METHOD FOR PRODUCING A MULTILAYER COMPOSITE FILM, MULTILAYER COMPOSITE FILM AND USE THEREOF
The described method addresses the challenges of shrinkage and property deficiencies in multilayer films by optimizing layer structures and processing conditions, resulting in stable, high-performance films for packaging.
Patent Information
- Application Number
- JP2023176716
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-03
- Filing Date
- 2023-10-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-04-30
AI Technical Summary
Existing multilayer films produced by coextrusion and biaxial stretching suffer from significant shrinkage (>5%) in the machine and transverse directions, lacking sufficient barrier, sealing properties, heat resistance, mechanical strength, and printability, and require complex and resource-intensive lamination processes.
A method involving coextrusion and biaxial orientation of films with specific layer structures, including a heat-sealable polyolefin innermost layer and a thermoplastic resin outermost layer, combined with controlled stretching and relaxation processes at optimized temperatures and durations to achieve minimal shrinkage (<5%) while maintaining properties like oxygen barrier, heat resistance, and printability.
The method produces stable, multilayer films with minimal shrinkage, enhanced barrier properties, and improved mechanical strength without lamination, suitable for packaging applications.
Smart Images

Figure 0007595727000023 
Figure 0007595727000024 
Figure 0007595727000025
Abstract
Description
[Technical field]
[0001] The present application relates to coextruded and biaxially stretched (biaxially oriented) multilayer films, which can be used, for example, as packaging materials, especially for foodstuffs, to processes for their production and to their use for packaging, preferably, foodstuffs, fine foodstuffs or liquid or solid, especially powdery, goods. However, the present application does not relate to laminated multilayer films and the corresponding production processes. [Background technology]
[0002] On the one hand, laminated multilayer films are known from the state of the art and are excellent packaging materials. Thus, laminates consisting of at least two or three or even more independently produced layers are widely used in the packaging market. A distinction is made between so-called "double" laminate films and so-called "triple" laminate films. "Double" laminate films are films extruded by cast or blow processes, which contain a barrier film having 5, 7 or 9 layers, and which are laminated together (glued or bonded) in a separate process with a biaxially oriented film of either polyethylene terephthalate (PET), polyamide (PA) or polypropylene (PP), which is also produced separately. So far, only with these films, which are produced and laminated in successive, separate process steps, can the sum of the desired and / or required properties be achieved. For example, two of the required properties (tightness and oxygen or odor barrier) are achieved by the extruded monolayer or multilayer film part, while the other properties, such as printability, heat resistance and mechanical strength, are achieved by the separately biaxially oriented film part. Moreover, it is also common practice to specifically achieve or increase the oxygen barrier by means of a metal coating applied in a further process step.
[0003] Examples of commonly used double layer films on the market: [Table 1]
[0004] [Table 2]
[0005] A "tri-laminate" film is similar in that the sum of the desired and / or required properties is produced in three films that are manufactured separately and then laminated (glued or bonded) together.
[0006] In this case, a biaxially oriented film made of PET, PA or PP is laminated with another aluminum foil and this composite is then laminated with an extrusion cast or blown film.
[0007] Here, the extrusion cast or blown film is responsible for the hermeticity, the aluminum foil for the barrier, and the biaxially oriented film for optimal printability, heat resistance and mechanical strength. The disadvantage of laminated films, however, is that their production is inherently complex, resource-intensive and expensive, and the entire composite film is often very thick, since multiple films must first be produced separately and then glued or joined by hot melt or liquid adhesives in several successive process steps to finally obtain the laminated multilayer film.
[0008] Examples of commonly used triple layer films on the market: [Table 3]
[0009] [Table 4] [Brief description of the drawings]
[0010] [Figure 1] Known double film. [Diagram 2] Known double film. [Diagram 3] Known double film. [Figure 4] Known double film. [Diagram 5] Known triple film. [Figure 6] Known triple film.
[0011] On the other hand, multilayer films are known from the state of the art and are produced by coextrusion and biaxial stretching or biaxial orientation. The production processes used for this purpose make it possible to produce multilayer films in only one process step by coextrusion, completely eliminating the subsequent bonding / lamination process of the individual film layers, with the associated disadvantages. At best, biaxial stretching of coextruded raw multilayer films is carried out to achieve the sum of the desired properties (sealability, heat resistance, barrier, mechanical strength, printability). Apart from sealability, many of the required properties, such as mechanical strength, heat resistance, printability and barrier (essentially oxygen or gas barrier), are achieved by using raw materials such as PET, PA, ethylene-vinyl alcohol copolymer (EVOH), polyvinyl alcohol (PVOH) or polylactic acid (PLA).
[0012] Thus, although materials such as EVOH, PVOH, PVDC and PA are preferably used to obtain oxygen or gas barrier, materials such as PET or PLA also provide significantly better barrier protection compared to polyolefin-based materials such as PE or PP, especially after orientation, ideally even after biaxial orientation.
[0013] Furthermore, PET and PA in particular are used in the outermost layers of the film to achieve particularly good heat resistance and excellent printability, especially after biaxial orientation.
[0014] In addition to their outstanding heat resistance, printability and good gas and oxygen barrier properties, PA and PET in particular also make a decisive contribution to maintaining the desired mechanical strength, especially after biaxial orientation.
[0015] Many composites in this regard are therefore known from the state of the art, for example from DE 10227580 A1, DE 10254172 A1, DE 102006046483 A1, DE 102006036844 A1, EP 0476836 A1, EP 1190847 A1, EP 1084035 A1 and EP 1985444 A1.
[0016] However, the embodiments and methods known from the state of the art have something in common, namely that all these coextruded multilayer barrier films generally have a relatively large shrinkage, usually more than 20%, in each case always more than 5%, in the machine direction (MD) and in the transverse direction (TD), respectively, which is advantageous or even desirable for many applications, e.g. shrink bag / lid films or cover films.
[0017] [Table 5]
[0018] [Table 6]
[0019] However, multilayer barrier films produced by coextrusion and biaxial orientation have relatively little or no shrinkage (less than 5%, preferably less than 3%) in the machine direction (MD) and transverse direction (TD), respectively, but to date have lacked sufficient barrier, airtightness, heat resistance, mechanical strength and printability. Summary of the Invention
[0020] It is therefore an object of the present invention to provide a method for producing a coextruded and biaxially oriented composite film, preferably a coextruded and biaxially oriented multilayer barrier film, and the resulting multilayer film, preferably a multilayer barrier film, which has at least one of the following properties, preferably all of the following properties: sufficient oxygen and / or water vapor barrier, hermeticity, heat resistance, printability, and mechanical strength, even without an additional lamination step. The resulting multilayer barrier film should further have relatively low or no shrinkage (less than 5%, preferably less than 3%) in the machine direction (MD) and in the transverse direction (TD), respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] From the state of the art and practical use, it is known that the outermost layer materials, such as PET and PA, achieve the best possible printability and maintain the best possible heat resistance.However, also materials, such as PLA or EVOH, are much more suitable than polyolefin-based pipe materials, such as PE or PP, in terms of printability, heat resistance and further processability.
[0022] [Table 7]
[0023] [Table 8]
[0024] [Table 9]
[0025] To obtain a sufficient barrier against oxygen or gas, raw materials such as PET, PA, EVOH, PVOH and PVDC are established.
[0026] [Table 10]
[0027] Source: Oxygen transmission rates at 20°C measured for various barrier plastics (Joachim Nentwig, Kunststoff-Folien, 3rd edition, 2006, Carl Hanser Verlag; Table 26 from Kyoichiro)
[0028] However, as is known to those skilled in the art, the barrier properties of many of these materials are only sufficient if they are properly protected against moisture.
[0029] Therefore, when these materials are provided with a barrier, they are always used in the middle or innermost layers of the film.
[0030] In order to obtain the best possible sealability, polyolefin-based materials, such as PE or PP, or similar, which have the lowest possible sealing temperature or melting point, as is known from practical experience, should be used in each case.
[0031] [Table 11]
[0032] It is noteworthy that the raw materials ideally used to achieve properties such as heat resistance, printability and oxygen barrier also have much higher strength, especially after biaxial stretching (=biaxial orientation), than polyolefins are even remotely capable of, despite the biaxial stretching.
[0033] In an optimal layer structure, the oxygen barrier layer should therefore be made of EVOH, PVOH or PA and should be located between one of the middle or intermediate and innermost sealant layers made of a heat-sealable polyolefin.
[0034] The outermost layer should be made of one of the ideal heat-resistant and printable materials for this purpose, such as PET or PA.
[0035] Looking closely at the materials that have advantageous properties such as heat resistance, printability, oxygen barrier, and strength, we see that all of the materials share various common characteristics, e.g., they all have a modulus of less than 1.0 g / cm 3 It is apparent that they all have higher densities, they are all polar materials, and they nearly all have melting points greater than 170°C.
[0036] Further consideration of the materials preferably used as the sealant layer, they all have a viscosity of 0.95 g / cm 3 It is also apparent that it has a density less than 100 nm and a melting point less than 120°C.
[0037] [Table 12]
[0038] 1.0g / cm 3 All of these materials have greater density, but are not equally ideal for printability like PA or PET, or for heat resistance like PET or PA. They do not all have equally high oxygen barriers like EVOH, PVOH or PA, and they do not all have equally increased strength like PA or PET. But they all show significantly improved properties in each of the individual properties, especially after biaxial orientation and when combined into composite films, much more so than polyolefin-based materials.
[0039] The heat resistance, printability and oxygen barrier properties of these materials are 1.0g / cm 3 Due to the different optimum characteristics of the raw material having a higher density and the resulting ideal or preferred distribution into at least two separate layers, this distribution leads to a further very positive effect, namely a partially significant increase in the strength and stiffness of the film.
[0040] This effect is 1.0 g / cm 3 This becomes more pronounced the further away two layers containing ingredients with greater density are from each other in the overall composite of layers.
[0041] Therefore, on the one hand, 1.0 g / cm 3 It is necessary to select a layer structure that includes at least two independent layers having a density greater than 0.95 g / cm, one of which forms the outermost layer and the other an intermediate layer. On the other hand, the composite film should include a heat-sealable layer that forms the innermost layer, and has a density of 0.95 g / cm. 3 The material should be made of a material having a density less than 100° C. and a melting point less than 120° C., preferably a polyolefin.
[0042] Although such a layer structure solves in an excellent manner the sum of the desired properties (in particular sufficient oxygen and / or water vapor barrier, hermeticity, heat resistance, printability and mechanical strength), in particular after biaxial stretching, the adjustment or setting of the desired low shrinkage, in particular after biaxial stretching, is not yet solved thereby.
[0043] This cannot be achieved on the raw material side alone, at least if the produced film is not subjected to biaxial orientation. This requires a suitable production method and / or suitable processing to meet this objective.
[0044] Especially after stretching, and especially after biaxial stretching, polymers or films made of polymers often have significant shrinkage that varies from polymer to polymer and necessarily depends on whether and how much heat or temperature has been applied to the film.
[0045] In other words, the higher the temperature and the longer the exposure time, the more the film will shrink.
[0046] To reduce the shrinkage of stretched films, processes and treatments are known from the prior art which are used for uniaxially stretched films, but also in particular for biaxially stretched films.
[0047] Particularly for uniaxially stretched films, but also for biaxially stretched films, post-treatments are known, i.e. treatments after the stretching step (=orientation step), in which the film is guided over temperature-controlled rolls (so-called tempering rolls) and the wrap is as high as possible, which introduces heat or temperature into the film, i.e. thermally fixes it and thus reduces the residual shrinkage.
[0048] In the stretching (=orientation) of flat films, the so-called tenter process, post-treatments (tempering), also known as thermo fixings or heat-settings (thermally fixed), are also known, in which the film passes vertically downstream of a heated oven after the centrifuge and is treated with hot air, thereby reducing the shrinkage.
[0049] Furthermore, thermal post-treatment following stretching is also known from the so-called triple-bubble or multi-bubble process for blown films, in which the film in tubular form passes through an oven and is treated at temperature, often with hot air, as in the tenter process, or the film is treated with infrared radiation or hot water vapor in the triple-bubble process to reduce the shrinkage caused by stretching.
[0050] Various techniques are known to reduce the shrinkage associated with biaxial orientation, for example by temperature application, however in addition to the degree of temperature applied the time or duration of the temperature effect is also an important factor here.
[0051] However, to reduce or even completely eliminate shrinkage in films, treating the film exclusively with heat / temperature is the only means and is sufficient for a few film types.
[0052] For example, films produced in the tenter process, such as BoPET, BoPA or BoPP (Bo = biaxial orientation = biaxial stretching), are stabilized by a very high heat treatment (thermo fixing), so that they contain little or no shrinkage.
[0053] The situation is similar for certain films that are biaxially stretched in the double bubble process and thermally fixed by tempering rollers or vertical hot air ovens, in which case especially BoPP or BoPA films are also often treated or fixed exclusively by temperature and exhibit little or no shrinkage.
[0054] This is because, regardless of the stretching process, these types of films are primarily mono-type films in which only one type of raw material is used: BoPET (exclusively PET), BoPA (exclusively PA), BoPP (exclusively PP).
[0055] In this case, a high heat setting temperature (relaxation temperature) just below the softening or melting point of the corresponding raw material can be selected for stabilization, so that shrinkage can be significantly reduced or even eliminated by temperature treatment alone.
[0056] Up until now, however, this has been thought to be impossible for film types made from various materials, ie different types of materials, especially materials with widely different softening or melting points.
[0057] In fact, for example, no coextruded or biaxially oriented film is known that contains a combination of various raw materials having widely differing softening or melting temperatures and yet has no or very little shrinkage despite stretching.
[0058] An exception to this is the stand-alone multilayer film produced by the tenter or double bubble process, which essentially contains the following layer structure (from inside to outside; HV=adhesion promoter):
[0059] PP-HV-EVOH-HV-P
[0060] Since homo-PP (homopolymer PP; melting point: 155-165°C) is almost exclusively used in combination with EVOH and EVOH types with high ethylene content and lower melting points (melting point: 170-180°C) than those with low ethylene content, these composites can almost exclusively be stabilized at similar temperatures by heat treatment, reducing or eliminating shrinkage.
[0061] However, these multilayer films based on PP, which consist mostly of PP, do not exhibit the desired heat resistance and certainly do not exhibit the required printability.
[0062] PP is not an ideal material to be used in the outermost layer, since even the most heat-resistant homo-PP types melt at temperatures below 170°C, and PP is also one of the most non-polar materials, making it completely unsuitable for printing without further post-treatment.
[0063] Furthermore, as is well known in the market, due to the fundamentally poor sealing properties of the PP types used and compared to preferred raw materials, such as PE, these PP-based multilayer films have only very poor or moderate sealability, i.e. relatively high sealing temperatures. Therefore, these films are subsequently conventionally laminated with PE-based films.
[0064] As a result, it is not currently believed possible to produce a multi-layer, coextruded and then biaxially oriented film that includes a sealant layer having a low melting point, which further includes an oxygen barrier layer disposed on a non-subsequently laminated, heat resistant and printable (polar) outer layer and an intermediate layer, and has no or minimal shrinkage.
[0065] This is because such multi-layer composites cannot be made stable at the temperatures required to eliminate or reduce shrinkage below 5%, or even below 3%, without further process measures, or can not be made at all.
[0066] Thus, even before the temperatures required to eliminate shrinkage are reached, the individual layers in the multi-layer composite will soften or even melt, inevitably disrupting or at least massively impairing the film manufacturing process.
[0067] When or how often the process is lost or even interrupted is determined by the fact that the layer portion of the entire film composite is less than 1.00 g / cm 3 It depends on whether and how many layers it is made of non-polyolefinic materials, i.e. temperature resistant materials, having a higher density and a melting point above 170°C.
[0068] 1.00g / cm 3 If the mass proportion of materials with a higher density is greater than 40% relative to the total mass of the layer structure of the film, the composite film also allows processing (heat fixing) at temperatures of 80-100°C and with mass proportions of 50% and much more.
[0069] But 1.00g / cm 3 Even with a high mass fraction of more than 40% of material with a higher density, the film composite is 0.95 g / cm 3 As long as the sealant layer is of a polyolefin-based material having a higher density and a melting point less than 120° C., process failure or interruption will always occur before reaching a residual shrinkage of less than 5% in MD and TD, respectively. The temperature required to heat set the film must be at least between 120 and 150° C., and in this case, the film will not shrink below 1.00 g / cm 3 . 3 Even materials with higher densities and melting points above 170° C. are no longer sufficient to keep the manufacturing process stable.
[0070] In order not to impair the film manufacturing process, only temperatures that do not completely eliminate the shrinkage or shrinkage can be selected for the thermal post-treatment.
[0071] Nevertheless, in order to reduce shrinkage to a minimum or even to eliminate it completely, a further process step is required according to the invention. In addition to treating the biaxially oriented film with temperature to eliminate shrinkage, a further process step, namely relaxation, is common, especially in the triple-bubble or multi-bubble process. In this process, the film is allowed to shrink back again in a controlled manner after stretching or orientation; this is known as relaxation and occurs with the introduction of temperature or heat.
[0072] Relaxation can occur in both directions, ie in the direction of manufacture or machine direction (MD) as well as in the direction transverse to manufacture (TD).
[0073] Relaxation can occur equally in both directions (MD and TD) or differently in one or the other direction (quantitative stretching).
[0074] Furthermore, relaxation is also possible in only one direction, i.e. only in MD or only in TD. The choice of relaxation direction can always be made independently of each other. In the context of the present invention, the quantitative extension of the relaxation is expressed by the so-called relaxation factor, as defined in more detail below.
[0075] However, even relaxation of the film alone does not sufficiently reduce shrinkage, and in no case can shrinkage be completely eliminated.
[0076] This is because the films (shrink film / lid film) are usually only treated or fixed at temperatures up to a maximum of 60-80° C. during relaxation, and these relatively low temperatures are already sufficient to achieve a controlled return of the film and to reduce the residual shrinkage to values of approximately 10-20% in MD and TD, respectively, but at best more than 5-10% in one of the two directions.
[0077] Lower shrinkage values have so far been unattainable because the relaxation achievable at these conditions (temperatures) and the temperatures applied are not sufficient to reduce the shrinkage to below 5% in the MD and TD, respectively.
[0078] The degree of relaxation that can be achieved depends substantially on the degree of temperature at which the film is treated or fixed.
[0079] Therefore, the highest possible relaxation, which has a further positive influence on the residual shrinkage, ie which reduces it further, can only be achieved at correspondingly high temperatures in the treatment (heat setting) of the film.
[0080] In this case, however, the same problem as above also arises, namely that with films, especially films comprising a combination of raw materials with widely differing melting points, when treated at the temperatures required to eliminate shrinkage, softening or even melting of the individual layers occurs, thus inevitably interrupting the film production process or at least impairing it to a large extent.
[0081] When a film is subjected to a combination of temperature and relaxation, the temperature range at which the manufacturing process is disturbed or interrupted is also determined by the mass fraction (1.00 g / cm) of material in the layer structure of the film. 3 Depends on the density (larger).
[0082] Surprisingly, however, the percentage of material in the film (1.00 g / cm 3 The greater density) can be significantly lower with proper relaxation than with heat treatment only without relaxation.
[0083] Thus, with appropriate relaxation, it is possible to use materials with a mass fraction (1.00 g / cm 3 ) of in any case less than 40%, preferably less than 30%, in particular less than 20%, and far less than 10% by mass relative to the total mass of the layer structure of the film. 3Treatment at significantly higher temperatures, in any case above 60° C., preferably above 70° C., in particular above 80° C., up to temperatures of 180° C., preferably up to 150° C., in particular up to 120° C., with a simultaneous reduction in the amount of the thermoplastic resin (having a higher density). In this case, a temperature of 1.00 g / cm 3 relative to the total mass of the layer structure of the film can be applied. 3 The proportion by mass of thermoplastic resin having the greater density is at least 1%, preferably at least 5%.
[0084] In the method according to the invention, therefore, during relaxation, the temperature of the composite film is preferably adjusted or set in one of the following ranges: 60-180°C, preferably 60-150°C, particularly preferably 60-120°C, most preferably 80-100°C.
[0085] It is essential for the method according to the invention that the sum of the relaxation factor in the machine direction (MD) and the relaxation factor in the transverse direction (TD) is at least 0.05 (=5%), preferably at least 0.1 (=10%), preferably at least 0.2 (=20%), in particular at least 0.4 (=40%), in that the relaxation factor in the machine direction and the relaxation factor in the transverse direction are each at least greater than 0.00.
[0086] As a result, the relaxation factor is an essential factor in addition to the introduced fix temperature (temperature of the composite film during relaxation) to reduce or eliminate again the shrinkage introduced during the stretching of the film.
[0087] In the context of the present invention, it has proven advantageous to reduce or relax again in a controlled manner the introduced stretching or elongation of the film during stretching.
[0088] Considering the sum of the process steps including stretching and subsequent relaxation, a residual stretch or elongation is obtained in the film after both process steps. The residual stretch factor can be determined, and is defined in detail hereinafter, and is based on the ratio of the length of a section of the composite film after stretching and relaxation to the length of the same section before stretching and relaxation.
[0089] Since the residual stretch factor results equally from both processes (stretching and relaxing), it ideally can also be affected or changed equally by both processes.
[0090] A closer look at this dependence reveals that even a reduction in the stretch factor under otherwise identical conditions has a similar effect on the subsequent relaxation of the film, i.e., less stretching occurs, and even a smaller relaxation can achieve very small shrinkage, while at higher stretches a higher relaxation is also required to keep the shrinkage small, but surprisingly, the effect of the relaxation factor is fundamentally significantly greater than that of the stretch factor.
[0091] Nevertheless, it is not the mitigation alone, but rather the sum or factor of both process steps that is crucial.
[0092] Thus, the residual stretch factor and, of course, the temperature at which relaxation is introduced, essentially determine whether and to what extent shrinkage remains in the film.
[0093] The stretching step as well as the relaxation step and the temperatures introduced therein have a significant influence on the remaining residual shrinkage, and since the stretching step is also subjected to a temperature treatment, the influence from this must also be taken into account.
[0094] Indeed, without simultaneous changes in other process parameters, an effect is also seen here, ie at low stretching temperatures, that there is a larger residual shrinkage compared to high stretching temperatures.
[0095] In comparison with relaxation, however, the stretching process is much more delicate, i.e. the temperature required to obtain a quite stable process is often within a temperature window of only + / - 2 to + / - 3° C. Therefore, in this case the temperature range to be changed is smaller or limited.
[0096] Furthermore, the effect of the temperature of the composite film during stretching is, to the inventors' knowledge, fairly small.
[0097] The temperature during stretching of the composite film is therefore an influencing factor, but not as critical as the temperature during relaxation or stretching factors as well as the relaxation or residual stretching factors.
[0098] A closer look at the process steps and their effects reveals another important factor: the time or duration of exposure to the individual process steps and the governing conditions.
[0099] However, it is found that the effect of the time factor on the drawing process is fairly negligible compared to the effects of the temperature and drawing factors.
[0100] In contrast, in a relaxation process, it is found that the time (duration) of relaxation can be at least as important as the relaxation parameters and the prevailing temperature.
[0101] It turns out that the interaction of time (duration) and relaxation factors is not as important as time (duration) in relation to temperature, or more precisely, the duration for which the film is exposed to temperature during relaxation.
[0102] The longer the duration of the temperature treatment, the greater the effect and therefore the reduction in residual shrinkage.
[0103] However, it can also be seen that this cannot increase indefinitely, but rather that after a certain duration under the influence of temperature, no further increase, i.e. shrinkage reduction, can be achieved, a certain saturation begins.
[0104] Much more critical, however, is the duration for which the film is at least minimally subjected to the influence of temperature, where a duration or residence time at temperature of at least 2 seconds is required to realize the desired effect.
[0105] The method according to the invention can therefore be limited to the point that the composite film has a temperature in one of said temperature ranges during relaxation for a certain time (so-called "dwell time at temperature"). The duration of the relaxation at temperature or the dwell time during relaxation should therefore preferably be at least 2 seconds, in particular more than 5 seconds. Thereby, the duration of the relaxation at temperature or the dwell time during relaxation can be limited to a maximum of 30 seconds, preferably a maximum of 20 seconds, in particular a maximum of 10 seconds.
[0106] Just as temperature or relaxation alone cannot produce a correspondingly low shrinkage, dwell time at temperature alone cannot do so: these influencing variables and the effects they achieve are interdependent and affect each other.
[0107] Thus, the residual shrinkage of the film is small despite the short residence time at temperature, high temperature processing and simultaneously high relaxation.
[0108] However, the residual shrinkage of the film is also small at high temperature processing and long residence times despite the low relaxation.
[0109] The remaining residual shrinkage of the film is also small, despite moderate temperature treatment, long residence time at temperature, and high relaxation.
[0110] Therefore, only a combination of these influencing variables can achieve the desired low residual shrinkage of the film.
[0111] [Table 13]
[0112] [Table 14]
[0113] [Table 15]
[0114] [Table 16]
[0115] [Table 17]
[0116] Therefore, in addition to the ideally applied layer structure, preferably with the raw materials contained therein, the combination of temperatures, process factors, and here in particular the stretching, relaxation and residual stretching factors, as well as the residence times, at least the duration of the thermal fixation (relaxation), applied in the individual process steps, is of decisive importance in order to achieve the given objective. The combination of the characteristics and parameters defined above or in the independent claims according to the invention achieves for the first time the objective of producing, in particular stably producing, by coextrusion and without lamination, a versatile composite film, which in addition to the targeted properties, such as heat resistance, printability and oxygen barrier, also has no shrinkage or a shrinkage of less than 5% in MD and TD, respectively, preferably less than 3%.
[0117] It is particularly preferred that the thermoplastic resin contained in or consisting of layer (c) has a melting point below 120° C. The increased temperature difference compared to the melting point of the outermost layer means that the composite film can be sealed earlier, i.e. at a lower temperature. Furthermore, a higher number of cycles can be achieved during further processing of the composite film.
[0118] It is also particularly preferred if the thermoplastic resin contained in or of which layer (a) consists has a melting point of greater than 170° C. Due to the higher temperature of the outermost layer, higher temperatures can be used in further processing and therefore a higher number of cycles can be achieved in further processing of the composite film.
[0119] Furthermore, according to the invention, the thermoplastic resin of layer (a), i.e. the outermost layer or layer (a), is advantageously of a thickness of 100 mm or less, preferably 100 mm or less, preferably 100 mm or less, more preferably 100 mm or less. -5 The surface tension of the liquid can have a given polarity, expressed in terms of the surface tension, given by the polarity (equal to the polarity of the liquid) of the surface tension of the liquid (equal to the polarity of the liquid). This value is preferably greater than 40 dyn / cm, in particular greater than 42 dyn / cm, allowing the best possible printability.
[0120] According to the invention, in an advantageous embodiment, it can further be provided that the outermost layer (a) consists of or comprises EVOH.
[0121] Up to now, no universal composite film is known from the state of the art in which EVOH is used as a layer component of the outermost layer (a) or in which layer (a) would consist of EVOH. Thus, the use of EVOH as a material with excellent oxygen barrier is known from the state of the art. However, use for this purpose requires an intermediate layer arrangement of EVOH, since EVOH quickly loses its good oxygen barrier properties due to water vapor penetration. Therefore, EVOH has only been used as a layer component or layer material surrounded or sandwiched on both sides by protective layers, for example polyolefins or polyamides, some of which also have a high water vapor barrier. However, the use of EVOH in universal composite films for different purposes and in different ways or in different arrangements, for example as an outermost layer or or sealant layer (innermost layer; surface towards the packaged goods), is not known so far.
[0122] In contrast, the present invention provides the possibility of deliberately using EVOH in layer (a), i.e. in the outermost layer constituting the surface of the composite film towards the outside. In this regard, the outermost layer (a) can comprise or consist of EVOH. However, when EVOH is provided in the outermost layer (a), the properties of EVOH as an oxygen barrier do not play a role. Rather, what is important according to the present invention is that the use of EVOH in the outermost layer substantially increases the recyclability of the film compared to composite films having an outermost layer with PA or PET. This is because EVOH has a lower melting point compared to the PA and PET materials already provided in the outermost layer, and the difference in melting point of the outermost layer and the sealant layer (innermost layer) is reduced. Thereby, the overall melting point required for recycling can be reduced, thereby improving the recyclability of the composite film.
[0123] Furthermore, the inventors have found that EVOH in the outermost layer can further improve the mechanical properties, such as stiffness and printability, of films similar to PET or PA, compared to polyolefins, such as PE or PP. For example, the higher melting point of EVOH compared to these polyolefins and the associated higher temperature resistance for the innermost layer (sealant layer) leads to a general improvement in further processability (number of cycles) of the composite film.
[0124] The following contents are also disclosed within the scope of the present application: The above object is solved by the contents described in the following figures.
[0125] 1. A method for producing a multi-layer composite film, the method comprising at least the following steps: co-extruding at least three layers (a), (b) and (c); - said layer (a) forms an outer layer of said composite film; - said layer (c) forms the surface of said composite film that faces or contacts the goods to be packaged; and - said layer (b) is disposed between said layers (a) and (c); - said layer (b) consists of a single layer or of several layers (b1, b2, b3, b4, ...), preferably 2, 3 or 4 layers; stretching the coextruded composite film; and relaxing the stretched / oriented composite film; Including, The stretching is biaxial; the stretch factor in the machine or longitudinal direction (MD) is at least 2.0; The stretch factor in the transverse direction (TD) is at least 2.0; the sum of the stretch factor in the machine direction (MD) and the stretch factor in the transverse direction (TD) is at least 5.0; The composite film has a temperature of 70 to 130° C. during stretching; Moderation factors in the longitudinal direction (MD) were greater than 0.00; The relaxation factor in the transverse direction (TD) was greater than 0.00; the sum of the relaxation factor in the machine direction (MD) and the relaxation factor in the transverse direction (TD) is at least 0.05 (=5%), preferably at least 0.1 (=10%), preferably at least 0.2 (=20%), in particular at least 0.4 (=40%); The composite film has a temperature during relaxation of 60 to 180°C, preferably 60 to 150°C, more preferably 60 to 120°C, and particularly preferably 80 to 100°C; the residence time during relaxation, preferably during relaxation at temperature, is preferably at least 2 seconds, in particular greater than 5 seconds, or the duration of said relaxation is preferably at least 2 seconds, in particular greater than 5 seconds, the residence time during relaxation, preferably during relaxation at temperature, is preferably at most 30 seconds, preferably at most 20 seconds, in particular at most 10 seconds, or the duration of said relaxation is preferably at most 30 seconds, preferably at most 20 seconds, in particular at most 10 seconds; The residual stretch factor in the machine direction (MD) is a maximum of 5.0; The residual stretch factor in the transverse direction (TD) is a maximum of 5.0; The layer (a) has a density of 1.00 g / cm3 comprising or consisting of a thermoplastic resin having a greater density; The layer (b) or layers (b1, b2, ...) each have a hardness of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a higher density; and The layer (c) has a density of 0.95 g / cm 3 comprising or consisting of a thermoplastic resin having a density of less than ,method.
[0126] 2. A method for producing a multi-layer composite film, the method comprising at least the following steps: co-extruding at least four layers (a), (b), (d), and (c); said layer (a) forms an outer layer of said composite film, - said layer (c) forms the surface of said composite film that faces or contacts the goods to be packaged; and - said layer (b) is disposed between said layers (a) and (c); - said layer (d) is disposed between said layers (a) and (c), preferably between said layers (a) and (b); - said layer (b) consists of a single layer or of several layers (b1, b2, ...), preferably 2, 3 or 4 layers; - said layer (d) consists of a single layer or of several layers (d1, d2, ...), preferably 2, 3 or 4 layers; stretching the coextruded composite film; and relaxing the stretched / oriented composite film; Including, The stretching is biaxial; the stretch factor in the machine or longitudinal direction (MD) is at least 2.0; The stretch factor in the transverse direction (TD) is at least 2.0; the sum of the stretch factor in the machine direction (MD) and the stretch factor in the transverse direction (TD) is at least 5.0; The composite film has a temperature of 70 to 130° C. during stretching; Moderation factors in the longitudinal direction (MD) were greater than 0.00; The relaxation factor in the transverse direction (TD) was greater than 0.00; the sum of the relaxation factor in the machine direction (MD) and the relaxation factor in the transverse direction (TD) is at least 0.05 (=5%), preferably at least 0.1 (=10%), preferably at least 0.2 (=20%), in particular at least 0.4 (=40%); The composite film has a temperature during relaxation of 60 to 180°C, preferably 60 to 150°C, more preferably 60 to 120°C, and particularly preferably 80 to 100°C; the residence time during the relaxation, preferably at temperature, is preferably at least 2 seconds, in particular greater than 5 seconds, or the duration of the relaxation is preferably at least 2 seconds, in particular greater than 5 seconds; the residence time during the relaxation, preferably at temperature, is preferably at most 30 seconds, preferably at most 20 seconds, in particular at most 10 seconds, or the duration of the relaxation is preferably at most 30 seconds, preferably at most 20 seconds, in particular at most 10 seconds; The residual stretch factor in the machine direction (MD) is a maximum of 5.0; The residual stretch factor in the transverse direction (TD) is a maximum of 5.0; The layer (a) has a density of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a greater density; The layer (d) or layers (d1, d2, ...) each have a viscosity of 1.00 g / cm 3 Less than 0.98 g / cm 3 comprising or consisting of a thermoplastic resin, preferably a polyolefin, having a density less than The layer (b) or layers (b1, b2, ...) each have a hardness of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a higher density; and The layer (c) has a density of 0.95 g / cm 3 comprising or consisting of a thermoplastic resin having a density of less than , method, preferably method according to number 1.
[0127] 3. The thermoplastic resin of the layer (a) and the thermoplastic resin of the layer (b) are different; or the thermoplastic resin of layer (a) is different from the thermoplastic resin of layer (b) or different from all the thermoplastic resins of layers (b1, b2, ...); or the thermoplastic resin of layer (a) and the thermoplastic resin of layer (b) are the same; or 3. The method according to claim 1 or 2, characterized in that the thermoplastic resin of layer (a) is identical to at least one of the thermoplastic resins of layers (b1, b2, ...).
[0128] 4. The thermoplastic resin of layer (a) has a melting point greater than 170° C.; and / or 4. The method according to any one of the above numbers 1 to 3, characterized in that the thermoplastic resin of layer (a) has a surface tension of more than 40 dyn / cm, in particular more than 42 dyn / cm.
[0129] 5. The thermoplastic resin of layer (c) is a polyolefin having a sealing temperature lower than the sealing temperature of the thermoplastic resin of layer (a); and / or The method according to any one of the above numbers 1 to 4, characterized in that the thermoplastic resin of the layer (c) is a polyolefin having a melting point of less than 120°C.
[0130] 6. The thermoplastic resin of the layer (b) is 100 cm 3 / m 2 or the layers (b1, b2, ...) each or together have an oxygen permeability of less than 100 cm 3 / m 2 has an oxygen permeability of less than d bar; and / or The layer (b) is 100 cm 3 / m 2 d bar or the layers (b1, b2, ...) each or together have an oxygen permeability of less than 100 cm 3 / m 2 6. The method according to any one of the above numbers 1 to 5, characterized in that the oxygen permeability is less than .d.bar.
[0131] 7. The method according to any one of the above numbers 1 to 6, characterized in that the stretching is carried out simultaneously or in several steps consecutively.
[0132] 8. After stretching and relaxation, the composite film has a shrinkage in the machine direction (MD) of less than 0.05 (=5%), preferably less than 0.03 (=3%); and / or After stretching and relaxing, the composite film has a shrinkage in the transverse direction (TD) of less than 0.05 (=5%), preferably less than 0.03 (=3%); and / or 8. The method according to any one of the above numbers 1 to 7, characterized in that after stretching and relaxing, the composite film preferably has a sum of shrinkage in the machine direction (MD) and shrinkage in the transverse direction (TD) (=total shrinkage) of less than 0.05 (=5%).
[0133] 9. The thickness of said layer (a) does not exceed 20%, preferably 10%, of the total thickness of the composite film; and / or 9. The method according to any one of the above numbers 1 to 8, characterized in that the thickness of layer (b) or the total thickness of layers (b1, b2, ...) does not exceed 20%, preferably 10%, of the total thickness of the composite film.
[0134] 10. The mass proportion of the layer (a) in relation to the total mass of the composite film does not exceed 10%; and / or 10. The method according to any one of the above numbers 1 to 9, characterized in that the mass proportion of the layer (b) or the sum of the mass proportions of the layers (b1, b2, ...) relative to the total mass of the composite film does not exceed 10%.
[0135] 11. The method according to any one of the above numbers 1 to 10, characterized in that the sum of the mass proportions of layers (a) and (b) or of layers (a) and layers (b1, b2, ...) relative to the total mass of the composite film does not exceed 10%.
[0136] 12. The method according to any one of the above numbers 1 to 11, characterized in that the thermoplastic resin of layer (a) comprises or consists of a polyester, preferably polyethylene terephthalate (PET) or polylactic acid or polylactide (PLA), a polyamide (PA), an ethylene-vinyl alcohol copolymer (EVOH), or any mixture thereof.
[0137] 13. The method according to any one of the above numbers 1 to 12, characterized in that the thermoplastic resin of layer (c) comprises or consists of a polyolefin (PO), preferably polyethylene (PE) and / or polypropylene (PP), an ethylene-vinyl acetate copolymer (EVA), an ionomer (IO), an ethylene-methyl methacrylate copolymer (EMMA), an ethylene-methacrylic acid copolymer (EMA), or any mixture thereof.
[0138] 14. A multi-layer composite film produced according to any one of the above numbers 1 to 13, wherein the composite film is preferably in the form of a sheet or a tube.
[0139] 15. At least three layers (a), (b) and (c) - said layer (a) forms an outer layer of said composite film; - said layer (c) forms the surface of said composite film that faces or contacts the goods to be packaged; and - said layer (b) is disposed between said layers (a) and (c); - said layer (b) consists of a single layer or of several layers (b1, b2, b3, b4, ...), preferably 2, 3 or 4 layers; A multilayer, coextruded, biaxially stretched / oriented, and relaxed composite film comprising: the composite film has a residual stretch factor in the machine direction (MD) of at most 5.0; The composite film has a residual stretch factor in the transverse direction (TD) of at most 5.0; The layer (a) has a density of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a greater density; The layer (b) or layers (b1, b2, ...) each have a hardness of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a density greater than The layer (c) has a density of 0.95 g / cm 3 comprising or consisting of a thermoplastic resin having a density of less than , preferably produced by the method according to any one of the above numbers 1 to 13.
[0140] 16. At least four layers (a), (b), (d) and (c) - said layer (a) forms an outer layer of said composite film; - said layer (c) forms the surface of the composite film that faces or contacts the goods to be packaged; and - said layer (b) is disposed between said layers (a) and (c); - said layer (d) is disposed between said layers (a) and (c), preferably between said layers (a) and (b); - said layer (b) consists of a single layer or of several layers (b1, b2, ...), preferably 2, 3 or 4 layers; - said layer (d) consists of a single layer or of several layers (d1, d2, ...), preferably 2, 3 or 4 layers; A multilayer, coextruded, biaxially oriented and relaxed composite film comprising: the composite film has a residual stretch factor in the machine direction (MD) of at most 5.0; The composite film has a residual stretch factor in the transverse direction (TD) of at most 5.0; The layer (a) has a density of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a greater density; The layer (d) or layers (d1, d2, ...) each have a viscosity of 1.00 g / cm 3 Less than 0.98 g / cm 3 comprising or consisting of a thermoplastic resin, preferably a polyolefin, having a density less than The layer (b) or layers (b1, b2, ...) each have a hardness of 1.00 g / cm 3comprising or consisting of a thermoplastic resin having a greater density; and The layer (c) has a density of 0.95 g / cm 3 comprising or consisting of a thermoplastic resin having a density of less than A film, preferably a composite film as described in numeral 15 above.
[0141] 17. The thermoplastic resin of the layer (a) and the thermoplastic resin of the layer (b) are different; or the thermoplastic resin of layer (a) is different from the thermoplastic resin of layer (b) or from all the thermoplastic resins of layers (b1, b2, ...); or the thermoplastic resin of layer (a) and the thermoplastic resin of layer (b) are the same; or A composite film according to any one of the above numbers 14 to 16, characterized in that the thermoplastic resin of the layer (a) is the same as at least one of the thermoplastic resins of the layers (b1, b2, ...).
[0142] 18. A composite film according to any one of the above numbers 14 to 17, characterized in that the thermoplastic resin of layer (a) has a melting point of greater than 170°C.
[0143] 19. The thermoplastic resin of layer (c) is a polyolefin having a sealing temperature lower than the sealing temperature of the thermoplastic resin of layer (a); and / or The composite film according to any one of the above numbers 14 to 18, characterized in that the thermoplastic resin of the layer (c) is a polyolefin having a melting point of less than 120°C.
[0144] 20. The thermoplastic resin of the layer (b) or the thermoplastic resin of the layers (b1, b2, ...) each or in total has a thickness of 100 cm 3 / m 2 has an oxygen permeability of less than d bar; and / or The layer (b) or the layers (b1, b2, ...) each or in total have a thickness of 100 cm 3 / m 220. A composite film according to any one of the above numbers 14 to 19, characterized in that it has an oxygen permeability of less than .d.bar.
[0145] 21. After stretching and relaxation, the composite film has a shrinkage in the machine direction (MD) of less than 0.05 (=5%), preferably less than 0.03 (=3%); and / or After stretching and relaxing, the composite film has a shrinkage in the transverse direction (TD) of less than 0.05 (=5%), preferably less than 0.03 (=3%); and / or A composite film according to any of the above numbers 14 to 20, characterized in that after stretching and relaxing, the composite film preferably has a sum of shrinkage in the machine direction (MD) and shrinkage in the transverse direction (TD) (=total shrinkage) of less than 0.05 (=5%).
[0146] 22. The thickness of said layer (a) does not exceed 20%, preferably 10%, of the total thickness of the composite film; and / or 22. A composite film according to any of the above figures 14 to 21, characterized in that the thickness of layer (b) or the total thickness of layers (b1, b2, ...) does not exceed 20%, preferably 10%, of the total thickness of the composite film.
[0147] 23. The mass proportion of the layer (a) relative to the total mass of the composite film does not exceed 10%; and / or 23. The method according to any of the above numbers 14 to 22, characterized in that the mass proportion of the layer (b) or the sum of the mass proportions of the layers (b1, b2, ...) relative to the total mass of the composite film does not exceed 10%.
[0148] 24. A composite film according to any one of the above numbers 14 to 23, characterized in that the sum of the mass proportions of layers (a) and (b) and / or the sum of the mass proportions of layers (a) and (b1, b2, ...) relative to the total mass of the composite film does not exceed 10%.
[0149] 25. A composite film according to any one of the above numbers 14 to 24, characterized in that the thermoplastic resin of layer (a) comprises or consists of a polyester, preferably polyethylene terephthalate (PET) or polylactic acid or polylactide (PLA), polyamide (PA), ethylene-vinyl alcohol copolymer (EVOH), or any mixture thereof.
[0150] 26. A composite film according to any one of the above numbers 14 to 25, characterized in that the thermoplastic resin of layer (c) comprises or consists of a polyolefin (PO), preferably polyethylene (PE) and / or polypropylene (PP), an ethylene-vinyl acetate copolymer (EVA), an ionomer (IO), an ethylene-methyl methacrylate copolymer (EMMA), an ethylene-methacrylic acid copolymer (EMA), or any mixture thereof.
[0151] 27. Use of a multilayer composite film according to any one of the above numbers 14 to 26 or a casing made thereof for packaging goods, preferably foodstuffs, fine foodstuffs or liquid or solid, in particular powdered, goods.
[0152] 28. The method according to any one of the numbers 1 to 13, the composite film according to any one of the numbers 14 to 26 or the use according to number 27, characterized in that the mass proportion of the layer components having a melting point above 170°C, preferably of the thermoplastic resin of layer (a) having a melting point above 170°C, is from 1 to less than 40%, preferably from 1 to less than 30%, preferably from 1 to less than 20%, in particular from 5 to less than 20%, relative to the total mass of the composite film.
[0153] Supplementary disclosure (definitions, etc.)
[0154] The process for producing the multilayer composite film according to the invention described herein may be characterized in that it does not include a lamination step, i.e., a step of bonding or adhering layers or layer composites.
[0155] Thus, the multilayer composite films described herein according to the present invention can be non-laminated composite films.
[0156] Length definition (based on length or width, respectively)
[0157] L0:=Length of a given section of the composite film before stretching L1:=the length of the same section of the composite film after stretching and before relaxation L2:=Length of the same section of the composite film after stretching and before relaxation L3:=Length of the same section of the composite film after stretching and relaxation
[0158] Definition of the stretch factor: Stretch factor V = length L1 of a given section of the composite film after stretching and before relaxation divided by the length L0 of the same section of the composite film before stretching; (V = L1 / L0)
[0159] Definition of relaxation factor: Relaxation factor RL = the amount of difference between (the length L3 of a given section of a composite film after stretching and relaxation and the length L2 of the same section of the composite film after stretching and before relaxation) divided by the length L2 of the same section of the composite film after stretching and before relaxation; (RL = |(L3-L2)| / L2)
[0160] Definition of residual stretch factor: Residual stretch factor RV = length L3 of a given section of a composite film after stretching and relaxation divided by the length L0 of the same section of the composite film before stretching and relaxation; (RV = L3 / L0)
[0161] Preferably, the composite film according to the present invention is a multi-layer composite film having a barrier function or a multi-layer barrier film, said barrier property referring to reduced oxygen transmission rate or reduced water vapor transmission rate or both.
[0162] Shrinkage (or Heat Shrinkage): Measured in water at 90°C preferably within 1 second after immersion, but at least 10 seconds after immersion.
[0163] According to the invention, to determine the shrinkage (or thermal shrinkage), the sample is immersed in water at 90° C. for a given time, in particular the aforementioned time, and after removal is immediately cooled in water to room temperature. After this treatment, the length of the previously marked section is measured, referring to the length of the same section of the sample before treatment. The ratio of the lengths obtained ('shrinkage' to 'unshrinkage'), given as a percentage, defines the shrinkage or shrink. Depending on the direction of the length measurement, the shrinkage is obtained in the longitudinal direction (MD) and in the transverse direction (TD). The total shrinkage is calculated by adding the shrinkage in the longitudinal and transverse directions. Multiple determinations of the length measurements, for example triplicate or quadruplicate determinations, and the formation of corresponding average values therefrom, advantageously increase the accuracy of the determination. According to the invention, the shrinkage and the total shrinkage can be determined in particular according to ASTM 2732.
[0164] According to the present invention, oxygen transmission rate is measured at 23° C. and 75% relative humidity (ASTM D 1434).
[0165] The method according to the invention and the composite film according to the invention can be preferably carried out or produced using the so-called double bubble and especially triple bubble method, for which the applicant provides suitable equipment known to the skilled person. In that respect, the multi-layer composite film can be, for example, co-extruded from each resin melt by nozzle blowing in the applicant's setup for producing a composite film with three or more layers, preferably cooled in the applicant's water cooling system, reheated, biaxially stretched / oriented (in the machine direction (MD) and in the transverse direction (TD)) by the trapped compressed air bubbles, and finally relaxed (= heat-set or thermofixed) in a further step at a given temperature method. The composite film according to the invention can be a composite film comprising a barrier against gas diffusion, especially against oxygen diffusion and / or against water vapor diffusion. Such manufacturing methods are also known to the skilled person from the text "Sausage Casings" by Savic, Z., Savic, I., 1st edition, 2002, VICTUS Lebensmittelindustriebedarf Vertriebsgesellshaft mbH, Vienna, Austria, chapter 7, esp. subchapter 4.2, pages 267-270.
[0166] Another method of producing films according to the present invention is by stretching / orienting a coextruded flat film by tenter processes known to those skilled in the art.
[0167] If an apparatus for rapid cooling of the thin thermoplastic tube after extrusion as disclosed in the same applicant's DE 19916428 is additionally used, the composite film of the invention can be advantageously obtained on an apparatus or device or plant of the same application for producing blown food films for packaging foodstuffs by the jet-blowing process, such as shrink films or shrink bags for example. For this purpose, the corresponding further development according to DE 10048178 can also be considered.
[0168] In that respect, the blown film produced from the plastic melt in the nozzle blow head is subjected to intensive cooling, during which the amorphous structure of the thermoplastic resin from the plastic melt is preserved. The blown film extruded vertically from the plastic melt in the nozzle blow head passes to a cooling device for cooling without first coming into contact with a wall, as described in detail in DE 19916428 and DE 10048178. In order to avoid repetition, reference is made in full to the contents of DE 19916428 and DE 10048178 for details of the processing, construction and operation of this cooling system, also referred to as the calibration device.
[0169] The blown film passes through supports in a cooling system against which the film is supported and as a result of the differential pressure between the interior of the blown film and the cooling system, a liquid film or coating is maintained between the film and the supports, eliminating sticking of the blown film. The diameter of the supports thereby affects the diameter of the blown film, which is why this cooling system of the same applicant is also referred to as a calibration device.
[0170] According to the invention, the polyamide (PA) can be a material selected from the group consisting of PAs of ε-caprolactam or poly(ε-caprolactam) (PA6), PAs of hexamethylenediamine and adipic acid or polyhexamethyleneadipamide (PA6.6), PAs of ε-caprolactam and hexamethylenediamine / adipic acid (PA6.66), PAs of hexamethylenediamine and dodecanedioic acid or polyhexamethylenedodecanamide (PA6.12), PAs of 11-aminoundecanoic acid or polyundecaneamide (PA11), PAs of 12-laurinlactam or poly(ω-laurinlactam) (PA12), or mixtures of these PAs or mixtures of these PAs with amorphous PAs or with other polymers. The general notation PAx.y is synonymous with PAx / y or PAxy.
[0171] For the purposes of this application, polyolefin (PO) can be a material selected from the group consisting of PP, PE, LDPE, LLDPE, polyolefin plastomer (POP), ethylene-vinyl acetate copolymer (EVA), ethylene-methyl methacrylate copolymer (EMMA), ethylene-methacrylic acid copolymer (EMA), ethylene-acrylic acid copolymer (EAA), cycloolefin / cycloalkene and 1-alkene copolymers or cycloolefin copolymers (COC), ionomers (IO) or mixtures or blends thereof. Furthermore, in the context of the present invention, PO also includes blends of said PO with ionomers and / or adhesion promoters.
[0172] In the context of the present invention, polyesters can be used as layer components of layer (a). Polyesters are polymers with ester functional groups in their main chain and can in particular be aliphatic or aromatic polyesters. Polyesters can be obtained by polycondensation of the corresponding dicarboxylic acids with diols. Any dicarboxylic acid suitable for forming polyesters, in particular terephthalic acid and isophthalic acid, as well as dimers of unsaturated aliphatic acids, can be used to synthesize polyesters. As further components for the synthesis of polyesters, diols can be used, for example: polyalkylene glycols, such as ethylene glycol, propylene glycol, tetramethylene glycol, neopentyl glycol, hexamethylene glycol, diethylene glycol, polyethylene glycol and polytetramethylene oxide glycol; 1,4-cyclohexanedimethanol, and 2-alkyl-1,3-propanediols.
[0173] Particularly preferred is PET, which stands for the polyester polyethylene terephthalate (PET), which can be obtained by polycondensation of terephthalic acid (1,4-benzenedicarboxylic acid) and ethylene glycol (1,2-dihydroxyethane).
[0174] Another preferred polyester is polylactide or polylactic acid (PLA), which may be included as a layer component in layers in which the polyester is provided as a layer component. These polymers are biocompatible / biodegradable and have high melting temperatures or points and good tensile strength, in addition to low moisture absorption.
[0175] In the context of the present invention, EVOH denotes EVOH as well as blends of EVOH with other polymers, ionomers, EMA or EMMA. In particular, EVOH also includes blends of EVOH and PA or of EVOH and ionomers.
[0176] The adhesion promoter (HV) may be provided as an intermediate layer in the composite film according to the invention and represents an adhesive layer providing good bond adhesion between the individual layers. In this respect, the HV may be based on a base substance or material selected from the group consisting of PE, PP, EVA, EMA, EMMA, EAA and ionomers, or mixtures thereof. Particularly suitable adhesion promoters (HV) according to the invention are EVA, EMA or EMMA, each with a purity of more than 99%, preferably more than 99.9%.
[0177] According to a further preferred embodiment, the layer comprising HV as layer component may also comprise a mixture of PO and HV or a mixture of EVA, EMA, EMMA and / or EAA and HV or a mixture of ionomers and HV or a mixture of several HVs.
[0178] For the purposes of the present invention, the melting point of the polymer is determined by dynamic differential calorimetry or differential thermal analysis according to DIN 51007:2019-04 or DIN EN ISO 11357-1:2017-02, or the ASTM D3418 method, also known from the prior art.
[0179] For the purposes of the present invention, the softening point of a polymer is determined by the method for determining the Vicat softening temperature (VST) according to DIN EN ISO 306:2014-03.
[0180] For the purposes of the present invention, printability is measured in accordance with DIN 16500 2:2018-09.
[0181] For the purposes of the present invention, the designation of a material as a "layer component" means that a layer of the composite film according to the invention at least partially comprises this material. In this regard, the designation "layer component" in the sense of the present invention can in particular include that the layer consists entirely or exclusively of this material.
[0182] For the purposes of the present invention, a "middle" or "intermediate" layer means a layer of a composite film arranged between layers (a) and (c). According to the present invention, layer (a) is the layer that forms the outer layer of the composite film (outermost layer). According to the present invention, layer (c) is the layer that forms the surface of the composite film that faces or is in contact with the goods to be packaged (innermost layer). By definition, layers (a) and (c) of a composite film according to the present invention cannot be "middle" or "intermediate" layers.
[0183] Preferably, the composite film according to the present invention is in sheet or tubular form. Preferably, the composite film is a food film or food casing. More preferably, the composite film is suitable for use as a non-heat shrinkable packaging material.
[0184] Example of a coextruded and biaxially oriented multilayer film with barrier function according to the present invention having at least three layers (a), (b) and (c)
[0185] [Table 18]
[0186] Example of a coextruded and biaxially oriented multilayer film with barrier function according to the present invention having at least four layers (a), (b), (d) and (c)
[0187] [Table 19]
[0188] [Table 20]
[0189] [Table 21]
[0190]
Table 22
Claims
1. 1. A method for producing a multi-layer composite film, the method comprising at least the steps of: co-extruding at least three layers (a), (b) and (c); - said layer (a) forms the outer layer of said composite film; - said layer (c) forms the surface of said composite film that faces or contacts the goods to be packaged; and - said layer (b) is disposed between said layers (a) and (c); - said layer (b) consists of a single layer or of several layers (b1, b2, b3, b4, ...); stretching the coextruded composite film; and Relaxing the stretched composite film Including, The stretching is biaxial; The stretch factor in the machine or longitudinal direction (MD) is at least 2.0; The stretch factor in the transverse direction (TD) is at least 2.0; the sum of the stretch factor in the machine direction (MD) and the stretch factor in the transverse direction (TD) is at least 5.0; The composite film has a temperature of 70 to 130° C. during stretching; The relaxation factor in the machine direction (MD) is greater than 0.00; The relaxation factor in the transverse direction (TD) is greater than 0.00; The sum of the relaxation factor in the machine direction (MD) and the relaxation factor in the transverse direction (TD) is at least 0.05 (=5%); The composite film has a temperature during relaxation of 60 to 180°C; the dwell time between relaxations is at least 2 seconds, or the duration of said relaxations is at least 2 seconds; the dwell time between relaxations is at most 30 seconds, or the duration of said relaxations is at most 30 seconds; The residual stretch factor in the machine direction (MD) is at most 5.0; The residual stretch factor in the transverse direction (TD) is a maximum of 5.0; Here, the residual stretch factor is defined as follows: Residual stretch factor RV=L3, the length of a given section of the composite film after stretching and relaxation, divided by L0, the length of the same section of the composite film before stretching and relaxation; (RV=L3 / L0); The layer (a) has a density of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a higher density; The layer (b) or layers (b1, b2, ...) each have a hardness of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a higher density; The layer (c) has a thickness of 0.95 g / cm 3 comprising or consisting of a thermoplastic resin having a density less than The 1.00 g / cm 3 The method of claim 1, wherein the thermoplastic resin having the higher density has a mass percentage of at least 1% and less than 30% relative to the total mass of the layer structure of the composite film.
2. The method includes at least the following steps: co-extruding at least four layers (a), (b), (d), and (c); - said layer (a) forms the outer layer of said composite film; - said layer (c) forms the surface of said composite film that faces or contacts the goods to be packaged; and - said layer (b) is disposed between said layers (a) and (c); - said layer (d) is disposed between said layers (a) and (c); - said layer (b) consists of a single layer or of several layers (b1, b2,...); - said layer (d) consists of a single layer or of several layers (d1, d2,...); stretching the coextruded composite film; and relaxing the stretched composite film; Including, The stretching is biaxial; The stretch factor in the machine or longitudinal direction (MD) is at least 2.0; The stretch factor in the transverse direction (TD) is at least 2.0; the sum of the stretch factor in the machine direction (MD) and the stretch factor in the transverse direction (TD) is at least 5.0; The composite film has a temperature of 70 to 130° C. during stretching; The relaxation factor in the machine direction (MD) is greater than 0.00; The relaxation factor in the transverse direction (TD) is greater than 0.00; The sum of the relaxation factor in the machine direction (MD) and the relaxation factor in the transverse direction (TD) is at least 0.05 (=5%); The composite film has a temperature during relaxation of 60 to 180°C; At least 2 seconds between relaxations, or the duration of the relaxations is at least 2 seconds the dwell time between relaxations is at most 30 seconds, or the duration of the relaxations is at most 30 seconds; The residual stretch factor in the machine direction (MD) is at most 5.0; The residual stretch factor in the transverse direction (TD) is a maximum of 5.0; Here, the residual stretch factor is defined as follows: Residual stretch factor RV = length L3 of a given section of a composite film after stretching and relaxation divided by length L0 of the same section of the composite film before stretching and relaxation; (RV = L3 / L0) and The layer (a) has a density of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a higher density; The layer (d) or layers (d1, d2, . . .) each have a viscosity of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a density less than The layer (b) or layers (b1, b2, ...) each have a hardness of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a higher density; and The layer (c) has a thickness of 0.95 g / cm 3 comprising or consisting of a thermoplastic resin having a density of less than 2. The method according to claim 1 .
3. the thermoplastic resin of layer (a) and the thermoplastic resin of layer (b) are different; or the thermoplastic resin of layer (a) is different from the thermoplastic resin of layer (b) or different from all the thermoplastic resins of layers (b1, b2, ...); or the thermoplastic resin of layer (a) and the thermoplastic resin of layer (b) are the same; or 3. The method according to claim 1 or 2, characterized in that the thermoplastic resin of layer (a) is identical to at least one of the thermoplastic resins of layers (b1, b2, ...).
4. The thermoplastic resin of layer (a) has a melting point greater than 170° C.; and / or The thermoplastic resin of layer (c) is a polyolefin having a sealing temperature lower than the sealing temperature of the thermoplastic resin of layer (a); and / or The thermoplastic resin of layer (c) is a polyolefin having a melting point of less than 120° C.; and / or The thermoplastic resin of the layer (b) is 100 cm 3 / m 2 The thermoplastic resins of the layers (b1, b2, ...) each or together have an oxygen permeability of less than 100 cm 3 / m 2 has an oxygen transmission rate of less than d bar; and / or The layer (b) is 100 cm 3 / m 2 have an oxygen permeability of less than 100 cm 3 / m 2 has an oxygen transmission rate of less than d bar; and / or The stretching is carried out simultaneously or in several steps successively; and / or After stretching and relaxing, the composite film has a shrinkage in the machine direction (MD) of less than 0.05 (=5%); and / or After stretching and relaxing, the composite film has a shrinkage in the transverse direction (TD) of less than 0.05 (=5%); and / or 4. The method according to claim 1, wherein after stretching and relaxing, the composite film has a sum of shrinkage in the machine direction (MD) and shrinkage in the transverse direction (TD) (=total shrinkage) of less than 0.05 (=5%).
5. the thickness of said layer (a) does not exceed 20% of the total thickness of the composite film; and / or the thickness of said layer (b) or the total thickness of said layers (b1, b2, ...) does not exceed 20% of the total thickness of the composite film; and / or the proportion by weight of said layer (a) relative to the total weight of said composite film does not exceed 10%; and / or the mass proportion of the layer (b) or the sum of the mass proportions of the layers (b1, b2, ...) does not exceed 10% of the total mass of the composite film; and / or 5. The method according to claim 1 , wherein the sum of the mass proportions of layers (a) and (b) or of layers (a) and (b1, b2, ...) relative to the total mass of the composite film does not exceed 10%.
6. The thermoplastic resin of layer (a) comprises or consists of polyester, polyamide (PA), ethylene-vinyl alcohol copolymer (EVOH), or any mixture thereof; and / or 6. The method according to any one of claims 1 to 5, characterized in that the thermoplastic resin of layer (c) comprises or consists of polyolefin (PO), ethylene-vinyl acetate copolymer (EVA), ionomer (IO), ethylene-methyl methacrylate copolymer (EMMA), ethylene-methacrylic acid copolymer (EMA), or any mixture thereof.
7. At least three layers (a), (b) and (c) - said layer (a) forms the outer layer of the composite film; - said layer (c) forms the surface of said composite film that faces or contacts the goods to be packaged; and - said layer (b) is disposed between said layers (a) and (c); - said layer (b) consists of a single layer or of several layers (b1, b2, b3, b4, ...); A coextruded, biaxially oriented and relaxed multi-layer composite film comprising: The composite film has a residual stretch factor in the machine direction (MD) of at most 5.0; The composite film has a residual stretch factor in the transverse direction (TD) of at most 5.0; Here, the residual stretch factor is defined as follows: Residual stretch factor RV = length L3 of a given section of a composite film after stretching and relaxation divided by length L0 of the same section of the composite film before stretching and relaxation; (RV = L3 / L0) and The layer (a) has a density of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a higher density; The layer (b) or layers (b1, b2, ...) each have a hardness of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a higher density; The layer (c) has a thickness of 0.95 g / cm 3 comprising or consisting of a thermoplastic resin having a density less than The 1.00 g / cm 3 A composite film, in which the thermoplastic resin having a higher density has a mass proportion of at least 1% and less than 30% relative to the total mass of the layer structure of the composite film.
8. At least four layers (a), (b), (d) and (c) - said layer (a) forms the outer layer of said composite film; - said layer (c) forms the surface of said composite film that faces or contacts the goods to be packaged; and - said layer (b) is disposed between said layers (a) and (c); - said layer (d) is disposed between said layers (a) and (c); - said layer (b) consists of a single layer or of several layers (b1, b2,...); - said layer (d) consists of a single layer or of several layers (d1, d2,...); A coextruded, biaxially oriented, relaxed multi-layer composite film comprising: The composite film has a residual stretch factor in the machine direction (MD) of at most 5.0; The composite film has a residual stretch factor in the transverse direction (TD) of at most 5.0; Here, the residual stretch factor is defined as follows: Residual stretch factor RV = length L3 of a given section of a composite film after stretching and relaxation divided by length L0 of the same section of the composite film before stretching and relaxation; (RV = L3 / L0) and The layer (a) has a density of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a higher density; The layer (d) or layers (d1, d2, . . .) each have a viscosity of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a density less than The layer (b) or layers (b1, b2, ...) each have a hardness of 1.00 g / cm 3 comprising or consisting of a thermoplastic resin having a higher density; and The layer (c) has a thickness of 0.95 g / cm 3 comprising or consisting of a thermoplastic resin having a density of less than The composite film of claim 7.
9. the thermoplastic resin of layer (a) and the thermoplastic resin of layer (b) are different; or the thermoplastic resin of layer (a) is different from the thermoplastic resin of layer (b) or from all the thermoplastic resins of layers (b1, b2, ...); or the thermoplastic resin of layer (a) and the thermoplastic resin of layer (b) are the same; or 9. A composite film according to claim 7 or 8, characterized in that the thermoplastic resin of the layer (a) is identical to at least one of the thermoplastic resins of the layers (b1, b2, ...).
10. The thermoplastic resin of layer (a) has a melting point greater than 170° C.; and / or The thermoplastic resin of layer (c) is a polyolefin having a sealing temperature lower than the sealing temperature of the thermoplastic resin of layer (a); and / or The thermoplastic resin of layer (c) is a polyolefin having a melting point of less than 120° C.; and / or The thermoplastic resin of the layer (b) is 100 cm 3 / m 2 The thermoplastic resins of the layers (b1, b2, ...) each or together have an oxygen permeability of less than 100 cm 3 / m 2 has an oxygen transmission rate of less than d bar; and / or The layer (b) is 100 cm 3 / m 2 have an oxygen permeability of less than 100 cm 3 / m 2 10. A composite film according to any one of claims 7 to 9, characterized in that it has an oxygen permeability of less than .d.bar.
11. After stretching and relaxing, the composite film has a shrinkage in the machine direction (MD) of less than 0.05 (=5%); and / or After stretching and relaxing, the composite film has a shrinkage in the transverse direction (TD) of less than 0.05 (=5%); and / or 11. A composite film according to any one of claims 7 to 10, characterized in that after stretching and relaxing, the composite film has a sum of shrinkage in the machine direction (MD) and shrinkage in the transverse direction (TD) (=total shrinkage) of less than 0.05 (=5%).
12. the thickness of said layer (a) does not exceed 20% of the total thickness of the composite film; and / or the thickness of said layer (b) or the total thickness of said layers (b1, b2, ...) does not exceed 20% of the total thickness of the composite film; and / or the proportion by weight of said layer (a) in relation to the total weight of said composite film does not exceed 10%; and / or the mass proportion of the layer (b) or the sum of the mass proportions of the layers (b1, b2, ...) relative to the total mass of the composite film does not exceed 10%; and / or 12. The composite film according to claim 7, wherein the sum of the mass proportions of layers (a) and (b) or layers (a) and (b1, b2, ...) relative to the total mass of the composite film does not exceed 10%.
13. The thermoplastic resin of layer (a) comprises or consists of polyester, polyamide (PA), ethylene-vinyl alcohol copolymer (EVOH), or any mixture thereof; and / or 13. A composite film according to any one of claims 7 to 12, characterized in that the thermoplastic resin of layer (c) comprises or consists of polyolefin (PO), ethylene-vinyl acetate copolymer (EVA), ionomer (IO), ethylene-methyl methacrylate copolymer (EMMA), ethylene-methacrylic acid copolymer (EMA), or any mixture thereof.
14. Use of a multi-layer composite film according to any one of claims 7 to 13 or a casing made thereof for packaging foodstuffs, luxury foodstuffs or liquid, solid or powdered goods.
15. 7. The method according to claim 1, wherein the mass proportion of layer components having a melting point above 170° C. is from 1 to less than 40%, relative to the total mass of the composite film.
16. 14. Composite film according to claim 7, characterized in that the mass proportion of layer components having a melting point above 170° C. is from 1 to less than 40%, relative to the total mass of the composite film.
17. 15. Use according to claim 14, characterized in that the mass proportion of layer components having a melting point above 170° C. is from 1 to less than 40%, relative to the total mass of the composite film.
Citation Information
Patent Citations
Simultaneously oriented PLA film with improved mechanical properties
US20100151219A1
Sealable and Peelable Polyester Film
US20170321024A1
BI-axially oriented and heat-set multilayer thermoplastic film for packaging
WO2001068363A1
Deep-drawing packaging container, deep-drawing package, and method for production of the packaging container or the package
WO2008038776A1
Cited By
Method for producing multi-layer composite film, multi-layer composite film and use thereof