Method for forming doped metal oxide thin films on electrodes for intermediate phase control

Doped metal oxide layers on cathode materials address SEI instability and transition metal dissolution in lithium-ion batteries, enhancing stability and performance through controlled porosity and ionic conductivity.

JP7596409B2Active Publication Date: 2024-12-09LAIR LIQUIDE SA POUR LETUDE & LEXPLOITATION DES PROCEDES GEORGES CLAUDE
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022578650
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-25
Filing Date
2021-06-22
Publication Date
2024-12-09
Estimated Expiration
2041-06-22

AI Technical Summary

Technical Problem

Current lithium-ion batteries face issues such as non-uniform and unstable solid electrolyte interface (SEI) formation, leading to capacity reduction, physical cracking, lithium dendrite formation, and intercalation barriers, while high nickel cathode materials suffer from transition metal dissolution and SEI destabilization, causing rapid battery degradation.

Method used

Deposition of doped metal oxide layers on cathode materials using ALD or CVD to protect against electrolyte decomposition and transition metal dissolution, enhancing electrochemical performance by allowing Li ion diffusion through controlled porosity and ionic conductivity.

Benefits of technology

The doped metal oxide layers improve battery stability and capacity retention by reducing SEI degradation and transition metal dissolution, maintaining high electrochemical activity and capacity over multiple cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596409000001
    Figure 0007596409000001
  • Figure 0007596409000002
    Figure 0007596409000002
  • Figure 0007596409000003
    Figure 0007596409000003
Patent Text Reader

Abstract

The present invention provides a novel solution for forming an artificial intermediate phase on an electrode to protect it from rapid degradation of its electrochemical properties by depositing a doped metal oxide layer by ALD or CVD. The metals considered here are the IVA-VIA elements (Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W), and the dopants, including B, Al, C, Si, N, P, and S, allow the oxide network to be porous, which can be promoted by the presence of the dopant. The film must also be thin, possibly discontinuous, and sufficiently lithium-ion conductive, so that the addition of this thin-film interface allows for fast lithium-ion transport at the electrode-electrolyte interface.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 043,611, filed June 24, 2020, and U.S. Provisional Patent Application No. 63 / 044,008, filed June 25, 2020, the entire contents of which are incorporated herein by reference. [Background technology]

[0002] During the first cycle of a lithium-ion battery, the formation of a solid electrolyte interface (SEI) on the anode and / or cathode is observed from the decomposition of the electrolyte at the electrolyte / electrode interface. The initial capacity decline of a lithium-ion battery occurs as a result of the consumption of lithium during the formation of this SEI. Furthermore, the formed SEI layer is non-uniform and unstable, and is not efficient for passivating the electrode surface against the degradation of the electrode active material due to the continuous decomposition of the electrolyte. The SEI layer may undergo physical cracking during the cycling of the battery, and lithium dendrites may form, leading to short circuits and subsequent thermal runaway. Furthermore, the SEI layer also creates a barrier potential that makes the intercalation of lithium ions in the electrode more difficult.

[0003] In current designs, lithium-ion batteries use (lithium) metal oxide, phosphate or fluoride coatings (e.g., Al) on the surfaces of the electrodes and / or electrode active materials by wet coating, dry coating or sputtering of continuous films of metal oxides and / or phosphates to stabilize the interphase between the electrode and the electrolyte. x O y , Li x M y PO z , M=Nb, Zr, AlTi, etc. or AlM x F yM=W, Y, etc. Lithium-containing thin films are known for their use as surface coating layers of electrode materials in lithium-ion battery applications. Examples of lithium-containing thin films include LiPON, lithium phosphate, lithium borate, lithium borophosphate, lithium niobate, lithium titanate, lithium zirconium oxide, etc. Surface coating of electrodes by ALD / CVD techniques is a preferred means of forming the above-mentioned solid electrolyte interfacial thin films, thus avoiding the formation of these unstable layers. However, deposition of lithium-containing films is difficult to carry out due to the lack of suitable lithium precursors for mass production. Most are not volatile, are not stable enough, and they may contain undesirable impurities. Another important application of mesophase thin films is in the formation of solid electrolyte materials used in solid-state batteries. Solid-state batteries are solvent-free systems with longer service life, faster charging times, and higher energy density than conventional lithium-ion batteries. They are considered to be the next technological step in battery development. ALD / CVD techniques can also provide uniform and conformal electrode / electrolyte interfacial thin films on complex structures such as 3D batteries.

[0004] Silicon anodes are also in the scope of mesophase thin film applications. Silicon is considered to be the next generation of anodes in the development of lithium-ion batteries, and graphite anodes (Li + / Li) at the same potential level (0.05V vs. + / Li at 0.2 V) with a graphite anode (372 mAhg -1 ) with higher specific capacity (3600mAhg -1 The main drawback of silicon anodes is their volume expansion of up to 300% during charge / discharge, leading to destabilization of the SEI and physical cracking of the electrode.

[0005] The application of thin film mesophases can be extended to lithium metal anode technology. Lithium metal anodes are considered to be post-lithium ion batteries (LIBs) because they can provide at least three times the theoretical capacity compared to LIBs. Lithium metal is also attracting attention due to its high capacity (10 times that of graphite), reduced battery volume, and process simplicity. However, uncontrolled lithium metal surfaces can lead to the growth of Li dendrites, which can cause short circuits and ultimately fires.

[0006] For next-generation cathode active materials, much research has been focused on identifying and developing metal oxide cathode materials. Among the wide range of layered oxides, high-Ni cathode materials such as NMC (nickel-lithium manganese cobalt oxide) and NCA (nickel-lithium cobalt aluminum oxide) are the most promising current candidates for practical application. However, high-Ni cathode materials tend to become amorphous when high voltages are applied. One of the main drawbacks of these metal oxide materials is the continuous dissolution of transition metals, especially nickel, due to parasitic reactions of the cathode material with the electrolyte. This leads to structural degradation of the cathode active material along with gas (O2) evolution at the electrode / electrolyte interface during charging of the battery. Furthermore, the dissolved nickel ions migrate to the anode side, and their deposition on the anode surface causes rapid decomposition of the SEI in the anode, ultimately leading to the failure of the battery.

[0007] Spinel cathode materials have been extensively investigated for their high rate capability and low or zero cobalt content. One of the main issues with spinel cathode materials such as LMO (lithium manganese oxide), LNMO (lithium nickel manganese oxide) is the dissolution of divalent manganese ions (2Mn 3+ →Mn 4+ +Mn 2+ ), which occurs primarily at the electrode / electrolyte interface followed by redeposition on the anode and destruction of its SEI as by the same mechanism for high Ni cathode materials.

[0008] Deposition of thin films on the cathode and / or cathode materials can be used to address interface issues between the electrolyte and the cathode electrode, such as dissolution of transition metals, excessive electrolyte decomposition, etc. For example, US Patent No. 8,535,832 B2 discloses wet coating of metal oxides (Al2O3, Bi2O3, B2O3, ZrO2, MgO, Cr2O3, MgAl2O4, Ga2O3, SiO2, SnO2, CaO, SrO, BaO, TiO2, Fe2O3, MoO3, MoO2, CeO2, La2O3, ZnO, LiAlO2 or combinations thereof) onto cathode active materials containing Ni, Mn and Co. US Patent No. 9,543,581 B2 discloses dry coating of amorphous Al2O3 onto precursor particles of cathode active materials containing Ni, Mn and Co elements. U.S. Pat. No. 9,614,224 B2 describes the deposition of Li on a cathode active material containing Mn using a sputtering method. x PO y Mn z Coatings are described. US Patent No. 9,837,665 B2 describes lithium phosphate oxynitride (LiPON) thin film coatings using a sputtering method on cathode active materials including Li, Mn, Ni, and oxygen-containing compounds with at least one dopant of Ti, Fe, Ni, V, Cr, Cu, and Co. US Patent No. 9,196,901 B2 describes Al2O3 thin film coatings using an atomic layer deposition (ALD) method on cathode stacks and cathode active materials including Co, Mn, V, Fe, Si, or Sn and being oxides, phosphates, silicates, or mixtures of two or more thereof. US Patent No. 10,224,540 B2 describes Al2O3 thin film coatings using an ALD method on porous silicon anodes. US Patent No. 10,177,365 B2 describes AlW thin film coatings using ALD on cathode active materials including LiCoO2. x F y Or AlW x F y C z Thin film coatings are described. US Pat. No. 9,531,004 B2 describes lithium titanate Li (4+x) Ti5O 12Hybrid thin film coatings including a first layer of Al2O3, TiO2, SnO2, V2O5, HfO2, ZrO2, ZnO and a second layer of fluoride-, carbide-, and nitride-based coatings using ALD methods on anode materials consisting of (0≦x≦3) (LTO), graphite, silicon, silicon-containing alloys, tin-containing alloys, and combinations thereof are described. Summary of the Invention [Means for solving the problem]

[0009] The present invention provides the following solution, by depositing, by ALD or CVD, doped metal oxide layers on the cathode or cathode active material, forming an artificial intermediate phase on the electrode to protect it from a rapid degradation of its electrochemical properties. These doped metal oxide layers reduce the excessive decomposition of the electrolyte at the electrode / electrolyte interface during the SEI formation, reducing the capacity loss in the first cycle. The presence of such doped metal oxide layers also reduces the dissolution of the transition metal cations of the cathode active material, caused by parasitic reactions between the electrolyte and the cathode active material, and then their redeposition on the anode. The electrochemical activity of the battery is thereby improved. As described above, other types of membranes have been proposed, in particular high-purity metal oxides such as Al2O3. However, this type of material acts as an ionic insulator and therefore does not allow the best electrochemical performance of the obtained cathode and battery. The composition of the doped metal oxide layer takes into account the need for diffusion of Li ions, by the choice of a transition metal that can undergo a change of oxidation number. The corresponding metal oxides are deposited using vapor phase metal precursors containing dopants such as C, Si, Sn, B, Al, N, P, and / or S, together with separate dopant chemistries. The deposition conditions are selected to produce doped metal oxide films rather than metal oxide films. Without wishing to be bound by any particular theory, doped metal oxide films would be considered to be "low quality" films that are not suitable for most applications in most circumstances. For example, such materials are generally low density due to porosity caused by the dopant elements (especially carbon and phosphorus). However, it may be such porosity that aids in the balance between protecting the cathode and allowing the movement of Li ions. Also, the addition of first row transition elements, preferably Mn, Ni, Co, Fe, Cu, can increase the ionic conductivity of the film, thereby improving the electrochemical performance.

[0010] The present invention can be further understood in connection with the following non-limiting exemplary embodiments, which are set forth as enumerated sentences:

[0011] 1. A cathode or cathode active material comprising at least a partial surface coating of a doped metal oxide film, preferably wherein the metal is selected from niobium, tantalum, vanadium, zirconium, titanium, hafnium, tungsten, molybdenum, chromium and combinations thereof.

[0012] 2. The cathode or cathode active material of claim 1, wherein the doped metal oxide film is either a metal, oxygen and carbon containing film or a metal, oxygen and phosphorus containing film.

[0013] 3. The cathode or cathode active material according to claim 1, wherein the doped metal oxide film is a doped niobium oxide film.

[0014] 4. The cathode or cathode active material according to claim 1, wherein the doped metal oxide film is a niobium, oxygen and carbon containing film or a niobium, oxygen and phosphorus containing film.

[0015] 5. The cathode or cathode active material according to any one of claims 1 to 4, wherein the cathode or cathode active material is only partially coated with a doped metal oxide film.

[0016] 6. The cathode or cathode active material according to any one of claims 1 to 5, wherein the doped metal oxide film has an average thickness of 0.02 nm to 10 nm, preferably 0.1 nm to 5 nm, and most preferably 0.2 to 2 nm.

[0017] 7. The cathode or cathode active material according to any one of paragraphs 1 to 4, wherein the doped metal oxide film has an atomic percentage of carbon atoms of 5% to 50%, preferably 10% to 30%, and most preferably 15 to 25%.

[0018] 8. The cathode or cathode active material according to any one of claims 3 to 7, wherein the doped metal oxide film has a refractive index of 1.5 to 2.5, preferably 1.6 to 2.1, and most preferably 1.7 to 2.0.

[0019] 9. Doped metal oxides are called MxO y D z wherein M is a transition metal or an element II-A to VI-B, O is oxygen, and D is a dopant atom other than lithium, M or O, preferably D is selected from C, Si, Sn, B, Al, N, P, or S, and x=10-60%, y is in the range of 10-60%, and z is in the range of 5-50%, preferably 10-30%.

[0020] 10. The cathode or cathode active material of sentence 9, wherein the cathode or cathode active material is only partially coated with the doped metal oxide film.

[0021] 11. The cathode or cathode active material according to sentence 9 or 10, wherein the doped metal oxide film has an average thickness of 0.02 nm to 10 nm, preferably 0.1 nm to 5 nm, and most preferably 0.2 to 2 nm.

[0022] 12. The cathode or cathode active material according to any one of paragraphs 9 to 11, wherein the doped metal oxide film has an atomic percentage of carbon atoms of 5% to 50%, preferably 10% to 30%, and most preferably 15 to 25%.

[0023] 13. The cathode or cathode active material according to any one of claims 9 to 12, wherein the doped metal oxide film has a refractive index of 1.5 to 2.5, preferably 1.6 to 2.1, and most preferably 1.7 to 2.0.

[0024] 14. A proton exchange membrane battery comprising the cathode or cathode active material according to any one of claims 1 to 13.

[0025] 15. A method for coating a cathode or cathode active material with a doped metal oxide film, comprising the steps of: a1. exposing a cathode or a cathode active material to vapor of a chemical precursor; A method comprising the step b1. depositing a doped metal oxide film on a cathode or cathode active material.

[0026] 16. The method of claim 15, further comprising step a2. exposing the cathode or cathode active material to a co-reactant.

[0027] 17. The method of sentence 16, wherein step a1 of exposing the cathode or cathode active material to vapor of a chemical precursor and step a2 of exposing the cathode or cathode active material to a co-reactant are performed sequentially.

[0028] 18. The method of sentence 17, further comprising the step a1.i of purging the vapor of the chemical precursor prior to step a2 of exposing the cathode or cathode active material to the co-reactant.

[0029] 19. The method of claim 18, wherein step b1. of depositing a doped metal oxide film on the cathode or cathode active material comprises an atomic layer deposition process.

[0030] 20. The method of claim 18, wherein step b1. of depositing a doped metal oxide film on the cathode or cathode active material comprises a chemical vapor deposition process.

[0031] 21. The method according to any one of claims 15 to 20, wherein the co-reactant is O2, O3, H2O, H2O2, NO, NO2, N2O or NOx; an oxygen source such as an oxygen-containing silicon precursor, an oxygen-containing tin precursor, trimethyl phosphate, a phosphate such as diethyl phosphoramidate, or a sulfate.

[0032] 22. The doped metal oxide film produced by step b1. is MxO y D zwherein M is a transition metal or an element II-A to VI-B, preferably M is selected from niobium, tantalum, vanadium, tungsten, molybdenum, chromium, hafnium, zirconium, titanium, and combinations thereof, O is oxygen, and D is a dopant atom other than lithium, M, or O, preferably D is selected from C, Si, Sn, B, Al, N, P, or S, and x=0.1 to 0.3, y=0.3 to 0.65, and z=0.1 to 0.3.

[0033] 23. The method of any one of sentences 15 to 22, in which one or more steps are repeated.

[0034] 24. The method according to any one of sentences 15 to 23, wherein the temperature of the vapor of the chemical precursor and / or the cathode or cathode active material is 200°C or less, preferably 50°C to 200°C, more preferably 100°C to 200°C, and even more preferably 100°C to 150°C.

[0035] 25. The method according to any of sentences 15 to 24, wherein the cathode active material, or the cathode active material in the cathode, is selected from the group consisting of: a) layered oxides, such as high Ni cathode materials, such as NMC (lithium cobalt manganese nickel oxide) and NCA (lithium cobalt aluminum nickel oxide); b) spinel cathode materials, such as LMO (lithium manganese oxide), LNMO (lithium manganese nickel oxide); c) olivine structured cathode materials, in particular olivine phosphate types, such as LCP (lithium cobalt phosphate), LNP (lithium nickel phosphate); and combinations thereof.

[0036] For a further understanding of the nature and objects of the present invention, reference should be made to the following detailed description taken in conjunction with the accompanying drawings, in which like elements are given the same or similar reference numerals, and in which: [Brief description of the drawings]

[0037] [Figure 1]We demonstrate the long-term cyclic performance at 1 C (first three preliminary cycles at 0.2 C) of the deposition of NbOC thin films on NMC622 powder using NbCp(=NtBu)(NMe2)2 ("Nab") / HO using a powder ALD (PALD) reactor. [Diagram 2] Normalized long-term cyclic performance (normalized to their original discharge capacity at 1 C) of deposition of NbOC thin films on NMC622 powder using NbCp(=NtBu)(NMe2)2 ("Nab") / HO using a powder ALD (PALD) reactor is shown. [Diagram 3] 1 shows the C-rate performance of deposition of NbOC thin films on NMC622 powder using NbCp(=NtBu)(NMe2)2 ("Nab") / HO using a powder ALD (PALD) reactor. [Figure 4] FIG. 1 shows the normalized C-rate performance (normalized to their original discharge capacity at 0.2 C) of the deposition of NbOC thin films on NMC622 powder using NbCp(=NtBu)(NMe) (“Nab”) / HO using a powder ALD (PALD) reactor. [Diagram 5] 1 shows SEM images of pristine and NbOC formed using NbCp(=NtBu)(NMe2)2 ("Nab") / H2O by Powder ALD (PALD)-100C-20Cy before and after battery cycling. [Figure 6] 1 shows the long-term cyclic performance at 1 C (first three preparatory cycles at 0.2 C) of the ALD method of depositing NbOC thin films on an NMC622 electrode (EALD) using NbCp(=NtBu)(NMe2)2 ("Nab") / HO. [Figure 7] 1 shows the normalized long-term cyclic performance (normalized to their original discharge capacity at 1C) of NbOC thin films deposited on NMC622 electrodes (EALD) by ALD using NbCp(=NtBu)(NMe2)2 ("Nab") / HO. [Figure 8] FIG. 1 shows the C-rate performance of NbOC thin films on NMC622 electrodes using NbCp(=NtBu)(NMe2)2 ("Nab") / H2O. [Figure 9] FIG. 1 shows the normalized C-rate performance (normalized to their original discharge capacity at 0.2 C) of NbOC thin films on ALD-based NMC622 electrodes (EALD) using NbCp(=NtBu)(NMe2)2 ("Nab") / HO. [Figure 10] 1 shows the long-term cycling performance at 1C (first three preparatory cycles at 0.2C) of NbOCP thin films on NMC622 electrodes (ECVD) using Nb(=NtBu)(NMe2)2(OEt) ("Nau"), TMPO, and O3. [Figure 11] Normalized long-term cycling performance (normalized to their original discharge capacity at 1C) of NbOCP thin films on CVD-based NMC622 electrodes (ECVD) using Nb(=NtBu)(NMe2)2(OEt) (“Nau”) / TMPO / O3 is shown. [Figure 12] 1 shows the C-rate performance of the deposition of NbOCP thin films on NMC622 electrodes (ECVD) using Nb(=NtBu)(NMe2)2(OEt) (“Nau”) / TMPO / O3. [Figure 13] 1 shows the normalized C-rate performance (normalized to their original discharge capacity at 0.2 C) of the deposition of NbOCP thin films on NMC622 electrodes (ECVD) using Nb(=NtBu)(NMe2)2(OEt) (“Nau”) / TMPO / O3. [Figure 14] “ZrCp” e.g., ZrCp(NMe2)3 / O3 is used to show the long-term cycling performance at 1C (first three preparatory cycles at 0.2C) of ALD-scheme ZrOC thin films on LNMO electrodes. [Figure 15] Normalized long-term cyclic performance (normalized to their original discharge capacity at 1C) of ALD-based ZrOC thin films on LNMO electrodes using “ZrCp”, e.g., ZrCp(NMe2)3 / O3. [Figure 16] “ZrCp” shows the C-rate performance of ZrOC thin films on LNMO electrodes using, for example, ZrCp(NMe2)3 / O3. [Figure 17]Figure 1 shows the normalized C-rate performance (normalized to their original discharge capacity at 0.2 C) of ZrOC thin films on ALD-based LNMO electrodes using ZrCp(NMe2)3 / O3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] The present disclosure provides a solution to form an interphase on an electrode to protect it from rapid degradation of its electrochemical properties. The interphase is formed on the cathode active material before or after its introduction into the final cathode. A doped metal oxide layer is simultaneously formed by chemical vapor deposition (CVD) or atomic layer deposition (ALD) using volatile precursors delivered in sequence and / or by pulsing of the vapor phase of the precursors.

[0039] As used herein, "doped metal oxide" and "doped metal oxide film" refer to a transition metal oxide film having one or more additional elements in an atomic ratio of MxOyDz, where M=the aggregate moiety of the transition metal, O is oxygen, and D is the aggregate moiety of other elements that dope the film, such as carbon and phosphorus. Typically, x is in the range of 10-60%, y is in the range of 10-60%, and z is in the range of 5-50%, preferably 10-30%.

[0040] Preferably, M is a transition metal that forms one or more stable ions with incompletely filled d-orbitals. In particular, M may be one or more of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, or W.

[0041] Preferably, at least one D is selected from C, Si, Sn, B, N, P, or S, more preferably carbon and / or phosphorus. Other possible Ds may include Al, Mn, Co, Fe, and Cu. Particular preferred doped metal oxide layers include C-containing titanium oxide, Si-containing titanium oxide, P-doped titanium oxide, C-containing zirconium oxide, Si-containing zirconium oxide, P-doped zirconium oxide, C-containing niobium oxide, Si-containing niobium oxide, P-doped niobium oxide.

[0042] The doped metal oxide film is formed by a CVD or ALD process that deposits a doped metal oxide layer on the cathode active material before, during, or after its introduction into the final cathode intermediate manufacturing step. The doped metal oxide film can be a continuous film that completely coats the cathode active material before inclusion in the cathode, for example by powder ALD of the powdered cathode active material. The film can be discontinuous, either by controlled deposition conditions that limit film growth or as a result of the cathode active material being introduced into the cathode such that only a portion of its surface is subjected to the CVD or ALD deposition process. Typically, the doped metal oxide film has an average thickness of 0.125 to 10 nm, for example 0.125 nm to 1.25 nm, preferably 0.3 nm to 4 nm.

[0043] A doped metal oxide deposit may be deposited on the electrode consisting of: • layered oxides, preferably "NMC" (nickel lithium manganese cobalt oxide), NCA (nickel lithium aluminum cobalt oxide) or LNO (lithium nickel oxide); • spinels, preferably LNMO (lithium nickel manganese oxide) or LMO (lithium manganese oxide); ● Olivine (lithium metal phosphate, metals can be iron, cobalt, manganese); ● A form of carbon anode, such as graphite, doped or undoped; ● Silicon anode, ● Tin anode, Silicon-tin anodes, or ● Lithium metal.

[0044] Deposition can be performed on electrode active material powder, on electrode active material porous material, on different shapes of electrode active material, or in a preformed electrode where the electrode active material can already be mixed with conductive carbon and / or binder and already supported by a current collector foil.

[0045] "Cathode" in a lithium-ion battery refers to the positive electrode in an electrochemical cell (battery) where reduction of the cathode material occurs by insertion of electrons and lithium ions during charging. During discharging, the cathode material is oxidized by releasing electrons and lithium ions. Lithium ions move from the cathode to the anode in the electrochemical cell through the electrolyte, or vice versa, while electrons move through an external circuit. The cathode is generally composed of a cathode active material (i.e., lithiated metal layered oxide) and a conductive carbon black agent (acetylene black Super C65, Super P) and a binder (PVDF, CMC).

[0046] A "cathode active material" is a major element in the composition of a cathode (positive electrode) for a battery cell. Cathode active materials are, for example, cobalt, nickel, and manganese in a crystalline structure, such as a layered structure, forming a multi-metal oxide material into which lithium is intercalated. Examples of cathode active materials are layered lithium cobalt manganese nickel oxide (LiNixMnyCozO2), spinel lithium manganese oxide (LMn2O4), and olivine lithium iron phosphate (LiFePO4).

[0047] Doped metal oxide films are formed by CVD or ALD using vapors of one or more chemical precursors that contribute to the final film formation. Any suitable precursors can be selected for use in forming metal oxides or doped metal oxides used for other applications based on their known applicability. Generally, known precursors of metal oxides are used in characteristic CVD or ALD process parameters to produce doped metal oxides. Such parameters include, for example, lower vapor and / or substrate temperatures compared to deposition of metal oxides that intentionally produce "low quality" films with carbon content greater than 1%, relatively low refractive index compared to metal oxides, and / or higher levels of porosity (and therefore lower density) compared to comparable metal oxides.

[0048] A wide variety of precursors can be suitably used to form doped metal oxides under optimized deposition conditions.

[0049] Preferred IVA metal precursors are: M(OR)4, each R is independently a C1 to C6 carbon chain (linear or branched), most preferably M(OMe)4, M(OiPr)4, M(OtBu)4, M(OsBu)4 ● M(NR 1 R 2 )4, each R 1 and R 2 are independently C1 to C6 carbon chains (linear or branched), most preferably M(NMe2)4, M(NMeEt)4, M(NEt2)4 ● ML(NR 1 R 2 )3, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, or cyclooctadienyl, and each R 1 and R 2 are independently a C1 to C6 carbon chain (linear or branched), most preferably MCp(NMe2)3, M(MeCp)(NMe2)3, M(EtCp)(NEt2)3, MCp*(NMe2)3, MCp(NMe2)3, M(MeCp)(NMe2)3, M(EtCp)(NEt2)3, MCp*(NMe2)3, M(iPrCp)(NMe2)3, M(sBuCp)(NMe2)3, M(tBuCp)(NMe2)3, N(secPenCp)(NMe2)3, M(nPrCp)(NMe2)3 ● ML(OR)3, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl, and each R is independently a C1-C6 carbon chain (linear or branched), most preferably MCp(OiPr)3, M(MeCp)(OiPr)3, M(EtCp)(OEt)3, MCp*(OEt)3, M(iPrCp)(NMe2)3, M(sBuCp)(NMe2)3, M(tBuCp)(NMe2)3, N(secPenCp)(NMe,)3, M(nPrCp)(NMe2)3 Preferred VA metal precursors are as follows: M(OR)5, each R is independently a C1 to C6 carbon chain (linear or branched), most preferably M(OEt)5, M(OiPr)5, M(OtBu)5, M(OsBu)5 ● M(NR 1 R 2 )5, each R 1 and R 2 are independently C1 to C6 carbon chains (linear or branched), most preferably M(NMe2)5, M(NMeEt)5, M(NEt2)5 ● ML(NR 1 R 2 ) x , x=3 or 4, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl or imide of the form NR, each R 1 and R 2 are independently a C1 to C6 carbon chain (linear or branched), most preferably MCp(NMe2)3, M(MeCp)(NMe2)3, M(EtCp)(NEt2)3, MCp*(NMe2)3M(=NtBu)(NMe2)3, M(=NtAm)(NMe2)3, M(=NtBu)(NEt2)3, M(=NtBu)(NEtMe)3, M(=NiPr)(NEtMe)3. ● M(=NR 1 )L(NR 2 R 3 ) x , x=1 or 2, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, or cyclooctadienyl, and each R 1 and R 2 and R 3 are independently a C1 to C6 carbon chain, most preferably MCp(=NtBu)(NMe2)2, M(MeCp)(N=tBu)(NMe2)2, M(EtCp)(N=tBu)(NMe2)2, MCp*(=NtBu)(NMe2)2, MCp(=NtBu)(NEtMe)2, M(MeCp)(N=tBu)(NEtMe)2, M(EtCp)(N=tBu)(NEtMe)2. ● ML(OR) x x=3 or 4, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl or imide of the NR form, and each R is independently a C1-C6 carbon chain (linear or branched), most preferably MCp(OiPr)3, M(MeCp)(OiPr)3, M(EtCp)(OEt)3, MCp*(OEt)3M(=NtBu)(OiPr)3, M(=NtAm)(OiPr)3, ● ML(OR) x (NR 1 R 2 ) y , x and y are independently equal to 1 or 2, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl or imide of the NR form, and each R is independently a C1-C6 carbon chain (linear or branched), most preferably MCp(OiPr)2(NMe2), M(MeCp)(OiPr)2(NMe2), M(EtCp)(OEt)2(NMe2), M(=NtBu)(OiPr)2(NMe2), M(=NtBu)(OiPr)(NMe2), M(=NtBu)(OiPr)2(NMe2), M(=NtBu)(OiPr)2(NMe2), (NMe2), M(=NtBu)(OiPr)2(NEtMe), M(=NtBu)(OiPr)2(NEt2), M(=NtBu)(OEt)2(N Me2), M(=NtBu)(OEt)2(NEtMe), M(=NtBu)(OEt)2(NEt2), M(=NiPr)(OiPr)2(NMe2 ), M(=NiPr)(OiPr)2(NMe2)2, M(=NiPr)(OiPr)2(NEtMe), M(=NiPr)(OiPr)2(NEt2 ), M(=NiPr)(OEt)2(NMe2), M(=NiPr)(OEt)2(NEtMe), orM(=NiPr)(OEt)2(NEt2). Preferred VIA metal precursors are as follows: M(OR)6, each R is independently a C1 to C6 carbon chain (linear or branched), most preferably M(OEt)5, M(OiPr)5, M(OtBu)5, M(OsBu)5 ● M(NR1 R 2 )6, each R 1 and R 2 are independently C1 to C6 carbon chains (linear or branched), most preferably M(NMe2)6, M(NMeEt)6, M(NEt2)6 ● M(NR 1 R 2 ) x L y , x and y are independently equal to 1 to 4; L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl, or an imide of the NR form; 1 and R 2 are independently C1 to C6 carbon chains (linear or branched), most preferably MCp(NMe2)3, M(MeCp)(NMe2)3, M(EtCp)(NEt2)3, MCp*(NMe2)3M(=NtBu)2(NMe2)2, M(=NtAm)2(NMe2)2, M(=NtBu)(NEt2)2 ● M(OR) x (NR 1 R 2 ) y L z ML, x, y and z are independently equal to 0 to 4, L represents an imide of the form unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl or NR, and each R is independently a C1 to C6 carbon chain (linear or branched), most preferably MCp(OiPr)3, M(MeCp)(OiPr)3, M(EtCp)(OEt)3, M(=NtBu)2(OiPr)2, M(=NtAm)2(OiPr)2, M(=NtBu)2(OtBu)2, M(=NiPr)2(OtBu)2, M(=NtBu)2(OiPr)2, M(=NiPr)2(OiPr)2. ● M(=O)xLy, x, y and z are independently equal to 0-4, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl, amide or imide in NR form, each R is independently a C1-C6 carbon chain (linear or branched), most preferably M(=O)2(OtBu)2, M(=O)2(OiPr)2, M(=O)2(OsecBu)2, M(=O)2(OsecPen)2, M(=O)2(NMe2)2, M(=O)2(NEt2)2, M(=O)2(NiPr2)2, M(=O)2(NnPr2)2, M(=O)2(NEtMe)2, M(=O)2(NPen2)2.

[0050] A single precursor or a combination of two or more precursors can be used to form doped metal oxide films, in each case optionally using an oxidizing co-reactant (if necessary or desirable). A single precursor can provide all elements found in the final film, including oxygen and the dopant element D. Alternatively, the metal can come from one precursor, the oxygen from the oxidizing co-reactant, and the dopant D element from a second precursor. For example, the metal precursors listed above can be combined with a second precursor that provides or increases the amount of dopant element D, one or both of which are deposited in an oxidizing environment that results in some metal oxide in the final film. Alternatively, the second precursor provides the dopant D and oxidizes the metal to result in the metal oxide in the final film. A person skilled in the art can select appropriate precursors and co-reactants from those known in the art to produce doped metal oxide films with the desired composition when used under optimized deposition conditions to "tune" the levels of metal oxide and dopant D. Typical of the various precursor options include: - Oxygen can come from an O source such as O2, O3, H2O, H2O2, NO, NO2, N2O or Nox. - The oxygen can come from a dopant source such as an oxygen-containing silicon precursor, an oxygen-containing tin precursor, a phosphate such as trimethyl phosphate, diethyl phosphoramidate, or a sulfate. - Nitrogen can come from N sources such as N2, NH3, N2H4, N2H4 containing mixtures, alkylhydrazines, NO, NO2, N2O or NOx. - Nitrogen can come from dopant sources such as nitrogen-containing silicon precursors, nitrogen-containing tin precursors, or phosphates such as diethyl phosphoramidate. ● Carbon can come from C sources such as hydrocarbons, carbon-containing silicon precursors, carbon-containing tin precursors, carbon-containing boron precursors, carbon-containing aluminum precursors, carbon-containing phosphorus precursors, trimethyl phosphate, phosphates such as diethyl phosphoramidate, or sulfates. - Silicon can come from a Si source such as a silane or silicon-containing organometallic precursor. - Tin can come from a Sn source such as a stannane or a tin-containing organometallic precursor. - Aluminium can come from an Al source such as an alane, such as an alkylalane, or an aluminium-containing organometallic precursor. Phosphorus can be derived from a phosphine, such as an organophosphine, or a phosphate, such as trimethyl phosphate or diethyl phosphoramidate. • Sulfur can come from S sources such as sulfur, S8, H2S, H2S2, SO2, organic sulfites, sulfates, or sulfur-containing organometallic precursors. - First row transition metals may be derived from known organometallic or other precursors suitable for use in vapor deposition. EXAMPLES

[0051] Examples 1-5: Deposition and electrochemical performance of NbOC thin films deposited on NMC622 powder at 100 and 150 °C Experimental conditions for deposition / film formation: Deposition was carried out on NMC622 powder using a fluidized bed reactor with the following experimental conditions: Reactor temperature x°C Reactor pressure: 1 Torr Precursor canister T: 115℃ Precursor canister P: 50 Torr Number of cycles: y

[0052] Pulse sequence: Nb precursor: 30s Purge: 20s H2O: 5s Purge: 5s

[0053] The Nb precursor for these Examples 1-5 is NbCp(=NtBu)(NMe2)2 ("NAB"). The number of cycles for NMC622 electrodes or NMC powders is typically limited to 5-20 ALD cycles, which corresponds to about 1.5-4 Å, an insufficient thickness to achieve the film composition. Therefore, such characterization was performed on films deposited after 300 ALD cycles. The corresponding thicknesses and film compositions are as follows: ● Processing temperature: 150℃⇒GPC approx. 0.27Å. Nb: approx. 24%, O approx. 47%, C approx. 27%, N <DL ● Processing temperature: 100℃⇒GPC approx. 0.78Å. Nb: approx. 25%, O approx. 48%, C approx. 27%, N <DL

[0054] The refractive index of these films is approximately 1.7 vs. 2.25 for Nb2O5 thin films above 200°C.

[0055] Electrochemical characterization: Test conditions: - Cathode material NMC622 - The test electrode is composed of 88:7:5 wt% cathode active material:carbon black (C65):PVDF (Solef5130), which is then cast onto an Al current collector using a doctor blade (200 microns). - 5 or 20 NbCp(=NtBu)(NMe2)2 / H2O ALD cycles at the processing temperatures given in the graph - Electrolyte: 1M LiPF6 in EC:EMC (1:1wt) - Use of Li metal as the anode material - Approximately 5mg / cm 2 Electrode composition, 40 micron thickness - 1C=180mAg -1 , (Li+ / Li) Battery cycled between 3.0~4.3V

[0056] As seen in FIG. 1, the NbOC powder-coated NMC622 electrodes, especially the sample with fewer ALD cycles (NbCp(=NtBu)(NMe2)2 / H2O powder ALD-100C-5Cy), show higher initial capacity at 0.2 C compared to the pristine NMC622 electrodes. When ALD is performed for 20 cycles, the initial capacity becomes very close to the pristine one, probably due to the thicker NbOC film. The long-term stability at 1 C for subsequent battery cycles (FIG. 2) shows that the NbOC powder-coated NMC622 electrodes effectively maintain their capacity, yielding at least >92.5% capacity retention after 80 cycles, while the pristine electrodes only maintain 84%.

[0057] As shown in Figures 3 and 4, when comparing C-rate performance, the NMC622 electrode coated with NbOC powder has higher capacity in the entire range of C-rates (0.2C to 10C) even for the sample cycled 20 times ALD compared to the pristine electrode. This improved morphology may be due to the effect of carbon doping, which makes the film more porous compared to other metal oxide thin films such as Al2O3, where 10 ALD cycles are detrimental to battery performance (S.-H. Lee et al., US Patent No. 9196901B2, 2012). The porosity may allow better Li+ ion movement compared to densified metal oxide films.

[0058] Based on the scanning electron micrograph analysis shown in Figure 5, the presence of NbOC deposits / partial films allows the maintenance of the material morphology, while the pristine material tends to be degraded by the presence of distinct grains of NiOx, which may result from the dissolution of nickel from the NMC particles and then reposition on the electrode surface. These image analyses correlate well with the improved electrochemical performance discussed below.

[0059] Examples 6-9: Deposition and electrochemical performance of NbOC thin films deposited on NMC622 electrodes at 50, 75 and 100 °C Experimental conditions for the formation of deposits: Deposition was carried out on a NMC622 electrode in a thermal ALD reactor with the following experimental conditions: Reactor temperature x°C Reactor pressure: 1 Torr Precursor canister T: 95℃ Precursor canister P: 50 Torr Number of cycles: y

[0060] Pulse sequence: Nb precursor: 30s Purge: 20s H2O: 5s Purge: 5s

[0061] The Nb precursor is NbCp(=NtBu)(NMe2)2 ("NAB"). The number of cycles for NMC622 electrodes or NMC powders is typically limited to 5-100 ALD cycles, which corresponds to about 1.1-85 Å, an insufficient thickness to achieve film compositions. Thus, such characterization was performed on films deposited after 300 ALD cycles. The corresponding thicknesses and film compositions are as follows: - Processing temperature: 100℃⇒GPC approx. 0.23Å. Nb: approx. 17%, O approx. 40%, C approx. 42%, N <DL - Processing temperature: 75℃⇒GPC approx. 0.28Å. Nb: approx. 20%, O approx. 45%, C approx. 34%, N <DL - Processing temperature: 50℃⇒GPC approx. 0.85Å. Nb: approx. 16%, O approx. 35%, C approx. 48%, N <DL

[0062] The refractive index of these films is approximately 1.7 vs. 2.22 for Nb2O5 thin films above 275C.

[0063] Electrochemical characterization: Test conditions: - Cathode material NMC622 - The electrode is composed of 88:7:5 wt% active material:carbon black (C65):PVDF (Solef5130), which is then cast onto an Al current collector using a doctor blade (200 microns). - Five NbCp(=NtBu)(NMe2)2 / H2O ALD cycles at the processing temperatures given in the graph - Electrolyte: 1M LiPF6 in EC:EMC (1:1wt) - Use of Li metal as the anode material - Approximately 5mg / cm 2 Electrode composition, 40 micron thickness - 1C=180mAg -1 , (Li + / Li) Battery cycled between 3.0~4.3V

[0064] The long-term cycling stability of NMC622 electrodes coated with NbOC thin films (Fig. 6) not only shows higher discharge capacity in the first cycle (4th cycle) at 1C regardless of the ALD temperature, but also demonstrates at least >92% capacity retention after 80 battery cycles, whereas 84% ​​retention is observed for the pristine NMC622 electrode (Fig. 7). Temperature dependence is also observed by ALD at 100 °C, which is the optimal temperature for better long-term cycling stability under these conditions for this experimental battery.

[0065] In terms of C-rate performance, the deposition of NbOC thin films on NMC622 electrodes allows them to provide higher capacity at 0.2 C to 5 C compared to the pristine electrodes (FIGS. 8 and 9). At 10 C, only the NbCp(=NtBu)(NMe2)2 / H2O electrode ALDed at 100° C. exhibits higher capacity than the pristine electrodes. As already demonstrated in the long-term cycling test (FIG. 6), the C-rate results also confirm that the optimal ALD temperature is 100° C. in these experiments.

[0066] Examples 10-13: Deposition and electrochemical performance of NbOC thin films deposited on NMC622 electrodes at 75, 100, 125 and 150 °C using Nb(=NtBu)(NMe2)2(OEt) / H2O Similar experiments were carried out with the precursor Nb(=NtBu)(NMe2)2(OEt) ("NAU") used instead of NAB. The resulting films had the following properties: ● Thickness: 3~61Å ● Refractive index: 2.06~2.28 ● Atomic composition of 300-cycle film: ○ Processing temperature: 150℃⇒GPC approx. 0.66A. Nb: approx. 25%, O approx. 60%, C approx. 11%, N approx. 2% ○ Processing temperature: 125℃⇒GPC approx. 1.69A. Nb: approx. 30%, O approx. 64%, C approx. 4%, N approx. 1% ○ Processing temperature: 100℃⇒GPC approx. 2.25A. Nb: approx. 27%, O approx. 57%, C approx. 14%, N approx. 1% ○ Processing temperature: 75℃⇒GPC approx. 3.07A. Nb: approx. 25%, O approx. 58%, C approx. 15%, N approx. 2%

[0067] These electrodes had similar improvements in electrochemical performance as the electrodes with the NAB-derived membrane.

[0068] Examples 14-15: Chemical vapor deposition and electrochemical performance of NbOCP thin films deposited on NMC622 electrodes NbOCP deposition was accomplished according to the following experimental conditions: Deposition conditions and characterization: Reactor temperature: 100~150℃ Reactor pressure: 1 Torr Nb precursor canister T: 95℃ Nb precursor canister P: 10 Torr Nb precursor bubbling FR: 50sccm TMPO canister T: 30℃ TMPO Canister P: 10 toll TMPO bubbling FR: 50sccm Reaction time: y minutes (specified on the graph) Flow rate of the precursor: Nb precursor: 5 sccm TMPO: 5 sccm O3: 100 sccm

[0069] The niobium precursor is Nb(=NtBu)(NMe2)2(OEt). The corresponding thickness and film composition at 100 °C are a thickness of approximately 2.1 nm. Nb: 29.6%, O: 58.0%, C: 7.8%, P: 2.6%, N < DL; at 150 °C, the thickness is approximately 1.8 nm. Nb: 24.3~%, O: 60.1~%, C: 7.6~%, P: 6.4%, N < DL.

[0070] Determination of electrochemical properties: - Cathode material NMC622 - The electrode is composed of 88:7:5 wt% active material: carbon black (C65): PVDF (Solef5130), which is then cast onto an Al current collector using a doctor blade (200 microns). - NbOP deposited by electrode CVD using the following: - CVD processing temperature = 100~150 °C; time: 1 and 2 minutes - Electrolyte: 1 M LiPF6 in EC:EMC (1:1 wt) - Use of Li metal as the anode material - An electrode loading of approximately 5 mg / cm 2 with a thickness of 40 um - 1 C = 180 mAg -1 , (for Li + / Li) a battery repeated between 3.0~4.3 V

[0071] As shown in Figures 10 and 11, the initial capacity at 0.2C for the NbOCP thin film coated NMC622 electrode is increased compared to the pristine NMC622 electrode. For subsequent cycles, the NbOCP thin film coated NMC622 electrode clearly shows better cycling performance, maintaining >95% retention after 80 battery cycles at 1C for the Nb(=NtBu)(NMe2)2(OEt) / TMPO / O3ECVD-150°C-1min electrode. The NMC622 electrode with NbOCP thin film shows higher capacity at low and moderate C rates up to 5C compared to the pristine NMC622 electrode (Figures 12 and 13).

[0072] Examples 16-19: Deposition and electrochemical performance of ZrOC thin films deposited on LNMO electrodes Deposition conditions and characterization: Reactor temperature: 75~150℃ Reactor pressure: 1 Torr Zr precursor canister T: 100℃ Zr precursor canister P: 20 Torr Zr precursor bubbling FR: 40sccm Reaction time: y minutes (specified on the graph) Precursor flow rate: Zr precursor: 2sccm O3: 100sccm Pulse sequence: Zr precursor: 20s Purge: 5s O3: 5s Purge: 5s

[0073] The zirconium precursor was ZrCp(NMe2)3 and can be represented as "ZrCp". The average film thickness was about 2-20 Å. The films contained about 20%-25% Zr, about 1%-5% nitrogen, about 40%-60% oxygen, and about 12-30% C. The refractive index ranged from 1.92 at 75°C to 2.15 at 150°C (compared to 2.21 for ZrO2).

[0074] Electrochemical characterization: - Cathode material LNMO - ZrOC deposited on the electrode by CVD using: Processing temperature = 50-150°C; Time: 5-50 cycles - Electrolyte: 1M LiPF6 in EC:EMC (1:1wt) - Use of Li metal as the anode - Approximately 5mg / cm 2 Mixture amount, thickness 40um

[0075] As shown in Figures 14 and 15, the initial capacity at 0.2C for the LNMO electrode coated with ZrOC thin film decreased slightly compared to the pristine NMC622 electrode when the ALD temperature increased due to the dense ALD coating film. For subsequent cycles, the LNMO electrode coated with ZrOC thin film clearly showed better cycling performance, especially for ZrCp / O3-125C-20Cy and ZrCp / O3-150C-20Cy, which maintained 97% and 100% retention after 80 battery cycles at 1C, respectively, while 82% capacity retention was observed for the pristine LNMO electrode. The LNMO electrode with ZrOC thin film showed higher capacity at low and moderate C rates up to 5C compared to the pristine NMC622 electrode (Figures 16 and 17), while no apparent capacity was observed for both the pristine and ZrOC thin film coated LNMO electrodes.

[0076] Although the present invention has been described with specific embodiments thereof, it is apparent that many alternatives, modifications, and variations will be apparent to those skilled in the art in light of the foregoing description. It is therefore intended to embrace all such alternatives, modifications, and variations that fall within the spirit and broad scope of the appended claims. The present invention may suitably comprise, consist of, or consist essentially of the elements disclosed, and may be practiced in the absence of elements not disclosed. Furthermore, where there is language referring to a sequence such as first and second, it should be understood in a typical sense and not in a limiting sense. For example, it may be recognized by one skilled in the art that certain steps may be combined into a single step.

[0077] The singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0078] "Comprising" in the claims is an open transition term meaning that the claim elements identified thereafter are a non-exclusive recitation, i.e., nothing else may be further included and may be within the scope of "comprising." "Comprising" is defined herein as necessarily including the more narrow transition terms "consisting essentially of" and "consisting of." Thus, "comprising" may be replaced with "consisting essentially of" or "consisting of" and is within the clearly defined scope of "comprising."

[0079] "Providing" in the claims is defined to mean providing, supplying, making available, or preparing something. Steps may be performed by any actor, absent express language to the contrary in the claims.

[0080] Optional or optional means that the subsequently described event or circumstance may or may not occur. The description includes instances where the event or circumstance occurs and instances where it does not occur.

[0081] Ranges may be expressed herein from broadly one particular value and / or to broadly another particular value. When such a range is expressed, it should be understood that another embodiment is from the one particular value and / or to the other particular value, along with all combinations within said ranges.

[0082] All documents cited herein are each incorporated by reference in their entirety into this application as well as for the specific information for which each is cited.

Claims

1. 1. A cathode or cathode active material comprising at least a partial surface coating of a doped metal oxide film, The doped metal oxide film is a metal, oxygen and carbon containing film having an atomic percentage of carbon atoms between 10% and 30%; or Any of metal, oxygen and phosphorus containing films, The metal is selected from niobium, or zirconium, and combinations thereof; Cathode or cathode active material.

2. 2. The cathode or cathode active material of claim 1, wherein the doped metal oxide film is a doped niobium oxide film.

3. 2. The cathode or cathode active material of claim 1, wherein the doped metal oxide film is a niobium, oxygen and carbon containing film or a niobium, oxygen and phosphorus containing film.

4. The cathode or cathode active material of any one of claims 1 to 3, which is only partially coated with the doped metal oxide film.

5. The cathode or cathode active material of any one of claims 1 to 4, wherein the doped metal oxide film has an average thickness of 0.1 nm to 5 nm.

6. The cathode or cathode active material of any one of claims 1 to 5, wherein the doped metal oxide film has an atomic percentage of carbon atoms of 15% to 25%.

7. The cathode or cathode active material of any one of claims 1 to 6, wherein the doped metal oxide film has a refractive index of 1.6 to 2.

1.

8. The doped metal oxide is M x O y D zwherein M is niobium, zirconium or a combination thereof, O is oxygen, and D is a dopant atom selected from C or P, and x=10-60%, y is in the range of 10-60%, and z is in the range of 10-30%.

9. 9. The cathode or cathode active material of claim 8 which is only partially coated with the doped metal oxide film.

10. 10. The cathode or cathode active material of claim 8 or 9, wherein the doped metal oxide film has an average thickness of 0.1 nm to 5 nm.

11. The cathode or cathode active material of any one of claims 8 to 10, wherein the doped metal oxide film has an atomic percentage of carbon atoms of 15 to 25%.

12. The cathode or cathode active material of any one of claims 8 to 11, wherein the doped metal oxide film has a refractive index of 1.6 to 2.

1.

13. A lithium ion battery comprising the cathode or cathode active material of any one of claims 1 to 12.

14. A method for coating a cathode or cathode active material with a doped metal oxide film, comprising the steps of: The doped metal oxide film is a metal, oxygen and carbon containing film having an atomic percentage of carbon atoms between 10% and 30%; or Any of metal, oxygen and phosphorus containing films, the metal is selected from niobium, or zirconium, and combinations thereof; a1. exposing the cathode or cathode active material to vapors of chemical precursors containing niobium and / or zirconium; b1. exposing the cathode or cathode active material to a co-reactant.

15. The method of claim 14, wherein the co-reactant is an oxygen source.

16. 16. The method of claim 15, wherein the step a1. of exposing the cathode or cathode active material to vapor of the chemical precursor and the step b1. of exposing the cathode or cathode active material to a co-reactant are performed sequentially.

17. 17. The method of claim 16, further comprising the step a1.i of purging the chemical precursor vapor prior to step b1. of exposing the cathode or cathode active material to a co-reactant.

18. The method of claim 17 , wherein the method is atomic layer deposition.

19. The method of claim 14 , wherein the method is chemical vapor deposition.

20. The method of any one of claims 15 to 19, wherein the co-reactant is selected from O 2 and O 3 .

21. The doped metal oxide film produced by step b1. is M x O y D z wherein M is selected from niobium, zirconium or a combination thereof, O is oxygen, and D is a dopant atom selected from C or P, and x=0.1 to 0.

3. The method according to any one of claims 14 to 20, wherein y = 0.3 to 0.65 and z = 0.1 to 0.

3.

22. The method of any one of claims 14 to 21, wherein each set of steps is repeated.

23. A method according to any one of claims 14 to 22, wherein the temperature of the chemical precursor vapour and / or the cathode or cathode active material is between 50°C and 200°C.

24. 24. The method of any one of claims 14 to 23, wherein the cathode active material, or the cathode active material in the cathode, is selected from the group consisting of: a) layered oxides; b) spinel cathode materials; c) olivine structured cathode materials; and combinations thereof.

Citation Information

Patent Citations

  • Preparation method of atomic layer deposition coated high-nickel ternary positive electrode material

    CN111082025A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and manufacturing method of positive electrode active material for nonaqueous electrolyte secondary battery

    JP2009016302A

  • Manufacturing method of power storage device and power storage device

    JP2015103471A

  • Positive electrode active material for non-aqueous secondary battery and method of manufacturing thereof

    US20150270539A1

  • Positive Electrode Material, Positive Electrode, and Lithium Secondary Battery Which Include Spinel-Structured Lithium Manganese-Based Positive Electrode Active Material

    US20200083524A1