Coated positive electrode active material for lithium ion batteries and lithium ion batteries
A coated manganese-based lithium metal oxide with a lithium styrene sulfonate polymer layer addresses manganese elution in lithium ion batteries, improving cycle characteristics and structural stability.
Patent Information
- Application Number
- JP2020119291
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-07-10
AI Technical Summary
Lithium ion batteries using manganese-based positive electrode active materials face issues with manganese elution due to acid generation during charging and discharging, leading to structural changes and deteriorated cycle characteristics.
A coated positive electrode active material is developed using manganese-based lithium metal oxide particles coated with a polymer compound containing lithium styrene sulfonate as a constituent monomer, which suppresses manganese elution and improves cycle characteristics.
The coating effectively reduces manganese elution, enhancing the cycle performance and structural integrity of lithium ion batteries.
Smart Images

Figure 0007595429000001 
Figure 0007595429000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a coated positive electrode active material for a lithium ion battery and a lithium ion battery. [Background technology]
[0002] Lithium ion (secondary) batteries have been widely used in recent years for various purposes as secondary batteries capable of achieving high energy density and high power density.
[0003] Many of the lithium metal oxides used as the positive electrode active material in lithium-ion batteries contain rare metals, which increases the cost per energy unit, so the use of cheaper manganese-based lithium metal oxides is being investigated.
[0004] However, repeated charging and discharging causes the electrolyte to deteriorate and produce a strong acid. When a manganese-based lithium metal oxide is used as the positive electrode active material, the strong acid corrodes the positive electrode active material, causing manganese to dissolve from the lithium metal oxide. This changes the structure of the positive electrode active material and deteriorates the cycle characteristics of the lithium-ion battery.
[0005] In order to solve this problem, studies have been made on the use of nickel-based metal oxides, which are acid scavengers, in combination with manganese-based metal oxides to suppress the elution of manganese (for example, Non-Patent Document 1).
[0006] However, nickel-based metal oxides are scarce resources, and because they easily absorb moisture in the storage environment, they have issues such as the need to store them at a low dew point, so this was not considered a sufficient countermeasure. [Prior art documents] [Non-patent literature]
[0007] [Non-Patent Document 1] "Development of Energy Storage Solutions Using Innovative Lithium-ion Secondary Batteries" NEC Corporation Smart Energy Research Laboratories Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above problems, and aims to provide a coated positive electrode active material for lithium ion batteries that can suppress the elution of manganese from the positive electrode active material particles that accompanies charging and discharging, even when a manganese-based lithium metal oxide is used as the positive electrode active material particles, and can improve the cycle characteristics of the lithium ion battery. [Means for solving the problem]
[0009] The present inventors discovered that by using lithium styrenesulfonate as a constituent monomer of a coating resin that covers positive electrode active material particles of manganese-based lithium metal oxide, it is possible to suppress the elution of manganese from the positive electrode active material that occurs during charging and discharging, and thereby improve the cycle characteristics of lithium-ion batteries, and thus arrived at the present invention. That is, the present invention relates to a coated positive electrode active material for lithium ion batteries, in which at least a portion of the surface of positive electrode active material particles is coated with a coating layer containing a polymer compound, the positive electrode active material particles including particles made of a manganese-based lithium metal oxide, and the polymer compound including a polymer having lithium styrenesulfonate as a constituent monomer; and a lithium ion battery comprising the coated positive electrode active material for lithium ion batteries of the present invention. Effect of the Invention
[0010] The coated positive electrode active material for lithium ion batteries of the present invention can suppress the elution of manganese from the positive electrode active material particles that accompanies charging and discharging, even when a manganese-based lithium metal oxide is used as the positive electrode active material particles, and can improve the cycle characteristics of the lithium ion battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Coated cathode active material for lithium-ion batteries> The coated positive electrode active material for lithium ion batteries of the present invention is a coated positive electrode active material for lithium ion batteries in which at least a portion of the surface of positive electrode active material particles is coated with a coating layer containing a polymer compound, characterized in that the positive electrode active material particles include particles made of a manganese-based lithium metal oxide, and the polymer compound includes a polymer having lithium styrenesulfonate as a constituent monomer.
[0012] (Cathode active material particles) The positive electrode active material particles include particles made of a manganese-based lithium metal oxide. Manganese-based lithium metal oxides include composite oxides of lithium and manganese (e.g., LiAlMnO4, LiMnO2, and LiMn2O4), composite oxides of lithium, manganese, and transition metals (e.g., LiFeMnO4 and LiMn 1-y Co y O2, etc.), and composite oxides of lithium, manganese, and two transition metals (e.g., LiMn a M b M' c O2 (M and M' are different transition metal elements and satisfy a+b+c=1), lithium manganese phosphate (for example, LiMnPO4), and the like. From the viewpoint of suitably suppressing the elution of manganese from the positive electrode active material during charge and discharge and improving cycle characteristics, lithium manganate (LiMn2O4) is preferred. The positive electrode active material particles may be used alone or in combination of two or more kinds.
[0013] The positive electrode active material particles may contain positive electrode active material particles other than particles made of manganese-based lithium metal oxide, as long as the effects of the present invention are not impaired. Positive electrode active material particles other than particles made of manganese-based lithium metal oxides include composite oxides of lithium and transition metals other than manganese {composite oxides containing one type of transition metal (LiCoO2 and LiNiO2, etc.), composite oxides containing two types of transition metal elements other than manganese (for example, LiNi 1-x Co x O2, LiNi 1 / 3 Co1 / 3 Al 1 / 3 O2 and LiNi 0.8 Co 0.15 Al 0.05 O2) and composite oxides containing three or more metal elements other than manganese [e.g. LiM a M' b M'' c O2(M, M' and M'' are different transition metal elements and satisfy a+b+c=1. For example, LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2), etc.}, lithium transition metal (excluding manganese) phosphates (e.g., LiFePO4, LiCoPO4, and LiNiPO4), transition metal oxides (e.g., MnO2 and V2O5), transition metal sulfides (e.g., MoS2 and TiS2), and conductive polymers (e.g., polyaniline, polypyrrole, polythiophene, polyacetylene, poly-p-phenylene, and polyvinylcarbazole). However, it is preferable not to use nickel-based metal oxides, cobalt-based metal oxides, etc., since there are problems such as limited resources.
[0014] In terms of energy density, the weight ratio of the particles made of manganese-based lithium metal oxide to the total weight of the positive electrode active material particles is preferably 80% by weight or more, and more preferably 85% by weight or more.
[0015] From the viewpoint of the electrical characteristics of the battery, the volume average particle diameter of the positive electrode active material particles is preferably 0.01 to 100 μm, more preferably 0.1 to 35 μm, and even more preferably 2 to 30 μm.
[0016] (polymer compound) The polymer compound includes a polymer having lithium styrenesulfonate as a constituent monomer. The weight proportion of lithium styrenesulfonate in the polymer compound is preferably 1 to 15% by weight based on the total weight of the constituent monomers of the polymer. When the weight proportion of lithium styrenesulfonate is within the above range, elution of manganese from the positive electrode active material due to charging and discharging can be suitably suppressed, and the cycle characteristics can be improved, and also the mechanical strength can be suitably imparted to the positive electrode. The weight proportion of lithium styrenesulfonate in the polymer compound is more preferably 5% by weight or more, and even more preferably 10% by weight or more, based on the total weight of the constituent monomers of the polymer.
[0017] The polymer compound preferably contains at least one of (meth)acrylic acid and an alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms as a constituent monomer. Incidentally, (meth)acrylic acid means acrylic acid and methacrylic acid.
[0018] The alkyl group having 4 to 12 carbon atoms may be a linear alkyl group or a branched alkyl group. Examples of the linear alkyl group having 4 to 12 carbon atoms include a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, and a dodecyl group. Examples of branched alkyl groups having 4 to 12 carbon atoms include 1-methylpropyl group (sec-butyl group), 2-methylpropyl group, 1,1-dimethylethyl group (tert-butyl group), 1-methylbutyl group, 1,1-dimethylpropyl group, 1,2-dimethylpropyl group, 2,2-dimethylpropyl group (neopentyl group), 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 4-methylpentyl group, 1,1-dimethylbutyl group, 1,2-dimethylbutyl group, 1,3-dimethylbutyl group, 2,2-dimethylbutyl group, 2, 3-dimethylbutyl group, 1-ethylbutyl group, 2-ethylbutyl group, 1-methylhexyl group, 2-methylhexyl group, 2-methylhexyl group, 4-methylhexyl group, 5-methylhexyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 1,1-dimethylpentyl group, 1,2-dimethylpentyl group, 1,3-dimethylpentyl group, 2,2-dimethylpentyl group, 2,3-dimethylpentyl group, 2-ethylpentyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylhept ... ethylheptyl, 5-methylheptyl, 6-methylheptyl, 1,1-dimethylhexyl, 1,2-dimethylhexyl, 1,3-dimethylhexyl, 1,4-dimethylhexyl, 1,5-dimethylhexyl, 1-ethylhexyl, 2-ethylhexyl, 1-methyloctyl, 2-methyloctyl, 3-methyloctyl, 4-methyloctyl, 5-methyloctyl, 6-methyloctyl, 7-methyloctyl, 1,1-dimethylheptyl, 1,2-dimethylheptyl, 1,3-dimethyl heptyl group, 1,4-dimethylheptyl group, 1,5-dimethylheptyl group, 1,6-dimethylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, 1-methylnonyl group, 2-methylnonyl group, 3-methylnonyl group, 4-methylnonyl group, 5-methylnonyl group, 6-methylnonyl group, 7-methylnonyl group, 8-methylnonyl group, 1,1-dimethyloctyl group, 1,2-dimethyloctyl group, 1,3-dimethyloctyl group, 1,4-dimethyloctyl group, 1,5-dimethyloctyl group, 1,6-dimethyloctyl group, 1,7-dimethyloctyl group, 1-ethyloctyl group, 2-ethyloctyl group, 1-methyldecyl group, 2-methyldecyl group, 3-methyldecyl group, 4-methyldecyl group, 5-methyldecyl group, 6-methyldecyl group, 7-methyldecyl group, 8-methyldecyl group, 9-methyldecyl group, 1,1-dimethylnonyl group, 1,2-dimethylnonyl group, 1,3-dimethylnonyl group, 1,4-dimethylnonyl group, 1,5-dimethylnonyl group, 1,6-dimethylnonyl group, 1,7-dimethylnonyl group, 1,8-dimethylnonyl group, 1-ethylnonyl group, 2-ethylnonyl group, 1-methylundecyl group, Examples of the decyl group include 2-methylundecyl group, 3-methylundecyl group, 4-methylundecyl group, 5-methylundecyl group, 6-methylundecyl group, 7-methylundecyl group, 8-methylundecyl group, 9-methylundecyl group, 10-methylundecyl group, 1,1-dimethyldecyl group, 1,2-dimethyldecyl group, 1,3-dimethyldecyl group, 1,4-dimethyldecyl group, 1,5-dimethyldecyl group, 1,6-dimethyldecyl group, 1,7-dimethyldecyl group, 1,8-dimethyldecyl group, 1,9-dimethyldecyl group, 1-ethyldecyl group, and 2-ethyldecyl group. From the viewpoints of lowering the glass transition temperature of the polymer compound to impart adhesion and favorably imparting mechanical strength to the positive electrode, a 2-ethylhexyl group or a dodecyl group (lauryl group) is preferred.
[0019] The total weight proportion of (meth)acrylic acid and alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms in the polymer compound is preferably 85% by weight or more based on the total weight of the constituent monomers of the polymer. When the total weight ratio of (meth)acrylic acid and alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms is within the above range, the strength of the positive electrode can be suitably imparted. The total weight proportion of the (meth)acrylic acid and the alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms in the polymer compound is preferably 99% by weight or less, and more preferably 95% by weight or less, based on the total weight of the constituent monomers of the polymer.
[0020] The polymer compound may contain lithium styrene sulfonate as one of the monomers constituting the polymer, or may contain a polymer made of lithium styrene sulfonate and a polymer made of a monomer other than lithium styrene sulfonate. When the polymer comprises lithium styrene sulfonate and a polymer comprised of a monomer other than lithium styrene sulfonate, the weight ratio of the polymer comprised of lithium styrene sulfonate to the total weight of the polymer comprised of lithium styrene sulfonate and the polymer comprised of a monomer other than lithium styrene sulfonate is preferably in the range of 1 to 15% by weight, more preferably 5% by weight or more, and even more preferably 10% by weight or more.
[0021] The polymer compound may contain other monomers as long as the effects of the present invention are not impaired. As the other monomer, for example, monomers used in the resin for coating an active material in JP2017-054703A and WO2015-005117A can be appropriately selected and used.
[0022] The polymer compound can be produced by a known polymerization method (bulk polymerization, solution polymerization, emulsion polymerization, suspension polymerization, etc.) using, for example, a known polymerization initiator {azo initiator [2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-methylpropionamidine) dihydrochloride, etc.], peroxide initiator (benzoyl peroxide, di-t-butyl peroxide, lauryl peroxide, etc.), etc.}. The amount of the polymerization initiator used is preferably 0.01 to 5% by weight, more preferably 0.05 to 2% by weight, and even more preferably 0.1 to 1.5% by weight based on the total weight of the monomers, from the viewpoint of adjusting the weight average molecular weight within a preferred range, and the polymerization temperature and polymerization time are adjusted depending on the type of polymerization initiator, etc., but the polymerization temperature is preferably -5 to 150°C (more preferably 30 to 120°C), and the reaction time is preferably 0.1 to 50 hours (more preferably 2 to 24 hours).
[0023] Examples of the solvent used in the case of solution polymerization include esters (having 2 to 8 carbon atoms, such as ethyl acetate and butyl acetate), alcohols (having 1 to 8 carbon atoms, such as methanol, ethanol, and octanol), hydrocarbons (having 4 to 8 carbon atoms, such as n-butane, cyclohexane, and toluene), amides (such as N,N-dimethylformamide (hereinafter abbreviated as DMF)), and ketones (having 3 to 9 carbon atoms, such as methyl ethyl ketone). From the viewpoint of adjusting the weight average molecular weight to a preferred range, the amount of the solvent used is preferably 5 to 900% by weight, more preferably 10 to 400% by weight, and even more preferably 30 to 300% by weight based on the total weight of the monomers, and the monomer concentration is preferably 10 to 95% by weight, more preferably 20 to 90% by weight, and even more preferably 30 to 80% by weight.
[0024] Examples of the dispersion medium in the emulsion polymerization and suspension polymerization include water, alcohol (e.g., ethanol), ester (e.g., ethyl propionate), light naphtha, etc., and examples of the emulsifier include metal salts of higher fatty acids (having 10 to 24 carbon atoms) (e.g., sodium oleate and sodium stearate), metal salts of higher alcohol (having 10 to 24 carbon atoms) sulfate (e.g., sodium lauryl sulfate), ethoxylated tetramethyldecynediol, sodium sulfoethyl methacrylate, dimethylaminomethyl methacrylate, etc. Furthermore, polyvinyl alcohol, polyvinylpyrrolidone, etc. may be added as a stabilizer. The monomer concentration in the solution or dispersion is preferably 5 to 95% by weight, more preferably 10 to 90% by weight, and even more preferably 15 to 85% by weight, and the amount of the polymerization initiator used is preferably 0.01 to 5% by weight, more preferably 0.05 to 2% by weight, based on the total weight of the monomers. In the polymerization, known chain transfer agents such as mercapto compounds (dodecyl mercaptan, n-butyl mercaptan, etc.) and / or halogenated hydrocarbons (carbon tetrachloride, carbon tetrabromide, benzyl chloride, etc.) can be used.
[0025] The polymer compound may be a crosslinked polymer obtained by crosslinking the polymer compound with a crosslinking agent (A') having a reactive functional group that reacts with a carboxyl group {preferably a polyepoxy compound (a'1) [polyglycidyl ether (bisphenol A diglycidyl ether, propylene glycol diglycidyl ether, glycerin triglycidyl ether, etc.), polyglycidylamine (N,N-diglycidylaniline, 1,3-bis(N,N-diglycidylaminomethyl)), etc.] and / or a polyol compound (a'2) (ethylene glycol, etc.)}.
[0026] As a method of crosslinking a polymer compound by using a crosslinking agent (A'), a method of coating a positive electrode active material particle with a polymer compound and then crosslinking the polymer compound can be mentioned.Specifically, a method of producing a coated positive electrode active material by mixing a resin solution containing a positive electrode active material particle and a polymer compound and removing the solvent, and then mixing a solution containing a crosslinking agent (A') with the coated positive electrode active material and heating the solution to cause desolvation and crosslinking reaction, and a reaction of crosslinking the polymer compound by the crosslinking agent (A') can be mentioned on the surface of the positive electrode active material particle. The heating temperature is adjusted depending on the type of crosslinking agent, but is preferably 70°C or higher when a polyepoxy compound (a'1) is used as the crosslinking agent, and is preferably 120°C or higher when a polyol compound (a'2) is used.
[0027] The lower limit of the weight average molecular weight of the polymer compound is preferably 3,000, more preferably 5,000, and still more preferably 7,000. On the other hand, the upper limit of the weight average molecular weight of the polymer compound is preferably 100,000, and more preferably 70,000.
[0028] The weight average molecular weight of the polymer compound can be determined by gel permeation chromatography (hereinafter abbreviated as GPC) measurement under the following conditions. Apparatus: Alliance GPC V2000 (Waters) Solvent: orthodichlorobenzene, DMF, THF Standard material: polystyrene Sample concentration: 3mg / ml Column stationary phase: PLgel 10 μm, MIXED-B 2 columns in series (Polymer Laboratories) Column temperature: 135℃
[0029] (Conductive assistant) From the viewpoint of internal resistance and the like, the coating layer preferably contains a conductive assistant. The conductive assistant is preferably selected from materials having electrical conductivity. Preferred conductive assistants include metals [aluminum, stainless steel (SUS), silver, gold, copper, titanium, etc.], carbon [graphite and carbon black (acetylene black, ketjen black, furnace black, channel black, thermal lamp black, etc.)], and mixtures thereof. These conductive assistants may be used alone or in combination of two or more, and may also be used as alloys or metal oxides thereof. Among these, from the viewpoint of electrical stability, aluminum, stainless steel, carbon, silver, gold, copper, titanium and mixtures thereof are more preferable, silver, gold, aluminum, stainless steel and carbon are further preferable, and carbon is particularly preferable. Furthermore, these conductive assistants may be formed by coating a particulate ceramic material or a resin material with a conductive material (preferably a metal one of the conductive assistants described above) by plating or the like.
[0030] The shape (form) of the conductive additive is not limited to a particulate form, and may be a form other than a particulate form, and may be a form that is in practical use as a so-called filler-based conductive additive, such as carbon nanofibers or carbon nanotubes.
[0031] The average particle size of the conductive assistant is not particularly limited, but from the viewpoint of the electrical characteristics of the battery, it is preferably about 0.01 to 10 μm. In this specification, the "particle diameter of the conductive assistant" refers to the maximum distance L between any two points on the contour line of the conductive assistant. The value of the "average particle diameter" is calculated as the average value of particle diameters of particles observed in several to several tens of fields of view using an observation means such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM).
[0032] The ratio of the polymer compound to the conductive assistant is not particularly limited, but from the viewpoint of the internal resistance of the battery, etc., the weight ratio of the polymer compound (resin solid content weight):conductive assistant is preferably 1:0.01 to 1:50, and more preferably 1:0.2 to 1:3.0.
[0033] (Method of manufacturing coated positive electrode active material for lithium ion batteries)
[0034] The coated positive electrode active material for lithium ion batteries of the present invention can be obtained by coating positive electrode active material particles with a coating layer containing a polymer compound and a conductive assistant. For example, the positive electrode active material particles are placed in a universal mixer and stirred at 30 to 500 rpm, and a resin solution containing the polymer compound that constitutes the coating layer is added dropwise over 1 to 90 minutes to mix, and the conductive assistant is mixed in. The mixture is heated to 50 to 200°C while still stirring, and the pressure is reduced to 0.007 to 0.04 MPa, and the mixture is maintained for 10 to 150 minutes to remove the solvent.
[0035] The blending ratio of the positive electrode active material particles to the polymer compound constituting the coating layer and the resin composition containing the conductive assistant is not particularly limited, but it is preferable that the weight ratio of the positive electrode active material particles:resin composition is 1:0.001 to 0.1.
[0036] At least a part of the surface of the positive electrode active material particles may be covered with a coating layer. From the viewpoint of cycle characteristics, the positive electrode active material particles preferably have a coverage rate, calculated by the following formula, of 30 to 95%. Coverage rate (%) = {1 - [BET specific surface area of coated positive electrode active material / (BET specific surface area of positive electrode active material particles × weight ratio of positive electrode active material particles contained in coated positive electrode active material + BET specific surface area of conductive additive × weight ratio of conductive additive contained in coated positive electrode active material)]} × 100
[0037] <Lithium-ion battery> The lithium ion battery of the present invention has the coated positive electrode active material for lithium ion batteries of the present invention. The lithium ion battery of the present invention comprises a positive electrode, a separator, and a negative electrode.
[0038] (positive electrode) The positive electrode comprises a positive electrode active material layer containing the coated positive electrode active material for lithium ion batteries of the present invention and an electrolytic solution containing an electrolyte and a solvent. In the positive electrode active material layer, the coated positive electrode active material for lithium ion batteries of the present invention preferably accounts for 40 to 95% by weight, and more preferably 60 to 90% by weight, based on the weight of the positive electrode active material layer.
[0039] As the electrolyte, electrolytes used in known electrolytic solutions can be used, for example, lithium salts of inorganic anions such as LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, and LiN(FSO2)2, and lithium salts of organic anions such as LiN(CF3SO2)2, LiN(C2F5SO2)2, and LiC(CF3SO2)3. Of these, LiN(FSO2)2 is preferred from the viewpoint of battery output and charge / discharge cycle characteristics.
[0040] As the solvent, a non-aqueous solvent used in a known electrolytic solution can be used, for example, a lactone compound, a cyclic or chain carbonate ester, a chain carboxylate ester, a cyclic or chain ether, a phosphate ester, a nitrile compound, an amide compound, a sulfone, a sulfolane, and a mixture thereof can be used.
[0041] Examples of the lactone compound include lactone compounds having a five-membered ring (such as γ-butyrolactone and γ-valerolactone) and a six-membered ring (such as δ-valerolactone).
[0042] Examples of the cyclic carbonate ester include propylene carbonate, ethylene carbonate (EC), and butylene carbonate (BC). Examples of the chain carbonate ester include dimethyl carbonate (DMC), methyl ethyl carbonate (MEC), diethyl carbonate (DEC), methyl-n-propyl carbonate, ethyl-n-propyl carbonate, and di-n-propyl carbonate.
[0043] Examples of the chain carboxylate include methyl acetate, ethyl acetate, propyl acetate, and methyl propionate.
[0044] Examples of cyclic ethers include tetrahydrofuran, tetrahydropyran, 1,3-dioxolane, and 1,4-dioxane. Examples of chain ethers include dimethoxymethane and 1,2-dimethoxyethane.
[0045] Examples of phosphate esters include trimethyl phosphate, triethyl phosphate, ethyl dimethyl phosphate, diethyl methyl phosphate, tripropyl phosphate, tributyl phosphate, tri(trifluoromethyl) phosphate, tri(trichloromethyl) phosphate, tri(trifluoroethyl) phosphate, tri(triperfluoroethyl) phosphate, 2-ethoxy-1,3,2-dioxaphospholan-2-one, 2-trifluoroethoxy-1,3,2-dioxaphospholan-2-one, and 2-methoxyethoxy-1,3,2-dioxaphospholan-2-one.
[0046] Examples of the nitrile compound include acetonitrile, etc. Examples of the amide compound include DMF, etc. Examples of the sulfone include dimethyl sulfone and diethyl sulfone, etc.
[0047] These solvents may be used alone or in combination of two or more.
[0048] The concentration of the electrolyte in the electrolytic solution is preferably 1.2 to 5.0 mol / L, more preferably 1.5 to 4.5 mol / L, further preferably 1.8 to 4.0 mol / L, and particularly preferably 2.0 to 3.5 mol / L. Such an electrolyte has an appropriate viscosity and can form a liquid film between the coated positive electrode active materials, thereby imparting a lubricating effect (position adjustment ability of the coated positive electrode active material) to the coated positive electrode active material.
[0049] The positive electrode active material layer may further contain a conductive assistant in addition to the conductive assistant contained as necessary in the coating layer of the above-mentioned coated positive electrode active material. The conductive assistant contained as necessary in the coating layer is integral with the coated positive electrode active material, whereas the conductive assistant contained in the positive electrode active material layer is contained separately from the coated positive electrode active material. As the conductive assistant that may be contained in the positive electrode active material layer, those described in [Coated positive electrode active material for lithium ion batteries] can be used.
[0050] When the positive electrode active material layer contains a conductive assistant, the total content of the conductive assistant contained in the positive electrode and the conductive assistant contained in the coating layer is preferably less than 4 wt % and more preferably less than 3 wt % based on the weight of the positive electrode active material layer excluding the electrolyte solution, while the total content of the conductive assistant contained in the positive electrode and the conductive assistant contained in the coating layer is preferably 2.5 wt % or more based on the weight of the positive electrode active material layer excluding the electrolyte solution.
[0051] The positive electrode active material layer preferably does not contain a binder. In this specification, the binder refers to an agent that cannot reversibly fix positive electrode active material particles to each other or to a current collector, and examples of such binders include known solvent-drying binders for lithium ion batteries, such as starch, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, polyvinylpyrrolidone, tetrafluoroethylene, styrene-butadiene rubber, polyethylene, and polypropylene. These binders are used by dissolving or dispersing in a solvent, and are solidified by volatilizing or distilling off the solvent, thereby irreversibly fixing the positive electrode active material particles to each other and between the positive electrode active material particles and the current collector.
[0052] The positive electrode active material layer may contain an adhesive resin. The adhesive resin means a resin that has adhesiveness and does not solidify even when the solvent component is evaporated and dried, and is a material different from a binder and is to be distinguished from it. In addition, the coating layer constituting the coated positive electrode active material is fixed to the surface of the positive electrode active material particles, whereas the adhesive resin reversibly fixes the surfaces of the positive electrode active material particles to each other. The adhesive resin can be easily separated from the surface of the positive electrode active material particles, but the coating layer cannot be easily separated. Therefore, the coating layer and the adhesive resin are different materials.
[0053] The adhesive resin may be a polymer containing at least one low Tg monomer selected from the group consisting of vinyl acetate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, butyl acrylate, and butyl methacrylate as an essential constituent monomer, in which the total weight ratio of the low Tg monomer is 45% by weight or more based on the total weight of the constituent monomers. When an adhesive resin is used, it is preferable to use 0.01 to 10% by weight of the adhesive resin based on the total weight of the positive electrode active material particles.
[0054] From the viewpoint of battery performance, the thickness of the positive electrode active material layer is preferably 150 to 600 μm, and more preferably 200 to 450 μm.
[0055] The positive electrode active material layer can be prepared, for example, by applying a positive electrode active material layer slurry containing the coated positive electrode active material of the present invention, an electrolyte solution containing an electrolyte and a solvent, and, if necessary, a conductive assistant, to a current collector, followed by drying. Specifically, the positive electrode active material layer slurry is applied to a current collector using a coating device such as a bar coater, and then a nonwoven fabric is placed on the positive electrode active material particles to absorb the liquid, thereby removing the solvent, and if necessary, pressing with a press.
[0056] Examples of materials constituting the current collector include metal materials such as copper, aluminum, titanium, stainless steel, nickel, and alloys thereof, as well as baked carbon, conductive polymer materials, conductive glass, and the like. The shape of the current collector is not particularly limited, and may be a sheet-like current collector made of the above-mentioned material, or a deposition layer made of fine particles made of the above-mentioned material. The thickness of the current collector is not particularly limited, but is preferably 50 to 500 μm.
[0057] The positive electrode for a lithium ion battery preferably further comprises a current collector, and the positive electrode active material layer is provided on the surface of the current collector. For example, the positive electrode of the present invention preferably comprises a resin current collector made of a conductive polymer material, and the positive electrode active material layer is provided on the surface of the resin current collector.
[0058] The conductive polymer material constituting the resin collector may be, for example, a resin to which a conductive material has been added. As the conductive material constituting the conductive polymer material, the same conductive assistant as the optional component of the coating layer can be suitably used. Examples of resins that constitute the conductive polymer material include polyethylene (PE), polypropylene (PP), polymethylpentene (PMP), polycycloolefin (PCO), polyethylene terephthalate (PET), polyethernitrile (PEN), polytetrafluoroethylene (PTFE), styrene butadiene rubber (SBR), polyacrylonitrile (PAN), polymethyl acrylate (PMA), polymethyl methacrylate (PMMA), polyvinylidene fluoride (PVdF), epoxy resin, silicone resin, and mixtures thereof. From the viewpoint of electrical stability, polyethylene (PE), polypropylene (PP), polymethylpentene (PMP) and polycycloolefin (PCO) are preferred, and polyethylene (PE), polypropylene (PP) and polymethylpentene (PMP) are more preferred. The resin current collector can be obtained by a known method described in, for example, JP 2012-150905 A and WO 2015 / 005116 A.
[0059] (Separator) Examples of the separator include known separators for lithium ion batteries, such as porous films made of polyethylene or polypropylene, laminated films of porous polyethylene film and porous polypropylene, nonwoven fabrics made of synthetic fibers (polyester fibers, aramid fibers, etc.) or glass fibers, and those having ceramic particles such as silica, alumina, titania, etc. attached to their surfaces.
[0060] (Negative electrode) The negative electrode includes a negative electrode current collector and a negative electrode active material layer.
[0061] As the negative electrode current collector, a known metal current collector and a resin current collector composed of a conductive resin composition containing a conductive material and a resin (such as the resin current collectors described in JP 2012-150905 A and WO 2015-005116 A, etc.) can be used. From the viewpoint of battery characteristics and the like, the negative electrode current collector is preferably a resin current collector. The thickness of the negative electrode current collector is not particularly limited, but is preferably 5 to 150 μm.
[0062] The negative electrode active material layer contains negative electrode active material particles. Examples of the negative electrode active material particles include carbon-based materials [graphite, non-graphitizable carbon, amorphous carbon, resin baked bodies (e.g., phenolic resin, furan resin, etc. baked and carbonized), cokes (e.g., pitch coke, needle coke, petroleum coke, etc.), and carbon fibers, etc.], silicon-based materials [silicon, silicon oxide (SiOx), silicon-carbon composites (carbon particles whose surfaces are coated with silicon and / or silicon carbide, silicon particles or silicon oxide particles whose surfaces are coated with carbon and / or silicon carbide, and silicon carbide, etc.), and silicon alloys (silicon-aluminum Examples of the conductive materials include: conductive polymers (e.g., polyacetylene and polypyrrole), metals (tin, aluminum, zirconium and titanium), metal oxides (titanium oxide and lithium-titanium oxide), metal alloys (e.g., lithium-tin alloy, lithium-aluminum alloy and lithium-aluminum-manganese alloy), and mixtures of these with carbon-based materials. These negative electrode active material particles may be used alone or in combination of two or more kinds.
[0063] From the viewpoint of the electrical characteristics of the battery, the volume average particle diameter of the negative electrode active material particles is preferably 0.01 to 100 μm, more preferably 0.1 to 20 μm, and even more preferably 2 to 10 μm.
[0064] The negative electrode active material particles may be a coated negative electrode active material in which at least a part of the surface thereof is coated with a coating layer containing a polymer compound. When the negative electrode active material particles are covered with a coating layer, the volume change of the negative electrode is alleviated, and the expansion of the negative electrode can be suppressed.
[0065] As the coating layer, the same coating layer as described in the coated positive electrode active material for lithium ion batteries of the present invention can be suitably used.
[0066] The negative electrode active material layer preferably does not contain a binder. The binder has the same meaning as described above for the positive electrode.
[0067] The negative electrode active material layer may contain an adhesive resin. As the adhesive resin, the same adhesive resin as the optional component of the positive electrode active material layer can be suitably used.
[0068] The negative electrode active material layer may contain a conductive assistant. As the conductive assistant, a conductive material similar to the conductive filler contained in the positive electrode active material layer can be suitably used. The weight ratio of the conductive assistant in the negative electrode active material layer is preferably 2 to 10% by weight.
[0069] The negative electrode active material layer may contain an electrolyte. As the electrolyte, any of those described in the positive electrode active material layer can be appropriately selected and used.
[0070] The negative electrode active material layer can be prepared, for example, by a method in which a mixture containing negative electrode active material particles and an electrolyte is applied to the surface of a negative electrode current collector or a substrate, and excess electrolyte is removed. When the negative electrode active material layer is formed on the surface of the substrate, the negative electrode active material layer may be combined with the negative electrode current collector by a method such as transfer. If necessary, the mixture may contain a conductive assistant, an adhesive resin, etc. The negative electrode active material particles may be a coated negative electrode active material.
[0071] The thickness of the negative electrode active material layer is not particularly limited, but from the viewpoint of battery performance, it is preferably 150 to 600 μm, and more preferably 200 to 450 μm.
[0072] (Lithium-ion battery manufacturing method) The lithium ion battery of the present invention can be produced, for example, by stacking a positive electrode, a separator and a negative electrode in this order, and then injecting an electrolyte solution as necessary. EXAMPLES
[0073] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples as long as they do not deviate from the gist of the present invention. In addition, unless otherwise specified, parts means parts by weight and % means % by weight.
[0074] Example 1 <Preparation of polymer compound for coating positive electrode> A four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen gas inlet tube was charged with 150 parts of DMF and heated to 75°C. Next, a monomer composition in which 15 parts of lithium styrenesulfonate, 10 parts of acrylic acid and 75 parts of 2-ethylhexyl acrylate were dissolved in 50 parts of DMF, and an initiator solution in which 0.1 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) and 0.4 parts of 2,2'-azobis(2-methylbutyronitrile) were dissolved in 30 parts of DMF were continuously dropped into the four-neck flask with stirring over 2 hours using a dropping funnel to carry out radical polymerization while blowing nitrogen into the flask. After the dropping was completed, the temperature was raised to 80°C and the reaction was continued for 2 hours. The temperature was then raised to 85° C. and the reaction was continued for 2 hours, and then further raised to 95° C. and the reaction was continued for 1 hour to obtain a polymer solution (polymer compound solution for coating positive electrodes) with a resin concentration of 30%.
[0075] <Preparation of polymer compound for coating negative electrode> A four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen gas inlet tube was charged with 150 parts of DMF and heated to 65 ° C. Next, a monomer composition in which 90 parts of acrylic acid and 10 parts of methyl methacrylate were dissolved in 50 parts of DMF and an initiator solution in which 0.1 parts of 2,2'-azobis (2,4-dimethylvaleronitrile) were dissolved in 30 parts of DMF were continuously dropped into the four-neck flask with a dropping funnel over 2 hours while blowing nitrogen into the flask, and radical polymerization was performed. After the dropping was completed, the temperature was raised to 70 ° C. and the reaction was continued for 2 hours. Next, the temperature was raised to 80 ° C. and the reaction was continued for 2 hours, and a polymer solution (polymer compound solution for negative electrode coating) with a resin concentration of 30% was obtained.
[0076] <Preparation of coated positive electrode active material for lithium-ion batteries> 84 parts of positive electrode active material particles (lithium manganate powder, volume average particle diameter 4 μm) were placed in a universal mixer, high speed mixer FS25 [manufactured by EarthTechnica Corporation], and while stirring at room temperature and 720 rpm, 8 parts of the positive electrode coating polymer compound solution were added dropwise over 2 minutes, and the mixture was further stirred for 5 minutes. Next, while stirring, 3 parts of acetylene black (Denka Black (registered trademark) manufactured by Denka Co., Ltd.) as a conductive additive and 3 parts of graphite powder (product name "flake graphite" manufactured by Nippon Graphite Co., Ltd.) were added in portions over a period of 2 minutes, and stirring was continued for 30 minutes. Thereafter, the pressure was reduced to 0.01 MPa while continuing stirring, and then the temperature was raised to 140°C while continuing stirring and reducing pressure, and the stirring, reducing pressure and temperature were maintained for 8 hours to distill off the volatile matter. The obtained powder was classified using a sieve with an opening of 200 μm to prepare a coated positive electrode active material for lithium ion batteries.
[0077] <Preparation of coated negative electrode active material for lithium ion batteries> 80 parts of negative electrode active material particles [non-graphitizable carbon (hard carbon), manufactured by Kureha Battery Materials Japan, Ltd., Carbotron (registered trademark) PS(F)] were placed in a universal mixer, high-speed mixer FS25 [manufactured by EarthTechnica Corporation], and while stirring at room temperature and 720 rpm, 11 parts of the negative electrode coating polymer compound solution were added dropwise over 2 minutes, and the mixture was further stirred for 5 minutes. Next, while stirring, 9 parts of acetylene black (Denka Black (registered trademark) manufactured by Denka Co., Ltd.) serving as a conductive assistant was added in portions over a period of 2 minutes, and stirring was continued for 30 minutes. Thereafter, the pressure was reduced to 0.01 MPa while continuing stirring, and then the temperature was raised to 140°C while continuing stirring and reducing pressure, and the stirring, reducing pressure and temperature were maintained for 8 hours to distill off the volatile matter. The obtained powder was classified using a sieve with an opening of 200 μm to prepare a coated negative electrode active material for a lithium ion battery.
[0078] <Preparation of resin collector> A resin mixture was obtained by melt-kneading 70 parts of polypropylene [product name: "SunAllomer PL500A", manufactured by SunAllomer Co., Ltd.], 25 parts of carbon nanotubes [product name: "FloTube9000", manufactured by CNano Corporation], and 5 parts of a dispersant [product name: "UMEX 1001", manufactured by Sanyo Chemical Industries, Ltd.] in a twin-screw extruder at 200°C and 200 rpm. The obtained resin mixture was passed through a T-die extrusion film molding machine and stretched and rolled to obtain a conductive film for resin current collector with a thickness of 100 μm. Next, the obtained conductive film for resin current collector was cut to 17.0 cm × 17.0 cm, and nickel was vapor-deposited on one side, and then a resin current collector was produced by connecting a terminal (5 mm × 3 cm) for taking out current.
[0079] <Preparation of positive electrodes for lithium-ion batteries> An electrolyte was prepared by dissolving LiN(FSO2)2 at a ratio of 2.0 mol / L in a mixed solvent of ethylene carbonate (EC) and propylene carbonate (PC) (volume ratio 1:1). 42 parts of the electrolyte and 4.2 parts of carbon fiber [DonaCarbo Milled S-243, manufactured by Osaka Gas Chemicals Co., Ltd.: average fiber length 500 μm, average fiber diameter 13 μm: electrical conductivity 200 mS / cm] were mixed for 5 minutes at 2000 rpm using a planetary stirring type mixer and kneader {Awatori Rentaro [manufactured by Thinky Corporation]}, followed by adding 30 parts of the electrolyte and 206 parts of the coated positive electrode active material for lithium ion batteries, and then mixing for 2 minutes at 2000 rpm with the Awatori Rentaro, adding 20 parts of the electrolyte, and then stirring with the Awatori Rentaro at 2000 rpm for 1 minute, and then adding 2.3 parts of the electrolyte, and then stirring with the Awatori Rentaro at 2000 rpm for 2 minutes to prepare a slurry for a positive electrode active material layer. The obtained slurry for a positive electrode active material layer had a basis weight of 80 mg / cm 2 The mixture was applied to one side of the resin collector so as to obtain the above composition, and pressed at a pressure of 1.4 MPa for approximately 10 seconds to produce a positive electrode for a lithium ion battery according to Example 1 (16.2 cm×16.2 cm) having a thickness of 340 μm.
[0080] <Preparation of negative electrodes for lithium-ion batteries> 42 parts of the electrolyte and 4.2 parts of carbon fiber [DonaCarbo Milled S-243, manufactured by Osaka Gas Chemicals Co., Ltd.: average fiber length 500 μm, average fiber diameter 13 μm: electrical conductivity 200 mS / cm] were mixed for 5 minutes at 2000 rpm using a planetary stirring type mixer and kneader {Awatori Rentaro [manufactured by Thinky Corporation]}, followed by adding 30 parts of the electrolyte and 206 parts of the coated negative electrode active material for lithium ion batteries, and further mixing for 2 minutes at 2000 rpm with the Awatori Rentaro, further adding 20 parts of the electrolyte, and further mixing with the Awatori Rentaro at 2000 rpm for 1 minute, further adding 2.3 parts of the electrolyte, and further mixing with the Awatori Rentaro at 2000 rpm for 2 minutes to prepare a slurry for a negative electrode active material layer. The obtained slurry for a negative electrode active material layer had a basis weight of 23 mg / cm 2 The mixture was applied to one side of the resin collector so as to obtain the above composition, and pressed at a pressure of 1.4 MPa for approximately 10 seconds to prepare a negative electrode for a lithium ion battery according to Example 1 (17.0 cm×17.0 cm) having a thickness of 400 μm.
[0081] [Making a lithium-ion battery] The obtained positive electrode was combined with the obtained negative electrode via a separator (#3501 manufactured by Celgard) to prepare a laminate cell.
[0082] (Examples 2 to 7, Comparative Examples 1 to 6) Each coated positive electrode active material for a lithium ion battery was prepared in the same manner as in Example 1, except that the monomer used in preparing the positive electrode coating polymer compound was changed to the type and amount (wt%) of the monomer shown in Table 1, and that in Example 4 and Comparative Example 5, the solvent was changed from DMF to toluene. A positive electrode for a lithium ion battery and a lithium ion battery were produced in the same manner as in Example 1, except that the produced coated positive electrode active materials for a lithium ion battery were used.
[0083] Example 8 <Preparation of polymer compound A for coating positive electrode> A four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen gas inlet tube was charged with 150 parts of toluene and heated to 75 ° C. Next, a monomer composition in which 95 parts of lauryl methacrylate and 5 parts of methacrylic acid were dissolved in 50 parts of toluene, and an initiator solution in which 0.1 parts of 2,2'-azobis (2,4-dimethylvaleronitrile) and 0.4 parts of 2,2'-azobis (2-methylbutyronitrile) were dissolved in 30 parts of toluene were continuously dropped into the four-neck flask with stirring over 2 hours using a dropping funnel to carry out radical polymerization while blowing nitrogen into the flask. After the dropping was completed, the reaction was continued for 3 hours at 75 ° C. Next, the temperature was raised to 80 ° C. and the reaction was continued for 3 hours to obtain a polymer solution (polymer compound A solution for covering positive electrodes) with a resin concentration of 30%.
[0084] <Preparation of polymer compound B for coating the positive electrode> A four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen gas inlet tube was charged with 150 parts of water and heated to 75°C. Next, a monomer composition in which 100 parts of lithium styrenesulfonate was dissolved in 50 parts of water and an initiator solution in which 0.2 parts of 2,2'-azobis(2-methylpropionamidine) dihydrochloride was dissolved in 30 parts of water were continuously dropped into the four-neck flask with a dropping funnel over a period of 2 hours while blowing nitrogen into the flask, and radical polymerization was carried out. After the dropping was completed, the reaction was continued for 3 hours at 75°C. Next, the temperature was raised to 80°C and the reaction was continued for 3 hours, to obtain a polymer solution with a resin concentration of 30%. The obtained polymer solution was transferred to a Teflon (registered trademark) vat and dried under reduced pressure at 100°C and 0.01 MPa for 3 hours, and the water was distilled off to obtain a polymer. This polymer was roughly crushed with a hammer and then further crushed in a mortar to prepare a powder of polymer compound B for coating the positive electrode.
[0085] <Lithium-ion battery> 86 parts of positive electrode active material particles (lithium manganate powder, volume average particle diameter 4 μm) were placed in a universal mixer, high speed mixer FS25 [manufactured by EarthTechnica Corporation], and while stirring at room temperature and 720 rpm, 7.2 parts of the positive electrode coating polymer compound A solution were added dropwise over 2 minutes, and the mixture was further stirred for 5 minutes. Next, while stirring, 3 parts of acetylene black (Denka Black (registered trademark) manufactured by Denka Co., Ltd.), 3 parts of graphite powder (product name "flake graphite" [manufactured by Nippon Graphite Co., Ltd.]), and 0.24 parts of powdered positive electrode coating polymer compound B were added in portions over a period of 2 minutes, and stirring was continued for 30 minutes. Thereafter, the pressure was reduced to 0.01 MPa while continuing stirring, and then the temperature was raised to 140°C while continuing stirring and reducing pressure, and the stirring, reducing pressure and temperature were maintained for 8 hours to distill off the volatile matter. The obtained powder was classified using a sieve with an opening of 200 μm to prepare a coated positive electrode active material for lithium ion batteries. A coated positive electrode active material for a lithium ion battery was produced in the same manner as in Example 1, except that the above-mentioned positive electrode coating polymer compounds A and B were used. A positive electrode for a lithium-ion battery and a lithium-ion battery were produced in the same manner as in Example 1, except that the produced coated positive electrode active material for a lithium-ion battery was used.
[0086] (Example 9) A coated positive electrode active material for a lithium-ion battery was produced in the same manner as in Example 8, except that the weight ratio (weight %) of the polymer compound A for positive electrode coating and the polymer compound B for positive electrode coating was changed as shown in Table 2. A positive electrode for a lithium-ion battery and a lithium-ion battery were produced in the same manner as in Example 1, except that the produced coated positive electrode active material for a lithium-ion battery was used.
[0087] <Measurement of Mn elution amount> The lithium-ion batteries produced in the examples and comparative examples were charged at a constant current of 0.05C to a voltage of 4.2V using a charge-discharge measurement device "Battery Analyzer 1470 type" [manufactured by Toyo Technica Co., Ltd.] at 25°C, and then charged at a constant voltage of 4.2V until the current value reached 0.01C. After a 10-minute rest, the battery was discharged at a constant current of 0.01C to a voltage of 2.5V and then charged at a constant current of 0.05C to a voltage of 4.2V. Next, the charged lithium-ion batteries were stored in a constant temperature bath at 60°C for two weeks. Thereafter, the coated negative electrode active material for a lithium-ion battery was taken out from each lithium-ion battery, and this was used as a sample for fluorescence X-ray analysis under the following conditions. Apparatus: Fluorescence X-ray analyzer Axios Manufacturer name: Spectris Co., Ltd. Sample: 200 mg of coated negative electrode active material particles for a lithium-ion battery Sample solution: 6 wt% EC / PC = 50 / 50 solution Measurement method: Rhus powder method Measurement container: PP cup and 2.5 μm thick Mylar film Analysis method: FP method (semi-quantitative analysis method) The ratio of the peak intensity of MnKα to the peak intensity of FeKα (Mn / Fe intensity ratio) was calculated and used as the Mn elution amount, and evaluated according to the following criteria. The results are shown in Table 1 and Table 2. The FeKα peak is derived from the negative electrode active material particles. (Evaluation Criteria) ◎: The Mn / Fe intensity ratio was 0.2 or less. ◯: The Mn / Fe intensity ratio was greater than 0.2 but less than 0.6. △: The Mn / Fe intensity ratio was more than 0.6 but less than 1. ×: The Mn / Fe intensity ratio exceeded 1.
[0088] <Impedance measurement> The lithium ion batteries prepared in the Examples and Comparative Examples were charged at 25° C. using a charge / discharge measuring device "Battery Analyzer 1470" [manufactured by Toyo Corporation] at a constant current of 0.05 C to a voltage of 4.2 V, and then charged at a constant voltage of 4.2 V until the current value reached 0.01 C. After a 10-minute break, the batteries were discharged at a constant current of 0.01 C to a voltage of 2.5 V, and then charged at a constant current of 0.05 C to a voltage of 4.2 V. Next, the charged lithium-ion battery was stored in a thermostatic chamber at 60° C. for one or two weeks. After that, the lithium ion batteries were transferred to a thermostatic chamber at 25°C after storage for one or two weeks, and measurements were taken using an "Impedance Analyzer 1280Z" [manufactured by Toyo Corporation], changing the frequency from 20,000 Hz to 1,000 Hz. The value at a frequency of 1,000 Hz was taken as the impedance value, and the results were evaluated according to the following criteria. The results are shown in Tables 1 and 2. (Evaluation criteria for impedance measurement after one week storage) ◎: 10 Ω or less. ○: Over 10 Ω but below 20 Ω. △: More than 20 Ω but less than 25 Ω. ×: Exceeded 25 Ω. (Evaluation criteria for impedance measurement after 2 weeks of storage) ◎: 15 Ω or less. ○: Over 15 Ω but below 30 Ω. △: More than 30 Ω but less than 40 Ω. ×: Exceeded 40 Ω.
[0089] <Three-point bending test> The positive electrodes for lithium ion batteries prepared in the Examples and Comparative Examples were subjected to a three-point bending test (conditions: test speed 2 mm / min, distance between supports 80 mm, indenter radius 5 mm, support table radius 5 mm) using a precision universal testing machine (Shimadzu Corporation, Autograph AG-Xplus) and evaluated according to the following criteria. The results are shown in Tables 1 and 2. (Evaluation Criteria) ◎: 0.1N or more. ○: 0.06N or more but less than 0.1N. △: 0.02N or more and less than 0.06N. ×: Less than 0.02N.
[0090] <Cycle test> The lithium ion batteries prepared in the Examples and Comparative Examples were charged to 4.2 V at a current of 0.1 C using a charge / discharge measuring device "Battery Analyzer 1470" [manufactured by Toyo Corporation] at 25°C, and after a 10-minute break, discharged to 2.5 V at a current of 0.1 C. This charge / discharge cycle was repeated 20 times. A graph of voltage drop (ΔV) - current (I) was created from the difference (ΔV) between the voltage at the start of discharge and the voltage 10 seconds after discharge and the current value (I) at 20 cycles, and the internal resistance R (Ω) at which ΔV = RI was calculated using the least squares method and evaluated according to the following criteria. The results are shown in Tables 1 and 2. (Evaluation Criteria) ◎: Less than 13 Ω. ○: Between 13Ω and 14Ω. △: 14 Ω or more and less than 14.5 Ω. ×: 14.5 Ω or more.
[0091] [Table 1]
[0092] [Table 2]
[0093] From Examples 1 to 9, it was confirmed that even if a manganese-based lithium metal oxide is used as the positive electrode active material particles, the elution of manganese from the positive electrode active material particles during charging and discharging can be suppressed, and the cycle characteristics of the lithium ion battery can be improved. [Industrial Applicability]
[0094] A lithium ion battery using the coated positive electrode active material for a lithium ion battery of the present invention is particularly useful as a lithium ion battery for use in mobile phones, personal computers, hybrid automobiles, and electric automobiles.
Claims
1. A coated positive electrode active material for a lithium ion battery, in which at least a part of the surface of a positive electrode active material particle is coated with a coating layer containing a polymer compound, the positive electrode active material particles include particles made of manganese-based lithium metal oxide, the polymer compound includes a polymer having lithium styrene sulfonate as a constituent monomer, The weight ratio of the lithium styrene sulfonate in the polymer compound is 1 to 15% by weight based on the total weight of the constituent monomers of the polymer. A coated positive electrode active material for a lithium ion battery.
2. A coated positive electrode active material for a lithium ion battery, in which at least a portion of the surface of a positive electrode active material particle is coated with a coating layer containing a polymer compound, the positive electrode active material particles include particles made of manganese-based lithium metal oxide, the polymer compound includes a polymer having lithium styrene sulfonate as a constituent monomer, The polymer compound contains at least one of (meth)acrylic acid and an alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms as a constituent monomer. A coated positive electrode active material for a lithium ion battery.
3. 3. The coated positive electrode active material for lithium ion batteries according to claim 2, wherein the weight ratio of the lithium styrene sulfonate in the polymer compound is 1 to 15% by weight based on the total weight of the constituent monomers of the polymer.
4. 4. The coated positive electrode active material for lithium ion batteries according to claim 2 or 3, wherein the total weight ratio of the (meth)acrylic acid and the alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms in the polymer compound is 85% by weight or more based on the total weight of the constituent monomers of the polymer.
5. A lithium ion battery comprising the coated positive electrode active material for lithium ion batteries according to any one of claims 1 to 4.
Citation Information
Patent Citations
Electrode for secondary battery and method for making same, and secondary battery using this electrode
JP2008235249A