Acrylic rubber, rubber composition and crosslinked product thereof, and rubber hose

By adjusting the ethyl acrylate to n-butyl acrylate ratio and limiting toluene-insoluble content, the acrylic rubber composition achieves enhanced bending fatigue and tensile strength, suitable for durable rubber hoses and seals.

JP7596316B2Active Publication Date: 2024-12-09DENKA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021574667
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-30
Filing Date
2021-01-20
Publication Date
2024-12-09
Estimated Expiration
2041-01-20

AI Technical Summary

Technical Problem

Existing acrylic rubber compositions do not adequately address the issue of bending fatigue resistance, which is crucial for applications requiring flexibility and durability, such as hose members in automobile engine rooms.

Method used

The composition of acrylic rubber is optimized by controlling the mass ratio of ethyl acrylate to n-butyl acrylate and limiting the toluene-insoluble content to improve bending fatigue resistance, with additional components like ethylene and crosslinking monomers with carboxyl groups enhancing the properties.

Benefits of technology

The optimized acrylic rubber composition exhibits improved bending fatigue resistance, tensile strength, and cold resistance, making it suitable for durable applications like rubber hoses and seals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596316000001
    Figure 0007596316000001
Patent Text Reader

Abstract

One aspect of the present invention is an acrylic rubber which contains ethyl acrylate and n-butyl acrylate as monomer units and which contains toluene-insoluble components. The mass ratio of the content of ethyl acrylate relative to the content of n-butyl acrylate is 2 or more. The content of toluene-insoluble components is 5 mass% or less based on the total amount of the acrylic rubber.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an acrylic rubber, a rubber composition and a crosslinked product thereof, and a rubber hose. [Background technology]

[0002] Acrylic rubber and its crosslinked products are excellent in physical properties such as heat resistance, oil resistance, and mechanical properties, and are therefore widely used, for example, as materials for hose members in the engine compartment of an automobile. One of the properties required for such crosslinked products of acrylic rubber is that cracks are unlikely to occur when the crosslinked product is bent (called flex fatigue resistance). For example, Patent Document 1 discloses an acrylic rubber composition in which a specific antioxidant, carbon black, and a crosslinking agent are added to acrylic rubber as an acrylic rubber composition capable of giving a crosslinked product excellent in flex fatigue resistance and the like. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-211239 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the above-mentioned Patent Document 1, an attempt is made to improve the flex fatigue resistance by making the acrylic rubber composition have a specific composition. However, according to the studies of the present inventors, there is also room for improvement in the acrylic rubber itself in order to improve the flex fatigue resistance.

[0005] Therefore, an object of one aspect of the present invention is to provide an acrylic rubber capable of improving the flex fatigue resistance of a cross-linked product. [Means for solving the problem]

[0006] The present inventors have found that, in an acrylic rubber containing ethyl acrylate and n-butyl acrylate as monomer units, by setting the mass ratio of the ethyl acrylate content to the n-butyl acrylate content and the content of toluene insolubles contained in the acrylic rubber within predetermined ranges, it is possible to improve the flexural fatigue resistance of the crosslinked product compared to cases where the mass ratio and the toluene insolubles are outside those ranges.

[0007] One aspect of the present invention is an acrylic rubber which contains ethyl acrylate and n-butyl acrylate as monomer units and contains toluene-insoluble matter, wherein the mass ratio of the ethyl acrylate content to the n-butyl acrylate content is 2 or more, and the toluene-insoluble matter content is 5 mass% or less based on the total amount of the acrylic rubber.

[0008] The acrylic rubber may include a methacrylate as a monomer unit. The acrylic rubber may further include ethylene as a monomer unit. The acrylic rubber may further include a crosslinking monomer having a carboxyl group as a monomer unit.

[0009] The acrylic rubber may contain only ethyl acrylate, n-butyl acrylate, ethylene, and a crosslinking monomer having a carboxyl group as monomer units. In this case, the content of ethyl acrylate may be 70 to 90 mass% based on the total amount of monomer units. The content of n-butyl acrylate may be 10 to 30 mass% based on the total amount of monomer units. The content of ethylene may be 0.5 to 5 mass% based on the total amount of monomer units. The content of the crosslinking monomer may be 0.5 to 5 mass% based on the total amount of monomer units.

[0010] Another aspect of the present invention is a rubber composition containing the above-mentioned acrylic rubber. Another aspect of the present invention is a crosslinked product of the rubber composition. Another aspect of the present invention is a rubber hose containing the crosslinked product. Effect of the Invention

[0011] According to one aspect of the present invention, it is possible to provide an acrylic rubber capable of improving the flex fatigue resistance of a cross-linked product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] One embodiment of the present invention is an acrylic rubber that includes ethyl acrylate and n-butyl acrylate as monomer units.

[0013] The content of ethyl acrylate may be preferably 70% by mass or more, 72% by mass or more, 74% by mass or more, or 76% by mass or more based on the total amount of monomer units contained in the acrylic rubber, from the viewpoint of improving the tensile strength of the crosslinked product (hereinafter also simply referred to as "crosslinked product") of the acrylic rubber (composition containing the acrylic rubber). The content of ethyl acrylate may be preferably 90% by mass or less, 87% by mass or less, 85% by mass or less, or 82% by mass or less based on the total amount of monomer units contained in the acrylic rubber, from the viewpoint of improving the cold resistance of the crosslinked product. The content of ethyl acrylate may be 70 to 90 mass%, 70 to 87 mass%, 70 to 85 mass%, 70 to 82 mass%, 72 to 90 mass%, 72 to 87 mass%, 72 to 85 mass%, 72 to 82 mass%, 74 to 90 mass%, 74 to 87 mass%, 74 to 85 mass%, 74 to 82 mass%, 76 to 90 mass%, 76 to 87 mass%, 76 to 85 mass%, or 76 to 82 mass%, based on the total amount of monomer units contained in the acrylic rubber.

[0014] The total content of ethyl acrylate and n-butyl acrylate, based on the total amount of monomer units contained in the acrylic rubber, may be 90 mass% or more, 93 mass% or more, 95 mass% or more, or 96 mass% or more, and may be 99.5 mass% or less or 99 mass% or less, or may be 90 to 99.5 mass%, 90 to 99 mass%, 93 to 99.5 mass%, 93 to 99 mass%, 95 to 99.5 mass%, 95 to 99 mass%, 96 to 99.5 mass%, or 96 to 99 mass%.

[0015] The content of n-butyl acrylate may be preferably 10% by mass or more, 12% by mass or more, or 15% by mass or more based on the total amount of monomer units contained in the acrylic rubber from the viewpoint of improving the cold resistance of the crosslinked product. The content of n-butyl acrylate may be preferably 30% by mass or less, 25% by mass or less, or 22% by mass or less based on the total amount of monomer units contained in the acrylic rubber from the viewpoint of improving the tensile strength of the crosslinked product. The content of n-butyl acrylate may be 10 to 30% by mass, 10 to 25% by mass, 10 to 22% by mass, 12 to 30% by mass, 12 to 25% by mass, 12 to 22% by mass, 15 to 30% by mass, 15 to 25% by mass, or 15 to 22% by mass based on the total amount of monomer units contained in the acrylic rubber.

[0016] The mass ratio of the ethyl acrylate content to the n-butyl acrylate content in the monomer units (ethyl acrylate content (mass) / n-butyl acrylate content (mass)) is 2 or more from the viewpoint of improving the flex fatigue resistance of the crosslinked product, and may be preferably 2.1 or more, 2.2 or more, 2.3 or more, 2.5 or more, 3 or more, 3.5 or more, 3.8 or more, 4 or more, or 4.1 or more from the viewpoint of further improving the flex fatigue resistance of the crosslinked product and also improving the tensile strength of the crosslinked product. The mass ratio may be preferably 12 or less, 11 or less, 10 or less, 8 or less, 6 or less, or 5 or less from the viewpoint of improving the cold resistance of the crosslinked product.

[0017] The acrylic rubber may further contain ethylene as a monomer unit. The ethylene content may be 0.5% by mass or more, 0.7% by mass or more, or 1% by mass or more, and 5% by mass or less, 4% by mass or less, or 3% by mass or less, based on the total amount of monomer units contained in the acrylic rubber. The ethylene content may be 0.5 to 5% by mass, 0.5 to 4% by mass, 0.5 to 3% by mass, 0.7 to 5% by mass, 0.7 to 4% by mass, 0.7 to 3% by mass, 1 to 5% by mass, 1 to 4% by mass, or 1 to 3% by mass, based on the total amount of monomer units contained in the acrylic rubber.

[0018] The acrylic rubber may further contain a crosslinking monomer having a carboxyl group as a monomer unit. The crosslinking monomer is a monomer that is copolymerizable with ethyl acrylate and n-butyl acrylate and has a carboxyl group for forming a crosslinking site (also called a crosslinking point). The crosslinking monomer has a polymerizable carbon-carbon double bond, and has, for example, an acryloyl group, a methacryloyl group, an allyl group, a methallyl group, a vinyl group, or an alkenylene group.

[0019] Examples of crosslinkable monomers having a carboxyl group include acrylic acid, methacrylic acid, crotonic acid, 2-pentenoic acid, maleic acid, fumaric acid, itaconic acid, and maleic acid monoalkyl esters.

[0020] The content of the crosslinking monomer may be 0.5% by mass or more, 0.7% by mass or more, or 1% by mass or more, and 5% by mass or less, 4% by mass or less, or 3% by mass or less, based on the total amount of monomer units contained in the acrylic rubber. The content of the crosslinking monomer may be 0.5 to 5% by mass, 0.5 to 4% by mass, 0.5 to 3% by mass, 0.7 to 5% by mass, 0.7 to 4% by mass, 0.7 to 3% by mass, 1 to 5% by mass, 1 to 4% by mass, or 1 to 3% by mass, based on the total amount of monomer units contained in the acrylic rubber.

[0021] The acrylic rubber may further contain, as a monomer unit, other monomers in addition to the above-mentioned monomers.

[0022] Examples of other monomers include alkyl acrylates other than ethyl acrylate and n-butyl acrylate, alkyl methacrylates, alkoxyalkyl (meth)acrylates, fluorine-containing (meth)acrylates, hydroxyl group-containing (meth)acrylates, tertiary amino group-containing (meth)acrylates, alkyl methacrylates, alkyl vinyl ketones, vinyl ethers, allyl ethers, aromatic vinyl compounds, vinyl nitriles, vinyl halides, and vinylidene halides.

[0023] Examples of alkyl acrylates other than ethyl acrylate and n-butyl acrylate include methyl acrylate, n-propyl acrylate, isobutyl acrylate, n-pentyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-methylpentyl acrylate, n-octyl acrylate, and 2-ethylhexyl acrylate. Examples of alkyl methacrylates include methyl methacrylate and octyl methacrylate.

[0024] Examples of alkoxyalkyl (meth)acrylates include 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-(n-propoxy)ethyl (meth)acrylate, 2-(n-butoxy)ethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 2-(n-propoxy)propyl (meth)acrylate, and 2-(n-butoxy)propyl (meth)acrylate.

[0025] Examples of fluorine-containing (meth)acrylates include 1,1-dihydroperfluoroethyl (meth)acrylate, 1,1-dihydroperfluoropropyl (meth)acrylate, 1,1,5-trihydroperfluorohexyl (meth)acrylate, 1,1,2,2-tetrahydroperfluoropropyl (meth)acrylate, 1,1,7-trihydroperfluoroheptyl (meth)acrylate, 1,1-dihydroperfluorooctyl (meth)acrylate, and 1,1-dihydroperfluorodecyl (meth)acrylate.

[0026] Examples of hydroxyl group-containing (meth)acrylates include 1-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and hydroxyethyl (meth)acrylate. Examples of tertiary amino group-containing (meth)acrylates include diethylaminoethyl (meth)acrylate and dibutylaminoethyl (meth)acrylate.

[0027] Examples of alkyl vinyl ketones include methyl vinyl ketone. Examples of vinyl ethers include vinyl ethyl ether. Examples of allyl ethers include allyl methyl ether. Examples of aromatic vinyl compounds include styrene, α-methylstyrene, chlorostyrene, and vinyltoluene. Examples of vinyl nitriles include acrylonitrile and methacrylonitrile. Examples of vinyl halides include vinyl chloride and vinyl fluoride. Examples of vinylidene halides include vinylidene chloride and vinylidene fluoride.

[0028] The content of the other monomers may be 1% by mass or more and 10% by mass or less based on the total amount of monomer units contained in the acrylic rubber.

[0029] The acrylic rubber preferably does not contain methacrylate as a monomer unit, and more preferably contains only ethyl acrylate, n-butyl acrylate, ethylene, and a crosslinking monomer having a carboxyl group as a monomer unit.

[0030] The acrylic rubber can be obtained by copolymerizing the above-mentioned monomers by a known method such as emulsion polymerization or suspension polymerization, and more specifically, can be obtained by, for example, the following method.

[0031] First, a monomer mixture containing ethyl acrylate and n-butyl acrylate and an aqueous solution of an emulsifier (e.g., an aqueous polyvinyl alcohol solution) are mixed in a reaction vessel to prepare a suspension. Then, after replacing the inside of the reaction vessel with nitrogen gas, ethylene is pressurized at a pressure of, for example, 0.5 to 5 MPa as necessary. Then, while stirring the suspension, a polymerization initiator is added to the suspension to initiate polymerization, and the polymerization is allowed to proceed for, for example, 1 to 24 hours at 40 to 100°C. A coagulant (e.g., an aqueous sodium borate solution) is added to the obtained copolymer to solidify the copolymer, and the copolymer is washed with water, dehydrated, and dried in this order to obtain an acrylic rubber. When obtaining an acrylic rubber by such a method, the method of mixing the monomer mixture with an aqueous solution of an emulsifier in advance to prepare a suspension tends to result in less toluene insoluble matter, which will be described later, than the method of mixing an aqueous solution of an emulsifier to prepare a suspension in advance and then adding the monomer mixture to the suspension.

[0032] The emulsifier may be, for example, polyvinyl alcohol or other surfactants. Examples of other surfactants include salts of fatty acids such as myristic acid, palmitic acid, oleic acid, and linolenic acid, alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate, higher alcohol sulfates such as sodium lauryl sulfate, higher phosphates such as sodium alkyl phosphates, alkyl sulfosuccinates, polyoxyethylene alkyl ethers such as polyoxyethylene dodecyl ether, polyoxyethylene alkylphenol ethers such as polyoxyethylene nonylphenyl ether, polyoxyethylene alkyl esters, polyoxyethylene sorbitan alkyl esters, polyoxyethylene polyoxypropylene glycol, and polyethylene glycol monostearate. When these surfactants are used as emulsifiers, the amount of toluene insolubles tends to be further reduced compared to when polyvinyl alcohol is used as emulsifiers.

[0033] The monomer mixture may further contain, as necessary, the above-mentioned monomers constituting the acrylic rubber (excluding gaseous monomers such as ethylene) in addition to ethyl acrylate and n-butyl acrylate.

[0034] A pH adjuster may be further added to the suspension. The pH adjuster may be, for example, an alkali metal salt such as sodium acetate, sodium hydroxide, potassium hydroxide, sodium phosphate, or sodium citrate, and is preferably sodium acetate. The amount of the pH adjuster added may be, for example, 0.1 parts by mass or more and 5 parts by mass or less with respect to 100 parts by mass of the total amount of the monomers constituting the acrylic rubber.

[0035] The polymerization initiator may be, for example, an azo compound such as azobisisobutyronitrile, an organic peroxide such as tert-butyl hydroperoxide, cumene hydroperoxide, or benzoyl peroxide, or an inorganic peroxide such as sodium persulfate or ammonium persulfate, and is preferably tert-butyl hydroperoxide. The amount of the polymerization initiator added may be, for example, 0.01 parts by mass or more and 2 parts by mass or less with respect to 100 parts by mass of the total amount of the monomers constituting the acrylic rubber.

[0036] The content of the toluene insoluble matter in the acrylic rubber obtained as described above is 5% by mass or less based on the total amount of the acrylic rubber from the viewpoint of improving the flex fatigue resistance of the crosslinked product, and from the viewpoint of further improving the flex fatigue resistance of the crosslinked product, it is preferably 4.5% by mass or less, more preferably 4% by mass or less, even more preferably 3.5% by mass or less, and particularly preferably 3% by mass or less. The content of the toluene insoluble matter in the acrylic rubber is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and particularly preferably 1.5% by mass or more based on the total amount of the acrylic rubber from the viewpoint of improving the moldability of the crosslinked product.

[0037] The toluene insoluble content in the acrylic rubber is measured as follows. 1 g of acrylic rubber is precisely weighed and dissolved in 100 mL of toluene at 25°C for 48 hours, and then the solution is transferred to a 250 mL centrifuge tube whose mass (referred to as X(g)) has been measured in advance. Next, the solution is centrifuged at 10°C, 8500 rpm, and 60 minutes using an angle rotor with a maximum centrifugal radius of 13.8 cm, and the non-precipitate is removed by decantation. The precipitate in the centrifuge tube is dried in a vacuum dryer at 70°C for 24 hours, and the mass of the centrifuge tube after drying (referred to as Y(g)) is measured. The toluene insoluble content is calculated from the measured X and Y using the following formula. Toluene insolubles (mass%) = (YX) x 100

[0038] As described above, the toluene insoluble content in the acrylic rubber can be adjusted by the order of mixing when preparing a suspension by mixing the monomer mixture and the aqueous solution of the emulsifier. The toluene insoluble content in the acrylic rubber can also be adjusted by the mass ratio of the content of ethyl acrylate to the content of n-butyl acrylate in the monomer units contained in the acrylic rubber. The larger this mass ratio is, the smaller the toluene insoluble content in the acrylic rubber tends to be.

[0039] The Mooney viscosity of the acrylic rubber may be, for example, 10 or more, 20 or more, or 30 or more, and may be 70 or less, 60 or less, or 50 or less. The Mooney viscosity of the acrylic rubber is a value measured according to the method specified in JIS K6300, and specifically means a value measured using an L-type rotor at 100°C, after 1 minute of preheating, and 4 minutes after the start of rotation.

[0040] The acrylic rubber described above is used as a rubber composition in combination with other components as necessary. That is, another embodiment of the present invention is a rubber composition containing the above acrylic rubber (and other components used as necessary). The content of the acrylic rubber may be, for example, 50 mass% or more, 55 mass% or more, or 60 mass% or more, and 90 mass% or less, based on the total amount of the rubber composition.

[0041] Other components that may be included in the rubber composition include, for example, fillers, lubricants, antioxidants, surfactants, crosslinking agents, and crosslinking accelerators.

[0042] Examples of the filler include carbon black, silica, talc, and calcium carbonate. The content of the filler may be, for example, 30 parts by mass or more and 100 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.

[0043] Examples of the lubricant include liquid paraffin, stearic acid, stearylamine, fatty acid zinc, fatty acid ester, and organosilicone. The content of the lubricant may be, for example, 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.

[0044] Examples of the antioxidant include aromatic amine compounds and phenol compounds. The content of the antioxidant may be, for example, 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.

[0045] The surfactant may be, for example, an alkyl sulfate ester salt. The content of the surfactant may be, for example, 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.

[0046] Examples of the crosslinking agent include an imidazole compound and a diamine compound. The content of the crosslinking agent may be, for example, 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.

[0047] The crosslinking accelerator is preferably used when the rubber composition contains a crosslinking agent. Examples of the crosslinking accelerator include a trimethylthiourea compound, a phenothiazine compound, and a guanidine compound. The content of the crosslinking accelerator may be, for example, 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the acrylic rubber.

[0048] The rubber composition is preferably used in a crosslinked state (as a crosslinked product). That is, another embodiment of the present invention is a crosslinked product of the above-mentioned rubber composition. The crosslinked product is obtained by crosslinking the rubber composition. In the crosslinked product, crosslinks between the acrylic rubbers are formed by crosslinking sites (crosslinking points) of the crosslinking site monomer contained as a monomer unit in the acrylic rubber. When the rubber composition contains a crosslinking agent, crosslinks between the acrylic rubbers are further formed by the crosslinking agent.

[0049] The method for crosslinking the rubber composition may be a known method, and may, for example, include a first crosslinking step of heating and pressurizing the rubber composition, and a second crosslinking step of further heating the rubber composition after the first crosslinking step.

[0050] In the first crosslinking step, the heating temperature may be, for example, 150° C. or higher and 220° C. or lower. The pressure during pressing may be, for example, 0.4 MPa or higher and 20 MPa or lower. The time for which heating and pressing are performed may be, for example, 5 minutes or longer and 2 hours or shorter.

[0051] In the second crosslinking step, the heating temperature may be, for example, 150° C. or more and 220° C. or less. The heating time may be, for example, 30 minutes or more and 24 hours or less.

[0052] The cross-linked product of the rubber composition is preferably used as a rubber hose or a sealing part such as a gasket or packing, and is particularly preferably used as a rubber hose. That is, another embodiment of the present invention is a rubber hose or a sealing part containing the above-mentioned cross-linked product, and preferably a rubber hose containing the above-mentioned cross-linked product. The rubber hose and the sealing part may be composed only of the cross-linked product of the rubber composition, or may include the cross-linked product and other parts.

[0053] Examples of rubber hoses include transmission oil cooler hoses for automobiles, construction machinery, hydraulic equipment, etc., engine oil cooler hoses, air duct hoses, turbo intercooler hoses, hot air hoses, radiator hoses, power steering hoses, fuel system hoses, and drain system hoses.

[0054] Examples of sealing parts include engine head cover gaskets, oil pan gaskets, oil seals, lip seal packings, O-rings, transmission seal gaskets, crankshafts, camshaft seal gaskets, valve stems, power steering seal belt cover seals, constant velocity joint boot materials, and rack and pinion boot materials. EXAMPLES

[0055] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0056] <Examples 1 to 5> In a pressure-resistant reaction vessel having an internal volume of 40 liters, 11 kg of a monomer mixture containing the monomers shown in Table 1 (excluding ethylene), 17 kg of a 4 mass% aqueous solution of polyvinyl alcohol, and 22 g of sodium acetate were charged and mixed thoroughly in advance with a stirrer to prepare a uniform suspension. After replacing the air in the upper part of the vessel with nitrogen, ethylene was pressed into the upper part of the vessel at a pressure of 3 MPa (except for Example 5). Stirring was continued and the vessel was kept at 55°C, and then 2 liters of an aqueous t-butyl hydroperoxide solution (0.25 mass%) was added to start polymerization. The temperature in the vessel was kept at 55°C, and the reaction was terminated after 6 hours. 7 liters of an aqueous sodium borate solution (3.5 mass%) was added to the obtained copolymer to solidify the copolymer. The solidified copolymer was washed with water, and then dehydrated and dried to obtain an acrylic rubber.

[0057] <Comparative Examples 1 and 2> In a pressure-resistant reaction vessel with an internal volume of 40 liters, 17 kg of a 4% by mass aqueous solution of polyvinyl alcohol and 22 g of sodium acetate were charged and mixed thoroughly in advance with a stirrer to prepare a uniform suspension. After replacing the air in the upper part of the vessel with nitrogen, ethylene was pressed into the upper part of the vessel at a pressure of 3 MPa. Stirring was continued, and the vessel was kept at 55°C, and then 11 kg of a monomer mixture containing the monomers shown in Table 1 (excluding ethylene) and 2 liters of an aqueous t-butyl hydroperoxide solution (0.25% by mass) were added over 6 hours to initiate polymerization. The temperature in the vessel was kept at 55°C, and the reaction was terminated after 6 hours. 7 liters of an aqueous sodium borate solution (3.5% by mass) was added to the obtained copolymer to solidify the copolymer. The solidified copolymer was washed with water, and then dehydrated and dried to obtain an acrylic rubber.

[0058] <Comparative Example 3> In a pressure-resistant reaction vessel with an internal volume of 40 liters, 1 kg of a monomer mixture containing the monomers shown in Table 1 (excluding ethylene), 17 kg of a 4 mass% aqueous solution of polyvinyl alcohol, and 22 g of sodium acetate were charged and mixed thoroughly in advance with a stirrer to prepare a uniform suspension. After replacing the air in the upper part of the vessel with nitrogen, ethylene was pressed into the upper part of the vessel at a pressure of 3 MPa. After continuing the stirring and maintaining the inside of the vessel at 55°C, 10 kg of a monomer mixture containing the monomers shown in Table 1 (excluding ethylene) and 2 liters of an aqueous t-butyl hydroperoxide solution (0.25 mass%) were added over 6 hours to initiate polymerization. The temperature inside the vessel was maintained at 55°C, and the reaction was terminated after 6 hours. 7 liters of an aqueous sodium borate solution (3.5 mass%) was added to the obtained copolymer to solidify the copolymer. The solidified copolymer was washed with water, dehydrated and dried to obtain an acrylic rubber.

[0059] The composition of the monomer units contained in the obtained acrylic rubber is shown in Table 1. The content of the monomer units was measured by nuclear magnetic resonance spectroscopy.

[0060] In addition, the content of toluene insoluble matter in the obtained acrylic rubber and the Mooney viscosity ML(1+4)100° C. of the acrylic rubber were measured. The results are shown in Table 1.

[0061] The toluene insoluble matter was measured by the following method. That is, first, 1 g of acrylic rubber was precisely weighed and dissolved in 100 mL of toluene at a temperature of 25 ° C. for 48 hours, and then the solution was transferred to a centrifuge tube with a capacity of 250 mL whose mass (referred to as X (g)) had been measured in advance. Next, the solution was centrifuged at a temperature of 10 ° C., 8500 rpm, and 60 minutes using an angle rotor with a maximum centrifugal radius of 13.8 cm, and the non-precipitate was removed by decantation. The precipitate in the centrifuge tube was dried in a vacuum dryer at a temperature of 70 ° C. for 24 hours, and the mass (referred to as Y (g)) of the centrifuge tube after drying was measured. The toluene insoluble matter was calculated from the measured X and Y using the following formula. Toluene insolubles (mass%) = (YX) x 100

[0062] The Mooney viscosity ML(1+4)100°C was measured according to the method specified in JIS K6300.

[0063] Subsequently, 100 parts by mass of each of the obtained acrylic rubbers, 45 parts by mass of a filler (carbon black (Tokai Carbon Co., Ltd., SEATO)), 1 part by mass of a lubricant a (liquid paraffin (Kaneda Co., Ltd., Hicol K-230)), 1 part by mass of a lubricant b (paraffin wax (Nippon Seiro Co., Ltd., Paraffin Wax 135F)), 1 part by mass of a lubricant c (stearic acid (NOF Corporation)), 0.3 parts by mass of a lubricant d (stearylamine (Kao Corporation, Farmin 80)), 0.5 parts by mass of an antioxidant a (4,4'-bis(α,α-dimethylbenzyl)diphenylamine (Addivant Corporation, Naugard #445)), 1 part by mass of an antioxidant b (N-phenyl-N'-isopropyl-p-phenylenediamine (Ouchi Shinko Chemical Industry Co., Ltd., Nocrac 810-NA)), and a release agent (phosphate ester compound (Tomoe Engineering Co., Ltd., A rubber composition was obtained by kneading 0.5 parts by mass of Moldwith INT-21G), 0.7 parts by mass of a crosslinking agent (hexamethylenediamine carbamate (Diak#1 manufactured by Du Pont)), and 1.5 parts by mass of a crosslinking accelerator (XLA-60 manufactured by Lanxess) with an 8-inch open roll.

[0064] The obtained rubber composition was cut into a sheet having a thickness of 2.4 mm, and then heated and pressed at 170°C and a pressure of 10 MPa for 20 minutes using a press vulcanizer. Then, the rubber composition was heated in a gear oven at 170°C for 4 hours to obtain a crosslinked product of the rubber composition.

[0065] (Evaluation of tensile strength of cross-linked product) The tensile strength of the crosslinked product was measured in accordance with JIS K6251:2010.

[0066] (Evaluation of flexural fatigue resistance of cross-linked products) According to JIS-K6260:2010, the number of times the crosslinked material was bent until a 0.5 mm crack was generated was measured in environments of 23°C and 100°C. The number of times the crosslinked material was bent was the average value of the results of similar measurements performed on five samples. The higher the number of times the crosslinked material was bent, the better the resistance to bending fatigue.

[0067] (Evaluation of cold resistance of cross-linked products) The T100 of the crosslinked product was measured according to JIS K6261:2006. T100 means the temperature at which the specific modulus of the crosslinked product is 100 times the value at 23° C. The lower the T100, the better the cold resistance.

[0068] (Evaluation of moldability) The rubber composition obtained was molded into a tube (inner diameter: 9 mm, outer diameter: 14 mm) using a rubber single-screw extruder (screw diameter: 50 mm) under the following conditions: screw rotation speed: 20 rpm, head temperature: 110° C., cylinder temperature: 90° C., and hopper temperature: 70° C. The mass W (g), length L (cm) in the extrusion direction, and density ρ (g / cm 3 ) was measured, and the die swell (DS) (%) was calculated according to the following formula. DS=(W / LρS0-1)×100 where S0 is the die area (cm 2 The smaller the die swell, the better the formability.

[0069] The results of the above evaluations are shown in Table 1.

Table 1

Claims

1. An acrylic rubber containing ethyl acrylate and n-butyl acrylate as monomer units and containing a toluene-insoluble matter, a mass ratio of the content of the ethyl acrylate to the content of the n-butyl acrylate is 3 or more; The acrylic rubber (excluding acrylic rubber used in a tire bladder) has a toluene-insoluble content of 4.2 mass% or less based on the total amount of the acrylic rubber.

2. 2. The acrylic rubber of claim 1, which does not contain methacrylate as a monomer unit.

3. 3. The acrylic rubber according to claim 1 or 2, further comprising ethylene as a monomer unit.

4. The acrylic rubber according to any one of claims 1 to 3, further comprising, as a monomer unit, a crosslinkable monomer having a carboxyl group.

5. 2. The acrylic rubber according to claim 1, comprising, as monomer units, only the ethyl acrylate, the n-butyl acrylate, ethylene, and a crosslinking monomer having a carboxyl group.

6. The acrylic rubber according to claim 5, wherein the content of the ethyl acrylate is 70 to 90 mass% based on the total amount of the monomer units.

7. The acrylic rubber according to claim 5 or 6, wherein the content of the n-butyl acrylate is 10 to 30 mass% based on the total amount of the monomer units.

8. The acrylic rubber according to any one of claims 5 to 7, wherein the ethylene content is 0.5 to 5 mass% based on the total amount of the monomer units.

9. The acrylic rubber according to any one of claims 5 to 8, wherein the content of the crosslinking monomer is 0.5 to 5 mass% based on the total amount of the monomer units.

10. A rubber composition (excluding rubber compositions used for tire bladders) comprising the acrylic rubber according to any one of claims 1 to 9.

11. A crosslinked product of the rubber composition according to claim 10 (excluding the crosslinked product used for a tire bladder).

12. A rubber hose comprising the cross-linked product according to claim 11.

Citation Information

Patent Citations

  • Process for preparation of carboxyl group-containing rubber

    JP2002187901A

  • Acrylic rubber composition and heat-resistant hose

    JP2003082029A

  • Acrylic rubber composition

    JP2011006509A

  • Acrylic rubber composition and rubber crosslinked product

    JP2012211239A

  • Tire bladder

    WO2012099117A1