Positive electrode active material for secondary battery, and secondary battery
The use of a lithium transition metal composite oxide with a tailored particle size distribution in the positive electrode active material stabilizes the O2 crystal structure, enhancing battery capacity and reducing capacity loss during cycling.
Patent Information
- Application Number
- JP2021554303
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-29
- Filing Date
- 2020-10-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-10-13
AI Technical Summary
Lithium transition metal composite oxides with an O2 structure face issues of low capacity retention during charging and discharging cycles due to voltage drops and structural instability.
A positive electrode active material comprising a lithium transition metal composite oxide with a specific particle size distribution, having a first peak on the small particle size side and a second peak on the large particle size side, enhances packing density and contact area with the electrolyte, while maintaining a stable O2 crystal structure.
This configuration improves battery capacity and suppresses the decrease in capacity retention rate during charge/discharge cycles, ensuring higher performance and stability.
Smart Images

Figure 0007595308000002 
Figure 0007595308000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode active material for a secondary battery, and a secondary battery using the positive electrode active material. [Background technology]
[0002] Conventionally, lithium transition metal composite oxides have been widely used as positive electrode active materials for secondary batteries such as lithium ion batteries. For example, Patent Document 1 discloses a lithium transition metal composite oxide having a crystal structure defined by the O2 structure and containing Li in the transition metal layer. In addition, a lithium transition metal composite oxide having a crystal structure defined by the O3 structure and containing Li in the transition metal layer is also known. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-204281 A Summary of the Invention
[0004] Compared with lithium transition metal composite oxides with the O3 structure, lithium transition metal composite oxides with the O2 structure are capable of suppressing voltage drop during the charge-discharge cycle of a secondary battery, but they have problems such as low secondary battery capacity and low capacity retention rate during charge-discharge cycles.
[0005] The positive electrode active material for a secondary battery according to one embodiment of the present disclosure includes a lithium transition metal composite oxide, and the lithium transition metal composite oxide is represented by the general formula Li α [Li x Mn y Co z Me (1-x-y-z) ]O 2(In the formula, Me is at least one selected from Ni, Fe, Ti, Bi, and Nb, 0.5 < α < 1, 0.05 < x < 0.25, 0.4 < y < 0.7, 0 < z < 0.25), it has a crystal structure of the O2 structure, and the particle size distribution of the lithium transition metal composite oxide has a first peak on the small particle size side and a second peak on the large particle size side.)
[0006] A secondary battery according to one aspect of the present disclosure includes a positive electrode containing the above positive electrode active material, a negative electrode, and an electrolyte.)
[0007] According to the positive electrode active material for a secondary battery according to one aspect of the present disclosure, the capacity of the secondary battery can be improved, and a decrease in the capacity retention rate during charge and discharge cycles can be suppressed.)
Brief Description of the Drawings
[0008] [Figure 1] FIG. 1 is a cross-sectional view of a secondary battery which is an example of an embodiment.)
Modes for Carrying Out the Invention
[0009] The positive electrode active material for a secondary battery according to one aspect of the present disclosure contains a lithium transition metal composite oxide, and the lithium transition metal composite oxide has the general formula Li α [Li x Mn y Co z Me (1-x-y-z) O 2(In the formula, Me is at least one selected from Ni, Fe, Ti, Bi, and Nb, 0.5 < α < 1, 0.05 < x < 0.25, 0.4 < y < 0.7, 0 < z < 0.25), has a crystal structure of the O2 structure, and the particle size distribution of the lithium transition metal composite oxide has a first peak on the small particle size side and a second peak on the large particle size side. And according to the positive electrode active material for a secondary battery which is one aspect of the present disclosure, the capacity of the secondary battery can be improved, and a decrease in the capacity retention rate in the charge-discharge cycle can be suppressed. Although the mechanism for achieving this effect is not fully clear, the following can be considered. The lithium transition metal composite oxide of the present disclosure includes a first particle group corresponding to the first peak on the small particle size side and a second particle group corresponding to the second peak on the large particle size side in the particle size distribution. However, due to such a mixture of the first particle group with a small particle size and the second particle group with a large particle size, the packing density of the positive electrode active material is improved, and due to the presence of the first particle group with a small particle size, the contact area with the electrolyte increases, so it is presumed that the capacity of the secondary battery is improved. In addition, the lithium transition metal composite oxide represented by the above general formula and having an O2 structure has high stability of the crystal structure. Therefore, when charge and discharge are repeated, the crystal structure collapse is suppressed even in the first particle group with a small particle size having a large reaction area, so it is considered that a decrease in the capacity retention rate in the charge-discharge cycle is suppressed.)
[0010] Hereinafter, an example of a secondary battery which is one aspect of the present disclosure will be described.)
[0011] FIG. 1 is a cross-sectional view of a secondary battery as an example of an embodiment. The secondary battery 10 shown in FIG. 1 includes a wound electrode body 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, an electrolyte, insulating plates 18 and 19 respectively arranged above and below the electrode body 14, and a battery case 15 for accommodating the above-mentioned members. The battery case 15 is composed of a cylindrical case body 16 with a bottom and a sealing body 17 for closing an opening of the case body 16. Note that, instead of the wound electrode body 14, an electrode body of another form may be applied, such as a laminated electrode body formed by alternately stacking positive and negative electrodes with a separator interposed therebetween. In addition, examples of the battery case 15 include a metallic case having a cylindrical shape, a square shape, a coin shape, a button shape, etc., and a resin case formed by laminating a resin sheet (so-called laminate type).
[0012] The electrolyte may be an aqueous electrolyte, but is preferably a non-aqueous electrolyte containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted product in which at least a portion of the hydrogen of these solvents is replaced with a halogen atom such as fluorine. Examples of the electrolyte salt include LiPF 6 The electrolyte is not limited to a liquid electrolyte, and may be a solid electrolyte using a gel polymer or the like.
[0013] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has a protruding portion 22 that supports the sealing body 17, for example, a part of the side surface of the case body 16 protruding inward. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.
[0014] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are laminated in this order from the electrode body 14 side. Each member constituting the sealing body 17 has, for example, a disk shape or a ring shape, and each member except the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between each of their peripheral edges. When the internal pressure of the secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 deforms and breaks so as to push the upper valve body 26 toward the cap 27, and the current path between the lower valve body 24 and the upper valve body 26 is interrupted. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0015] In the secondary battery 10 shown in Fig. 1, a positive electrode lead 20 attached to the positive electrode 11 passes through a through hole in an insulating plate 18 and extends toward the sealing body 17, and a negative electrode lead 21 attached to the negative electrode 12 passes outside an insulating plate 19 and extends toward the bottom side of the case body 16. The positive electrode lead 20 is connected to the underside of a filter 23, which is the bottom plate of the sealing body 17, by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as a positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the case body 16 by welding or the like, and the case body 16 serves as a negative electrode terminal.
[0016] The positive electrode 11, the negative electrode 12, and the separator 13 will be described in detail below.
[0017] [Positive electrode] The positive electrode 11 has a positive electrode core and a positive electrode composite layer provided on the surface of the positive electrode core. For the positive electrode core, a foil of a metal such as aluminum that is stable in the potential range of the positive electrode 11, a film with the metal disposed on the surface layer, or the like can be used. The positive electrode composite layer contains a positive electrode active material, a binder, and a conductive material, and is preferably provided on both sides of the positive electrode core except for the part to which the positive electrode lead 20 is connected. The positive electrode 11 can be produced, for example, by applying a positive electrode composite slurry containing a positive electrode active material, a binder, a conductive material, and the like to the surface of the positive electrode core, drying the coating, and then compressing it to form a positive electrode composite layer on both sides of the positive electrode core.
[0018] Examples of the conductive material contained in the positive electrode composite layer include carbon materials such as carbon black, acetylene black, ketjen black, and graphite. Examples of the binder contained in the positive electrode composite layer include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. These resins may be used in combination with cellulose derivatives such as carboxymethyl cellulose (CMC) or its salts, polyethylene oxide (PEO), and the like.
[0019] The positive electrode active material contains a lithium transition metal composite oxide. The lithium transition metal composite oxide has the general formula Li α [Li x Mn y Co z Me (1-x-y-z) O 2 (wherein Me is at least one selected from Ni, Fe, Ti, Bi, and Nb, 0.5 < α < 1, 0.05 < x < 0.25, 0.4 < y < 0.7, 0 < z < 0.25).
[0020] In the present embodiment, the positive electrode active material is described as containing only the above lithium transition metal composite oxide (hereinafter referred to as "composite oxide A"). However, the positive electrode active material may contain compounds other than composite oxide A as long as the object of the present disclosure is not impaired.
[0021] Composite oxide A has a crystal structure of the O2 structure. The O2 structure is preferably 50% by volume or more, more preferably 90% by volume or more, of the crystal structure of composite oxide A from the viewpoint of crystal structure stability and the like. Here, the O2 structure is a layered crystal structure in which lithium is present at the center of an oxygen octahedron and there are two types of overlapping patterns of oxygen and transition metals per unit cell, and it belongs to the space group P6 3 mc. Such a layered crystal structure has a lithium layer, a transition metal layer, and an oxygen layer. In the above general formula of composite oxide A, the lithium layer contains Li α , and the transition metal layer contains Li x Mn y Co z Me (1-x-y-z)The oxygen layer is O 2 Includes.
[0022] The composite oxide A may contain a composite oxide of T2 structure or O6 structure that is synthesized as a by-product when synthesizing the composite oxide A. Here, the T2 structure is a layered crystal structure in which lithium exists at the center of an oxygen tetrahedron, and there are two types of overlapping of oxygen and transition metals per unit cell, and belongs to the space group Cmca. The O6 structure is a layered crystal structure in which lithium exists at the center of an oxygen octahedron, and there are six types of overlapping of oxygen and transition metals per unit cell, and belongs to the space group R-3m.
[0023] In the composite oxide A, the Li contained in the transition metal layer may be more than 5 mol% and less than 25 mol% relative to the total number of moles of the metal elements contained in the transition metal layer, but is preferably more than 10 mol% and less than 20 mol%, in terms of the stability of the crystal structure, etc. The Mn content may be more than 40 mol% and less than 75 mol% relative to the total number of moles of the metal elements contained in the transition metal layer, but is preferably more than 50 mol% and less than 65 mol%. The Co content may be more than 0 mol% and less than 25 mol% relative to the total number of moles of the metal elements contained in the transition metal layer, but is preferably more than 5 mol% and less than 20 mol%.
[0024] The metal element Me other than Li, Mn, and Co contained in the composite oxide A is preferably at least one selected from Ni, Fe, Ti, Bi, and Nb. Among them, Ni and Fe are preferable. The content of Me is preferably more than 3 mol% and less than 20 mol% with respect to the total number of moles of the metal elements contained in the transition metal layer. Note that the composite oxide A may contain metal elements other than the above as long as the object of the present disclosure is not impaired.
[0025] The amount of each metal component constituting the composite oxide A is measured by inductively coupled plasma (ICP) emission spectrometry.
[0026] The particle size distribution of the composite oxide A has a first peak on the small particle size side and a second peak on the large particle size side. The particle size distribution of the composite oxide A in this specification refers to a cumulative particle size distribution based on volume, and can be measured using a laser diffraction type particle size distribution measuring device (e.g., MT3300EXII manufactured by Microtrack Bell Co., Ltd.) with water as a dispersion medium. Although the particle size distribution may have three or more peaks, the following description focuses on the first peak on the small particle size side and the second peak on the large particle size side.
[0027] The composite oxide A has a first particle group corresponding to a first peak on the small particle size side and a second particle group corresponding to a second peak on the large particle size side. The first particle group and the second particle group are classified by dividing the waveform showing the particle size distribution of the composite oxide A by the particle size at which the frequency between the first peak and the second peak is the smallest. The abundance ratio of the first particle group contained in the composite oxide A is preferably smaller than the abundance ratio of the second particle group contained in the composite oxide A. When the abundance ratio of the first particle group contained in the composite oxide A is smaller than the abundance ratio of the second particle group contained in the composite oxide A, the packing density of the positive electrode active material may be further increased, and the capacity of the secondary battery may be further improved.
[0028] The abundance ratio of the first particle group contained in the composite oxide A is, for example, preferably 5% or more and 30% or less, and more preferably 10% or more and 20% or less. The abundance ratio of the second particle group contained in the composite oxide A is, for example, preferably 70% or more and 95% or less, and more preferably 80% or more and 90% or less. The abundance ratio is a value obtained from the relative particle amount based on the volume standard of the first peak or the second peak.
[0029] The average particle diameter (Da) of the first particle group is preferably 30 nm or more and 5 μm or less, more preferably 40 nm or more and 1 μm or less. The average particle diameter (Db) of the second particle group is preferably 1 μm or more and 15 μm or less, more preferably 2 μm or more and 10 μm or less. The ratio (Db / Da) of the average particle diameter (Da) of the first particle group to the average particle diameter (Db) of the second particle group is preferably 1 / 2 or less. By the average particle diameter (Da) of the first particle group, the average particle diameter (Db) of the second particle group, and Db / Da satisfying the above ranges, the collapse of the crystal structure due to the charge / discharge cycle is suppressed, and the packing density of the positive electrode active material is improved, so that the capacity of the secondary battery is improved or the decrease in the capacity retention rate during the charge / discharge cycle is suppressed compared to the case where the above ranges are not satisfied. The average particle diameter of the first particle group is the median value of the particle diameter range of the first peak, and the average particle diameter of the second particle group is the median value of the particle diameter range of the second peak.
[0030] The first particle group and the second particle group may have the same composition or different compositions as long as they are within the range of the above general formula.
[0031] The composite oxide A is produced, for example, by (1) a first step of producing a precursor, a composite oxide containing Mn, Co, Li and Na, and (2) a second step of carrying out an ion exchange treatment on the precursor in a molten salt containing lithium or in a solvent containing a lithium compound.
[0032] (1st step) The precursor Mn-, Co-, Li- and Na-containing composite oxide is produced by adding and mixing raw materials such as sodium compounds, manganese compounds, cobalt compounds, and lithium compounds in a predetermined molar ratio, and firing the resulting mixture. The firing temperature of the mixture is preferably in the range of 750°C to 850°C. The firing atmosphere is preferably an oxygen atmosphere or air. By setting the firing temperature and firing atmosphere under the above conditions, it is easy to obtain composite oxide A that shows a particle size distribution having a first peak on the small particle size side and a second peak on the large particle size side.
[0033] The sodium compound is not particularly limited, but for example, Na 2 O, Na 2 O 2 Oxides such as Na 2 CO 3 , NaNO 3 and hydroxides such as NaOH. The manganese compound is not particularly limited, but examples thereof include Mn 3 O 4 ,Mn 2 O 3 , MnO 2 Oxides such as MnSO 4 , MnCO 3 , MnCl 2 Salts such as Mn(OH) 2 The cobalt compound is not particularly limited, but examples thereof include CoO, Co 2 O 3 Oxides such as CoSO 4 , CoCl 2 Salts such as Co(OH) 2 The lithium compound is not particularly limited, but may be Li 2 CO 3 , LiOH, LiCl, etc. As the raw material of the precursor, composite hydroxides and carbonates of manganese, nickel, cobalt, etc. can also be used.
[0034] (2nd process) The precursor obtained in the first step is subjected to an ion exchange treatment in a molten salt containing lithium or a solvent containing a lithium compound, thereby obtaining a composite oxide A. The molten salt containing lithium may be, for example, a salt that melts at a low temperature, such as lithium nitrate, lithium chloride, lithium bromide, or lithium iodide. The lithium compound may be, for example, a lithium carbonate, a lithium acetate, a lithium nitrate, or a lithium halide, and the organic solvent may be, for example, a higher alcohol such as hexanol, an ether such as diethylene glycol monoethyl ether, or an organic solvent having a boiling point of 140° C. or higher. The treatment temperature of the ion exchange treatment is, for example, preferably 0° C. or higher and 300° C. or lower. The time of the ion exchange treatment is, for example, preferably 1 hour or higher and 48 hours or lower.
[0035] [Negative electrode] The negative electrode 12 has a negative electrode core and a negative electrode composite layer provided on the surface of the negative electrode core. For the negative electrode core, a foil of a metal such as copper that is stable in the potential range of the negative electrode 12, a film with the metal disposed on the surface layer, or the like can be used. The negative electrode composite layer contains a negative electrode active material and a binder, and is preferably provided on both sides of the negative electrode core except for the part to which the negative electrode lead 21 is connected. The negative electrode 12 can be produced, for example, by applying a negative electrode composite slurry containing a negative electrode active material and a binder to the surface of the negative electrode core, drying the coating, and then compressing it to form a negative electrode composite layer on both sides of the negative electrode core.
[0036] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions, but preferably contains a carbon-based active material. Suitable carbon-based active materials include natural graphite such as flake graphite, lump graphite, and earthy graphite, and artificial graphite such as lump artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB). The negative electrode active material may also include a Si-based active material composed of at least one of Si and a Si-containing compound.
[0037] As in the case of the positive electrode 11, the binder may be a fluororesin, PAN, polyimide, acrylic resin, polyolefin, or the like, but it is preferable to use styrene-butadiene rubber (SBR). The negative electrode mixture layer preferably further contains CMC or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), or the like. Among them, it is preferable to use SBR in combination with CMC or a salt thereof, or PAA or a salt thereof.
[0038] [Separator] For example, a porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have either a single-layer structure or a laminated structure. A heat-resistant layer or the like may be formed on the surface of the separator.
[0039] <Example> The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0040] <Example 1> [Synthesis of positive electrode active material] NiSO 4 , CoSO 4 , and MnSO 4 The mixture was mixed in an aqueous solution in a stoichiometric ratio of 13.5:13.5:73 and co-precipitated to give (Ni,Co,Mn)(OH). 2 Next, (Ni,Co,Mn)(OH) 2 , Na 2 CO 3 , and LiOH H 2 O was mixed to give a stoichiometric ratio of (Ni+Co+Mn):Na:Li of 87:83:13, and the mixture was kept at 800°C for 10 hours in air to synthesize a precursor.
[0041] The composition of the obtained precursor was analyzed using an inductively coupled plasma (ICP) emission spectrometer (manufactured by Thermo Fisher Scientific, product name "iCAP6300"), and the result was Na:Li:Mn:Co:Ni = 0.756:0.133:0.633:0.117:0.117.
[0042] Next, 10 times the equivalent amount (25 g) of a molten salt made by mixing lithium nitrate and lithium chloride in a molar ratio of 88:12 was added to 5 g of the precursor. The mixture was then kept at 280°C for 2 hours to ion-exchange the Na in the precursor with Li, and lithium iodide was added to produce a lithium transition metal composite oxide.
[0043] The composition of the obtained composite oxide was analyzed using an inductively coupled plasma (ICP) emission spectrometer (manufactured by Thermo Fisher Scientific, product name "iCAP6300"). The result was Li:Mn:Co:Ni = 1.13:0.724:0.137:0.139. This was used as the positive electrode active material.
[0044] [Preparation of positive electrode] The positive electrode active material, acetylene black, and polyvinylidene fluoride (PVdF) were mixed in a mass ratio of 92:5:3, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode composite slurry. Next, this positive electrode composite slurry was applied to the surface of a positive electrode core made of aluminum foil, and the coating was dried and compressed, and then cut into a predetermined electrode size to produce a positive electrode in which a positive electrode composite layer was formed on the positive electrode core.
[0045] [Preparation of non-aqueous electrolyte] LiPF was added to a mixed solvent of fluoroethylene carbonate (FEC) and methyl 3,3,3-trifluoropropionate (FMP) in a mass ratio of 1:3. 6 was dissolved at a concentration of 1 mol / L to prepare a non-aqueous electrolyte solution.
[0046] [Preparation of test cell] An electrode assembly was prepared by attaching lead wires to the positive electrode and the Li metal counter electrode, and arranging the positive electrode and the counter electrode facing each other via a polyolefin separator. The electrode assembly and the nonaqueous electrolyte were enclosed in an exterior body made of an aluminum laminate film to prepare a test cell.
[0047] <Example 2> A positive electrode active material was produced in the same manner as in Example 1, except that in the synthesis of the precursor, the firing conditions were changed to a condition of maintaining the material in an oxygen atmosphere at 800° C. for 10 hours. In addition, a test cell was produced in the same manner as in Example 1, except that the positive electrode active material was used.
[0048] <Comparative Example> A positive electrode active material was produced in the same manner as in Example 1, except that in the synthesis of the precursor, the calcination conditions were changed to a condition of maintaining the precursor in air at 900° C. for 10 hours. In addition, a test cell was produced in the same manner as in Example 1, except that the positive electrode active material was used.
[0049] [Evaluation of positive electrode active material] The positive electrode active materials of Examples 1 and 2 and the Comparative Example were subjected to XRD measurement to identify the crystal structure. The positive electrode active materials of Examples 1 and 2 and the Comparative Example were found to belong to the space group P6 3 The O2 structure assigned to mc was the predominant structure.
[0050] The particle size distribution of the positive electrode active material of Examples 1, 2 and Comparative Example was measured using a laser diffraction type particle size distribution measuring device (MT3300EXII, manufactured by Microtrack Bell Co., Ltd.). The particle size distribution of the positive electrode active material of Examples 1 and 2 had a first peak on the small particle size side and a second peak on the large particle size side. When the particle size distribution obtained for the positive electrode active material of Example 1 was analyzed, the abundance ratio of the first particle group corresponding to the first peak on the small particle size side contained in the positive electrode active material was 10%, and the abundance ratio of the second particle group corresponding to the second peak on the large particle size side was 90%. In addition, the average particle size of the first particle group corresponding to the first peak on the small particle size side was 40 nm, and the average particle size of the second particle group corresponding to the second peak on the large particle size side was 3 μm.
[0051] On the other hand, the particle size distribution of the positive electrode active material of the comparative example had only one peak. The average particle size of the positive electrode active material of the comparative example was 3 μm.
[0052] [Evaluation of battery capacity and capacity retention rate during charge / discharge cycles] The test cells of each Example and Comparative Example were charged at a constant current of 0.05C in a temperature environment of 25°C until the closed circuit voltage of the battery reached 4.7V (based on the Li counter electrode), and then charged at a constant voltage of 4.7V until the current value became less than 0.02C, and then discharged at a constant current of 0.05C until the closed circuit voltage of the battery reached 2.0V (based on the Li counter electrode). This charge and discharge was repeated for 10 cycles. The discharge capacity in the first cycle was taken as the battery capacity, and the results are summarized in Table 1. The capacity retention rate in the charge and discharge cycles was calculated using the following formula, and the results are summarized in Table 1.
[0053] Capacity retention rate (%) = 10th cycle discharge capacity ÷ 1st cycle discharge capacity × 100
[0054] [Table 1]
[0055] As shown in Table 1, Examples 1 and 2 had higher capacity than the Comparative Example, and the decrease in the capacity retention rate during charge / discharge cycling was suppressed. In other words, by using the positive electrode active materials of the Examples, a secondary battery having a high capacity and good cycle characteristics can be provided. [Explanation of symbols]
[0056] 10 Secondary battery 11 Positive electrode 12 Negative electrode 13 Separator 14 Electrode body 15 Battery case 16 Case body 17 Sealing body 18 Insulating plate 18,19 Insulating plate 20 Positive lead 21 Negative lead 22 Overhang 23 Filters 24 Lower valve body 25 Insulating materials 26 Upper valve 27 Cap 28 Gasket
Claims
1. A positive electrode active material for a secondary battery containing a lithium transition metal composite oxide, The lithium transition metal composite oxide has the general formula Li α [Li x Mn y Co z Me (1-x-y-z) ]O 2 (wherein Me is at least one selected from Ni, Fe, Ti, Bi, and Nb, 0.5<α<1, 0.05<x<0.25, 0.4<y<0.7, and 0<z<0.25), and has a crystal structure of O2 structure; The particle size distribution of the lithium transition metal composite oxide has a first peak on the small particle size side and a second peak on the large particle size side, The average particle size (Da) of the first particle group corresponding to the first peak on the small particle size side is 30 nm or more and 5 μm or less, and the average particle size (Db) of the second particle group corresponding to the second peak on the large particle size side is 2 μm or more and 15 μm or less, a ratio (Da / Db) of an average particle size (Da) of the first particle group to an average particle size (Db) of the second particle group is 1 / 2 or less.
2. 2. The positive electrode active material for a secondary battery according to claim 1, wherein an abundance ratio of the first particle group corresponding to the first peak on the small particle size side contained in the lithium transition metal composite oxide is smaller than an abundance ratio of the second particle group corresponding to the second peak on the large particle size side contained in the lithium transition metal composite oxide.
3. A positive electrode active material for a secondary battery as described in claim 2, wherein the abundance ratio of the first particle group corresponding to the first peak on the small particle size side contained in the lithium transition metal complex oxide is 5% or more and 30% or less, and the abundance ratio of the second particle group corresponding to the second peak on the large particle size side contained in the lithium transition metal complex oxide is 70% or more and 95% or less.
4. A secondary battery comprising a positive electrode containing the positive electrode active material for a secondary battery according to any one of claims 1 to 3, a negative electrode, and an electrolyte.
Citation Information
Patent Citations
Positive electrode active material and nonaqueous electrolyte secondary battery
JP2000082466A
Composite metal oxide, positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery
JP2012204281A
Cathode active material for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and method of manufacturing cathode active material for nonaqueous electrolyte secondary battery
JP2015179661A
Positive electrode active material for lithium secondary battery, method for manufacturing the same, lithium secondary battery electrode, and lithium secondary battery
JP2018041657A