Aluminum alloy bare material and brazing sheet with excellent thermal conductivity

The aluminum alloy composition with optimized Fe, Si, and Cu additions, along with controlled particle distribution, addresses the trade-off in thermal conductivity and strength in automotive heat exchangers, achieving high electrical conductivity and structural integrity for improved heat exchanger performance.

JP7596100B2Active Publication Date: 2024-12-09MA ALUMINUM CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020151160
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-09
Publication Date
2024-12-09
Estimated Expiration
2040-09-09

AI Technical Summary

Technical Problem

Existing aluminum alloys used in automotive heat exchangers face a trade-off between high thermal conductivity and structural strength due to the addition of Mn, which reduces electrical conductivity, and 1000 series alloys lack sufficient strength for heat exchanger structures.

Method used

An aluminum alloy composition with controlled additions of Fe, Si, and Cu, optimized for particle size and distribution, achieves high electrical conductivity and structural strength by incorporating Al-Fe or Al-Fe-Si compounds, with a balanced composition of Fe: 0.6-0.8%, Si: 0.1-0.7%, Cu: 0.05-0.6%, and limited Mn: 0.2% or less, along with a brazing sheet design that maintains these properties.

Benefits of technology

The solution provides an aluminum alloy and brazing sheet with electrical conductivity of 55% IACS or more, equivalent to Al-Mn alloys, while ensuring structural integrity and corrosion resistance, suitable for high-performance heat exchangers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596100000005
    Figure 0007596100000005
  • Figure 0007596100000006
    Figure 0007596100000006
  • Figure 0007596100000007
    Figure 0007596100000007
Patent Text Reader

Abstract

To provide a bare material having high strength and high electric conductivity, and a brazing sheet.SOLUTION: An aluminum alloy bare material contains, in mass%, Fe: 0.6% to 0.8%, Si: 0.7% or less, and Cu: 0.6% or less, with the contents of Mn and Zn controlled to 0.2% or less and 0.3% or less respectively, and the balance being Al and unavoidable impurities. The electric conductivity is 55%IACS or more. The number of Al-Fe compound particles or Al-Fe-Si compound particles with a circle equivalent diameter of 0.5-2.0 μm, distributed in a matrix, is 0.1×104-4.0×104 / mm2.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum alloy bare material and a brazing sheet having excellent thermal conductivity. [Background technology]

[0002] In recent years, new heat exchangers for automobiles, such as inverter coolers, are being installed in automobiles due to the trend toward electric vehicles. Inverter coolers are required to have improved heat dissipation performance in order to reduce size and weight by saving space. For example, in inverter coolers that have a structure with high component bonding density, the higher the thermal conductivity of the aluminum material used in the components, the better the heat dissipation performance of the inverter cooler. Aluminum alloys used in automotive heat exchangers are generally Al-Mn alloys because of their strength and corrosion resistance. However, Mn added to Al alloys significantly reduces electrical conductivity when dissolved in the Al matrix. The thermal conductivity and electrical conductivity of Al are proportional, and a decrease in electrical conductivity leads to a decrease in thermal conductivity. Therefore, automotive heat exchangers using Al alloys with added Mn, which has poor electrical conductivity, have limited heat dissipation performance. On the other hand, 1000 series alloys that do not contain Mn have high electrical conductivity, but their strength is low as a component of automotive heat exchangers and they cannot maintain the structural strength of the heat exchanger. For this reason, in order to improve the heat dissipation performance while ensuring the structural strength and corrosion resistance of automotive heat exchangers, it is necessary to ensure strength and improve thermal conductivity by using aluminum alloys other than Al-Mn alloys.

[0003] An aluminum alloy material having a composition of 2.0 to 3.0 mass% Fe, 0.5 to 1.5 mass% Si, 0.05 mass% or less Ti, and the balance being Al and unavoidable impurities, is known as an aluminum alloy material that exhibits high strength and high thermal conductivity (see Patent Document 1). In addition, an aluminum alloy fin material for heat exchangers is provided, which is composed of 0.010 to 0.4 mass% Fe, less than 0.005 mass% Cu, the balance being Al and impurities, has an Al purity of 99.30 mass% or more, has an average grain size of subgrains of 2.5 μm or less, and has an intermetallic compound content of 2000 particles / mm2 with a maximum length exceeding 3 μm. 2 The following aluminum fin material is known (see Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2002-256365 A [Patent Document 2] JP 2014-074198 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, with the demand for further miniaturization and high heat dissipation performance of heat exchangers, high electrical conductivity (= high thermal conductivity) of aluminum alloys is required, so the present inventors have been developing materials for Al alloys of a different system from Al-Mn alloys. As a result of studying a composition system in which Fe, Si, and Cu are added to Al in connection with this material development, the present inventors have dramatically improved electrical conductivity compared to Al-Mn alloys by adding Fe and Si, which are hardly dissolved in the aluminum base material, and by taking a step of optimizing the particle size and density of Al-Fe or Al-Fe-Si compounds present in the Al matrix. In addition, they have found that it is possible to obtain strength equivalent to that of Al-Mn alloys by adding Cu, which does not affect the distribution state of these compounds, and have arrived at the present invention.

[0006] The present invention has been made in view of the above background, and has an object to provide an aluminum alloy and an aluminum alloy brazing sheet which have strength equivalent to that of Al-Mn alloys and can obtain high electrical conductivity. [Means for solving the problem]

[0007] (1) The aluminum alloy bare material of this embodiment contains, by mass%, Fe: 0.6 to 0.8%, Si: 0.1~ 0.7 %、 Cu: 0.05~ 0.6 % The matrix contains Mn: 0.2% or less, Zn: 0.3% or less, and the balance is Al and unavoidable impurities. The matrix has an electrical conductivity of 55% IACS or more, and the number of Al-Fe compound particles or Al-Fe-Si compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is ​​0.1×10 4 ~4.0×10 4 pieces / mm 2 It is characterized in that: (2) The aluminum alloy bare material of this form is The number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having an equivalent circle diameter of 0.5 to 2.0 μm is preferably 0.35×10 4 ~2.58×10 4 particles / mm 2 . (3) In the aluminum alloy bearing material of this embodiment, after applying a heat treatment equivalent to brazing of a heat exchanger in which it is heated to 600°C and held for 5 minutes, and then cooled to 300°C at 60 to 100°C / min, it has an electric conductivity of 50% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having an equivalent circle diameter of 0.5 to 2.0 μm distributed in the matrix is 0.12×10 4 ~2.42×10 4 particles / mm 2 is preferably the case. (4) The aluminum alloy bare material according to this embodiment is preferably used for a heat exchanger.

[0008] ( 5 The aluminum alloy brazing sheet for heat exchangers of this embodiment is: (1) Any one of ~(3) described This product is characterized in that the core material is an aluminum alloy bare material, and an aluminum alloy layer containing 3.0 to 12.0% by mass of Si as a brazing material, with the remainder being Al and unavoidable impurities, is bonded to one or both surfaces of the core material. ( 6 In the aluminum alloy brazing sheet for heat exchangers of this embodiment, the brazing filler metal preferably further contains, by mass %, Zn: 0.1 to 4.0%. ( 7 ) This embodiment ( 5 )or( 6The aluminum alloy brazing sheet for heat exchangers described in ) has an electrical conductivity of 53% IACS or more, and the number of Al-Fe compound particles or Al-Fe-Si compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix of the core material is 0.1 × 10 4 ~4.0×10 4 pieces / mm 2 It is preferable that:

[0009] ( 8 ) This embodiment (7) In the aluminum alloy brazing sheet for heat exchangers according to the present invention, The number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having an equivalent circle diameter of 0.5 to 2.0 μm is preferably 0.35×10 4 ~2.58×10 4 particles / mm 2 . (9) This embodiment relates to 5 )~( 7 In the aluminum alloy brazing sheet for heat exchangers according to any one of the preceding claims, Heated to 600°C and held for 5 minutes, cooled to 300°C at 60 to 100°C / min After heat treatment equivalent to brazing a heat exchanger is applied, the number of Al-Fe compound particles or Al-Fe-Si compound particles having an electrical conductivity of 45% IACS or more and having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the matrix is 0.12 ×10 4 ~ 2.42 ×10 4 pieces / mm 2 It is preferable that: (10) The aluminum alloy brazing sheet for a heat exchanger according to any one of (6) to (9) according to this embodiment is the above-mentioned The pitting potential difference between the core material and the brazing material surface after the heat treatment equivalent to that of heat exchanger brazing is 80 to 204 mV It is preferable that: Effect of the Invention

[0010] The present invention can provide an aluminum alloy bare material or an aluminum alloy brazing sheet having high electrical conductivity and sufficient strength to maintain the structure of a heat exchanger. The aluminum alloy bare material or brazing sheet of the present invention has excellent electrical conductivity while having the strength to maintain the structure of a heat exchanger, and can therefore be applied as an aluminum alloy bare material and brazing sheet suitable for use in automotive heat exchangers, which have been required to be further miniaturized and have high heat dissipation performance in recent years. [Brief description of the drawings]

[0011]

Figure 1

Figure 2

Figure 3

Figure 4

Figure 5

[0012] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. Note that the drawings used in the following description may show characteristic portions in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand.

[0013] FIG. 1 shows an example of an aluminum alloy bare material according to the present invention, and FIG. 2 shows a cross-sectional structure of an aluminum alloy brazing sheet of a first embodiment having a core material with the same composition as the aluminum alloy bare material shown in FIG. The aluminum alloy brazing sheet A of this embodiment is in the form of a plate or sheet, and has a three-layer structure in which a first brazing material layer 2 is laminated on both the upper and lower sides of a core material 1 having the same composition as the aluminum alloy bare material M shown in Fig. 1. The brazing material layer 2 may be laminated on only one side of the core material 1 as in other embodiments described later. The aluminum alloy and aluminum alloy brazing sheet of this embodiment are preferably used for heat exchangers.

[0014] "Aluminum alloy bare material and core material" The aluminum alloy bare material M and the core material 1 are made of an aluminum alloy containing, by mass%, Fe: 0.6-0.8%, Si: 0.7% or less, Cu: 0.6% or less, Mn: 0.2% or less, Zn: 0.3% or less, and the balance being Al and unavoidable impurities. In addition, when the range of mass% is expressed using "~", the lower and upper limits are included unless otherwise specified. For example, 0.6-0.8% means that the content is 0.6 mass% or more and 0.8 mass% or less. As an example, the aluminum alloy bare material M can be rolled into a plate shape as shown in Fig. 1 and used as a fin for a heat exchanger, or the aluminum alloy bare material M and a double-sided clad material can be processed into a cup shape and used as a component to be brazed by stacking them alternately. One example of the use of the aluminum alloy bare material M of this embodiment is the brazing sheet A shown in Fig. 2, which uses the same composition for the core material 1, but it goes without saying that it can also be used for other purposes.

[0015] The reasons for limiting the composition of the component elements contained in the aluminum alloy constituting the bare material M and the core material 1 will be explained below. Fe: 0.6 to 0.8% Fe is added to Al to precipitate Al-Fe or Al-Fe-Si compound particles in the aluminum alloy matrix and improve the material strength by particle dispersion strengthening. If the Fe content is below the lower limit, the desired dispersion state (required number per unit area) of Al-Fe compound particles or Al-Fe-Si compound particles cannot be obtained. If the Fe content exceeds the upper limit, the distribution number of Al-Fe compound particles or Al-Fe-Si compound particles increases, which is undesirable because it promotes wear and deterioration of the mold during punching. Si: 0.7% or less Silicon improves the strength of aluminum by dissolving in aluminum or by precipitating in the aluminum alloy matrix as particles of compounds such as Al-Fe and Al-Fe-Si. If the silicon content exceeds the upper limit, the silicon solubility increases and the electrical conductivity after brazing decreases. If the silicon content exceeds the upper limit, the melting point of the aluminum alloy decreases, which is undesirable because the bare material and the core material melt during brazing and the shape of the heat exchanger cannot be maintained.

[0016] Cu: 0.6% or less Cu is added to dissolve in Al to improve the material strength of Al. If the Cu content exceeds the upper limit, the Cu solubility increases and the electrical conductivity after brazing decreases. If the Cu content exceeds the upper limit, a large amount of Cu precipitates on the bare material or the core surface of the brazing sheet during corrosion, reducing the self-corrosion resistance. In addition, the diffusion of Cu from the core to the brazing sheet becomes significant, increasing the electric potential of the brazing material, and the electric potential difference between the core and brazing material decreases, which may reduce the sacrificial corrosion protection effect of the brazing material on the core material. Mn: 0.2% or less It is difficult to completely eliminate Mn from the aluminum alloy when manufacturing it, so it is necessary to add a small amount for manufacturing reasons. Even if a small amount of Mn is added, it significantly reduces the electrical conductivity when it dissolves in Al. However, if the Mn content is 0.2% or less, the amount of Mn dissolved in Al can be minimized by carrying out a predetermined homogenization treatment, thereby suppressing the reduction in electrical conductivity. The Mn content is preferably 0.1% or less. Zn: 0.3% or less Zn is an element that contributes to ensuring corrosion resistance, and if the Zn content exceeds 0.3%, the self-corrosion resistance of the bare material and the core material decreases. The Zn content is more preferably 0.2% or less.

[0017] "Brazing material" The reasons for limiting the composition of the component elements contained in the brazing material 2 will be explained below. Si: 3.0-12.0% Silicon is added to form a molten braze during brazing and to form a fillet at the joint. If the Si content is below the lower limit, the molten brazing filler metal will be insufficient, resulting in poor brazing joinability, whereas if the Si content is above the upper limit, the molten brazing filler metal generated during brazing will be excessive, causing the core material 1 or the brazing target material to melt violently, making it impossible to maintain the shape of the heat exchanger, resulting in poor performance and impaired appearance. Zn: 0.1-4.0% Zn is added to the brazing filler metal to protect the core material from sacrificial corrosion. If more than 4.0% Zn is added, the corrosion rate increases too much, causing the brazing filler metal to corrode early, resulting in a decrease in corrosion resistance as the core material cannot be protected from corrosion.

[0018] "Particle size of Al-Fe compound particles or Al-Fe-Si compound particles" 0.5~2.0μm If the particle size (circle equivalent diameter) of the compound particles is less than 0.5 μm, the compound will be redissolved in the matrix during brazing, and the electrical conductivity of the material after brazing will decrease. If the particle size exceeds 2.0 μm, effective particle dispersion strengthening cannot be obtained, and the material strength will decrease, so the structural strength as a heat exchanger cannot be maintained. In addition, if there are many compounds larger than 2.0 μm, it is undesirable because it promotes wear and deterioration of the mold during processing. The particle size of the compound particles is affected by the homogenization temperature, homogenization time, etc., and tends to be less than 0.5 μm when the homogenization temperature is low and the homogenization time is short. The particle size of the compound particles exceeds 2.0 μm when the homogenization temperature is high and the homogenization time is long.

[0019] "Number of Al-Fe compound particles or Al-Fe-Si compound particles" 0.1×10 4 ~4.0×10 4 pieces / mm 2 When the amount of element added to the material is large, the number of compound particles is 0.1×10 4 If the amount of the added element is less than 1, the added element will be in a state of almost solid solution in the matrix, and the electrical conductivity will be significantly reduced. Conversely, if the amount of the added element is small, the degree of solid solution will be low and the electrical conductivity will be high, but since the number of compound particles is small, the desired particle dispersion strengthening cannot be obtained, and the material strength will be low, and the structural strength required for the heat exchanger will not be maintained. The number of compound particles is 4.0×10 4 If the number exceeds 1, the Al-Fe compound particles have high hardness, which undesirably promotes wear and deterioration of the die when processing the material.

[0020] "Manufacturing method" For example, aluminum alloys for bare materials, core materials, and brazing materials are cast by semi-continuous casting. An aluminum alloy for bare material and core material can be made with a composition containing, by mass%, Fe: 0.6-0.8%, Si: 0.7% or less, Cu: 0.6% or less, Mn: 0.2% or less, Zn: 0.3% or less, with the remainder being Al and unavoidable impurities. This aluminum alloy can be used to manufacture bare material and brazing sheet core material. The aluminum alloy for brazing material contains, by mass %, 3.0 to 12.0% Si, and may further contain 0.1 to 4.0% Zn as necessary, with the remainder being Al and unavoidable impurities.

[0021] "Homogenization treatment" The obtained bare material and aluminum alloy for core material can be subjected to homogenization treatment at 400 to 600°C for a treatment time of 3 to 12 hours. By selecting the appropriate temperature and time, it is possible to obtain the desired properties of high electrical conductivity and optimal dispersion of the compounds in the matrix.

[0022] The brazing material can be subjected to homogenization treatment at a temperature of 400° C. to 500° C. for a treatment time of 1 to 10 hours, but it is not necessary to perform the homogenization treatment.

[0023] "Pasting" When used as a brazing sheet, it can be produced by combining brazing material on one or both sides of a sheet-shaped or plate-shaped core material with a cladding ratio of brazing material:core material=5-15%:85-95%. In the case of both sides, it can be produced by combining with a cladding ratio of skin material:core material:skin material=5-15%:70-90%:5-15%. There is no particular restriction on the preparation of the brazing material, and it can be produced based on the conditions for preparing brazing material when producing a general brazing sheet. After homogenization, the surface is ground, rolled to the desired plate thickness by hot rolling, cut to a specified length, and the core material and brazing material are bonded together to obtain a brazing sheet.

[0024] "Hot rolling, cold rolling, annealing" The aluminum alloy for bare material and the material obtained by combining the core material and the skin material can be manufactured by hot rolling (or clad rolling) using a hot rolling mill. After the hot rolling, cold rolling can be performed to a predetermined thickness. At this time, annealing may be performed during the cold rolling to continue the rolling. The thickness of the final material is not limited, but the reduction ratio from the thickness finished by hot rolling and the thickness annealed for continuing the rolling to the final thickness is preferably 20 to 99%. In addition, annealing may be performed after cold rolling to achieve O temper. Annealing may be performed by performing heat treatment at 200°C to 500°C for 1 to 10 hours using, for example, a batch annealing furnace.

[0025] The aluminum alloy bare material M or the brazing sheet A manufactured according to the steps described above is used for the purpose of brazing by placing it in an inert gas atmosphere for about 1 to 30 minutes at a brazing temperature in the range of, for example, about 590 to 620°C when manufacturing a heat exchanger or the like. For example, it is used in assembling heat exchangers by laminating it with brazing target components such as fins and tubes of various heat exchangers or cup-shaped bodies, and after assembling the fins, tubes or cup-shaped bodies, the whole is heated to the brazing temperature to melt the brazing material 2 of the aluminum alloy brazing sheet A, and then cooled to room temperature to complete the brazing. Alternatively, components such as fins and tubes of a heat exchanger can be directly formed from the brazing sheet and used for brazing. The workpiece to be brazed may be a bare aluminum alloy material M shown in FIG.

[0026] FIG. 3 shows a brazing sheet B obtained by cladding and rolling a brazing material 2 on only one side of a core material 1, and FIG. 4 is an explanatory diagram showing the state in which this brazing sheet B is used to braze a brazing target member 3 such as a fin. Brazing is completed by brazing the brazing sheet B and the brazing target member 3 shown in FIG. 4 under the brazing conditions described above. The aluminum alloy bare material M or the brazing sheets A and B have excellent high electrical conductivity and strength sufficient to maintain the structure of a heat exchanger, and therefore can be provided as a brazing sheet suitable for use in automotive heat exchangers, which have been required to be further miniaturized and have high heat dissipation performance in recent years.

[0027] 5 shows an aluminum heat exchanger 5 in which fins 6 are formed using the brazing sheet A or brazing sheet B, and an aluminum alloy tube 7 is used as the brazing target component. The fins 6 and tubes 7 are assembled with a reinforcing material 8 and a header plate 9, and then brazed to obtain the aluminum heat exchanger 5 for automotive use, etc. The brazing sheets A and B have high electrical conductivity and strength sufficient to maintain the structure of a heat exchanger, and therefore can be used in automotive heat exchangers, which have been required to be further miniaturized and have high heat dissipation performance in recent years, and can provide automotive heat exchangers, which are being further miniaturized and have high heat dissipation performance.

[0028] The brazing sheet can be used for various component applications such as heat exchanger components, such as tubes, header pipes, etc., in addition to the application of forming fins of heat exchangers. In such cases, various laminated structures can be adopted depending on the application, such as a single-sided brazing material type, a double-sided brazing material type, and a multi-layer structure formed by combining with a sacrificial material or an intermediate material. EXAMPLES

[0029] Aluminum alloys having the compositions shown in Tables 1 and 2 were produced by semi-continuous casting. The resulting aluminum alloy ingots were subjected to homogenization annealing under the conditions shown in Tables 1 and 2. After that, they were hot-rolled and then cold-rolled to 1.0 mm with a rolling reduction of 85%, and annealed at 350°C for 5 hours to prepare bare material samples.

[0030] Additionally, sample brazing sheets were prepared by bonding aluminum alloys having the compositions shown in Tables 1 and 2 as core materials in combination with the brazing filler metals shown in Tables 3 and 4. The brazing filler metal was bonded to one side with a cladding ratio of 10%. After bonding, the sheets were hot-rolled and then cold-rolled to 1.0 mm with a rolling reduction of 85%, and annealed at 350°C for 5 hours to prepare the samples.

[0031] "Heat treatment equivalent to brazing" Since it is difficult to directly evaluate the above-mentioned aluminum alloy bare material and brazing sheet material used in the brazed heat exchanger, the aluminum alloy bare material and brazing sheet material alone were subjected to a brazing-equivalent heat treatment in a batch furnace. The conditions of the brazing-equivalent heat treatment were not limited to the conditions in this example, but the material was heated from room temperature to 600°C, held at 600°C for 5 minutes, and cooled to 300°C at 60 to 100°C / min. After reaching 300°C, the material was quickly cooled to room temperature using a fan or the like. The obtained aluminum alloy bare material and brazing sheet were subjected to the evaluation described below.

[0032] "Evaluation Method" <Electrical conductivity> The measurement was performed by a four-terminal method. A current of 500 mA was applied to the sample in a room temperature environment of 20 to 25° C., and the resistance was calculated from the voltage value, and then the electrical conductivity was calculated. <Observation of compound particle distribution> The cross sections parallel to the rolling direction were observed for the manufactured aluminum alloy bare material and brazing sheet core material, and for the aluminum alloy bare material and brazing sheet core material that had been subjected to heat treatment equivalent to brazing. The observation was performed using a field emission scanning electron microscope (FE-SEM) on the cross sections that had been subjected to CP processing based on the ion milling method. The circle equivalent diameter and distribution density of the compound particles were calculated by image analysis based on the observed images. It has been confirmed that the structure of each sample contains some compound particles with a circle-equivalent diameter of less than 0.5 μm or more than 2.0 μm, but the distribution density of these particles is smaller than that of compound particles with a circle-equivalent diameter of 0.5 to 2.0 μm. In this example, the homogenization temperature and homogenization time are selected to precipitate a large number of compound particles with a circle-equivalent diameter of 0.5 to 2.0 μm.

[0033] <Electrochemical polarization measurement> A 2.67% AlCl3 aqueous solution that had been thoroughly degassed with high-purity N2 gas and an electrochemical measurement cell were used, Pt was used as the working counter electrode, and the Luggin capillary and reference electrode Ag / AgCl were bypassed. The liquid temperature during the measurement was kept at 40°C. The measurement area of ​​the brazing material surface and core material of the sample that was subjected to heat treatment equivalent to brazing was 10 mm 2 The test area was exposed to light, and the rest was masked with insulating paint. As pretreatment for the measurement area, it was immersed in 5% NaOH at 50°C for 30 seconds, washed with water, and then immersed in 30% HNO3 at room temperature for 1 minute and washed with water. After holding the specimen at the natural potential for about 5 minutes, the potential was swept from the natural potential at a rate of 0.5 mV / s. The bending point (the region where the current suddenly stops flowing (passivation region) and the region where the current suddenly starts flowing) observed after a constant sweep of the polarization curve was determined as the pitting potential. In addition, since no bending point was observed in specimens containing a large amount of Zn, a bending potential of 0.1 mA / cm was used. 2 The potential was determined as the pitting potential.

[0034] Regarding the brazing material potential, a brazing sheet was prepared, brazed, and then 10 mm 2 The rest was masked and measurements were taken. The core potential was measured by measuring the core potential on the opposite side of the brazing material of the single-sided brazing material. 2 The rest were masked and measurements were taken. When measuring the core potential of double-sided brazing material, immerse the brazed material in 5% NaOH at 50°C to expose the core, then immerse it in 30% HNO3 at room temperature for 1 minute and measure the core potential of the material by 10 mm on the desmutted surface. 2 The rest were masked and measurements were taken.

[0035] Tables 1 and 2 show the composition of the bare aluminum alloy material used in the evaluation of each test, the results of measuring the electrical conductivity before and after brazing, and the results of measuring the number of compound particles.

[0036] Tables 3 and 4 show the composition of the brazing sheets used in the evaluation of each test, the results of measuring the electrical conductivity before and after brazing, the results of measuring the number of compound particles, the potential of the core material and the brazing material, and the potential difference.

[0037] [Table 1]

[0038] [Table 2]

[0039] [Table 3]

[0040] [Table 4]

[0041] The aluminum alloy bare materials of alloy Nos. A1 to A22 shown in Table 1 contain, in mass%, Fe: 0.6 to 0.8%, Si: 0.7% or less, Cu: 0.6% or less, with the balance being Al and unavoidable impurities, or, in addition to this composition, if Mn and Zn are added, the Mn content is restricted to 0.2% or less and the Zn content to 0.3% or less. In addition, in each column of Table 1, "-" indicates that the corresponding component is not contained (less than the measurement limit).

[0042] The aluminum alloy bare materials of Alloy Nos. A1 to A22 showed excellent electrical conductivity of 55% IACS or more (55 to 64% IACS) before brazing and 50% IACS or more (50 to 64% IACS) after brazing. The bare aluminum alloys of alloy No. A1 to A22 had a compound particle count of 0.1×10 4 ~4.0×10 4 pieces / mm 2 Range (0.4~2.6×10 4 pieces / mm 2 ), and the number of compound particles after brazing is less than 0.1×10 4 ~4.0×10 4 pieces / mm 2 Range (0.1~2.4×10 4 pieces / mm 2 ) was shown.

[0043] The brazing sheets No. B1 to B40 shown in Tables 3 and 4 showed excellent electrical conductivity of 55% IACS or more (55 to 63% IACS) before brazing and 45% IACS or more (48 to 59% IACS) after brazing. For brazing sheets No. B1 to B40, the number of compound particles before brazing was 0.1 × 10 4 ~4.0×10 4 pieces / mm 2 Range (0.3~2.6×10 4 pieces / mm 2 ), and the number of compound particles after brazing is less than 0.1×10 4 ~4.0×10 4 pieces / mm 2 Range (0.1~2.4×10 4 pieces / mm 2 ) was shown.

[0044] In contrast to these Examples, the alloy No. A23 sample in Table 2, which shows a comparative example, had a low Fe content and therefore reduced strength, and the alloy No. A24 sample had a large amount of Al-Fe compound particles, which led to increased die wear and reduced productivity. The alloy No. A25 sample, which shows a comparative example, is a sample with a higher Si content than the preferred range, and the alloy No. A26 sample is a sample with a higher Cu content than the preferred range, but both samples had electrical conductivity below 50% IACS after brazing. The sample of alloy No. A27, which is a comparative example, is a sample in which the contents of Mn and Zn are higher than the preferred range. Although the number of compounds is large due to the addition of Mn, the sample has electrical conductivity below 50% IACS before and after brazing. The alloy Nos. A28 and A29 samples had a small number of compound precipitates and thus had low electrical conductivity, while the No. A30 sample had a high homogenization temperature, which resulted in an increase in particles larger than 2.0 μm and a decrease in strength.

[0045] Nos. B1 to B40 shown in Tables 3 and 4 are brazing sheet samples using core materials that have an aluminum alloy composition containing, by mass, 0.7% Fe, 0.2% Si, and 0.5% Cu, with the balance being Al and unavoidable impurities, and have been subjected to homogenization annealing for 3 to 12 hours at temperatures of 400 to 600°C as shown in Table 1. These aluminum alloy brazing sheets have high electrical conductivity before and after brazing, and the number of compound particles is within a preferable range.

[0046] The brazing sheets of Comparative Example Nos. B41 to B44 shown in Table 4 use Comparative Example alloys Nos. A23 to A26, and therefore show the same tendency as in the case of alloys Nos. A23 to A26.

[0047] In the examples shown in Tables 3 and 4, some samples can achieve a potential difference of 80 mV or more. When the potential difference is 80 mV or more, the sacrificial corrosion protection effect (corrosion resistance) of the core material by the brazing material is further improved. When the potential difference is 80 mV or less, the sacrificial corrosion protection effect may not be sufficient, and the corrosion of the core material may be accelerated. The fact that the corrosion resistance is improved when the potential difference is 80 mV or more was confirmed by the corrosion test described below.

[0048] For the corrosion test, the brazing material and the core material were overlapped to prepare a test sample so that the core material was exposed after brazing, and the test sample was immersed in OY water. The composition of OY water is 195 ppm Cl. - , 60 ppm SO4 2- , 1ppmCu 2+ , 30 ppm Fe 3+ It is an aqueous solution containing The test cycle consisted of 8 hours at 88°C, followed by 16 hours at room temperature. The corrosive solution was stirred using a magnetic stirrer while heating to 88°C. The specific liquid volume was 16.7ml / cm 2 The sample size was adjusted so that the potential difference was 80 mV or more. After four weeks of OY water testing, the core material had 0.1 pits / mm2 or less in depth. 2 The number of defects was less than 100, and the corrosion resistance was good.

[0049] The potential difference becomes less than 80 mV because (1) the amount of Cu added to the core material increases, causing Cu to concentrate in the brazing filler metal during brazing, thereby reducing the potential difference between the core material and the brazing filler metal, and (2) the amount of Zn in the brazing filler metal decreases, thereby reducing the potential difference. [Explanation of symbols]

[0050] A, B...aluminum alloy brazing sheet, M...aluminum alloy bare material, 1...core material, 2...filler material, 3...part to be brazed (fin), 5...heat exchanger, 6...fin, 7...tube.

Claims

1. The composition contains, by mass%, Fe: 0.6-0.8%, Si: 0.1-0.7%, Cu: 0.05-0.6%, Mn: 0.2% or less, Zn: 0.3% or less, and the balance being Al and unavoidable impurities. The composition has an electrical conductivity of 55% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5-2.0 μm distributed in the matrix is ​​0.1×10 4 ~4.0 x 10 4 pieces / mm 2 1. An aluminum alloy bare material comprising:

2. The aluminum alloy bare material according to claim 1, characterized in that the number of Al-Fe compound particles or Al-Fe-Si compound particles having an equivalent circle diameter of 0.5 to 2.0 μm is 0.35×10 4 to 2.58×10 4 particles / mm 2 .

3. After subjecting a heat treatment equivalent to brazing a heat exchanger, which involves heating to 600°C, holding for 5 minutes, and cooling to 300°C at 60 to 100°C / min, the material has an electrical conductivity of 50% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in a matrix is ​​0.12 × 10 4 ~2.42 x 10 4 pieces / mm 2 2. The aluminum alloy bare material according to claim 1,

4. The aluminum alloy bare material according to any one of claims 1 to 3, which is used for a heat exchanger.

5. 4. An aluminum alloy brazing sheet for heat exchangers, comprising a core material made of the aluminum alloy bare material according to claim 1, and an aluminum alloy layer containing, as a brazing material, 3.0 to 12.0% by mass of Si, with the remainder being Al and unavoidable impurities, laminated on one or both surfaces of the core material.

6. The aluminum alloy brazing sheet for heat exchangers according to claim 5, characterized in that the brazing material further contains, by mass%, Zn: 0.1 to 4.0%.

7. The core material has an electrical conductivity of 53% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in the core material matrix is ​​0.1×10 4 ~4.0 x 10 4 pieces / mm 2 7. The aluminum alloy brazing sheet for heat exchangers according to claim 5 or 6, 8. The aluminum alloy brazing sheet for heat exchangers according to claim 7, characterized in that the number of Al-Fe based compound particles or Al-Fe-Si based compound particles having an equivalent circle diameter of 0.5 to 2.0 μm is 0.35×10 4 to 2.58×10 4 particles / mm 2 .

9. After subjecting a heat treatment equivalent to brazing a heat exchanger, which comprises heating to 600°C, holding for 5 minutes, and cooling to 300°C at 60 to 100°C / min, the material has an electrical conductivity of 45% IACS or more, and the number of Al-Fe-based compound particles or Al-Fe-Si-based compound particles having a circle equivalent diameter of 0.5 to 2.0 μm distributed in a matrix is ​​0.12 × 10 4 ~2.42 x 10 4 pieces / mm 2 The aluminum alloy brazing sheet for heat exchangers according to any one of claims 5 to 7, characterized in that

10. An aluminum alloy brazing sheet for heat exchangers as described in any one of claims 6 to 9, characterized in that the pitting potential difference between the core material and the brazing material surface after the heat treatment equivalent to heat exchanger brazing is 80 to 204 mV.

Citation Information

Patent Citations

  • Aluminum alloy fin material for heat exchanger

    JP1990133540A

  • Manufacture of aluminum alloy fin material for heat exchanger

    JP1990133553A

  • Aluminum alloy brazing sheet excellent in strength and corrosion resistance for heat exchanger

    JP2002030367A

  • High strength and high thermal conduction aluminum alloy material, material fin for heat exchanger and method for producing the aluminum alloy material

    JP2002256365A

  • Fin material for air-conditioning heat exchanger and air-conditioning heat exchanger

    JP2013204076A