Positive plate and battery
The positive electrode plate with graded particle sizes and auxiliary materials in sublayers addresses uneven lithium ion distribution, enhancing battery performance and safety by ensuring uniform charge distribution and reduced impedance.
Patent Information
- Application Number
- JP2022580298
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-24
- Filing Date
- 2021-05-13
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-05-13
AI Technical Summary
Lithium-ion batteries with layered cathode materials face issues of uneven lithium ion desorption/insertion rates, leading to high impedance, low rate performance, and fast cycle decay due to non-uniform charge distribution among particles, especially at high surface densities and agglomerations, which can increase safety hazards.
The positive electrode plate features a current collector with a positive electrode active material layer composed of multiple sublayers, where the main cathode material particle sizes gradually increase from the current collector to the outer layers, accompanied by the use of auxiliary cathode materials with smaller particles to fill gaps, ensuring uniform lithium ion desorption/insertion rates and improved charge distribution.
This design enhances the uniformity of lithium ion desorption/insertion rates, reduces polarization, increases the compressed density, and improves the conductive performance, rate, and safety of the battery.
Smart Images

Figure 0007596410000008 
Figure 0007596410000001 
Figure 0007596410000002
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to Chinese Patent Application No. “202010585072.2” filed by BYD Company Limited on June 24, 2020, entitled “Positive Plate and Battery,” all of which are incorporated herein by reference.
[0002] The present invention relates to the technical field of batteries, and in particular to positive plates and batteries. [Background technology]
[0003] Lithium ion batteries have the advantages of high energy density, small volume, light weight, long cycle life, no memory effect, etc., and are widely used in the fields of portable electronic devices and new energy electric vehicle batteries. In lithium battery systems, layered positive electrode materials have become the focus of attention as positive electrode materials due to their advantages of high energy density, low cost, high platform voltage, etc. In particular, with people's urgent demand for high energy density, the requirements for the surface density and small and high density of the electrode plate are also becoming higher. In the case of high surface density and high aggregation, the migration path of lithium ions on the electrode plate away from the electrolyte is extended, the local desorption and insertion of lithium on the electrode plate is uneven, and the large and small particles on the electrode plate all have different speeds to complete desorption / insertion, resulting in uneven distribution of the charge state between particles, which causes problems such as large battery impedance, low rate, and fast cycle decay, as well as increasing potential safety hazards. Summary of the Invention
[0004] The present application aims to solve at least one of the technical problems in the prior art. To this end, a positive electrode plate according to a first aspect of the present application includes a current collector and a positive electrode active material layer disposed on the current collector, the positive electrode active material layer includes m positive electrode active material sublayers, the positive electrode active material in each positive electrode active material sublayer includes a main positive electrode material and an auxiliary positive electrode material, and D of the main positive electrode material in the positive electrode active material layer is 50 The particle size satisfies the following:
number
[0005] A battery according to a second aspect of the present application includes the positive electrode plate described above.
[0006] The beneficial effects of the present disclosure are as follows: In the positive electrode plate according to the present disclosure, by setting the particle size of the main positive electrode material in the positive electrode active material sub-layer of each layer in the positive electrode active material layer to satisfy the following:
number
[0007] [Figure 1] 1A to 1C are Raman spectroscopic images of micro-areas of positive electrode plates manufactured in one embodiment and a comparative example according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The following description is a preferred embodiment of the present disclosure, and those skilled in the art may make some improvements and modifications without departing from the principles of the present disclosure, and these improvements and modifications are also included in the scope of protection of the present disclosure.
[0009] A positive electrode plate according to an embodiment of the present disclosure includes a current collector and a positive electrode active material layer disposed on the current collector. The positive electrode active material layer includes m positive electrode active material sublayers. The positive electrode active material in each positive electrode active material sublayer includes a main positive electrode material and an auxiliary positive electrode material. 50 The particle size satisfies the following:
number
[0010] The auxiliary positive electrode material D 90 The particle size is the D of the main positive electrode material in the positive electrode active material sub-layer of the first layer. 10 That is, the particle size of the auxiliary positive electrode material and the particle size of the main positive electrode material in the positive electrode active material sub-layer of the first layer are smaller than D 90 補助 < D 10 1 and D above is satisfied. 90 補助 is the D of the auxiliary positive electrode material 90 The above represents the particle size. D 10 1 is the D of the main positive electrode material in the first positive electrode active material sublayer 10 Represents particle size.
[0011] The m positive electrode active material sublayers are disposed on the same side of the current collector, and from the direction away from the current collector, the m positive electrode active material sublayers include a first positive electrode active material sublayer, a second positive electrode active material sublayer, ... the (m-1)th positive electrode active material sublayer, and an mth positive electrode active material sublayer, which are disposed in this order, and the first positive electrode active material sublayer is in direct contact with the current collector. In one embodiment, the m is an integer between 3 and 6. In another embodiment, the m=4.
[0012] D of the main positive electrode material in the positive electrode active material layer 50 The particle size satisfies the following:
number
[0013] In the particle size relationship of the gradient distribution as shown in the relational expression 1, the particle size of the main positive electrode material of the positive electrode active material layer gradually increases from the current collector to one side away from the current collector, so that the lithium ion desorption / insertion speed in the entire positive electrode active material layer becomes uniform, and the charge distribution between adjacent particles in the thickness direction of the positive electrode plate becomes uniform, which can reduce the polarization caused by the difference in charge state between the thickness direction of the positive electrode plate and between large and small particles, and can further improve the conductive performance of the manufactured battery, and improve the rate performance and safety performance of the manufactured battery. The transport of lithium ions in the battery mainly includes two aspects, one of which is solid-phase diffusion, i.e., the particle size of the active material particles in the electrode, and the other is liquid-phase diffusion, i.e., the diffusion distance of lithium ions in a liquid phase environment. When the particle diameters of the positive electrode material particles at each position throughout the positive electrode active material layer are not distributed according to the rule of the above Relation 1, for example, when the particle diameters of the positive electrode material particles throughout the positive electrode active material layer are the same, the solid-phase diffusion distance of the lithium ions in the active material is the same, but the distances from the solid-liquid interface of the active material at different thicknesses of the electrode plate are different, which causes the lithium ions to be desorbed and inserted at different distances in the liquid phase. In this case, the lithium desorption and insertion speed of the active material in the surface layer of the electrode plate (position close to the separator) becomes faster and the lithium desorption and insertion speed of the active material in the back layer of the electrode plate (position close to the current collector) becomes slower, and further the distribution of the charge state between the particles of the active material becomes uneven, causing problems such as high battery impedance, poor rate, and fast cycle decay. The speed at which lithium ions complete their desorption / insertion into large particles of the positive electrode material is slower than the speed at which they complete their desorption / insertion into small particles of the main positive electrode material, resulting in uneven distribution of the charge state among the particles of the positive electrode material, leading to problems such as high battery impedance, low rate, and fast cycle decay.
[0014] In general, the lithium desorption / insertion rate of large-sized positive electrode material particles is slow, while the lithium desorption / insertion rate of small-sized positive electrode material particles is fast. In the present application, the particle size of the main positive electrode material particles in the positive electrode active material sublayer adjacent to the electrolyte (or the side away from the current collector) is set to be large, and the particle size of the main positive electrode material particles in the positive electrode active material sublayer away from the electrolyte (or the side adjacent to the current collector) is set to be small, so that the lithium desorption / insertion rate of the large-sized main positive electrode material particles adjacent to the electrolyte is equivalent to the lithium desorption / insertion rate of the small-sized main positive electrode material particles away from the electrolyte, and further the lithium desorption / insertion rate of the positive electrode active material in each layer of the positive electrode active material sublayer is the same, thereby improving the consistency of the lithium desorption / insertion rate of the entire positive electrode active material layer.
[0015] For example, the particle size of the main positive electrode material in the first layer of the positive electrode active material sublayer is the smallest, and the lithium ions are precipitated from the particles of the main positive electrode material in a short time, but the first layer of the positive electrode active material sublayer is the furthest from the electrolyte, and the precipitated lithium ions can enter the electrolyte in a long time, while the particle size of the main positive electrode material in the mth layer of the positive electrode active material sublayer is the largest, and the lithium ions are precipitated from the particles of the main positive electrode material in a long time, but the mth layer of the positive electrode active material sublayer is the closest to the electrolyte, and the precipitated lithium ions can enter the electrolyte in a short time. As can be seen from this, the total time that the lithium ions precipitate from the particles of the main positive electrode material in the first layer of the positive electrode active material sublayer and reach the electrolyte tends to be consistent with the total time that the lithium ions precipitate from the particles of the main positive electrode material in the mth layer of the positive electrode active material sublayer and reach the electrolyte, that is, the desorption / insertion rate of the lithium ions in the first layer of the positive electrode active material sublayer is equivalent to the desorption / insertion rate of the lithium ions in the mth layer of the positive electrode active material sublayer. Similarly, the lithium ion desorption / insertion rates in the second layer and the m-1th layer of the positive electrode active material layer are equivalent, and the lithium ion desorption / insertion rates in the adjacent nth and n-1th layers of the positive electrode active material sublayers are also equivalent, or the lithium ion desorption / insertion rates in any two layers of the positive electrode active material sublayers of the positive electrode active material layers are also equivalent. Therefore, for the entire positive electrode active material layer, the D 50 By distributing the particle sizes in accordance with the above Relational Formula 1, the lithium ion desorption / insertion rate becomes uniform throughout the positive electrode active material layer, and the charge distribution between adjacent particles in the thickness direction of the positive electrode plate becomes uniform, thereby reducing polarization due to differences in charge state in the thickness direction of the positive electrode plate and between large and small particles.
[0016] In addition, in the positive electrode active material of the present application, Auxiliary cathode material is further installed, and the particle size of the auxiliary positive electrode material and the particle size of the main positive electrode material in the positive electrode active material sub-layer of the first layer are D 90 補助 < D 10 1that is, overall, 90% of the auxiliary positive electrode material has a particle size smaller than that of the main positive electrode material in 10% of the positive electrode active material sub-layers, and the auxiliary positive electrode material with a smaller particle size is distributed in the gaps between the particles of the main positive electrode material with a relatively larger particle size in the positive electrode active material sub-layers of each layer, thereby effectively increasing the compression density of the positive electrode plate.
[0017] In this application, the main positive electrode material is preferably a layered positive electrode material, and the auxiliary positive electrode material is preferably a polyanion positive electrode material, the polyanion positive electrode material has excellent structural stability, the polyanion positive electrode is not easily reactive with the electrolyte, or when reacting with the electrolyte, the effect on the structure of the positive electrode active material layer is small, and the structural stability of the positive electrode active material layer is not destroyed, and the combined use of the polyanion positive electrode material and the layered positive electrode material can improve the cycle and safety performance of the positive electrode plate. The layered positive electrode material may be a layered positive electrode material formed by applying and compressing the main positive electrode material.
[0018] In the positive electrode plate according to the present disclosure, when the particle size of the main positive electrode material in the positive electrode active material sub-layers of each layer of the positive electrode active material layer is set so as to satisfy the above Relation 1, and when small particles of auxiliary positive electrode material are filled into the gaps between the large particles of the main positive electrode material, the uniformity of the charge distribution between adjacent particles in the thickness direction of the positive electrode plate is improved and polarization due to differences in charge states in the thickness direction of the positive electrode plate and between large and small particles is reduced, the compressed density of the positive electrode plate can be further effectively increased.
[0019] In one embodiment, the auxiliary positive electrode material D 50 The particle size of the auxiliary positive electrode material is 200 nm or less. 50 補助 ≦200 nm and above D 50 補助 is the D of the auxiliary positive electrode material 50 The particle size of the auxiliary positive electrode material is represented by D 50 When the particle size is less than or equal to 200 nm, the auxiliary positive electrode material can be better distributed among the particles of the main positive electrode material, and the compression density of the positive electrode plate can be further improved.
[0020] In one embodiment, D of the main positive electrode material in the n-1th positive electrode active material sublayer 90 The particle size is the D 10 That is, the particle size of the main positive electrode material in the (n-1)th positive electrode active material sub-layer and the particle size of the main positive electrode material in the nth positive electrode active material sub-layer are equal to or smaller than D 90 n-1 ≦D 10 n and D above is satisfied. 90 n-1 is the D of the main positive electrode material in the positive electrode active material sublayer of the n-1th layer. 90 The above D represents the particle size. 10 n is the D of the main positive electrode material in the nth positive electrode active material sublayer. 10 represents the particle size. In the (n-1)th positive electrode active material sublayer, 90% of the particle size of the main positive electrode material is smaller than 10% of the particle size of the main positive electrode material in the nth positive electrode active material sublayer. In this way, it is possible to ensure that the particle size of the main positive electrode material particles in two adjacent layers gradually transitions from small to large, and the gradient regularity of the particle size distribution of the main positive electrode material particles in each positive electrode active material sublayer can be further improved for the entire positive electrode active material layer.
[0021] In one embodiment, the particle size of the main positive electrode material in the positive electrode active material layer is 4.0 μm≦D 50 [m / 2]+1 ≦8.0 μm, and the above [m / 2] represents rounding down to an integer, and the above D 50 [m / 2]+1 is the D of the main positive electrode material in the positive electrode active material sublayer of the [m / 2]+1th layer. 50 For example, when m is 4, the particle size of the main positive electrode material in the positive electrode active material layer is 4.0 μm≦ D 50 3 ≦8.0 μm, that is, the D 50 The particle size is between 4.0 μm and 8.0 μm. When m is 5, the particle size of the main positive electrode material in the positive electrode active material layer is 4.0 μm≦ D 50 3≦8.0 μm, that is, the D 50 The particle size is between 4.0 μm and 8.0 μm.
[0022] The above setting limits the particle size of the main positive electrode material adjacent to or in the intermediate layer, and the particle size distribution of the main positive electrode material in the first positive electrode active material sub-layer to the last positive electrode active material sub-layer can be known from the particle size distribution relational expression 1 in each layer.
[0023] In one embodiment, the percentage of the surface density of the main positive electrode material in the first to m-th positive electrode active material sublayers of the positive electrode active material layers relative to the surface density of the main positive electrode material in the positive electrode active material layer exhibits a normal distribution, where the surface density of the main positive electrode material in the positive electrode active material layer refers to the mass of the main positive electrode material in the positive electrode active material layer per unit area at a given thickness, and the surface density of the main positive electrode material in the positive electrode active material sublayer refers to the mass of the main positive electrode material in the positive electrode active material sublayer per unit area at a given thickness.
[0024] That is, the surface density of the main positive electrode material in the positive electrode active material sublayers at both ends of the positive electrode active material layer is small, and the surface density of the main positive electrode material in the positive electrode active material sublayer of the intermediate layer is large, and such a distribution can improve the uniformity of the charge distribution between adjacent particles in the thickness direction of the positive electrode plate. Since the difference in particle size of the main positive electrode material in the positive electrode active material sublayers at both ends is the largest, and the difference in the speed at which lithium ions are desorbed / inserted into the particles of the main positive electrode material at both ends is the largest, setting the surface density of the main positive electrode material in the positive electrode active material sublayers at both ends to be small can reduce the amount of particles of the main positive electrode material with a large difference in the desorption / insertion speed of lithium ions at both ends, thereby improving the consistency of the lithium ion desorption / insertion speed in the entire positive electrode active material layer, and further improving the uniformity of the charge distribution between adjacent particles in the thickness direction of the positive electrode plate.
[0025] In one embodiment, in the cathode active material layer, the percentage of the surface density of the main cathode material in each cathode active material sub-layer relative to the surface density of the main cathode material in the cathode active material layer is: ρ 1 ≦10.0%, ρ m ≦10.0%, ρ 2 ≧10.0%, ρ m-1 ≧10.0%, 40.0%≦ρ m / 2 Meets ≦60.0% Here, the m is an integer of 3 or more, and the ρ 1 represents the percentage of the surface density of the main positive electrode material in the positive electrode active material sub-layer of the first layer relative to the surface density of the main positive electrode material in the positive electrode active material layer, and the above ρ 2 represents the percentage of the surface density of the main positive electrode material in the positive electrode active material sub-layer of the second layer relative to the surface density of the main positive electrode material in the positive electrode active material layer, and the above ρ m represents the percentage of the surface density of the main positive electrode material in the mth positive electrode active material sub-layer relative to the surface density of the main positive electrode material in the positive electrode active material layer, and the above ρ m-1 represents the percentage of the surface density of the main positive electrode material in the (m-1)th layer of the positive electrode active material sub-layer relative to the surface density of the main positive electrode material in the positive electrode active material layer, and when m is an odd number, the above ρ m / 2 represents the percentage of the surface density of the main positive electrode material in the [m / 2]+1-th positive electrode active material sub-layer relative to the surface density of the main positive electrode material in the positive electrode active material layer, where [m / 2] represents rounding down to an integer, and when m is an even number, the above ρ m / 2 represents the percentage of the surface density of the main positive electrode material in at least one of the [m / 2]th positive electrode active material sublayer and the [m / 2]+1th positive electrode active material sublayer relative to the surface density of the main positive electrode material in the positive electrode active material layer.
[0026] For example, when m=4, ρ 1 = 8%, ρ 2 = 45%, ρ 3 = 38%, ρ 4 =9%.
[0027] If m=5, then ρ 1= 8%, ρ 2 = 17%, ρ 3 = 50%, ρ 4 = 17%, ρ 5 = 8%. When m = 6, ρ 1 = 5%, ρ 2 = 10%, ρ 3 = 40%, ρ 4 = 30%, ρ 5 = 10%, ρ 6 That is, the surface density of the main positive electrode material in the positive electrode active material sub-layers at both ends is low, and the surface density of the main positive electrode material in the intermediate positive electrode active material sub-layer is high.
[0028] In one embodiment, the positive electrode active material sub-layer of each layer further comprises a conductive agent and a binder.
[0029] Preferably, the surface density of the positive electrode active material layer is 300 g / m 2 ≦ρ≦500g / m 2 The above ρ represents the surface density of the positive electrode active material layer, which includes a main positive electrode material, an auxiliary positive electrode material, a conductive agent, and a binder, and the surface density of the positive electrode active material layer refers to the mass of all of the main positive electrode material, the auxiliary positive electrode material, the conductive agent, and the binder in the positive electrode active material layer per unit area at a given thickness.
[0030] The surface density of the positive electrode active material layer of the present invention is high, at 300 g / m 2 and 500g / m 2 and has a high electric capacity. On the other hand, a positive electrode active material layer with a large surface density has a larger thickness in a positive electrode plate of the same area, and in this application, for a positive electrode active material layer with a larger thickness, the particle size distribution relational formula 1 of each positive electrode active material sublayer is used, and the improvement of the charge state distribution between the particles of the positive electrode material of the positive electrode plate is more obvious. Alternatively, for a positive electrode plate with a larger thickness, the setting of the above relational formula 1 is used, and the effect of improving the electric performance of the positive electrode plate is more obvious, specifically, it can be expressed as reducing the impedance of the positive electrode plate, improving the charge uniformity of the positive electrode plate, and improving the rate performance of the manufactured battery.
[0031] The conductive agent is at least one of conductive carbon black, acetylene black, carbon nanotubes, and graphene, and the binder is polyvinylidene fluoride or a copolymer containing vinylidene fluoride.
[0032] In one embodiment, the surface density of the positive electrode active material layer is 350 g / m 2 ≦ρ≦450g / m 2 In a further embodiment, the surface density of the positive electrode active material layer is 400 g / m 2 ≦ρ≦450g / m 2 Meet the following.
[0033] In one embodiment, the mass of the auxiliary positive electrode material is 0.5% to 20.0% of the mass of the positive electrode active material in the positive electrode active material layer. The positive electrode plate obtained using the above mass ratio has a good plate compression density.
[0034] In a further embodiment, the mass of the auxiliary positive electrode material accounts for 4.0% to 12.0% of the mass of the positive electrode active material in the positive electrode active material layer.
[0035] In one embodiment, the layered cathode material is at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganate, lithium nickel cobalt manganate, and lithium nickel cobalt aluminate, and the polyanion cathode material is at least one of lithium iron phosphate, lithium iron manganese phosphate, lithium manganese phosphate, lithium vanadium phosphate, lithium vanadium fluorophosphate, lithium manganese silicate, lithium iron silicate, and lithium cobalt silicate.
[0036] The battery according to the present disclosure includes the positive electrode plate according to any one of the above. The electrode plate is installed in a battery, which can reduce polarization caused by the difference in charge in the thickness direction of the positive electrode plate and between large and small particles, eliminate polarization caused by non-uniform lithium desorption / insertion, reduce the impedance of the battery, and improve the electrochemical performance and cycle performance of the battery at different rates.
[0037] In order to better illustrate the technical solutions of the present disclosure, specific examples are given below. EXAMPLES
[0038] (1) A positive electrode active material, a conductive agent and a binder are dissolved in a solvent of N-methylpyrrolidone in a mass ratio of 94:3.0:3.0, and uniformly dispersed to prepare a slurry. The positive electrode active material includes a layered positive electrode material and a polyanion positive electrode material. The layered positive electrode material is LiNi 0.83 Co 0.13 Mn 0.04 O 2 The polyanion positive electrode material is a lithium iron phosphate positive electrode material, and the mass percentage of the lithium iron phosphate positive electrode material in the positive electrode active material is 6.5%.
[0039] (2) Prepare a first positive electrode slurry according to the above steps, and the first positive electrode slurry is D 50 = 0.80μm LiNi 0.83 Co 0.13 Mn 0.04 O 2 and D. 50 = 200 nm lithium iron phosphate positive electrode material Including, The second positive electrode slurry is prepared according to the above steps, and the second positive electrode slurry is 50 = 2.2μm LiNi 0.83 Co 0.13 Mn 0.04 O 2 and D. 50 = 200 nm lithium iron phosphate positive electrode material Including, The third positive electrode slurry is prepared according to the above steps, and the third positive electrode slurry is 50 = 5.2μm LiNi 0.83 Co 0.13 Mn 0.04 O 2 and D. 50 = 200 nm lithium iron phosphate positive electrode material Including, The fourth positive electrode slurry is prepared according to the above steps, and the fourth positive electrode slurry is50 = 12.0 μm LiNi 0.83 Co 0.13 Mn 0.04 O 2 and D. 50 = 200 nm lithium iron phosphate positive electrode material Includes.
[0040] (3) The first positive electrode slurry, the second positive electrode slurry, the third positive electrode slurry and the fourth positive electrode slurry are applied to a current collector in this order to form a first positive electrode active material sub-layer, a second positive electrode active material sub-layer, a third positive electrode active material sub-layer and a fourth positive electrode active material sub-layer, and the four positive electrode active material sub-layers constitute a positive electrode active material layer of the positive electrode plate. By continuously vibrating the positive electrode plate coated with the four slurries, the particles of the positive electrode active material in the positive electrode active material sub-layers of each layer in the positive electrode plate exhibit a gradient distribution in particle size, thereby reducing the particle size difference in the interface layer.
[0041] (4) The positive electrode plate is sintered, rolled, and then cut to a specific size for use, and the occupancy rates of the main positive electrode material in the first positive electrode active material sub-layer, the second positive electrode active material sub-layer, the third positive electrode active material sub-layer, and the fourth positive electrode active material sub-layer relative to the surface density of the main positive electrode material in the positive electrode active material layer are 8.0%, 45.0%, 38.0%, and 9.0%, respectively, and the surface density of the positive electrode active material layer is 420 g / m 2 The LiNi 0.83 Co 0.13 Mn 0.04 O 2 D 50 The particle size satisfies the following.
number
[0042] The positive electrode plate was prepared in the same manner as in Example 1, with the difference being that the selected positive electrode active material sub-layer was prepared by using layered positive electrode material D 50 The particle size is three kinds, and the D of the layered positive electrode material in the first positive electrode active material sub-layer, the second positive electrode active material sub-layer, and the third positive electrode active material sub-layer is50 The particle sizes are 2.0 μm, 6.5 μm, and 15.0 μm, respectively, and the D 50 The particle size satisfies the relational expression 1, and other conditions are the same as those in Example 1 to manufacture a positive electrode plate. EXAMPLES
[0043] The positive electrode plate was prepared in the same manner as in Example 1, with the difference being that the selected positive electrode active material sub-layer was prepared by using layered positive electrode material D 50 D of layered positive electrode material in the first positive electrode active material sublayer, the second positive electrode active material sublayer, the third positive electrode active material sublayer, the fourth positive electrode active material sublayer, and the fifth positive electrode active material sublayer, 50 The particle sizes are 0.5 μm, 1.5 μm, 4.5 μm, 8.0 μm, and 18.0 μm, respectively, and the D 50 The particle size satisfies the relational expression 1, and other conditions are the same as those in Example 1 to manufacture a positive electrode plate. EXAMPLES
[0044] The positive electrode plate was manufactured in the same manner as in Example 1, with the difference being that the selected lithium iron phosphate D 50 The particle size is 125 nm, and a positive electrode plate is manufactured. EXAMPLES
[0045] The positive electrode plate was manufactured in the same manner as in Example 1, with the difference being that the selected lithium iron phosphate D 50 The particle size is 300 nm, and a positive electrode plate is manufactured. EXAMPLES
[0046] The positive electrode plate is manufactured in the same manner as in Example 1, except that the layered positive electrode materials selected are lithium cobalt oxide and lithium nickel cobalt aluminate, and the molar ratio of the two is 1:1. EXAMPLES
[0047] A positive electrode plate is manufactured in the same manner as in Example 1, except that the content of lithium iron phosphate in the positive electrode active material is 15.0%. EXAMPLES
[0048] A positive electrode plate was manufactured in the same manner as in Example 1, except that the content of lithium iron phosphate in the positive electrode active material was 2.0%. EXAMPLES
[0049] A positive electrode plate is manufactured in the same manner as in Example 1, except that the polyanion in the positive electrode active material is lithium iron manganese phosphate. Comparative Example 1
[0050] The positive electrode plate was manufactured in the same manner as in Example 1, with the difference being that the positive electrode active material was D 50 = 5.4μm LiNi 0.83 Co 0.13 Mn 0.04 O 2 The positive electrode plate is manufactured by containing only Comparative Example 2
[0051] The positive electrode plate was manufactured in the same manner as in Example 1, except that the positive electrode active material was a polyanion positive electrode. material The positive electrode plate is manufactured by using the above-mentioned method. Comparative Example 3
[0052] The positive electrode plate was manufactured in the same manner as in Example 1, with the difference being that the positive electrode active material was D 50 = 5.4μm LiNi 0.83 Co 0.13 Mn 0.04 O 2 The positive electrode active material contains only polyanion positive electrode material The positive electrode plate is manufactured by using the above-mentioned method. Comparative Example 4
[0053] The positive electrode plate was prepared in the same manner as in Example 1, with the difference being that the selected positive electrode active material sub-layer was prepared by using layered positive electrode material D 50 The particle size is four kinds, and the LiNi particles in the first positive electrode active material sublayer, the second positive electrode active material sublayer, the third positive electrode active material sublayer, and the fourth positive electrode active material sublayer are 0.83 Co 0.13 Mn 0.04 O 2 D 50 Positive electrode plates are manufactured with particle sizes of 0.6 μm, 3.0 μm, 7.0 μm, and 20.0 μm, respectively.
[0054] The positive plates in the above Examples 1 to 9 and Comparative Examples 1 to 4 are used to manufacture corresponding batteries according to the following method: The positive plate is laminated in order with a separator and a negative plate to obtain a bare cell, and the cell is then placed in a case, fired and dried, after which an electrolyte is injected, welded and sealed, and a battery is obtained through processes such as high-temperature aging, chemical conversion, and aging.
[0055] For the batteries manufactured using the positive electrode plates in Examples 1 to 9 and Comparative Examples 1 to 4, performance tests including an impedance performance test, a rate performance test, a cycle performance test, a safety performance test, and a charge state performance test were carried out. The specific data are shown in FIG. 1 and Table 1.
[0056] In the impedance performance test method, the battery is fully charged at 25°C with a constant current and constant voltage of 0.2C, left to stand, and then discharged to 2.5V with a constant current of 0.2C. This is repeated three times, and the third discharge capacity is taken as C0. The battery is adjusted to 50% SOC with a current of 0.2C0, and then discharged at a constant current of 1.5C for 30 seconds to calculate the magnitude of the impedance value.
[0057] In the rate performance test method, the battery is fully charged at a constant current and constant voltage of 0.2C at 25°C, left to stand, and then further discharged to 2.5V at a constant current of 0.2C. This is repeated three times, and the third discharge capacity is taken as C0. The battery is fully charged at constant current and constant voltage of 0.2C0 and 5.0C0, and then further fully discharged at the same current. The discharge capacity at 0.2C0 is taken as the standard, and the discharge capacity at 5.0C0 and its ratio are used as indicators for evaluating the rate performance.
[0058] In the cycle performance test method, the battery is fully charged at a constant current and constant voltage of 0.2C at 25°C, left to stand, and then further discharged to 2.5V at a constant current of 0.2C. This is repeated three times, and the third discharge capacity is taken as C0. The battery is then fully charged at a constant current and constant voltage of 1.0C0 in an environment of 45°C, and further discharged at a constant current of 1.0C0. 500 cycles are repeated in this manner, and the capacity retention is recorded.
[0059] In the safety performance test method, the stability of the DSC test electrode is used as an index to evaluate the safety performance. The battery is fully charged, the positive electrode plate is taken out into the glove box, an appropriate amount of positive electrode material is scraped off and placed in a crucible, a certain amount of electrolyte is added, and the battery is transferred to the device. The test atmosphere is pure argon gas, and the heating rate is 2℃ / min. The thermal runaway start temperature, thermal runaway peak temperature, and heat dissipation power are recorded respectively.
[0060] In the state of charge (SOC) performance test method, the battery was quickly fully charged at a current of 2.0 C, and the positive plate was taken out into a glove box and cut with an Ar ion beam to obtain the cross section of the plate. The cross section was then scanned using a Raman spectrum. The vibration levels of different metals and oxygen / different valence metals and oxygen are different, and the peak positions, peak shapes, and peak intensities in the Raman spectrum are different. -1 Peak and 470cm -1 By using the peak area ratio as an index for evaluating the SOC state, the ratio of each point within the scanned area can be obtained, i.e., the SOC distribution status within the area can be obtained, and the average SOC within the area can be calculated to characterize the actual SOC state of the electrode plate.
[0061] As shown in FIG. 1, the left side of FIG. 1 shows the SOC distribution of the battery prepared according to Example 1, and the right side of FIG. 1 shows the SOC distribution of the battery prepared according to Comparative Example 3. It can be seen that the SOC distribution in the positive electrode plate prepared in Example 1 is obviously uniform, which indicates that the polarization of the positive electrode plate is smaller, which is favorable for the insertion / ejection of lithium ions.
[0062] [Table 1]
[0063] As can be seen from Table 1, the effects of Examples 1 to 9 are higher than those of Comparative Examples 1 to 4. In one embodiment, in Examples 1 to 9, in terms of battery impedance, the battery impedance value can reach a minimum of 151 mΩ, indicating that the lower the battery impedance value, the higher the conductive performance of the battery; in terms of rate performance, the rate ratio is at most 99.3% and at most 86.2%, indicating that the higher the rate ratio, the more stable the electrochemical performance of the battery at different rates is, that is, the higher the rate performance is; and in terms of cycle performance, the cycle capacity retention rate is at its highest. The cycle capacity retention rate was 93.2% at the highest and 82.0% at the lowest. The higher the cycle capacity retention rate, the more stable the battery performance and the longer the service life. In terms of safety performance, the thermal runaway onset temperature was 204.2°C at the highest, the thermal runaway peak temperature was 210.2°C at the highest, and the heat dissipation power was 948.4 J / g at the lowest. The higher the thermal runaway onset temperature and the thermal runaway peak temperature, the more the battery can withstand high temperatures and is safer. The lower the heat dissipation power, the less the battery generates heat and the safer it is. In terms of SOC, the maximum was 98.7%. The higher the SOC ratio, the more uniform the SOC in the positive plate.
[0064] In comparison with Comparative Example 1, the particle size of the layered positive electrode material in the positive electrode active material layer in Comparative Example 1 is only one type, and the particle size distribution of Relation 1 as in Example 1 is not used. Therefore, the manufactured battery is worse than Example 1 in terms of impedance, rate, cycle capacity retention, safety performance and SOC. The battery impedance in Comparative Example 1 is 195 mΩ, which is larger than that of Example 1, indicating that the conductive performance of the battery is deteriorated, the rate is only 87.8%, the capacity retention is only 76.8%, the thermal runaway onset temperature and thermal runaway peak temperature are lower than those of Example 1, the heat dissipation function is higher than that of Example 1, and the SOC ratio is lower than that of Example 1.
[0065] In comparison with Comparative Example 2, no polyanion positive electrode material is added in Comparative Example 2, which affects the compression density of the positive plate and further affects the conductive performance of the positive plate. As can be seen from the data of Comparative Example 2, the battery manufactured in Comparative Example 2 is lower than that of Example 1 in terms of impedance, rate, cycle capacity retention, safety performance and SOC.
[0066] In comparison with Comparative Example 3, there is only one particle size in Comparative Example 3, and no polyanion positive electrode material is added. As can be seen from the data of Comparative Example 3, the battery produced in Comparative Example 3 is lower than that of Example 1 in impedance, rate, cycle capacity retention, safety performance and SOC.
[0067] In Comparative Example 4, the LiNi 0.83 Co 0.13 Mn 0.04 O 2 D 50 The particle size does not satisfy the relational formula 1 of the present disclosure, that is, the particle size between each layer does not show the regular distribution in the relational formula 1. As can be seen from the data of Comparative Example 4, the battery manufactured in Comparative Example 4 is lower than that of Example 1 in terms of impedance, rate, cycle capacity retention, safety performance and SOC. This is because, based on the relational formula 1 of the present disclosure, the LiNi 0.83 Co 0.13 Mn 0.04 O2 D 50 It will be explained that the electrical performance of the battery can be improved by adjusting the particle size.
[0068] As can be seen by comparing Example 5 with Examples 1 and 4, D 50 The performance effect of the positive electrode plate made with lithium iron phosphate having a particle size≦200 nm is higher.
[0069] As can be seen by comparing Examples 7 and 8 with Example 1, the performance effect of the positive electrode plate manufactured using the lithium iron phosphate positive electrode material having a mass percentage of 6.5% in the positive electrode active material is higher, and the present disclosure has discovered through more experimental data that the performance of the positive electrode plate manufactured when the auxiliary positive electrode material occupies 4.0% to 12.0% of the mass of the positive electrode active material in the positive electrode active material layer is excellent.
[0070] As can be seen from the experimental results of the examples and comparative examples in Table 1, by using a positive electrode plate that satisfies the particle size distribution of Relational Formula 1 of the present disclosure, it is possible to reduce polarization caused by differences in SOC state between large and small particles in the thickness direction of the positive electrode plate, eliminate polarization caused by non-uniform lithium insertion, reduce battery impedance, and improve rate and cycle performance. The polyanion positive electrode material has excellent structural stability, and by using it in combination, it not only improves cycle performance, but also improves safety performance (thermal stability).
[0071] The above examples merely show some embodiments of the present disclosure, and the description is specific and detailed, but should not be understood as limiting the patent scope of the present disclosure. However, those skilled in the art can make some modifications and improvements without departing from the concept of the present disclosure, and all of these belong to the scope of protection of the present disclosure. Therefore, the scope of protection of the patent of the present disclosure should be based on the scope of the attached claims.
Claims
1. a current collector; and a positive electrode active material layer disposed on the current collector, the positive electrode active material layer including m positive electrode active material sublayers, the positive electrode active material in each of the positive electrode active material sublayers including a main positive electrode material and an auxiliary positive electrode material, 50 The particle size satisfies the following: [0010] Here, m is an integer of 2 or more, n is an integer of 2 to m, and D 50 1 is the D of the main positive electrode material in the first positive electrode active material sub-layer 50 represents the particle size, and 50 n is the D of the main positive electrode material in the nth positive electrode active material sub-layer 50 a particle size, a distance from the nth positive electrode active material sub-layer to the current collector is greater than a distance from the (n-1)th positive electrode active material sub-layer to the current collector, D of the auxiliary positive electrode material 90 The particle size is the D of the main positive electrode material in the positive electrode active material sub-layer of the first layer. 10 Smaller than the particle size the primary positive electrode material is a layered positive electrode material, and the auxiliary positive electrode material is a polyanionic positive electrode material; the layered positive electrode material is at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganate, lithium nickel cobalt manganate, and lithium nickel cobalt aluminate; The polyanion positive electrode material is at least one of lithium iron phosphate, lithium iron manganese phosphate, lithium manganese phosphate, lithium vanadium phosphate, lithium vanadium fluorophosphate, lithium manganese silicate, lithium iron silicate, and lithium cobalt silicate.
2. D of the auxiliary positive electrode material 50 The positive electrode plate according to claim 1 , wherein the particle size is 200 nm or less.
3. D of the main positive electrode material in the n-1th positive electrode active material sublayer 90 The particle size is the D of the main positive electrode material in the nth positive electrode active material sub-layer. 10 The positive electrode plate according to claim 1 , characterized in that the particle size is less than or equal to the particle size.
4. The particle size of the main positive electrode material in the positive electrode active material layer is 4.0 μm≦D50 [m/2]+1 ≦8.0 μm, and the [m / 2] represents rounding down to an integer, and the D 50 [m/2]+1 is the D of the main positive electrode material in the positive electrode active material sub-layer of the [m / 2]+1th layer. 50 4. The positive electrode plate of claim 3, characterized in that it exhibits a grain size.
5. The positive electrode plate according to any one of claims 1 to 4, characterized in that the percentage of the surface density of the main positive electrode material in each of the first positive electrode active material sublayer to the mth positive electrode active material sublayer of the positive electrode active material layer with respect to the surface density of the main positive electrode material in the positive electrode active material layer exhibits a normal distribution.
6. In the positive electrode active material layer, the percentage of the surface density of the main positive electrode material in each positive electrode active material sub-layer relative to the surface density of the main positive electrode material in the positive electrode active material layer is ρ 1 ≦10.0%, ρ m ≦10.0%, ρ 2 ≧10.0%, ρ m-1 ≧10.0%, 40.0%≦ρ m/2 ≦60.0%, Here, m is an integer of 3 or more, and ρ 1 represents the percentage of the surface density of the main positive electrode material in the positive electrode active material sub-layer of the first layer relative to the surface density of the main positive electrode material in the positive electrode active material layer, and ρ 2 represents the percentage of the surface density of the main positive electrode material in the positive electrode active material sub-layer of the second layer relative to the surface density of the main positive electrode material in the positive electrode active material layer, and ρ mrepresents the percentage of the surface density of the main positive electrode material in the mth positive electrode active material sub-layer relative to the surface density of the main positive electrode material in the positive electrode active material layer, and the ρ m-1 represents the percentage of the surface density of the main positive electrode material in the (m-1)th positive electrode active material sub-layer relative to the surface density of the main positive electrode material in the positive electrode active material layer, and when m is an odd number, the ρ m/2 represents a percentage of the surface density of the main positive electrode material in the [m / 2]+1-th positive electrode active material sub-layer relative to the surface density of the main positive electrode material in the positive electrode active material layer, and the [m / 2] represents rounding down to an integer. When m is an even number, the ρ m/2 represents a percentage of the surface density of the main positive electrode material in at least one of the [m / 2]th layer of positive electrode active material sublayers and the [m / 2]+1th layer of positive electrode active material sublayers relative to the surface density of the main positive electrode material in the positive electrode active material layer.
7. The positive electrode active material sub-layer of each layer further includes a conductive agent and a binder, and the surface density of the positive electrode active material layer is 300 g / m 2 ≦ρ≦500g / m 2 The positive electrode plate according to any one of claims 1 to 4, wherein ρ represents a surface density of the positive electrode active material layer.
8. The positive electrode plate according to any one of claims 1 to 4, wherein the mass of the auxiliary positive electrode material is 0.5% to 20.0% of the mass of the positive electrode active material in the positive electrode active material layer.
9. The positive electrode plate according to any one of claims 1 to 4, wherein m is an integer between 3 and 6.
10. The positive electrode plate according to any one of claims 1 to 4, characterized in that m = 4.
11. A battery comprising the positive electrode plate according to any one of claims 1 to 10.
Citation Information
Patent Citations
Negative pole piece, electrochemical device and electronic device
CN111261834A
Electrode and electrochemical device
JP2008251401A
Electrode, lithium secondary battery, and method of manufacturing electrode
JP2013137928A
Electrode for secondary battery and lithium secondary battery including the same
JP2019501492A
Power storage element
WO2020017580A1