Pipe joint, piping structure, and method for manufacturing pipe joint

The pipe joint design with a foamed and non-foamed resin layer structure addresses the challenges of insulation, strength, and water-tightness, enhancing performance without thickness or foaming ratio increases.

JP7596413B2Active Publication Date: 2024-12-09SEKISUI CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023006097
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-11
Filing Date
2023-01-18
Publication Date
2024-12-09
Estimated Expiration
2040-03-19

AI Technical Summary

Technical Problem

Conventional pipe joints with foam layers for heat insulation face challenges in maintaining sufficient heat insulation, strength, and water-tightness without increasing the thickness or foaming ratio, leading to potential damage and poor work efficiency.

Method used

A pipe joint design incorporating a tubular body with a foamed resin layer and a non-foamed resin layer, composed of specific monomer units and a rubber component, with controlled ratios and dimensions to enhance heat insulation, strength, and water-tightness.

Benefits of technology

The design achieves improved heat insulation, moldability, and water-tightness without increasing the foam layer thickness or foaming ratio, ensuring durability and efficient assembly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596413000003
    Figure 0007596413000003
  • Figure 0007596413000004
    Figure 0007596413000004
  • Figure 0007596413000001
    Figure 0007596413000001
Patent Text Reader

Abstract

To provide a pipe joint and a piping structure which exhibit sufficient heat insulation properties without increasing the thickness of a foam layer or the expansion ratio of the foam layer, and which are excellent in formability, watertightness and strength. [Solution] The pipe fitting has a tubular main body (10) formed of a resin containing a copolymer having at least one selected from vinyl cyanide monomer units and acrylic monomer units, a rubber component, and an aromatic vinyl monomer unit, the main body (10) having a flow path therein, and one or more receiving portions (20a) formed integrally with the main body (10), the main body (10) having a foamed resin layer (30) and a non-foamed resin layer (50) covering the foamed resin layer (30), the contents of the rubber component in the foamed resin layer (30) and the non-foamed resin layer (50) being determined by pyrolysis gas chromatography mass spectrometry are within a specific range, and the length L from the base end (21a) to the opening end (22a) of the receiving portion (20a) is a and the thickness d of the receiving portion 20a at the open end 22a. a Relative to L a / d a Pipe fitting 1, where the value is 2.0 or more and 10.0 or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pipe fitting and a piping structure used for connecting drain pipes, etc. This application claims priority based on Japanese Patent Application No. 2019-54448 filed in Japan on March 22, 2019, and Japanese Patent Application No. 2019-165664 filed in Japan on September 11, 2019, the contents of which are incorporated herein by reference. [Background technology]

[0002] Conventionally, it has been common to prevent condensation around the pipes, which are made of steel pipes or synthetic resin pipes used to drain condensed water (drain) generated by air conditioning equipment, by covering the pipes with insulation material such as glass wool. However, the conventional method requires wrapping or covering the pipes with heat-insulating material in addition to the piping work, which results in poor work efficiency and may make it impossible to carry out the work in a small work space. For example, Patent Document 1 proposes a resin pipe joint having a foam layer that serves as a heat insulating layer. By providing the heat insulating layer, the pipe joint of Patent Document 1 can prevent condensation without covering with a heat insulating material after piping installation. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 2017-155868 Summary of the Invention [Problem to be solved by the invention]

[0004] However, in order to further improve the heat insulating properties of the pipe joint, it is necessary to either thicken the foam layer of the pipe joint or increase the foaming ratio of the foam layer. If the foam layer of the pipe joint is made thicker, the weight of the pipe joint increases, and there is a risk of the pipe joint being damaged by impact such as being dropped. If the foaming ratio of the foam layer is increased, there is a risk of the pipe joint being damaged by impact such as being dropped. In addition, pipe joints are required to be able to be molded into a desired shape (moldability) and to prevent water leakage from the joint with the piping (piping structure) (watertightness).

[0005] Therefore, an object of the present invention is to provide a pipe fitting and a piping structure which exhibit sufficient heat insulation properties without increasing the thickness of the foam layer or the foaming ratio of the foam layer, and which also has excellent moldability, water-stopping properties and strength. [Means for solving the problem]

[0006] In order to solve the above problems, the present invention has the following aspects. [1] A pipe fitting formed of a resin containing one or more monomers selected from vinyl cyanide-based monomer units and acrylic-based monomer units, and a copolymer having a rubber component and an aromatic vinyl-based monomer unit, the pipe fitting having a tubular main body having an internal flow path, and one or more receiving ports formed integrally with the main body, the main body having a foamed resin layer and a non-foamed resin layer covering the foamed resin layer, wherein the rubber component content of the foamed resin layer as determined by pyrolysis-gas chromatography-mass spectrometry is 10% by mass or more and 45% by mass or less with respect to the total mass of resin contained in the foamed resin layer, the rubber component content of the non-foamed resin layer as determined by pyrolysis-gas chromatography-mass spectrometry is 10% by mass or more and 45% by mass or less with respect to the total mass of resin contained in the non-foamed resin layer, and the ratio L / d of the length L from the base end to the open end of the receiving port to the thickness d of the receiving port at the open end is 2.0 or more and 10.0 or less. [2] The pipe fitting according to [1], wherein the thermal resistance value of the main body is 0.04 K / W or more. [3] A piping structure comprising the pipe fitting according to [1] or [2] and a pipe member inserted and connected to the receiving portion of the pipe fitting. Effect of the Invention

[0007] According to the pipe joint and piping structure of the present invention, sufficient heat insulation is exhibited without increasing the thickness of the foam layer or the expansion ratio of the foam layer, and the pipe joint and piping structure are excellent in moldability, water stoppage property and strength. [Brief description of the drawings]

[0008] [Figure 1] 1 is a cross-sectional view showing a pipe joint according to an embodiment of the present invention. [Diagram 2] 1 is a plan view showing a piping structure according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Pipe fittings] BEST MODE FOR CARRYING OUT THE PRESENTLY PREFERRED EMBODIMENTS A pipe joint according to an embodiment of the present invention will now be described with reference to the drawings. As shown in Fig. 1, the pipe joint 1 of this embodiment is an example of a joint used to connect a drain pipe (a three-way branching T-shaped pipe joint commonly called "tees"). The pipe joint 1 has a first pipe axis O1 and a second pipe axis O2. The two pipe axes O1 and O2 intersect with each other at an angle of 90.0°±1.1°. The pipe joint 1 has a tubular main body portion 10 having a flow passage (for example, a drain flow passage) therein, and three socket portions 20a, 20b, and 20c formed integrally with the main body portion 10.

[0010] The main body 10 has a foamed resin layer 30 and a non-foamed resin layer 50. Both sides of the foamed resin layer 30 are covered with the non-foamed resin layer 50. That is, the wall of the main body 10 has a three-layer structure in which, from the flow path side, the non-foamed resin layer 50, the foamed resin layer 30, and the non-foamed resin layer 50 are located. The receiving portion 20a, the receiving portion 20b, and the receiving portion 20c are formed of the non-foamed resin layer 50. That is, the walls of the receiving portion 20a, the receiving portion 20b, and the receiving portion 20c have a single-layer structure formed of the non-foamed resin layer 50. From the viewpoint of enhancing water-stopping properties, it is preferable that the receiving portions 20a, 20b, and 20c are transparent. That is, from the viewpoint of facilitating confirmation of the connection state between the pipe fitting 1 and the pipe member inserted and connected to the receiving portions, it is preferable that the non-foamed resin layer 50 is transparent. Here, "transparent" means transparent enough that the inserted pipe and the adhesive applied to the inner surface of the receiving portion can be visually recognized from the outer surface of the receiving portion, and may be translucent or colored transparent. More specifically, the haze of the receiving portion measured in accordance with JIS K 7136:2000 is preferably 1 or more and 70 or less, and more preferably 1 or more and 60 or less.

[0011] The main body 10, which is a straight pipe, has openings 10a, 10b formed at both ends in the direction of the first pipe axis O1, and each opening has a cylindrical socket portion 20a, 20b. An opening 10c formed in the main body 10 in the direction of the second tube axis O2 is provided with a cylindrical socket portion 20c. In the main body 10, an injection gate 14 is provided at a position facing the opening 10c across the first tube axis O1, and serves as a position from which injection is performed during molding.

[0012] Inner diameter R of the receiving portion 20a 20a In order to insert and connect a tubular member having a foam layer, the inner diameter R of the opening 10a of the main body 10 is 10a Specifically, the ratio R 20a / R 10a However, it is preferably more than 1.0 and 2.0 or less, more preferably 1.2 or more and 1.8 or less, and even more preferably 1.4 or more and 1.6 or less. Similarly, the inner diameter R of the receiving portion 20b 20b is the inner diameter R of the opening 10b of the main body 10 10b Specifically, the ratio R 20b / R 10b However, it is preferably more than 1 and 2.0 or less, more preferably 1.2 or more and 1.8 or less, and even more preferably 1.4 or more and 1.6 or less. Similarly, the inner diameter R of the receiving portion 20c 20c is the inner diameter R of the opening 10c of the main body 10 10c Specifically, the ratio R 20c / R 10c However, it is preferably more than 1 and 2.0 or less, more preferably 1.2 or more and 1.8 or less, and even more preferably 1.4 or more and 1.6 or less.

[0013] At the boundary between the receiving portion 20a and the main body portion 10, an inner diameter R 20a and inner diameter R 10aA step 12a is formed based on the difference between the height of the pipe and the width of the receiving portion 20. The step 12a functions as a stopper that prevents the pipe member inserted into the receiving portion 20a from entering the receiving portion 20a. At the boundary between the receiving portion 20b and the main body portion 10, an inner diameter R 20b and inner diameter R 10b A step 12b is formed based on the difference between the height and the width of the receiving portion 20. The step 12b functions as a stopper that prevents the pipe member inserted into the receiving portion 20b from entering the receiving portion 20b. At the boundary between the receiving portion 20c and the main body portion 10, an inner diameter R 20c and inner diameter R 10c A step 12c is formed based on the difference between the height of the pipe and the depth of the receiving portion 20. The step 12c functions as a stopper that prevents the pipe member inserted into the receiving portion 20c from entering the receiving portion 20.

[0014] The step 12a is formed by a peripheral wall 13 located on the periphery of the opening 10a of the main body 10. The peripheral wall 13 is formed around the entire inner periphery of the cylindrical receiving portion 20a and has an annular shape. The step 12b is formed by a peripheral wall 13 located on the periphery of the opening 10b of the main body 10. The peripheral wall 13 is formed around the entire inner periphery of the cylindrical receiving portion 20b, and is annular in shape. The step 12c is formed by a peripheral wall 13 located on the periphery of the opening 10c of the main body 10. The peripheral wall 13 is formed around the entire inner periphery of the cylindrical receiving portion 20c, and is annular in shape.

[0015] The peripheral wall 13 is solid. The inside of the peripheral wall 13 is formed of a foamed resin layer 30, and the foamed resin layer 30 is covered with a non-foamed resin layer 50. It is preferable that a foamed resin layer 30 is formed around the entire periphery of the peripheral wall 13. When the foamed resin layer 30 is formed around the entire periphery of the peripheral wall 13, the base ends of the receiving portions 20a, 20b, and 20c also have thermal insulation properties, and the thermal insulation properties of the pipe fitting 1 can be further improved. When the pipe member inserted into the receiving portion 20a, 20b, or 20c has a foam layer, it is preferable to provide an annular water-stopping member between the end face of the pipe member and the peripheral wall 13. An example of the annular water-stopping member is a foam packing. When the foam layer of the pipe member is an open-cell structure, it is preferable to provide an annular water-stopping member between the end face of the pipe member and the peripheral wall 13. By providing the water-stopping member, it is possible to prevent drain water from entering the foam layer of the pipe member. When the foam layer of the pipe member is a closed cell, it is not necessary to provide a water-stopping member between the end face of the pipe member and the peripheral wall 13. However, when the pipe member is cut at an angle, drain water may be retained between the end face of the pipe member and the peripheral wall 13, and therefore it is preferable to provide a water-stopping member.

[0016] The socket portion 20a extends in the direction of the first pipe axis O1 from the base end 21a. The base end 21a is located at the boundary between the socket portion 20a and the main body portion 10. The length from the base end 21a to the open end 22a of the socket portion 20a is L. a The length L a is equal to the length of the socket 20a. The thickness of the socket 20a at the open end 22a is d a The thickness d a is equal to the socket thickness of the socket portion 20a. The socket portion 20b extends in the direction of the first pipe axis O1 from the base end 21b. The base end 21b is located at the boundary between the socket portion 20b and the main body portion 10. The length from the base end 21b to the open end 22b of the socket portion 20b is L. b The length L b is equal to the length of the socket 20b. The thickness of the socket 20b at the open end 22b is d b The thickness d b is equal to the socket thickness of the socket portion 20b. The socket portion 20c extends in the direction of the second pipe axis O2 from the base end 21c. The base end 21c is located at the boundary between the socket portion 20c and the main body portion 10. The length from the base end 21c of the socket portion 20c to the open end 22c is L. c The length L c is equal to the length of the socket 20c. The thickness of the socket 20c at the open end 22c is d c The thickness d c is equal to the socket thickness of the socket portion 20c.

[0017] The length L from the base end 21a to the opening end 22a of the receiving portion 20a aand the thickness d of the receiving portion 20a at the open end 22a. a (hereinafter, "L a / d a The ratio is from 2.0 to 10.0, preferably from 2.0 to 9.0, more preferably from 2.5 to 8.0, even more preferably from 3.0 to 7.0, and particularly preferably from 3.5 to 6.0. L a / d a When the ratio is equal to or greater than the lower limit, the foamed resin layer 30 is easily prevented from penetrating into the receiving portion 20a, and the strength of the receiving portion 20a is easily prevented from decreasing. a / d a When the ratio is equal to or greater than the lower limit, the length L of the receiving portion 20a a Since the length is sufficiently long, the adhesive strength of the pipe or the like inserted into the pipe fitting 1 is sufficient, and the waterproofing property can be further improved. L a / d a When the ratio is equal to or less than the upper limit, the thickness d a is sufficiently thick, so that the pipe joint 1 is less likely to be destroyed by expansion and contraction fatigue. a / d a If the ratio is equal to or less than the upper limit, the length L a If the length of the die is not too long, the resin forming the receiving portion 20a can be easily filled up to the end of the die, and molding defects due to insufficient filling (also called "short") are unlikely to occur. a / d a When the ratio is equal to or less than the above upper limit, the formability of the pipe joint 1 can be further improved. L a / d a The ratio can be adjusted by the shape of the molding die. L at the socket portion 20b of the pipe fitting 1 b / d b The ratio is L a / d a Similar to ratio. L at the socket portion 20c of the pipe fitting 1 c / d c The ratio is L a / d a Similar to ratio.

[0018] The melt mass flow rate (hereinafter, also referred to as "MFR") of the pipe fitting 1 is, for example, preferably 3 g / 10 min or more and 90 g / 10 min or less, more preferably 4 g / 10 min or more and 80 g / 10 min or less, even more preferably 5 g / 10 min or more and 70 g / 10 min or less, and particularly preferably 6 g / 10 min or more and 60 g / 10 min or less. If the MFR of the pipe fitting 1 is equal to or more than the above lower limit, it is easy to fill the resin up to the end of the mold when manufacturing the pipe fitting 1, and molding defects due to insufficient filling, which are particularly likely to occur at the receiving port, are unlikely to occur. In other words, if the MFR of the pipe fitting 1 is equal to or more than the above lower limit, the moldability of the pipe fitting 1 can be further improved. If the MFR of the pipe fitting 1 is equal to or less than the above upper limit, the molecular weight is not too low, and the pipe fitting 1 has excellent strength and chemical resistance. The MFR of the pipe fitting 1 can be measured in accordance with JIS K 7210:1999 at a test temperature of 220°C and a test load of 10 kg.

[0019] The thermal resistance value of the main body 10 is preferably 0.04 K / W or more, more preferably 0.05 K / W to 0.50 K / W or less, even more preferably 0.06 K / W to 0.45 K / W or less, particularly preferably 0.07 K / W to 0.40 K / W or less, and most preferably 0.08 K / W to 0.35 K / W or less. When the thermal resistance value of the main body 10 is equal to or greater than the lower limit, the heat insulation of the pipe fitting 1 can be further improved. When the thermal resistance value of the main body 10 is equal to or less than the upper limit, the strength of the main body 10 is sufficient, and in addition, the pipe fitting 1 can be made lightweight. The thermal resistance value of the main body 10 can be increased by lowering the thermal conductivity of the main body 10 or by increasing the thickness (wall thickness) of the main body 10 through the composition and type of resin, including the copolymer described below, or through the molding conditions of the pipe fitting 1. A typical drain pipe has an outer diameter of 30 mm to 80 mm and a wall thickness of about 5 mm to 10 mm, and the wall thickness of the main body of the pipe fitting 1 used to connect such a drain pipe is set to be 8 mm or more and 20 mm or less. The thermal resistance value of the main body 10 is calculated from the thermal conductivity (W / m K) measured in accordance with JIS A 1412-1:2016 and the thickness (m) of the main body 10 at the point where the thermal conductivity is measured, using the following formula (1). Thermal resistance (K / W) = thickness (m) / thermal conductivity (W / m K) (1)

[0020] <Foamed resin layer> The foamed resin layer 30 is formed by foaming and molding a foamable resin composition. The pipe fitting 1 of this embodiment has the foamed resin layer 30, and thus has excellent heat insulating properties.

[0021] The expansion ratio of the foamed resin layer 30 is preferably 1.0 to 8.0 times, more preferably 1.1 to 5.0 times, and even more preferably 1.2 to 3.0 times. By setting the expansion ratio within the above range, it is possible to achieve both high heat insulating performance and impact resistance. The expansion ratio can be adjusted by the type or amount of resin, the type or amount of foaming agent, production conditions, and the like. The expansion ratio is measured in accordance with the method of 6.2(a) or 6.2(b) described in JIS K 9798:2006.

[0022] In the foamed resin layer 30, a plurality of cells are formed, the walls of the cells are substantially free of pores, and at least some of the cells are closed cells that are not interconnected. The closed cell ratio is preferably 85% or more, more preferably 90% or more. The upper limit is not particularly limited, but is substantially 99% or less. Within the above range, low thermal conductivity can be maintained for a long period of time, and heat insulation is excellent. The closed cell ratio is measured in accordance with JIS K 7138:2006.

[0023] <Foamable resin composition> The foamable resin composition of the present embodiment contains one or more selected from vinyl cyanide monomer units and acrylic monomer units, a resin containing a copolymer having a rubber component and an aromatic vinyl monomer unit (hereinafter also referred to as a "first resin"), and a foaming agent. In this specification, the term "unit" refers to a structural portion derived from a monomer compound (monomer) before polymerization, for example, a "vinyl cyanide monomer unit" refers to a "structural portion derived from a vinyl cyanide monomer (acrylonitrile)." The content ratio of each monomer unit in a polymer corresponds to the content ratio of the monomer in the monomer mixture used in the production of the polymer.

[0024] (First Resin) The first resin contains at least one selected from vinyl cyanide monomer units and acrylic monomer units, and a copolymer having a rubber component and an aromatic vinyl monomer unit. The copolymer of the present embodiment is preferably a resin obtained by polymerizing at least one selected from vinyl cyanide monomer units and acrylic monomer units with an aromatic vinyl monomer in the presence of a rubber component. In this case, the copolymer is a so-called "graft copolymer." However, in the present invention, the copolymer is not limited to one obtained by graft copolymerization, and may be one produced by a polymer blending method. In this specification, the rubber component refers to diene rubber such as polybutadiene or polyisoprene, or acrylic rubber. Examples of the rubber component include diene rubbers such as polymers of diene compounds such as butadiene, isoprene, ethylene, and propylene, and examples of the acrylic rubbers include polymers of acrylic esters such as ethyl acrylate, butyl acrylate, butoxyethyl acrylate, and methoxyethyl acrylate. Examples of the vinyl cyanide monomer include acrylonitrile and methacrylonitrile, with acrylonitrile being preferred. Examples of the acrylic monomer include monomers constituting acrylic resins. Examples of the acrylic resin include polymers of acrylic acid esters and polymers of methacrylic acid esters. Examples of the polymers of acrylic acid esters include polymethyl acrylate, polyethyl acrylate, and polyglycidyl acrylate. Examples of the polymers of methacrylic acid esters include polymethyl methacrylate, polyethyl methacrylate, and polyglycidyl methacrylate. That is, examples of the acrylic monomers include methyl acrylate, ethyl acrylate, glycidyl acrylate, methyl methacrylate, ethyl methacrylate, and glycidyl methacrylate, with methyl methacrylate being preferred. Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, β-methylstyrene, 4-methylstyrene, β-bromostyrene, and the like, with styrene and α-methylstyrene being preferred. Specific examples of the copolymer of the present embodiment include acrylonitrile-butadiene-styrene copolymer (ABS resin), acrylonitrile-ethylene propylene diene-styrene copolymer (AES resin), acrylonitrile-acrylic rubber-styrene copolymer (AAS resin), methyl methacrylate-butadiene-styrene copolymer (MBS resin), and the like, and further, a mixture of these may be used.

[0025] The content of the rubber component in the first resin is 10% by mass or more and 45% by mass or less, preferably 15% by mass or more and 40% by mass or less, and more preferably 20% by mass or more and 35% by mass or less, based on the total mass of the first resin. When the content of the rubber component is equal to or more than the lower limit, the strength of the pipe fitting 1 is easily improved. When the content of the rubber component is equal to or less than the upper limit, the flowability during molding of the pipe fitting 1 is easily improved.

[0026] In addition, it is also a preferred embodiment of the present invention that the rubber component in the first resin contains both a diene rubber and an acrylic rubber. By containing both a diene rubber and an acrylic rubber in the rubber component, not only impact resistance but also chemical resistance can be improved. When the rubber component contains both a diene rubber and an acrylic rubber, the content of the diene rubber is preferably 5 mass% or more and 40 mass% or less, more preferably 10 mass% or more and 40 mass% or less, even more preferably 15 mass% or more and 40 mass% or less, and particularly preferably 20 mass% or more and 40 mass% or less, relative to the total mass of the first resin. When the rubber component contains both diene rubber and acrylic rubber, the content of the acrylic rubber is preferably 0.1% by mass to 10% by mass, more preferably 0.3% by mass to 5% by mass, and even more preferably 0.5% by mass to 3% by mass, based on the total mass of the first resin. When the content of the acrylic rubber is within the above numerical range, the chemical resistance can be further improved, particularly when the content of the diene rubber is 15% by mass or more based on the total mass of the first resin. Note that the "content of the acrylic rubber" referred to here refers to the "content of the acrylic acid ester" added to the first resin.

[0027] The content of the vinyl cyanide monomer unit in the first resin is preferably 10% by mass or more and 50% by mass or less, more preferably 15% by mass or more and 45% by mass or less, based on the total mass of the first resin. When the content of the vinyl cyanide monomer unit is equal to or more than the lower limit, the tensile strength can be improved. When the content of the vinyl cyanide monomer unit is equal to or less than the upper limit, the impact strength can be improved.

[0028] The content of the acrylic monomer unit in the first resin is preferably 20% by mass or more and 60% by mass or less, and more preferably 30% by mass or more and 50% by mass or less, based on the total mass of the first resin. When the content of the acrylic monomer unit is within the above numerical range, it is easy to increase the strength and transparency of the pipe joint 1. Therefore, the water-stopping property of the pipe joint 1 can be further improved.

[0029] The content of the aromatic vinyl monomer unit in the first resin is preferably 15% by mass or more and 60% by mass or less, more preferably 20% by mass or more and 50% by mass or less, based on the total mass of the first resin. When the content of the aromatic vinyl monomer unit is equal to or more than the lower limit, the indentation hardness can be improved. When the content of the aromatic vinyl monomer unit is equal to or less than the upper limit, the impact strength can be improved. The first resin may contain any monomer unit other than the vinyl cyanide monomer unit, the acrylic monomer unit, and the aromatic vinyl monomer unit, and examples thereof include a polycarbonate resin and its monomers.

[0030] The content of each component in the first resin is determined by analysis using pyrolysis gas chromatography mass spectrometry (hereinafter also referred to as "PGC / MS"). An example of measurement conditions using PGC / MS is shown below. [Measurement conditions] ·Device Pyrolysis apparatus: PY-2020iD (Frontier Labs, Inc.). Gas chromatograph: GC 2010 (Shimadzu Corporation). Mass spectrometer: GCMS-QP 2010 (Shimadzu Corporation). Pyrolysis conditions Pyrolysis temperature: 550℃. Interface temperature: 250℃. Gas chromatographic conditions. Carrier flow rate: 1 ml / min (He). Split ratio: 100:1. Separation column: DB-1 (1.00 μm, 0.25 mm φ × 30 m). Oven temperature: 40℃(3min)-320℃(10min). ·Mass spectrometry conditions Interface temperature: 250℃. Ionization temperature: 220℃. Mass range: 28-700 m / z. Voltage: 1.2kV.

[0031] A method for calculating the content of each component in the first resin by PGC / MS measurement will be described. First, each component constituting the first resin is pyrolyzed and separated by pyrolysis gas chromatography, and a pyrolysis pattern (pyrogram) is obtained in which each component is recorded as a peak. Next, for each peak in the pyrolysis pattern, the acrylonitrile, rubber component, and styrene component are identified by a mass spectrum obtained by a mass spectrometer. Here, since the depolymerization rate (the rate at which a polymer decomposes into monomers) due to thermal decomposition differs for each component, acrylonitrile, rubber component, and styrene, the peak area (Z) of each component is calculated by dividing the area (X) of each peak in the pyrogram by the depolymerization rate (Y) of each component due to thermal decomposition. The depolymerization rates (Y) of each component are acrylonitrile: 0.15, rubber component: 0.10, and styrene: 1.0. For example, when the first resin contains an acrylic resin such as polymethyl methacrylate as another resin, the depolymerization rate of the acrylic resin is 1.0. The ratio (Z / T) of the peak area (Z) of each component in the thermal decomposition pattern to the sum (T) is defined as the content (mass %) of each component in the first resin.

[0032] Table 1 shows an example of the content of each component obtained by PGC / MS measurement of acrylonitrile-butadiene-styrene copolymer (ABS resin) containing acrylic resin. In Table 1, "retention time" means the time at which each component is thermally decomposed and appears as a peak in the pyrogram. "Sample amount" is the mass of the ABS resin subjected to analysis.

[0033] [Table 1]

[0034] The MFR of the foamable resin composition of this embodiment is, for example, preferably 3 g / 10 min to 90 g / 10 min, more preferably 4 g / 10 min to 80 g / 10 min, even more preferably 5 g / 10 min to 70 g / 10 min, and particularly preferably 6 g / 10 min to 60 g / 10 min. If the MFR of the foamable resin composition of this embodiment is equal to or greater than the lower limit, the resin is easily filled up to the end of the mold, and molding defects due to insufficient filling, which are particularly likely to occur at the receiving portion, are less likely to occur. In other words, if the MFR of the foamable resin composition of this embodiment is equal to or greater than the lower limit, the moldability of the pipe joint 1 can be further improved. When the MFR of the foamable resin composition of the present embodiment is equal to or less than the above upper limit, the molecular weight is not too low, and the strength and chemical resistance are excellent. The MFR of the foamable resin composition of the present embodiment can be measured in accordance with JIS K 7210:1999 at a test temperature of 220° C. and a test load of 10 kg. The MFR of the foamable resin composition of this embodiment is the same as the MFR of the pipe fitting 1 of this embodiment.

[0035] In the foamable resin composition, the content of the first resin relative to the total mass of the foamable resin composition is preferably from 45 to 90 mass%, more preferably from 50 to 85 mass%.

[0036] The foamable resin composition of the present embodiment may contain one or more types selected from vinyl cyanide monomer units and acrylic monomer units, and a resin other than the copolymer having a rubber component and an aromatic vinyl monomer unit. Examples of the other resins include polyvinyl resins, polyester resins, polyether resins, polyimide resins, etc. These may be used alone or in combination of two or more kinds.

[0037] In the foamable resin composition, the content of one or more selected from vinyl cyanide monomer units and acrylic monomer units, and a copolymer consisting of a rubber component and an aromatic vinyl monomer unit, relative to the total mass of the first resin, is preferably 70 mass% or more and 100 mass% or less, and more preferably 85 mass% or more and 100 mass% or less.

[0038] (foaming agent) As the foaming agent, either a volatile foaming agent or a decomposition type foaming agent may be used. Examples of the volatile blowing agent include aliphatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, ethers, ketones, etc. Among these, examples of the aliphatic hydrocarbons include propane, butane (normal butane, isobutane), pentane (normal pentane, isopentane, etc.), etc., and examples of the alicyclic hydrocarbons include cyclopentane, cyclohexane, etc. Examples of the halogenated hydrocarbons include one or more halogenated hydrocarbons such as trichlorofluoromethane, trichlorotrifluoroethane, tetrafluoroethane, chlorodifluoroethane, difluoroethane, etc. Furthermore, examples of the ethers include dimethyl ether, diethyl ether, etc., and examples of the ketones include acetone, methyl ethyl ketone, etc.

[0039] Examples of decomposition type foaming agents include inorganic foaming agents such as sodium bicarbonate (sodium hydrogen carbonate), sodium carbonate, ammonium bicarbonate, ammonium nitrite, azide compounds, and sodium borohydride, and organic foaming agents such as azodicarbonamide, barium azodicarboxylate, and dinitrosopentamethylenetetramine. Other gases such as carbon dioxide, nitrogen, and air may also be used as the foaming agent. From the viewpoint of excellent foaming performance, the decomposition type foaming agents are preferred, and among them, sodium bicarbonate and azodicarbonamide are more preferred. These may be used alone or in combination of two or more. The content of the foaming agent is preferably from 0.1 to 8 parts by mass, more preferably from 1 to 5 parts by mass, and even more preferably from 1 to 3 parts by mass, relative to 100 parts by mass of the first resin.

[0040] The foamable resin composition of the present embodiment may contain other components (optional components) in addition to the first resin and the foaming agent, as long as the effects of the present invention are not impaired.

[0041] The content of the optional component is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, based on 100 parts by mass of the first resin.

[0042] The foamable resin composition of the present embodiment may include a first resin, a foaming agent, and an optional component. The foamable resin composition may be a mixture in which all components are mixed in advance, or may be a form in which all or a part of all components are mixed in a molding machine. The mixture in which all components are mixed in advance may be in the form of a powder or pellets.

[0043] <Non-foamed resin layer> The non-foamed resin layer 50 is formed by molding a non-foamable resin composition. By having the non-foamed resin layer 50, the pipe joint 1 of the present embodiment can have an increased strength. The non-foamed resin layer 50 covers the foamed resin layer 30 .

[0044] <Non-foamable resin composition> The non-foamable resin composition of the present embodiment contains one or more selected from vinyl cyanide monomer units and acrylic monomer units, and a resin containing a copolymer composed of a rubber component and an aromatic vinyl monomer unit (hereinafter, also referred to as a "second resin").

[0045] (Second Resin) The second resin is a resin containing at least one selected from vinyl cyanide monomer units and acrylic monomer units, and a copolymer formed of a rubber component and an aromatic vinyl monomer unit. The second resin may be the same as the first resin or may be different.

[0046] The content of the rubber component in the second resin is 10% by mass or more and 45% by mass or less, preferably 15% by mass or more and 40% by mass or less, and more preferably 20% by mass or more and 35% by mass or less, based on the total mass of the second resin. When the content of the rubber component is equal to or more than the lower limit, the strength of the pipe fitting 1 is easily improved. When the content of the rubber component is equal to or less than the upper limit, the flowability during molding of the pipe fitting 1 is easily improved. The second resin constitutes the receiving portions 20a, 20b, and 20c. From the viewpoint of further improving the impact resistance of the pipe fitting 1, it is preferable that the content of the rubber component in the second resin is greater than the content of the rubber component in the first resin. In this specification, when the second resin contains an acrylic monomer unit, the monomer component that is the raw material of the acrylic rubber is not included in the rubber component.

[0047] In a preferred embodiment of the present invention, the rubber component in the second resin contains both a diene rubber and an acrylic rubber. By containing both a diene rubber and an acrylic rubber in the rubber component, not only impact resistance but also chemical resistance can be improved. When the rubber component contains both a diene rubber and an acrylic rubber, the content of the diene rubber is preferably 5 mass% or more and 40 mass% or less, more preferably 10 mass% or more and 40 mass% or less, even more preferably 15 mass% or more and 40 mass% or less, and particularly preferably 20 mass% or more and 40 mass% or less, relative to the total mass of the second resin. When the rubber component contains both diene rubber and acrylic rubber, the content of the acrylic rubber is preferably 0.1% by mass to 10% by mass, more preferably 0.3% by mass to 5% by mass, and even more preferably 0.5% by mass to 3% by mass, based on the total mass of the second resin. When the content of the acrylic rubber is within the above numerical range, the chemical resistance can be further improved, particularly when the content of the diene rubber is 15% by mass or more based on the total mass of the second resin. Note that the "content of the acrylic rubber" referred to here refers to the "content of the acrylic acid ester" added to the first resin.

[0048] The content of the vinyl cyanide monomer unit in the second resin is preferably 10% by mass or more and 50% by mass or less, more preferably 15% by mass or more and 45% by mass or less, based on the total mass of the second resin. When the content of the vinyl cyanide monomer unit is equal to or more than the lower limit, the tensile strength can be improved. When the content of the vinyl cyanide monomer unit is equal to or less than the upper limit, the impact strength can be improved.

[0049] The content of the acrylic monomer unit in the second resin is preferably 20% by mass or more and 60% by mass or less, and more preferably 30% by mass or more and 50% by mass or less, based on the total mass of the second resin. When the content of the acrylic monomer unit is within the above numerical range, it is easy to increase the strength and transparency of the pipe joint 1. Therefore, the water-stopping property of the pipe joint 1 can be further improved.

[0050] The content of the aromatic vinyl monomer unit in the second resin is preferably 15% by mass or more and 60% by mass or less, more preferably 20% by mass or more and 50% by mass or less, based on the total mass of the second resin. When the content of the aromatic vinyl monomer unit is equal to or more than the lower limit, the indentation hardness can be improved. When the content of the aromatic vinyl monomer unit is equal to or less than the upper limit, the impact strength can be improved.

[0051] The content of each component in the second resin is determined by analysis using PGC / MS. The measurement conditions may be the same as those for the first resin.

[0052] The MFR of the non-foamable resin composition of this embodiment is, for example, preferably 3 g / 10 min or more and 90 g / 10 min or less, more preferably 4 g / 10 min or more and 80 g / 10 min or less, even more preferably 5 g / 10 min or more and 70 g / 10 min or less, and particularly preferably 6 g / 10 min or more and 60 g / 10 min or less. When the MFR of the non-foamable resin composition of this embodiment is equal to or more than the above lower limit, the resin is easily filled up to the end of the mold, and molding defects due to insufficient filling, which are particularly likely to occur at the receiving portion, are unlikely to occur. That is, when the MFR of the non-foamable resin composition of this embodiment is equal to or more than the above lower limit, the moldability of the pipe joint 1 can be further improved. When the MFR of the non-foamable resin composition of this embodiment is equal to or less than the above upper limit, the molecular weight is not too low, and the strength and chemical resistance are excellent. From the viewpoint of making it easier to fill the resin into the mold up to the edges, the MFR of the non-foamable resin composition is preferably higher than the MFR of the foamable resin composition. The MFR of the non-foamable resin composition of this embodiment can be measured in the same manner as for the MFR of the foamable resin composition of this embodiment.

[0053] In the non-foamable resin composition, the content of the second resin relative to the total mass of the non-foamable resin composition is preferably 50 mass% or more and 100 mass% or less, more preferably 70 mass% or more and 100 mass% or less, and even more preferably 80 mass% or more and 100 mass% or less.

[0054] The non-foamable resin composition of the present embodiment may contain one or more types selected from vinyl cyanide monomer units and acrylic monomer units, and a resin other than the copolymer composed of a rubber component and an aromatic vinyl monomer unit. Examples of the other resins include polyvinyl resins, polyester resins, polyether resins, polyimide resins, etc. These may be used alone or in combination of two or more kinds.

[0055] In the non-foamable resin composition, the content of one or more selected from vinyl cyanide monomer units and acrylic monomer units, and the copolymer consisting of a rubber component and an aromatic vinyl monomer unit, relative to the total mass of the second resin, is preferably from 40 mass% to 100 mass%, more preferably from 45 mass% to 100 mass%, and even more preferably from 50 mass% to 100 mass%.

[0056] The non-foamable resin composition of the present embodiment may contain other components (optional components) in addition to the second resin, as long as the effects of the present invention are not impaired. Optional components include colorants, flame retardants, antioxidants, ultraviolet absorbers, and light stabilizers.

[0057] The content of the optional component is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, based on 100 parts by mass of the second resin. The non-foamed resin layer 50 does not need to contain the foaming agent, but may contain the foaming agent. The amount of the foaming agent contained in the non-foamed resin layer 50 is preferably 0 parts by mass or more and 8 parts by mass or less, more preferably 0 parts by mass or more and 5 parts by mass or less, even more preferably 0 parts by mass or more and 3 parts by mass or less, and particularly preferably 0 parts by mass or more and less than 1 part by mass, relative to 100 parts by mass of the second resin. The expansion ratio in the non-foamed resin layer 50 is preferably 1.0 times, but low expansion ratios of 1.5 times or less are not excluded from the present invention.

[0058] The non-foamable resin composition of the present embodiment may contain a second resin and an optional component. The non-foamable resin composition may be a mixture in which all components are mixed in advance, or may be a form in which all or a part of all components are mixed in a molding machine. The mixture in which all components are mixed in advance may be in the form of a powder or pellets. The non-foamable resin composition of this embodiment forms the non-foamed resin layer 50 and covers the outer surface of the pipe fitting 1. In addition, in the non-foamable resin composition of this embodiment, the content of the rubber component in the second resin is 10 mass % or more and 45 mass % or less with respect to the total mass of the second resin. Therefore, the non-foamed resin layer 50 has excellent strength, and the pipe fitting 1 has excellent strength.

[0059] <Manufacturing method of pipe joints> The fitting is manufactured by injection molding or extrusion. For example, a pipe fitting having a desired expansion ratio can be obtained by heating and melting the foamable resin composition, injecting it into a mold, heating it at a desired temperature for a desired time, and cooling it at a desired temperature for a desired time. In the case of extrusion molding, the foamable resin composition is heated and melted, injected from an extruder into a mold, and heated at a desired temperature for a desired time to foam and mold the foamable resin composition. After cooling at a desired temperature for a desired time, the composition is cut to a desired length to obtain a pipe fitting having a desired expansion ratio.

[0060] In an injection molding machine, the temperature of the foamable resin composition immediately before being injected into a mold (molding temperature) is preferably 200° C. or higher and 280° C. or lower, more preferably 220° C. or higher and 260° C. or lower. When the molding temperature is within the above numerical range, the foamable resin composition is sufficiently melted, and good fluidity of the foamable resin composition is obtained. In addition, when the non-foamable resin composition contains an acrylic resin, the transparency of the pipe fitting 1 can be increased by setting the molding temperature to the above lower limit or higher. The time for molding in a mold is preferably 1 minute or more and 10 minutes or less. When the time for molding in a mold is equal to or more than the above lower limit, the foamable resin composition can be sufficiently cured. When the time for molding in a mold is equal to or less than the above upper limit, the productivity of the pipe fitting 1 can be easily improved. In addition, it is preferable to dry the non-foaming resin composition before molding. By drying before molding, it is possible to suppress the generation of unintended bubbles inside or on the surface of the joint due to moisture evaporated in the molding machine, and to suppress a decrease in the transparency of the receiving part and a decrease in the strength of the main body. As a drying method, a method in which hot air at 60 to 90°C is blown onto the pellets for 2 to 6 hours using a hot air dryer such as a hopper dryer or a box-type drying oven to dry the non-foaming resin composition in advance can be mentioned.

[0061] Although the pipe joint of the present invention has been described in detail above, the present invention is not limited to the above-described embodiment, and can be modified appropriately without departing from the spirit and scope of the present invention. For example, the pipe joint may have a two-layer structure in which the inner surface serving as a flow path is formed of a non-foamed resin layer and the outer surface is formed of a foamed resin layer. Also, the pipe joint may have a two-layer structure in which the inner surface serving as a flow path is formed of a foamed resin layer and the outer surface is formed of a non-foamed resin layer. Also, for example, the pipe joint may have only a foamed resin layer without having a non-foamed resin layer. In that case, the foamed resin layer may have a rubber component content of 10% by mass or more and 45% by mass or less with respect to the total mass of the first resin. When the pipe joint is formed only with a foamed resin layer, it is preferable that the outer surface of the foamed resin layer forms a high-density layer similar to the non-foamed resin layer. The boundary between the main body and the socket may be curved rather than flat. In this case, the length L from the base end to the open end of the socket can be expressed as the insertion length of the tubular member when inserted into the socket (the length from the open end of the socket to the step that serves as the stopper).

[0062] The pipe joint of the present invention may be a multi-layer molded product having a body portion including a foamed resin layer, and may further include a different resin layer. Examples of the other resin layer include a non-foamed resin layer, a foamed resin layer that is the same as the outer surface, and a foamed resin layer that is different from the outer surface. The resin that is the raw material for these resin layers may be the same thermoplastic resin as the foamed resin layer that forms the outer surface, or may be a different thermoplastic resin. From the viewpoint of suppressing peeling between the resin layers, it is preferable that the resin that is the raw material for these resin layers is the same thermoplastic resin as the foamed resin layer that forms the outer surface.

[0063] The pipe joint of the present invention is not limited to the above-described embodiment, and may be a pipe joint having another shape, such as an elbow, a nipple, or a valve socket.

[0064] As described above, the pipe joint of the present invention has excellent heat insulating properties because it has a foamed resin layer. In addition, the pipe joint of the present invention has a rubber component content of 10% by mass or more and 45% by mass or less with respect to the total mass of the resin, so that the pipe joint of the present invention has excellent strength. Furthermore, in the pipe joint of the present invention, the ratio L / d of the length L from the base end to the open end of the socket portion to the thickness d of the socket portion at the open end is 2.0 to 10.0, preferably 2.0 to 9.0, so that the pipe joint of the present invention has excellent formability, watertightness and strength.

[0065] [Piping structure] The piping structure of the present invention comprises the pipe fitting of the present invention, and a pipe member that is inserted and connected to the socket portion of the pipe fitting. A piping structure according to an embodiment of the present invention will be described with reference to the drawings. As shown in FIG. 2, the piping structure 100 includes a pipe joint 1 and three pipe members 201, 202, and 203. The pipe member is not particularly limited, and may be any pipe member that can be connected to the pipe joint of the present invention. The pipe member may be a steel pipe or a synthetic resin pipe. From the viewpoint of excellent heat insulation, the pipe member is preferably a synthetic resin pipe, and more preferably a synthetic resin pipe having a foamed layer. The foamed layer may be an open cell type in which the bubbles are connected to each other, or a closed cell type in which the bubbles are not connected to each other.

[0066] In this embodiment, the pipe member 201 is inserted and connected to the socket portion 20a of the pipe fitting 1 along the direction of the first pipe axis O1. The pipe member 202 is inserted and connected to the socket portion 20b of the pipe fitting 1 along the direction of the first pipe axis O1. The pipe member 203 is inserted and connected to the socket portion 20c of the pipe fitting 1 along the direction of the second pipe axis O2. Outer diameter R of the pipe member 201 201 is the inner diameter R of the receiving portion 20a 20a The inner diameter R of the receiving portion 20a is slightly smaller than the 20a refers to the inner diameter of the socket end of the socket portion 20a, and the ratio R 201 / R 20a is preferably 0.986 to 0.997. Outer diameter R of the pipe member 202 202 is the inner diameter R of the receiving portion 20b 20b The inner diameter R of the receiving portion 20b is slightly smaller than the 20b refers to the inner diameter of the socket end of the socket portion 20b, and the ratio R 202 / R 20b is preferably 0.986 to 0.997. Outer diameter R of the pipe member 203 203 is the inner diameter R of the receiving portion 20c 20c The inner diameter R of the receiving portion 20c is slightly smaller than the 20c refers to the inner diameter of the socket end of the socket portion 20c, and the ratio R 203 / R 20c is preferably 0.986 to 0.997.

[0067] The piping structure 100 functions as a connection portion of a pipe for discharging a drainage water. In addition, the piping structure 100 functions as a branch portion of a pipe for discharging a drainage water.

[0068] <Manufacturing method of piping structure> The manufacturing method of the piping structure is not particularly limited, and the piping structure of the present invention can be obtained by inserting a pipe member into the socket of the pipe joint of the present invention and connecting them. The method of connecting the pipe joint and the pipe member is not particularly limited, and they may be connected using an adhesive or without using an adhesive.

[0069] In the piping structure 100 of the present embodiment, the pipe joint 1 and the pipe members 201, 202, and 203 are connected with an adhesive. By connecting the pipe joint and the pipe members with an adhesive, the watertightness and strength of the piping structure can be further improved. The adhesive used to connect the pipe joint and the pipe member is not particularly limited, and examples of the adhesive include known adhesives such as instant adhesives and hot melt adhesives.

[0070] The piping structure of the present invention has excellent heat insulation properties because it includes the pipe joint of the present invention. In addition, the piping structure of the present invention is excellent in strength since it includes the pipe joint of the present invention. Furthermore, the piping structure of the present invention is provided with the pipe joint of the present invention, and therefore has excellent watertightness. EXAMPLES

[0071] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples. The raw materials and evaluation methods used in each of the examples and comparative examples are as follows.

[0072] [Raw materials used] <Resin> ABS resin (ABS resin having the composition shown in Table 2). MBS resin (MBS resin having the composition shown in Table 2). Acrylic resin (polymethyl methacrylate). <Rubber component> Acrylic rubber (copolymer of acrylonitrile and butyl acrylate). <Foaming agent> ADCA (manufactured by Otsuka Chemical Co., Ltd., product name "AZ-HM", azodicarbonamide).

[0073] [Example 1] A resin composition obtained by kneading polymethyl methacrylate into ABS resin was used as a non-foaming resin composition. At this time, the non-foaming resin composition was kneaded at such a ratio that the peak area ratio of each component obtained by measuring the non-foaming resin composition with PGC / MS is shown in Table 2. This non-foaming resin composition was made into pellets and dried at 70°C for 4 hours using a known hot air dryer. The dried pellet-shaped non-foaming resin composition was mixed with azodicarbonamide as a foaming agent to obtain a foaming resin composition, which was injection molded at a molding temperature of 240°C to produce a DV joint type tee (pipe joint) with a receiving part of 48.3 mm inner diameter as shown in FIG. 1, which has a solid receiving part made of a non-foaming resin layer, a thickness between the inner and outer wall surfaces of the receiving part at the end of the receiving part of 3.7 mm, a length of the receiving part of 22 mm, a thickness between the inner and outer wall surfaces of the main body of 10 mm, and a foamed resin layer with a foaming ratio of 1.8 times. In Table 2, "methyl methacrylate" represents polymethyl methacrylate.

[0074] [Examples 2 to 4] Cheese was produced in the same manner as in Example 1, except that the resin composition, the thickness between the inner and outer wall surfaces at the end of the receiving mouth, and the length of the receiving mouth were set to the values ​​shown in Table 2. In Table 2, "-" indicates that polymethyl methacrylate was not mixed into the ABS resin.

[0075] [Example 5] Cheese was produced in the same manner as in Example 2, except that the thickness between the inner and outer wall surfaces of the main body was 15 mm and the expansion ratio was 1.5 times.

[0076] [Example 6] A cheese was produced in the same manner as in Example 2, except that the expansion ratio of the main body was set to 2.2 times.

[0077] [Example 7] Cheese was produced in the same manner as in Example 2, except that the resin composition, the thickness between the inner and outer wall surfaces at the end of the receiving mouth, and the length of the receiving mouth were set to the values ​​shown in Table 2.

[0078] [Example 8] Cheese was produced in the same manner as in Example 2, except that the pellet-shaped non-foamable resin composition was used without drying and injection molding was performed at a molding temperature of 195°C.

[0079] [Examples 9 to 10] Cheese was produced in the same manner as in Example 2, except that acrylic rubber was added as the rubber component and the resin composition was set to the values ​​shown in Table 2.

[0080] [Example 11] Cheese was produced in the same manner as in Example 2, except that the thickness between the inner and outer wall surfaces at the end of the receiving mouth and the length of the receiving mouth were set to the values ​​shown in Table 2.

[0081] [Comparative Examples 1 to 2] Cheese was produced in the same manner as in Example 2, except that the resin composition was set to the values ​​shown in Table 2.

[0082] [Comparative Example 3] Cheese was produced in the same manner as in Example 2, except that the thickness between the inner and outer wall surfaces at the end of the receiving mouth and the length of the receiving mouth were set to the values ​​shown in Table 2.

[0083] [Comparative Example 4] Cheese was produced in the same manner as in Example 2, except that the resin composition was set to the values ​​shown in Table 2, and the thickness between the inner and outer wall surfaces of the end of the receiving mouth and the length of the receiving mouth were set to the values ​​shown in Table 2.

[0084] [MFR measurement] The MFR of the cheese produced in each example was measured in accordance with JIS K 7210:1999 at a test temperature of 220°C and a test load of 10 kg. The results are shown in Table 2.

[0085] [Measurement of thermal resistance] The main body was cut out from the cheese obtained in the above Examples and Comparative Examples, and the thermal resistance was calculated from the thermal conductivity (W / m K) measured in accordance with JIS A 1412-1:2016 and the thickness (m) of the main body at the point where the thermal conductivity was measured, using the following formula (1). The results are shown in Table 2. Thermal resistance (K / W) = thickness (m) / thermal conductivity (W / m K) (1)

[0086] [Measurement of foaming ratio] The main body was cut out from the cheese obtained in the above Examples and Comparative Examples, and the expansion ratio was measured in accordance with the method of 6.2(b) described in JIS K 9798: 2006. The results are shown in Table 2.

[0087] [Impact resistance evaluation] The cheeses obtained in the above examples and comparative examples were used as test specimens, and a drop test was conducted on each test specimen, applying an acceleration equivalent to a fall from a height of 4 m to the test specimen, and impacting the test specimen against a horizontal surface such that the first tube axis O1 and the horizontal surface formed an angle of 45°. The test specimens of each example were each subjected to three tests to evaluate their impact resistance. The impact resistance was evaluated according to the following evaluation criteria by visually checking the test specimens for cracks and chips. The results are shown in Table 2. Evaluation Criteria ◯: No cracks or chips occurred in the socket and body of the test specimen. △: Cracks or chips occurred in either the socket or body of the test specimen. ×: Significant cracks or chips were observed in both the socket and main body of the test specimen.

[0088] [Evaluation of chemical resistance] For each of the cheeses obtained in the above Examples and Comparative Examples, the receiving portion was cut into a dumbbell shape in the tube axial direction to obtain a test piece. The obtained test piece was fixed to a bending jig prepared so that an expansion and contraction stress of 3 MPa was applied in a room at 23°C, and a cotton of 10 mm x 20 mm size soaked in 2 mL of polyethylene glycol (Nacalai Tesque #200, average molecular weight 190 to 210) was placed on the center of the test piece. Three test pieces were prepared for each example, and one of the three test pieces was left for 36 hours, after which the cotton was removed and visually confirmed. The other two of the three test pieces were left for 72 hours, after which the cotton was removed and visually confirmed to evaluate the chemical resistance. The chemical resistance was evaluated by the presence or absence of cracks in the test piece according to the following evaluation criteria. The results are shown in Table 2. (Evaluation Criteria) ◯: No breakage or cracks occurred even after 72 hours. △: Fracture or cracks occurred after being left for 1 hour or more but less than 72 hours. ×: Breakage or cracking occurred within 1 hour of placement.

[0089] [Evaluation of moldability] Based on the above examples and comparative examples, ten cheese pieces for each example were produced, and the cheese mouth was visually inspected for molding defects (mainly short circuits caused by the resin not being filled up to the edge of the mold). Moldability was evaluated according to the following evaluation criteria. The results are shown in Table 2. Evaluation Criteria ○: No molding defects in any of the 10 pieces. ×: One or more molding defects.

[0090] [Watertightness evaluation] The tees obtained in the above Examples and Comparative Examples were used as test specimens, and two of the receiving ports of each test specimen were blocked with a blocking jig. A pipe with an adhesive applied to one end was inserted and joined to the remaining receiving port, and the adhesive was dried at room temperature (20 to 30°C) for 24 hours to form a piping structure. Thereafter, a water pressure of 0.35 MPa was applied to the other end of the pipe and maintained for 1 minute, and the presence or absence of water leakage from the joint between the receiving part and the pipe was visually confirmed. The watertightness was evaluated according to the following evaluation criteria. The results are shown in Table 2. Evaluation Criteria ○: No leakage from joints. ×: Water leakage from joints.

[0091] [Haze's evaluation] The mouth of each of the cheeses obtained in the above Examples and Comparative Examples was cut to obtain test pieces, and the haze was measured using a haze meter (NDH7000SP, manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K 7136. The results are shown in Table 2.

[0092] [Table 2]

[0093] As shown in Table 2, Examples 1 to 11 to which the present invention was applied were evaluated as "○" in impact resistance, and were found to have excellent strength. In addition, they were found to have good moldability and water-stopping properties. On the other hand, Comparative Example 1, in which the rubber component (butadiene) content relative to the total resin mass was less than 10 mass%, was rated as "x" for impact resistance. Comparative Example 2, in which the rubber component content relative to the total resin mass was more than 45 mass%, was rated as "x" for moldability. Comparative Example 3, in which the L / d ratio was less than 2.0, was evaluated as “x” in terms of water stoppage ability. Comparative Example 4, in which the L / d ratio was more than 10.0, was evaluated as “x” in terms of impact resistance and moldability.

[0094] It has been found that the pipe joint of the present invention exhibits sufficient heat insulation properties and is excellent in moldability, water stoppage properties and strength, without having to thicken the foam layer or increase the foaming ratio of the foam layer. [Explanation of symbols]

[0095] 1 Pipe fittings 10 Main body 10a, 10b, 10c opening 12a, 12b, 12c steps 13 Peripheral wall 14 Injection gate section 20a, 20b, 20c socket 21a, 21b, 21c proximal end 22a, 22b, 22c open end 30 Foamed resin layer 50 Non-foamed resin layer

Claims

1. A pipe fitting comprising a tubular main body portion formed of a resin containing one or more selected from an acrylonitrile-butadiene-styrene copolymer and a methyl methacrylate-butadiene-styrene copolymer, the main body portion having a flow path therein, and one or more receiving portions formed integrally with the main body portion, the main body portion having a foamed resin layer and a non-foamed resin layer covering the foamed resin layer, a content of the rubber component in the foamed resin layer determined by pyrolysis gas chromatography mass spectrometry is 15% by mass or more and 45% by mass or less with respect to a total mass of resins contained in the foamed resin layer, the content of the rubber component in the non-foamed resin layer determined by pyrolysis gas chromatography mass spectrometry is 15% by mass or more and 45% by mass or less with respect to the total mass of resins contained in the non-foamed resin layer; A ratio L / d of a length L from a base end to an open end of the socket portion to a thickness d of the socket portion at the open end is 4.2 or more and 8.0 or less; A pipe joint, wherein the resin contained in the foamed resin layer is the same as the resin contained in the non-foamed resin layer.

2. 2. The pipe fitting according to claim 1, comprising two or more receiving portions, each of the receiving portions being cylindrical, a circular circumferential wall being formed around an entire inner circumferential surface of each of the receiving portions at a boundary between the receiving portion and the main body portion, the interior of the circumferential wall being constructed from the foamed resin layer, and the foamed resin layer being formed around the entire periphery of the circumferential wall.

3. 3. The pipe joint according to claim 1, wherein the wall thickness of the main body is 10 mm or more and 20 mm or less.

4. The pipe joint according to any one of claims 1 to 3, wherein the melt mass flow rate (MFR) of the foamable resin composition constituting the foamed resin layer is 3 g / 10 min or more and 90 g / 10 min or less.

5. 5. The pipe joint according to claim 4, wherein the non-foamable resin composition constituting the non-foamable resin layer has a melt mass flow rate (MFR) of 3 g / 10 min or more and 90 g / 10 min or less.

6. A piping structure comprising: the pipe joint according to any one of claims 1 to 5; and a pipe member inserted and connected to the receiving portion of the pipe joint, the pipe member having a foam layer.

7. A method for manufacturing a pipe joint according to claim 5, Using a hot air dryer, blow hot air at 60 to 90°C for 2 to 6 hours to pre-dry the non-foamable resin composition. A foaming agent is mixed with the non-foamable resin composition to obtain a foamable resin composition having an MFR of 4 g / 10 min or more and 60 g / 10 min or less, as measured in accordance with JIS K 7210:1999 at a test temperature of 220° C. and a test load of 10 kg. The foamable resin composition is heated to a temperature of 200° C. or higher and 280° C. or lower to be melted, injected into a mold, and then cooled.

Citation Information

Patent Citations

  • Pipe joint having heat insulation layer, and its manufacture

    JP1999201382A

  • Pipe joint with heat insulating layer

    JP2012107669A

  • Transparent ABS resin composition

    JP2016088955A

  • Foam pipe joint

    JP2017155868A

  • Pipe-connection moulded part having thermal insulation and method of producing the pipe-connection moulded part

    US20080084059A1