Curable composition, dry film, cured product and electronic component
The curable composition with a silicone compound, hydrophilic silica, and organic thixotropic agent addresses flux repellency and silica agglomeration, ensuring improved wettability and solderability in solder resist compositions.
Patent Information
- Application Number
- JP2023187643
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-11-01
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2039-03-27
AI Technical Summary
Existing alkali-developable photocurable/thermocurable solder resist compositions face issues with flux repellency and silica agglomeration, leading to poor solderability and wettability, particularly when using silicon-based surface conditioners and untreated hydrophilic silica.
A curable composition comprising a silicone compound, hydrophilic silica, and an organic thixotropic agent, with specific particle size and concentration ratios, to maintain wettability and prevent silica aggregation, enhancing solderability.
The composition ensures good wettability and solderability by preventing silica precipitation and improving flux adhesion to the cured product, addressing the issues of flux repellency and silica agglomeration.
Smart Images

Figure 0007596487000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable composition, a dry film, a cured product, and an electronic component, and in particular to an alkali-developable curable composition, a dry film thereof, a cured product thereof, and an electronic component comprising the cured product. [Background technology]
[0002] Conventionally, in the solder resists of consumer printed circuit boards and industrial printed wiring boards, from the viewpoint of high precision and high density, liquid developable solder resists have been used in which an image is formed by irradiating with ultraviolet light and developing, and then the finish curing (main curing) is carried out by irradiating with heat and / or light. Among liquid developable solder resists, alkaline developable photo solder resists that use an alkaline aqueous solution as a developer have become mainstream due to considerations of environmental issues.
[0003] In general, a silicon-based surface conditioner is added to a solder resist composition that is applied to a substrate to form a photosolder resist on the substrate in order to improve the wettability of the solder resist composition to the substrate and to improve the leveling ability (flatness) of the coating film.
[0004] After the photo solder resist is formed on the board, components are mounted on the board by soldering. However, because molten solder has low wettability to the board, flux is applied to the entire board surface, including the solder resist surface, to improve wettability (to clean the soldering surface and prevent oxidation).
[0005] However, the inventors have found through their research that if a silicon-based surface conditioner is contained in the solder resist formed on a substrate, the flux is repelled from the substrate, resulting in a problem of reduced solderability.
[0006] On the other hand, it is well known that silica is added as an inorganic filler to a solder resist composition in order to increase the rigidity of the solder resist and to suppress the cure shrinkage of the solder resist composition.
[0007] In the examples of Patent Document 1, an alkali-developable, photocurable, thermosetting solder resist composition containing a silicon-based surface conditioner is disclosed as the above-mentioned conventional solder resist composition, and as Comparative Example 2, an alkali-developable, photocurable, thermosetting solder resist composition containing fused spherical silica that has not been subjected to a surface modification treatment as an inorganic powder is disclosed. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2009-194222 A Summary of the Invention [Problem to be solved by the invention]
[0009] According to the example of Patent Document 1, an alkali-developable photocurable / thermosetting solder resist composition containing a silicon-based surface conditioner improves the wettability of the solder resist composition to a substrate, but the formed solder resist repels flux, resulting in a decrease in solderability.
[0010] In addition, in the alkali-developable photocurable / thermosetting solder resist composition of Comparative Example 2 of Patent Document 1, the added silica has not been subjected to a surface modification treatment and is hydrophilic, so there is a risk of problems with aggregation and precipitation if left as is, and it is necessary to solve the problems of aggregation and precipitation, for example by modifying the surface to make it hydrophobic. Moreover, since no silicon-based surface conditioner is added to the alkali-developable photocurable / thermosetting solder resist composition of Comparative Example 2, the wettability of the solder resist composition to the substrate is not improved.
[0011] The present invention has been made in view of the above problems, and an object of the present invention is to provide a curable composition, a dry film, a cured product, and an electronic device which contain hydrophilic silica and a silicon-based surface conditioner, and which have good solderability and which are free from the problem of silica aggregation and precipitation. [Means for solving the problem]
[0012] The present inventors have conducted extensive research to achieve the above object, and have unexpectedly found that when a silicone compound, hydrophilic silica, and an organic thixotropic agent are combined, the wettability of the copper-clad substrate and the solder resist composition is maintained, while the problems of aggregation and precipitation of hydrophilic silica and the problem of flux repelling caused by the silicone compound are resolved, leading to the completion of the present invention.
[0013] That is, the above object of the present invention is to (A) an alkali-soluble resin; (B) a photopolymerization initiator; (C) an epoxy resin; (D) a silicone compound; (E) hydrophilic silica; (F) an organic thixotropic agent; It has been found that this can be achieved by a curable composition comprising:
[0014] In the curable composition of the present invention, the hydrophilic silica (E) preferably has a median particle size D50 of 0.2 μm or more and 2.0 μm or less.
[0015] Further, the amount of the (F) organic thixotropic agent is more preferably 0.01 to 15 parts by mass per 100 parts by mass of the (E) hydrophilic silica, and more preferably 0.05 part by mass or more per 2 parts by mass of the (D) silicone compound.
[0016] Moreover, it is preferable to further contain (G) an antioxidant.
[0017] The above object of the present invention is also to provide a dry film obtained by applying the curable composition of the present invention onto a carrier film and drying the same. A cured product obtained by curing a dried coating film obtained by applying the curable composition of the present invention onto a substrate and drying it, or a coating film obtained by applying the curable composition onto a carrier film and drying it to obtain a dry film, which is then laminated onto a substrate; and An electronic component comprising the cured product. This can also be achieved by: Effect of the Invention
[0018] According to the present invention, the problem of aggregation and precipitation of hydrophilic silica in the curable composition is resolved, and when the curable composition is applied to a substrate, the silicone compound (D) maintains the wettability of the substrate. At the same time, the wettability of the flux to the obtained cured product is improved. Therefore, when the cured product is used as a solder resist, the effect of improving solderability can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] <Curable composition> The curable composition of the present invention comprises (A) an alkali-soluble resin; (B) a photopolymerization initiator; (C) an epoxy resin; (D) a silicone compound; (E) hydrophilic silica; (F) an organic thixotropic agent; Includes.
[0020] [(A) Alkali-soluble resin] The alkali-soluble resin is a resin that enables the hardenable composition to be dissolved in an alkaline developer, that is, to be developed with an alkali.
[0021] As the alkali-soluble resin, it is preferable to use a carboxyl group-containing resin or a phenol resin, and in particular, it is more preferable to use a carboxyl group-containing resin from the viewpoint of developability.
[0022] As the carboxyl group-containing resin, various conventionally known carboxyl group-containing resins that have a carboxyl group in the molecule and further have no ethylenically unsaturated group (non-photosensitive) or have such an ethylenically unsaturated group (photosensitive) can be used.
[0023] In the present invention, the ethylenically unsaturated group is a substituent having an ethylenically unsaturated bond, and examples thereof include a vinyl group and a (meth)acryloyl group. From the viewpoint of reactivity, the (meth)acryloyl group is preferable. Here, the (meth)acryloyl group is a general term for an acryloyl group and a methacryloyl group.
[0024] Specific examples of the carboxyl group-containing resin having no ethylenically unsaturated group include the following compounds (which may be either oligomers or polymers).
[0025] (1) Carboxyl group-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with diol compounds containing carboxyl groups such as dimethylolpropionic acid, dimethylolbutanoic acid, and the like, such as dialcohol compounds, polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0026] (2) Carboxylic acid-containing urethane resin obtained by the polyaddition reaction of diisocyanate and a carboxyl-containing dialcohol compound.
[0027] (3) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc.
[0028] (4) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid, such as adipic acid, phthalic acid, or hexahydrophthalic acid, with a difunctional epoxy resin or a difunctional oxetane resin, and then adding a dibasic acid anhydride, such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride, to the resulting hydroxyl groups.
[0029] (5) A carboxyl group-containing resin obtained by ring-opening an epoxy resin or an oxetane resin and reacting the generated hydroxyl group with a polybasic acid anhydride.
[0030] (6) A carboxyl group-containing resin obtained by reacting a reaction product such as a polyalcohol resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule, i.e., a polyphenol compound, with an alkylene oxide such as ethylene oxide or propylene oxide, with a polybasic acid anhydride.
[0031] Specific examples of the carboxyl group-containing resin having an ethylenically unsaturated group include the following compounds (which may be either oligomers or polymers): The ethylenically unsaturated bond in the carboxyl group-containing resin is preferably derived from acrylic acid, methacrylic acid, or a derivative thereof.
[0032] (7) Carboxyl group-containing photosensitive urethane resins obtained by polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with diol compounds containing carboxyl groups such as dimethylolpropionic acid, dimethylolbutanoic acid, and the like, such as dialcohol compounds, polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0033] (8) Carboxylic group-containing photosensitive urethane resin obtained by a polyaddition reaction of a diisocyanate, a (meth)acrylate of a bifunctional epoxy resin such as bisphenol A type epoxy resin, hydrogenated bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bixylenol type epoxy resin, or biphenol type epoxy resin, or a partially acid anhydride-modified product thereof, and a carboxyl group-containing dialcohol compound.
[0034] (9) A photosensitive urethane resin containing a carboxyl group, which is terminated with (meth)acrylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (7) or (8) described above.
[0035] (10) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acryloyl group obtained by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (8) or (9) described above.
[0036] (11) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl groups present in the side chains.
[0037] (12) A carboxyl group-containing photosensitive resin obtained by reacting a multifunctional epoxy resin with the hydroxyl groups of a bifunctional (solid) epoxy resin further epoxidized with epichlorohydrin, reacting the resin with (meth)acrylic acid, and adding a dibasic acid anhydride to the resulting hydroxyl groups.
[0038] (13) Carboxyl group-containing polyester photosensitive resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.
[0039] (14) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule, i.e., a polyphenol compound, with an alkylene oxide such as ethylene oxide or propylene oxide to obtain a reaction product such as a polyalcohol resin, with an unsaturated group-containing monocarboxylic acid such as (meth)acrylic acid, and further reacting the resulting reaction product with a polybasic acid anhydride.
[0040] (15) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0041] (16) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any of the resins (7) to (15) above.
[0042] The photosensitive carboxyl group-containing resin may be any other than those described as (7) to (16), and may be used alone or in combination of two or more. Among the carboxyl group-containing resins, resins having an aromatic ring are particularly preferred.
[0043] The above-mentioned carboxyl group-containing resins, whether photosensitive or non-photosensitive, have the following characteristics: Since they have many carboxyl groups on the side chains of the backbone polymer, they can be developed with a dilute alkaline aqueous solution.
[0044] The acid value of the carboxyl group-containing resin is preferably in the range of 40 to 200 mgKOH / g, more preferably 45 to 120 mgKOH / g. If the acid value of the carboxyl group-containing resin is within this range, alkaline development becomes easy, dissolution of the exposed area by the developer is suppressed, lines do not become thinner than necessary, and normal pattern drawing without dissolution and peeling by the developer becomes possible.
[0045] The weight-average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but is generally preferably in the range of 2,000 to 150,000, more preferably 5,000 to 100,000. If the weight-average molecular weight is within this range, the tack-free performance is excellent, the moisture resistance of the coating film after exposure is good, and the resolution, developability, and storage stability are excellent. The amount of the carboxyl group-containing resin in the curable composition (solid content) is suitably in the range of 20% by mass to 80% by mass, preferably 30% by mass to 70% by mass. If the amount of the carboxyl group-containing resin in the curable composition is within this range, the coating strength will not decrease, and thickening or deterioration in workability will not occur.
[0046] In the present invention, as the alkali-soluble resin (A), either a photosensitive carboxyl group-containing resin or a carboxyl group-containing resin having no photosensitivity can be used, or a mixture of these can be used.
[0047] The phenolic resin may be a compound having a phenolic hydroxyl group, for example, a compound having a biphenyl skeleton or a phenylene skeleton, or both skeletons, or a phenolic hydroxyl group-containing compound, for example, a phenolic resin having various skeletons synthesized using phenol, orthocresol, paracresol, metacresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, 3,5-xylenol, catechol, resorcinol, hydroquinone, methylhydroquinone, 2,6-dimethylhydroquinone, trimethylhydroquinone, pyrogallol, phloroglucinol, or the like.
[0048] For example, known and commonly used phenolic resins such as phenol novolac resin, alkylphenol volac resin, bisphenol A novolac resin, dicyclopentadiene type phenolic resin, Xylok type phenolic resin, terpene modified phenolic resin, polyvinylphenols, bisphenol F, bisphenol S type phenolic resin, poly-p-hydroxystyrene, condensates of naphthol and aldehydes, and condensates of dihydroxynaphthalene and aldehydes can be used.
[0049] These may be used alone or in combination of two or more.
[0050] Examples of commercially available phenolic resins include HF-1M (manufactured by Meiwa Kasei Co., Ltd.), Phenolite TD-2090, Phenolite TD-2131 (manufactured by DIC Corporation), Besumor CZ-256-A (manufactured by DIC Corporation), Shounol BRG-555, Shounol BRG-556 (manufactured by Aica Kogyo Co., Ltd.), CGR-951 (manufactured by Maruzen Oil Co., Ltd.), and polyvinylphenols CST70, CST90, S-1P, and S-2P (manufactured by Maruzen Oil Co., Ltd.). These phenolic resins can be used alone or in appropriate combination of two or more kinds.
[0051] [(B) Photopolymerization initiator] (B) The photopolymerization initiator is added to initiate radical polymerization of ethylenically unsaturated groups upon irradiation with energy rays.
[0052] (B) Photopolymerization initiators include, for example, benzoin and benzoin alkyl ethers such as benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether; acetophenones such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, and 1,1-dichloroacetophenone; 2-methyl-1-[4-(methylthio)phenyl] -Aminoalkylphenones such as 2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone; anthraquinones such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tertiary butylanthraquinone, 1-chloroanthraquinone; 2,4-dimethylthioxanthrate thioxanthones such as thioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; ketals such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzophenones such as 4,4'-bis(diethylamino)benzophenone; (2,6-dimethoxybenzoyl)-2,4,4-pentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and 2,4,6-trimethylbenzoyl-phenylphosphine oxide. Examples of the initiator include phosphine oxides such as ethyl benzoyldiphenylphosphine oxide and ethyl 2,4,6-trimethylbenzoylphenylphosphinate; oxime esters such as 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); various peroxides, titanocene initiators, etc. These may be used in combination with photosensitizers such as tertiary amines such as N,N-dimethylaminobenzoic acid ethyl ester, N,N-dimethylaminobenzoic acid isoamyl ester, pentyl-4-dimethylaminobenzoate, triethylamine, triethanolamine, etc.These photopolymerization initiators can be used alone or in combination of two or more kinds.
[0053] The amount of the photopolymerization initiator (B) blended in the curable composition of the present invention is in the range of 0.01 parts by mass or more and 30 parts by mass or less, and preferably in the range of 0.5 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass (solid content) of the alkali-soluble resin (A).
[0054] [(C) Epoxy resin] The (C) epoxy resin is a compound added for thermally curing the curable composition of the present invention.
[0055] The epoxy resin (C) may be a known, commonly used multifunctional epoxy resin having at least two epoxy groups in one molecule. Examples of the epoxy resin (C) include bisphenol A type epoxy resins such as jER828, jER834, jER1001, and jER1004 manufactured by Mitsubishi Chemical Corporation, EPICLON840, EPICLON850, EPICLON850-S, EPICLON1050, and EPICLON2055 manufactured by DIC Corporation, Epotohto YD-011, YD-013, YD-127, and YD-128 manufactured by Tohto Kasei Co., Ltd., DER317, DER331, DER661, and DER664 manufactured by Dow Chemical Co., Ltd., and Sumi-Epoxy ESA-011, ESA-014, ELA-115, and ELA-128 manufactured by Sumitomo Chemical Co., Ltd. (all trade names); and jER manufactured by Mitsubishi Chemical Corporation. Brominated epoxy resins such as YL903, EPICLON152, EPICLON165 manufactured by DIC, Epototo YDB-400, YDB-500 manufactured by Tohto Kasei, DER542 manufactured by Dow Chemical, Sumi-Epoxy ESB-400, ESB-700 manufactured by Sumitomo Chemical Co., Ltd. (all trade names); jER152, jER154 manufactured by Mitsubishi Chemical, DEN431, DEN438 manufactured by Dow Chemical, EPICLON N-730, EPICLON N-770, EPICLON N-865, Epotohto YDCN-701, YDCN-704 manufactured by Tohto Kasei Co., Ltd., EPPN-201, EOCN-1025, EOCN-1020, EOCN-104S, RE-306, NC-3000 manufactured by Nippon Kayaku Co., Ltd., Sumi-Epoxy ESCN-195X, ESCN-220 manufactured by Sumitomo Chemical Co., Ltd., YDCN-700-2, YDCN-700-3, YDCN-700-5, YDCN-700-7, YDCN-700-10, YDCN-704 YDCN-704A manufactured by Nippon Steel Chemical Co., Ltd., EPICLON N-680, EPICLON N-690, EPICLON manufactured by DIC Corporation Novolac type epoxy resins such as N-695 (all trade names); bisphenol F type epoxy resins such as EPICLON830 manufactured by DIC Corporation, jER807 manufactured by Mitsubishi Chemical Corporation, and Epotohto YDF-170, YDF-175, and YDF-2004 manufactured by Tohto Kasei Co., Ltd. (all trade names);Hydrogenated bisphenol A type epoxy resins such as Epotohto ST-2004, ST-2007, and ST-3000 (trade names) manufactured by Tohto Kasei Co., Ltd. and YX8034 manufactured by Mitsubishi Chemical Corporation; glycidylamine type epoxy resins such as jER604 manufactured by Mitsubishi Chemical Corporation, Epotohto YH-434 manufactured by Tohto Kasei Co., Ltd. and Sumi-Epoxy ELM-120 manufactured by Sumitomo Chemical Co., Ltd. (all trade names); hydantoin type epoxy resins; alicyclic epoxy resins such as Celloxide 2021 manufactured by Daicel Chemical Industries, Ltd. (all trade names); YL-933 manufactured by Mitsubishi Chemical Corporation and EPPN- trihydroxyphenylmethane type epoxy resins such as EPPN-501, EPPN-502 (all trade names); bixylenol type or biphenol type epoxy resins or mixtures thereof such as YL-6056, YX-4000, YL-6121 (all trade names) manufactured by Mitsubishi Chemical Corporation; bisphenol S type epoxy resins such as EBPS-200 manufactured by Nippon Kayaku Co., Ltd., EPX-30 manufactured by ADEKA Corporation, EXA-1514 (trade name) manufactured by DIC Corporation; bisphenol A novolac type epoxy resins such as jER157S (trade name) manufactured by Mitsubishi Chemical Corporation; jER manufactured by Mitsubishi Chemical Corporation Tetraphenylolethane type epoxy resins such as YL-931 (all trade names); diglycidyl phthalate resins such as Blenmer DGT manufactured by Nippon Oil & Fats Co., Ltd.; heterocyclic epoxy resins such as TEPIC manufactured by Nissan Chemical Industries, Ltd. (all trade names); tetraglycidyl xylenoylethane resins such as ZX-1063 manufactured by Tohto Kasei Co., Ltd.; naphthalene group-containing resins such as ESN-190, ESN-360 manufactured by Nippon Steel Chemical Co., Ltd., HP-4032, EXA-4750, EXA-4700 manufactured by DIC Corporation. Epoxy resins include, but are not limited to, epoxy resins having a dicyclopentadiene skeleton, such as HP-7200 and HP-7200H manufactured by DIC Corporation; glycidyl methacrylate copolymer epoxy resins, such as CP-50S and CP-50M manufactured by Nippon Oil & Fats Corporation; copolymer epoxy resins of cyclohexylmaleimide and glycidyl methacrylate; and CTBN-modified epoxy resins (e.g., YR-102 and YR-450 manufactured by Tohto Kasei Co., Ltd.);
[0056] When the (C) epoxy resin is blended, it is blended in an amount of 0.8 epoxy equivalents or more and 2.0 epoxy equivalents or less relative to the carboxylic acid equivalent of the (A) alkali-soluble resin. Here, the carboxylic acid equivalent represents the weight of the (A) alkali-soluble resin required to obtain 1 mol of carboxyl groups, and is expressed in g / mol. The epoxy equivalent represents the weight of the (C) epoxy resin required to obtain 1 mol of epoxy groups, and is expressed in g / mol. The mass of the (C) epoxy resin is 0.8 epoxy equivalents or more and 2.0 epoxy equivalents or less relative to the carboxylic acid equivalent of the (A) alkali-soluble resin. When the epoxy equivalent is within this range, a cured product with excellent heat resistance, electrical properties, and crack resistance can be obtained.
[0057] [(D) Silicone compounds] The silicone compound (D) is blended to improve the wettability of the curable composition of the present invention to a copper-clad substrate (base material), suppress repellency, and improve leveling properties.
[0058] The (D) silicone compound is polydimethylsiloxane or a derivative having a polydimethylsiloxane as a basic structure, and examples thereof include polydimethylsiloxane, polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, polyester-modified polymethylalkylsiloxane, polyether-modified polymethylalkylsiloxane, aralkyl-modified polymethylalkylsiloxane, polyether-modified siloxane, and polyester-modified hydroxyl group-containing polydimethylsiloxane.
[0059] (D) Commercially available silicone compounds include BYK (registered trademark)-300, BYK (registered trademark)-302, BYK (registered trademark)-306, BYK (registered trademark)-307, BYK (registered trademark)-310, BYK (registered trademark)-315N, BYK (registered trademark)-320, BYK (registered trademark)-322, BYK (registered trademark)-323, BYK (registered trademark)-325, BYK (registered trademark)-330, BYK (registered trademark) -331, BYK (registered trademark) -333, BYK (registered trademark) -342, BYK (registered trademark) -345, BYK (registered trademark) -346, BYK (registered trademark) -347, BYK (registered trademark) -348, BYK (registered trademark) -349, BYK (registered trademark) -370, BYK (registered trademark) -377, BYK (registered trademark) -378, BYK (registered trademark) -3455 (all manufactured by BYK-Chemie Japan KK).
[0060] The silicone compound (D) is blended in the curable composition of the present invention in an amount of 0.1 to 10 parts by mass, preferably 1 to 5 parts by mass, per 100 parts by mass (solid content) of the alkali-soluble resin (A). By blending the silicone compound (D) in an amount of 0.1 to 10 parts by mass, the wettability of the curable composition to the copper-clad substrate (base material) is ensured, the leveling property is improved, and the wettability of the flux to the cured product is also improved.
[0061] [(E) Hydrophilic silica] (E) Hydrophilic silica is added to suppress cure shrinkage of the curable composition of the present invention and to increase the rigidity of the obtained cured product.
[0062] In the present invention, the hydrophilic silica (E) refers to untreated silica that has not been subjected to a surface treatment for adding a hydrophobic organic group to its hydrophilic surface, and examples of the hydrophilic silica include fused silica, spherical silica, amorphous silica, and crystalline silica.
[0063] The surface treatment to add a hydrophobic organic group refers to treating the surface of (untreated) hydrophilic silica with a coupling agent having a hydrophobic organic group such as an ethylenically unsaturated group (photocurable reactive group) or an alkyl group, and silica that has been subjected to such surface treatment is not included in the above-mentioned (E) hydrophilic silica.
[0064] Commercially available products include FB-15D, FB-105, FB-105X, FB-5SDX, SFP-20M, SFP-130MC (all manufactured by Denki Kagaku Kogyo Co., Ltd.), Excelilica (registered trademark) (manufactured by Tokuyama Corporation), and SR-NP (manufactured by M-Tech Chemical Co., Ltd.).
[0065] (E) Hydrophilic silica has a median diameter (D50) of 30 μm or less when used to form a cured film on a printed wiring board, and 5 μm or less when used to form a cured film on an IC package substrate, and a median diameter (D50) of 0.2 μm or more and 2 μm or less is preferable from the viewpoint of dispersibility in the curable composition. The method for measuring the median diameter (D50) is as follows.
[0066] <Measuring method for median diameter (D50)> 30 ml of ethanol and 1 g of silica powder were placed in a 100 ml beaker and stirred for 3 minutes in a tabletop ultrasonic cleaner. The volume-based median diameter (D50) was then measured in ethanol solvent using a laser diffraction / scattering particle size distribution analyzer (Microtrack MT-3300, manufactured by Microtrack Bell).
[0067] In addition, the (E) hydrophilic silica is blended in the curable composition of the present invention in an amount of 10 to 200 parts by mass, preferably 20 to 180 parts by mass, per 100 parts by mass (solid content) of the (A) alkali-soluble resin. By blending the (E) hydrophilic silica in the amount of 10 to 200 parts by mass, the effect of suppressing cure shrinkage and enhancing the rigidity of the cured product can be obtained, while the dispersibility is also good.
[0068] [(F) Organic thixotropic agent] The (F) organic thixotropic agent is added to suppress aggregation and precipitation of the (E) hydrophilic silica in the curable composition of the present invention, and, as has become clear for the first time in the present invention, to improve the wettability of the flux to the cured product of the curable composition of the present invention.
[0069] The (F) organic thixotropic agent that can be used in the curable composition of the present invention includes fatty acid amides (amide wax type) synthesized from vegetable oil fatty acids and amines; surfactants such as fatty acid esters, polyethers, sulfated oils, and higher alcohol sulfates; polycarboxylic acid esters; polycarboxylic acid amides; and urea-modified compounds, but does not include hydrogenated castor oil type, known as castor oil wax, or oxidized polyethylene type, which is a wax obtained by oxidizing polyethylene and introducing polar groups.
[0070] (F) Commercially available organic thixotropic agents include BYK (registered trademark)-R606, BYK (registered trademark)-405, BYK (registered trademark)-R605, BYK (registered trademark)-R607, BYK (registered trademark)-410, BYK (registered trademark)-411, BYK (registered trademark)-415, BYK (registered trademark)-430, BYK (registered trademark)-431, BYK (registered trademark)-7410ET, BYK (registered trademark)-7411ES (hereinafter referred to as Examples of the above are manufactured by BYK Japan), Talen 1450, Talen 2000, Talen 2200A, Talen 7200-20, Talen 8200-20, Talen 8300-20, Talen 8700-20, Talen BA-600, Flonon SH-290, Flonon SH-295S, Flonon SH-350, Flonon HR-2, and Flonon HR-4AF (all manufactured by Kyoeisha Chemical Co., Ltd.).
[0071] The amount of the (F) organic thixotropic agent in the curable composition of the present invention is 0.01 to 15 parts by mass, preferably 0.05 to 10 parts by mass, per 100 parts by mass (solid content) of the (E) hydrophilic silica.
[0072] The amount of the (F) organic thixotropic agent in the curable composition of the present invention is 0.05 parts by mass or more, and preferably 0.1 parts by mass or more, per 2 parts by mass of the (D) silicone compound.
[0073] Within the above range, the hydrophilic silica (E) is well dispersed, and the wettability of the flux to the cured product of the curable composition is also good.
[0074] [(G) Antioxidants] The curable composition of the present invention preferably contains an antioxidant (G) which inhibits oxidation of copper in a copper-clad substrate (substrate) and thereby improves adhesion between the substrate and the curable composition.
[0075] Examples of the (G) antioxidant include hindered phenol compounds such as 3-(N-salicyloyl)amino-1,2,4-triazole, sulfur-based antioxidants such as zinc salts of 2-mercaptobenzimidazole, phosphorus-based antioxidants such as triphenyl phosphite, aromatic amine-based antioxidants such as di-tert-butyldiphenylamine, and heterocyclic dry compounds containing nitrogen as a heteroatom (excluding sulfur-based antioxidants) such as melamine, benzotriazole, and tolyltriazole. Of these, melamine is preferred.
[0076] The blending amount of the (G) antioxidant in the curable composition of the present invention is from 0.1 to 5 parts by mass, and preferably from 0.5 to 2 parts by mass, per 100 parts by mass (solid content) of the (A) alkali-soluble resin.
[0077] [Other ingredients] Furthermore, it is preferable to add a photopolymerizable polyfunctional monomer to the curable composition of the present invention. The photopolymerizable polyfunctional monomer is a compound having two or more ethylenically unsaturated groups in one molecule, and is used to assist the photocuring of the alkali-soluble resin (A) by irradiation with active energy rays (when the alkali-soluble resin (A) contains an ethylenically unsaturated group) and to photocure the curable composition.
[0078] Examples of compounds used as photopolymerizable polyfunctional monomers include commonly known polyester (meth)acrylates, polyether (meth)acrylates, urethane (meth)acrylates, carbonate (meth)acrylates, and epoxy (meth)acrylates. Specific examples of such compounds include polyhydric alcohols such as hexanediol, trimethylolpropane, pentaerythritol, dipentaerythritol, and tris-hydroxyethyl isocyanurate, and polyhydric acrylates such as ethylene oxide adducts, propylene oxide adducts, and ε-caprolactone adducts thereof; polyhydric acrylates such as phenoxy acrylate, bisphenol A diacrylate, and ethylene oxide adducts or propylene oxide adducts of these phenols; glycerin diglycidyl ether, glycerol diglycidyl ether, and glycerol diglycidyl ether; Polyhydric acrylates of glycidyl ethers such as phosphorus triglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and, without being limited to the above, examples include acrylates and melamine acrylates obtained by directly acrilating polyols such as polyether polyols, polycarbonate diols, hydroxyl-terminated polybutadienes, and polyester polyols, or by urethane acrilation via diisocyanates, and at least one of the methacrylates corresponding to the above acrylates.
[0079] The photopolymerizable polyfunctional monomer is blended in the curable composition of the present invention in an amount of 3 parts by mass or more and 30 parts by mass or less, and preferably in an amount of 10 parts by mass or more and 20 parts by mass or less, per 100 parts by mass (solid content) of the alkali-soluble resin (A).
[0080] The curable composition of the present invention preferably further contains a curing catalyst such as dicyandiamide, a boron trifluoride-amine catalyst, an organic acid hydrazide, etc. The curing catalyst is added in an amount of 5 parts by mass or less, preferably 0.1 parts by mass or more and 2 parts by mass or less, per 100 parts by mass (solid content) of the alkali-soluble resin (A) in the curable composition of the present invention.
[0081] Furthermore, for the purpose of coloring, a color pigment, a dye, etc. may be added to the curable composition of the present invention. As the color pigment, dye, etc., known and commonly used ones represented by a color index can be used.For example, Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 60, Solvent Blue 35, 63, 68, 70, 83, 87, 94, 97, 122, 136, 67, 70, PigmentGreen 7, 36, 3, 5, 20, 28, Solvent Yellow 163, Pigment Yellow 24, 108, 193, 147, 199, 202, 110, 109, 139 179 185 93, 94, 95, 128, 155, 166, 180, 120, 151, 154, 156, 175, 181, 1, 2, 3, 4, 5, 6, 9, 10, 12, 61, 62, 62:1, 65, 73, 74, 75, 97, 100 , 104, 105, 111, 116, 167, 168, 169, 182, 183, 12, 13, 14, 16, 17, 55, 63, 81, 83, 87, 126, 127, 152, 170, 172, 174, 176, 188, 198, Pigment Orange 1, 5, 13, 14, 16, 17, 24, 34, 36, 38, 40, 43, 46, 49, 51, 61, 63, 64, 71, 73, Pigment Red 1, 2, 3, 4, 5, 6, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 112, 114, 146, 147, 151, 170, 184, 187, 188, 193, 2 10, 245, 253, 258, 266, 267, 268, 269, 37, 38, 41, 48:1, 48:2, 48:3, 48:4, 49:1, 49:2, 50:1, 52:1, 52:2, 53 :1, 53:2, 57:1, 58:4, 63:1, 63:2, 64:1, 68, 171, 175, 176, 185, 208, 123, 149, 166, 178, 179, 190, 194, 224 , 254, 255, 264, 270, 272, 220, 144, 166, 214, 220, 221, 242, 168, 177, 216, 122, 202, 206, 207, 209, Solvent Red 135, 179, 149, 150, 52, 207, Pigment Violet 19, 23, 29, 32, 36, 38, 42, Solvent Violet 13, 36, Pigment Brown 23, 25, Pigment Black 1, 7, etc.These color pigments, dyes, etc. can be added in an amount ranging from 0.01 to 5 parts by mass, and preferably from 0.1 to 3 parts by mass, relative to 100 parts by mass of the curable composition.
[0082] Furthermore, if necessary, known and commonly used additives such as a polymerization inhibitor, a photopolymerization sensitizer, a light stabilizer, a dispersant, a flame retardant, and a flame retardant assistant, such as hydroquinone, hydroquinone monomethyl ether, t-butylcatechol, pyrogallol, and phenothiazine, may be blended.
[0083] The curable composition of the present invention may also contain an organic solvent used to adjust viscosity. As the organic solvent, for example, ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether (DPM), dipropylene glycol diethyl ether, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha can be used. These organic solvents can be used alone or in combination of two or more kinds.
[0084] <Dry film and cured product of the curable composition of the present invention> The curable composition of the present invention can be in the form of a dry film obtained by applying it to a carrier film (support) and drying it. When forming a dry film, the curable composition of the present invention is diluted with the above organic solvent to adjust the viscosity to an appropriate level, and applied to a carrier film in a uniform thickness using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like, and usually dried at a temperature of 50 to 130°C for 1 to 30 minutes to form a dry coating film. There is no particular restriction on the coating film thickness, but it is generally appropriately selected within the range of 0.1 to 100 μm, preferably 0.5 to 50 μm, in terms of the film thickness after drying.
[0085] As the carrier film, a plastic film is used, and it is preferable to use a plastic film such as a polyester film such as polyethylene terephthalate, a polyimide film, a polyamideimide film, a polypropylene film, a polystyrene film, etc. There is no particular limitation on the thickness of the carrier film, but it is generally appropriately selected in the range of 0.1 to 150 μm.
[0086] In this case, after forming the coating film on the carrier film, it is preferable to further laminate a peelable cover film on the surface of the coating film for the purpose of preventing dust from adhering to the surface of the coating film, etc. As the peelable cover film, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, surface-treated paper, etc. can be used, and it is sufficient that the adhesive strength between the coating film and the cover film is smaller than the adhesive strength between the coating film and the carrier film when the cover film is peeled off.
[0087] In addition, the curable composition of the present invention is adjusted to a viscosity suitable for the coating method using the organic solvent, and then coated on a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, curtain coating, or die coating, and the organic solvent contained in the composition is evaporated and dried (temporarily dried) at a temperature of about 50° C. to 90° C., thereby forming a tack-free dry coating film. In addition, in the case of a dry film obtained by coating the curable composition of the present invention on a carrier film, drying, and winding it up as a film, this is laminated on the substrate by a laminator or the like so that the coating film of the curable composition contacts the substrate, and then peeling off the carrier film, thereby forming a coating layer on the substrate.
[0088] These coating films can be photocured by, for example, irradiation with active energy rays or thermally cured by heating to a temperature of 100° C. to 250° C. to obtain a cured product.
[0089] Examples of the substrate include printed wiring boards and flexible printed wiring boards with pre-formed circuits, as well as copper-clad laminates such as paper + phenol resin, paper + epoxy resin, paper + glass cloth + epoxy resin, nonwoven glass cloth + epoxy resin, woven glass cloth + epoxy resin, and glass fiber + polyimide resin.
[0090] The volatilization drying carried out after application of the curable composition of the present invention can be carried out by a method of counter-contacting hot air in a dryer equipped with a heat source of an air heating method using steam, such as a hot air circulation drying oven, an IR oven, a hot plate, or a convection oven, or by a method of spraying the hot air from a nozzle onto a support.
[0091] The exposure machine used for the active energy ray irradiation may be any machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm. In addition, a direct imaging machine (for example, a direct imaging machine that directly irradiates active energy rays to draw an image based on CAD data from a computer) may also be used. The light source of the direct imaging machine may be any machine that uses light with a maximum wavelength in the range of 350 to 410 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 20 to 1000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 The range may be:
[0092] The developing method may be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution may be an alkaline aqueous solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.
[0093] As described above, the dry film and cured product obtained from the curable composition of the present invention are excellent in heat resistance, rigidity, adhesion to substrates, and insulation, and therefore can be applied to various uses, and there is no particular limitation on the application target. For example, it can be used to prepare an etching resist, solder resist, marking resist, etc. for a printed wiring board, and among them, it can be suitably used as a solder resist that requires high heat resistance, since the solderability is improved.
[0094] <Electronic components using the cured product of the curable composition as an insulating cured coating> When the cured product of the curable composition pattern-printed on the substrate is used as a solder resist, it is heated in a soldering process for mounting components. Soldering may be performed by any of manual soldering, flow soldering, reflow soldering, etc., but in the case of reflow soldering, for example, the solder is preheated at 100°C to 140°C for 1 to 4 hours, and then heated at 240°C to 280°C for about 5 to 20 seconds multiple times (for example, 2 to 4 times) to heat and melt the solder in a reflow process, and after cooling, components are mounted as necessary to complete the electronic component.
[0095] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following, "parts" refers to parts by mass unless otherwise specified. EXAMPLES
[0096] (Synthesis of alkali-soluble resin) [Synthesis Example 1] 380 parts of bisphenol F type epoxy resin (epoxy equivalent 950g / eq, softening point 85°C) and 925 parts of epichlorohydrin were dissolved in 462.5 parts of dimethyl sulfoxide, and then 60.9 parts of 98.5% NaOH were added over 100 minutes at 70°C under stirring. After the addition, the reaction was continued for another 3 hours at 70°C. After the reaction was completed, 250 parts of water were added and washed with water. After oil-water separation, most of the dimethyl sulfoxide and excess unreacted epichlorohydrin were distilled and recovered from the oil layer under reduced pressure, and the reaction product containing the remaining by-product salt and dimethyl sulfoxide was dissolved in 750 parts of methyl isobutyl ketone, and 10 parts of 30% NaOH were added and reacted at 70°C for 1 hour. After the reaction was completed, the reaction was washed twice with 200 parts of water. After oil-water separation, methyl isobutyl ketone was distilled and recovered from the oil layer to obtain an epoxy resin (a) with an epoxy equivalent of 310 g / eq and a softening point of 69°C. The epoxy resin (a) obtained was calculated from the epoxy equivalent, and about 5 of the 6.2 alcoholic hydroxyl groups in the starting material bisphenol F type epoxy resin were epoxidized. 310 parts of this epoxy resin (a) and 282 parts of carbitol acetate were charged in a flask, heated to 90°C, stirred, and dissolved. The resulting solution was once cooled to 60°C, and 72 parts (1 mole) of acrylic acid, 0.5 parts of methylhydroquinone, and 2 parts of triphenylphosphine were added, heated to 100°C, and reacted for about 60 hours to obtain a reaction product with an acid value of 0.2 mgKOH / g. 140 parts (0.92 moles) of tetrahydrophthalic anhydride were added to this, heated to 90°C, and reacted to obtain a photosensitive carboxyl group-containing resin varnish (A-1). The resulting carboxyl group-containing resin varnish (A-1) had a solid content of 62.5% and an acid value of the solid content (mgKOH / g) of 100.
[0097] [Synthesis Example 2] 220 parts of cresol novolac epoxy resin (manufactured by Dai Nippon Ink and Chemicals, Inc., registered trademark "Epiclon" N-695, epoxy equivalent: 220) was placed in a four-neck flask equipped with a stirrer and a reflux condenser, 214 parts of carbitol acetate was added, and the mixture was dissolved by heating. Next, 0.1 parts of hydroquinone as a polymerization inhibitor and 2.0 parts of dimethylbenzylamine as a reaction catalyst were added. This mixture was heated to 95-105°C, 72 parts of acrylic acid were gradually added dropwise, and the mixture was reacted for 16 hours. The reaction product was cooled to 80-90°C, 106 parts of tetrahydrophthalic anhydride was added, and the mixture was reacted for 8 hours, cooled, and then taken out. The photosensitive resin thus obtained, which had both ethylenically unsaturated bonds and carboxyl groups, had a non-volatile content of 65%, an acid value of the solid matter of 85 mgKOH / g, and a weight average molecular weight Mw of about 3,500. Hereinafter, this resin solution is referred to as varnish (A-2). The weight average molecular weight of the obtained resin was measured by high performance liquid chromatography using three pumps, LC-804, KF-803, and KF-802, all of which are manufactured by Shimadzu Corporation.
[0098] <1. Preparation of Curable Compositions of Examples 1 to 9 and Comparative Examples 1 to 3> The resin solution of the synthesis example and each material shown in Table 1 were mixed and premixed with a stirrer, and then kneaded with a three-roll mill to prepare a curable composition. In Table 1, (A-1) to (A-3) indicate the parts by mass of each resin solution including the solvent.
[0099] The above compositions were subjected to the following property tests, the results of which are shown in Table 1.
[0100] <2. Evaluation of repellency and leveling properties of curable compositions on substrates> Each of the curable compositions prepared in <1. Preparation of curable compositions of Examples 1 to 9 and Comparative Examples 1 to 3> was printed on a copper-clad substrate (substrate) whose surface had been roughened by chemical polishing treatment using a screen (Tetron 100 mesh) to a film thickness of 10 μm over the entire surface of the copper-clad substrate.
[0101] The coating film immediately after printing was visually observed to check for the presence or absence of repellency of the curable composition and the leveling state (smoothness). The printed substrate was then dried at 80°C for 30 minutes, and after returning to room temperature, the state of the coating film after drying was similarly visually checked. (Note that although visual check was performed in this example, if visual judgment is difficult, the surface roughness may be observed using a surface roughness measuring device (Surfcorder: manufactured by Kosaka Laboratory Co., Ltd.) or a shape measuring laser microscope (VK-X-100 / manufactured by KEYENCE Corporation).) The evaluation criteria are as follows:
[0102] ○: No repelling, no mesh marks △: Repelling and no mesh marks, or no repelling and mesh marks ×: Repelling and mesh marks
[0103] <3. Evaluation of flux repellency> Using a screen (Tetron 100 mesh), each of the curable compositions prepared in <1. Preparation of curable compositions of Examples 1 to 4 and Comparative Examples 1 to 4> was printed to a film thickness of 10 μm on the entire surface of an FR-4, 35 μm-thick copper-clad laminate with an outer dimension of 150 × 95 mm and a thickness of 1.6 mm, the surface of which had been roughened by chemical polishing treatment.
[0104] After drying at 80°C for 30 minutes, the film was exposed to light at 600 mJ / cm using a 95 x 150 mm exposure mask to form a pattern. 2 After exposure to light at 4000 mJ / cm, alkaline development (1% Na2O3aq, 30°C, 60 sec development) was performed, and thermal curing was performed at 150°C / 60 min., followed by exposure to light at 4000 mJ / cm 2 Post-UV treatment was performed.
[0105] An FR-4 substrate (base material) to which the cured product of the curable composition was fixed was subjected to an electroless Sn plating treatment (Sn: 1.1 μm / Tsukada Riken Kogyo Co., Ltd.), and a reflow process (265°C) was repeated from one to three times. After the electroless Sn plating treatment, a wet tension test was performed on the FR-4 substrate to which the cured product of the curable composition was fixed at each stage: before the reflow process, after the first reflow process, after the second reflow process, and after the third reflow process.
[0106] The wetting tension test was performed based on JIS K6768, and the mixtures used for the wetting tension test were "Wetting tension test mixture No. 60.0" before the reflow process after electroless Sn plating, "Wetting tension test mixture No. 38.0" after the first reflow process, "Wetting tension test mixture No. 36.0" after the second reflow process, and "Wetting tension test mixture No. 34.0" after the third reflow process. All the mixtures for the wetting tension test were manufactured by Fujifilm Wako Pure Chemical Industries. The No. of each mixture indicates the surface tension (unit: mN / m) of the mixture.
[0107] Specifically, the wet tension test involved tracing the substrate with a cotton swab coated with the wet tension test mixture and observing the state of the liquid film after 2 seconds. If the liquid film was not broken and maintained the same state as when it was applied for 2 seconds or more, it was judged to be wet.
[0108] In addition, the larger the NO. number of the mixture for the wetting tension test, the more difficult it is to wet, so the wetting tension test is a test to evaluate flux repellency (flux wettability).
[0109] In Table 1, the evaluation criteria are as follows:
[0110] ◯: It is judged that the surface is wet (no repellency) at all stages from before the reflow process after electroless Sn plating to after three reflow processes.
[0111] ×: There are cases where it is judged that there is no wetting (repellency) even once among the cases before the reflow process after the electroless Sn plating process and after three reflow processes.
[0112] [Table 1]
[0113] *1: Cyclomer P(ACA)Z250 (unsaturated group-containing carboxyl group-containing copolymer resin solution with 45 wt% solid content, manufactured by Daicel Chemical Industries, Ltd.) *2: 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO H: manufactured by IGM Resins BV) *3: 2-Dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one (Omnirad 379: manufactured by IGM Resins BV) *4: Bisphenol A type epoxy resin (JER (registered trademark)-834: manufactured by Mitsubishi Chemical Corporation) *5: Triglycidyl isocyanurate (TEPIC-HP: manufactured by Nissan Chemical Industries, Ltd.) *6: Polyester modified polydimethylsiloxane (BYK (registered trademark)-313: manufactured by BYK Japan) *7: Polyether modified polydimethylsiloxane (BYK (registered trademark)-300: manufactured by BYK Japan) *8: Spherical silica (D50=0.6μm) (SFP-130MC: manufactured by Denki Kagaku Kogyo Co., Ltd.) *9: Spherical silica (D50 = 0.4 μm) (SFP-20M: manufactured by Denki Kagaku Kogyo Co., Ltd.) *10: Polyhydroxycarboxylic acid ester (BYK (registered trademark)-R 606: manufactured by BYK Japan) *11: Melamine (Melamine: Nissan Chemical Industries, Ltd.) *12: Spherical silica with a methacrylsilane-treated surface (1.5 μm SM-C4: manufactured by Admatechs Co., Ltd.) *13: Dipentaerythritol hexaacrylate (DPHA: manufactured by Nippon Kayaku Co., Ltd.) *14: Dicyandiamide (DICY7: manufactured by Mitsubishi Chemical Corporation) *15: Blue pigment (Firstgen Blue 5380: manufactured by DIC). Table 1 indicates the mass parts of solid content. *16: Yellow pigment (Cromophtal (registered trademark) Yellow S1515: manufactured by BASF). Table 1 indicates the mass parts of solid content. *17: Dipropylene glycol methyl ether (Dowanol (registered trademark) DPM: manufactured by Dow Chemical Japan)
[0114] As shown in the examples of Table 1, when (D) a silicone compound, (E) hydrophilic silica, and (F) an organic thixotropic agent are blended, the wettability of the curable composition of the present invention to a copper-clad substrate (base material) is maintained, the leveling property is good, and aggregation and precipitation of (E) hydrophilic silica does not occur. In addition, even when the mixture for wetting tension test is applied to a base material to which a cured product of the curable composition of the present invention is fixed, there is no repulsion of the mixture for wetting tension test on the cured product, and the wettability of the mixture for wetting tension test to the cured product is maintained.
[0115] On the other hand, in Comparative Example 1 in which the surface of the silica was subjected to hydrophobic treatment, even if the (F) organic thixotropic agent was blended, the wettability of the mixture for the wet tension test to the substrate on which the cured product of the curable composition was fixed was reduced, and it was considered that the solderability was reduced. In Comparative Example 2 in which the (F) organic thixotropic agent was not included, even if the (D) silicone compound and (E) hydrophilic silica were blended, the wettability of the mixture for the wet tension test to the substrate on which the cured product of the curable composition was fixed was reduced, and it was considered that the solderability was reduced. Furthermore, in Comparative Example 3 in which the (D) silicone compound was not included, the wettability of the curable composition to the copper-clad substrate (substrate) was insufficient, or the leveling property was deteriorated.
Claims
1. (A) an alkali-soluble resin; (B) a photopolymerization initiator; (C) an epoxy resin; and (D) a silicone compound; (E) hydrophilic silica; and (F) an organic thixotropic agent; Including, The (F) organic thixotropic agent is a polyhydroxycarboxylic acid ester, the amount of the hydrophilic silica (E) is in the range of 20 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the alkali-soluble resin (A); (E) A curable composition characterized in that the median diameter D50 of hydrophilic silica is 5.0 μm or less.
2. (E) The curable composition described in claim 1, characterized in that the median diameter D50 of the hydrophilic silica is 2.0 μm or less.
3. (E) The curable composition according to claim 1, characterized in that the median diameter D50 of the hydrophilic silica is 0.2 μm or more.
4. The curable composition according to claim 1, characterized in that the median diameter D50 of the hydrophilic silica (E) is 0.2 μm or more and 2.0 μm or less.
5. The curable composition according to any one of claims 1 to 4, characterized in that the amount of the organic thixotropic agent (F) is 0.01 parts by mass or more and 15 parts by mass or less relative to 100 parts by mass of the hydrophilic silica (E), and is 0.05 parts by mass or more relative to 2 parts by mass of the silicone compound (D).
6. The curable composition according to any one of claims 1 to 5, further comprising (G) an antioxidant.
7. A dry film obtained by applying the curable composition according to any one of claims 1 to 6 onto a carrier film and drying the applied composition.
8. A cured product obtained by curing a dried coating film obtained by applying the curable composition according to any one of claims 1 to 7 onto a substrate and drying the same, or a coating film obtained by applying the curable composition onto a carrier film and drying the same to a substrate and laminating the resulting dry film on the substrate.
9. An electronic component comprising the cured product according to claim 8.
Citation Information
Patent Citations
White alkali-developable photocurable and thermosetting solder resist composition, and metal-base circuit substrate using the same
JP2009194222A
Photosensitive resin composition and printed wiring board
JP2013156506A
Photosensitive resin composition, dry film, cured product and printed wiring board
JP2019032474A