Method for activating lithium secondary battery containing positive electrode additive
The method addresses structural instability in lithium secondary batteries by employing multi-stage activation with degassing and pressurization to form a stable SEI film, improving electrical performance and safety.
Patent Information
- Application Number
- JP2022568933
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-04-07
- Filing Date
- 2022-04-19
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2042-04-19
AI Technical Summary
Conventional lithium secondary battery additives are structurally unstable, leading to oxygen gas generation, electrode expansion, and decreased electrical conductivity, limiting high-speed charging and discharging capabilities and battery safety.
A method involving multiple activation stages with degassing processes at varying State of Charge (SOC) levels, including low and high-rate charging, and pressurization to remove gases, forming a stable Solid Electrolyte Interphase (SEI) film, using specific positive electrode additives like lithium cobalt oxide, and optimizing electrode composition.
Improves electrical performance and safety by reducing gas generation, preventing electrode expansion, and enhancing the stability and efficiency of lithium secondary batteries.
Smart Images

Figure 0007595963000001 
Figure 0007595963000002 
Figure 0007595963000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority to Korean Patent Application No. 10-2021-0071222, filed June 2, 2021, and Korean Patent Application No. 10-2022-0043177, filed April 7, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a method for activating a lithium secondary battery containing a positive electrode additive. [Background technology]
[0003] With the development of technology and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and working potential, long cycle life, and low self-discharge rate, have been commercialized and are widely used.
[0004] Recently, as lithium secondary batteries are used as power sources for medium- to large-sized devices such as electric vehicles, there is an increasing demand for high capacity, high energy density, and low cost of lithium secondary batteries, and the irreversible additives used in electrodes are also required to have higher irreversible capacity. However, there is a limit to the development of positive electrode additives having such high irreversible capacity.
[0005] Meanwhile, conventional irreversible additives such as Li6CoO4 are generally prepared by reacting cobalt oxide with an excess amount of lithium oxide. The irreversible additives prepared in this way are structurally unstable and generate a large amount of oxygen gas (O2) as charging proceeds, as described below. If the irreversible additives do not all react during the initial charging of the secondary battery and remain, they may react during the charging and discharging process performed after the initial charging to generate a large amount of oxygen gas inside the battery. The oxygen gas thus generated may induce volume expansion of the electrode assembly, and act as one of the main factors that cause a deterioration in battery performance.
[0006] [ka]
[0007] In addition, the non-reversible additives that have been commonly used in the past have a 2D percolating network that makes them nearly non-conductive up to 10 -11 It exhibits very low powder electrical conductivity of 1.5 S / cm. Such low powder electrical conductivity increases the electrical resistance of the positive electrode, and in this case, a large capacity of 200mAh / g or more is shown at a low C-rate, but as the C-rate increases, the performance rapidly decreases as charging and discharging proceeds due to the large resistance, so the charge and discharge capacity of the battery decreases and high-speed charging and discharging is difficult.
[0008] Therefore, there is a demand for the development of lithium secondary batteries that have excellent electrical performance and improved battery safety. Summary of the Invention [Problem to be solved by the invention]
[0009] SUMMARY OF THE PRESENTLY PREFERRED EMBODIMENTS Accordingly, an object of the present invention is to provide a method for activating a lithium secondary battery, which can improve the electrical performance and safety of the lithium secondary battery. [Means for solving the problem]
[0010] In order to solve the above problems, in one embodiment, the present invention provides a method for activating a lithium secondary battery containing an electrode assembly having a positive electrode containing a positive electrode active material and a positive electrode additive, and an electrolyte, the method comprising the step of charging the lithium secondary battery to a State of Charge (SOC) of 90% or more.
[0011] In this case, during the activation step, a degassing process for removing gas from inside the secondary battery is performed at least once during the charging process at SOC 90% or more.
[0012] In one embodiment, the activation step is divided into two or more steps according to the SOC level of the lithium secondary battery, and the degassing step is performed between the steps divided according to the SOC level of the lithium secondary battery.
[0013] In yet another embodiment, the activation step is divided into two or more steps according to the SOC level of the lithium secondary battery, and in an early step where the SOC level is low, low-rate charging of 0.5C or less is performed, and in a later step where the SOC level is high, high-rate charging of more than 0.5C is performed.
[0014] In a specific embodiment, the degassing step can be carried out two or three times.
[0015] In yet another embodiment, the activation step may include an activation step 1 in which the lithium secondary battery is charged at SOC 20% or less, an activation step 2 in which the lithium secondary battery after the activation step 1 is charged at SOC 20% or more and 40% or less, an activation step 3 in which the lithium secondary battery after the activation step 2 is charged at SOC 40% or more and 70% or less, and an activation step 4 in which the lithium secondary battery after the activation step 3 is charged at SOC 90% or more. In this case, a degassing process can be performed after at least one of the activation steps 1 to 3.
[0016] In a specific embodiment, a degassing step can be carried out after each of the first to third activation steps. In this case, the degassing step is carried out three times.
[0017] In still another specific embodiment, the first activation stage is low-rate charging at 0.5 C or less, and the second to fourth activation stages are high-rate charging at more than 0.5 C. For example, the first activation stage is performed by charging the lithium secondary battery with a constant current in the range of 0.01 C to 0.2 C, and the second to fourth activation stages are performed by charging the lithium secondary battery with a constant current in the range of 0.15 C to 1 C.
[0018] The degassing process may be carried out in a vacuum state.
[0019] The activation step may further include a step of pressurizing the lithium secondary battery, and may be performed under a temperature condition of 40° C. to 70° C. The activation step may be performed under a voltage condition of 3.3V to 4.5V.
[0020] Moreover, the positive electrode additive may be a lithium cobalt oxide represented by the following chemical formula 1:
[0021] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0022] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0023] Specifically, in the above chemical formula 1, M 1 is a Zn element, and q may be a compound in which 0.2≦q≦0.4.
[0024] The content of the positive electrode additive may be 0.1 to 5% by weight based on the total weight of the positive electrode mixture layer.
[0025] After the activation step, an aging step of aging the activated lithium secondary battery at a temperature of 40°C to 80°C may be included.
[0026] In one embodiment, the present invention provides a battery comprising an electrode assembly including a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, and an electrolyte, The positive electrode comprises a positive electrode current collector, and a positive electrode mixture layer located on the positive electrode current collector and including a positive electrode active material, a positive electrode additive represented by the following chemical formula 1, a conductive material, and a binder; The positive electrode active material is a lithium nickel composite oxide represented by the following chemical formula 2, providing a lithium secondary battery.
[0027] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0028] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u
[0029] In the above chemical formulas 1 and 2, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively; M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the range of 1.0≦x≦1.30, 0.1≦y<0.95, and 0.01, respectively. <z≦0.5、0.01<w≦0.5、0≦v≦0.2、1.5≦u≦4.5である。
[0030] The negative electrode may include a negative electrode current collector and a negative electrode mixture layer located on the negative electrode current collector and containing a negative electrode active material, and the negative electrode active material may contain a carbon material and a silicon material.
[0031] Moreover, the silicon substance may be contained in an amount of 1 to 20 parts by weight per 100 parts by weight of the negative electrode mixture layer. Effect of the Invention
[0032] The activation method of the lithium secondary battery according to the present invention has an advantage that by-reaction gases can be removed by performing a degassing process during activation, and thus a stable SEI film can be formed on the surface of the electrode, improving the battery performance and improving the safety of the battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] Although the present invention can be modified in various ways and can have various embodiments, a specific embodiment will be described in detail in the detailed description.
[0034] However, it should be understood that this is not intended to limit the invention to the particular embodiment, but rather to include all modifications, equivalents, or alternatives falling within the spirit and scope of the invention.
[0035] In the present invention, the terms "comprise" or "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0036] In addition, in the present invention, when a part such as a layer, film, region, or plate is described as being "on" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part in between. Conversely, when a part such as a layer, film, region, or plate is described as being "under" the other part, this includes not only the case where it is "directly under" the other part, but also the case where there is another part in between. In addition, in the present application, being "located on" can include not only the case where it is located at the top, but also the case where it is located at the bottom.
[0037] The present invention will now be described in more detail.
[0038] <How to activate lithium secondary batteries> In one embodiment, the present invention provides a method for activating a lithium secondary battery containing an electrode assembly including a positive electrode containing a positive active material and a positive electrode additive, and an electrolyte, comprising the step of activating the lithium secondary battery to a state of charge (SOC) of 90% or more. In this case, during the activation step, a degassing process for removing gas from inside the secondary battery may be performed one or more times.
[0039] Specifically, the activation step involves charging the lithium secondary battery to a SOC (State of Charge) of 90% or more, 90-100%, 90-99.9%, 95-100%, or 95-99%. In the present invention, the activation step includes substantially fully charging the lithium secondary battery.
[0040] The activation method of a lithium secondary battery according to the present invention is a method for a lithium secondary battery containing an irreversible additive, i.e., a cathode additive, in a cathode, which is added to replenish lithium ions lost due to an irreversible reaction occurring in the anode during initial charging, and has the effect of increasing the delithiation efficiency of the cathode additive contained in the cathode during initial charging of the battery.
[0041] For this purpose, the activation method of the lithium secondary battery according to the present invention includes an activation step of charging a lithium secondary battery containing a positive electrode additive together with a positive electrode active material in a positive electrode at SOC 100%, and a degassing step for removing gas inside the lithium secondary battery is performed at least once during the activation step. In general, a large amount of gas is generated inside a lithium secondary battery due to delithiation and / or decomposition of a positive electrode additive contained in a composite layer of a positive electrode, and if this gas is not removed, it may induce volume expansion of the electrode assembly, causing a decrease in battery performance. In the present invention, the degassing step is performed at least once during the activation step to prevent volume expansion of the electrode assembly and reduce the content of the total amount of gas generated during charging. That is, by removing by-reaction gases through the degassing step during the activation step, a strong SEI film is formed due to a reduction in resistance between the electrolyte and the electrode interface, thereby improving the performance of the battery.
[0042] In one example, the activation step is divided into two or more steps according to the SOC level of the lithium secondary battery, and the degassing step is performed between the steps divided according to the SOC level of the lithium secondary battery. In a specific example, the degassing step can be performed two or three times.
[0043] In yet another embodiment, the activation step is divided into two or more steps according to the SOC level of the lithium secondary battery. In an early stage where the SOC level is low, low-rate charging is performed at 0.5C or less, and in a later stage where the SOC level is high, high-rate charging is performed at a rate exceeding 0.5C. Specifically, in the early stage, low-rate charging is performed at a rate in the range of 0.1-0.5C, 0.1-0.4C, or 0.15-0.3C. In addition, in a later stage where the SOC level is high, high-rate charging is performed at a rate in the range of more than 0.5 and 10C or less, 0.8-5C, or 0.8-1.2C. This is to induce stable formation of an SEI film through low-rate charging in the early stage of charging, and to increase process efficiency through high-rate charging in the later stage of charging.
[0044] Meanwhile, in one embodiment, the activation step in the activation method of the lithium secondary battery according to the present invention may include a total of four steps. In a specific example, the present invention may include an activation step 1 in which the lithium secondary battery is charged at SOC 20% or less, an activation step 2 in which the lithium secondary battery after the activation step 1 is charged at SOC 20% or more and 40% or less, an activation step 3 in which the lithium secondary battery after the activation step 2 is charged at SOC 40% or more and 70% or less, and an activation step 4 in which the lithium secondary battery after the activation step 3 is charged at SOC 100%. In this case, a degassing process can be performed after at least one of the activation steps 1 to 3.
[0045] When a lithium secondary battery is initially charged, lithium ions originating from the positive electrode active material and the lithium transition metal oxide such as the positive electrode additive contained in the positive electrode move to the carbon electrode of the negative electrode. The lithium ions are highly reactive and react with the carbon negative electrode to form compounds such as Li2CO3, LiO, and LiOH, and these compounds form an SEI film on the surface of the negative electrode. The SEI film is a non-conductor formed when the amount of ion movement in the battery increases. When the SEI film is formed, it prevents the lithium ions from reacting with other materials at the negative electrode during subsequent charging of the secondary battery, and acts as a kind of ion tunnel to allow only the lithium ions to pass through. When the SEI film is formed, the lithium ions do not react with the negative electrode or other materials, so the amount of lithium ions is reversibly maintained, and the charge and discharge of the secondary battery is reversibly maintained, thereby improving the life of the secondary battery. Even when left at high temperatures or repeatedly charged and discharged, the battery does not easily break down, so there is little change in thickness.
[0046] The first activation stage of the present invention can be said to be a stage in which lithium ions derived from the positive electrode active material of the positive electrode and / or the positive electrode additive form an SEI film (solid electrolyte interphase) on the surface of the negative electrode. The second activation stage can be said to be a stage in which a current is applied to the lithium secondary battery that has undergone the first activation stage to induce delithiation and decomposition of the lithium ions of the positive electrode additive, thereby charging the battery and simultaneously forming gas derived from the positive electrode additive inside the battery. The third and fourth activation stages can be said to be stages in which a current is applied to the lithium secondary battery that has undergone the second activation stage to complete the initial charging of the battery so that the SOC (State of Charge) is satisfied at a certain level.
[0047] Meanwhile, in the activation method of the lithium secondary battery according to the present invention, a degassing process may be performed after at least one of the first to third activation steps. Alternatively, in the activation method of the lithium secondary battery according to the present invention, a degassing process may be performed sequentially after each of the first to third activation steps. In a specific example, the activation method of the lithium secondary battery according to the present invention is Activation stage 1 → Degassing process → Activation stage 2 → Activation stage 3 → Activation stage 4; Activation stage 1 → Activation stage 2 → Degassing process → Activation stage 3 → Activation stage 4; Activation stage 1 → Degassing process → Activation stage 2 → Degassing process → Activation stage 3 → Activation stage 4; Activation stage 1 → degassing process → activation stage 2 → activation stage 3 → degassing process → activation stage 4; Activation stage 1 → Activation stage 2 → Degassing step → Activation stage 3 → Degassing step → Activation stage 4; or It is possible to carry out activation stage 1 → degassing process → activation stage 2 → degassing process → activation stage 3 → degassing process → activation stage 4, etc.
[0048] Meanwhile, the activation step may include a process of pressurizing the lithium secondary battery. In a specific example, the activation process of a lithium secondary battery including the positive electrode additive of Chemical Formula 1 may include a process of pressurizing the lithium secondary battery during charging, so that gas generated during the activation process is discharged to the outside of the battery without remaining inside the battery. That is, the process of charging the lithium secondary battery to SOC 100% may be performed under a pressurized condition where a predetermined pressure is applied. Here, pressurizing the lithium secondary battery means pressurizing a portion in which the electrode assembly is accommodated, and the lithium secondary battery may be pressurized to collect gas generated during the activation process in a gas pocket portion.
[0049] The pressurization process can be performed by using a common pressurizing member such as a pressurizing tool to pressurize the lithium secondary battery. At this time, the pressure applied to the lithium secondary battery is 0 kgf / cm. 2 Excess 20kgf / cm 2 or 0.5 kgf / cm 2 ~15kgf / cm 2 or 1kgf / cm 2 ~10kgf / cm 2 If the pressure is too high, the battery may be damaged by excessive pressure.
[0050] In addition, the degassing process is for removing gas from inside the lithium secondary battery, and may be performed without being limited to a method commonly used in the battery field. The degassing process may also include the pressurizing process described above. For example, in the activation step, a gas pocket is pierced to form a hole, and the chamber in which the lithium secondary battery is housed is made into a vacuum state, and the lithium secondary battery gas is discharged to the outside through the hole and removed. Then, the open portion may be sealed.
[0051] In another example, when degassing steps are performed sequentially after each activation step, the gases can be removed in the degassing steps under the same conditions or different conditions.
[0052] As described above, the second activation stage is a stage where gas derived from the positive electrode additive is formed, and in the second to fourth activation stages, a degassing process may be performed for a longer period of time than in the first activation stage, or a higher pressure may be applied during charging, but is not limited thereto.
[0053] In addition, the first activation stage may involve low-rate charging at 0.5C or less, and the second to fourth activation stages may involve high-rate charging at over 0.5C. Specifically, the first activation stage may involve charging the lithium secondary battery at a rate in the range of 0.1-0.5C, 0.1-0.4C, or 0.15-0.3C. In addition, the second to fourth activation stages may involve charging the lithium secondary battery at a rate in the range of over 0.5 and 10C or less, 0.8-5C, or 0.8-1.2C. This is because the first activation stage involves charging at a low constant current, and the second to fourth activation stages involve charging at a relatively high constant current, thereby improving both the stability of the battery and the process efficiency.
[0054] Also, the activation step may be performed under a voltage condition of 0.1 V to 4.5 V. The voltage condition in the activation step is a charging voltage, and for example, the activation 1 step may be performed under a voltage condition of 3.3 V to 3.6 V, and the activation 2 step to the activation 4 step may be performed under a voltage condition of 3.4 V to 3.7 V, respectively.
[0055] By controlling the voltage conditions of each activation step as described above, the present invention can uniformly form an SEI film in activation step 1, and after the SEI film is formed, the redox reaction of the positive electrode active material, i.e., the reversible reaction rate of the positive electrode active material is maintained low in activation steps 2 to 4, while promoting the phase change of the positive electrode additive, thereby inducing delithiation of the positive electrode additive at a high rate during initial charging. In addition, it is possible to prevent charging at low voltage conditions outside the above-mentioned voltage conditions in activation steps 2 to 4, which would result in insufficient induction of irreversible reactions of the positive electrode additive, and to prevent problems such as reduced battery life and capacity and instantaneous generation of excessive gas, which would result in reduced safety, caused by charging at high voltages outside the above-mentioned voltage conditions.
[0056] In addition, the activation method of the lithium secondary battery according to the present invention can increase the SOC stepwise by performing each activation step. For example, the SOC of the lithium secondary battery having undergone the first activation step may be 10% or less to form an SEI film, the SOC of the lithium secondary battery having undergone the second activation step may be more than 10% and less than 40% to sufficiently induce the irreversible reaction of the positive electrode additive to generate gas in the battery, and the SOC of the lithium secondary battery having undergone the third activation step may be more than 40% and less than 70%.
[0057] As an example, the activation method of the lithium secondary battery according to the present invention can adjust the SOC of the first activation stage to 10-18%, the SOC of the second activation stage to 30-38%, the SOC of the third activation stage to 60-70%, and the SOC of the fourth activation stage to 100%.
[0058] Also, each activation step may be performed at a temperature higher than room temperature in order to reduce the resistance of the electrode. Specifically, each activation step may be performed at a temperature of 40°C to 70°C, more specifically, at a temperature of 40°C to 60°C, 45°C to 60°C, 50°C to 65°C, 50°C to 60°C, or 52°C to 58°C. In the present invention, each activation step is performed at a temperature satisfying the above range, so that the secondary battery can be charged under a lower resistance condition of the positive electrode, thereby increasing the efficiency of the activation step and improving the uniformity of the SEI coating formed in one activation step.
[0059] In addition, the execution time of each activation step may be from 1 minute to 100 minutes, specifically, from 1 minute to 100 minutes; from 1 minute to 60 minutes; from 1 minute to 40 minutes; from 10 minutes to 40 minutes; from 20 minutes to 40 minutes; from 10 minutes to 30 minutes; from 1 minute to 10 minutes; and from 2 minutes to 9 minutes, respectively.
[0060] As an example, the activation step 1 may be performed for 2 to 8 minutes, the activation step 2 may be performed for 30 to 39 minutes, and the activation step 3 may be performed for 21 to 29 minutes, but is not limited to these.
[0061] In addition, the activation method of the lithium secondary battery according to the present invention may further include an aging step of aging the activated lithium secondary battery after the three activation steps. The aging step may allow the SEI coating to be more stabilized and re-formed with a uniform thickness by thermal energy and electrochemical energy. To this end, the aging step may be performed at 40 to 80°C, 50 to 70°C, 55 to 65°C, or about 60°C for 0.5 to 30 hours.
[0062] In addition, after the fourth activation step or the aging step, a degassing step may be performed to remove gas generated within the lithium secondary battery. Gas generated within the battery may cause swelling of the battery, so the degassing step can remove the generated gas.
[0063] <Lithium secondary battery> In one embodiment, the present invention comprises: A positive electrode and A negative electrode; an electrode assembly including a separator disposed between a positive electrode and a negative electrode; and an electrolyte.
[0064] In this case, the positive electrode includes a positive electrode current collector and a positive electrode mixture layer produced by applying a positive electrode slurry onto the positive electrode current collector, drying and pressing the positive electrode mixture layer, and the positive electrode mixture layer has a configuration containing a positive electrode active material, a positive electrode additive, a conductive material and a binder.
[0065] In a specific example, the positive electrode additive may be lithium cobalt oxide represented by the following formula 1:
[0066] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0067] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0068] Specifically, in the above formula 1, M 1 is a Zn element, and q may be 0.2≦q≦0.4.
[0069] The positive electrode additive contains an excess of lithium and can provide lithium to replace lithium consumption that occurs due to irreversible chemical and physical reactions at the negative electrode during initial charging, thereby increasing the charging capacity of the battery and reducing the irreversible capacity, thereby improving the life characteristics.
[0070] As such a positive electrode additive, the present invention may include a lithium cobalt oxide represented by Chemical Formula 1. In this case, the lithium cobalt oxide represented by Chemical Formula 1 may be Li6CoO4, Li6Co 0.5 Zinc 0.5 O4, Li6Co 0.7 Zinc 0.3 O4, etc. may be used alone or in combination. The lithium cobalt oxide represented by Chemical Formula 1 has a higher lithium ion content and a lower voltage range required for delithiation compared to nickel-containing oxides commonly used in the industry, and therefore has the advantage that lithium ions can be desorbed without affecting the reaction of the positive electrode active material during battery activation.
[0071] In addition, the lithium cobalt metal oxide represented by the above formula 1 may have a tetragonal crystal structure, and may have a space group of P42 / nmc. In general, lithium metal oxides having a tetragonal crystal structure have a tetrahedral structure formed by cobalt and oxygen elements, and have a structurally unstable structure. Due to this structural instability, gas including oxygen gas is generated during charging after activation of the battery. In the present invention, the decomposition and / or delithiation efficiency of the positive electrode additive during initial charging can be significantly improved by continuously performing three activation steps under current and voltage conditions that satisfy a specific range, and therefore the charge / discharge capacity of the lithium secondary battery can be improved and the amount of oxygen gas (O2) generated during charging and discharging after the initial charging can be significantly reduced.
[0072] The content of the positive electrode additive may be 0.1 to 5 parts by weight, specifically 0.1 to 3 parts by weight, or 1 to 3 parts by weight, relative to 100 parts by weight of the total positive electrode mixture layer.
[0073] Moreover, the mixture layer may further contain a conductive material, a binder, an additive, and the like in addition to the positive electrode active material and the positive electrode additive.
[0074] On the other hand, the positive electrode used in the present invention comprises a composite layer formed on a current collector, and the composite layer contains a positive electrode active material that exhibits electrical activity and a positive electrode additive that imparts irreversible capacity.
[0075] The positive electrode mixture layer may include a lithium nickel composite oxide represented by the following Chemical Formula 2 as a positive electrode active material capable of reversible intercalation and deintercalation:
[0076] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u
[0077] In the above chemical formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the range of 1.0≦x≦1.30, 0.1≦y<0.95, and 0.01, respectively. <z≦0.5、0.01<w≦0.5、0≦v≦0.2、1.5≦u≦4.5である。
[0078] The lithium nickel composite oxide represented by the above chemical formula 2 is a composite metal oxide containing lithium, nickel, cobalt and manganese, and in some cases, other transition metals (M 2 For example, the positive electrode active material may be doped with LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.8 Co0.1 Mn 0.05 Al 0.05 O2 and LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 O2. As an example, the positive electrode active material may contain one or more compounds selected from the group consisting of lithium nickel composite metal oxide represented by Chemical Formula 2, LiNi 0.6 Co 0.2 Mn 0.2 O2 and LiNi 0.8 Co 0.1 Mn 0.1 O2 can be used alone or in combination.
[0079] The content of the positive electrode active material may be 85 to 95 parts by weight, specifically 88 to 95 parts by weight, 90 to 95 parts by weight, 86 to 90 parts by weight, or 92 to 95 parts by weight, relative to 100 parts by weight of the mixture layer.
[0080] In this case, the conductive material can be used to improve the performance of the positive electrode, such as the electrical conductivity, and can be one or more selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber. For example, the conductive material may include acetylene black.
[0081] The conductive material may be contained in an amount of 1 to 10 parts by weight, specifically 2 to 8 parts by weight, or 2 to 6 parts by weight, relative to 100 parts by weight of the mixture layer.
[0082] The binder may include one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, and copolymers thereof. As an example, the binder may include polyvinylidene fluoride.
[0083] The binder may be contained in an amount of 1 to 10 parts by weight, specifically 1 to 8 parts by weight, or 1 to 6 parts by weight, relative to 100 parts by weight of the entire mixture layer.
[0084] In addition, the average thickness of the composite layer is not particularly limited, but may be specifically 50 μm to 300 μm, and more specifically 100 μm to 200 μm; 80 μm to 150 μm; 120 μm to 170 μm; 150 μm to 300 μm; 200 μm to 300 μm; or 150 μm to 190 μm.
[0085] In addition, the positive electrode can be a current collector having high conductivity without inducing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. can be used, and in the case of aluminum or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the current collector can be formed with fine irregularities on the surface to increase the adhesive force of the positive electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the positive electrode to be manufactured.
[0086] In addition, the negative electrode of the lithium secondary battery used in the present invention is manufactured by applying, drying, and pressing a negative electrode active material onto a negative electrode current collector, and may selectively further contain the same conductive material, organic binder polymer, additive, etc. as the positive electrode if necessary.
[0087] In addition, the negative electrode active material includes, for example, graphite having a complete layered crystal structure such as natural graphite, soft carbon having a low crystalline layered crystal structure (graphene structure; a structure in which hexagonal honeycomb-shaped planes of carbon are arranged in layers), and hard carbon in which such a structure is mixed with an amorphous part, artificial graphite, expanded graphite, carbon fiber, graphitization-resistant carbon, carbon black, carbon nanotube, fullerene, activated carbon, and other carbon and graphite materials; LixFe2O3 (0≦x≦1), LixWO2 (0≦x≦1), SnxMe1-xMe’yOz (Me: Mn, Fe, Pb, Ge; Me’, Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0<x≦1; 1≦y≦3; 1≦z≦8), and other metal composite oxides; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; titanium oxides; lithium titanium oxides, etc. can be used.
[0088] As an example, the negative electrode active material may contain both graphite and silicon (Si)-containing particles. The graphite may include one or more of natural graphite having a layered crystal structure and artificial graphite having an isotropic structure. The silicon (Si)-containing particles are particles mainly containing silicon (Si) as a metal component, and may include silicon (Si) particles, SiO particles, SiO2 particles, or a mixture of one or more of these particles.
[0089] In this case, the negative electrode active material may contain 80 to 95 parts by weight of graphite and 1 to 20 parts by weight of silicon (Si)-containing particles, based on a total of 100 parts by weight. By adjusting the contents of graphite and silicon (Si)-containing particles contained in the negative electrode active material within the above ranges, the present invention can reduce the lithium consumption and irreversible capacity loss during initial charging and discharging of the battery, and improve the charging capacity per unit mass.
[0090] The negative electrode mixture layer may have an average thickness of 100 μm to 200 μm, specifically, 100 μm to 180 μm, 100 μm to 150 μm, 120 μm to 200 μm, 140 μm to 200 μm, or 140 μm to 160 μm.
[0091] In addition, the negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and for example, copper, stainless steel, nickel, titanium, calcined carbon, etc. can be used. In the case of copper or stainless steel, it is also possible to use a material that has been surface-treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode current collector can be formed with fine irregularities on the surface like the positive electrode current collector to strengthen the binding force with the negative electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the negative electrode current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the negative electrode to be manufactured.
[0092] The separator is a thin insulating membrane interposed between the positive and negative electrodes and having high ion permeability and mechanical strength. The separator is not particularly limited as long as it is one commonly used in the industry, and specifically, a sheet or nonwoven fabric made of chemically resistant and hydrophobic polypropylene, glass fiber, or polyethylene can be used. In some cases, a composite separator made of a porous polymer substrate such as the sheet or nonwoven fabric coated with inorganic particles / organic particles by an organic binder polymer can be used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as the separator. The pore diameter of the separator may be an average of 0.01 to 10 μm, and the thickness may be an average of 5 to 300 μm.
[0093] Meanwhile, the positive and negative electrodes may be wound in a jelly roll form and housed in a cylindrical battery, a prismatic battery, or a pouch-type battery, or may be housed in a pouch-type battery in a folded or stack-and-folded form, but is not limited thereto.
[0094] The lithium salt-containing electrolyte according to the present invention may be composed of an electrolyte and a lithium salt. The electrolyte may be a non-aqueous organic solvent, an organic solid electrolyte, or an inorganic solid electrolyte.
[0095] Specifically, the electrolyte may contain a compound represented by the following Chemical Formula 3:
[0096] [Chemical formula 3] [ka]
[0097] In the above chemical formula 3, R1 is a substituted or unsubstituted C1-4 alkylamine group; a substituted or unsubstituted 4- to 7-substituted heteroalkyl group; or a substituted or unsubstituted 4- to 7-substituted heteroaryl group, and the heteroalkyl and heteroaryl groups contain one or more nitrogen atoms (N); n is an integer from 1 to 4.
[0098] Specifically, in the compound represented by Chemical Formula 3, R1 is a dimethylamine group, a diethylamine group, a diisopropylamine group, a pyrrolidyl group, a piperidyl group, a piperazinyl group, a morpholinyl group, a pyrrolyl group, or an imidazolyl group, and one or more hydrogen atoms present in the pyrrolidyl group, the piperidyl group, the piperazinyl group, the morpholinyl group, the pyrrolyl group, and the imidazolyl group may be unsubstituted or substituted with a C1-4 alkyl group or a nitrile group, and n is 1 or 2.
[0099] As an example, the compound represented by the above formula 3 may be a compound represented by the following formula 4:
[0100] [Chemical formula 4] [ka]
[0101] The compound represented by the above formula 4 contains a triple bond at the end, and can strengthen the SEI film formed on the surface of the negative electrode, and can adsorb and remove impurities such as metal foreign matter present in the electrolyte, thereby suppressing side reactions of the electrolyte. In addition, R1 of the above compound can stabilize the lithium salt using nitrogen atoms contained in an alkylamine group, heteroalkyl group, or heteroaryl group, thereby suppressing the generation of decomposition products such as HF and PF5 in the electrolyte, thereby preventing the deterioration of the battery and the voltage from decreasing due to acidic HF, PF5, etc. Above all, R1 can stabilize the reaction site of the positive electrode additive contained in the positive electrode mixture layer, thereby preventing the electrode resistance of the positive electrode from being reduced by the positive electrode additive, while improving the charge and discharge capacity of the battery.
[0102] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran (franc), 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0103] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymeric materials containing ionic dissociation groups.
[0104] Examples of the inorganic solid electrolyte that can be used include nitrides, halides, and sulfates of Li, such as Li3N, LiI, Li5Ni2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2.
[0105] The lithium salt is a substance that is easily dissolved in a non-aqueous electrolyte, and examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium tetraphenylboronate, imides, etc. can be used.
[0106] In addition, for the purpose of improving charge / discharge characteristics, flame retardancy, etc., the electrolyte may contain, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. In some cases, in order to impart non-flammability, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further contained, and in order to improve high-temperature storage characteristics, carbon dioxide gas may be further contained, and fluoroethylene carbonate (FEC), propene sultone (PRS), etc. may be further contained.
[0107] In addition, the positive and negative electrodes may be wound in a jelly roll shape and housed in a cylindrical battery, a prismatic battery, or a pouch-type battery, or may be folded or stacked and folded and housed in a pouch-type battery. For example, the lithium secondary battery according to the present invention may be a pouch-type battery.
[0108] The present invention will now be described in more detail with reference to examples and experimental examples.
[0109] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.
[0110] <Production example: Manufacturing of lithium secondary batteries> LiNi as the positive electrode active material 0.8 Co 0.1 Mn 0.1 95 parts by weight of O2, Li6Co as a positive electrode additive 0.7 Zinc 0.3A positive electrode composite layer slurry was prepared by mixing 0.9 parts by weight of O4, 1.6 parts by weight of PVDF as a binder, and 2.5 parts by weight of carbon black as a conductive material in an N-methylpyrrolidone (NMP) solvent. The composite layer slurry was applied to an aluminum foil, dried, and then rolled to form a positive electrode having a positive electrode composite layer (average thickness: 130 μm).
[0111] A negative electrode composite layer slurry was prepared by mixing 85 parts by weight of natural graphite as a carbon-based active material, 5 parts by weight of SiO (silicon oxide) as a silicon-based active material, 6 parts by weight of carbon black as a conductive material, and 4 parts by weight of PVDF as a binder in an N-methylpyrrolidone solvent. The slurry was then applied to a copper foil to prepare a negative electrode having a negative electrode composite layer (average thickness: 180 μm).
[0112] The prepared positive and negative electrodes were laminated with a separator (thickness: about 16 μm) made of a porous polyethylene (PE) film between them to prepare an electrode assembly. The electrode assembly was placed inside a battery case, and an electrolyte was injected into the case. The case was then left at room temperature for 3 days to allow the electrolyte to be sufficiently impregnated, thereby preparing a lithium secondary battery. E2DVC containing the compound represented by the following Chemical Formula 4 as an electrolyte additive was injected to prepare a full cell type cell. The compound represented by the Chemical Formula 4 was weighed to be contained at 1 wt % based on the electrolyte.
[0113] Here, "E2DVC" refers to a type of carbonate-based electrolyte, a solution in which lithium hexafluorophosphate (LiPF6, 1.0M) and vinylene carbonate (VC, 2% by weight) are mixed with a mixture of ethylene carbonate (EC): dimethyl carbonate (DMC): diethyl carbonate (DEC) = 1:1:1 (volume ratio).
[0114] [Chemical formula 4] [ka]
[0115] <Examples 1 to 6. Activation of lithium secondary batteries> The activation step was carried out on the lithium secondary battery manufactured in the manufacturing example. At this time, the temperature for carrying out each activation step was 55°C. Meanwhile, the activation step 1 was carried out under the conditions of 0.2C and 3.4V, and the activation steps 2 to 4 were carried out under the conditions of 1C and 3.6V. The time for each activation step, the presence or absence of a degassing step, and the presence or absence of a pressurizing step in the activation step are shown in Table 1. Meanwhile, the activation step was carried out in a state where the lithium secondary battery was pressurized with a pressurizing tool, so that the gas inside the lithium secondary battery was collected in the gas pocket. Then, in the degassing step, the gas pocket was pierced to form a hole, and a negative pressure of -5 to -90 kPa was applied to remove the gas collected in the gas pocket. The lithium secondary battery that had undergone the activation step was aged for 24 hours at a temperature of 60°C, and the lithium secondary battery that had undergone the aging step had the gas inside the battery degassed.
[0116] <Comparative Example 1. Activation of Lithium Secondary Battery> The lithium secondary battery manufactured in the manufacturing example was activated by charging at 0.3 C for 10 hours until the voltage reached 4.3 V. After the activation step, gas in the battery was removed using a jig.
[0117] [Table 1]
[0118] <Experimental Example> In order to evaluate the performance difference of the lithium secondary battery depending on the activation method, the following experiment was carried out.
[0119] A) Analysis of the gas content generated during the activation stage The amount of gas generated during the formation of the lithium secondary batteries according to the examples and comparative examples and the total amount of gas generated therein were analyzed, and the results are shown in Table 2 below.
[0120] [Table 2]
[0121] As shown in Table 2 above, the lithium secondary batteries activated under the conditions of the examples had a larger total gas generation amount than the lithium secondary batteries activated under the comparative examples. Also, Example 1, in which the degassing process was performed after each activation stage, had a larger total gas generation amount than Examples 2 to 6. Moreover, looking at Examples 2, 4, and 5, in which the degassing process was performed a total of three times in the activation stage, the lithium secondary batteries of Examples 2 and 4, in which the degassing process was performed after the first activation stage, had a larger total gas generation amount than the lithium secondary battery of Example 5. Generally, since SEI formation is most active in the first activation stage, it is considered that the lithium secondary batteries of Examples 2 and 4, in which the degassing process was performed after the first activation stage, have a larger total gas generation amount than the lithium secondary battery of Example 5.
[0122] The lithium secondary battery activated under the conditions of the embodiment can easily remove gas generated in the lithium secondary battery by performing a degassing process during the activation step. In particular, this process is believed to improve the performance of the lithium secondary battery by preventing the gas generated in the secondary battery from interfering with the formation of SEI or participating in a side reaction.
[0123] b) Evaluation of initial resistance value The lithium secondary batteries activated in the examples and comparative examples were each discharged at a C-rate of 2C at SOC 50% for 10 seconds, and the resistance was measured. The results are shown in Table 3.
[0124] [Table 3]
[0125] As shown in Table 3 above, it was confirmed that the lithium secondary batteries activated according to the Examples had lower resistance values than the Comparative Examples. In particular, the lithium secondary batteries of Examples 1 to 4, which were subjected to a degassing process after the first activation step, had lower resistance values than those of Examples 5 and 6. This is believed to be because the by-reaction gases inside the lithium secondary batteries were removed, increasing the impregnation of the electrolyte, thereby causing a uniform electrode-electrolyte reaction.
[0126] C) Evaluation of cycle life performance The lithium secondary batteries activated in the examples and comparative examples were each discharged at a discharge current of 0.1 C to a cut-off voltage of 2 V, and the initial charge / discharge capacity per unit mass was measured.
[0127] Next, the capacity during charging and discharging was measured by repeatedly charging and discharging 100 times at 45°C and 0.3 C, and the charge / discharge capacity retention rate after 100 charge / discharge cycles was calculated. The results are shown in Table 4 below.
[0128] [Table 4]
[0129] Referring to Table 4 above, it was confirmed that the lithium secondary battery activated according to the embodiment has an initial charge / discharge capacity of 100 mAh or more and a capacity retention rate after 100 charge / discharge cycles of 90% or more, while the lithium secondary battery activated according to the comparative example has a lower initial charge / discharge capacity and a lower capacity retention rate after 100 charge / discharge cycles compared to the embodiment.
[0130] In the case of the lithium secondary battery activated according to the embodiment, the SEI film formed stably was well maintained without being decomposed by further electrolyte decomposition reaction, etc., by removing the side reaction gas due to the increase in SOC during activation. On the other hand, in the case of the comparative example, since the degassing process was not performed during the activation process, it is believed that the gas generated in the lithium secondary battery during the activation process interfered with the formation of the SEI film or participated in the side reaction. As a result, it is predicted that the lithium secondary battery of the comparative example had a small reaction for forming the SEI film, and therefore the electrolyte decomposition reaction intensified during cycling, causing cycle degradation.
[0131] From these results, the activation method of the lithium secondary battery according to the present invention has an advantage that the total amount of gas generated during charging and discharging can be reduced by performing a degassing process for removing gas from the inside of the secondary battery at least once during the activation step, thereby improving the safety of the battery, and also improving the charge / discharge capacity and capacity retention rate after repeated use of the lithium secondary battery.
[0132] Although the present invention has been described above with reference to preferred embodiments thereof, it will be understood that a person skilled in the art or having ordinary knowledge in the art can make various modifications and variations to the present invention without departing from the spirit and technical scope of the present invention as described in the claims below.
[0133] Therefore, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.
Claims
1. A method for activating a lithium secondary battery containing an electrode assembly having a positive electrode containing a positive electrode active material and a positive electrode additive, and an electrolyte, comprising: An activation step of charging the lithium secondary battery to an SOC of 90% or more, In the activation step, a degassing process is performed at least once to remove gas from the secondary battery during charging to an SOC of 90% or more; The positive electrode additive is a lithium cobalt oxide represented by the following formula 1: The activation step comprises: An activation stage in which the lithium secondary battery is charged to an SOC of 20% or less; a second activation step in which the lithium secondary battery that has undergone the first activation step is charged to an SOC range of more than 20% and less than 40%; a third activation stage in which the lithium secondary battery that has undergone the second activation stage is charged to a SOC range of more than 40% and not more than 70%; and a fourth activation stage in which the lithium secondary battery that has been subjected to the third activation stage is charged to an SOC of 90% or more. The method for activating a lithium secondary battery comprises performing a degassing step after at least one of the first to third activation steps. [Chemical formula 1] Li p Co (1-q) M 1 q O 4 In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
2. 2. The method for activating a lithium secondary battery according to claim 1, wherein the degassing step is performed two or three times.
3. 2. The method for activating a lithium secondary battery according to claim 1, further comprising the step of carrying out a degassing step after each of the first to third activation steps.
4. The first activation stage involves low-rate charging at 0.5C or less.
2. The method for activating a lithium secondary battery according to claim 1, wherein the second to fourth activation stages are performed at a high rate of charging at a rate exceeding 0.5 C.
5. 2. The method of claim 1, wherein the activation step further comprises a step of pressurizing the lithium secondary battery.
6. 2. The method for activating a lithium secondary battery according to claim 1, wherein the activation step is carried out under a temperature condition of 40° C. to 70° C.
7. In the above Chemical Formula 1, M 1 2. The method for activating a lithium secondary battery according to claim 1, wherein q is Zn and q satisfies 0.2≦q≦0.
4.
8. 2. The method of claim 1, wherein the content of the positive electrode additive is 0.1 to 5 wt % based on the total weight of the positive electrode mixture layer.
9. 2. The method for activating a lithium secondary battery according to claim 1, further comprising an aging step of aging the activated lithium secondary battery at a temperature of 40°C to 80°C after the activation step.
10. A lithium secondary battery used in the activation method of the lithium secondary battery according to claim 1, A positive electrode and A negative electrode; an electrode assembly including a separator disposed between a positive electrode and a negative electrode; an electrolyte; The positive electrode comprises a positive electrode current collector, and a positive electrode mixture layer located on the positive electrode current collector and including a positive electrode active material, a positive electrode additive represented by the following Chemical Formula 1, a conductive material, and a binder, The positive electrode active material is a lithium nickel composite oxide represented by the following chemical formula 2: [Chemical formula 1] Li p Co (1-q) M 1 q O 4 [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u In the above Chemical Formulas 1 and 2, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively; M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the ranges of 1.0≦x≦1.30, 0.1≦y<0.95, 0.01<z≦0.5, 0.01<w≦0.5, 0≦v≦0.2, and 1.5≦u≦4.5, respectively.
11. The negative electrode includes a negative electrode current collector and a negative electrode mixture layer located on the negative electrode current collector and containing a negative electrode active material, The lithium secondary battery according to claim 10 , wherein the negative electrode active material contains a carbon material and a silicon material.
Citation Information
Patent Citations
Lithium secondary battery
JP1994342673A
Method of manufacturing lithium secondary battery
JP2010282874A
Method for manufacturing nonaqueous electrolyte secondary battery
JP2015005350A
Power storage device
JP2015088268A
Method for manufacturing nonaqueous electrolyte secondary battery
JP2018190504A