aspect, a magnesium secondary battery capable of improving the charge and discharge capacity can be provided.
[0016] In the second aspect of the present disclosure, for example, the positive electrode active material for a magnesium secondary battery according to the first aspect may contain a compound represented by the composition formula of Mg x Fe y BO4, and the condition of 0 < x + y ≦ 2 may be satisfied.
[0017] In a third aspect of the present disclosure, for example, the positive electrode active material for a magnesium secondary battery according to the first aspect contains Mg x Mn y and may contain a compound represented by the composition formula of BO5, and the condition of 0 < x + y ≦ 3 may be satisfied.
[0018] According to the second and third aspects, a magnesium secondary battery capable of further improving the charge and discharge capacity can be provided.
[0019] The magnesium secondary battery according to a fourth aspect of the present disclosure includes a positive electrode, a negative electrode, and an electrolyte having magnesium ion conductivity. The positive electrode contains a positive electrode active material for a magnesium secondary battery according to any one of the first to third aspects.
[0020] According to the fourth aspect, a magnesium secondary battery capable of improving the charge and discharge capacity can be provided.
[0021] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the following embodiments are merely examples, and the present disclosure is not limited to the following forms.
[0022] [Embodiment 1] In Embodiment 1, an embodiment of the positive electrode active material for a magnesium secondary battery of the present disclosure will be described.
[0023] The positive electrode active material for a magnesium secondary battery of the present embodiment contains magnesium, a transition metal, and an oxyborate anion. Thereby, a magnesium secondary battery capable of improving the charge and discharge capacity can be provided. In the present disclosure, a compound containing magnesium, a transition metal, and an oxyborate anion is referred to as an oxyborate material.
[0024] In the positive electrode active material for a magnesium secondary battery, the molar ratio of magnesium, a transition metal, and an oxyborate anion is not limited to a specific value. By appropriately adjusting the molar ratio of magnesium, a transition metal, and an oxyborate anion, a magnesium secondary battery capable of further improving charge and discharge efficiency can be provided.
[0025] That the positive electrode active material for a magnesium secondary battery of the present embodiment contains an oxyborate anion can be confirmed, for example, by powder X-ray diffraction (XRD) measurement. The molar ratio of magnesium, a transition metal, and boron in the oxyborate material of the present embodiment can be confirmed, for example, by inductively coupled plasma (ICP) emission spectrometry.
[0026] The crystal structure of the positive electrode active material for a magnesium secondary battery is not limited to a specific crystal structure. The crystal structure of the positive electrode active material for a magnesium secondary battery may be, for example, a crystal structure in which the crystal structure is not easily collapsed even when magnesium is extracted from the positive electrode active material and the crystal structure can be stably maintained. Thereby, the charge and discharge efficiency of the magnesium secondary battery can be surely improved.
[0027] The positive electrode active material for a magnesium secondary battery contains, for example, a transition metal. Examples of the transition metal are Fe and Mn.
[0028] The positive electrode active material for a magnesium secondary battery may contain Mg, Fe, and an oxyborate anion. The positive electrode active material for a magnesium secondary battery may contain a compound represented by the following compositional formula (1). The positive electrode active material for a magnesium secondary battery may be a compound represented by the following compositional formula (1).
[0029] Mg x Fe y BO4···(1)
[0030] In the compositional formula (1), x + y satisfies the condition of 0 < x + y ≤ 2.
[0031] According to the above configuration, a magnesium secondary battery capable of further improving the charge and discharge efficiency can be provided.
[0032] The positive electrode active material for a magnesium secondary battery may contain Mg, Mn, and an oxyborate anion. The positive electrode active material for a magnesium secondary battery may contain a compound represented by the following compositional formula (2). The positive electrode active material for a magnesium secondary battery may be a compound represented by the following compositional formula (2).
[0033] Mg x Mn y BO5···(2)
[0034] In the compositional formula (2), x + y satisfies the condition of 0 < x + y ≤ 3.
[0035] According to the above configuration, a magnesium secondary battery capable of further improving the charge and discharge efficiency can be provided.
[0036] In the compositional formulas (1) and (2), the composition ratio of each atom can be confirmed by, for example, powder X-ray diffraction measurement and / or ICP emission spectrometry.
[0037] Next, a method for manufacturing the positive electrode active material for a magnesium secondary battery in the present embodiment will be described.
[0038] The positive electrode active material for a magnesium secondary battery in the present embodiment can be manufactured, for example, by mixing a boron-containing material, a magnesium-containing material, and a transition metal-containing material and firing them in an active atmosphere or an inert atmosphere.
[0039] In the production of the positive electrode active material for magnesium secondary batteries, the firing temperature is, for example, 800° C. or more and 1500° C. or less. The production of the positive electrode active material for magnesium secondary batteries may be carried out in the air, in an active atmosphere, or in an inert atmosphere. In the production of the positive electrode active material for magnesium secondary batteries, when a sufficient amount of oxygen is contained in the raw material, an inert gas such as nitrogen, argon, helium, or neon may be used.
[0040] Examples of boron-containing materials are boron, boric acid, calcium boride, magnesium borate, and diborides. Examples of diborides are aluminum diboride and magnesium diboride.
[0041] Examples of magnesium-containing materials are magnesium metal, magnesium oxide, magnesium hydride, magnesium hydroxide, magnesium borate, and magnesium diboride.
[0042] Examples of materials containing transition metals are transition metals, transition metal compounds, transition metal oxides, transition metal hydroxides, and transition metal borates.
[0043] The amount of each ingredient is adjusted according to the desired composition of the oxyborate material. The composition of the oxyborate material can also be adjusted by the conditions of the heat treatment and / or the conditions of the retreatment after the heat treatment. An example of the conditions of the retreatment after the heat treatment is washing with an acid and a second heat treatment.
[0044] [Embodiment 2] An embodiment of the battery of the present disclosure will be described in embodiment 2. Note that descriptions that overlap with embodiment 1 above will be omitted as appropriate.
[0045] The positive electrode active material for magnesium secondary batteries according to this embodiment can be used in magnesium secondary batteries. The magnesium secondary battery includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode includes the positive electrode active material for magnesium secondary batteries described in embodiment 1. The electrolyte has magnesium ion conductivity.
[0046] FIG. 3 is a cross-sectional view illustrating a schematic configuration example of the magnesium secondary battery 10. As shown in FIG.
[0047] The magnesium secondary battery 10 includes a positive electrode 21, a negative electrode 22, a separator 14, a case 11, a sealing plate 15, and a gasket 18. The separator 14 is disposed between the positive electrode 21 and the negative electrode 22. The positive electrode 21, the negative electrode 22, and the separator 14 are impregnated with a non-aqueous electrolyte, and are housed in the case 11. The case 11 is closed by the gasket 18 and the sealing plate 15.
[0048] The case 11 houses the positive electrode 21, the negative electrode 22, and the separator 14. The shape and material of the case 11 are not limited to a specific embodiment. The case 11 is not limited to the one shown in FIG. 3, and any known battery case can be appropriately selected and used.
[0049] The magnesium secondary battery 10 may have a cylindrical, rectangular, button, coin, or flat structure.
[0050] The positive electrode 21 includes a positive electrode current collector 12 and a positive electrode active material layer 13 disposed on the positive electrode current collector 12. The positive electrode active material layer 13 is disposed between the positive electrode current collector 12 and a separator 14.
[0051] The positive electrode active material layer 13 contains the positive electrode active material described in embodiment 1. With such a configuration, it is possible to provide a positive electrode for a magnesium secondary battery that can improve the charge / discharge capacity.
[0052] The positive electrode active material layer 13 may further contain a conductive assistant, an ion conductor and / or a binder, if necessary.
[0053] Examples of the conductive assistant are carbon materials, metals, inorganic compounds, and conductive polymers. Examples of the carbon materials are graphite, acetylene black, carbon black, graphite, carbon nanotubes, carbon nanofibers, graphene, fullerene, ketjen black, carbon whiskers, needle coke, and carbon fibers. Examples of the graphite are natural graphite and artificial graphite. Examples of the natural graphite are lump graphite and flake graphite. Examples of the metal are copper, nickel, aluminum, silver, and gold. Examples of the inorganic compounds are tungsten carbide, titanium carbide, tantalum carbide, molybdenum carbide, titanium boride, and titanium nitride. Examples of the conductive polymer are polyaniline, polypyrrole, and polythiophene. These materials may be used alone or in a mixture of two or more kinds.
[0054] Examples of ion conductors are gel electrolytes, organic solid electrolytes, and inorganic solid electrolytes. Examples of gel electrolytes are polymethyl methacrylate and polymethyl methacrylate. Examples of organic solid electrolytes are polyethylene oxide. Examples of inorganic solid electrolytes are MgSc2Se4.
[0055] The binder is used to improve the binding of the materials constituting the electrode. Examples of the binder include polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, polytetrafluoroethylene, carboxymethyl cellulose, polyacrylic acid, styrene-butadiene copolymer rubber, polypropylene, polyethylene, and polyimide.
[0056] The positive electrode active material layer 13 is formed, for example, by the following method. First, the positive electrode active material, the conductive additive, and the binder are mixed to obtain a mixture of these materials. Next, an appropriate solvent is added to this mixture to obtain a paste-like positive electrode mixture. Next, this positive electrode mixture is applied to the surface of the positive electrode current collector 12 and dried. In this way, the positive electrode active material layer 13 is formed on the positive electrode current collector 12. The positive electrode active material layer 13 may be compressed to increase the electrode density.
[0057] The thickness of the positive electrode active material layer 13 is not limited to a specific value and is, for example, 1 μm or more and 100 μm or less.
[0058] The material of the positive electrode current collector 12 is, for example, a simple metal or an alloy. More specifically, the material of the positive electrode current collector 12 may be a simple metal or an alloy containing at least one material selected from the group consisting of copper, chromium, nickel, titanium, platinum, gold, aluminum, tungsten, iron, and molybdenum. The material of the positive electrode current collector 12 may be stainless steel.
[0059] The positive electrode collector 12 may be a porous sheet or a non-porous sheet. The positive electrode collector 12 may be a porous film or a non-porous film. Metal foils and meshes may be used as the sheet or film. A conductive auxiliary material may be applied to the surface of the positive electrode collector 12 from the viewpoint of reducing the resistance value of the secondary battery, imparting a catalytic effect, or improving the bonding strength between the positive electrode active material layer 13 and the positive electrode collector 12. An example of the conductive auxiliary material is a carbon material such as carbon.
[0060] The positive electrode current collector 12 may be in the form of a plate or foil. The positive electrode current collector 12 may be a laminated film.
[0061] When the case 11 also serves as a positive electrode current collector, the positive electrode current collector 12 may be omitted.
[0062] The negative electrode 22 includes, for example, a negative electrode active material layer 17 containing a negative electrode active material, and a negative electrode current collector 16. The negative electrode active material layer 17 is disposed between the negative electrode current collector 16 and the separator .
[0063] The negative electrode active material layer 17 contains a negative electrode active material capable of absorbing and releasing magnesium ions. An example of the negative electrode active material is a carbon material. Examples of the carbon material are graphite, non-graphitic carbon, and graphite intercalation compounds. Examples of the non-graphitic carbon are hard carbon and coke.
[0064] The negative electrode active material layer 17 may further contain a conductive assistant, an ion conductor, and / or a binder as necessary. For the conductive assistant, the ion conductor, and the binder, for example, the conductive assistant, the ion conductor, and the binder described in relation to the positive electrode can be appropriately used.
[0065] The thickness of the negative electrode active material layer 17 is not limited to a specific value and is, for example, 1 μm or more and 50 μm or less.
[0066] The negative electrode active material layer 17 may contain a negative electrode active material capable of precipitating and dissolving magnesium. In this case, examples of the negative electrode active material include metallic magnesium and magnesium alloys. The magnesium alloy is, for example, an alloy of magnesium and at least one metal selected from the group consisting of aluminum, silicon, gallium, zinc, tin, manganese, bismuth, and antimony.
[0067] The material of the negative electrode current collector 16 may be, for example, the same material as that of the positive electrode current collector 12 described in the description of the positive electrode. The negative electrode current collector 16 may be in the form of a plate or foil.
[0068] When the sealing plate 15 also serves as the negative electrode current collector, the negative electrode current collector 16 may be omitted.
[0069] When the negative electrode current collector 16 is made of a material capable of depositing and dissolving magnesium on its surface, the negative electrode active material layer 17 may be omitted. That is, the negative electrode 22 may be made of only the negative electrode current collector 16 capable of depositing and dissolving magnesium. In this case, the negative electrode current collector 16 may be stainless steel, nickel, copper, or iron.
[0070] Examples of the material of the separator 14 include a microporous thin film, a woven fabric, and a nonwoven fabric. The material of the separator 14 may be a polyolefin such as polypropylene and polyethylene. The thickness of the separator 14 is, for example, 10 μm or more and 300 μm or less. The separator 14 may be a single-layer film made of one type of material, or a composite film or a multi-layer film made of two or more types of materials. The porosity of the separator 14 is, for example, 30% or more and 70% or less.
[0071] The electrolyte can be a material that has magnesium ion conductivity.
[0072] The electrolyte is, for example, a non-aqueous electrolyte solution that contains a non-aqueous solvent and a magnesium salt dissolved in the non-aqueous solvent.
[0073] Examples of magnesium salts are MgBr2, MgI2, MgCl2, Mg(AsF6)2, Mg(ClO4)2, Mg(PF6)2, Mg(BF4)2, Mg(CF3SO3)2, Mg[N(CF3SO2)2]2, Mg(SbF6)2, Mg(SiF6)2, Mg[C(CF3SO2)3]2, Mg[N(FSO2)2]2, Mg[N(C2F5SO2)2]2, MgB 10 Cl 10 , MgB 12 Cl 12 , Mg[B(C6F5)4]2, Mg[B(C6H5)4]2, Mg[N(SO2CF2CF3)2]2, Mg[BF3C2F5]2, Mg[PF3(CF2CF3)3]2, and Mg[B(OCH(CF3)2)4]2. As the magnesium salt, only one of the above substances may be used, or two or more of them may be used in combination.
[0074] The non-aqueous solvent may be any non-aqueous solvent generally used in secondary batteries, including cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, pyrocarbonates, phosphates, borates, sulfates, sulfites, cyclic sulfones, chain sulfones, nitriles, sultones, cyclic ethers, chain ethers, nitriles, and amides.
[0075] Examples of cyclic carbonates are ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, 4,5-difluoroethylene carbonate, 4,4,4-trifluoroethylene carbonate, fluoromethylethylene carbonate, trifluoromethylethylene carbonate, 4-fluoropropylene carbonate, and 5-fluoropropylene carbonate. As cyclic carbonates, it is also possible to use compounds in which some or all of the hydrogen groups of the above compounds are fluorinated. Examples of fluorinated compounds are trifluoropropylene carbonate and fluoroethyl carbonate.
[0076] Examples of the chain carbonate esters are dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate. As the chain carbonate esters, it is also possible to use compounds in which some or all of the hydrogen groups of the above compounds are fluorinated.
[0077] Examples of cyclic carboxylic acid esters are γ-butyrolactone, γ-valerolactone, γ-caprolactone, ε-caprolactone, α-acetolactone, and derivatives thereof.
[0078] Examples of the chain carboxylic acid ester include methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, and derivatives thereof.
[0079] Examples of pyrocarbonates are diethylpyrocarbonate, dimethylpyrocarbonate, di-tert-butyldicarbonate, and derivatives thereof.
[0080] Examples of phosphate esters are trimethyl phosphate, triethyl phosphate, hexamethylphosphoramide, and derivatives thereof.
[0081] Examples of borate esters are trimethylborate, triethylborate, and derivatives thereof.
[0082] Examples of sulfate esters are trimethyl sulfate, triethyl sulfate, and derivatives thereof.
[0083] Examples of sulfites are ethylene sulfite and its derivatives.
[0084] An example of a cyclic sulfone is sulfolane and its derivatives. An example of a linear sulfone is alkylsulfone and its derivatives. An example of a nitrile is acetonitrile, valeronitrile, propionitrile, trimethylacetonitrile, cyclopentanecarbonitrile, adiponitrile, pimelonitrile, and its derivatives. An example of a sultone is 1,3-propane sultone and its derivatives.
[0085] Examples of cyclic ethers are 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, and crown ethers.
[0086] Examples of the chain ethers are 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl.
[0087] An example of an amide is dimethylformamide.
[0088] The non-aqueous solvent may contain a glyme. The glyme may be bidentate with respect to the magnesium ion. The use of a glyme can improve the solubility of the magnesium imide salt in the non-aqueous solvent. Examples of glymes are 1,2-dimethoxyethane (DME), diglyme, triglyme, and tetraglyme.
[0089] As the solvent, only one of the above substances may be used, or two or more of them may be used in combination. EXAMPLES
[0090] The present disclosure will be described in more detail below with reference to examples. Note that the following examples are merely illustrative and the present disclosure is not limited to the following examples.
[0091] Example 1 [Preparation of oxyborate materials] Iron oxide (II), magnesium oxide powder in an amount of 28.1% by mass relative to iron oxide (II), and boric acid in an amount of 43.0% by mass relative to iron oxide (II) were weighed and placed in an agate mortar, and were pulverized and mixed using the agate mortar to obtain a mixture. The obtained mixture was heated in a firing furnace in the atmosphere at a rate of 5°C per minute from room temperature (25°C) until it reached 1300°C, and was further fired at 1300°C for 3 hours. After that, the heating was stopped, and the mixture was allowed to cool naturally. The obtained mixture was pulverized in the agate mortar to obtain an oxyboric acid material, which is a positive electrode active material according to Example 1.
[0092] [Preparation of positive electrode] The oxyborate material according to Example 1, acetylene black as a conductive assistant, and polytetrafluoroethylene (PTFE) as a binder were weighed in a mass ratio of 8:1:1, and these were thoroughly mixed using an agate mortar to obtain a positive electrode mixture according to Example 1. The positive electrode mixture was rolled using a roll press machine to obtain a positive electrode mixture sheet according to Example 1. The obtained positive electrode mixture sheet was punched into a rectangle of 5 mm x 5 mm. The punched positive electrode mixture sheet was placed on the tip of a mesh of 5 mm x 30 mm and pressure-bonded. The mesh was made of platinum. In this manner, a positive electrode according to Example 1 was produced.
[0093] [Preparation of evaluation cell] FIG. 4 is a schematic diagram showing a schematic configuration of an evaluation cell according to an embodiment.
[0094] The evaluation cell 30 includes a positive electrode 31, a reference electrode 34, a negative electrode 35, and a non-aqueous electrolyte 36. The non-aqueous electrolyte 36 is stored in a glass beaker 37. The glass beaker 37 is surrounded by an aluminum block 38. The positive electrode 31 includes a mesh 32 and a positive electrode mixture 33. The positive electrode mixture 33 is disposed at the tip of the mesh 32. The positive electrode 31, the reference electrode 34, and the negative electrode 35 are immersed in the non-aqueous electrolyte 36.
[0095] The magnesium ribbon was cut into pieces of 5 mm x 40 mm to obtain magnesium foils. The surface of the magnesium foil was scraped to remove the oxide film, and the surface was washed with hexane. In this way, the reference electrode 34 and the negative electrode 35 were produced.
[0096] 2.5 mL of nonaqueous electrolyte 36 was stored in a glass beaker 37. For the nonaqueous electrolyte 36, 1,2-dimethoxyethane (DME) was used as the nonaqueous solvent. Nonaqueous electrolyte 36 was prepared by dissolving Mg[B(OCH(CF3)2)4]2·3DME, an organoboron ate complex salt in which DME is coordinated, in DME at a concentration of 0.3 mol / L.
[0097] A positive electrode 31, a reference electrode 34, and a negative electrode 35 were immersed in a nonaqueous electrolyte 36 to prepare an evaluation cell 30 having the configuration shown in Fig. 4. The preparation of the electrolyte and the preparation of the evaluation cell were carried out in a glove box in an Ar atmosphere with a dew point of -60°C or less and a volumetric oxygen concentration of 5 ppm or less.
[0098] Example 2 [Preparation of oxyborate materials] An oxyboric acid material, which is the positive electrode active material of Example 2, was obtained in the same manner as in Example 1, except that manganese oxide (II), magnesium oxide powder in an amount of 56.8% by mass relative to manganese oxide (II), and boric acid in an amount of 58.1% by mass relative to manganese oxide (II), were weighed and placed in an agate mortar.
[0099] [Preparation of positive electrode] A positive electrode according to Example 2 was produced in the same manner as in Example 1, except that the oxyboric acid material according to Example 2 was used and an aluminum mesh was used instead of the platinum mesh.
[0100] [Preparation of evaluation cell] An evaluation cell according to Example 2 was produced in the same manner as in Example 1, except that the positive electrode according to Example 2 was used.
[0101] Comparative Example 1 [Preparation of vanadium oxide positive electrode] Vanadium oxide (VO) was used as the active material of Comparative Example 1. A positive electrode according to Comparative Example 1 was obtained in the same manner as in Example 2, except that vanadium oxide, acetylene black as a conductive assistant, and polytetrafluoroethylene (PTFE) as a binder were weighed in a mass ratio of 8:1:1.
[0102] [Preparation of evaluation cell] An evaluation cell according to Comparative Example 1 was produced in the same manner as in Example 2, except that the positive electrode according to Comparative Example 1 was used.
[0103] [Charge / discharge test] Charge / discharge tests were carried out on the evaluation cells according to Examples 1 and 2 and Comparative Example 1 under the following conditions to evaluate the charge / discharge characteristics.
[0104] First, the evaluation cell was placed on a hot plate at 60°C.
[0105] The theoretical capacity of MgFeBO4 was assumed to be 346mAh / g. The evaluation cell according to Example 1 was charged at a constant current with a current value corresponding to a 0.01C rate for this theoretical capacity. At this time, the constant current per unit weight of 1g of the positive electrode active material was 3.46mAh / g. When the charge capacity reached 50% of the theoretical capacity, the charge was terminated. The evaluation cell was then left to stand for 5 hours.
[0106] Next, the evaluation cell was discharged at a current value of 0.01 C rate. When the discharge capacity and the charge capacity became equal, the discharge was terminated. Thus, the charge capacity and the discharge capacity of the evaluation cell according to Example 1 were measured. The results are shown in Table 1.
[0107] Mg 1.5 Mn 1.5 Except for assuming that the theoretical capacity of BO5 was 257 mAh / g, the evaluation cell according to Example 2 was charged and discharged, and the charge capacity and discharge capacity were measured in the same manner as in Example 1. The results are shown in Table 1.
[0108] In the charge-discharge test of the evaluation cell according to Comparative Example 1, it was assumed that one molecule of Mg was absorbed per one molecule of vanadium oxide. Therefore, the theoretical capacity of MgV2O5 was assumed to be 295mAh / g. The evaluation cell according to Comparative Example 1 was discharged at a constant current at a current value that was 0.01C rate for this theoretical capacity. At this time, the constant current per unit weight of 1g of the positive electrode active material was 2.95mAh / g. When the potential of the positive electrode relative to the reference electrode reached 1V, the discharge was terminated. The evaluation cell was then left to stand for 5 hours.
[0109] Next, the evaluation cell according to Comparative Example 1 was charged until the potential of the positive electrode relative to the reference electrode reached 3 V. Thereby, the charge capacity and discharge capacity of the evaluation cell according to Comparative Example 1 were measured. The results are shown in Table 1.
[0110] [Table 1]
[0111] [Consideration] FIG. 1 is a diagram showing the results of powder X-ray diffraction measurement of the positive electrode active material according to Example 1. FIG. 1 also shows the results of powder X-ray diffraction of MgFeBO4 and Fe2O3 obtained by simulation. The powder X-ray diffraction pattern of MgFeBO4 was obtained using data of No. 251952 of the International Crystal Structure Database (ICSD). The powder X-ray diffraction pattern of Fe2O3 was obtained using data of No. 15840 of the ICSD. As shown in FIG. 1, the powder X-ray diffraction pattern of the oxyborate material according to Example 1 closely matched the powder X-ray diffraction pattern of MgFeBO4, which is an oxyborate material in the main phase, although it contained a small amount of Fe2O3 as an impurity.
[0112] FIG. 2 is a diagram showing the results of powder X-ray diffraction measurement of the positive electrode active material according to Example 2. 1.71 Mn 1.29 The powder X-ray diffraction results for BO5 are also shown. 1.71 Mn 1.29The powder X-ray diffraction pattern of BO5 was used with the data of No. 62366 in ICSD. As shown in Fig. 2, the powder X-ray diffraction pattern of the oxyboric acid material according to Example 2 is Mg 1.71 Mn 1.29 which well matched the powder X-ray diffraction pattern of BO5. However, since the powder X-ray diffraction pattern of the oxyboric acid material according to Example 2 was complex, the composition of the oxyboric acid material according to Example 2 was determined by ICP emission spectrometry. As a result, the composition of the oxyboric acid material according to Example 2 was Mg 1.28 Mn 1.61 BO5.
[0113] Table 1 shows the charge capacities and discharge capacities of the evaluation cells according to Example 1, Example 2, and Comparative Example 1. The oxyboric acid materials according to Example 1 and Example 2 showed higher charge capacities and higher discharge capacities than vanadium oxide according to Comparative Example 1. In the oxyboric acid materials according to Example 1 and Example 2, the anion coordinating with magnesium is oxyborate anion rather than oxygen. Thus, in the oxyboric acid materials according to Example 1 and Example 2, it is considered that the interaction between magnesium and oxygen is reduced, and magnesium can easily move within the active material. According to the positive electrode active material for magnesium secondary battery of the present disclosure, since the interaction between magnesium and oxyborate anion is weaker than the interaction between magnesium and oxygen, the charge and discharge capacities can be improved.
[0114] The powder X-ray diffraction pattern of the oxyboric acid material according to Example 1 well matched No. 251952 in ICSD which is the powder X-ray diffraction pattern of MgFeBO4. In the crystal structure of MgFeBO4, Mg and Fe can share the same site. Therefore, according to Example 1, when the composition formula of the oxyboric acid material is defined as Mg x Fe y BO4, x + y can satisfy the condition of 0 < x + y ≤ 2.
[0115] The powder X-ray diffraction pattern of the oxyboric acid material according to Example 2 is Mg 1.71 Mn 1.29It was in good agreement with ICSD No. 62366, which is the powder X-ray diffraction pattern of BO5. Mg 1.71 Mn 1.29 In the crystal structure of BO5, Mg and Mn can share the same site. Therefore, according to Example 2, when the composition formula of the oxyboric acid material is defined as Mg x Mn y BO5, x + y can satisfy the condition of 0 < x + y ≤ 3.
Industrial Applicability
[0116] The positive electrode active material for a magnesium secondary battery of the present disclosure can be used in a magnesium secondary battery.
Explanation of Signs
[0117] 10 Magnesium secondary battery 11 Case 12 Positive electrode current collector 13 Positive electrode active material layer 14 Separator 15 Sealing plate 16 Negative electrode current collector 17 Negative electrode active material layer 18 Gasket 21 Positive electrode 22 Negative electrode 30 Evaluation cell 31 Positive electrode 32 Mesh 33 Positive electrode mixture 34 Reference electrode 35 Negative electrode 36 Non-aqueous electrolyte 37 Beaker 38 Aluminum block
Claims
1. comprising magnesium, a transition metal, and an oxyborate anion; the compound contains a compound represented by the composition formula Mg x Fe y BO 4 , and satisfies the condition 0<x+y≦2; the compound contains a compound represented by the composition formula Mg x Mn y BO 5 , and satisfies the condition 0<x+y≦3; Positive electrode active material for magnesium secondary batteries (excluding materials in which some of the silicon has been replaced with boron).
2. Mg x Fe y B.O. 4 2. The positive electrode active material for a magnesium secondary battery according to claim 1 , comprising a compound represented by the following composition formula:
3. Mg x Mn y B.O. 5 2. The positive electrode active material for a magnesium secondary battery according to claim 1, comprising a compound represented by the following composition formula:
4. A positive electrode and A negative electrode; and an electrolyte having magnesium ion conductivity; A magnesium secondary battery, wherein the positive electrode comprises the positive electrode active material for magnesium secondary batteries according to claim 1 .
Citation Information
Patent Citations
All-solid battery
JP2007258165A
Cathode active substance material, cathode active substance layer, all-solid battery, and method for producing cathode active substance material
JP2012099323A
Magnesium secondary battery with boron-doped olivine positive electrode
JP2016054078A
Magnesium compound, method for producing same, positive electrode active material, positive electrode, and magnesium ion secondary battery
WO2014017461A1