Laminated tube container and manufacturing method thereof
The tube container with a specific ultra-low density polyethylene resin and shoulder angle design addresses deformation and cap fitting issues, achieving reduced residual bulk and efficient manufacturing.
Patent Information
- Application Number
- JP2017210146
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2017-10-31
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2037-10-31
AI Technical Summary
Existing tube containers with flexible shoulders and mouths face issues with incomplete content usage due to deformation, difficulty in cap attachment, and high manufacturing complexity, especially when producing small amounts, leading to increased residual bulk and manufacturing challenges.
The tube container is designed with a substantially cylindrical body, a conical shoulder, and a cylindrical mouth made of ultra-low density polyethylene resin, with specific elastic modulus, melting point, and density ranges, and a shoulder angle between 120° and 180°, ensuring flexibility and smooth cap fitting.
This design reduces residual bulk by preventing deformation and enabling easy cap attachment, while allowing continuous and cost-effective manufacturing with reduced material adhesion to equipment.
Smart Images

Figure 0007596057000003 
Figure 0007596057000004 
Figure 0007596057000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated tube container that improves the ease of using up the contents (bulk) in the tube container and reduces the amount of bulk remaining.In particular, the present invention relates to a method for manufacturing laminated tube containers that can be continuously produced by preventing the preform, which is a raw material of a flexible material, from adhering more than necessary to the manufacturing equipment when manufacturing laminated tube containers by a compression method. [Background technology]
[0002] Conventionally, various types of tube containers have been known that contain paste-like or gel-like medicines, quasi-drugs, seasonings, cosmetics, chemical materials, etc. This type of tube container is composed of a cap, a cylindrical mouth portion having an extraction port to which the cap is screwed, a conical shoulder portion connected to the mouth portion, and a substantially cylindrical body portion formed from a laminated tube roll. Materials for the cylindrical body include those made of metals such as aluminum, lead, and tin, those made of plastics using materials such as polyethylene, and those made of multi-layer laminates of materials such as aluminum, paper, and polyethylene.
[0003] In order to take out the contents from these tube containers, it is necessary to push the body with a finger. The bulk pushed with the finger is pressed against the inside of a conical shoulder formed to close the axial end of the body, and is pushed out through an extraction port having a smaller diameter than the body. Due to the structure of such tube containers, even if the tube body is crushed, it is not possible to completely use up the bulk around the shoulder and the inside of the mouth. In addition, the shoulder and mouth themselves are generally made of resin such as high-density polyethylene, and are difficult to crush due to their high rigidity.
[0004] Known methods for reducing the residual bulk include forming the shoulder of the tube body by bending it at an angle (see, for example, Patent Document 1), and containers with a structure that crushes the shoulder (see, for example, Patent Document 2). Regarding laminated tube containers, tube containers in which the shoulder and mouth are formed from a flexible material have been developed (Patent Document 3, Patent Document 4).
[0005] Furthermore, when using the compression method to manufacture laminated tube containers with flexible shoulders and mouths, in the process of dropping the ring-shaped preform from the extruder around the convex part of the mandrel using a scraping plate (stripper plate), it can be difficult to hold the preform in a ring shape or it can adhere to the surface of the stripper plate, making it difficult to drop; however, a laminated tube container that solves these problems has also been developed (Patent Document 5). However, even with materials within the disclosed range, sufficient flexibility is not obtained, and problems remain with regard to the stable supply of preforms and the moldability of the shoulder and mouth portions.
[0006] In addition, if the shoulder and mouth are made of a flexible material, the shoulder will deform (e.g., be crushed) toward the end of use, making it difficult to fit the cap smoothly and causing a problem of deterioration in airtightness. In particular, the amount of medicines and the like that are expensive is often relatively small when pressed out at one time. For example, in the case of an insect bite medicine with a body diameter of 19.05 mm and a content of 20 g, the average amount used at one time is 0.04 to 0.05 g, and in the case of an ointment with a body diameter of 12.7 mm and a content of 5 g, the average amount used at one time is about 0.03 to 0.04 g. In such cases where the amount used at one time is relatively small, the cap is attached and pressed out several times even at the end of use, so smooth cap fitting at the end of use is particularly important.
[0007] In view of the above problems, the reality is that tube containers with flexible shoulders and mouths are limited to blown tubes, which are used for wasabi and other products and are entirely made of flexible materials. The inventor aimed to develop a tube container that uses a roughly cylindrical body formed from a laminated tube base material and has sufficiently flexible shoulder and mouth portions, and has been working day and night on research and development of a laminated tube container that can reduce the amount of remaining bulk, allows a cap to be fitted smoothly even towards the end of use, and allows for stable formation of the shoulder and mouth portions. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Utility Model Application Publication No. 62-19945 [Patent Document 2] Japanese Utility Model Application Publication No. 7-37949 [Patent Document 3] JP 1998-249966 A [Patent Document 4] JP 2005-306415 A [Patent Document 5] JP 2004-203394 A Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made to solve the above-mentioned shortcomings of the prior art, and its object is to prevent irregular deformation of the tube as much as possible by forming the shoulder and mouth from a flexible ultra-low density polyethylene resin and the body from a laminate material, while making it possible to push out the contents without requiring excessive force, thereby reducing the amount of bulk remaining.
[0010] Another object of the present invention is to provide a laminated tube container that prevents excessive pressure on the shoulder portion when the contents are finally used up, prevents deformation (crushing, etc.) of the shoulder portion, and enables the cap to be smoothly screwed or fitted onto the mouth portion. Another object of the present invention is to reduce the manufacturing costs of laminated tube containers, while using a compression laminated tube manufacturing device to prevent unnecessary adhesion of soft material to manufacturing equipment such as molds, thereby enabling smooth continuous production of laminated tube containers and mass production of laminated tube containers with little bulk remaining. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention has the following configuration. (1) A laminated tube container comprising a substantially cylindrical body formed from a laminated tube raw material on which a metal layer is laminated, a substantially conical shoulder welded to one end of the body, and a cylindrical mouth, the shoulder and mouth of the laminated tube container having a flexural modulus of 40 to 100 MPa, a melting point of 110°C to 130°C, and a density of 0.87 to 0.91 g / cm 3 The laminated tube container is formed from an ultra-low density polyethylene resin, and the body of the laminated tube container is formed from a laminate material laminated with a metal material. The ultra-low density polyethylene resin in the present invention has a density of 0.87 g / cm 3 Density 0.87 g / cm or more is preferable. 3 If the density is less than 0.91 g / cm, the flexibility becomes too strong, and there is a risk of problems occurring in screwing or fitting with the cap. 3 It is preferable that the density is 0.91 g / cm or less. 3 If the pressure exceeds this value, more force than necessary is required to push out the bulk remaining in the shoulder and mouth. The body of the laminated tube container of the present invention can be made of a wide range of materials, including laminated metal materials and other laminated materials.
[0012] The ultra-low density polyethylene resin in the present invention preferably has a melting point of 110° C. to 130° C. This is because a preform cannot be smoothly fed to the tip of the mandrel if the melting point is less than 110° C. If the melting point is more than 130° C., it is difficult to produce an ultra-low density polyethylene resin. Furthermore, the ultra-low density polyethylene resin in the present invention preferably has a flexural modulus of 40 to 100 MPa. If the flexural modulus is less than 40 MPa, the resin becomes too soft, which may cause problems in fitting with the cap. If the flexural modulus exceeds 100 MPa, the flexibility of the shoulder portion decreases, and the effect of the present invention may not be sufficiently obtained.
[0013] (2) The laminated tube container according to (1) above, wherein the ultra-low density polyethylene resin further has an MFR (melt flow rate) of 1 g / 10 min to 5 g / 10 min. The properties of the ultra-low density polyethylene resin used in the present invention are preferably MFR (melt flow rate) of 1 g / 10 min to 5 g / 10 min. If the MFR is less than 1 g / 10 min, the resin flow is poor, making it difficult to extrude the resin, and molding defects of the preform are likely to occur. In addition, since the resin does not flow sufficiently in the mold, molding defects such as sink marks may occur. If the MFR exceeds 5 g / 10 min, the resin flow becomes too good, and there is a risk that the shape of the preform cannot be maintained.
[0014] (3) A laminated tube container as described in (1) or (2) above, characterized in that a cap is screwed or fitted onto the mouth portion constituting the laminated tube container, and the shoulder portion constituting the laminated tube container has a shoulder angle (θ) of 120<θ<180°. By employing such a configuration for the laminated tube container, it is possible to prevent the shoulder portion from being deformed more than necessary (such as being crushed) toward the end of use, and to maintain smooth fitting of the cap. The shoulder angle here means the opening angle (θ) centered on the intersection point P of the lines Q1 and Q2 of the opposing shoulders, as shown in FIG. Laminated tube containers generally have a shoulder angle. The diameter of the mouth of a laminated tube container is smaller than the diameter of the body. Therefore, a shoulder angle (θ) is formed to improve the flow of the contents into the mouth, which has a smaller diameter than the body, when pushing out the contents. However, if the shoulder angle (θ) is set to 120° or less (the shoulder angle becomes more inclined), the amount of contents remaining inside the shoulder increases. On the other hand, if the shoulder angle (θ) approaches 180° (the shoulder angle becomes more gentle), the flow of the contents to the mouth decreases, making it difficult to squeeze out when only a small amount remains. Also, if the shoulder angle is too shallow, it can cause deterioration of the adhesion between the shoulder and the body when manufacturing a laminated container by the compression method.
[0015] In view of the above-mentioned problems with the present invention, it is more preferable that the shoulder angle is 140° or more and 160° or less. By forming the shoulder angle within the above range, the cap screwed onto the mouth can be smoothly fitted at the end when the contents are used up. That is, if the shoulder angle (θ) is less than 140°, a large amount of contents remains inside the shoulder as described above, and the user presses the shoulder, particularly the vicinity of the connection with the body, to push out the residue. This results in the shape of the shoulder being deformed (crushed, etc.). The shoulder in the present invention has a flexural modulus of elasticity of 40 to 100 MPa, a melting point of 110°C to 130°C, and a density of 0.87 to 0.91 g / cm 3 Since the shoulder is made of ultra-low density polyethylene resin, it is difficult to restore the original shape of the shoulder once it has been deformed. Therefore, the deformation of the shoulder causes the lower part of the cap screwed onto the mouth to come into contact with or separate from the deformed shoulder, making it difficult to screw or fit the cap smoothly.
[0016] (4) A method for manufacturing a laminated tube container by attaching a laminated tube raw material having a metal layer laminated thereon to a mandrel and rotating a turntable, the method comprising the steps of: forming a convex portion at the tip of the mandrel for forming a mouth portion of the laminated tube; forming a ring-shaped tube in the vicinity of the base portion of the convex portion; and forming a flexural modulus of elasticity of 40 to 100 MPa, a melting point of 110°C to 130°C, and a density of 0.87 to 0.91 g / cm3. 3 and then, after placing molten resin made of ultra-low density polyethylene resin, pressing the mandrel into the cavity of a molding die set on a turntable and forcing the molten resin into the cavity while surrounding the end of the laminate tube roll with molten resin, thereby welding an approximately conical shoulder portion and a cylindrical mouth portion formed by the molten resin to the end of the approximately cylindrical body portion formed by the laminate tube roll.
[0017] (5) The method for producing a laminated tube container according to (3) above, wherein the molten resin is further formed of an ultra-low density polyethylene resin having an MFR (melt flow rate) of 1 g / 10 min to 5 g / 10 min. (6) The method for manufacturing a laminated tube container described in (4) or (5) above, further comprising a step of screwing or fitting a cap onto the mouth portion, wherein the shoulder portion constituting the laminated tube container is formed with a shoulder angle of 120°<θ<180°. Effect of the Invention
[0018] By adopting the structure of the laminated tube container according to the present invention, it is possible to prevent irregular deformation of the tube as much as possible and to push out the contents without requiring excessive force, thereby achieving the effect of reducing the remaining bulk amount. In addition, by setting the shoulder angle within a predetermined range, the laminated tube container of the present invention prevents excessive pressure on the shoulder at the final stage when the contents are used up, prevents deformation (crushing, etc.) of the shoulder, and enables the cap to be smoothly screwed or fitted onto the mouth.
[0019] Furthermore, by adopting the manufacturing method of the laminated tube container according to the present invention, it is possible to reduce the manufacturing cost of the laminated tube container, while preventing unnecessary adhesion of soft material to the manufacturing equipment, such as molds, by the laminated tube manufacturing equipment for compression, thereby enabling smooth continuous production of laminated tube containers, and having the excellent effect of enabling mass production of laminated tube containers with little bulk remaining. [Brief description of the drawings]
[0020] [Figure 1] 1 is a partial cross-sectional view for explaining the shoulder angle in a laminated tube container, where (a) shows a small shoulder angle (θ1) and (b) shows a large shoulder angle (θ2). [Diagram 2] 1 is a graph showing the results of comparing bulk remaining amounts in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The laminated tube container of the present invention is composed of a laminated tube container having an approximately cylindrical body portion formed from a laminated tube roll, an approximately conical shoulder portion welded to one end of the body portion, and a cylindrical mouth portion. The shoulder and mouth parts in the present invention have a flexural modulus of elasticity of 40 to 100 MPa, a melting point of 110°C to 130°C, and a density of 0.87 to 0.91 g / cm 3 It is characterized in that it is made of very low density polyethylene resin.
[0022] The raw material for the laminate tube used in the present invention is formed by laminating a biaxially oriented polyester film, a metal foil, a polyethylene resin, an ethylene-carboxylic acid copolymer resin, and the like.
[0023] Examples of biaxially stretched polyester films include polyethylene terephthalate film (PET), polybutylene terephthalate film (PBT), polyethylene isophthalate, polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), etc. Among these, PET is particularly preferred. Examples of metal foils include aluminum (AL), stainless steel, tin, lead, copper, iron, nickel, and alloys thereof (e.g., JIS 8079 materials). In particular, AL foil and AL alloy foil are preferred in terms of availability, price, good elongation, etc. However, laminate tubes that do not use metal foils are also included in the scope of the present invention.
[0024] Examples of ethylene-carboxylic acid copolymer resins include ethylene-acrylic acid copolymer (EAA) and ethylene-methacrylic acid copolymer (EMAA). Such ethylene-carboxylic acid copolymer resins are preferably laminated to the above-mentioned metal foil by extrusion lamination. Extrusion lamination may be performed by applying an anchor coating agent to the lamination surface and extruding the resin. By laminating in this manner by extrusion lamination, no adhesive layer is formed at the interface with the metal foil, so that delamination between the metal foil and the ethylene-carboxylic acid copolymer resin can be prevented.
[0025] Examples of polyolefin resins include linear low density polyethylene (L-LDPE), high density polyethylene (HDPE), low density polyethylene (LDPE), and ethylene-vinyl acetate copolymer (EVA). Also, a coextrusion stretched film may be laminated. As the coextrusion stretched film, a film obtained by laminating a polyolefin resin on both sides of a polyamide resin and coextrusion stretching the film can be used. As the polyamide resin, nylon (Ny) is particularly preferable because it has a high barrier property against the penetration of contents and is excellent in alkali resistance. As the nylon, for example, 6-nylon, 66-nylon, 11-nylon, MXD6 nylon, etc. can be used. As the polyolefin resin, L-LDPE is preferable.
[0026] Next, an example of a method for producing a laminated tube container according to the present invention will be described. In a method for manufacturing a laminated tube container, a laminated tube raw material having a metal layer laminated thereon is attached to a mandrel and a turntable is rotated, and a convex portion for forming a mouth portion of the laminated tube is formed at the tip of the mandrel, and a ring-shaped molded material having a bending elastic modulus of 40 to 100 MPa, a melting point of 110°C to 130°C, and a density of 0.87 to 0.91 g / cm is formed near the base of the convex portion. 3 and then, after placing molten resin made of ultra-low density polyethylene resin, pressing the mandrel into the cavity of a molding die set on a turntable and forcing the molten resin into the cavity while surrounding the end of the laminate tube roll with molten resin, thereby welding a substantially conical shoulder portion and a cylindrical mouth portion formed by the molten resin to the end of the substantially cylindrical body portion formed by the laminate tube roll. The method for producing a laminated tube container according to (3) above, wherein the molten resin is further formed of an ultra-low density polyethylene resin having an MFR (melt flow rate) of 1 g / 10 min to 5 g / 10 min.
[0027] In the present invention, a member for forming a tube is attached to a mandrel, and a shoulder and a mouth are formed on a laminate tube container while rotating the mandrel counterclockwise on a turntable. A laminate tube raw material is wound around the mandrel in advance in a cylindrical shape. A convex portion for forming the mouth of the laminate tube is formed at the tip of the mandrel, and molten resin formed of ultra-low density polyethylene resin molded into a ring shape is placed near the base of the convex portion. The molten resin is placed by dropping the ultra-low density polyethylene resin molded into a ring shape from above onto the outer periphery of the mandrel. The ultra-low density polyethylene resin has a flexural modulus of elasticity of 40 to 100 MPa, a melting point of 110°C to 130°C, and a density of 0.87 to 0.91 g / cm. 3 It needs to be.
[0028] The primary objective of the present invention is to form a shoulder portion having flexibility, but the material that imparts flexibility has high viscosity in the preform state, and therefore adheres to the manufacturing equipment, making processing difficult. If an ultra-low density polyethylene resin having the characteristics limited in the present invention is not used, the preform molded into a ring shape may adhere to the stripper plate and not fall. If an ultra-low density polyethylene resin having such characteristics is used, the preform can be fed without adhering to the stripper plate, and a shoulder portion and a mouth portion having the desired flexibility can be molded. Next, rotate the mandrel counterclockwise on the turntable and drive the mold cavity from above. If the mold is a split mold, the shoulder and mouth can be removed from the mold without moving the mandrel by rotating it. EXAMPLES
[0029] Example 1 (Product of the Invention) The results of tests on the ease of disposing of the contents (bulk) of the laminated tube container according to the present invention are described below. The laminate base material used in the test was formed into a cylindrical tube body base material by laminating PE / PET / PE / colored PE / PE on both sides of an AL foil with EAA between them toward the outer layer side, and laminating PE on the inner layer side. The raw roll for the tube body is then formed with a shoulder and a mouth by a compression method. At this time, the shoulder and mouth are formed with a bending modulus of elasticity of 70 MPa, a melting point of 115°C, and a density of 0.9 g / cm 3 The laminated tube container is made of ultra-low density polyethylene with MFR of 2.0 g / 10 min. The shoulder angle of the shoulder part that constitutes the laminated tube container is θ2 (150°) as shown in Fig. 1(b). Example 2 (Product of the Invention) A tube having the same body as the laminated tube container of Example 1 described above was manufactured, with the shoulder and mouth molded from ultra-low density polyethylene having the following physical properties. The manufacturing method used was the compression method, as in the case of the product of the present invention. However, the shoulder angle was formed at θ1 (120°) as shown in Figure 1(a). Flexural modulus: 70MPa Melting point: 115℃ Density: 0.900g / cm 3 MFR: 2.0g / 10min
[0030] Comparative Examples 1 to 6 For comparison, laminated tube containers were manufactured using materials with the following characteristics for forming the shoulder and mouth. The manufacturing method was the compression method, as in the case of the product of the present invention. However, the shoulder angle of the shoulder constituting the laminated tube container was 120° in all cases. Comparative Example 1 (conventional product) A tube having the same body as the above-mentioned product of the present invention was manufactured, with the shoulder and mouth molded from high density polyethylene (HDPE) having the following physical properties. The manufacturing method used was the compression method, as in the product of the present invention. Flexural modulus: 820MPa Melting point: 132℃ Density: 0.953g / cm 3 MFR: 5.0g / 10min Comparative Example 2 A tube having the same body as the above-mentioned product of the present invention was manufactured, with the shoulder and mouth molded from low-density polyethylene (LDPE) having the following physical properties. The manufacturing method used was the compression method, as in the product of the present invention. Flexural modulus: 220MPa Melting point: 114℃ Density: 0.928g / cm 3 MFR: 3.0g / 10min
[0031] Comparative Example 3 A tube having the same body as the above-mentioned product of the present invention was manufactured, with the shoulder and mouth molded from low-density polyethylene (LDPE) having the following physical properties. The manufacturing method used was the compression method, as in the product of the present invention. Flexural modulus: 185MPa Melting point: 107℃ Density: 0.919g / cm 3 MFR: 2.0g / 10min Comparative Example 4 A tube having the same body as the above-mentioned product of the present invention was manufactured, with the shoulder and mouth molded from linear low density polyethylene (LLDPE) having the following physical properties. The manufacturing method used was the compression method, as in the product of the present invention. Flexural modulus: 340MPa Melting point: 123℃ Density: 0.930g / cm 3 MFR: 2.5g / 10min
[0032] Comparative Example 5 A tube having the same body as the above-mentioned product of the present invention was manufactured, with the shoulder and mouth molded from linear low density polyethylene (LLDPE) having the following physical properties. The manufacturing method used was the compression method, as in the product of the present invention. Flexural modulus: 50MPa Melting point: 93℃ Density: 0.900g / cm 3 MFR: 4.0g / 10min Comparative Example 6 A tube having the same body as the above-mentioned product of the present invention was manufactured, with the shoulder and mouth molded from linear low density polyethylene (LLDPE) having the following physical properties. The manufacturing method used was the compression method, as in the product of the present invention. Flexural modulus: 50MPa Melting point: 93℃ Density: 0.903g / cm 3 MFR: 2.0g / 10min
[0033] Table 1 summarizes the productivity and flexibility results for each resin. Productivity is the result of an evaluation taking into consideration stable supply of preforms (whether resin adheres to the stripper plate, etc.) and moldability (sink marks, dimensional accuracy). Regarding the evaluation of productivity in Table 1, ○ indicates that the laminated tube container was produced without any problem. △ indicates that the preform adhered to the stripper plate or the like, which may have caused tube molding defects. × indicates that a problem occurred in molding or supplying the preform, and the tube could not be produced. Flexibility was determined by assessing whether the mouth part could be easily deformed by finger pressure. Regarding the evaluation of flexibility in Table 1, ○ indicates that the opening can be deformed without excessive force, × indicates that it is difficult to deform the opening with finger pressure and the flexibility is poor. Also, - indicates that the productivity was poor and it was not possible to manufacture tubes sufficient for verification, so the flexibility was not evaluated.
[0034] [Table 1]
[0035] As is clear from the results in Table 1, the laminated tube containers of Examples 1 and 2 have excellent flexibility and good productivity, and it has been demonstrated that laminated tube containers can be continuously produced using a compression laminated tube manufacturing apparatus. On the other hand, it was found that the laminated tube containers according to Comparative Examples 2 and 4 did not have sufficient flexibility compared to Comparative Example 1 (conventional product). Moreover, in Comparative Example 5, it was found that it was difficult to produce a laminate tube container by the compression method. Moreover, in Comparative Example 3, since the preform adhered to the stripper plate, there was a risk of problems occurring in the production of laminated tube containers by the compression method, and it was found that practical use was difficult. Also, although Comparative Example 6 had sufficient flexibility, it was found that there was a possibility of problems occurring in the production of laminated tube containers using the compression method.
[0036] The above tests demonstrated that only the laminated tube containers according to Examples 1 and 2 of the present invention were excellent in flexibility and could be stably and continuously produced. Next, commercially available hand cream was filled into the above tubes of Example 1, Example 2, and Comparative Example 1, and a content ejection test was conducted by three monitors (a woman in her 30s, a woman in her 40s, and a man in his 50s) to measure the remaining bulk amount. The results are shown in the following Table 2 and Figure 2. The reduction rate is a result calculated based on the tube container of Comparative Example 1 (conventional product).
[0037] [Table 2]
[0038] As is clear from the results in Table 2 and FIG. 2, the bulk remaining amount in the laminated tube containers of Examples 1 and 2 is significantly reduced compared to the tube container of Comparative Example 1 (conventional product). The results of Example 2 indicate that the contents near the mouth and shoulder were easily squeezed out by finger pressure because the shoulder and mouth were made of a flexible material. However, the shoulders of all three can become deformed (crushed, etc.), which can cause problems with the cap fitting towards the end of use. On the other hand, the tube of Example 1 showed the same remaining amount reduction as Example 2, and the shoulder was not deformed (crushed, etc.). In other words, it means that the contents near the shoulder were discharged without deforming the shoulder, and it can be said that a significant reduction in the remaining amount and smooth cap fitting at the end of use were achieved compared to the conventional product.
Claims
1. A laminated tube container comprising a substantially cylindrical body portion formed from a laminated tube raw material, a substantially conical shoulder portion welded to one end of the body portion, and a cylindrical mouth portion, wherein the shoulder portion and the mouth portion of the laminated tube container have a bending elastic modulus of 40 to 100 MPa, a melting point of 110 to 130°C, and a density of 0.87 to 0.91 g / cm 3 a cap is screwed or fitted onto a mouth portion constituting the laminated tube container; a shoulder portion constituting the laminated tube has a shoulder angle of 120°<θ<180°; and the ultra-low density polyethylene resin further has an MFR (melt flow rate) of 1 g / 10 min to 5 g / 10 min.
2. In a method for manufacturing a laminated tube container by attaching a laminated tube raw material to a mandrel and rotating a turntable, a convex portion for forming a mouth portion of the formed laminated tube is formed at the tip of the mandrel, and a ring-shaped molded material having a bending elastic modulus of 40 to 100 MPa, a melting point of 110 to 130°C, and a density of 0.87 to 0.91 g / cm is formed near the base of the convex portion. 3 a mandrel is pressed into a cavity of a molding die set on a turntable, and the molten resin is pressure-filled into the cavity while surrounding an end of the laminate tube roll with the molten resin, thereby welding a substantially conical shoulder portion and a cylindrical mouth portion formed by the molten resin to an end of a substantially cylindrical body portion formed by the laminate tube roll, with a shoulder angle of 120°<θ<180°, and the molten resin is formed of an ultra-low density polyethylene resin having an MFR (melt flow rate) of 1 g / 10 min to 5 g / 10 min.
3. 3. The method for producing a laminated tube container according to claim 2, further comprising a step of screwing or fitting a cap onto the opening of the laminated tube container.
Citation Information
Patent Citations
JP1987019945U
collapsible plastic container
JP1995037949U
JP1996-3000506A
Plastic core for adhesive tape and adhesive tape laminate using the plastic core
JP1998017216A
Polyolefin composition for exterior parts
JP1998139958A