Manufacturing method of epoxy resin composition, liquid ejection head using the epoxy resin composition, and manufacturing method of the liquid ejection head
Patent Information
- Application Number
- JP2020182573
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-17
- Filing Date
- 2020-10-30
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2040-10-30
AI Technical Summary
【0008】 1液で十分な可使時間があり、短時間での加熱硬化性に優れ、接着信頼性の高い接着剤として有用なエポキシ樹脂組成物が得られる。
Smart Images

Figure 0007596118000007 
Figure 0007596118000008 
Figure 0007596118000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an epoxy resin composition, a liquid ejection head using the epoxy resin composition, and a method for producing the liquid ejection head. [Background technology]
[0002] Epoxy adhesives are widely used due to their high adhesiveness and chemical resistance. In particular, when joining precision parts, they must be able to harden in a short time (also called temporary fixing) to prevent misalignment. A representative example of an epoxy adhesive having such characteristics is a photocationic polymerization type epoxy resin adhesive. This adhesive is suitable for industrial use because it is a single liquid with a long pot life and hardens with heating for a few seconds. For example, the adhesive can be stably applied to the adherend because there is little change in physical properties such as viscosity at room temperature. In addition, after application, UV irradiation is performed, the adherend is laminated, and the adhesive is hardened by heating at 100°C for a few seconds, so there is little positional deviation and there is no need to hold the adherend for a long time, allowing for quick transfer to the next process. Additional heating can be performed as necessary to further increase the crosslink density and improve mechanical properties and chemical resistance. In this way, two-stage curing improves productivity and reliability.
[0003] Photo-cationically polymerized epoxy resins have excellent chemical resistance because ether bonds are formed by opening the epoxy rings. However, the number of functional groups that contribute to adhesion, such as hydroxyl groups, decreases as the ether bonds are formed, and the adhesiveness may be insufficient. Among the epoxy resin polymerization reactions, thiol curing, which uses polythiol as a curing agent, is one that has a fast reaction rate. Polythiol is an anionic polymerization that reacts with epoxy resin at high speed in the presence of a basic catalyst or curing accelerator. The adhesive described in Patent Document 1 is known as an adhesive that uses this thiol curing. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2016 / 171072 Summary of the Invention [Problem to be solved by the invention]
[0005] Although thiol curing is extremely reactive, it has a short pot life, such as curing in the syringe while being applied to multiple adherends, and some kind of ingenuity is required for practical use. In such thiol curing, a method of selecting a solid basic catalyst or curing accelerator is one way to extend the pot life. For example, if a solid basic compound is used for thiol curing, the time until it dissolves and becomes a basic catalyst can be saved. However, along with the epoxy resin, which is the main agent, the polythiol curing agent is usually liquid. In particular, solid basic compounds are easily dissolved in relatively low-viscosity polythiols, and even if the start of the reaction can be delayed slightly, the pot life may still be insufficient. In addition, even if the pot life is successfully extended by reducing the amount of basic compounds, the curing property of short-term heating may be poor, and the temporary fixing property may not be sufficient. If the adhesive is made into a two-part instead of a one-part to solve the pot life problem, it is necessary to knead it every time, fill it into a syringe, and set it in the device, which significantly reduces productivity. Furthermore, since the reaction continues after kneading, the pot life is short, resulting in even lower productivity.
[0006] An object of the present invention is to provide an epoxy resin composition that has a sufficient pot life as a single liquid and is curable by short-term heating. The present invention also provides a liquid ejection head using the epoxy resin composition, and a method for producing the liquid ejection head. [Means for solving the problem]
[0007] The present invention, which achieves the above object, An epoxy resin, a solid basic compound, and a polythiol, A method for producing an epoxy resin composition comprising: The epoxy resin and the solid basic compoundand kneading the mixture 1 with the polythiol to produce a mixture 2. death, The polythiol is a polythiol having an ether skeleton. The present invention relates to a method for producing an epoxy resin composition comprising the steps of: The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: An epoxy resin, a thixotropic agent, a solid basic compound, and a polythiol, The method for producing an epoxy resin composition comprising the steps of: kneading the epoxy resin and the thixotropic agent to produce a mixture 3; kneading the solid basic compound into the mixture 3 to produce a mixture 4; and kneading the polythiol into the mixture 4 to produce a mixture 5. Yes , The polythiol is a polythiol having an ether skeleton. The present invention relates to a method for producing an epoxy resin composition comprising the steps of: Furthermore, the present invention provides a method for producing a An epoxy resin, a thixotropic agent, a solid basic compound, and a polythiol, A method for producing an epoxy resin composition comprising: The epoxy resin and the solid basic compound and kneading the above to produce a mixture 1. The polythiol and the thixotropic agent A step of kneading to produce a mixture 6, and Mixture 6 and kneading the above to produce a mixture 7, The polythiol is a polythiol having an ether skeleton. The present invention relates to a method for producing an epoxy resin composition comprising the steps of: or, An epoxy resin, a thixotropic agent, a solid basic compound, and a polythiol, A method for producing an epoxy resin composition comprising: The epoxy resin and The thixotropic agent A step of producing a mixture 3 by kneading the above; Mixture 3 To The solid basic compound A step of kneading to produce a mixture 4; The polythiol and The thixotropic agent and kneading the mixture 4 to produce a mixture 6. Mixture 6 and kneading the mixture to produce a mixture 8. The polythiol is a polythiol having an ether skeleton. The present invention relates to a method for producing an epoxy resin composition comprising the steps of: By using any of the above-mentioned manufacturing methods, a one-liquid epoxy resin composition can be obtained, which is an epoxy resin comprising at least an epoxy resin, a solid basic compound, and a polythiol, and in which the content of the solid basic compound is 3 to 10 parts by mass per 100 parts by mass of the epoxy resin. In addition, the present invention relates to a method for manufacturing a liquid ejection head having a recording element substrate that ejects ink, a support member that supports the recording element substrate and has a supply flow path that supplies ink to the recording element substrate, and a flow path member that supplies ink to the supply flow path, the method comprising the steps of: producing an adhesive by the above-described method for producing an epoxy resin composition; and applying the adhesive to at least one bonding surface between any two of the recording element substrate, the support member, and the flow path member to bond the two members together. Effect of the Invention
[0008] The resulting epoxy resin composition is useful as an adhesive with sufficient pot life and excellent heat curing properties in a short time, and has high adhesive reliability. [Brief description of the drawings]
[0009] [Figure 1] FIG. [Diagram 2] FIG. 1 is a schematic cross-sectional view of an inkjet head. [Diagram 3] FIG. 1 is a schematic diagram showing a state when adhesive strength is measured by the butting method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention provides an epoxy resin composition (adhesive) containing an epoxy resin, a solid basic compound, and a polythiol. However, since solid basic compounds are easily dissolved in polythiols having a relatively low viscosity, and the solid basic compounds are coordinated to the polythiols when dissolved, and the epoxy resins and the polythiols react with each other very quickly. Therefore, it was thought that a sufficient pot life could not be obtained even if such solid basic compounds were used as catalysts.
[0011] However, according to the study of the present inventors, it was found that the dissolution of the solid basic compound in a relatively low-viscosity polythiol can be suppressed by wrapping the surface of the solid basic compound with an epoxy resin. The solid basic compound wrapped in the epoxy resin dissolves in the polythiol and becomes a basic catalyst, and it takes time for the epoxy resin and the polythiol to start reacting. Therefore, even at room temperature, the viscosity rise is slow in one liquid, and sufficient working time can be obtained. Furthermore, since the working time can be sufficiently secured by wrapping the surface of the solid basic compound with an epoxy resin, the solid basic compound can be blended in an amount that was not possible before, and the reaction initiation points increase, so that curing can be achieved by heating for an even shorter time. In this way, although it is a one-liquid, sufficient working time and curing in a short time are both achieved. In particular, in a system to which a thixotropic agent is added, it can be applied and adhered without spreading due to the expression of thixotropy, and therefore has excellent applicability to fine parts. In addition, the viscosity of the epoxy resin and / or polythiol can be increased with the thixotropic agent, so that the dissolution of the solid basic compound in the polythiol can be further suppressed, and the working time can be longer.
[0012] The adhesive obtained by the method of the present invention is a basic thiol curing adhesive, and therefore is less susceptible to the reduction of functional groups that contribute to adhesion, such as hydroxyl groups, due to the curing reaction, and has excellent adhesive properties. For this reason, a manufacturing method of an adhesive according to one embodiment of the present invention is characterized by preparing a mixture 1 by kneading an epoxy resin and a solid basic compound, and then kneading a polythiol into the mixture 1. By going through this process, the solid basic compound is covered with the epoxy resin, so that dissolution contact of the solid basic compound with the polythiol can be suppressed, and the adhesive of the present invention has a slow viscosity increase even at room temperature as a single liquid, and a sufficient pot life can be obtained for the adhesive of the present invention.
[0013] In another embodiment of the adhesive manufacturing method of the present invention, the step of kneading the epoxy resin and / or polythiol with a thixotropic agent in advance can further suppress dissolution and contact of the solid basic compound with the polythiol. As a result, the pot life of the one-liquid can be further ensured. This thixotropic agent allows a larger amount of the solid basic compound to be blended, and the thiol curing property of the epoxy, which is originally highly reactive, can be further improved. Although it is a one-liquid, it can be cured at a temperature of about 100°C in a few seconds and can exhibit excellent temporary bonding properties. At the same time, an adhesive with sufficient pot life can be obtained.
[0014] The adhesive of the present invention is thiol curing (anionic polymerization reaction), and functional groups such as hydroxyl groups that contribute to adhesion remain even after curing, and the thiol-derived -S- has flexibility, so that strong adhesion to the adherend can be expected even in harsh environments. For example, it can be applied to an adhesive that bonds parts of a liquid ejection head, such as an inkjet head. The ink used in an inkjet head is composed of a polar solvent, water, and a coloring material, and an adhesive that bonds the parts that come into contact with the ink is required to maintain a strong adhesive force. Furthermore, in order to prevent different colors from mixing between the separated liquid flow paths, it is desired to maintain a strong adhesive force at the interface between the adherend and the adhesive. This is because if a gap is formed at the interface between the adherend and the adhesive, the ink will enter the gap from the liquid flow paths of each color due to capillary force, increasing the possibility that different colors will mix.
[0015] In addition, in the manufacturing process of inkjet heads, small parts are fixed with adhesive so that they do not move, and then the process of attaching the next part is repeated, and finally the adhesive is cured over a relatively long period of time. The process of fixing the parts with adhesive so that they do not move is called temporary fixing, and the process of curing the adhesive over a relatively long period of time is called full curing. For example, temporary fixing is performed at 100°C for a few seconds, and finally full curing is performed at 150°C for two hours. The adhesive of the present invention is suitable for the temporary fixing process of inkjet heads because it cures in a few seconds at a temperature of about 100°C.
[0016] Each component will be described below. (Epoxy resin) The epoxy resin as the main component may be one type or may contain two or more types. Since it is necessary to cover the solid basic compound as a catalyst, the epoxy resin composition needs to be in a liquid state in the step of kneading the solid basic compound. When using an epoxy resin that is solid at room temperature, it is preferable to heat the epoxy resin to a temperature at which the solid basic compound does not melt, to make it liquid, or to dissolve the solid basic compound in another liquid epoxy resin.
[0017] Examples of epoxy resins include bisphenol A type, bisphenol F type, and bisphenol AD type epoxy resins, as well as glycidyl ethers of compounds obtained by further adding alkylene oxide to these, epoxy novolac resins, glycidyl ether type and glycidyl amine type epoxy resins such as bisphenol A novolac diglycidyl ether and bisphenol F novolac diglycidyl ether, alicyclic epoxy resins, etc. Examples of epoxy resins that are solid at room temperature include epoxy resins having a biphenyl skeleton, a naphthalene skeleton, a cresol novolac skeleton, a trisphenolmethane skeleton, a dicyclopentadiene skeleton, a phenolbiphenylene skeleton, etc.
[0018] (Polythiol) The polythiol used as the curing agent is not particularly limited, but usually, a polythiol having high reactivity and a relatively low molecular weight is selected. Such polythiols are often liquid at room temperature. Examples include pentaerythritol trispropanethiol (PEPT), trimethylolpropane tris(3-mercaptopropionate) (TMMP), pentaerythritol tetrakis(3-mercaptopropionate), and p-xylene dithiol. Commercially available products include PEPT (manufactured by SC Organic Chemicals), TMMP (manufactured by SC Organic Chemicals), Cupcure 3-800 (trade name, manufactured by Mitsubishi Chemical Corporation), and QX11 (trade name, manufactured by Mitsubishi Chemical Corporation). When the adhesive of the present invention is used in a portion requiring higher chemical resistance, a polythiol having an ether skeleton, which has higher chemical resistance, is preferred. A polythiol having an ether skeleton refers to a compound having two or more thiol groups in the side chain, not containing a hydrolyzable ester bond in the main chain, and having an ether bond that has high bonding strength and therefore has excellent properties such as chemical resistance.
[0019] The content of polythiol is preferably an amount in which the thiol equivalent of polythiol is 0.5 to 1 equivalent per 1 equivalent of epoxy resin. When the amount of polythiol is small relative to the epoxy resin, the reaction rate of epoxy resin and polythiol decreases, so the reaction slows down as a whole system, and curing in a short time may not be expected. In addition, when the equivalent of polythiol is small, the polymerization reaction between epoxy resin and polythiol may not be the main reaction, but the polymerization reaction between epoxy resin and base derived from solid basic compound may become the main reaction. Therefore, the flexibility of the thioether structure (-S-) derived from polythiol decreases, which is not preferable from the viewpoint of adhesion. When the equivalent of polythiol is too large relative to epoxy resin, the amount of polythiol that cannot react with epoxy resin increases. Unreacted polythiol remains as a plasticizer, and mechanical properties such as a decrease in adhesive strength may deteriorate. Furthermore, when an adhesive is used in a portion that comes into contact with ink, unreacted polythiol may dissolve into the ink, and ink may invade the space left by the dissolved polythiol, causing the adhesive to swell with the ink, which is undesirable.
[0020] (Solid basic compounds) There are no particular limitations on the solid basic compound that is the curing catalyst as long as it is solid at room temperature, but it is preferable to use one that is difficult to dissolve in epoxy resins. For example, examples of latent curing agents that are generally used include dicyandiamide, dihydrazide compounds, solid aromatic amines such as diaminodiphenylmethane (DDM) and diaminodiphenylsulfone (DDS), various imidazoles, and various amine adduct-based latent curing agents.
[0021] The content of the solid basic compound is preferably 3 to 10 parts by mass relative to 100 parts by mass of the epoxy resin. If the amount of the solid basic compound relative to the epoxy resin is too small, curing in a short time is not expected. If the amount of the solid basic compound relative to the epoxy resin is too large, the amount of the solid basic compound that is protected by the epoxy resin but dissolves in the polythiol increases, shortening the pot life. In particular, the production method of the present invention makes it possible to add a large amount of the solid basic compound, such as 3 to 10 parts by mass, relative to 100 parts by mass of the epoxy resin while maintaining a sufficient pot life.
[0022] (thixotropic agent) For the purpose of reducing the fluidity of the liquid component and further suppressing the dissolution of the solid basic compound in the polythiol, a thixotropic agent may be added to the epoxy resin composition (adhesive) as a component other than the above-mentioned epoxy resin, solid basic compound, and polythiol.
[0023] As the thixotropic agent, inorganic fine particles such as general fumed silica can be used. There are also liquid types that can impart thixotropy without increasing the viscosity too much, but in this case, other fillers such as glass, titanium oxide, alumina, aluminum hydroxide, magnesium hydroxide, talc, mica, and silica are required. As the liquid type, polyamide-based, ester-based, hydrogenated castor oil-based, polyethylene oxide-based, surfactant-based, and the like can be used. These may be used alone or in combination of two or more.
[0024] The content of the thixotropic agent is preferably 1 to 20 parts by mass per 100 parts by mass of the epoxy resin. The more the thixotropic agent, the longer the pot life tends to be. Therefore, it is advisable to adjust the amount of the thixotropic agent according to the desired pot life. The method of mixing the thixotropic agent will be described later.
[0025] (Method of producing epoxy resin composition) In the method for producing the epoxy resin composition (adhesive) according to the present invention, the raw materials of the adhesive are mixed in the following order for the purpose of suppressing dissolution of the solid basic compound in the polythiol.
[0026] (Adhesive that does not contain thixotropic agents) The adhesive manufacturing method according to this embodiment includes a step of manufacturing a mixture 1 by kneading an epoxy resin and a solid basic compound, and a step of kneading a polythiol into the mixture 1 to manufacture a mixture 2. Compared to a case where an epoxy resin, a solid basic compound, and a polythiol are kneaded all at once without taking the above-mentioned order, the adhesive kneaded in the above order does not increase in viscosity easily even when stored at room temperature, and has a sufficient pot life. Since the adhesive kneaded in the above order has a sufficient pot life, it is possible to add an amount of solid basic compound that would not be possible with an adhesive kneaded all at once, and it is expected to harden in a short time.
[0027] (Adhesives containing thixotropic agents) In addition, the adhesive containing a thixotropic agent can be manufactured in the following order of steps: First, a step of kneading an epoxy resin and a thixotropic agent to manufacture a mixture 3; a step of kneading the mixture 3 with a solid basic compound to produce a mixture 4; A step of kneading the mixture 4 with a polythiol to produce a mixture 5. The adhesive mixed in this order had a longer pot life. Alternatively, a manufacturing method may include a step of preparing mixture 1 by kneading an epoxy resin and a solid basic compound, a step of kneading a polythiol and a thixotropic agent to prepare mixture 6, and a step of kneading mixture 1 and mixture 6 to prepare mixture 7. In this case, the viscosity of the polythiol is increased by the thixotropic agent, and the contact between the solid basic compound coated with the epoxy resin and the polythiol is further suppressed. Alternatively, a method may be used in which mixture 4 is prepared and mixture 4 and mixture 6 are kneaded to prepare mixture 8. In this case, a larger amount of thixotropic agent can be kneaded, and the pot life can be further extended.
[0028] (Silane coupling agent) A silane coupling agent may further be added to the adhesive of the present invention. Silane coupling agents that have an epoxy group, a mercapto group, an isocyanate group, or a fluorene skeleton can be used. However, since silane coupling agents are low-viscosity liquids, it is not appropriate to use basic silane coupling agents such as amine compounds, because they act as catalysts and immediately start a reaction, shortening the usable time.
[0029] When the adhesive of the present invention is used in a situation where stronger adhesion is required at the interface between the adherend and the adhesive, the silane coupling agent is preferably one having an epoxy group or a mercapto group. Since the base agent is an epoxy resin and the curing agent is a polythiol, it is believed that the compatibility with these silane coupling agents is good and peeling at the interface between the adherend and the adhesive is unlikely to occur. The order of mixing the silane coupling agents is not particularly limited, but it is preferable to mix the epoxy group-containing silane coupling agent and the mercapto group-containing silane coupling agent together at the same time as the polythiol.
[0030] (Other Ingredients) The resin composition containing the above components may optionally contain diluents and other additives that are commonly used in epoxy adhesives, such as fillers, which may be added as needed.
[0031] (Inkjet head) The epoxy resin composition of the present invention can be suitably used as an adhesive for bonding components of an inkjet head. Fig. 1 is a perspective view showing one embodiment of an inkjet head, and Fig. 2 is a schematic cross-sectional view showing one embodiment of an inkjet head. The inkjet head 1 includes a recording element substrate 2 that ejects ink, a support member 4 that supports the recording element substrate 2 and has a supply flow path 3 that supplies ink to the recording element substrate, and a flow path member 5 that supplies ink to the supply flow path 3. The flow path member 5 may be composed of a plurality of parts. For example, as shown in FIG.
[0032] In the manufacturing process of an inkjet head, two components such as each flow path member must be bonded together with high accuracy, so they may be assembled using the following procedure. An adhesive is applied to the support member 4, and the recording element substrate is temporarily attached for a short period of time, and then the adhesive is fully cured. The third flow path member 8 and the second flow path member 7 are bonded together, and the first flow path member 6 is then bonded to the second flow path member 7 to create the flow path member 5. Next, the support member 4 and the first flow path member 6 of the flow path member 5 are temporarily bonded together. Finally, the adhesive is fully cured.
[0033] The epoxy resin composition of the present invention has a sufficient pot life after being prepared as a one-part solution, and further has excellent temporary bonding properties, and therefore can be suitably used as an adhesive, particularly for the bonding surface between the support member 4 and the first flow path member 6. It can be suitably used for at least one bonding surface between two members, such as the bonding surface between the first flow path member 6 and the second flow path member 7, or the bonding surface between the second flow path member 7 and the third flow path member 8. Of course, it can also be suitably used for the bonding surface between the support member 4 and the recording element substrate 2. Ceramics such as alumina and resins (engineering plastics) with excellent dimensional accuracy, such as modified polyphenylene ether resin (Zylon (registered trademark), manufactured by Asahi Kasei Corporation, etc.), are used for the support member 4 and the flow path member 5. The adhesive of the present invention is a basic thiol-curing adhesive, and therefore functional groups that contribute to adhesion, such as hydroxyl groups, are relatively not lost during the curing reaction, making it suitable for use as an adhesive for bonding inkjet head components. EXAMPLES
[0034] Next, the method for producing the adhesive of the present invention will be described with reference to examples. (Examples 1 to 13, Comparative Examples 1 to 9) Table 1 shows the composition ratios of the examples, and Table 2 shows the composition ratios of the comparative examples. The mixing method is shown with arrows indicating the mixing order of each mixture. Mixture 1 (base agent + curing catalyst), Mixture 2 (mixture 1 + curing agent), Mixture 3 (base agent + thixotropic agent), Mixture 4 (mixture 3 + curing catalyst), Mixture 5 (mixture 4 + curing agent), Mixture 6 (curing agent + thixotropic agent), Mixture 7 (mixture 1 + mixture 6), Mixture 8 (mixture 4 + mixture 6).
[0035] In Examples 1, 2, and 7, the epoxy resin as the base material and the solid basic compound as the catalyst were kneaded together, and after 12 hours, the polythiol as the curing agent was kneaded together (Mixture 1→2). In Examples 3 to 6 and 8 to 12, the epoxy resin as the base material and the thixotropic agent were kneaded together, then the solid basic compound as the catalyst was kneaded together, and after 12 hours, the polythiol as the curing agent was kneaded together (Mixture 3→4→5). In Example 13, an epoxy resin as a base material and a solid basic compound as a catalyst were kneaded to prepare mixture 1, and a polythiol as a curing agent and a silica filler as a thixotropic agent were separately kneaded to prepare mixture 6. After 12 hours, mixture 1 and mixture 6 were kneaded together (mixture 1 → 6 → 7). In order to mix the thixotropic agent with the epoxy resin as the main agent, there is a limit in consideration of the subsequent mixing of the solid basic compound as the catalyst. In Example 14, 100 parts by mass of the epoxy resin as the main agent was mixed with 10 parts by mass of the silica filler as the thixotropic agent to prepare a mixture 3, and then a solid basic compound as the catalyst was mixed to prepare a mixture 4. Separately from this, 6.6 parts by mass of the silica filler as the thixotropic agent was mixed with 66 parts by mass of the polythiol as the curing agent to prepare a mixture 6. After 12 hours, the mixture 4 and the mixture 6 were mixed to prepare a mixture 8 (mixture 3 → 4 → 6 → 8). In contrast, in Comparative Examples 1 to 9, all of the materials were kneaded simultaneously.
[0036] The epoxy resin as the base material and the thixotropic agent were mixed in a HIVIS MIX model 3 manufactured by Primix Corporation at 60 rpm for 60 minutes in a vacuum, and materials other than the epoxy resin and the thixotropic agent were mixed at 60 rpm for 5 minutes in a vacuum.
[0037] The time it took for the viscosity to double at room temperature (25°C) was measured and used as the pot life of the adhesive. The gel time when heated to 100°C was measured to evaluate the adhesive's short-term hardening (temporary bonding) ability.
[0038] The judgment was as follows: ◎: Pot life is 8 hours or more and gel time is 3 seconds or less. 〇: Pot life is 3 hours or more and less than 8 hours, and gel time is more than 3 seconds and less than 10 seconds. ×: Pot life is less than 3 hours or gel time is 10 seconds or more.
[0039] In Comparative Examples 1 and 2, a liquid basic compound was used as a catalyst. In Comparative Example 1, the amount of catalyst was small, so the gel time was long. When the amount of catalyst added was increased as in Comparative Example 2, the gel time did not shorten despite the short pot life. It is considered that the liquid basic compound and polythiol are mixed together at the time of kneading the epoxy resin, liquid basic compound, and polythiol, so that both pot life and temporary fixing properties cannot be achieved.
[0040] In Comparative Examples 7 to 9, a solid basic compound was used. In Comparative Example 1 and Comparative Example 9, the time until the viscosity doubled was the same, 14 hours, but the gel time was shorter in Comparative Example 9. By using a solid basic compound instead of a liquid basic compound, both the pot life and temporary fixing properties were somewhat closer. However, the gel time in Comparative Example 9 was 78 seconds, which is long for the temporary fixing process. Although the adhesive had a sufficient pot life, it could not be said to have temporary fixing properties. In order to improve the temporary fixing property of Comparative Example 9, the amount of the solid basic compound was increased in Comparative Examples 6 to 8. The more the amount of the solid basic compound, the shorter the gel time and the improved temporary fixing property. On the other hand, the pot life was shortened. When all materials are mixed at the same time in a resin consisting of an epoxy resin, a polythiol, and a solid basic compound, it is preferable that the amount of the solid basic compound is less than 3 parts by mass, and further 0.5 parts by mass or less, per 100 parts by mass of the epoxy resin in order to obtain a sufficient pot life. When the amount of the solid basic compound is less than 3 parts by mass, the adhesive has a sufficient pot life, but cannot be said to have a temporary fixing property.
[0041] In Example 1 and Comparative Example 3, and Example 2 and Comparative Example 6, the composition was the same, but the manufacturing method was different. As can be seen from the comparison between Example 1 and Comparative Example 3, and Example 2 and Comparative Example 6, the gel time was the same, but the pot life was significantly extended in each of the Examples of the present invention. Since the solid basic compound was covered with the epoxy resin, it was possible to suppress the dissolution of the solid basic compound in the polythiol, and it is considered that the viscosity increase was slow even at room temperature in one liquid, and the pot life was extended. On the other hand, since the composition was the same, the gel time was not changed. By kneading the epoxy resin, which is the main agent, and the solid basic compound, which is the catalyst, to form a mixture, and kneading the mixture with the polythiol, which is the curing agent, an adhesive that has both pot life and temporary fixing properties was obtained.
[0042] As shown in Comparative Examples 6 to 9, when the amount of solid basic compound added as a catalyst is 3 parts by mass or more, the gel time is 10 seconds or less when the curing agent is an ester type curing agent with a relatively slow reactivity. The gel time is shorter as the amount of solid basic compound added is larger. If the amount is more than 10 parts by mass, the viscosity of the adhesive itself increases and the amount of unreacted catalyst also increases, so 3 to 10 parts by mass is preferable. However, in Comparative Examples 6 to 9, the process of covering the solid basic compound with an epoxy resin in advance is not performed, so the pot life is short.
[0043] The influence of the type of solid basic compound used as a catalyst was examined in Examples 3 to 5. Both the pot life and temporary fixing property were achieved for all solid basic compounds. In Examples 5 and 6, the effect of the type of polythiol used as the curing agent was examined. Both the pot life and temporary fixation were compatible for all polythiols. The temporary fixation time was shorter for polythiols with an ether skeleton than for polythiols with an ester skeleton. When temporary fixation in a shorter time is required, highly reactive ether-type polythiols are preferred.
[0044] In Examples 7 to 14, the amount of the thixotropic agent was examined. The pot life was extended up to 1 and 2.5 parts by mass in Examples 8 and 9 compared to no addition (0 parts by mass) in Example 7. The addition of a thixotropic agent to the epoxy resin increases the viscosity of the epoxy resin covering the solid basic compound, and the thixotropy can be increased. As a result, it is believed that the dissolution of the solid basic compound into the polythiol is suppressed, and it takes time for the solid basic compound to become a basic catalyst and initiate a polymerization reaction between the epoxy resin and the polythiol. In Examples 10 to 12, even when the amount exceeds 2.5 parts by mass (up to 5, 10, and 15 parts by mass), the pot life is almost unchanged. It is believed that this is because the effect of suppressing the dissolution of the solid basic compound into the polythiol is saturated. In Example 13, a thixotropic agent was added to the polyol. The pot life was slightly extended compared to the case of no addition in Example 7. It is believed that the addition of a thixotropic agent to the polythiol suppressed the dissolution of the solid basic compound in the polyol. In Example 14, 10 parts by mass of a thixotropic agent was added to the epoxy resin, and 6.6 parts by mass of a thixotropic agent was added to the polythiol. The pot life was further extended by making the content of the thixotropic agent a total of 16.6 parts by mass per 100 parts by mass of the epoxy resin. It is considered that the dissolution of the solid basic compound in the polythiol was further suppressed by adding the thixotropic agent to both the epoxy resin and the polythiol. Although it is possible to achieve both pot life and temporary fixing without adding a thixotropic agent, if a longer pot life is desired, it is preferable to add a thixotropic agent, depending on the type of base agent and curing agent, and it was confirmed that the content is preferably 1 to 20 parts by mass.
[0045] [Table 1]
[0046] [Table 2]
[0047] The abbreviations in the table are as follows. The same applies to the following tables. jER828: Product name, bisphenol A type epoxy resin (epoxy equivalent: 184-194) manufactured by Mitsubishi Chemical Corporation jER152 product name, manufactured by Mitsubishi Chemical Corporation Aerosil 200: Product name "AEROSIL200", manufactured by Nippon Aerosil Co., Ltd. PEPT: Pentaerythritol tripropanethiol (thiol equivalent: approx. 115), manufactured by SC Organic Chemicals TMMP: Trimethylolpropane tris(3-mercaptopropionate) (thiol equivalent: approx. 133), manufactured by SC Organic Chemicals PN23J: Product name "Amicure PN-23J", manufactured by Ajinomoto Fine-Techno Co., Ltd. MY-24: Product name "Amicure MY-24", manufactured by Ajinomoto Fine-Techno Co., Ltd. MY-25: Product name "Amicure MY-25", manufactured by Ajinomoto Fine-Techno Co., Ltd. PN40J: Product name "Amicure PN-40J", manufactured by Ajinomoto Fine-Techno Co., Ltd. 1B2PZ: Product name "Curesol 1B2PZ", manufactured by Shikoku Chemical Industry Co., Ltd.
[0048] (Examples 15 to 27) Tables 3 and 4 show the composition ratios of Examples 15 to 27. The composition ratios of Examples 5 and 6 are also shown. In Examples 15, 17 to 19, mixture 3 was prepared in the same manner as in Example 14, and then a silane coupling agent was added to mixture 3 and kneaded, and then a solid basic compound as a catalyst was added and kneaded to prepare mixture 4. In addition, mixture 6 was prepared by kneading the remaining thixotropic agent into polythiol as a curing agent. After 12 hours, mixture 6 was kneaded into mixture 4 to prepare mixture 8. In Example 16, a mercapto group-containing silane coupling agent was used, so the silane coupling agent was added to mixture 6, but the procedure was the same as in Example 14 to prepare mixture 8. In addition, in Examples 20, 21, and 23 to 27, the mixture 3 was prepared in the same manner as in Example 11, and then a silane coupling agent was added to mixture 3 and kneaded, and then a solid basic compound as a catalyst was added and kneaded to prepare mixture 4. After 12 hours, mixture 4 was kneaded with polythiol as a curing agent to prepare mixture 5. In Example 22, a mercapto-based silane coupling agent was kneaded with polythiol as a curing agent at the stage of preparing mixture 5.
[0049] The epoxy resin as the base material and the thixotropic agent were mixed in a HIVIS MIX model 3 manufactured by Primix Corporation at 60 rpm for 60 minutes in a vacuum, and materials other than the epoxy resin and the thixotropic agent were mixed at 60 rpm for 5 minutes in a vacuum.
[0050] The adhesive was evaluated by the following methods. The pot life and gel time, and whether the adhesive had both properties were evaluated in the same manner as above. In addition, 2 g of the cured product that had been heated at 160° C. for 2 hours was immersed in 20 g of ink (service head ink, manufactured by Canon) and heated for 10 hours at 121° C. The mass of the cured product after immersion was measured, and the mass change rate was calculated by comparing it with the mass before immersion. Furthermore, the components (alumina and alumina) constituting the inkjet head were bonded together with an adhesive and heated at 160°C for two hours. Here, as shown in FIG. 3, alumina plates 21 and 22 bonded together with adhesive 23 were placed on a base 24, and the adhesive strength was measured by abutting the alumina plate 21 with a measuring tool through a hole made in the alumina plate 21. At that time, the state of peeling was also observed. In addition, since accurate peel strength cannot be measured in the case of component destruction, the peel strength was displayed as ND. In addition, the components were bonded together with an adhesive and heated at 160°C for two hours, and then immersed in the above ink and heated at 121°C for 60 hours. After washing with water and drying, the adhesive strength was measured by abutting and the state of peeling was observed.
[0051] How to determine which adhesive is suitable for inkjet heads ◎: Adhesive strength 1.0kgf / mm 2 (9.8N / mm 2 ) does not peel off, but presses further and ends with the component breaking. 〇: Adhesive strength is 1.0kgf / mm 2 (9.8N / mm 2 ) and the interface was peeled off.
[0052] As described above, in Example 5, a polythiol having an ester skeleton (TMMP) was used, and in Example 6, a polythiol having an ether skeleton (PETE) was used. PETE and TMMP have different molecular weights relative to the thiol group, so different parts by mass of each polythiol were kneaded together. When PETE with an ether skeleton was used, the mass change rate was smaller and the adhesive strength after contact with ink was stronger than that of TMMP with an ester skeleton. This is thought to be because, compared to an ester skeleton, an ether skeleton has higher chemical resistance, higher reactivity, and higher crosslink density. Compared to a polythiol having an ester skeleton, a polythiol having an ether skeleton is more preferable as an adhesive for bonding parts of an inkjet head.
[0053] In Examples 15 to 22, the influence of the type of silane coupling agent was examined. All silane coupling agents had both pot life and temporary adhesion, and had sufficient adhesive strength. Among them, when a silane coupling agent containing an epoxy group or a mercapto group was used, the adhesive strength was measured after contact with ink, and the adhesive broke the part rather than peeling at the interface. When bonding the parts of an inkjet head, an adhesive that breaks the part is preferable to an adhesive that breaks at the interface so that different colors do not mix with each other. As an adhesive for bonding the parts of an inkjet head, an adhesive containing an epoxy group or a mercapto group-containing silane coupling agent is more preferable. Since the adhesive contains an epoxy resin as a base agent and a polythiol as a curing agent, it is considered that the silane coupling agent containing an epoxy group or a mercapto group is compatible with the base agent and the curing agent well, and therefore no interfacial peeling occurred.
[0054] In Examples 20, 23 to 25, the amount of polythiol added was examined. At any amount of polythiol, both the pot life and the temporary fixing property were compatible. When the amount of polythiol was reduced, the gel time was extended. In order to maintain the temporary fixing property, the thiol equivalent of the polythiol is preferably 0.5 or more relative to 1 epoxy equivalent of the epoxy resin. When the amount of polythiol was increased, the mass change rate was increased. It is considered that the amount of polythiol that could not react with the epoxy resin increased, the polythiol that could not react was dissolved into the ink, and the ink penetrated into the space where the polythiol had disappeared, resulting in a large mass change. In order not to increase the amount of polythiol that could not react, the thiol equivalent of the polythiol is preferably 1 or less relative to 1 epoxy equivalent of the epoxy resin.
[0055] In Examples 20, 26, and 27, the mixing ratio of two types of epoxy resins was varied. In each ratio, both the pot life and temporary adhesion were achieved. The adhesive was also suitable for bonding parts of an inkjet head.
[0056] [Table 3]
[0057] [Table 4]
[0058] The silane coupling agents in the table are as follows. A-186: Product name "Silquest A-186", manufactured by Momentive Performance Materials Japan, Inc. A-187: Product name "Silquest A-187", manufactured by Momentive Performance Materials Japan, Inc. KBM-803: Trade name, 3-mercaptopropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd. KBE-9007: Product name, 3-isocyanatepropyltriethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd. X-12-1156: Product name, multifunctional mercapto group-type silane coupling agent, manufactured by Shin-Etsu Chemical Co., Ltd. X-12-1159L: Product name, polyfunctional isocyanate-based silane coupling agent, manufactured by Shin-Etsu Chemical Co., Ltd. OCG-157-3: Fluorene-based silane coupling agent, manufactured by Osaka Gas Chemicals Co., Ltd.
[0059] (Example 28) Generally, when the adhesive is a mixture of liquid and solid components, if it is used in a narrow space of several tens of μm between the adherends, the movement of the solid components is restricted by the narrow gap, the components are separated, and bleeding occurs during the curing reaction, resulting in poor curing. In the present invention, the curing catalyst is solid, and there was a concern about bleeding, so the presence or absence of bleeding was confirmed using the following procedure. For the examples of the present invention, lamination was performed using a spacer of a specified size. The presence or absence of bleeding and curing was confirmed by varying the thickness from no spacer, 5, 10, 20, and 30 μm. In both cases, no bleeding was observed, and no uncured components were confirmed. This is because the solid components are catalysts and the reaction proceeds even with a small amount, but in the method of the present invention, a large amount of catalyst is used and the curing agent is polythiol, which is very reactive.
[0060] Due to its reactivity, the adhesive of the present invention is particularly suitable for precision bonding and the like, as it is carried out in two stages: a first thermal curing step for temporary bonding, and a second thermal curing step for full curing which takes longer than the first thermal curing step. For example, an ink supply system may be bonded with alumina to a recording element having an ink flow path and an ejection port on a Si substrate on which an ink ejection pressure generating element and wiring for applying an electric pulse are formed. In such a case, in order to bond the flow paths with high precision, it is necessary to hold the alignment and harden the adhesive. It takes at least about one hour for the adhesive to harden to the point where it can exhibit its ink resistance, and it is extremely difficult to align the adhesive with a jig or the like and hold it in a heat hardening oven. Therefore, if the adhesive of the present invention is used, it can be temporarily fixed by directly applying a heat tool to the Si substrate of the recording element to heat it, and it can be hardened in a few seconds at 100°C. After the temporary fixing, the adhesive has hardened, so that it will not shift even if the jig is removed, and the main curing can be performed in a heat curing oven. The second heat curing, which is the main curing, naturally requires a longer time than the first heat curing, which is the temporary fixing, in order to fully harden the adhesive. The second heat curing is preferably performed at a temperature higher than that of the first heat curing. The curing time and curing temperature may be appropriately selected according to the type and composition ratio of the base agent, curing agent, and solid basic compound to be combined, and other additives. In addition, in particular, if a system is added with a thixotropic agent, the flow of the adhesive into the fine flow paths of the inkjet head can be controlled, and if an ether-type polythiol is used, high ink resistance can be expected, and adhesion reliability can be ensured.
[0061] As shown in Table 5, an adhesive was prepared in the same manner as in Example 21, except that the amount of the solid basic compound PN40J was changed from 5 parts by mass to 3 parts by mass. This adhesive was used to bond two modified polyphenylene ether resin plates (product name "Zylon (registered trademark) L564Z", manufactured by Asahi Kasei Corporation, abbreviation: m-PPE) as parts of an inkjet head. The adhesive was cured at 150°C for 2 hours. When the parts were peeled off using the butting method, the adhesive failed cohesively. The adhesive of the present invention had sufficient adhesion to the m-PPE resin plate.
[0062] [Table 5]
[0063] (Examples 29 to 37) In Examples 29 to 37, thick coating was investigated. If the adherend has unevenness or undulations, if the adhesive is thin, the adhesive will not spread sufficiently and may peel off during use, so it is necessary to apply the adhesive thickly. Therefore, whether the adhesive can be applied thickly was investigated. Table 6 shows the composition ratios of Examples 29 to 37. The composition ratio of Example 16 is also shown. Example 29 was prepared in the same manner as Example 16, except for the addition of fused silica as a filler. As in Example 14, Examples 30 to 35 were prepared by kneading 10 parts by mass of silica filler as a thixotropic agent and an organic thixotropic agent with 100 parts by mass of epoxy resin as a main agent to prepare mixture 3, and then kneading a solid basic compound as a catalyst to prepare mixture 4. Separately from this, mixture 6 was prepared by kneading 6.6 parts by mass of silica filler as a thixotropic agent with 66 parts by mass of polythiol as a curing agent. After 12 hours, mixture 4 and mixture 6 were kneaded to prepare mixture 8 (mixture 3 was used for the organic thixotropic agent mixture).
[0064] In Example 36, 100 parts by mass of epoxy resin as the main component was kneaded with 10 parts by mass of silica filler as a thixotropic agent to prepare mixture 3, and then a solid basic compound as a catalyst was kneaded to prepare mixture 4. Separately, 66 parts by mass of polythiol as a curing agent was kneaded with 6.6 parts by mass of silica filler as a thixotropic agent and an organic thixotropic agent to prepare mixture 6. After 12 hours, mixture 4 and mixture 6 were kneaded to prepare mixture 8. (The organic thixotropic agent was mixed in mixture 6).
[0065] In Example 37, 100 parts by mass of epoxy resin as the main component were mixed with 10 parts by mass of silica filler as a thixotropic agent and 1.5 parts by mass of an organic thixotropic agent to prepare mixture 3, and then a solid basic compound as a catalyst was mixed to prepare mixture 4. Separately, 66 parts by mass of polythiol as a curing agent were mixed with 6.6 parts by mass of silica filler as a thixotropic agent and 1.5 parts by mass of an organic thixotropic agent to prepare mixture 6. After 12 hours, mixture 4 and mixture 6 were mixed to prepare mixture 8. (The organic thixotropic agent mixtures were mixtures 3 and 6).
[0066] The epoxy resin as the base material and the thixotropic agent were mixed in a HIVIS MIX model 3 manufactured by Primix Corporation at 60 rpm for 60 minutes in a vacuum, and materials other than the epoxy resin and the thixotropic agent were mixed at 60 rpm for 5 minutes in a vacuum. The thickness of the adhesive was evaluated as follows. Thixotropy was measured using a viscometer. Specifically, measurements were taken at 10 rpm and 50 rpm, and the thixotropy value was calculated by dividing the viscosity at 10 rpm by the viscosity at 50 rpm. The higher the thixotropy value, the higher the shape retention, and the thicker the adhesive could be applied. Thixotropy was measured every two hours at room temperature, and adhesives with a thixotropy of 3 or more after eight hours were marked with ◎. Those with a thixotropy of less than 3 were marked with 〇. Since it is difficult to apply thickly with a thixotropy of less than 3, the adhesive is limited to thin applications. Furthermore, to confirm whether thick application is possible, it was confirmed whether application to a thickness of 0.7 mm was possible. Application was performed using a 18G needle (inner diameter 0.84 mm), and adhesives with a height of 0.7 mm or more were marked with ◎, and adhesives with a height of less than 0.7 mm were marked with 〇.
[0067] In Example 16, the thixotropy was about 1, and it was not possible to apply the coating more than 0.7 mm thick. Similarly, in Example 29, the composition of Example 16 was filled with silica as a filler to increase the viscosity, but the thixotropy was about 1, and the coating properties were similar to those of Example 16. On the other hand, in Examples 30 to 37, an organic thixotropy agent was used in addition to an inorganic thixotropy agent. By using both, the thixotropy was 3 or more, and coating more than 0.7 mm thick was possible. This is presumed to be because the silica surface of the inorganic thixotropy agent has countless hydroxyl groups, which interact with the functional groups of the organic thixotropy agent to produce a high thixotropy.
[0068] [Table 6]
[0069] The thixotropic agents and fillers in the table are as follows. RHEOCIN, RHEOBYK-430, RHEOBYK-431, RHEOBYK-R606: BYK product names Disparlon 3600N, 3900EF: Product name manufactured by Kusumoto Chemicals Co., Ltd. FB-5D: Denka product name [Explanation of symbols]
[0070] 1 Inkjet head 2. Recording element board 3 Supply Channel 4 Support member 5 Flow path components 6 First flow path member 7 Second flow path member 8 Third flow path member
Claims
1. A method for producing an epoxy resin composition comprising an epoxy resin, a solid basic compound, and a polythiol, comprising the steps of: A step of kneading the epoxy resin and the solid basic compound to produce a mixture 1, and a step of kneading the polythiol into the mixture 1 to produce a mixture 2; having The method for producing an epoxy resin composition, wherein the polythiol is a polythiol having an ether skeleton.
2. A method for producing an epoxy resin composition comprising an epoxy resin, a thixotropic agent, a solid basic compound, and a polythiol, comprising the steps of: A step of producing a mixture 3 by kneading the epoxy resin and the thixotropic agent; kneading the solid basic compound into the mixture 3 to produce a mixture 4; kneading the polythiol into the mixture 4 to produce a mixture 5; having The method for producing an epoxy resin composition, wherein the polythiol is a polythiol having an ether skeleton.
3. A method for producing an epoxy resin composition comprising an epoxy resin, a thixotropic agent, a solid basic compound, and a polythiol, comprising the steps of: a step of kneading the epoxy resin and the solid basic compound to produce a mixture 1; A step of kneading the polythiol and the thixotropic agent to produce a mixture 6; A step of kneading the mixture 1 and the mixture 6 to produce a mixture 7; having The method for producing an epoxy resin composition, wherein the polythiol is a polythiol having an ether skeleton.
4. A method for producing an epoxy resin composition comprising an epoxy resin, a thixotropic agent, a solid basic compound, and a polythiol, comprising the steps of: A step of producing a mixture 3 by kneading the epoxy resin and the thixotropic agent; kneading the solid basic compound into the mixture 3 to produce a mixture 4; A step of kneading the polythiol and the thixotropic agent to produce a mixture 6; A step of kneading the mixture 4 and the mixture 6 to produce a mixture 8; having The method for producing an epoxy resin composition, wherein the polythiol is a polythiol having an ether skeleton.
5. The method for producing an epoxy resin composition according to any one of claims 2 to 4, wherein the thixotropic agent is mixed in an amount of 1 to 20 parts by mass relative to 100 parts by mass of the epoxy resin.
6. The method for producing an epoxy resin composition according to any one of claims 1 to 5, wherein the thiol equivalent of the polythiol is 0.5 to 1 equivalent per 1 epoxy equivalent of the epoxy resin.
7. The method for producing the epoxy resin composition according to any one of claims 1 to 6, further comprising a step of adding a silane coupling agent.
8. The method for producing an epoxy resin composition according to claim 7, wherein the silane coupling agent is a silane coupling agent having an epoxy group and / or a mercapto group.
9. The method for producing an epoxy resin composition according to any one of claims 2 to 5, wherein the thixotropic agent is inorganic silica, or a combination of inorganic silica and an organic thixotropic agent.
10. The method for producing an epoxy resin composition according to any one of claims 1 to 9, wherein the solid basic compound is mixed so that the content thereof is 3 to 10 parts by mass per 100 parts by mass of the epoxy resin.
11. A method for producing an epoxy resin composition described in any one of claims 1 to 10, wherein the polythiol is pentaerythritol trippropanethiol.
12. A method for manufacturing a liquid ejection head having a recording element substrate that ejects ink, a support member that supports the recording element substrate and has a supply flow path that supplies ink to the recording element substrate, and a flow path member that supplies ink to the supply flow path, comprising the steps of: A step of producing an adhesive by the method for producing an epoxy resin composition according to any one of claims 1 to 11; a step of applying the adhesive to at least one joining surface between any two of the recording element substrate, the support member, and the flow path member to bond the two members together; A method for manufacturing a liquid ejection head comprising the steps of:
13. A method for manufacturing a liquid ejection head having a recording element substrate that ejects ink, a support member that supports the recording element substrate and has a supply flow path that supplies ink to the recording element substrate, and a flow path member that supplies ink to the supply flow path, comprising: A step of producing an adhesive comprising an epoxy resin, a solid basic compound, and a polythiol; a step of applying the adhesive to at least one joining surface between any two of the recording element substrate, the support member, and the flow path member to bond the two members together; Including, The method for manufacturing a liquid ejection head, wherein the step of manufacturing the adhesive includes a step of kneading the epoxy resin and the solid basic compound to manufacture a mixture 1, and a step of kneading the polythiol into the mixture 1 to manufacture a mixture 2.
14. A method for manufacturing a liquid ejection head having a recording element substrate that ejects ink, a support member that supports the recording element substrate and has a supply flow path that supplies ink to the recording element substrate, and a flow path member that supplies ink to the supply flow path, comprising: A step of producing an adhesive including an epoxy resin, a thixotropic agent, a solid basic compound, and a polythiol; a step of applying the adhesive to at least one joining surface between any two of the recording element substrate, the support member, and the flow path member to bond the two members together; Including, the step of producing the adhesive includes a step of producing a mixture 3 by kneading the epoxy resin and the thixotropic agent, a step of kneading the solid basic compound into the mixture 3 to produce a mixture 4, and a step of kneading the polythiol into the mixture 4 to produce a mixture 5.
15. A method for manufacturing a liquid ejection head having a recording element substrate that ejects ink, a support member that supports the recording element substrate and has a supply flow path that supplies ink to the recording element substrate, and a flow path member that supplies ink to the supply flow path, comprising the steps of: A step of producing an adhesive including an epoxy resin, a thixotropic agent, a solid basic compound, and a polythiol; a step of applying the adhesive to at least one joining surface between any two of the recording element substrate, the support member, and the flow path member to bond the two members together; Including, The method for manufacturing a liquid ejection head, wherein the step of manufacturing the adhesive includes the steps of kneading the epoxy resin and the solid basic compound to manufacture a mixture 1, kneading the polythiol and the thixotropic agent to manufacture a mixture 6, and kneading the mixture 1 and the mixture 6 to manufacture a mixture 7.
16. A method for manufacturing a liquid ejection head having a recording element substrate that ejects ink, a support member that supports the recording element substrate and has a supply flow path that supplies ink to the recording element substrate, and a flow path member that supplies ink to the supply flow path, comprising the steps of: A step of producing an adhesive including an epoxy resin, a thixotropic agent, a solid basic compound, and a polythiol; a step of applying the adhesive to at least one joining surface between any two of the recording element substrate, the support member, and the flow path member to bond the two members together; Including, The method for manufacturing a liquid ejection head, wherein the step of manufacturing the adhesive includes the steps of: kneading the epoxy resin and the thixotropic agent to manufacture mixture 3; kneading the solid basic compound into mixture 3 to manufacture mixture 4; kneading the polythiol and the thixotropic agent to manufacture mixture 6; and kneading mixture 4 and mixture 6 to manufacture mixture 8.
17. The method for manufacturing a liquid ejection head according to any one of claims 12 to 16, wherein the adhesive is used to perform a first thermal curing step to temporarily bond the two components together, and a second thermal curing step to perform a main curing step that takes longer than the first thermal curing step.
Citation Information
Patent Citations
Epoxy resin composition
JP1994211969A
Electroconductive resin composition
JP2000230112A
Photo and heat curable composition, and cured product using the same
JP2009051954A
High heat-conductive epoxy resin-based composition
JP2009292881A
Liquid discharge head, manufacturing method thereof, liquid discharge device, and image formation device
JP2015221541A