Positive electrode and lithium secondary battery including the same
A dual-layer positive electrode with bimodal active materials addresses thermal instability and particle cracking in lithium secondary batteries, improving capacity, efficiency, and lifespan.
Patent Information
- Application Number
- JP2022571316
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-29
- Filing Date
- 2022-01-28
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2042-01-28
AI Technical Summary
Lithium cobalt oxide-based positive electrodes in lithium secondary batteries suffer from poor thermal stability, high cost, and limited scalability, while high-capacity nickel-based alternatives face issues with oxidation stability and particle cracking during charging and discharging, leading to reduced cycle life and safety concerns.
A positive electrode design featuring two layers of bimodal active material layers, with one layer comprising secondary particles and the other single particles, optimized for particle size, composition, and thickness ratios, enhancing thermal stability and conductivity.
The dual-layer structure improves capacity, efficiency, lifespan, and thermal stability of lithium secondary batteries, ensuring better particle packing and reduced cracking, thereby enhancing overall battery performance.
Smart Images

Figure 0007596009000005 
Figure 0007596009000006 
Figure 0007596009000001
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0012872 filed on January 29, 2021, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a positive electrode including multiple positive electrode active material layers and a lithium secondary battery including the same. [Background technology]
[0003] With the technological development and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.
[0004] Lithium transition metal composite oxides are used as the positive electrode active material for lithium secondary batteries, and among them, lithium cobalt composite metal oxides such as LiCoO2, which have high working voltage and excellent capacity characteristics, are mainly used. However, LiCoO2 has very poor thermal properties due to the instability of its crystal structure caused by delithiation. In addition, because it is expensive, there are limitations to its mass use as a power source in fields such as electric vehicles.
[0005] Materials that have been developed to replace LiCoO2 include lithium manganese composite metal oxides (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compounds (LiFePO4, etc.), and lithium nickel composite metal oxides (LiNiO2, etc.). Among these, research and development has been active on lithium nickel composite metal oxides, which have a high reversible capacity of about 200mAh / g and therefore make it easy to realize large-capacity batteries. However, LiNiO2 has inferior thermal stability compared to LiCoO2, and if an internal short circuit occurs due to external pressure while charging, the positive electrode active material itself decomposes, causing the battery to explode and catch fire.
[0006] Therefore, as a method for maintaining the excellent reversible capacity of LiNiO2 while improving its low thermal stability, nickel-cobalt-manganese-based lithium composite transition metal oxides in which part of Ni is replaced with Co and Mn, nickel-cobalt-aluminum-based lithium composite transition metal oxides in which part of Ni is replaced with Co and Al, and nickel-cobalt-manganese-aluminum-based composite transition metal oxides in which part of Ni is replaced with Co, Mn, and Al have been developed.
[0007] Meanwhile, when using high-capacity lithium transition metal oxides, the oxidation stability at high voltage decreases, resulting in poor stability, or many cracks occur between particles during long-term charge / discharge, resulting in the interruption of the conductive path, which causes an increase in cycle resistance.
[0008] Therefore, there is a demand for the development of a positive electrode for a lithium secondary battery having improved capacity, efficiency, life, output characteristics, and thermal stability. Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made to solve the above problems, and has an object to provide a positive electrode for a lithium secondary battery that can improve all of the capacity, efficiency, life, output characteristics, and thermal stability. [Means for solving the problem]
[0010] The present invention provides a positive electrode for a lithium secondary battery, comprising a positive electrode current collector, and a first positive electrode active material layer and a second positive electrode active material layer stacked in that order on the positive electrode current collector, wherein the first positive electrode active material layer and the second positive electrode active material layer comprise a bimodal positive electrode active material, the first positive electrode active material layer comprises small particle diameter particles in a monoparticle form, and the second positive electrode active material layer comprises small particle diameter particles in a secondary particle form.
[0011] The present invention also provides a lithium secondary battery comprising the positive electrode. Effect of the Invention
[0012] The positive electrode for a lithium secondary battery according to the present invention includes two positive electrode active material layers that satisfy specific conditions, and thus can improve the capacity, efficiency, life, output characteristics, and thermal stability. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a graph showing the capacity retention characteristics of half cells produced using the positive electrode active materials produced in the examples and comparative examples. [Diagram 2] FIG. 1 is a graph showing the resistance increase rate characteristics of half cells produced using the positive electrode active materials produced in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0015] In this specification, the terms "including," "comprising," or "having" are intended to indicate the presence of implemented features, numerals, steps, components, or combinations thereof, and should be understood as not precluding the presence or additional possibility of one or more other features, numerals, steps, components, or combinations thereof.
[0016] In this specification, the term "average particle size (D 50 The average particle size (D) can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. 50For example, the average particle diameter (D 50 The method for measuring the average particle size (D) is as follows: After dispersing the particles of the positive electrode active material in a dispersion medium, the particles are introduced into a commercially available laser diffraction particle size measuring device (e.g., HORIBA LA-960), and ultrasonic waves of about 28 kHz are irradiated at an output of 60 W. Then, the average particle size (D) corresponding to 50% of the cumulative volume in the measuring device is measured. 50 ) can be calculated.
[0017] In this specification, the term "single-particle positive electrode active material" refers to a positive electrode active material consisting of 10 or less primary particles, as opposed to a spherical secondary particle positive electrode active material produced by a conventional method, which is formed by agglomerating tens to hundreds of primary particles. Specifically, in the present invention, the single-particle positive electrode active material may be a single particle consisting of one primary particle, or may be a secondary particle formed by agglomerating several primary particles.
[0018] In this specification, the term "primary particle" refers to the smallest particle unit that can be recognized when observing a positive electrode active material with a scanning electron microscope, and the term "secondary particle" refers to a secondary structure formed by aggregation of a plurality of primary particles.
[0019] In this specification, "particle" refers to a particle of a micrometer unit, which, when observed under magnification, can be divided into "grains" having a crystalline shape of several tens of nanometers. When observed under further magnification, it is possible to confirm separate regions in which atoms form a lattice structure in a certain direction, which are called "crystal grains." The size of particles observed by XRD is defined as the crystal grain size. The crystal grain size can be quantitatively determined using the Scherrer equation from XRD data.
[0020] In this specification, overfiring means that the positive electrode active material is fired at a temperature that is 50° C. to 200° C. higher than the conventional appropriate firing temperature when the positive electrode active material is produced. For example, when a lithium composite transition metal oxide having a molar ratio of Ni:Co:Mn of 80:10:10 is produced as the positive electrode active material, the conventional appropriate firing temperature is known to be 750° C. to 900° C., but overfiring means that the positive electrode active material is fired at a temperature that is 50° C. to 100° C. higher than the appropriate firing temperature.
[0021] The present invention will now be described in more detail.
[0022] positive electrode The present inventors have found that the positive electrode includes two positive electrode active material layers, and the first positive electrode active material layer formed on the positive electrode current collector has an average particle diameter (D 50 The second positive electrode active material layer formed on the first positive electrode active material layer includes a positive electrode active material in a secondary particle form and a positive electrode active material in a single particle form, the average particle diameters (D 50 The present inventors have found that when the positive electrode active material contains two types of positive electrode active materials having different secondary particle shapes, a lithium secondary battery excellent in capacity, efficiency, life, output characteristics and thermal stability can be realized, and have completed the present invention.
[0023] The positive electrode of the present invention relates to a positive electrode for a lithium secondary battery, comprising a positive electrode current collector, and a first positive electrode active material layer and a second positive electrode active material layer laminated in order on the positive electrode current collector. The first positive electrode active material layer and the second positive electrode active material layer may comprise a bimodal positive electrode active material. That is, the first positive electrode active material layer may comprise large particle diameter particles (first positive electrode active material) and small particle diameter particles (second positive electrode active material), and the second positive electrode active material layer may comprise large particle diameter particles (third positive electrode active material) and small particle diameter particles (fourth positive electrode active material).
[0024] The first positive electrode active material layer can include a first positive electrode active material (large particle diameter) in the form of secondary particles formed by aggregation of a plurality of primary particles, and a second positive electrode active material (small particle diameter) in the form of a single particle.
[0025] The second positive electrode active material layer may include a third positive electrode active material (large particle diameter particles) in the form of secondary particles formed by agglomeration of a plurality of primary particles, and a fourth positive electrode active material (small particle diameter particles) in the form of secondary particles formed by agglomeration of a plurality of primary particles.
[0026] That is, in the present invention, the first positive electrode active material has a smaller average particle size (D 50 ) is larger than that of the fourth positive electrode active material, and the third positive electrode active material has a larger average particle size (D 50 The first positive electrode active material may be the same as the third positive electrode active material.
[0027] When the first positive electrode active material layer is present on the positive electrode current collector and the second positive electrode active material layer is present on the first positive electrode active material layer, the presence of a buffer layer reduces the heat transfer rate and improves thermal stability compared to when only the first or second positive electrode active material layer is present on the positive electrode current collector, and the resistance and output of a battery including a positive electrode can be improved by appropriately adjusting the thickness ratio of the first positive electrode active material layer to the second positive electrode active material layer and the ratio of the active material, conductive material, and binder contained in each layer. On the other hand, when the second positive electrode active material layer is present on the positive electrode current collector and the first positive electrode active material layer is present on the second positive electrode active material layer, the probability of the positive electrode active material particles on the surface of the electrode cracking during rolling increases, resulting in disadvantageous problems in terms of life and resistance.
[0028] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can usually have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0029] According to the present invention, the thickness ratio of the first positive electrode active material layer to the second positive electrode active material layer may be 3:7 to 7:3, specifically 5:5 to 6:4. When the thickness ratio of the first positive electrode active material layer to the second positive electrode active material layer is within the above range, there are advantages in that cracking of the particles of the positive electrode active material on the positive electrode surface is prevented and resistance and thermal stability are improved.
[0030] According to the present invention, the first positive electrode active material, the second positive electrode active material, the third positive electrode active material, and the fourth positive electrode active material may each independently have a composition represented by Chemical Formula 1 below.
[0031] [Chemical formula 1] Li x [Ni a Co b M 1 c M 2 d ]O2
[0032] In the above Chemical Formula 1, Said M 1 is one or more selected from Mn and Al, Said M 2 is one or more selected from B, Mg, Ca, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta and W, 0.9≦x≦1.1, 0.7≦a<1, 0 <b<0.3、0<c<0.3、0≦d≦0.1、a+b+c+d=1である。
[0033] The a means the atomic fraction of nickel among metal elements other than lithium in the active material, and may be 0.7≦a<1, 0.8≦a<1, or 0.85≦a≦0.95.
[0034] The b represents the atomic fraction of cobalt among the metal elements other than lithium in the active material, and is 0 <b<0.3、0<b<0.2、0.01≦b<0.2または0.02≦b≦0.1であることができる。
[0035] The c is M among the metal elements other than lithium in the active material. 1means the atomic fraction of an element, 0 <c<0.3、0<c<0.2、0.01≦c<0.2または0.02≦c≦0.1であることができる。
[0036] The d is the number of metal elements other than lithium in the active material, M 2 It means the atomic fraction of an element and can be 0≦d≦0.1 or 0≦d≦0.05.
[0037] According to the present invention, the first positive electrode active material has an average particle size (D 50 The second positive electrode active material may have an average particle size (D 50 The average particle diameter (D) of the first positive electrode active material and the second positive electrode active material may be 3 μm to 10 μm, specifically 4 μm to 10 μm, and more specifically 4 μm to 8 μm. 50 ) simultaneously satisfy the above-mentioned numerical ranges, not only is the energy density of the positive electrode high, but there is also the advantage that packing between the positive electrode active materials is easy during rolling.
[0038] According to the present invention, the third positive electrode active material has an average particle size (D 50 ) may be 5 μm to 20 μm, specifically 8 μm to 18 μm, and more specifically 10 μm to 16 μm, and the fourth positive electrode active material may have an average particle size (D 50 The average particle diameter (D ) of the third positive electrode active material and the fourth positive electrode active material may be 3 μm to 10 μm, specifically 4 μm to 10 μm, and more specifically 4 μm to 8 μm. 50 ) simultaneously satisfy the above-mentioned numerical ranges, not only is the energy density of the positive electrode high, but there is also the advantage that packing between the positive electrode active materials is easy during rolling.
[0039] The first positive electrode active material may have a crystal grain size of 100 nm to 150 nm, the second positive electrode active material may have a crystal grain size of 200 nm to 250 nm, the third positive electrode active material may have a crystal grain size of 100 nm to 150 nm, and the fourth positive electrode active material may have a crystal grain size of 70 nm to 100 nm.
[0040] When the crystal grain size of the first and third positive electrode active materials is within the above range, cracks present in the positive electrode active material particles can be few, and when the crystal grain size of the second positive electrode active material is within the above range, not only are cracks present in the positive electrode active material particles few, but the BET specific surface area is small, and side reactions hardly occur.
[0041] The BET specific surface area of the first positive electrode active material is 0.3 m 2 / g~0.7m 2 / g, and the BET specific surface area of the second positive electrode active material may be 0.2 m 2 / g~0.4m 2 The third positive electrode active material may have a BET specific surface area of 0.3 m 2 / g~0.7m 2 / g, and the BET specific surface area of the fourth positive electrode active material may be 0.7 m 2 / g~1.2m 2 / g.
[0042] The BET specific surface area can be measured by the amount of nitrogen gas adsorption at liquid nitrogen temperature (77 K) using a BELSORP-mini II (manufactured by Mictrotrac-BEL). When the BET specific surface area of each positive electrode active material is within the above range, a side reaction between the positive electrode active material and the electrolyte can be prevented.
[0043] According to the present invention, the first positive electrode active material layer may contain the first positive electrode active material and the second positive electrode active material in a weight ratio of 85:15 to 55:45, specifically 85:15 to 60:40, and more specifically 80:20 to 70:30, which may provide advantageous capacity characteristics and rolling density characteristics of the battery.
[0044] The sum of the content of the first positive electrode active material and the content of the second positive electrode active material may be 80 wt% to 99 wt%, more specifically 85 wt% to 98 wt%, based on the total weight of the first positive electrode active material layer. When the content is within the above range, excellent capacity characteristics can be exhibited.
[0045] According to the present invention, the second positive electrode active material layer may contain the third positive electrode active material and the fourth positive electrode active material in a weight ratio of 85:15 to 55:45, specifically 85:15 to 60:40, and more specifically 80:20 to 70:30, which may provide advantageous capacity characteristics and rolling density characteristics of the battery.
[0046] The sum of the content of the third positive electrode active material and the content of the fourth positive electrode active material may be 80 wt% to 99 wt%, more specifically 85 wt% to 98 wt%, based on the total weight of the second positive electrode active material layer. When the content is within the above range, excellent capacity characteristics can be exhibited.
[0047] The first positive electrode active material layer and the second positive electrode active material layer may each independently contain a positive electrode active material, a conductive material, and a binder.
[0048] The conductive material is used to give conductivity to the electrode, and according to the present invention, the first positive electrode active material layer may further include a dot-like conductive material, and the second positive electrode active material layer may further include a dot-like conductive material and a linear conductive material. Specific examples of the dot-like conductive material include furnace black, acetylene black, and lamp black, and examples of the linear conductive material include low-BET CNT (low BET specific surface area carbon nanotube), SWCNT (single-walled carbon nanotube), etc. When the second positive electrode active material layer further includes a dot-like conductive material and a linear conductive material, the conductive network between the positive electrode active material particles is improved, improving electronic conductivity and facilitating the movement of lithium ions, thereby improving output and life.
[0049] The conductive material may be contained in an amount of 1 wt % to 30 wt % relative to the total weight of each of the first and second positive electrode active material layers.
[0050] The binder serves to improve the adhesion between particles of the positive electrode active material and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 wt% to 30 wt% of the total weight of each of the first and second positive electrode active material layers.
[0051] The positive electrode may be manufactured by a conventional positive electrode manufacturing method. Specifically, the positive electrode may be manufactured by applying a composition for forming a positive electrode active material layer, which is prepared by dissolving or dispersing a positive electrode active material, and optionally a binder and a conductive material, in a solvent, onto a positive electrode current collector, followed by drying and rolling. In this case, the types and contents of the positive electrode active material, binder, and conductive material are as described above.
[0052] The solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to have a viscosity that can dissolve or disperse the positive electrode active material, conductive material, and binder and provide excellent thickness uniformity during subsequent coating for the manufacture of a positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.
[0053] As another method, the positive electrode can also be produced by casting the composition for forming a positive electrode active material layer on another support, peeling the composition from the support, and laminating the resulting film on a positive electrode current collector.
[0054] Lithium secondary battery The present invention also provides a lithium secondary battery including the positive electrode.
[0055] Specifically, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. Since the positive electrode is as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.
[0056] Also, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0057] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0058] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of typically 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0059] The negative electrode active material layer includes a negative electrode active material, and optionally a binder and a conductive material.
[0060] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β (0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites and Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, the carbon material may be either low crystalline carbon or high crystalline carbon. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.
[0061] The negative electrode active material may be included in an amount of 80% by weight to 99% by weight based on the total weight of the negative electrode active material layer.
[0062] The binder is a component that facilitates bonding between the conductive material, the active material, and the current collector, and may be added in an amount of 0.1% by weight to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0063] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of such conductive materials include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0064] The negative electrode active material layer can be produced by applying a negative electrode mixture, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent, onto a negative electrode current collector and drying the applied mixture. Alternatively, the negative electrode mixture can be cast onto a separate support, and then peeled off from the support to obtain a film, which can be laminated onto the negative electrode current collector.
[0065] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent humidification ability of the electrolyte solution is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, etc., can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used as a single layer or a multilayer structure.
[0066] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.
[0067] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0068] The organic solvent may be any solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of the battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, so that the electrolyte can exhibit excellent performance.
[0069] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO2, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as the lithium salt. The concentration of the lithium salt is preferably within the range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0070] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, in order to improve the life characteristics of the battery, suppress the decrease in the capacity of the battery, and improve the discharge capacity of the battery. In this case, the additives may be contained in an amount of 0.1% by weight to 5% by weight based on the total weight of the electrolyte.
[0071] As described above, the lithium secondary battery including the positive electrode active material according to the present invention exhibits excellent capacity, efficiency, life and output characteristics, and is therefore useful in portable devices such as mobile phones, notebook computers and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0072] Therefore, according to the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same can be provided.
[0073] The battery module or battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0074] The shape of the lithium secondary battery is not particularly limited, but may be a cylindrical type using a can, a square type, a pouch type, a coin type, or the like.
[0075] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but also preferably as a unit battery in a medium- to large-sized battery module including a large number of battery cells.
[0076] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.
[0077] Examples and Comparative Examples The particle shape, composition, and average particle size (D 50 ), crystal grain size and BET specific surface area are shown in Table 1 below.
[0078] [Table 1]
[0079] Example 1 The positive electrode active material A and the positive electrode active material B shown in the table were mixed in a weight ratio of 8:2, and then the mixed positive electrode active material A and positive electrode active material B were mixed with carbon black and a PVDF binder in a weight ratio of 97.5:1.0:1.5 in NMP solvent to prepare a first positive electrode slurry. The first positive electrode slurry was applied to one side of an aluminum current collector (thickness: 12 μm) and dried at 130° C. to form a first positive electrode active material layer on the aluminum current collector.
[0080] Cathode active material C and cathode active material D shown in the table were mixed in a weight ratio of 8:2, and then the mixed cathode active material C and cathode active material D were mixed with a conductive material made of carbon black and SWCNT mixed in a weight ratio of 90:10 and a PVDF binder in a weight ratio of 97.5:1.0:1.5 in NMP solvent to prepare a second cathode slurry. The second cathode slurry was applied onto the first cathode active material layer, dried at 130°C, and rolled to prepare a cathode.
[0081] In this case, the thickness ratio of the first positive electrode active material layer to the second positive electrode active material layer was 5:5.
[0082] Example 2 A positive electrode was manufactured in the same manner as in Example 1, except that the application amounts of the first positive electrode slurry and the second positive electrode slurry were adjusted so that the thickness ratio of the first positive electrode active material layer to the second positive electrode active material layer was 6:4.
[0083] Example 3 A positive electrode was produced in the same manner as in Example 1, except that the positive electrode active material A and the positive electrode active material B were mixed in a weight ratio of 7:3, and the application amounts of the first positive electrode slurry and the second positive electrode slurry were adjusted so that the thickness ratio of the first positive electrode active material layer to the second positive electrode active material layer was 6:4.
[0084] Comparative Example 1 Cathode active material C and cathode active material D shown in the table were mixed in a weight ratio of 8:2, and then the mixed cathode active material C and cathode active material D were mixed with a conductive material made of carbon black and SWCNT mixed in a weight ratio of 90:10 and a PVDF binder in a weight ratio of 97.5:1.0:1.5 in NMP solvent to prepare a cathode slurry. The cathode slurry was applied to one side of an aluminum current collector (thickness: 12 μm), dried at 130° C., and rolled to prepare a cathode.
[0085] Comparative Example 2 The positive electrode active material A and the positive electrode active material B shown in the table were mixed in a weight ratio of 8:2, and then the mixed positive electrode active material A and positive electrode active material B were mixed with carbon black and a PVDF binder in a weight ratio of 97.5:1.0:1.5 in NMP solvent to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector (thickness: 12 μm), dried at 130° C., and rolled to prepare a positive electrode.
[0086] Comparative Example 3 A positive electrode was manufactured in the same manner as in Example 1, except that the second positive electrode slurry was applied onto an aluminum current collector to form a second positive electrode active material layer, and the first positive electrode slurry was applied onto the second positive electrode active material layer to form a first positive electrode active material layer.
[0087] Experimental Example Experimental example 1: Evaluation of half-cell characteristics Half-cells were produced using the positive electrodes produced in Examples 1 to 3 and Comparative Examples 1 to 3, and the initial charge / discharge capacity, initial efficiency, life characteristics, resistance characteristics, and output characteristics of each half-cell were evaluated.
[0088] First, an electrode assembly was prepared by interposing a separator between each of the positive electrodes and Li metal disk negative electrodes prepared in Examples 1 to 3 and Comparative Examples 1 to 3, and then the electrode assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a lithium secondary battery. In this case, an electrolyte solution prepared by dissolving 1M LiPF6 in an organic solvent of EC / EMC (5 / 5, vol%) was injected to prepare a half cell.
[0089] The half cell prepared as above was charged at 25° C. at a constant current of 0.2 C until the voltage reached 4.25 V, and then discharged at a constant current of 0.2 C until the voltage reached 2.5 V. The initial charge capacity and initial discharge capacity are shown in Table 2 below, and the ratio of the initial discharge capacity to the initial charge capacity was defined as the initial efficiency (@0.2 C), which is also shown in Table 2 below. The initial efficiency (@1.0 C) and initial efficiency (@2.0 C) were determined in the same manner as above, except that the C rate was adjusted to 1.0 C and 2.0 C during charging and discharging, and are also shown in Table 2 below.
[0090] [Table 2]
[0091] The capacity of the half-cell was measured while repeating 30 charge-discharge cycles at a constant current of 0.3 C in the range of 2.5 to 4.25 V at 45° C., and in particular, the ratio of the Nth cycle capacity to the 1st cycle capacity was defined as the capacity retention (Capacity Retention, %), which is shown in Figure 1. The ratio of DCIR determined in the Nth discharge cycle to DCIR determined in the 1st discharge cycle was defined as the resistance increase rate (ΔDCIR, %), which is shown in Figure 2.
[0092] Finally, the half-cells prepared as described above were discharged by ΔSOC 30 (SOC 35% to SOC 20%) at -10°C (low temperature) and 25°C (normal temperature), respectively, and the change in voltage value was confirmed by a 0.4C IR drop for 1,350 seconds, and the results are shown in Table 3 below.
[0093] [Table 3]
[0094] 1 and 2, it can be seen that the batteries including the positive electrodes of Examples 1 to 3 are superior in capacity, efficiency, capacity retention rate, and low-temperature and room-temperature output characteristics to the batteries including the positive electrodes of Comparative Examples 1 to 3. In the case of the batteries including the positive electrodes of Comparative Examples 1 and 2, the positive electrode active material layer has a single-layer structure and there are few paths for lithium ions to move, so there is a problem that the capacity, efficiency, capacity retention rate, and low-temperature and room-temperature output characteristics are not as good as those of Examples 1 and 2.
[0095] In the case of a battery including the positive electrode of Comparative Example 3, there is a problem in that the cracks in the positive electrode active material particles present on the surface of the positive electrode become severe, resulting in an increase in the resistance of the battery.
[0096] Experimental Example 2: Evaluation of thermal stability (DSC, differential scanning calorimetry) Half-cells were produced using the positive electrodes produced in Examples 1 to 3 and Comparative Examples 1 to 3, and the thermal stability of each of the half-cells was evaluated.
[0097] First, an electrode assembly was prepared by interposing a separator between each of the positive electrodes and Li metal disk negative electrodes prepared in Examples 1 to 3 and Comparative Examples 1 to 3, and then the electrode assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a lithium secondary battery. In this case, an electrolyte solution prepared by dissolving 1M LiPF6 in an organic solvent of EC / DMC / EMC (3 / 4 / 3, vol%) was injected to prepare a half cell.
[0098] The half-cells prepared as described above were charged at a constant current of 0.1C and disassembled at 100% SOC. The positive electrodes and fresh electrolyte obtained from each half-cell were placed in a DSC measurement cell, and the temperature was increased from room temperature to 500°C at 10°C / min using a differential scanning calorimeter (Setaram, HP (High Pressure)-DSC). The temperature at which the heat flow peaked was the maximum was shown in Table 4 below.
[0099] [Table 4]
[0100] Referring to Table 4, it can be seen that the batteries including the positive electrodes of Examples 1 to 3 have less heat transfer due to the buffer layer effect of the double layer, and therefore have better thermal stability than the batteries including the positive electrodes of Comparative Examples 1 and 2. It can also be seen that the batteries including the positive electrodes of Examples 1 to 3 have better cracking of the positive electrode active material particles present on the surface of the positive electrode (the positive electrode active material particles are hardly cracked) than the battery including the positive electrode of Comparative Example 3, and therefore have better thermal stability.
Claims
1. A positive electrode for a lithium secondary battery comprising: a positive electrode current collector; and a first positive electrode active material layer and a second positive electrode active material layer laminated in this order on the positive electrode current collector, the first positive electrode active material layer and the second positive electrode active material layer contain a bimodal positive electrode active material, the first positive electrode active material layer includes small particles in the form of single particles and large particles in the form of secondary particles, the second positive electrode active material layer includes small particles in the form of secondary particles and large particles in the form of secondary particles, a thickness ratio of the first positive electrode active material layer to the second positive electrode active material layer is 3:7 to 7:3; the large particles contained in the first positive electrode active material layer have an average particle size (D 50 ) of 5 μm to 20 μm, and the small particles contained in the first positive electrode active material layer have an average particle size (D 50 ) of 3 μm to 10 μm; the large particles contained in the second positive electrode active material layer have an average particle size (D 50 ) of 5 μm to 20 μm, and the small particles contained in the second positive electrode active material layer have an average particle size (D 50 ) of 3 μm to 10 μm; the first positive electrode active material layer contains large particles and small particles in a weight ratio of 85:15 to 55:45; the second positive electrode active material layer contains large particles and small particles in a weight ratio of 85:15 to 55:45; The bimodal positive electrode active materials contained in the first positive electrode active material layer and the second positive electrode active material layer each independently have a composition represented by Chemical Formula 1, [Chemical formula 1] Li x [Nia Co b M 1 c M 2 d ] O 2 In the above Chemical Formula 1, M 1 is at least one selected from Mn and Al; M2 is at least one selected from B, Mg, Ca, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta and W; A positive electrode for a lithium secondary battery, wherein 0.9≦x≦1.1, 0.7≦a<1, 0<b<0.3, 0<c<0.3, 0≦d≦0.1, and a+b+c+d=1.
2. 2. The positive electrode for a lithium secondary battery according to claim 1, wherein, in Chemical Formula 1, 0.8≦a<1, 0<b<0.2, 0<c<0.2, and 0≦d≦0.
1.
3. The positive electrode for a lithium secondary battery according to claim 1 , wherein the first positive electrode active material layer further comprises dot-shaped conductive material.
4. The positive electrode for a lithium secondary battery according to claim 1 , wherein the second positive electrode active material layer further includes dot-shaped conductive materials and linear conductive materials.
5. A lithium secondary battery comprising the positive electrode for lithium secondary batteries according to claim 1.
Citation Information
Patent Citations
Positive electrode and electrochemical device
CN110429252A
Lithium metal composite oxide powder, positive electrode active material for lithium secondary battery, positive electrode, and lithium secondary battery
JP2020087879A
Electrode for lithium secondary battery
KR1020200117496A