Composite, antibacterial agent, and method for producing the composite
By forming a composite of silver nanoparticles on biomass nanofibers through pressurized fluidization and centrifugation, the composite achieves better antibacterial performance and efficient production, addressing the limitations of previous methods.
Patent Information
- Application Number
- JP2021092114
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-01
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-06-01
AI Technical Summary
Existing methods struggle to create a composite of small-sized silver nanoparticles effectively attached to biomass nanofibers, particularly those with a relatively small degree of polymerization, leading to insufficient antibacterial performance and inefficient manufacturing processes.
A composite is formed by precipitating and immobilizing silver nanoparticles with a predetermined particle size on biomass nanofibers with a specific degree of polymerization, using a pressurized fluidization and centrifugation process, ensuring 100% coverage of biomass nanofibers with silver nanoparticles of 9 nm or less and controlled standard deviation.
The composite exhibits enhanced antibacterial effects and is produced more efficiently, with improved manufacturing processes that maintain the inherent properties of silver nanoparticles.
Smart Images

Figure 0007595861000002 
Figure 0007595861000003 
Figure 0007595861000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite, an antimicrobial agent, and a method for producing the composite. [Background technology]
[0002] In recent years, in the fields of medicine and the environment, the use of composites of silver nanoparticles and nanofibers has been proposed as materials that have the function of capturing, removing, or inactivating bacteria, viruses, etc. In particular, nanofibers derived from biomass (biomass nanofibers) such as cellulose nanofibers, chitin nanofibers, and chitosan nanofibers are expected to be effectively used as alternative materials to fossil fuel-derived materials.
[0003] For example, Patent Document 1 proposes a method for easily and efficiently producing a composite in which small-sized silver nanoparticles are attached to the surface of cellulose fibers. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-3175 A Summary of the Invention [Problem to be solved by the invention]
[0005] According to the method of Patent Document 1, a composite is obtained in which small-sized silver nanoparticles are attached to the surface of cellulose nanofibers; however, it is not possible to support a sufficient amount of silver nanoparticles on biomass nanofibers, which have a relatively low degree of polymerization, making it difficult to produce a composite that can satisfactorily exhibit the inherent effects of silver nanoparticles.
[0006] Therefore, an object of the present invention is to provide a composite that can exhibit the inherent effect of silver nanoparticles better than conventional ones when used in, for example, an antibacterial agent, and an antibacterial agent containing the composite. Another object of the present invention is to provide a method for producing the composite that can produce the composite more efficiently. [Means for solving the problem]
[0007] As a result of intensive research in light of the above-mentioned circumstances, the present inventors discovered that by precipitating and fixing silver nanoparticles of a predetermined particle size on biomass nanofibers of a predetermined degree of polymerization, the surface area of the silver nanoparticles can be increased, and a composite can be obtained in which the inherent effects of the silver nanoparticles can be better exhibited than before, and thus the present invention was completed.
[0008] [1] A composite containing biomass nanofibers and silver nanoparticles, wherein the silver nanoparticles are precipitated and fixed on the biomass nanofibers, the amount of the precipitated silver nanoparticles is 0.1 parts by mass or more per 100 parts by mass of the biomass nanofibers, the average particle diameter of the silver nanoparticles is 9 nm or less, and the degree of polymerization of the biomass nanofibers is 200 to 700. [2] The composite according to [1], wherein the standard deviation of the average particle size of the silver nanoparticles is less than 9 nm. [3] The composite described in [1] or [2], wherein the biomass nanofibers and the silver nanoparticles have a crystalline structure, and in X-ray diffraction measurement, a peak due to the biomass nanofibers is present at a diffraction angle (2θ) of 18 to 25°, and a peak due to the silver of the silver nanoparticles is present at a diffraction angle (2θ) of 35 to 43°. [4] The complex described in any one of [1] to [3], wherein the biomass nanofiber is a chitosan nanofiber. [5] An antibacterial agent comprising the complex according to any one of [1] to [4]. [6] A method for producing a composite according to any one of [1] to [4], comprising: a pressurized fluidization step of subjecting a raw material liquid containing biomass nanofibers and having a silver compound dissolved therein to a pressurized fluidization process at a pressure of 1 to 600 MPa using a wet jet mill; and a centrifugation step of subjecting the treated liquid that has undergone the pressurized fluidization process to a centrifugation process, the centrifugal force in the centrifugation process being 500 to 4,800 x g. Effect of the Invention
[0009] According to the present invention, it is possible to provide a composite that can exhibit the inherent effect of silver nanoparticles better than conventional ones when used in an antibacterial agent, etc., and an antibacterial agent containing the composite. It is also possible to provide a method for producing the composite that can produce the composite more efficiently. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a diagram showing the relationship between specific viscosity and molecular weight of chitosan. [Diagram 2] 1 shows XRD patterns of the composites of Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Complex] The composite of the present invention contains biomass nanofibers and silver nanoparticles, and is formed by depositing and immobilizing the silver nanoparticles on the biomass nanofibers. The average fiber diameter of the biomass nanofibers is 2 nm to 100 nm, and the amount of deposited silver nanoparticles is 0.1 parts by mass or more, preferably 2 to 100 parts by mass, and more preferably 10 to 50 parts by mass, per 100 parts by mass of the biomass nanofibers. If the amount of deposition is less than 1 part by mass, the amount of silver is small, and the antibacterial and other functions are reduced. The amount of precipitated silver nanoparticles can be determined by measurement using inductively coupled plasma (ICP) emission spectrometry.
[0012] The average particle size of the silver nanoparticles is 9 nm or less, preferably 2 to 8 nm, and more preferably 2 to 6 nm. If the average particle size exceeds 9 nm, the specific surface area becomes small, and the antibacterial effect and other effects cannot be fully exerted. The average particle size of the silver nanoparticles can be calculated from the silver nanoparticle size (n=about 50) measured based on a field emission scanning electron microscope (FE-SEM) image.
[0013] The standard deviation of the average particle size of the silver nanoparticles is preferably less than 9 nm, more preferably 2 to 6 nm, and even more preferably 0.1 to 4 nm. By having a standard deviation of less than 9 nm, the silver nanoparticles can be evenly fixed onto the surface of the biomass nanofibers, thereby further improving the effect expression of the silver nanoparticles.
[0014] The degree of polymerization of the biomass nanofibers is 200 to 700, preferably 200 to 670, and more preferably 200 to 650. If the degree of polymerization of the biomass nanofibers is less than 200, a three-dimensional network of the biomass nanofibers cannot be formed, and molding processability such as film formation or porous formation decreases, whereas if it exceeds 700, the specific surface area of the biomass nanofibers is small, and silver nanoparticles do not precipitate efficiently.
[0015] Here, the degree of polymerization of biomass nanofibers in this specification is also called the viscosity average degree of polymerization, and is measured as described below.
[0016] For example, when the biomass nanofibers are derived from cellulose (cellulose nanofibers), the degree of polymerization of the biomass nanofibers is calculated with reference to the following paper. TAPPI International Standard;ISO / FDIS 5351,2009.Smith,DK;Bampton, RF;Alexander, WJ Ind. Eng. Chem.,Process Des. Dev.1963, 2, 57-62.
[0017] Specifically, 30 g of a suspension in which biomass nanofibers are diluted with ion-exchanged water to a content of 2±0.3% by mass is dispensed into a centrifuge tube and left to freeze overnight in a freezer. The suspension is then dried in a freeze dryer for 5 days or more, and then heated in a constant temperature dryer set at 105°C for 3 to 4 hours to obtain bone-dry biomass nanofibers. To measure the reference, add 15 ml of pure water and 15 ml of 1 mol / L copper ethylenediamine to an empty 50 ml screw tube to prepare a 0.5 mol / L copper ethylenediamine solution. Place 10 ml of the above 0.5 mol / L copper ethylenediamine solution in a Cannon-Fenske viscometer, leave for 5 minutes, and measure the drop time at 25°C to obtain the solvent drop time.
[0018] Next, to measure the viscosity of the biomass nanofibers, 0.14 g to 0.16 g of bone-dry biomass nanofibers are weighed into an empty 50 ml screw tube and 15 ml of pure water is added. 15 ml of 1 mol / L copper ethylenediamine is then added and stirred for 10 minutes at 1000 rpm in a planetary super mixer to obtain a 0.5 mol / L copper ethylenediamine solution in which the biomass nanofibers are dissolved. As in the reference measurement, 10 ml of the prepared 0.5 mol / L copper ethylenediamine solution is placed in a Cannon-Fenske viscometer, left for 5 minutes, and the fall time at 25°C is measured. The fall time is measured three times, and the average value is taken as the fall time of the biomass nanofiber solution.
[0019] The degree of polymerization is calculated using the following formula from the mass of the bone-dry biomass nanofibers used in the measurement, the solvent dripping time, and the biomass nanofiber solution dripping time. Note that if the degree of polymerization is measured twice or more, it is the average value.
[0020] Mass of biomass nanofiber in an absolute dry state used for measurement: a(g) (where a is 0.14 or more and 0.16 or less) Cellulose concentration in solution: c = a / 30 (g / mL) Solvent drop time: t0 (sec) Fall time of biomass nanofiber solution: t (sec) Relative viscosity of the solution: η rel =t / t0 Specific viscosity of the solution: η sp = η rel -1 Intrinsic viscosity:[η]=η sp / c(1+0.28η sp ) Degree of polymerization: DP=[η] / 0.57
[0021] Furthermore, when the biomass nanofibers are derived from chitosan (chitosan nanofibers), the degree of polymerization of the biomass nanofibers is calculated as follows. The measurement solution is prepared by dissolving 50 mg of chitosan sample in 50 ml of 4% acetic acid aqueous solution and 50 ml of 0.6 M / L saline. Using a capillary tube with an inner diameter of 0.5 mm of a Shibata Ostwald viscometer, the time it takes for the sample to pass from the scribed line a to the scribed line b is measured and this time is defined as t.
[0022] Prepare a solution that does not dissolve chitosan, and measure the time it takes to pass from scribed line a to scribed line b in the same manner, and define this time as t0. Measure both t and t0 three times and use the average value.
[0023] Next, the specific viscosity is calculated from the formula: specific viscosity = t / t0-1. From the relationship between specific viscosity and molecular weight shown in Figure 1, the molecular weight corresponding to the calculated specific viscosity is read, and this value is used as the chitosan monomer unit (CH 11 The degree of polymerization is calculated by dividing the molecular weight of NO4) by 161.
[0024] Furthermore, when the biomass nanofibers are derived from chitin (chitin nanofibers), they are deacetylated to produce chitosan using the method described in Japanese Patent No. 3781733, and the degree of polymerization of the chitin nanofibers is calculated using the same method as for the chitosan nanofibers described above.
[0025] In X-ray diffraction measurement of the composite of the present invention, a peak due to the biomass nanofibers is present at a diffraction angle (2θ) of 18 to 25°, and a peak due to the silver of the silver nanoparticles is present at a diffraction angle (2θ) of 35 to 43°. The presence of these peaks indicates that the biomass nanofibers and silver have a crystalline structure. The X-ray diffraction measurement can be performed by the method described in the Examples.
[0026] The average fiber diameter of the biomass nanofibers is preferably 10 to 100 nm, more preferably 10 to 40 nm, and even more preferably 10 to 25 nm. The average fiber diameter of biomass nanofibers can be calculated from fiber diameters (approximately n = 20) measured based on electron microscope photographs or atomic force microscope images taken at an appropriate magnification.
[0027] Biomass nanofibers are produced by various production methods, but among them, the biomass nanofibers according to this embodiment are preferably mechanically defibrated biomass nanofibers produced by mechanical defibration.
[0028] Mechanically defibrated biomass nanofibers are obtained by cutting the raw biomass to a specified length using a beater or refiner, and then fibrillating or pulverizing (mechanically pulverizing) it using a high-pressure homogenizer, grinder, impact crusher, bead mill, etc.
[0029] On the other hand, chemically modified biomass nanofibers produced through chemical modification are obtained by making the raw biomass easier to pulverize by chemical treatment, and then pulverizing it by mechanical defibration. As a chemical treatment for chemically modified biomass nanofibers, there is a treatment in which a hydrophilic substituent is introduced into the biomass nanofiber, and all or part of the hydroxyl groups on the surface of the biomass nanofiber are replaced with hydrophilic functional groups, so that the biomass nanofibers are easier to pulverize by using the electrostatic repulsion between the biomass nanofibers. Examples of hydrophilic functional groups are carboxyl groups, phosphate groups, and sulfate groups. However, in the case of chemically modified biomass nanofibers, there are problems such as low heat resistance, and a chemical plant is required for chemical modification, and the production costs are high. In contrast, mechanically defibrated biomass nanofibers are not chemically modified during pulverization, and only an aqueous medium is used as a medium, so they are chemically and thermally stable, and can be produced only with a wet jet mill (high-pressure homogenizer) required for the present invention, so the production costs can be reduced. In addition, even if treated with a high-pressure homogenizer, the degree of polymerization of mechanically defibrated biomass nanofibers is less likely to decrease.
[0030] Here, the amount of hydrophilic functional groups, which are any of a carboxyl group, a phosphate group, and a sulfate group, introduced into the mechanically defibrated biomass nanofiber per glucose unit of the biomass is 0.1 mmol / g or less, and preferably 0.01 mmol / g or less. Here, the amount introduced can also be read as the content. The amount introduced (content) can be determined, for example, by measurement using a known conductometric titration method.
[0031] In addition, the mechanically defibrated biomass nanofibers have a content of any one of sodium, aluminum, and copper (preferably any two of each, more preferably any three of each, and even more preferably any four of each) of 0.1% by mass or less, and preferably 0.01% by mass or less. The content can be determined by elemental analysis such as high-frequency inductively coupled plasma atomic emission spectrometry, EPMA using an electron probe microanalyzer, or fluorescent X-ray analysis.
[0032] As the mechanically defibrated biomass nanofibers as described above, for example, BiNFi-s manufactured by Sugino Machine Ltd. can be used.
[0033] Here, the biomass nanofibers are preferably chitosan nanofibers. By using chitosan nanofibers, the amount of silver nanoparticles precipitated can be increased. This is presumably due to the amino groups in the chitosan nanofibers. In other words, it is believed that silver ions coordinate with the amino groups and chemically bond to them, resulting in the precipitation of a large amount of silver nanoparticles in a stable manner.
[0034] The composite of the present invention as described above is suitable for use as an antibacterial agent, as described below, as well as an antifungal agent, a deodorant, a catalyst, and the like.
[0035] [Antibacterial agents] The antibacterial agent of the present invention includes the above-mentioned complex of the present invention. The antibacterial agent can be used in textiles, washing machines, paints, varnishes, sinks and sanitary ceramics, disinfectants, deodorants, kitchen utensils, cosmetics, personal care products, etc.
[0036] [Method of manufacturing the composite] The method for producing a composite of the present invention includes a pressurized fluidization process in which a raw material liquid containing biomass nanofibers and having a silver compound dissolved therein is subjected to a pressurized fluidization process, and then a centrifugation process in which the raw material liquid is subjected to a centrifugation process. Each step will be described below.
[0037] (Pressurized fluidization process) In the pressurized fluidization step, the raw material liquid containing the biomass nanofibers and the silver compound dissolved therein is subjected to a pressurized fluidization treatment at a pressure of 1 to 600 MPa using a wet jet mill.
[0038] The method for preparing the raw material liquid is not particularly limited. Biomass nanofibers may be dispersed in an aqueous solution in which a silver compound is dissolved (aqueous silver compound solution), or a silver compound may be dissolved in a dispersion in which biomass nanofibers are dispersed (biomass nanofiber dispersion). The aqueous silver compound solution and the biomass nanofiber dispersion may also be mixed.
[0039] From the viewpoint of obtaining a liquid in which the biomass nanofibers and silver compound are uniformly dispersed and dissolved, the biomass nanofiber concentration in the biomass nanofiber dispersion is not particularly limited, but is preferably 0.01 to 20 mass% in terms of solid content concentration. The concentration of the silver compound in the aqueous silver compound solution is not particularly limited, but is preferably 0.001 to 2 mol / L. The solvent or dispersion medium in the aqueous silver compound solution and the biomass nanofiber dispersion is usually water, but may contain a small amount of an organic solvent.
[0040] The raw material liquid prepared as described above is treated at a pressure of 1 to 600 MPa using a wet jet mill (pressurized fluidization treatment). If the pressure is less than 1 MPa, a composite in which silver nanoparticles are attached to the surface of the cellulose fiber cannot be obtained. From the viewpoint of increasing the amount of silver nanoparticles attached to the surface of the cellulose fiber, the pressure is preferably 10 MPa or more, more preferably 30 MPa or more, even more preferably 80 MPa or more, and particularly preferably 100 MPa or more.
[0041] On the other hand, if the pressure exceeds 600 MPa, the production costs will be too high and it is not industrially practical. From the viewpoint of reducing the variation in particle size of the silver nanoparticles, the pressure is preferably 300 MPa or less, more preferably 250 MPa or less, and even more preferably 200 MPa or less.
[0042] The liquid temperature when the raw material liquid is treated using a wet jet mill is set in relation to the pressure, but is preferably room temperature to 90° C. The treatment time is not particularly limited and is appropriately determined depending on the amount of the liquid to be treated.
[0043] Here, the wet jet mill is a device that applies pressure to the raw material aqueous solution or dispersion and pulverizes it by utilizing the shear force generated when the raw material passes through a slit. Wet jet mills are also called high-pressure homogenizers.
[0044] From the viewpoint of obtaining a desired amount of precipitated silver nanoparticles, the pressurized fluidization treatment using a wet jet mill may be carried out multiple times at the same pressure or different pressures.
[0045] (Centrifugation process) In the centrifugation process, the treatment liquid that has been subjected to the pressurized fluidization process is subjected to a centrifugation process. Here, the centrifugal force in the centrifugation process is set to 500 to 4800×g. If the centrifugal force is less than 500 g, it is difficult to efficiently collect the composite of biomass nanofibers and silver nanoparticles, and if it exceeds 4800 g, silver nanoparticles with a large specific gravity will be detached and even amorphous biomass nanofibers will be collected. The centrifugal force is preferably set to 2000 to 3800 g.
[0046] In terms of improving the recovery amount of the composite of biomass nanofibers and silver nanoparticles and removing unreacted silver ions and counter ions, the centrifugation process may also be performed multiple times, alternating between centrifugation at the same or different centrifugal forces and a washing step after adding water.
[0047] The composite of the present invention is produced through the above-mentioned steps. If necessary, the composite may be subjected to a treatment such as drying. EXAMPLES
[0048] The present invention will be described in more detail below with reference to examples, but these examples are not intended to limit or restrict the present invention in any way.
[0049] [Example 1] 500 mL of 2 mass% chitosan nanofiber (ChNF suspension, manufactured by Sugino Machine Ltd., product name: BiNFi-s Chitosan EFo-08002, chitosan nanofiber polymerization degree: 480) was prepared. 500 mL of an aqueous solution of silver nitrate (manufactured by Wako Pure Chemical Industries, Ltd.) was prepared so that the mass ratio of Ag (metal equivalent):chitosan nanofiber was 1:1. Then, a treatment was performed once at a pressure of 100 MPa using a high-pressure wet jet mill (Starburst manufactured by Sugino Machine Ltd.) (pressurized fluidization process). The treatment liquid was centrifuged at 2,800×g for 5 minutes using a centrifuge (Suprema 21; manufactured by Tommy Kogyo Co., Ltd.) (centrifugation step), and the precipitate was collected. Ion-exchanged water was added to the precipitate, and it was redispersed, and then centrifuged again under the same conditions to remove unreacted silver nitrate (washing step). This washing step was carried out twice in total. The obtained precipitate (complex) was used as the sample.
[0050] [Example 2] The precipitate was recovered in the same manner as in Example 1, except that the pressurized fluidization treatment using the high-pressure wet jet mill in the pressurized fluidization step was repeated five times, and the resulting precipitate (composite) was used as a sample.
[0051] [Example 3] Instead of 2% by mass of chitosan nanofiber, 500 mL of 2% by mass of cellulose nanofiber (CNF suspension, manufactured by Sugino Machine Ltd., product name: BiNFi-s Cellulose FMa-10002, cellulose nanofiber polymerization degree: 200) was prepared and used. The precipitate was recovered in the same manner as in Example 1, except for this. The obtained precipitate (composite) was used as the sample.
[0052] [Example 4] Instead of 2% by mass of chitosan nanofiber, 500 mL of 2% by mass of cellulose nanofiber (CNF suspension, manufactured by Sugino Machine Ltd., product name: BiNFi-s Cellulose WFo-10002, cellulose nanofiber polymerization degree: 650) was prepared and used. Except for this, the procedure was the same as in Example 1, and the precipitate was recovered, and the resulting precipitate (composite) was used as the sample.
[0053] [Comparative Example 1] The precipitate was collected in the same manner as in Example 1, except that the centrifugal force in the centrifugation step was set to 12,000×g, and the resulting precipitate (complex) was used as a sample.
[0054] [Comparative Example 2] The procedure was the same as in Example 1, except that 500 mL of 2 mass% cellulose nanofiber (CNF suspension, manufactured by Sugino Machine Ltd., product name: BiNFi-s Cellulose IMa-10002, cellulose nanofiber polymerization degree: 800) was prepared and used instead of 2 mass% chitosan nanofiber, and that centrifugation was performed at 4,800 x g. The precipitate was recovered, and the resulting precipitate (composite) was used as the sample.
[0055] [Comparative Example 3] The precipitate was collected in the same manner as in Example 1, except that the centrifugation step was omitted, and the obtained precipitate (complex) was used as a sample.
[0056] The samples obtained in each of the Examples and Comparative Examples were evaluated for the following physical properties. The results are shown in Table 1.
[0057] [Physical property evaluation] (1) X-ray diffraction measurement (peak confirmation) The collected samples were freeze-dried and then pulverized with a cutter mill to obtain powder samples. The obtained powder samples were immediately subjected to powder X-ray diffraction measurement (XRD, Smart Lab, Rigaku Corporation, voltage: 45 kV, current: 200 mA, 2θ=10°-50°, step width: 0.02°, scan speed: 1° / min, tube: Cu) so as not to change the crystal structure of the samples, and the crystal phase was identified (presence or absence of peaks). Only for the XRD measurement, freeze-dried samples were used. The XRD patterns of the composites of Example 1 and Comparative Example 1 are shown in FIG. 2.
[0058] (2) Calculation of the average particle size and standard deviation of Ag nanoparticles The collected samples were observed using a field emission scanning electron microscope (FE-SEM, SU8220, Hitachi High-Technologies Corporation, accelerating voltage: 1.0 kV), and the average particle size and standard deviation of Ag nanoparticles (n=50) were calculated. The freeze-dried products were used as samples for observation.
[0059] (3) Ag nanoparticle content (precipitation amount) The silver content in the sample was measured three times and calculated by ICP emission spectroscopy (ICP, iCAP6500Duo, Thermo Fisher Scientific Co., Ltd.). 10 ml of (1+1) nitric acid was added to the paste sample, heated on a sand bath at 250°C for 30 minutes, and solid-liquid separation was performed by filtration (No. 5B, Advantec Toyo Co., Ltd.). The filtrate was adjusted to a constant volume of 50 ml to prepare the solution for ICP measurement.
[0060] (Antibacterial Test) The obtained samples were subjected to antibacterial tests as described below. A sample was prepared by diluting 5% by mass of biomass nanofiber-silver nanoparticle composite 50 times with ion-exchanged water. This sample was sprayed onto a cellulose nonwoven fabric to coat it. The cellulose nonwoven fabric coated with the biomass nanofiber-silver nanoparticle composite was placed on a Petrifilm (AC plate, 3M Japan Co., Ltd.), and a non-sterile cellulose nanofiber aqueous dispersion (inoculation) was dripped onto it. After culturing at 32°C for 48 hours, samples that showed colonies were judged to have no antibacterial activity (×), and samples that showed no colonies were judged to have antibacterial activity (◯).
[0061] [Table 1]
[0062] As can be seen from Table 1, the inherent effect of silver was better expressed in the Examples than in any of the Comparative Examples. In Comparative Example 3, the centrifugation step was not provided, so that even unreacted silver nitrate was recovered, making it impossible to measure and evaluate.
Claims
1. A composite including biomass nanofibers and silver nanoparticles, The silver nanoparticles are precipitated and fixed on the biomass nanofibers, The amount of the silver nanoparticles precipitated is 0.1 parts by mass or more per 100 parts by mass of the biomass nanofibers, The average particle size of the silver nanoparticles is 9 nm or less, The degree of polymerization of the biomass nanofibers is 200 to 700; The antibacterial agent, wherein the biomass nanofibers are chitosan nanofibers.
2. The antibacterial agent according to claim 1 , wherein the standard deviation of the average particle size of the silver nanoparticles is less than 9 nm.
3. The antibacterial agent according to claim 1 or 2, wherein the biomass nanofibers and the silver nanoparticles have a crystalline structure, and in X-ray diffraction measurement, a peak due to the biomass nanofibers is present at a diffraction angle (2θ) of 18 to 25°, and a peak due to the silver of the silver nanoparticles is present at a diffraction angle (2θ) of 35 to 43°.
4. An antibacterial agent described in any one of claims 1 to 3, wherein the amount of precipitated silver nanoparticles is 10 parts by mass or more per 100 parts by mass of the biomass nanofibers.
5. A method for producing the antibacterial agent according to any one of claims 1 to 4, comprising the steps of: The method includes a pressurized fluidization process in which a raw material liquid containing biomass nanofibers and having a silver compound dissolved therein is subjected to a pressurized fluidization process at a pressure of 1 to 600 MPa using a wet jet mill, and a centrifugation process in which the treated liquid that has been subjected to the pressurized fluidization process is subjected to a centrifugation process, The method for producing an antibacterial agent, wherein the centrifugal force in the centrifugation treatment is 500 to 4800 × g.
Citation Information
Patent Citations
Method for preparing silver-loaded chitosan medical dressing
CN106729931A
Antiviral stock
JP2017150117A
Method for producing composite
JP2018003175A
Method for producing biomass nanofiber dry body and method for producing biomass nanofiber resin composite
JP2019131772A