Electrode wire for wire electric discharge machining, manufacturing method thereof, and evaluation method for electrode wire for wire electric discharge machining

By manufacturing electrode wires with a diameter standard deviation of 0.15 μm or less, wire marks are prevented, enhancing machining accuracy and reducing the need for additional processing, thus improving the quality and reliability of wire electrical discharge machining.

JP7595416B2Active Publication Date: 2024-12-06PROTERIAL LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020013185
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-30
Publication Date
2024-12-06
Estimated Expiration
2040-01-30

AI Technical Summary

Technical Problem

Wire marks or machining surface streaks occur during wire electrical discharge machining, leading to defective products when molds are used in press working or injection molding, and additional processing like polishing is required to remove these marks, complicating the process and increasing costs.

Method used

An electrode wire for wire electrical discharge machining with a standard deviation of diameters at multiple locations in the longitudinal direction of 0.15 μm or less is manufactured and evaluated using a specific method that measures and ensures the diameter variation meets this threshold, preventing wire marks by ensuring consistent diameter throughout the wire.

Benefits of technology

The solution improves machining accuracy by preventing wire marks, reducing the need for additional processing and enhancing surface accuracy of machined workpieces, thereby improving the performance and reliability of electrode wires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595416000001
    Figure 0007595416000001
  • Figure 0007595416000002
    Figure 0007595416000002
  • Figure 0007595416000003
    Figure 0007595416000003
Patent Text Reader

Abstract

To provide a wire-EDM electrode wire which is used for wire electric discharge machining for fusing and removing a processed matter by generating a pulse discharge between the wire-EDM electrode wire and the processed matter, being a wire-EDM electrode wire which can prevent a wire mark from being formed at the processed matter when performing electric discharge machining.SOLUTION: There is selected a wire-EDM electrode wire 1 which can prevent a wire mark from being formed by evaluating whether or not a diameters of the wire-EDM electrode wire 1 in a plurality of points in a longitudinal direction are equal to 0.15 μm or smaller with respect to the wire-EDM electrode wire 1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode wire for wire electric discharge machining, a manufacturing method thereof, and a method for evaluating an electrode wire for wire electric discharge machining. [Background technology]

[0002] One type of machine that machines the contour shape of a conductive workpiece is a wire EDM, which generates intermittent pulse discharges between the electrode wire for wire EDM and the workpiece, and uses the thermal action and impact force generated to melt and remove the workpiece.

[0003] Patent Document 1 (JP 2017-189829 A) describes forming larger crystal grains constituting the coating layer of a wire electrode for wire electric discharge machining in order to improve discharge properties. Patent Document 2 (WO 2018 / 211772 A) describes devising a composition for the coating layer of a wire electrode for wire electric discharge machining to thereby suppress circumferential irregularities (surface roughness) in order to improve the speed and accuracy of wire electric discharge machining. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-189829 A [Patent Document 2] International Publication No. 2018 / 211772 Summary of the Invention [Problem to be solved by the invention]

[0005] In wire electric discharge machining, streaks called wire marks or machined surface streaks may occur on the machined surface of the workpiece (e.g., a die). When a product is manufactured by performing press processing or injection molding using a die with such wire marks, the wire marks may be transferred to the product, resulting in a defective product. One method to prevent such transfer is to remove the wire marks by additional processing such as polishing or grinding the surface of the die, but this has the problem of making the process complicated and increasing manufacturing costs. In addition, even if such additional processing is performed, the wire marks may not be removed, and the workpiece may become a defective product.

[0006] An object of the present invention is to provide an electrode wire for wire electric discharge machining that can improve the accuracy of electric discharge machining. [Means for solving the problem]

[0007] A brief outline of a representative embodiment of the present invention will be described below.

[0008] The electrode wire for wire electric discharge machining according to one embodiment has a standard deviation of diameter at a plurality of points in the longitudinal direction of 0.15 μm or less.

[0009] Moreover, a manufacturing method of a wire electric discharge machining electrode wire in one embodiment includes a step of drawing the wire electric discharge machining electrode wire, a step of winding the wire electric discharge machining electrode wire, and a step of selecting the wire electric discharge machining electrode wire by extracting a portion of the wound wire electric discharge machining electrode wire and evaluating the standard deviation of the diameter of the wire electric discharge machining electrode wire at multiple locations aligned in the longitudinal direction.

[0010] Moreover, a method for evaluating an electrode wire for wire electric discharge machining according to one embodiment evaluates whether or not a standard deviation of diameters of the electrode wire for wire electric discharge machining at a plurality of points in the longitudinal direction is equal to or less than a predetermined threshold value. Effect of the Invention

[0011] According to one embodiment disclosed in the present application, it is possible to improve machining accuracy when performing electric discharge machining using an electrode wire for wire electric discharge machining. [Brief description of the drawings]

[0012] [Figure 1] 1 is a perspective view showing an electrode wire for wire electric discharge machining according to an embodiment; [Diagram 2] FIG. 1 is a schematic perspective view of a wire electric discharge machine including an electrode wire for wire electric discharge machining. [Diagram 3] 1 is a schematic diagram showing a wire drawing machine used in manufacturing an electrode wire for wire electric discharge machining according to an embodiment. [Figure 4] This is the formula for standard deviation. [Diagram 5] FIG. 2 is an enlarged perspective view of a workpiece on which a wire mark is formed. [Figure 6] FIG. 2 is a plan view of a workpiece on which a wire mark is formed. [Figure 7] FIG. 2 is a perspective view showing a wire electric discharge machining electrode wire which is a first comparative example. [Figure 8] 1 is Table 1 showing standard deviations, the presence or absence of wire marks, and surface precision in Example 1, Example 2, and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiments will be described in detail with reference to the drawings. In all the drawings for explaining the embodiments, the same reference numerals are used for the members having the same functions, and the repeated explanations are omitted. In the following embodiments, the explanations of the same or similar parts will not be repeated as a rule unless it is particularly necessary.

[0014] In this embodiment, the diameter of the wire electric discharge machining electrode wire is measured at multiple points in the longitudinal direction of the wire electric discharge machining electrode wire, the standard deviation of the diameter of the wire electric discharge machining electrode wire is calculated from the measured diameters, and the wire electric discharge machining electrode wire is evaluated and selected, thereby preventing the occurrence of wire marks due to wire electric discharge machining and improving the surface accuracy of the machined surface. When simply referring to a dimension in this application, the dimension refers to the diameter in the short direction of the wire electric discharge machining electrode wire (the direction parallel to the cross section of the wire electric discharge machining electrode wire).

[0015] <Structure of electrode wire for wire electric discharge machining and evaluation method of electrode wire for wire electric discharge machining> The structure of the electrode wire for wire electric discharge machining according to the present embodiment and a method for evaluating the electrode wire for wire electric discharge machining will be described below with reference to FIG.

[0016] 1, the wire electric discharge machining electrode wire 1 of the present embodiment is a flexible cylindrical wire having a circular cross section (transverse cross section) perpendicular to the longitudinal direction. The wire electric discharge machining electrode wire 1 is made of, for example, brass.

[0017] The main feature of the wire electric discharge machining electrode wire 1 in this embodiment is that the dimensions, i.e., diameters, of the wire electric discharge machining electrode wire 1 are measured at multiple locations along the longitudinal direction of the wire electric discharge machining electrode wire 1, and the standard deviation of the diameters calculated from the diameters at the multiple locations thus obtained is 0.15 μm or less.

[0018] In this way, the wire electric discharge machining electrode wire 1, whose diameter standard deviation is 0.15 μm or less, has small diameter variation in the longitudinal direction, and therefore when used in wire electric discharge machining (hereinafter simply referred to as electric discharge machining), it is possible to prevent wire marks from occurring on the surface of the workpiece.

[0019] In order to ensure the reliability of the standard deviation and to effectively prevent the occurrence of wire marks, it is important to measure the diameter at at least 50 points per meter. In this embodiment, specifically, the diameter is measured at 4000 points over 5 m, and the standard deviation is calculated from the multiple diameter values ​​obtained thereby. In other words, the dimensions are measured at 800 points per meter. It is desirable that the multiple points at which measurements are taken are equally spaced from each other in the longitudinal direction.

[0020] Also, it is preferable to measure the diameter of the wire electric discharge machining electrode wire 1 over a length of 5 m or more as a sample and calculate the standard deviation from the multiple diameter values ​​obtained. In other words, if the measurement points are less than 5 m long, the reliability of the standard deviation may decrease and the occurrence of wire marks may not be effectively suppressed. Therefore, in this embodiment, the diameter of the wire electric discharge machining electrode wire 1 is measured at multiple points over a length of 5 m. In other words, among the multiple points measured to calculate the standard deviation, the distance between both ends of the wire electric discharge machining electrode wire 1 in the longitudinal direction is 5 m or more.

[0021] A mode of use of the wire electric discharge machining electrode wire will be described below with reference to Fig. 2. Fig. 2 is a schematic perspective view of a wire electric discharge machine including the wire electric discharge machining electrode wire. The X and Y directions shown in Fig. 2 are directions in which the wire electric discharge machining electrode wire can move relative to the workpiece in a plan view. The X and Y directions are directions perpendicular to each other in a plan view. The Z direction shown in Fig. 2 is the longitudinal direction of the wire electric discharge machining electrode wire, and is a direction perpendicular to each of the X and Y directions.

[0022] As shown in FIG. 2, the wire electric discharge machine has a replaceable electrode wire 1 for wire electric discharge machining, which is a consumable part, and rolls 16 and 17 for fixing the electrode wire 1 for wire electric discharge machining in a stretched state so as to extend in the Z direction. Although not shown, the wire electric discharge machine also has a table that can be moved in the X and Y directions around the electrode wire 1 for wire electric discharge machining, and a workpiece (machined object, workpiece, steel material) 14 is fixed on the table. The rolls 16 are located above the table and the workpiece 14, respectively, and the rolls 17 are located below the table and the workpiece 14, respectively. FIG. 2 shows a state in which a start hole 15 is formed penetrating from the upper surface to the lower surface of the plate-shaped workpiece 14, and a predetermined area is machined from the start hole 15 by performing wire electric discharge. Although not shown, the workpiece 14 is immersed in a machining fluid. The machining fluid is, for example, a liquid with a constant electrical conductivity, and insulating oil or ion-exchanged water is used.

[0023] A wire electric discharge machine generates intermittent pulse discharges between the wire electric discharge machining electrode wire 1 and the workpiece 14, and performs machining while melting and removing the workpiece by the thermal action and impact force at this time. Here, machining is performed by moving the table and workpiece 14 in the X or Y direction. The wire electric discharge machining electrode wire 1 is fixed and does not move in the X and Y directions, but in the Z direction it is sent upward or downward as rolls 16, 17 rotate during machining. This is to prevent a decrease in machining accuracy and breakage due to wear of the wire electric discharge machining electrode wire 1 caused by discharge.

[0024] The wire electric discharge machining electrode wire 1 is made of a conductive material, such as brass. The workpiece 14 is also made of a conductive material. In wire electric discharge machining, discharge is generated between the wire electric discharge machining electrode wire 1 and the workpiece 14, both of which are conductive, while the workpiece 14 is scanned across the wire electric discharge machining electrode wire 1 to machine the workpiece 14. Since wire electric discharge machines can machine relatively hard materials, they are used, for example, in machining molds and the like.

[0025] <Manufacturing process> A method for manufacturing an electrode wire for wire electric discharge machining according to this embodiment will be described below with reference to Fig. 3. Fig. 3 is a schematic diagram showing a wire drawing machine used for manufacturing the electrode wire for wire electric discharge machining according to this embodiment.

[0026] In a wire drawing machine using a wire drawing die, it is possible to transport and stretch the metal wire using an inlet capstan that feeds the metal wire into the wire drawing die, and an outlet capstan that pulls out the metal wire sent out from the wire drawing die. The structure of such a device is shown in Figure 3. Here, we will explain a wire drawing machine for forming round wire, that is, metal wire with a circular cross section. In Figure 3, the point where lubricating oil for wire drawing is supplied is indicated by a dashed arrow.

[0027] As shown in FIG. 3, the metal wire 13 supplied to the wire drawing machine is transported through the capstan 6, the wire drawing die 3, the dancer 9, and the capstan 10 in this order. The wire drawing die 3 is made of, for example, a disk-shaped metal plate, and has a hole penetrating the metal plate. The hole has a structure in which the diameter gradually decreases from the surface side of the metal plate, so that the metal wire 13 fed from the surface side to pass through the hole is narrowed and stretched thinly when passing through the wire drawing die 3, and then exits the wire drawing die 3. Here, the feeding of the metal wire into the capstan or die is called "entering wire," and the exiting of the metal wire from the capstan or die is called "exiting wire." The capstan 6 is used to transport the metal wire 13 before it enters the wire drawing die 3. The capstan 10 is used to pull out the metal wire 13 from the wire drawing die 3 and transport it.

[0028] In the manufacturing process of the electrode wire for wire electric discharge machining, first, the metal wire 13, which is a round wire, is supplied to the wire drawing machine from a roll (not shown) on which the metal wire 13 is wound. Next, the metal wire 13 is wound around the capstan 6 and then sent to the wire drawing die 3. The capstan 6 is made of, for example, a metal roll (capstan) whose surface is covered with rubber. The metal wire 13 is wound so as to go around the capstan 6. The metal wire 13 is transported by friction with the capstan 6 that is driven to rotate. Note that the wire drawing machine has a plurality of wire drawing dies 3 arranged along the wire drawing direction. Among the plurality of wire drawing dies 3, a plurality of finishing wire drawing dies are arranged as the wire drawing dies 3 immediately before the wire is drawn out from the wire drawing machine. It is preferable that the exit portion of the die hole provided inside each of the plurality of finishing wire drawing dies (the portion from which the metal wire 13 that passes through the die hole is drawn out) has the same diameter. By drawing a metal wire using a wire drawing machine using such a plurality of finish wire drawing dies, the standard deviation of the diameter of the wire electric discharge machining electrode wire 1 obtained by the wire drawing can be made 0.15 μm or less.

[0029] Next, the metal wire 13 passes through the wire drawing die 3, whereby the metal wire 13 is stretched and thinned. By stretching and drawing the metal wire 13 in this manner, a wire electric discharge machining electrode wire 1 made of the metal wire 13 is formed. The wire electric discharge machining electrode wire 1 after being drawn has a diameter of, for example, 0.1 mm or more and 0.3 mm or less. A lubricant is supplied to the wire drawing die 3 to reduce friction with the wire electric discharge machining electrode wire 1, but the lubricant is removed from the surface of the wire electric discharge machining electrode wire 1 by passing the wire drawing die 3. The wire electric discharge machining electrode wire 1 stretched and drawn by the wire drawing die 3 is wound around a dancer 9, and then wound around a capstan 10 and transported. That is, the wire electric discharge machining electrode wire 1 is pulled out of the wire drawing die 3 by the capstan 10.

[0030] The capstan 10 is, for example, a metal roll with a rubber-covered surface, similar to the capstan 6. The electrode wire 1 for wire electric discharge machining is wound around the capstan 10 so as to go around it. The electrode wire 1 for wire electric discharge machining is transported by friction with the capstan 10, which is driven to rotate. In this manner, the wire drawing by the wire drawing machine is performed.

[0031] Here, the metal wire 13 is drawn thinner and longer after passing through the wire drawing die 3 than before passing through the wire drawing die 3. Therefore, the speed at which the wire electrode wire 1 for wire discharge machining is conveyed after being drawn out of the wire drawing die 3 is faster than the speed at which the metal wire 13 is conveyed before entering the wire drawing die 3. Therefore, in order to prevent abnormal elongation or breakage of the wire electrode wire 1 for wire discharge machining, a dancer 9, which is a speed adjustment mechanism for the wire electrode wire 1 for wire discharge machining, is provided between the wire drawing die 3 and the capstan 10. The dancer 9 is, for example, composed of a roll 16 whose rotation axis is fixed and a roll 17 which is movable in the vertical direction, and the metal wire 13 is wound around the rolls 16, 17 several times.

[0032] The wire electric discharge machining electrode wire 1 fed by the capstan 10 is wound, for example, around a bobbin (roll, drum) 11. The bobbin 11 and the wire electric discharge machining electrode wire 1 wound around the bobbin constitute a winding 12. In this manner, winding around the bobbin 11 is performed. The winding 12 wound around one bobbin 11 has, for example, 5 km of wire electric discharge machining electrode wire 1. In this manufacturing process, several tens of windings 12 can be obtained for each bobbin 11 around which, for example, 5 km of wire electric discharge machining electrode wire 1 is wound.

[0033] In order to manufacture a high-quality electrode wire 1 for wire electric discharge machining that can prevent the occurrence of wire marks, it is possible to devise measures such as quality control of the wire drawing die 3 or the lubricating oil supplied to the metal wire 13.

[0034] Next, the process moves to inspecting the wire electric discharge machining electrode wire 1. First, several hundred meters of the wire electric discharge machining electrode wire 1 for inspection is taken from the winding 12 wound around one bobbin. The wire electric discharge machining electrode wires 1 of the respective windings 12 wound around each bobbin 11 are manufactured under the same manufacturing conditions, and therefore have the same quality. Therefore, if any part of the wire electric discharge machining electrode wires 1 among the windings 12 is taken as an inspection sample and inspected, it can be considered that all of the multiple windings 12 have been evaluated.

[0035] When inspecting an arbitrary portion of the wire electric discharge machining electrode wire 1 as a sample, the sample may be taken from any portion in the longitudinal direction of the wire electric discharge machining electrode wire 1. From the viewpoint of ease of taking a sample, it is preferable to take and inspect a sample of about several hundred meters from the tip portion of the wire electric discharge machining electrode wire 1 wound around the surface (outside) of the winding 12.

[0036] In the inspection process, at least the dimensions of the wire electric discharge machining electrode wire 1 are evaluated. The dimensional evaluation performed in the inspection process is the same as the evaluation method described above with reference to FIG. 1. That is, in the inspection process, the diameter of the wire electric discharge machining electrode wire 1 is measured at multiple different positions in the longitudinal direction of the wire electric discharge machining electrode wire 1, and it is evaluated whether or not the standard deviation of the diameters obtained from the multiple measured diameters is 0.15 μm or less. In addition to evaluating the dimensions, the inspection process may also inspect physical properties of the wire electric discharge machining electrode wire 1, such as tensile strength and elongation.

[0037] To ensure the reliability of the standard deviation and to effectively prevent the occurrence of wire marks, it is desirable to measure the diameter of the wire electric discharge machining electrode wire 1 at least at 50 locations per meter in the longitudinal direction of the wire electric discharge machining electrode wire 1. Specifically, the diameter of the wire electric discharge machining electrode wire 1 is measured at 800 locations per meter, for example. It is desirable that the locations at which measurements are taken are equally spaced from one another in the longitudinal direction.

[0038] As described with reference to FIG. 2, the wire electric discharge machining electrode wire 1 performs electric discharge machining while being fed in the Z direction (vertical direction). Therefore, the diameter measurement is performed while feeding the wire electric discharge machining electrode wire 1 in the vertical direction using a traveling machine simulating the wire electric discharge machining machine described with reference to FIG. 2. That is, the traveling machine is provided with rolls 16, 17 (see FIG. 2) that can feed the wire electric discharge machining electrode wire 1 upward or downward by rotating, for example. Here, a laser outer diameter measuring device fixed between the rolls 16 and 17 of the traveling machine is used to continuously measure the diameter of the wire electric discharge machining electrode wire 1 fed at a uniform speed at equal intervals. This makes it possible to measure the diameter of the wire electric discharge machining electrode wire 1 at different points in the longitudinal direction of the wire electric discharge machining electrode wire 1.

[0039] Next, the standard deviation of the diameter of the wire electric discharge machining electrode wire 1 is calculated using the diameters at multiple points aligned in the longitudinal direction of the wire electric discharge machining electrode wire 1, and it is evaluated whether the calculated standard deviation is equal to or less than a predetermined threshold value (0.15 μm). The standard deviation of the diameter can be determined, for example, by the following formula. This completes the manufacturing process of the wire electric discharge machining electrode wire 1.

[0040] The standard deviation s of the diameters of the electrode wire 1 for wire electric discharge machining at a plurality of points arranged in the longitudinal direction can be expressed by the formula 1 shown in FIG. 4. In the formula 1, s represents the standard deviation, and s 2 represents the variance, and n represents the total number of data (measured diameters). In addition, in Equation 1, x i represents the individual diameter of the measured electrode wire 1 for wire electric discharge machining. In addition, in formula 1, x with a bar at the top represents the average value of the individual diameters of the measured electrode wire 1 for wire electric discharge machining.

[0041] According to the study by the present inventors, it has been confirmed that in the inspection process, the occurrence of wire marks can be prevented in wire electric discharge machining electrode wires 1 having a standard deviation of diameter of 0.15 μm or less, but wire marks occur in wire electric discharge machining electrode wires 1 having the standard deviation more than 0.15 μm. Therefore, by evaluating whether the wire electric discharge machining electrode wires 1 have the standard deviation of 0.15 μm or less in the inspection process, it is possible to select wire electric discharge machining electrode wires 1 capable of preventing the occurrence of wire marks.

[0042] <Effects of this embodiment> The effects of this embodiment will be described below with reference to Fig. 5, Fig. 6 and Fig. 7. Fig. 5 is an enlarged perspective view showing a workpiece having wire marks formed on its machined surface. Fig. 6 is a plan view showing a workpiece having wire marks formed on its machined surface. Fig. 7 is a perspective view explaining a method for evaluating a wire electric discharge machining electrode wire, which is Comparative Example 1.

[0043] In wire electric discharge machining, vertical lines, also called wire marks 18 or machined surface lines, may appear on the machined surface of a workpiece 14 (e.g., a die) as shown in Figures 5 and 6. Wire marks 18 are thought to be recesses (grooves) that extend on the surface of workpiece 14 along the extension direction of the wire electric discharge machining electrode wire used when machining workpiece 14. It is difficult to visually confirm each of the irregularities of wire marks 18, but by visually inspecting the machined surface on which wire marks 18 are formed, it is possible to confirm that a pattern is formed by the vertical lines.

[0044] When a product is manufactured by performing press working or injection molding using a die having such wire marks 18, the wire marks may be transferred to the product, resulting in a defective product. One method for preventing such transfer is to remove the wire marks by additional processing such as polishing or grinding the surface of the die, but this creates a problem in that the process becomes complicated and the manufacturing costs increase. In addition, even if such additional processing is performed, the wire marks may not be removed, and the processed product may become a defective product.

[0045] One possible method for preventing the occurrence of wire marks 18 is to measure the dimensions and roundness of wire electric discharge machining electrode wire 20 at one location or at several different locations (e.g., about three locations) of wire electric discharge machining electrode wire 20, as shown in Comparative Example 1 in Fig. 7. In this case, it was thought that the occurrence of wire marks 18 could be prevented if the measured dimensions were within the dimensional tolerance, which is a predetermined allowable range, and the roundness also satisfied the standard value.

[0046] However, even wire electric discharge machining electrode wires that meet such standards cannot sufficiently prevent the occurrence of wire marks when used in electric discharge machining, and there is a need for further improvement in the performance of wire electric discharge machining electrode wires and for establishing a method for evaluating high-performance wire electric discharge machining electrode wires.

[0047] As a result of investigations, the inventors have found that even if the dimensions of a wire electric discharge machining electrode wire are within the dimensional tolerances at several points and have a specified roundness, wire marks are likely to occur when the dimensions vary widely or when the dimensions change significantly within a small range in the longitudinal direction, etc. In other words, when the dimensions of the wire electric discharge machining electrode wire change suddenly in the longitudinal direction, a large change in the strength of the discharge occurs during electric discharge machining even if the diameter of the wire electric discharge machining electrode wire falls within the dimensional tolerances, resulting in wire marks.

[0048] Therefore, the inventors have devised a method for evaluating the quality of a wire electrode wire for electric discharge machining based on the standard deviation of diameters at a number of points aligned in the longitudinal direction of the wire electrode wire. As a result of carrying out an experiment to calculate this standard deviation for a number of wire electrode wires for electric discharge machining, it has been found that wire marks can be effectively prevented from occurring in a wire electrode wire for electric discharge machining with a standard deviation of 0.15 μm or less. This threshold value of the standard deviation is a commonly effective judgment index regardless of the material, thickness, and material of the wire electrode wire for electric discharge machining, and the material of the workpiece. In the wire electrode wire for electric discharge machining of this embodiment, it is important that the standard deviation of the dimensions is equal to or less than the predetermined threshold value of 0.15 μm.

[0049] That is, in the evaluation method of Comparative Example 1, the standard deviation is not used as an evaluation criterion, so the dimensions and roundness are measured at about 1 to 3 points, and the distance between the measurement points does not need to be equal. Therefore, it is difficult to find dimensional changes in the wire electric discharge machining electrode wire caused by wobbling, scratches, twists, dirt, etc. of the wire electric discharge machining electrode wire, and it is difficult to detect dimensional variations in the wire electric discharge machining electrode wire.

[0050] In contrast, in this embodiment, the standard deviation of the wire electric discharge machining electrode wire is used as the evaluation criterion. Therefore, in order to ensure the reliability of the standard deviation, the diameter of the wire electric discharge machining electrode wire is measured at at least 50 points per meter. The standard deviation of the multiple dimensions obtained as a result is calculated, and if the standard deviation is equal to or less than the threshold value of 0.15 μm, it is possible to evaluate the wire electric discharge machining electrode wire as a high-performance (high-quality) wire electric discharge machining electrode wire that can prevent the occurrence of wire marks. As a result, for example, it is possible to select wire electric discharge machining electrode wires that can prevent the occurrence of wire marks from other wire electric discharge machining electrode wires, and manage and sell them as wire electric discharge machining electrode wires of different qualities. In addition, by making the distance between the points to be measured equal, the reliability of the standard deviation can be improved, and it is possible to prevent the wire electric discharge machining electrode wire from being overlooked in terms of wobbling, scratches, twists, dirt, etc.

[0051] Moreover, the fact that the wire electric discharge machining electrode wire has such a small standard deviation means that the wire electric discharge machining electrode wire has a high roundness. In other words, by evaluating the standard deviation of the dimensions at multiple points in the longitudinal direction of the wire electric discharge machining electrode wire, it is possible to evaluate and manage the roundness of the wire electric discharge machining electrode wire. Furthermore, by evaluating the standard deviation, it is possible to evaluate and manage the presence or absence of wobbling, scratches, twists, dirt, etc. in the wire electric discharge machining electrode wire. Therefore, there is no need to perform a roundness inspection process in addition to the dimensional evaluation of this embodiment, and it is possible to prevent the inspection process from becoming complicated.

[0052] As described above, in this embodiment, the occurrence of wire marks can be prevented and the surface precision of the machined surface can be improved. Therefore, by using the wire electric discharge machining electrode wire of this embodiment, it is not necessary to remove the wire marks by additional processing. Therefore, the performance of the wire electric discharge machining electrode wire can be improved. Also, the accuracy and reliability of the evaluation method for wire electric discharge machining electrode wire can be improved. Also, it is possible to realize the selection of wire electric discharge machining electrode wires, which was difficult with the evaluation method for wire electric discharge machining electrode wires of Comparative Example 1.

[0053] In the following, a wire electric discharge machining electrode wire was actually fabricated, and the standard deviation of the diameter of the wire electric discharge machining electrode wire was calculated, and electric discharge machining was performed using the wire electric discharge machining electrode wire. The standard deviation, the presence or absence of wire marks, and surface precision in Example 1, Example 2, and Comparative Example 2 are shown in Table 1 of FIG.

[0054] <Example 1> A metal wire made of brass was fed to a wire drawing machine using multiple finishing wire drawing dies. The metal wire fed to the wire drawing machine was drawn by the wire drawing dies to produce a wire electrode wire for electric discharge machining having a circular cross section and an outer diameter of 0.2 mm (diameter tolerance: 0.198 mm to 0.200 mm). Next, a test sample having a length of 300 m was taken from the produced wire electrode wire for electric discharge machining. The diameter of the wire electrode wire for electric discharge machining was measured at multiple different positions (800 positions per meter) in the longitudinal direction of the sample, and the standard deviation of the diameter of the wire electrode wire for electric discharge machining was calculated from the diameters at the multiple positions obtained and formula 1 shown in FIG. 4, and the standard deviation was 0.15 μm.

[0055] A workpiece (SKD11, thickness 60 mm) made of steel was subjected to electric discharge machining using the electrode wire for wire electric discharge machining of Example 1. The number of electric discharge machining processes on the surface of the workpiece was 7. When the surface of the workpiece was visually inspected, no wire marks were found.

[0056] <Example 2> A metal wire made of brass is fed to a wire drawing machine using multiple finishing wire drawing dies. The metal wire fed to the wire drawing machine is drawn by the wire drawing dies to produce a wire electrode wire for electric discharge machining having a circular cross section and an outer diameter of 0.2 mm (diameter tolerance: 0.198 mm to 0.200 mm). Next, a test sample having a length of 300 m is taken from the produced wire electrode wire for electric discharge machining. The diameter of the wire electrode wire for electric discharge machining was measured at multiple different positions (800 positions per meter) in the longitudinal direction of the sample, and the standard deviation of the diameter of the wire electrode wire for electric discharge machining was calculated from the diameters at the multiple positions obtained and formula 1 shown in FIG. 4. The standard deviation was about 0.05 μm (standard deviation of 0.15 μm or less).

[0057] A workpiece (SKD11, thickness 60 mm) made of steel was subjected to electric discharge machining using the electrode wire for wire electric discharge machining of Example 2. The number of electric discharge machining processes on the surface of the workpiece was set to 7. When the surface of the workpiece was visually inspected, no wire marks were found to have occurred.

[0058] <Comparative Example 2> In Comparative Example 2, a metal wire was drawn in the same manner as in Example without using a wire drawing machine with multiple finish wire drawing dies to produce a wire electric discharge machining electrode wire having a circular cross section and an outer diameter of 0.2 mm (diameter tolerance: 0.198 mm to 0.200 mm). At this time, the standard deviation of the diameter of the wire electric discharge machining electrode wire was about 0.20 μm (standard deviation larger than 0.15 μm).

[0059] A workpiece (SKD11, thickness 60 mm) was subjected to electrical discharge machining using the electrode wire for wire electrical discharge machining of Comparative Example 2. The number of electrical discharge machining processes on the surface of the workpiece was set to 7. When the surface of the workpiece was visually inspected, wire marks were found to have occurred on the surface of the workpiece.

[0060] As a result of the above, the wire electric discharge machining electrode wires of Examples 1 and 2 and Comparative Example 2 were all within the diameter tolerance (diameter tolerance: 0.198 mm to 0.200 mm), but the wire electric discharge machining electrode wires of Examples 1 and 2 with a diameter standard deviation of 0.15 μm or less did not produce wire marks, while the wire electric discharge machining electrode wire of Comparative Example 2 produced wire marks. Furthermore, the wire electric discharge machining electrode wires with a diameter standard deviation of 0.15 μm or less had better surface precision of the surface of the workpiece than the wire electric discharge machining electrode wires with a diameter standard deviation of more than 0.15 μm. The surface precision was evaluated by the maximum height (Rz according to JIS B0601 (2001)) obtained by observing the surface of the workpiece with a roughness tester.

[0061] The invention made by the present inventors has been specifically described above based on an embodiment, but it goes without saying that the present invention is not limited to the above embodiment and can be modified in various ways without departing from the gist of the invention. [Explanation of symbols]

[0062] 1, 20 Electrode wire for wire electric discharge machining 3 Wire drawing dies 11 Bobbin 12 Windings 13 Metal Wire 14 Workpiece 16, 17 rolls 18 Wiremark

Claims

1. An electrode wire for wire electric discharge machining which suppresses the occurrence of wire marks, comprising a single wire having a diameter of 0.1 mm or more and 0.3 mm or less, said diameter being within a predetermined allowable dimensional tolerance, and wherein the standard deviation calculated by measuring said diameter at 50 or more points equally spaced per meter in the longitudinal direction over a length of 5 m or more is 0.15 μm or less.

2. (a) providing a metal wire; (b) forming a wire electric discharge machining electrode wire made of the metal wire and having a diameter of 0.1 mm or more and 0.3 mm or less, the diameter being within a dimensional tolerance that is a predetermined allowable range, by drawing the metal wire; (c) winding the wire electric discharge machining electrode wire; (d) after the step (c), measuring the diameter at 50 or more points at equal intervals per meter in the longitudinal direction of the wire electric discharge machining electrode wire over a length of 5 m or more to calculate a standard deviation, and if the standard deviation is 0.15 μm or less, evaluating that the occurrence of wire marks can be suppressed; The method for producing an electrode wire for wire electric discharge machining comprising the steps of:

3. 3. The method for producing a wire electric discharge machining electrode wire according to claim 2, a distance between both ends of the plurality of locations in the longitudinal direction is 5 m or more.

4. A method for evaluating an electrode wire for wire electric discharge machining, comprising: measuring the diameter of a wire electrode wire for wire electric discharge machining consisting of a single wire having a diameter of 0.1 mm or more and 0.3 mm or less, said diameter being within a predetermined allowable dimensional tolerance, over a length of 5 m or more at 50 or more locations evenly spaced per meter in the longitudinal direction, calculating the standard deviation, and evaluating that the occurrence of wire marks is suppressible if the standard deviation is 0.15 μm or less.

Citation Information

Patent Citations

  • JP1981121530U

  • Electrode wire rod for wire electric discharge machining

    JP1987208827A

  • Method for producing metal-clad metal-matrix composite wire

    JP2007521968A

  • Wire-cut electro-discharge machining method

    JP2010240761A

  • Zinc coated electrode wire for wire electrical discharge machining and manufacturing method thereof

    JP2014136273A