Bonded Steel and Titanium by Additive Manufacturing
By using a compatible third metal interfacial layer and a non-reactive environment, additive manufacturing effectively bonds steel and titanium, addressing the challenge of dissimilar metal joining and enhancing structural integrity and weight reduction in manufactured articles.
Patent Information
- Application Number
- JP2020142493
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-06
- Filing Date
- 2020-08-26
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2040-08-26
AI Technical Summary
Existing additive manufacturing techniques face challenges in joining dissimilar metals like steel and titanium, as they often fail to form graded alloys due to differences in lattice energies and spacings, leading to phase-separated systems.
Incorporating a thin interfacial layer of a mutually compatible third metal, such as vanadium, niobium, or tantalum, between the steel and titanium substrates, which forms graded alloys with both metals, and using a non-reactive environment to melt and bond the second metal to this layer.
This method enables strong, reliable bonding of steel and titanium components, facilitating high-strength, lightweight structures suitable for applications like aircraft components, with improved mechanical properties and reduced defects.
Smart Images

Figure 0007596096000001 
Figure 0007596096000002 
Figure 0007596096000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates generally to the field of additive manufacture of industrial articles, and more particularly to the field of additive manufacture of articles including bonded steel and titanium. [Background technology]
[0002] Additive manufacturing, or "3D printing", has been used to fabricate articles of complex topology. In this technique, a solid real-world article is built layer-by-layer based on an appropriate digital model that defines the desired topology of the article. The resulting article is a high-fidelity realization of the digital model, obtained with minimal human intervention or dedicated tooling. When applied to the production of metal-containing articles, additive manufacturing typically requires the localized fusion of a consumable metal by a focused high-energy beam. The locus of the article where material is to be added is controlled in real time by moving the article relative to the beam and / or rastering the beam across the article. The consumable metal may be provided as a thin coating of particulates that are deposited across the article to be formed, or it may be directly directed to the locus via a nozzle. Summary of the Invention [Problem to be solved by the invention]
[0003] In recent years, technologies have been developed that extend the reach of additive manufacturing to industrially important metals. Nevertheless, various challenges remain. One particular challenge relates to the additive manufacturing of articles that contain dissimilar bonded metals, such as steel and titanium. [Means for solving the problem]
[0004] Some of the examples disclosed herein relate to a method of additively manufacturing an article comprising a bonded first metal and a second metal, the first metal comprising one of steel and titanium and the second metal comprising the other of steel and titanium. The method includes disposing an interface layer of a third metal on a substrate of the first metal, the third metal being capable of forming an alloy with the first metal and capable of forming an alloy with the second metal. The method further includes providing a consumable form of the second metal at a trace of the interface layer and heating the trace of the interface layer in a non-reactive environment. In the method, the heating step melts the consumable form of the second metal to form a molten form of the second metal. offer , bonding a molten form of the second metal to the interface layer.
[0005] Another example relates to an article comprising a substrate of a first metal and a printed structure of a second metal. The printed structure of the second metal is formed by melting a consumable form of the second metal. offer and simultaneously bonded to a substrate through a partially dissolved layer of a third metal. The first metal comprises one of steel and titanium and the second metal comprises the other of steel and titanium. In the article so formed, the third metal at least infiltrates the substrate of the first metal.
[0006] Another example relates to a method of additively manufacturing an article comprising bonded first and second metals, where the first metal comprises one of steel and titanium and the second metal comprises the other of steel and titanium. The method includes disposing a layer of niobium on a substrate of the first metal and providing a consumable form of the second metal to a trace of the niobium layer. The method includes heating the trace of the niobium layer in a non-reactive environment, where the heating melts the consumable form of the second metal to provide a molten form of the second metal. offer and bonding a molten form of the second metal to the niobium layer.
[0007] This Summary is not intended to identify key or essential features of the claimed subject matter. Rather, the scope of the claimed subject matter is not limited to the contents of this Summary, nor to implementations that address any problems or shortcomings that may be noted in any part of this disclosure. The features, functions, and advantages described in this disclosure may be achieved independently in some embodiments and may be combined in other embodiments.
[0008] The present disclosure will be better understood from a reading of the following detailed description in conjunction with the accompanying drawings, in which: [Brief description of the drawings]
[0009] [Figure 1] 1 is a graph showing an exemplary desired composition across a joint of alloying metal A and metal B. [Figure 2A] FIG. 1 illustrates an embodiment of an exemplary product of manufacture including an article comprising bonded steel and titanium. [Figure 2B] FIG. 2B is another view of the article from FIG. 2A. [Diagram 3] FIG. 1 illustrates an embodiment of an exemplary apparatus configured for additive manufacturing of articles from consumable metal particulates. [Figure 4] FIG. 1 illustrates aspects of an exemplary apparatus configured for additively manufacturing an article from a consumable metal wire. [Diagram 5] FIG. 1 illustrates an embodiment of an exemplary method for additively manufacturing an article comprising bonded first and second metals. [Figure 6] 6A-6C illustrate embodiments of exemplary articles that may be formed according to the method of FIG. 5. [Figure 7] 6 shows a series of energy dispersive X-ray (EDX) radiation images of a region of a cleavage plane of an example article formed according to the method of FIG. 5. [Figure 8] FIG. 8 illustrates EDX line scan data extracted along two paths extending through the region shown in FIG. 7. [Figure 9]6 shows the results of nanoindentation line scan experiments performed on different areas of the cleaved facet of an article formed according to the method of FIG. 5. [Figure 10] 6 shows a scanning electron microscope (SEM) image of another area of the cleaved facet of an article formed according to the method of FIG. 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] As mentioned above, state-of-the-art additive manufacturing may not be suitable for articles that contain dissimilar bonded metals. To provide a high-strength article, each locus of molten consumable metal must be reliably bonded to the layer below it. In a scenario where the molten metal and the underlying layer contain different metals, the joint between these metals should exhibit a composition gradient, with atoms of the molten metal diffusing into the underlying layer and vice versa. Ideally, the joint contains an alloy of graded composition, as shown in the composition profile graph in Figure 1.
[0011] However, some combinations of dissimilar metals do not form such alloys. In many cases, the lattice energies of the pure metals and the lattice energies of the hypothetical alloys are such that the free energy of the alloy is greater than the free energy of the phase-separated system. This can occur, for example, when the lattice spacings of the metals being joined are very different. In other cases, the dissimilar metals can form stable intermetallic compounds of constant composition (e.g., 1:1, 2:1, etc.), as opposed to the graded alloy composition shown in FIG. 1. Without binding this disclosure to a particular theory, it is believed that both of these effects contribute to the observed difficulty of directly joining steel and titanium by direct additive manufacturing.
[0012] The inventors herein have found a solution to the above-mentioned difficulties, in which a relatively thin interfacial layer of a mutually compatible third metal is additively incorporated onto the substrate of the first metal and beneath the molten form of the dissimilar second metal. The composition of the interfacial layer is selected based on the ability of the interfacial layer to form a gradient alloy with each of the first and second metals to be joined.
[0013] Before describing this solution in detail, one exemplary application context for the additively manufactured article thus formed is presented. Figure 2A shows an embodiment of an exemplary manufactured product 200 in the form of an aircraft. The aircraft includes, among other things, a fuselage 202, a wing section 204, and a tail section 206 with a control surface 208. As shown in the cutaway portion of this drawing, the control surface 208 is actuated by a hydraulically driven rotatable gear 210 that controls the deflection of the control surface. The gear 210 includes a shaft 212 to which a sprocket 214 is coupled. This configuration is also shown in Figure 2B.
[0014] Substantially all of the structural and / or functional components of the aircraft may be optimized for mechanical strength. In addition, many of the same components are further optimized for weight reduction. To this end, the sprocket 214 may comprise a steel selected for strength, hardness, and durability. The shaft 212, being of significant length, may comprise titanium or a titanium alloy selected for high strength and light weight. Most steels have a density between 7.75 and 8.05 grams per cubic centimeter (g cm -1 ), whereas titanium has a density of 4.51 g cm -1 Because of this, incorporating titanium into components of any significant size is particularly advantageous. In some embodiments, it may be desirable to print the sprocket 214 directly onto a previously machined titanium or titanium alloy shaft 212 by additive manufacturing methods.
[0015] It will be understood that the examples shown in this disclosure in no way limit the applicability of the underlying technology. Indeed, the methods described herein may be applied to the additive manufacturing of a wide range of articles, including bonded steel and titanium. Such articles may or may not be specifically constructed to optimize mechanical strength to weight. Furthermore, it is not necessarily true that the substrate of an additively manufactured article comprises titanium or that the printed portion comprises steel, as the opposite configurations are envisioned as well.
[0016] FIG. 3 illustrates an embodiment of an exemplary apparatus 300 configured for additively manufacturing an article 310. The apparatus 300 includes a chamber 316 that surrounds the article 310 during the additive manufacturing process. The chamber 316 includes a rotating chuck 320 to which the article 310 is secured during the additive manufacturing process. In the particular non-limiting example illustrated in FIG. 3, a substrate 312 of the article 310 is secured to the rotating chuck 320. A rotary mount may be useful, for example, for additive manufacturing of articles having rotational symmetry. In other examples, the article may be secured by a vice, clamp, or anvil.
[0017] As used herein, a "substrate" is a basic component of an article to be formed by additive manufacturing. In some examples, the substrate is a component of relatively simple topology and may be formed by conventional machining. In some examples, the substrate may include titanium, and in other examples, the substrate may include steel.
[0018] 3 , an interface layer 322 comprising a thin foil of a third metal is disposed on the substrate 312. In some examples, the interface layer may be pre-welded to the substrate. In other examples, the interface layer may be initially disposed on the substrate but not firmly adhered to the substrate. During additive manufacturing of the article 310 (see below), the interface layer 322 may become welded to the substrate 312.
[0019] In apparatus 300, article 310 is formed in layers by spatially selective application of a molten form 314 of a second metal to underlying layers of the article, beginning with substrate 312, or beginning with interface layer 322 in embodiments in which an interface layer is included. Thus, apparatus 300 includes a metal particulate reservoir 324 that stores a supply of a consumable form of the second metal embodied as metal particulate 326. The metal particulate may include, for example, a coarse or fine metal powder. In examples in which the substrate includes titanium or a titanium alloy, the metal particulate may include steel, and in examples in which the substrate includes steel, the metal particulate may include titanium or a titanium alloy.
[0020] The apparatus 300 includes a metal particulate pump 328 that pumps metal particulate 326 from a metal particulate reservoir 324 and delivers the pumped metal particulate to a nozzle 330. In the illustrated example, the nozzle 330 is positioned above a trajectory 332 where the molten metal particulate will be added to the article 310. Other embodiments may include multiple nozzles that distribute a thin layer of metal particulate across the surface of the article to be formed. In either case, the chamber 316 may be configured to return the unmelted metal particulate to the metal particulate reservoir 324 for later use.
[0021] Apparatus 300 includes an energy beam source 334 that delivers an energy beam 336 to the trajectory 332 to melt the metal particles in the trajectory, thereby adding the molten metal particles to article 310. In some embodiments, the energy beam source may include a laser, such as a pulse-modulated high power infrared laser. The laser has a diameter of approximately 4 square millimeters (mm 2 ) at a focal area of 1500-2000 watts (W). In other embodiments, an electron beam source, a plasma arc, a gas metal arc source, or any energy source of substantially similar power and focal area may be used in place of the laser.
[0022] The apparatus 300 is configured to maintain a non-reactive environment 340 in the chamber 316 at least during melting of the metal particulate. The non-reactive environment can include, for example, an environment depleted of oxygen and nitrogen. In some examples, the non-reactive environment can include a vacuum. In other examples, the non-reactive environment can include an atmosphere of an inert gas, such as argon or helium. In some particular examples, the non-reactive environment can include nitrogen. In some examples, the inert gas can flow through the chamber 316. In other examples, the atmosphere can be nominally static to avoid excessive cooling of the molten metal particulate.
[0023] The apparatus 300 includes a translation stage 342 mechanically coupled to the rotating chuck 320. As the article is formed layer by layer in the apparatus 300, the translation stage 342 may be configured to gradually lower the height of the rotating chuck as successive layers of the article are built up. The translation stage 342 may also be configured to laterally move the rotating chuck 320 to controllably vary the relative position of the trajectory 332 to the reference frame of the rotating chuck and thus the reference frame of the article 310. The translation stage may include two or more component translation stages (e.g., linear actuators) that move the chuck in two or more corresponding directions, which may include, for example, Cartesian X-axis, Y-axis, and Z-axis. In some examples, one or more component rotation stages may be used instead of or in addition to one or more component translation stages. In other examples equally consistent with this disclosure, the translation or rotation stage may be mechanically coupled to the energy beam source 334 and / or the nozzle 330, and the rotating chuck 320 may be stationary. In other examples, the rotating chuck and the energy beam source and / or the nozzle may be movable. When applied to an energy beam source in the form of a laser, the rotation stage may include a mirror with controlled deflection to thereby reflect the focused laser beam to any desired trajectory 332.
[0024] The apparatus 300 includes a computer 344. The computer 344 is operatively coupled to the translation stage 342 and configured to control in real time the relative position of the trajectory 332 with respect to the reference frame of the rotating chuck 320 via a series of actuator control signals. In addition, the computer 344 is operatively coupled to the energy beam source 334 and configured to control in real time the power provided to the trajectory via one or more energy beam control signals. The computer 344 is further configured to receive a digital model 346 representing the topology of the article to be formed. The nature and / or digital data structure of the digital model are not particularly limited. In some examples, the digital model can include a CAD file. The computer is configured to vary the actuator control signal output and the energy beam control signal output based on the digital model to achieve additive manufacturing of the article defined by the digital model.
[0025] A variety of other additive manufacturing apparatuses may be used instead, and the aspects of the apparatus 300 should not be construed in a limiting sense. Figure 4 shows another apparatus 400 configured for additively manufacturing an article 410. In the apparatus 400, a chamber 416 surrounds an article secured to a rotating chuck 420. As noted in the previous configuration, an interface layer 422 comprises a thin foil of a third metal disposed over the substrate 412.
[0026] In the apparatus 400, the article 410 is formed in layers by spatially selective application of a molten form 414 of a second metal to underlying layers of the article, beginning with a substrate 412, or beginning with an interface layer 422 in embodiments in which an interface layer is included. Thus, the apparatus 400 includes a metal wire spool 492 that stores a supply of a consumable form of a second metal embodied as a metal wire 490. The metal wire can include, for example, wire of any shape, size, and / or gauge, e.g., 14, 16, 18, or 20 gauge. In examples in which the substrate includes titanium or a titanium alloy, the metal wire can include steel, and in examples in which the substrate includes steel, the metal wire can include titanium or a titanium alloy.
[0027] The apparatus 400 includes a wire feeder 494 that directs metal wire 490 from a metal wire spool 492 and delivers the metal wire to a nozzle 430. In the illustrated example, the nozzle 430 is positioned adjacent a track 432 where a molten form of the metal wire will be applied to the article 410.
[0028] In the apparatus 400, the energy beam source 434 takes the form of an electron beam emitter that emits an electron beam 436. The electron beam emitter may, in some instances, have a size of about 1-5 square millimeters (mm 2 ) at 1500-2000 watts (W). In other embodiments, a laser, plasma arc, gas metal arc source, or virtually any energy source may be used in place of the electron beam emitter.
[0029] As with the previous configurations, the apparatus 400 is configured to maintain a non-reactive environment 440 in the chamber 416 at least during melting of the metal wire 490. The non-reactive environment can include a vacuum or, in some examples, an atmosphere of an inert gas, such as argon or helium. In embodiments where the non-reactive environment is a vacuum environment, the energy beam source 434 can include an electrically heated filament that promotes thermionic emission of electrons. In embodiments where the non-reactive environment includes an inert gas, electron emission can be promoted by ionization of the inert gas. In these and other embodiments, the energy beam source 434 can be biased with a negative voltage while the rotating chuck 420, the substrate 412, and the article 410 are maintained at ground potential. In this manner, electrons from the energy beam source are accelerated toward a trajectory 432 of the article where material deposition is desired.
[0030] In the apparatus 400, a metal wire feeder 494 feeds a metal wire 490 directly into the electron beam 436 or into a track 432 heated by the electron beam. In this example, the energy beam source 434 includes a high melting point metal, such as tungsten, that is not intended to be consumed in an additive manufacturing process. In other examples, the energy beam source can take the form of a plasma arc or a gas metal arc. In some variations, the consumable metal wire itself may be part of the heating circuit, may conduct current, and may be biased at a different voltage than the article 410.
[0031] As with the previous configuration, the apparatus 400 includes a translation stage 442 mechanically coupled to a rotating chuck 420. In other examples equally consistent with this disclosure, the translation stage or rotation stage may be mechanically coupled to the energy beam source 434 and / or the nozzle 430, and the rotating chuck 420 may be stationary. In other examples, the rotating chuck and the energy beam source and / or nozzle may be movable.
[0032] In the apparatus 400, a computer 444 is operatively coupled to the translation stage 442, the energy beam source 434, and the metal wire feeder 494. The computer is configured to receive a digital model 446 of the article to be formed, as described above.
[0033] FIG. 5 illustrates an embodiment of an exemplary method 500 for additively manufacturing an article including a bonded first metal and a second metal, where the first metal includes one of steel and titanium, and the second metal includes the other of steel and titanium. In some examples, the "steel" referred to herein can include carbon steel. In other examples, the steel can include an alloy steel. One non-limiting example of an alloy steel that can be used in the method 500 is Maraging M300 steel, which includes, by mass, 67% iron, 18.5% nickel, 9% cobalt, 4.8% molybdenum, 0.6% titanium, 0.1% aluminum, 0.10% silicon, 0.10% manganese, 0.030% carbon, 0.01% zirconium, 0.01% sulfur, and 0.0030% boron. Similarly, the "titanium" referred to herein can include substantially pure titanium or any suitable titanium alloy. One non-limiting example of a titanium alloy that may be used in the method 500 is Ti-6AL-4V, which contains approximately 6% aluminum and 4% vanadium by mass.
[0034] The method 500 may be implemented using the apparatus 300 of Figure 3 described above. However, it will be appreciated that the method 500 may be implemented using any other suitable apparatus, which may differ significantly from the apparatus 300 in some implementations.
[0035] At 548 of method 500, the first metal, steel or titanium substrate is etched to facilitate additive manufacturing of the article. Etching may include chemical etching, electrochemical etching, mechanical etching (e.g., polishing such as sanding), or any desired combination of the above etches. Etching may be used to prime the exterior surface of the substrate, thereby enhancing adhesion of the additive metal to the substrate. At 550, the substrate is secured to an additive manufacturing apparatus. The substrate may be secured by, for example, a chuck, a vice, a clamp, or an anvil.
[0036] At 552, an interface (or so-called "buttering") layer of a third metal is disposed on the substrate of the first metal. The third metal can be any metal capable of forming an alloy with the first metal and capable of forming an alloy with the second metal. In some examples, the third metal can exhibit a lattice spacing intermediate between the lattice spacing of steel and the lattice spacing of titanium. Typically, the third metal does not form an intermetallic compound with either steel or titanium. In some examples, the interface layer can include one or more of vanadium, niobium, and tantalum. In some examples, the interface layer can include a foil. For example, a niobium foil having a thickness of about 0.01 to 0.10 inches can be used as the interface layer.
[0037] At 554, a consumable form of a second metal is provided to the locus of the interface layer. In examples where the substrate includes titanium or a titanium alloy, the consumable form of the second metal can include steel, and in examples where the substrate includes steel, the consumable form of the second metal can include titanium or a titanium alloy. In some examples, the consumable form of the second metal can include metal particulates. The metal particulates can be selectively provided to the locus of the interface layer where the second metal is to be added in some implementations. In other implementations, the metal particulates can be provided in a thin layer across the entire interface layer. In other examples, the consumable form of the second metal can include metal wires as described above.
[0038] At 556, the interface layer traces are heated in a non-reactive environment of the additive manufacturing device. As discussed above, the non-reactive environment is an oxygen and nitrogen depleted environment. The non-reactive environment may include a vacuum, or a static or flowing argon or helium atmosphere, in some examples. The interface layer traces may be heated using a laser beam, for example, a beam of a laser providing about 1500 to about 2000 watts at a focal region. In other embodiments, the traces may be heated by an electron beam of similar power and focal region.
[0039] The heating performed at 556 melts the consumable form of the second metal to form a molten form of the second metal. offer The second metal may be bonded to the interface layer by a molten form of the second metal. The molten form of the second metal may include, for example, molten metal particles or molten metal wires. In this manner, heating may cause a portion of the interface layer to melt into the molten form of the second metal. Similarly, heating may cause a portion of the molten form of the second metal to melt into the interface layer. Note that in some implementations, the terms "fuse," "fused," "fusion," and the like may refer to the localized melting (i.e., transition to a liquid state) of the consumable form of the second metal. In other implementations, the terms may refer to a softening or sintering action that does not itself form a liquid, but nevertheless facilitates mass transfer from one metal layer to another.
[0040] In some implementations, the heating performed at 556 can also serve to bond the interface layer to the substrate, thereby causing a portion of the interface layer to melt into the substrate and / or a portion of the substrate to melt into the interface layer. This configuration is useful because it simplifies the additive manufacturing method. Nevertheless, it is not always necessary or desirable to bond the substrate, the interface layer, and the molten form of the second metal simultaneously. Thus, in other examples, the interface layer may be bonded to the substrate prior to adding the molten form of the second metal.
[0041] Thus, in optional step 558, the interface layer may be pre-welded to the substrate within the non-reactive environment of the additive manufacturing apparatus. This optional step may be performed prior to providing a consumable form of the second metal to the track. In embodiments that include step 558, the pre-welding may cause a portion of the interface layer to dissolve into the substrate. Similarly, the pre-welding may cause a portion of the substrate to dissolve into the interface layer.
[0042] At 560, a subsequent layer of the molten form of the second metal is added to the already formed molten layer of the second metal. This step can be repeated any number of times until the desired article is constructed based on the topology of the article defined in the digital model.
[0043] At 562, the article is removed from the additive manufacturing apparatus and annealed under controlled temperature conditions for a suitable period of time. Annealing can help reduce the density of defect sites within the additively manufactured article, thereby increasing the strength of the article. The annealing process can also reduce residual stresses imparted to the article by the joining of dissimilar metals.
[0044] FIG. 6 illustrates an embodiment of an exemplary article 610 that may be formed according to the method 500 of FIG. 5. The article 610 includes a substrate 612 of a first metal bonded to a printed structure 614 of a second metal. As described above, the first metal may include one of steel and titanium, and the second metal may include the other of steel and titanium. The printed structure 614 of the second metal is formed by melting a consumable form of the second metal and is simultaneously bonded to the substrate through a partially melted layer of a third metal 622. The third metal may include any metal that can form an alloy with the first metal and can form an alloy with the second metal. In some examples, the third metal may exhibit a lattice spacing intermediate between that of steel and that of titanium. In some examples, the third metal does not form a stable intermetallic compound with either steel or titanium. In some examples, the third metal may include one or more of vanadium, niobium, and tantalum.
[0045] 6, the third metal 622 at least permeates the substrate 612. In some examples, the third metal 622 can also permeate the printed structure 614. Similarly, both the first metal from the substrate and the second metal from the molten metal particulate can permeate the boundary layer of the third metal. In some examples, the substrate can comprise a gear shaft and the printed structure can comprise a sprocket.
[0046] Neither the method embodiment of FIG. 5 nor the article embodiment of FIG. 6 should be construed in a limiting sense, as numerous variations, extensions, and omissions are contemplated. For example, the object used as a substrate in the additive manufacturing method of FIG. 5 may itself be a product of prior additive manufacturing. In some examples, such objects may include a single metal. In other examples, the object may include dissimilar metals that are bonded via an interface layer, as described herein. Thus, all portions of the article formed according to the method of FIG. 5 may be derived from additive manufacturing, in some examples.
[0047] 6-9 show analytical data collected on an article additively manufactured according to the method of FIG. 5. More specifically, the article was formed by additively adding Maraging M300 alloy steel metal particulate onto a "buttered" Ti 6AL-4V substrate. The interface layer attached to the substrate was 0.012 inch thick niobium foil. The niobium foil was pre-welded to the substrate (step 558 of FIG. 5) using an additive manufacturing apparatus similar to apparatus 300 of FIG. 3, with metal particulate delivery interrupted during pre-welding. A laser irradiance of 1500 W was applied to the substrate to produce a thickness of approximately 4 mm. 2 The laser was focused to a spot size of 0.0001 mm and translated at a speed of 39.4 inches per minute with a line length of 1.0 inches under an argon flow of 120 liters per minute (L / M). A single pass along this line was used for prewelding.
[0048] Following pre-weld, the laser power was increased to 1800 W and Maraging M300 alloy steel metal particulate was delivered at a flow rate of 25 g / min. The laser spot was translated 2 degrees at a speed of 39.4 in / min for the same 1.0 in line length, also under an argon flow of 120 L / M.
[0049] The articles thus formed were cleaved using a diamond saw in a plane parallel to the direction of material addition, also parallel to the direction of laser spot movement. The cleaved facets were sealed in Bakelite, ground using 320 grit sandpaper, and polished using diamond paste. All of the analyses reported here were performed on the polished cleaved facets.
[0050] FIG. 7 shows a series of images of the same region of the cleaved facet. Image 764 is a high magnification optical microscope image provided for reference, which shows titanium layer 766, niobium layer 768, and steel layer 770. The other images in FIG. 7 are energy dispersive X-ray (EDX) emission maps recorded over the same region of the cleaved facet during exposure to Mo Kα radiation. In image 772, the brightness of each pixel corresponds to Ti Kα emission intensity and thus reports on the relative concentration of titanium atoms at the cleaved facet. Similarly, the brightness of image 774 corresponds to Nb Lα emission intensity and reports on the niobium concentration, while the brightness of image 776 corresponds to Fe Kα emission intensity and reports on the iron concentration. These results demonstrate that niobium has significantly infiltrated into titanium layer 766 and steel layer 770. This morphology is more easily seen with reference to the EDX line scan data in FIG. 8.
[0051] FIG. 8 shows EDX line data extracted along two paths extending through the area imaged in FIG. 7. The two paths are substantially parallel to the material addition direction and are offset with respect to each other by a few millimeters. In these graphs, the solid line corresponds to Nb Lα emission intensity, the dashed line corresponds to Ti Kα emission intensity, and the dotted line corresponds to Fe Kα emission intensity. As noted above, niobium has significantly infiltrated both titanium layer 766 and steel layer 770.
[0052] Figure 9 shows the results of a nanoindentation line scan experiment performed on another area of the cleavage plane, also along a path substantially parallel to the material addition direction. In this study, the MTS nanoindenter was operated in CSM test mode with an indentation depth set at 700 nanometers and an indentation spacing set at 50 micrometers. The data shows a relatively gradual transition from the pure titanium phase 766 to the pure steel phase 770.
[0053] Figure 10 is a scanning electron microscope (SEM) image of another portion of the cleaved facet examined in Figures 6, 7, and 8. Prior to examination by SEM, the cleaved facet was chemically etched using Kroll's reagent. In addition to revealing the grain morphology of the steel layer 770, the SEM image shows significant disruption of the initially smooth niobium layer 768, which is consistent with significant mass migration of niobium into the titanium layer 766 and steel layer 770.
[0054] Additional articles were prepared according to the method of FIG. 5 using somewhat different conditions. These articles were also analyzed by electron microscopy, EDX spectroscopy, and nanoindentation as described above. An article prepared as described above, but using a higher laser power of 2000 W for pre-welding and a lower laser power of 1200 W for particulate melting, resulted in a non-uniform bond between the steel and titanium layers compared to the results shown in FIG. 10. EDX analysis of that article revealed significant penetration of niobium into the titanium and steel layers. Another article prepared as described above, using a laser power of 1500 W for pre-welding and particulate melting, and using a niobium foil as thin as 0.007 inches, revealed less intermixing of the metals at the joint. Notably, EDX analysis of that article revealed significant penetration of niobium into the titanium layer, but little or no penetration of niobium into the steel layer.
[0055] Additionally, this disclosure includes examples according to the following clauses:
[0056] Clause 1. A method of additively manufacturing an article 310, 410, 610 comprising a bonded first metal and a second metal, the first metal comprising one of steel and titanium and the second metal comprising the other of steel and titanium, the method comprising the steps of disposing an interface layer 322, 422 of a third metal 622 on a substrate 312, 412, 612 of the first metal, the third metal 622 being capable of forming an alloy with the first metal and capable of forming an alloy with the second metal; providing a consumable form of the second metal at loci 332, 432 of the interface layer 322, 422; and heating the loci 332, 432 of the interface layer 322, 422 in a non-reactive environment 340, 440, the heating step melting the consumable form of the second metal to form a molten form 314, 414 of the second metal. offer and bonding the molten form 314, 414 of the second metal to the interface layer 322, 422.
[0057] Clause 2. The method of clause 1, wherein the interface layer 322, 422 comprises one or more of vanadium, niobium, and tantalum.
[0058] Clause 3. The method of clause 1, wherein heating the locus 332, 432 of the interface layer 322, 422 causes dissolution of a portion of the interface layer 322, 422 into the molten form 314, 414 of the second metal.
[0059] Clause 4. The method of clause 1, wherein heating the loci 332, 432 of the interface layer 322, 422 bonds the interface layer 322, 422 to the substrate 312, 412, 612 and causes dissolution of a portion of the interface layer 322, 422 into the substrate 312, 412, 612.
[0060] Clause 5. The method of clause 1, further comprising the step of pre-welding the interface layer 322, 422 to the substrate 312, 412, 612 in a non-reactive environment 340, 440 prior to providing a consumable form of the second metal to the locus 332, 432, wherein the pre-welding step causes dissolution of a portion of the interface layer 322, 422 into the substrate 312, 412, 612.
[0061] Clause 6. The method of clause 1, wherein the non-reactive environment 440 comprises an environment of flowing argon.
[0062] Clause 7. The method of clause 1, wherein the step of heating the loci 332, 432 of the interface layer 322, 422 includes heating with a laser beam.
[0063] Clause 8. The method of clause 7, wherein the laser beam delivers 1.5 to 2.0 kilowatts at a focus of the laser beam.
[0064] Clause 9. The method of clause 1, wherein the step of heating the loci 332, 432 of the interface layer 322, 422 includes heating with an electron beam.
[0065] Clause 10. The method of clause 1, wherein the interface layer 422 comprises a foil.
[0066] Clause 11. The method of clause 1, wherein the steel comprises an alloy steel and the titanium comprises, by mass, about 6% aluminum and 4% vanadium.
[0067] Clause 12. The method of clause 1, wherein the consumable form of the second metal comprises particulate 326 and the molten form 414 of the second metal comprises molten particulate.
[0068] Clause 13. The method of clause 1, wherein the consumable form of the second metal comprises a wire 490.
[0069] Clause 14. The method of clause 1, further comprising annealing the article 310, 410, 610.
[0070] Clause 15. An article 310, 410, 610 comprising a substrate 312, 412, 612 of a first metal and a printed structure 614 of a second metal formed by melting a consumable form of the second metal and simultaneously bonded to the substrate 612 through a partially melted layer of a third metal 622, wherein the third metal 622 at least infiltrates the substrate 612, and wherein the first metal comprises one of steel and titanium and the second metal comprises the other of steel and titanium.
[0071] Clause 16. The article (310, 410, 610) of clause 15, wherein the third metal (622) comprises one or more of vanadium, niobium, and tantalum.
[0072] Clause 17. The article (310, 410, 610) of clause 15, wherein the third metal (622) also infiltrates the printed structure.
[0073] Clause 18. The article (310, 410, 610) described in clause 15, wherein the substrate (612) comprises a gear shaft (212) and the printing structure comprises a sprocket (214).
[0074] Clause 19. A method 500 for additively manufacturing an article 310, 410, 610 comprising a bonded first metal and a second metal, the first metal comprising one of steel and titanium and the second metal comprising another of steel and titanium, the method comprising the steps of disposing a niobium layer 768 on a substrate 312, 412, 612 of the first metal; providing a consumable form of the second metal to a locus 332, 432 of the niobium layer 768; and heating the locus 332, 432 of the niobium layer 768 in a non-reactive environment 340, 440, wherein the heating melts the consumable form of the second metal to form a molten form 314, 414 of the second metal. offer and bonding the molten form 314, 414 of the second metal to the niobium layer 768.
[0075] Clause 20. The method of clause 19, wherein heating the locus of the niobium layer causes dissolution of a portion of the niobium layer into the molten form of the second metal.
[0076] Clause 21. The method of clause 19, wherein heating the traces of the niobium layer bonds the niobium layer to the substrate and causes dissolution of a portion of the niobium layer into the substrate.
[0077] Clause 22. The method 500 of clause 19, further comprising the step of pre-welding the niobium layer 768 to the substrate 312, 412, 612 in a non-reactive environment 340, 440 prior to providing a consumable form of the second metal to the locus 332, 432, wherein the pre-welding causes dissolution of a portion of the niobium layer 768 into the substrate 312, 412, 612.
[0078] Clause 23. The method 500 of clause 19, wherein the step of heating the tracks 332, 432 of the niobium layer 768 includes heating with one or both of a laser beam and an electron beam.
[0079] Clause 24. The method 500 of clause 19, wherein the consumable form of the second metal comprises particulate 326 and the molten form 314, 414 of the second metal comprises molten particulate.
[0080] Clause 25. The method 500 of clause 19, wherein the consumable form of the second metal comprises a wire 490.
[0081] Clause 26. The method of clause 19, wherein the niobium layer comprises a foil having a thickness of 0.01 to 0.10 inches.
[0082] The present disclosure is presented by way of example with reference to the accompanying drawings. Components, method steps, and other elements that may be substantially the same in one or more of the drawings are identified in a coordinated manner and described with minimal repetition. It should be noted, however, that the elements identified in a coordinated manner may differ to some degree. It should also be noted that the drawings are schematic and generally not drawn to scale. Rather, the scales, aspect ratios, and number of components of the various figures shown in the drawings may be intentionally distorted to more easily view certain features or relationships.
[0083] It should be understood that the configurations and / or techniques described herein are exemplary in nature, and that these specific embodiments or examples are not to be considered in a limiting sense, as many variations are possible. The specific routines or processes described herein may represent one or more of any number of processing strategies. Thus, the various operations shown and / or described may be performed in the sequence shown and / or described, or in other sequences, in parallel, or may be omitted. Similarly, the order of the processes described above may be changed.
[0084] The subject matter of the present disclosure includes all novel and non-obvious combinations and subcombinations of the various methods, systems, and structures disclosed herein with other features, functions, operations, and / or properties, and all equivalents thereof. [Explanation of symbols]
[0085] 200 manufactured products 202 Torso 204 Wing Section 206 Tail Section 208 Control Surfaces 210 Gears 212 Shafts, gear shafts, titanium alloy shafts 214 Sprocket 300 equipment 310 Goods 312 Substrate 314 Melting Form 316 Chamber 320 Rotating Chuck 322 Interface layer 324 Metal fine particle reservoir 326 Metal fine particles, fine particles 328 Metallic particle pump 330 Nozzle 332 Trajectory 334 Energy Beam Source 336 Energy Beam 340 Non-reactive Environment 342 Translation Stage 344 Computer 346 Digital Model 400 equipment 410 Goods 412 Substrate 414 Melting Form 416 Chamber 420 Rotating Chuck 422 Interface layer 430 Nozzle 432 Trajectory 434 Energy Beam Source 436 Electron Beam 440 Non-reactive environment 442 Translation Stage 444 Computer 446 Digital Model 490 Wire, Metal Wire 492 Metal Wire Spool 494 Wire feeder, metal wire feeder 500 ways 610 Goods 612 Substrate 614 Printing structure 622 The third metal 764 images 766 Titanium layer, pure titanium phase 7 768 Niobium layer 770 Steel layer, pure steel phase 772 images 774 images 776 images
Claims
1. 1. A method of additively manufacturing an article (310, 410, 610) comprising bonded first and second metals, wherein the first metal comprises one of steel and titanium and the second metal comprises the other of the steel and the titanium, the method comprising: disposing an interface layer (322, 422) of a third metal (622) on the substrate (312, 412, 612) of the first metal, the third metal (622) being capable of forming an alloy with the first metal and capable of forming an alloy with the second metal; providing a consumable form of said second metal to the loci (332, 432) of said interface layer (322, 422); heating the trace (332, 432) of the interface layer (322, 422) in a non-reactive environment (340, 440), wherein the heating melts the consumable form of the second metal to provide a molten form (314, 414) of the second metal, bonds the molten form (314, 414) of the second metal to the interface layer (322, 422), bonds the interface layer (322, 422) to the substrate (312, 412, 612), and causes dissolution of a portion of the interface layer (322, 422) into the substrate (312, 412, 612); Including, The method of claim 1, wherein the third metal (622) comprises niobium.
2. The method of claim 1 , wherein heating the locus (332, 432) of the interface layer (322, 422) causes dissolution of a portion of the interface layer (322, 422) into the molten form (314, 414) of the second metal.
3. 2. The method of claim 1, further comprising the step of pre-welding the interface layer (322, 422) to the substrate (312, 412, 612) in the non-reactive environment (340, 440) prior to providing the consumable form of the second metal to the track (332, 432), the pre-welding causing dissolution of a portion of the interface layer (322, 422) into the substrate (312, 412, 612).
4. The method of claim 1 , wherein heating the loci (332, 432) of the interface layer (322, 422) comprises heating with one of a laser beam and an electron beam.
5. The method of claim 1 , wherein the interface layer (422) comprises a foil.
6. The method of claim 1 , wherein the consumable form of the second metal comprises particulate (326) and the molten form of the second metal comprises molten particulate (414).
7. A first metal substrate (312, 412, 612); a printed structure (614) of a second metal formed by melting of a consumable form of a second metal and simultaneously bonded to the substrate (612) through a partially melted layer of a third metal (622), the third metal (622) infiltrating at least the substrate (612), the first metal comprising one of steel and titanium, and the second metal comprising the other of the steel and titanium; Equipped with The article (310, 410, 610), wherein the third metal (622) comprises niobium.
8. The article (310, 410, 610) of claim 7, wherein the third metal (622) also infiltrates the printed structure.
Citation Information
Patent Citations
Method of cladding titanium on carbon steel
JP1997174255A
Method of manufacturing metals and Launching apparatus comprising metal accessories generated using the method
KR101981625B1
Joining metallurgically incompatible metals
US20180161931A1