Acrylic rubber, acrylic rubber composition and crosslinked product thereof

By incorporating specific monomers and additives, acrylic rubber compositions achieve enhanced heat, cold, and oil resistance, addressing the need for improved performance in automobile engine compartments.

JP7596302B2Active Publication Date: 2024-12-09DENKA CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021562725
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-05
Filing Date
2020-12-03
Publication Date
2024-12-09
Estimated Expiration
2040-12-03

AI Technical Summary

Technical Problem

Acrylic rubber compositions used in automobile engine compartments require further improved heat resistance due to recent exhaust gas countermeasures and higher engine outputs.

Method used

Formulating acrylic rubber with specific monomer units such as acrylic acid alkyl esters and methacrylic acid alkyl esters, along with crosslinking agents and additives, to enhance heat resistance, cold resistance, and oil resistance.

Benefits of technology

The formulated acrylic rubber and its crosslinked products exhibit superior heat resistance, maintaining mechanical properties under high temperatures and improving cold and oil resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596302000001
    Figure 0007596302000001
  • Figure 0007596302000002
    Figure 0007596302000002
Patent Text Reader

Abstract

An acrylic rubber which contains, as monomer units, 100 parts by mass of an acrylic acid alkyl ester and 30 parts by mass or more of a methacrylic acid alkyl ester.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an acrylic rubber, an acrylic rubber composition, and a crosslinked product thereof. [Background technology]

[0002] Acrylic rubber and its crosslinked products are widely used as materials for hose members and seal members in the engine compartment of automobiles, which require heat resistance. Known means for improving the heat resistance of acrylic rubber include a technique of incorporating a specific carbon black into an acrylic rubber composition (see, for example, Patent Document 1) and a technique of incorporating a specific antioxidant in combination (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2008 / 143300 [Patent Document 2] JP 2011-032390 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, due to the influence of recent exhaust gas countermeasures and higher engine power output, there is a demand for further improvement in the heat resistance of acrylic rubber.

[0005] In view of the above circumstances, one aspect of the present invention has an object to provide an acrylic rubber having excellent heat resistance and a crosslinked product thereof. [Means for solving the problem]

[0006] The present invention includes the following aspects. [1] An acrylic rubber containing, as monomer units, 100 parts by mass of an alkyl acrylate and 30 parts by mass or more of an alkyl methacrylate. [2] The acrylic rubber according to [1], wherein the alkyl methacrylate ester is n-butyl methacrylate. [3] The acrylic rubber according to [1] or [2], wherein the alkyl acrylate ester is at least one selected from the group consisting of ethyl acrylate and n-butyl acrylate. [4] The acrylic rubber according to any one of [1] to [3], further comprising, as a monomer unit, a crosslinkable monomer having a carboxy group. [5] The acrylic rubber according to any one of [1] to [4], further containing ethylene as a monomer unit. [6] The acrylic rubber according to any one of [1] to [5], wherein the content of the alkyl methacrylate is 30 parts by mass or more and 60 parts by mass or less. [7] An acrylic rubber composition comprising the acrylic rubber according to any one of [1] to [6]. [8] The acrylic rubber composition according to [7], further comprising one or more selected from the group consisting of a crosslinking agent and a crosslinking accelerator. [9] The acrylic rubber composition according to [7] or [8], further comprising one or more selected from the group consisting of fillers, reinforcing agents, plasticizers, lubricants, antioxidants, stabilizers, and silane coupling agents.

[10] A crosslinked product of the acrylic rubber composition according to any one of [7] to [9].

[11] A hose member comprising the cross-linked material according to

[10] .

[12] A sealing member comprising the cross-linked material described in

[10] .

[13] A vibration-isolating rubber member comprising the cross-linked product according to

[10] . Effect of the Invention

[0007] According to one aspect of the present invention, there is provided an acrylic rubber having excellent heat resistance and a crosslinked product thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to the embodiments described below.

[0009] (acrylic rubber) The acrylic rubber of the present embodiment contains, as monomer units, 100 parts by mass of an alkyl acrylate and 30 parts by mass or more of an alkyl methacrylate.

[0010] The alkyl acrylate forms the backbone of the acrylic rubber, and by adjusting the content of the alkyl acrylate contained as a monomer unit, the heat resistance, cold resistance, and oil resistance of the acrylic rubber and its crosslinked product can be adjusted.

[0011] The acrylic acid alkyl ester is not particularly limited, but examples thereof include acrylic acid alkyl esters having an alkyl group having 1 to 16 carbon atoms, specifically methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-methylpentyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, hexadecyl acrylate, 1-adamantyl acrylate, cyclohexyl acrylate, and the like. These acrylic acid alkyl esters may be used alone or in combination of two or more. From the viewpoint of further improving the heat resistance of the acrylic rubber and also improving the oil resistance and cold resistance, the acrylic acid alkyl ester is preferably an acrylic acid alkyl ester having an alkyl group having 2 to 4 carbon atoms, and more preferably one or more selected from the group consisting of ethyl acrylate and n-butyl acrylate.

[0012] The content of acrylic acid alkyl ester monomer units (hereinafter also referred to as acrylic acid alkyl ester units) in the acrylic rubber is preferably 40% by mass or more, more preferably 45% by mass or more, and even more preferably 50% by mass or more, based on the total monomer units (100% by mass) constituting the acrylic rubber. The content of acrylic acid alkyl ester units is preferably 99% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less, based on the total monomer units (100% by mass) constituting the acrylic rubber. The acrylic acid alkyl ester units are quantified based on the nuclear magnetic resonance spectrum obtained for the acrylic rubber or the acrylic rubber composition.

[0013] The acrylic rubber further contains a methacrylic acid alkyl ester as a monomer unit. The methacrylic acid alkyl ester is not particularly limited, but may be, for example, an alkyl methacrylate having an alkyl group having 1 to 4 carbon atoms, specifically, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, etc. These methacrylic acid alkyl esters may be used alone or in combination of two or more. The methacrylic acid alkyl ester is preferably n-butyl methacrylate from the viewpoint of further improving the heat resistance of the acrylic rubber.

[0014] In the acrylic rubber of this embodiment, the content of the methacrylic acid alkyl ester monomer unit (hereinafter also referred to as the methacrylic acid alkyl ester unit) is 30 parts by mass or more relative to 100 parts by mass of the acrylic acid alkyl ester unit. This improves the heat resistance of the acrylic rubber and its crosslinked product. In particular, even after the acrylic rubber is exposed to high temperatures for a long time, it becomes possible to maintain a high elongation at break, and the mechanical properties against heat are improved. From the viewpoint of further improving the heat resistance, the content of the methacrylic acid alkyl ester unit in the acrylic rubber is more preferably 33 parts by mass or more, even more preferably 35 parts by mass or more, and particularly preferably 37 parts by mass or more, 38 parts by mass or more, 40 parts by mass or more, 42 parts by mass or more, or 44 parts by mass or more relative to 100 parts by mass of the acrylic acid alkyl ester unit.

[0015] The content of the methacrylic acid alkyl ester units in the acrylic rubber is preferably 60 parts by mass or less, more preferably 58 parts by mass or less, even more preferably 55 parts by mass or less, and particularly preferably 50 parts by mass or less, relative to 100 parts by mass of the acrylic acid alkyl ester units. By having the ratio of the methacrylic acid alkyl ester units to the acrylic acid alkyl ester units within the above-mentioned range, it is possible to maintain the cold resistance and oil resistance of the acrylic rubber and its crosslinked product while further improving the heat resistance.

[0016] The content of the methacrylic acid alkyl ester units in the acrylic rubber is preferably 30 to 60 parts by mass, more preferably 33 to 58 parts by mass, further preferably 35 to 55 parts by mass, and particularly preferably 37 to 50 parts by mass, relative to 100 parts by mass of the acrylic acid alkyl ester units. The content of the methacrylic acid alkyl ester units in the acrylic rubber is quantified based on the nuclear magnetic resonance spectrum obtained for the acrylic rubber or the acrylic rubber composition, similar to the content of the acrylic acid alkyl ester units.

[0017] The acrylic rubber of the present embodiment may further contain a crosslinking group monomer as a monomer unit. The crosslinking group monomer refers to a monomer having a functional group that forms a crosslinking group (also called a crosslinking point). The crosslinking group monomer is preferably a monomer having a carboxy group. The carboxy group of the crosslinking group monomer enables intermolecular crosslinking of the acrylic rubber, making it possible to adjust the hardness and elongation at break of the acrylic rubber.

[0018] Examples of crosslinking monomers having a carboxy group include, but are not limited to, acrylic acid, methacrylic acid, crotonic acid, 2-pentenoic acid, maleic acid, fumaric acid, itaconic acid, maleic acid monoalkyl esters, fumaric acid monoalkyl esters, maleic acid monocyclohexyl, fumaric acid monocyclohexyl, cinnamic acid, etc. The crosslinking monomers may be used alone or in combination of two or more.

[0019] The crosslinking monomer is preferably a maleic acid monoalkyl ester having an alkyl group of 1 to 8 carbon atoms or a fumaric acid monoalkyl ester having an alkyl group of 1 to 8 carbon atoms, and more preferably monobutyl maleate or monobutyl fumarate, from the viewpoint of facilitating a copolymerization reaction between monomers and further improving the heat resistance of the acrylic rubber and its crosslinked product.

[0020] The content of the monomer unit of the crosslinking group monomer in the acrylic rubber (hereinafter also referred to as the crosslinking group monomer unit) is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the acrylic acid alkyl ester units. When the content of the crosslinking group monomer unit is 0.1 parts by mass or more, there is a sufficient effect of crosslinking the acrylic rubber, and the strength of the crosslinked product of the acrylic rubber is improved. When the content of the crosslinking group monomer unit is 5 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 3 parts by mass or less, relative to 100 parts by mass of the acrylic acid alkyl ester units. When the content of the crosslinking group monomer unit is 5 parts by mass or less, the crosslinked product of the acrylic rubber does not harden too much, and the rubber elasticity of the crosslinked product can be stably maintained. For example, when the crosslinking group monomer is a crosslinking group monomer having a carboxy group, the acrylic rubber is dissolved in toluene, and neutralization titration using potassium hydroxide can be performed.

[0021] The acrylic rubber may further contain ethylene as a monomer unit. When the acrylic rubber contains an ethylene monomer unit (hereinafter also referred to as an ethylene unit), the cold resistance and strength of the crosslinked product of the acrylic rubber are improved. When the acrylic rubber contains an ethylene unit, for example, when the crosslinked product of the acrylic rubber is used as a hose member, the appearance of the hose member becomes smooth, and the aesthetics of the hose member are improved. The content of the ethylene unit in the acrylic rubber is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the acrylic acid alkyl ester units. The content of the ethylene unit is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the acrylic acid alkyl ester units. When the ethylene unit is in the above range, the cold resistance and strength of the crosslinked product of the acrylic rubber are further improved. The content of the ethylene unit in the acrylic rubber can be quantified based on the nuclear magnetic resonance spectrum obtained for the acrylic rubber or the acrylic rubber composition.

[0022] The acrylic rubber may contain other monomers copolymerizable with the acrylic acid alkyl ester and the methacrylic acid alkyl ester as monomer units. Examples of the copolymerizable other monomers include ethylenically unsaturated compounds other than the above-mentioned monomers. Examples of the ethylenically unsaturated compounds include (meth)acrylic acid alkoxy esters, alkyl vinyl ketones, vinyl and allyl ethers, vinyl aromatic compounds, vinyl nitriles, maleic acid dialkyl esters, fumaric acid dialkyl esters, itaconic acid dialkyl esters, citraconic acid dialkyl esters, mesaconic acid dialkyl esters, 2-pentenedioic acid dialkyl esters, and acetylenedicarboxylic acid dialkyl esters. More specific examples of the compound include methoxyethyl acrylate, vinyl acetate, methyl vinyl ketone, vinyl ethyl ether, allyl methyl ether, styrene, α-methylstyrene, chlorostyrene, vinyl toluene, vinyl naphthalene, acrylonitrile, methacrylonitrile, acrylamide, propylene, butadiene, isoprene, pentadiene, vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, vinyl propionate, dimethyl maleate, dimethyl fumarate, dimethyl itaconate, dimethyl citraconate, dimethyl mesaconic acid, dimethyl 2-pentenedioate, and dimethyl acetylenedicarboxylate.

[0023] The acrylic rubber of the present embodiment can be obtained by copolymerizing the above-mentioned monomers by a known method such as emulsion polymerization, suspension polymerization, solution polymerization, or bulk polymerization.

[0024] (Acrylic rubber composition and crosslinked product thereof) The acrylic rubber composition of the present embodiment contains the above-mentioned acrylic rubber. The acrylic rubber composition may contain, for example, a crosslinking agent, a crosslinking accelerator, and other additives, which will be described later. In this case, the acrylic rubber composition is kneaded at a temperature equal to or lower than the crosslinking temperature, and then heated at a predetermined crosslinking temperature to obtain a crosslinked product. The acrylic rubber composition can be molded into various desired shapes and then crosslinked to obtain a crosslinked product, or can be molded into various shapes after crosslinking to obtain a crosslinked product.

[0025] Heating conditions for crosslinking can be appropriately set depending on the blending of the acrylic rubber composition and the type of crosslinking agent, and may be, for example, 100 to 200°C and 1 to 10 hours. As a heating method, a method used for crosslinking rubber, such as hot press heating, steam heating, oven heating, etc., can be used. Note that the crosslinking agent and the crosslinking accelerator are generally sometimes called vulcanizing agent and vulcanization accelerator, respectively, but in this specification, the crosslinking agent may be a compound containing sulfur or a compound not containing sulfur.

[0026] The apparatus for kneading, molding, and crosslinking the acrylic rubber composition and the apparatus for kneading and molding the crosslinked product of the acrylic rubber composition may be an apparatus that is generally used for acrylic rubber compositions. As the kneading apparatus, a roll, a kneader, a Banbury mixer, an internal mixer, a twin-screw extruder, etc. may be used.

[0027] The crosslinking agent is not particularly limited as long as it is one that is usually used for crosslinking acrylic rubber. When the acrylic rubber contains a crosslinking monomer having a carboxy group as a monomer unit, the crosslinking agent is preferably a polyamine compound and a carbonate of a polyamine compound, more preferably a polyamine compound having 4 to 30 carbon atoms and a carbonate thereof.

[0028] Specific examples of polyamine compounds include 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenyl sulfide, 1,3-bis(4-aminophenoxy)-2,2-dimethylpropane, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)pentane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]sulfone, 4,4'-diaminodiphenylsulfone, and bis(4-aminophenoxy)phenyl. (i) Aromatic polyamine compounds such as phenylsulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 4,4'-diaminobenzanilide, and bis[4-(4-aminophenoxy)phenyl]sulfone; and aliphatic polyamine compounds such as hexamethylenediamine, hexamethylenediamine carbamate, N,N'-dicinnamylidene-1,6-hexanediamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine.

[0029] The content of the crosslinking agent in the acrylic rubber composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, relative to 100 parts by mass of the acrylic rubber. The content of the crosslinking agent is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 3 parts by mass or less, relative to 100 parts by mass of the acrylic rubber. By keeping the content within the above range, sufficient crosslinking treatment can be performed.

[0030] The crosslinking accelerator is not particularly limited, but when the crosslinking agent is a polyamine compound or a carbonate thereof, examples of the crosslinking accelerator include aliphatic monovalent secondary amine compounds, aliphatic monovalent tertiary amine compounds, guanidine compounds, imidazole compounds, quaternary onium salts, tertiary phosphine compounds, alkali metal salts of weak acids, and diazabicycloalkene compounds. The crosslinking accelerator can be used alone or in combination of two or more.

[0031] Examples of the aliphatic monovalent secondary amine compound include dimethylamine, diethylamine, di-n-propylamine, diallylamine, diisopropylamine, di-n-butylamine, di-t-butylamine, di-sec-butylamine, dihexylamine, diheptylamine, dioctylamine, dinonylamine, didecylamine, diundecylamine, didodecylamine, ditridecylamine, ditetradecylamine, dipentadecylamine, dicetylamine, di-2-ethylhexylamine, dioctadecylamine, di-cis-9-octadecenylamine, and dinonadecylamine.

[0032] Examples of the aliphatic monovalent tertiary amine compounds include trimethylamine, triethylamine, tri-n-propylamine, triallylamine, triisopropylamine, tri-n-butylamine, tri-t-butylamine, tri-sec-butylamine, tripentylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, triundecylamine, tridodecylamine, tridecylamine, tritetradecylamine, tripentadecylamine, tricetylamine, tri-2-ethylhexylamine, trioct ... Examples of the amines include octadecylamine, tri-cis-9-octadecenylamine, trinonadecylamine, N,N-dimethyldecylamine, N,N-dimethyldodecylamine, N,N-dimethyltetradecylamine, N,N-dimethylcetylamine, N,N-dimethyloctadecylamine, N,N-dimethylbehenylamine, N-methyldidecylamine, N-methyldidodecylamine, N-methylditetradecylamine, N-methyldicetylamine, N-methyldioctadecylamine, N-methyldibehenylamine, and dimethylcyclohexylamine.

[0033] The guanidine compounds include 1,3-di-o-tolylguanidine, 1,3-diphenylguanidine, and the like.

[0034] The imidazole compounds include 2-methylimidazole, 2-phenylimidazole, and the like.

[0035] The quaternary onium salt is not particularly limited, but examples thereof include tetra-n-butylammonium chloride, trimethylphenylammonium chloride, trimethylstearylammonium chloride, trimethyllaurylammonium chloride, trimethylcetylammonium chloride, dimethyldistearylammonium chloride, tributylbenzylammonium chloride, tetra-n-butylammonium bromide, methyltriphenylammonium bromide, ethyltriphenylammonium bromide, trimethylphenylammonium bromide, trimethylbenzylammonium bromide, trimethylstearylammonium bromide, and tetrabutylammonium thiocyanate. and phosphonium salts such as tetra-n-butylphosphonium chloride, tetra-n-butylphosphonium bromide, methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, butyltriphenylphosphonium bromide, hexyltriphenylphosphonium bromide, benzyltriphenylphosphonium bromide, tetraphenylphosphonium chloride, tetraphenylphosphonium bromide, 4-butoxybenzyltriphenylphosphonium bromide, allyltributylphosphonium chloride, 2-propynyltriphenylphosphonium bromide, and methoxypropyltributylphosphonium chloride.

[0036] Tertiary phosphine compounds include triphenylphosphine, tri-p-tolylphosphine, and the like.

[0037] Examples of the alkali metal salts of weak acids include inorganic weak acid salts such as sodium and potassium phosphates and carbonates, and organic weak acid salts such as sodium and potassium stearates and laurates.

[0038] Examples of the diazabicycloalkene compound include 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), 1,5-diazabicyclo[4.3.0]nonene-5 (DBN), and 1,4-diazabicyclo[2.2.2]octane (DABCO). These diazabicycloalkene compounds may form salts with, for example, hydrochloric acid, sulfuric acid, carboxylic acid, sulfonic acid, and phenol. Examples of the carboxylic acid include octyl acid, oleic acid, formic acid, orthophthalic acid, and adipic acid. Examples of the sulfonic acid include benzenesulfonic acid, toluenesulfonic acid, dodecylbenzenesulfonic acid, and naphthalenesulfonic acid.

[0039] The crosslinking accelerator may contain a curing agent for the epoxy resin, such as a thermally decomposed ammonium salt, an organic acid, an acid anhydride, an amine, sulfur, or a sulfur compound, in order to adjust the crosslinking rate.

[0040] The content of the crosslinking accelerator in the acrylic rubber composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, relative to 100 parts by mass of the acrylic rubber. The content of the crosslinking accelerator is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 3 parts by mass or less, relative to 100 parts by mass of the acrylic rubber. By keeping the content within the above range, sufficient crosslinking treatment can be performed.

[0041] The acrylic rubber composition may contain additives such as a filler (reinforcing agent), a plasticizer, a lubricant, an antioxidant, a stabilizer, and a silane coupling agent depending on the purpose of practical use.

[0042] The filler (reinforcing agent) may be any filler (reinforcing agent) used in ordinary acrylic rubber, such as carbon black, acetylene black, silica, clay, talc, calcium carbonate, antimony trioxide, and aluminum hydroxide.

[0043] The total content of these additives in the acrylic rubber composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, per 100 parts by mass of the acrylic rubber, and is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, per 100 parts by mass of the acrylic rubber.

[0044] The cross-linked product of this embodiment is used as an industrial part, and is particularly suitable for use as a hose member such as a rubber hose; a sealing member such as a gasket or packing; and an anti-vibration rubber member. That is, another embodiment of the present invention is a hose member, a sealing part, or an anti-vibration rubber member that includes the above-mentioned cross-linked product. These members may consist of only the cross-linked product of the acrylic rubber composition, or may include the cross-linked product and other parts.

[0045] Examples of the hose member include a transmission oil cooler hose, an engine oil cooler hose, an air duct hose, a turbo intercooler hose, a hot air hose, a radiator hose, a power steering hose, a hose for a fuel system, a hose for a drain system, etc. The hose member may have a reinforcing yarn or wire in an intermediate layer or an outermost layer of the hose.

[0046] Examples of sealing members include engine head cover gaskets, oil pan gaskets, oil seals, lip seal packings, O-rings, transmission seal gaskets, crankshafts, camshaft seal gaskets, valve stems, power steering seal belt cover seals, constant velocity joint boot materials, and rack and pinion boot materials.

[0047] Examples of anti-vibration rubber members include damper pulleys, center support cushions, and suspension bushings. EXAMPLES

[0048] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0049] Six types of acrylic rubbers A to F were produced under the conditions shown below. <Acrylic rubber A> In a pressure-resistant reaction vessel with an internal volume of 40 liters, 17 kg of a 4% by mass aqueous solution of partially saponified polyvinyl alcohol and 56 g of sodium formaldehyde sulfoxylate were charged and mixed well in advance with a stirrer to prepare a uniform suspension. After replacing the air in the upper part of the tank with nitrogen, 0.9 kg of ethylene was pressed into the upper part of the tank to adjust the pressure to 3.5 MPa. After continuing the stirring and maintaining the tank at 55°C, 5.2 kg of ethyl acrylate, 2.9 kg of n-butyl acrylate, 3.1 kg of n-butyl methacrylate, 0.22 kg of monobutyl fumarate, and a 0.5% by mass aqueous solution of t-butyl hydroperoxide were separately pressed into the tank from a separate inlet to start polymerization. The temperature in the tank was kept at 55°C during the reaction, and the reaction was continued until the polymerization conversion rate reached 95%. 20 kg of a 0.3% by mass aqueous solution of sodium borate was added to the polymerization liquid to solidify the polymer, and acrylic rubber A was obtained by dehydrating and drying.

[0050] The acrylic rubber A had a copolymer composition of 45 parts by mass of ethyl acrylate units, 24 parts by mass of n-butyl acrylate units, 28 parts by mass of n-butyl methacrylate units, 1.5 parts by mass of ethylene units, and 1.5 parts by mass of monobutyl fumarate units. The amounts of these monomer components were quantified by nuclear magnetic resonance spectroscopy.

[0051] <Acrylic rubber B> Acrylic rubber B was obtained by the same method as for acrylic rubber A, except that n-butyl acrylate and monobutyl fumarate were not used, and the monomers used were changed to 7.6 kg of ethyl acrylate, 3.6 kg of n-butyl methacrylate, 0.9 kg of ethylene, and 0.28 kg of monobutyl maleate.

[0052] This acrylic rubber B had a copolymer composition of 67 parts by mass of ethyl acrylate units, 30 parts by mass of n-butyl methacrylate units, 1.6 parts by mass of ethylene units, and 1.5 parts by mass of monobutyl maleate units.

[0053] <Acrylic rubber C> Acrylic Rubber C was obtained by the same method as Acrylic Rubber A, except that n-butyl acrylate and monobutyl fumarate were not used, and the monomers used were changed to 8.3 kg of ethyl acrylate, 2.9 kg of n-butyl methacrylate, 0.9 kg of ethylene, and 0.28 kg of monobutyl maleate.

[0054] This acrylic rubber C had a copolymer composition of 72 mass % of ethyl acrylate units, 25 mass % of n-butyl methacrylate units, 1.7 mass % of ethylene units, and 1.6 mass % of monobutyl maleate units relative to the total monomer units (100 mass %).

[0055] <Acrylic rubber D> Acrylic Rubber D was obtained by the same method as Acrylic Rubber A, except that n-butyl acrylate and monobutyl fumarate were not used, and the monomers used were changed to 7.2 kg of ethyl acrylate, 4.0 kg of n-butyl methacrylate, 0.9 kg of ethylene, and 0.28 kg of monobutyl maleate.

[0056] This acrylic rubber D had a copolymer composition of 63 mass % of ethyl acrylate units, 34 mass % of n-butyl methacrylate units, 1.5 mass % of ethylene units, and 1.4 mass % of monobutyl maleate units relative to the total monomer units (100 mass %).

[0057] <Acrylic rubber E> Acrylic rubber E was obtained by the same method as for acrylic rubber A, except that n-butyl methacrylate and monobutyl fumarate were not used, and the monomers used were changed to 7.8 kg of ethyl acrylate, 3.4 kg of n-butyl acrylate, 0.9 kg of ethylene, and 0.28 kg of monobutyl maleate.

[0058] This acrylic rubber E had a copolymer composition of 68 mass % ethyl acrylate units, 29 mass % n-butyl acrylate units, 1.6 mass % ethylene units, and 1.5 mass % monobutyl maleate units relative to the total monomer units (100 mass %).

[0059] <Acrylic rubber F> Acrylic Rubber F was obtained by the same method as Acrylic Rubber A, except that n-butyl methacrylate and monobutyl fumarate were not used, and the monomers used were changed to 6.2 kg of ethyl acrylate, 3.9 kg of n-butyl acrylate, 1.1 kg of methyl methacrylate, 0.9 kg of ethylene, and 0.28 kg of monobutyl maleate.

[0060] This acrylic rubber F had a copolymer composition of 53 mass% ethyl acrylate units, 34 mass% n-butyl acrylate units, 1.6 mass% ethylene units, 9.7 mass% methyl methacrylate units, and 1.6 mass% monobutyl maleate units relative to the total monomer units (100 mass%).

[0061] <Acrylic rubber G> Acrylic rubber G was obtained by the same method as for acrylic rubber A, except that n-butyl methacrylate and monobutyl fumarate were not used, and the monomers used were changed to 6.2 kg of ethyl acrylate, 3.9 kg of n-butyl acrylate, 1.1 kg of methyl methacrylate, 0.9 kg of ethylene, and 0.40 kg of monobutyl maleate.

[0062] This acrylic rubber G had a copolymer composition of 53 mass% ethyl acrylate units, 34 mass% n-butyl acrylate units, 1.5 mass% ethylene units, 9.6 mass% methyl methacrylate units, and 2.2 mass% monobutyl maleate units relative to the total monomer units (100 mass%).

[0063] <Acrylic rubber H> Acrylic Rubber H was obtained by the same method as for Acrylic Rubber A, except that the amounts of monomers used were changed to 7.7 kg of ethyl acrylate, 2.4 kg of n-butyl acrylate, 1.1 kg of n-butyl methacrylate, 0.9 kg of ethylene, and 0.28 kg of monobutyl fumarate.

[0064] This acrylic rubber H had a copolymer composition of 68 mass% ethyl acrylate units, 19 mass% n-butyl acrylate units, 1.5 mass% ethylene units, 9.7 mass% n-butyl methacrylate units, and 1.5 mass% monobutyl fumarate units relative to the total monomer units (100 mass%).

[0065] The monomer compositions of the acrylic rubbers A to H are shown in the following Table 1. In addition, in Table 1, the values ​​shown are calculated assuming that the acrylic acid alkyl ester unit is 100 parts by mass.

[0066] [Table 1]

[0067] The above acrylic rubbers A to H and other materials were kneaded using an 8-inch open roll according to the formulations in Table 2 to obtain acrylic rubber compositions of Examples 1 to 4 and Comparative Examples 1 to 4. These acrylic rubber compositions (uncrosslinked) were molded to a thickness of 2 mm and heat-treated in a hot press at 170°C for 20 minutes to obtain a primary crosslinked product, and then heat-treated in hot air (Gear oven) at 170°C for 4 hours to obtain a crosslinked product of the acrylic rubber composition.

[0068] The reagents shown in Table 2 are as follows: Carbon black: SEAT SO manufactured by Tokai Carbon Co., Ltd. Lubricant A: Liquid paraffin (Kaneda Co., Ltd.) Lubricant B: Stearic acid (NOF Corporation) Lubricant C: Stearylamine (Farmin 80 manufactured by Kao Corporation) Antioxidant: 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (Addivant's Naugard 445) Crosslinker: Hexamethylenediamine carbamate (Diak#1 manufactured by Dupont) Crosslinking accelerator: LANXESS XLA-60

[0069] The heat resistance, oil resistance, and cold resistance of the obtained crosslinked product of the acrylic rubber composition were evaluated under the following conditions.

[0070] (Heat resistance test) The crosslinked acrylic rubber composition was heat treated at a test temperature of 190°C for 504 hours in accordance with JIS K6257:2017. The elongation at break of each of the crosslinked products before and after heat treatment was measured using a dumbbell-shaped No. 3 specimen in accordance with JIS K6251:2017. The elongation at break after heat treatment and the rate of change in the elongation at break before and after heat treatment were determined. The closer the rate of change is to 100, the less change there is before and after heat treatment, indicating high heat resistance.

[0071] (Oil resistance test) For Examples 1 to 4, ΔV (volume change rate) and ΔW (mass change rate) of the crosslinked products were also measured in accordance with JIS K6258:2016.

[0072] (Cold resistance test) For Examples 1 to 4, the T of the crosslinked product was measured according to JIS K6261:2006. 100 was measured. Here, T 100 is the temperature at which the modulus (specific modulus) becomes 100 times the modulus at 23°C of the crosslinked product.

[0073] [Table 2]

[0074] As shown in Table 2, the cross-linked products of the acrylic rubber compositions of the Examples exhibited superior heat resistance compared to the cross-linked products of the acrylic rubber compositions of the Comparative Examples.

Claims

1. An acrylic rubber containing, as monomer units, 100 parts by mass of an alkyl acrylate, 37 parts by mass or more of n-butyl methacrylate, and a crosslinking monomer having a carboxy group (excluding the case where the acrylic rubber contains 5 to 75% by weight of at least one methacrylic acid ester monomer unit selected from an alkoxyalkyl methacrylate monomer unit, a polyalkylene glycol methacrylate monomer unit, and an alkoxypolyalkylene glycol methacrylate monomer unit).

2. The acrylic rubber according to claim 1, wherein the alkyl acrylate is at least one selected from the group consisting of ethyl acrylate and n-butyl acrylate.

3. The acrylic rubber according to claim 1 or 2, further comprising ethylene as a monomer unit.

4. The acrylic rubber according to any one of claims 1 to 3, wherein the content of n-butyl methacrylate is 37 parts by mass or more and 60 parts by mass or less.

5. An acrylic rubber composition comprising the acrylic rubber according to any one of claims 1 to 4.

6. The acrylic rubber composition according to claim 5, further comprising at least one selected from the group consisting of a crosslinking agent and a crosslinking accelerator.

7. The acrylic rubber composition according to claim 5 or 6, further comprising at least one selected from the group consisting of a filler, a reinforcing agent, a plasticizer, a lubricant, an antioxidant, a stabilizer, and a silane coupling agent.

8. A crosslinked product of the acrylic rubber composition according to any one of claims 5 to 7.

9. A hose member comprising the cross-linked product according to claim 8.

10. A sealing member comprising the cross-linked product according to claim 8.

11. A vibration-isolating rubber member comprising the cross-linked product according to claim 8.

Citation Information

Patent Citations

  • Synthetic resin composite

    JP1994262713A

  • Acrylic rubber, acrylic rubber composition, and acrylic rubber crosslinked product

    JP2008214418A

  • Heat-resistant acrylic rubber composition

    JP2011032390A

  • Thermoplastic elastomer composition and method for producing same

    WO2006057445A1

  • Acrylic rubber composition, vulcanized rubber therefrom and use thereof

    WO2008143300A1