Heat-sealable resin composition, heat-sealing material, packaging material, lid material, and packaging container
The heat-sealable resin composition, combining ethylene-vinyl ester copolymer with alicyclic and aromatic hydrocarbon resins, addresses the challenge of achieving both transparency and peel strength in heat-sealing materials for APET and si-APET containers.
Patent Information
- Application Number
- JP2023506916
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-18
- Filing Date
- 2022-02-25
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2042-02-25
Smart Images

Figure 0007596510000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat-sealable resin composition, a heat-sealing material, a packaging material, a lid material, and a packaging container. [Background technology]
[0002] Packaging containers are widely used as containers for food, medicine, etc. A variety of heat-sealing materials have been proposed and put into practical use to seal these packaging containers with lids. For example, a resin composition containing an ethylene-vinyl ester copolymer is known as such a heat-sealing material.
[0003] As a technique relating to a resin composition containing such an ethylene-vinyl ester copolymer, Patent Document 1 proposes an adhesive for container lid sealants, which comprises 10 to 50 parts by weight of an ethylene-vinyl acetate copolymer (A) having a vinyl acetate content of 3 to 15% by weight, 10 to 50 parts by weight of an ethylene-vinyl acetate copolymer (B) having a vinyl acetate content of 8 to 25% by weight, and 5 to 40 parts by weight of a tackifier resin (C) (the total of (A), (B) and (C) is 100 parts by weight), and the difference between the vinyl acetate content of the ethylene-vinyl acetate copolymer (A) and the vinyl acetate content of the ethylene-vinyl acetate copolymer (B) is 3 to 20% by weight, and the vinyl acetate content of the ethylene-vinyl acetate copolymer (A) is smaller than the vinyl acetate content of the ethylene-vinyl acetate copolymer (B).
[0004] Patent Document 2 proposes a sealant adhesive for polyethylene terephthalate which contains 50 to 92 wt% of an ethylene-vinyl acetate copolymer (A) consisting of 68 to 90 wt% ethylene residue units and 3 to 32 wt% vinyl acetate residue units and having a melt flow rate of 1 to 40 g / 10 min as measured according to JIS K 6924-1, 3 to 30 wt% of a saponified ethylene-vinyl acetate copolymer (B) consisting of 50 to 94 wt% ethylene residue units, 0 to 40 wt% vinyl acetate residue units and 1.2 to 50 wt% vinyl alcohol residue units, and 5 to 20 wt% of a tackifier (C) (the total of (A), (B) and (C) is 100 wt%) and has a melt flow rate of 1 to 100 g / 10 min as measured according to JIS K 6924-1.
[0005] Furthermore, Patent Document 3 proposes a hot melt composition comprising 20 to 45% by weight of an ethylene-unsaturated ester copolymer (A), 3 to 45% by weight of a polyethylene wax grafted with a styrene monomer (B), and 30 to 70% by weight of a wax (C) having a melting point of 40°C or higher and lower than 80°C and a Saybolt universal viscosity at 120°C of 20 to 300 seconds, the total amount of the wax (B) and the wax (C) being 50 to 80% by weight. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP2018-76398A [Patent Document 2] JP2017-132851A [Patent Document 3] JP2017-149850A Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, the food packaging market has been switching from containers with a lid to containers in which the lid material is attached to the container body by heat sealing. Polyethylene, polystyrene, etc. are widely and generally used as container bodies. Amorphous polyethylene terephthalate (hereinafter also referred to as "APET") has also been attracting attention as a container body. However, with conventional heat seal materials, it was difficult to obtain sufficient peel strength with respect to the APET container body while maintaining the transparency of the heat seal material. In addition, there was a problem that the transparency of the heat seal material was impaired when trying to increase the peel strength of the heat seal material with respect to APET. This problem was particularly noticeable when amorphous polyethylene terephthalate coated with silicone (hereinafter also referred to as "si-APET") was used for the container body, and there was a demand for a heat seal material that exhibits sufficient peel strength with respect to si-APET while maintaining the transparency of the heat seal material.
[0008] The present disclosure has been made in view of the above, and aims to provide a heat-sealable resin composition capable of producing a heat-sealable material having excellent transparency and excellent peel strength against APET and si-APET, as well as a heat-sealable material, a packaging material, a lid material, and a packaging container obtained from the heat-sealable resin composition. [Means for solving the problem]
[0009] Specific means for solving the above problems include the following aspects. <1> An ethylene-vinyl ester copolymer (A), (B) an ethylene-unsaturated carboxylic acid ester copolymer; A tackifier resin (C); Including, the content of structural units derived from vinyl ester contained in the ethylene-vinyl ester copolymer (A) is 8 mass% or more based on the total structural units of the copolymer constituting the ethylene-vinyl ester copolymer (A); The tackifier resin (C) is a heat-sealable resin composition containing an alicyclic hydrocarbon resin (C1) and an aromatic hydrocarbon resin (C2). <2> The content of the tackifier resin (C) is 1% by mass or more and 40% by mass or less, when the total mass of the resin components contained in the heat-sealable resin composition is taken as 100% by mass. <1> The heat-sealable resin composition according to claim 1. <3> The softening point of the aromatic hydrocarbon resin (C2) is 70° C. or higher and 140° C. or lower. <1> or <2> The heat-sealable resin composition according to claim 1. <4> a mass ratio (C2 / (C1+C2)) of the content of the aromatic hydrocarbon resin (C2) to the total content of the alicyclic hydrocarbon resin (C1) and the aromatic hydrocarbon resin (C2) is 0.05 or more and 0.8 or less. <1> ~ <3> 13. The heat-sealable resin composition according to claim 12, <5> The content of the ethylene-vinyl ester copolymer (A) is 20% by mass or more and 80% by mass or less, when the total mass of the resin components contained in the heat-sealable resin composition is 100% by mass. <1> ~ <4> 13. The heat-sealable resin composition according to claim 12, <6> a mass ratio (B / A) of the content of the ethylene-unsaturated carboxylic acid ester copolymer (B) to the content of the ethylene-vinyl ester copolymer (A) is 0.20 or more and 1.0 or less; <1> ~ <5> 13. The heat-sealable resin composition according to claim 12, <7> The haze measured by the following method is less than 6.0% <1> ~ <6> 13. The heat-sealable resin composition according to claim 12, (method) Using a 40mmφ 3-type 3-layer cast molding machine, co-extruded low-density polyethylene (density = 917kg / m 3 The heat-sealable resin composition is laminated by cast molding with an air knife at a processing temperature of 200° C. and a processing speed of 30 m / min to obtain a packaging material of low-density polyethylene (thickness 22 μm) / heat-sealable resin composition layer (thickness 8 μm). Next, the haze of the obtained packaging material is measured by a haze meter in accordance with JIS K 7136:2000. <8> <1> ~ <7> A heat-sealing material comprising the heat-sealable resin composition according to any one of the above items. <9> A base material layer and a film provided on one surface of the base material layer. <8> A packaging material comprising a heat seal layer comprising the heat seal material according to claim 1. <10> <9> A lid material comprising the packaging material described in claim 1. <11> A container body having an opening, and a lid for covering the opening of the container body <10> A packaging container comprising the lid material described above. <12> At least a portion of the container body contains amorphous polyethylene terephthalate <11> The packaging container according to claim 1. <13> At least a portion of the container body comprises amorphous polyethylene terephthalate coated with silicone. <11> or <12> The packaging container according to claim 1. Effect of the Invention
[0010] According to the present disclosure, it is possible to provide a heat-sealable resin composition capable of producing a heat-sealable material having excellent transparency and excellent peel strength against APET and si-APET, as well as a heat-sealable material, a packaging material, a lid material, and a packaging container obtained from the heat-sealable resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present disclosure will be described as an example. The present disclosure is not limited to the following embodiment, and can be implemented with appropriate modifications within the scope of the object of the present disclosure.
[0012] In the present disclosure, "to" in a numerical range means including the numerical values before and after "to". In the numerical ranges described in stages in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples. In the present disclosure, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the constituent units of the plurality of substances present in the composition, unless otherwise specified. In this disclosure, (meth)acrylic acid means acrylic acid and methacrylic acid. In this disclosure, the total mass of the resin components means the combined mass of the ethylene-vinyl ester copolymer (A), the ethylene-unsaturated carboxylic acid ester copolymer (B), the tackifier resin (C), and other resins contained as necessary.
[0013] [Heat-sealable resin composition] The heat-sealable resin composition of the present disclosure comprises an ethylene-vinyl ester copolymer (A), an ethylene-unsaturated carboxylic acid ester copolymer (B), and a tackifier resin (C), wherein the content of constituent units derived from vinyl ester contained in the ethylene-vinyl ester copolymer (A) is 8 mass% or more based on all constituent units of the copolymers constituting the ethylene-vinyl ester copolymer (A), and the tackifier resin (C) comprises an alicyclic hydrocarbon resin (C1) and an aromatic hydrocarbon resin (C2).
[0014] In recent years, the food packaging market has been switching from containers with jointed lids to containers in which the lid material is bonded to the container body by heat sealing. The present inventors have been studying a resin composition containing an ethylene-vinyl ester copolymer (A) and a tackifier resin (C) as a heat-sealable resin composition to be used as a heat-sealing material for the lid material to be bonded to the container body.
[0015] However, when an alicyclic hydrocarbon resin (C1) was used as the tackifier resin (C) contained in the heat-sealable resin composition, the adhesion of the heat-sealable material to silicone-coated amorphous polyethylene terephthalate (si-APET) was insufficient. Furthermore, when an aromatic hydrocarbon resin (C2) was used as the tackifier resin (C) contained in the heat-sealable resin composition, the adhesion of the heat-sealable material to amorphous polyethylene terephthalate (APET) was insufficient, and it was difficult to prepare a heat-sealable material with excellent transparency. We also considered combining an alicyclic hydrocarbon resin (C1) with an aromatic hydrocarbon resin (C2) as the tackifier resin (C), but even when combining these, it was difficult to achieve both the adhesion of the heat seal material to si-APET and excellent transparency of the heat seal material.
[0016] Taking the above into consideration, the present inventors have found that it is possible to produce a heat-sealable material having excellent transparency and excellent peel strength against APET and si-APET by using a heat-sealable resin composition containing an ethylene-vinyl ester copolymer (A) having a content of constituent units derived from vinyl ester within a specific range, an ethylene-unsaturated carboxylic acid ester copolymer (B), and a tackifier resin (C) containing an alicyclic hydrocarbon resin (C1) and an aromatic hydrocarbon resin (C2). The heat-sealable resin composition of the present disclosure is preferably used to prepare a heat-sealing material for a container body made of, for example, amorphous polyethylene terephthalate (APET), polypropylene, polyester, polycarbonate, polyvinyl chloride, or the like, and more preferably used to prepare a heat-sealing material for a container body made of silicone-coated amorphous polyethylene terephthalate (si-APET).
[0017] Hereinafter, each component contained in the heat-sealable resin composition of the present disclosure will be described.
[0018] <Ethylene-vinyl ester copolymer (A)> The heat-sealable resin composition of the present disclosure contains an ethylene-vinyl ester copolymer (A). The ethylene-vinyl ester copolymer (A) is not particularly limited as long as it is a copolymer containing a structural unit derived from ethylene and a structural unit derived from a vinyl ester. The ethylene-vinyl ester copolymer (A) may be used alone or in combination of two or more kinds.
[0019] Examples of the ethylene-vinyl ester copolymer (A) include ethylene-vinyl acetate copolymer, ethylene-vinyl propionate copolymer, ethylene-vinyl butyrate copolymer, ethylene-vinyl stearate copolymer, etc. Among these, ethylene-vinyl acetate copolymer is preferred.
[0020] The ethylene-vinyl ester copolymer (A) may be a copolymer consisting only of structural units derived from ethylene and structural units derived from vinyl ester, or may be a copolymer containing structural units derived from a monomer other than ethylene and vinyl ester.
[0021] Examples of monomers other than ethylene and vinyl esters include unsaturated hydrocarbons such as propylene, butene, 1,3-butadiene, pentene, 1,3-pentadiene, and 1-hexene; oxides such as vinyl sulfate and vinyl nitrate; halogen compounds such as vinyl chloride and vinyl fluoride; primary and secondary amine compounds containing a vinyl group; carbon monoxide; and sulfur dioxide.
[0022] The content of constituent units derived from vinyl ester contained in the ethylene-vinyl ester copolymer (A) is 8% by mass or more, based on all constituent units of the copolymer constituting the ethylene-vinyl ester copolymer (A). From the viewpoint of the balance between the transparency when used as a heat seal material and the peel strength against si-APET, the content is preferably 8% by mass or more and 46% by mass or less, more preferably 9% by mass or more and 42% by mass or less, and even more preferably 10% by mass or more and 35% by mass or less.
[0023] The content of structural units derived from ethylene contained in the ethylene-vinyl ester copolymer (A) is preferably 54 mass% or more and 92 mass% or less, more preferably 58 mass% or more and 91 mass% or less, and even more preferably 65 mass% or more and 90 mass% or less, based on all structural units of the copolymer constituting the ethylene-vinyl ester copolymer (A).
[0024] The ethylene-vinyl ester copolymer (A) may or may not contain structural units derived from monomers other than ethylene and vinyl ester. The content of structural units derived from monomers other than ethylene and vinyl ester that can be contained in the ethylene-vinyl ester copolymer may be 0% by mass or more and 10% by mass or less, or 0% by mass or more and 5% by mass or less, based on the total structural units of the copolymer constituting the ethylene-vinyl ester copolymer (A).
[0025] The melt mass flow rate (MFR; JIS K 7210:1999, 190°C, load 2160 g) of the ethylene-vinyl ester copolymer (A) is preferably 0.1 g / 10 min to 50 g / 10 min, more preferably 0.5 g / 10 min to 20 g / 10 min, and further preferably 1 g / 10 min to 10 g / 10 min.
[0026] The content of the ethylene-vinyl ester copolymer (A) in the heat-sealable resin composition is preferably 20% by mass or more and 80% by mass or less, when the total mass of the resin components in the heat-sealable resin composition is taken as 100% by mass, and from the viewpoint of being able to produce a heat-sealable material having superior peel strength to APET, the content is more preferably 25% by mass to 70% by mass, and even more preferably 30% by mass to 60% by mass.
[0027] The method for producing the ethylene-vinyl ester copolymer (A) is not particularly limited, and it can be produced by a known method. For example, it can be obtained by radical copolymerization of each polymerization component under high temperature and pressure. It can be produced by either an autoclave method or a tubular method. In addition, the ethylene-vinyl ester copolymer (A) may be a commercially available product.
[0028] <Ethylene-unsaturated carboxylic acid ester copolymer (B)> The heat-sealable resin composition of the present disclosure contains an ethylene-unsaturated carboxylic acid ester copolymer (B). The ethylene-unsaturated carboxylic acid ester copolymer (B) is not particularly limited as long as it is a copolymer containing a structural unit derived from ethylene and a structural unit derived from an unsaturated carboxylic acid ester. A specific example of the ethylene-unsaturated carboxylic acid ester copolymer (B) is a copolymer composed of ethylene and an unsaturated carboxylic acid alkyl ester. The ethylene-unsaturated carboxylic acid ester copolymer (B) may be used alone or in combination of two or more kinds.
[0029] Examples of the unsaturated carboxylic acid in the unsaturated carboxylic acid ester, preferably the unsaturated carboxylic acid in the alkyl ester, include acrylic acid, methacrylic acid, 2-ethylacrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, maleic anhydride, fumaric anhydride, itaconic anhydride, monomethyl maleate, and monoethyl maleate. Among these, the unsaturated carboxylic acid preferably includes at least one selected from acrylic acid and methacrylic acid from the viewpoints of productivity, hygiene, etc. of the ethylene-unsaturated carboxylic acid ester copolymer (B).
[0030] The alkyl moiety in the unsaturated carboxylic acid alkyl ester may be an alkyl group having 1 to 12 carbon atoms, more specifically, methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, secondary butyl group, 2-ethylhexyl group, isooctyl group, etc. The number of carbon atoms in the alkyl moiety in the unsaturated carboxylic acid alkyl ester is preferably 1 to 8.
[0031] Examples of the unsaturated carboxylic acid alkyl ester include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, isobutyl (meth)acrylate, n-butyl (meth)acrylate, isooctyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. The unsaturated carboxylic acid alkyl ester may be used alone or in combination of two or more. Among these, it is more preferable to include at least one selected from methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, isobutyl (meth)acrylate, and n-butyl (meth)acrylate.
[0032] The ethylene-unsaturated carboxylic acid ester copolymer (B) is preferably an ethylene-(meth)acrylic acid ester copolymer, and specifically, preferred ethylene-unsaturated carboxylic acid ester copolymers include ethylene-methyl (meth)acrylate copolymer, ethylene-ethyl (meth)acrylate copolymer, ethylene-isopropyl (meth)acrylate copolymer, ethylene-n-propyl (meth)acrylate copolymer, ethylene-isobutyl (meth)acrylate copolymer, ethylene-n-butyl (meth)acrylate copolymer, ethylene-isooctyl (meth)acrylate copolymer, and ethylene-2-ethylhexyl (meth)acrylate copolymer.
[0033] The ethylene-unsaturated carboxylate copolymer (B) may be a copolymer consisting only of structural units derived from ethylene and structural units derived from an unsaturated carboxylate, or may be a copolymer containing structural units derived from a monomer other than ethylene and an unsaturated carboxylate.
[0034] Examples of monomers other than ethylene and unsaturated carboxylate esters include unsaturated hydrocarbons such as propylene, butene, 1,3-butadiene, pentene, 1,3-pentadiene, and 1-hexene; oxides such as vinyl sulfate and vinyl nitrate; halogen compounds such as vinyl chloride and vinyl fluoride; primary and secondary amine compounds containing a vinyl group; carbon monoxide; and sulfur dioxide.
[0035] The content of the constituent units derived from the unsaturated carboxylate contained in the ethylene-unsaturated carboxylate copolymer (B) is preferably 5 mass% or more and 50 mass% or less, more preferably 6 mass% or more and 45 mass% or less, and even more preferably 8 mass% or more and 40 mass% or less, based on the total constituent units of the copolymer constituting the ethylene-unsaturated carboxylate copolymer (B).
[0036] The content of the structural units derived from ethylene contained in the ethylene-unsaturated carboxylic acid ester copolymer (B) is preferably 50 mass% or more and 95 mass% or less, more preferably 55 mass% or more and 94 mass% or less, and even more preferably 60 mass% or more and 92 mass% or less, based on all the structural units of the copolymer constituting the ethylene-unsaturated carboxylic acid ester copolymer (B).
[0037] The ethylene-unsaturated carboxylate copolymer (B) may or may not contain structural units derived from monomers other than ethylene and unsaturated carboxylate esters. The content of structural units derived from monomers other than ethylene and unsaturated carboxylate esters that can be contained in the ethylene-unsaturated carboxylate copolymer may be 0% by mass or more and 10% by mass or less, or 0% by mass or more and 5% by mass or less, based on the total structural units of the copolymer constituting the ethylene-unsaturated carboxylate copolymer (B).
[0038] The melt mass flow rate (MFR; JIS K 7210:1999, 190°C, load 2160 g) of the ethylene-unsaturated carboxylic acid ester copolymer (B) is preferably 0.1 g / 10 min to 100 g / 10 min, more preferably 1 g / 10 min to 50 g / 10 min, and further preferably 5 g / 10 min to 30 g / 10 min.
[0039] In the heat-sealable resin composition, the mass ratio (B / A) of the content of the ethylene-unsaturated carboxylic acid ester copolymer (B) to the content of the ethylene-vinyl ester copolymer (A) is, from the viewpoints of the balance of the transparency and the peel strength against APET and si-APET when used as a heat-sealable material, preferably from 0.20 to 1.0, more preferably from 0.30 to 0.95, and even more preferably from 0.40 to 0.90.
[0040] The method for producing the ethylene-unsaturated carboxylic acid ester copolymer (B) is not particularly limited, and it can be produced by a known method. For example, it can be obtained by radical copolymerization of each polymerization component under high temperature and high pressure. It can be produced by either an autoclave method or a tubular method. In addition, the ethylene-unsaturated carboxylic acid ester copolymer (B) may be a commercially available product.
[0041] The average ester content of the vinyl ester-derived structural unit contained in the ethylene-vinyl ester copolymer (A) and the unsaturated carboxylate-derived structural unit contained in the ethylene-unsaturated carboxylate copolymer (B) is preferably more than 14% by mass, more preferably 15% by mass or more, even more preferably 16% by mass or more, and particularly preferably more than 18% by mass, from the viewpoint of the balance between the transparency when used as a heat seal material and the peel strength against si-APET. There is no particular limitation on the upper limit, but it is preferably 46% by mass or less from the viewpoint of preventing blocking, and more preferably 30% by mass or less, even more preferably 25% by mass or less, and particularly preferably 20% by mass or less from the viewpoint of the peel strength against si-APET. The average ester content can be calculated using the following formula: (Content of structural units derived from vinyl ester contained in ethylene-vinyl ester copolymer (A) [mass%] × Content of ethylene-vinyl ester copolymer (A) [mass%] + Content of structural units derived from unsaturated carboxylate contained in ethylene-unsaturated carboxylate copolymer (B) [mass%] × Content of ethylene-unsaturated carboxylate copolymer (B) [mass%]) ÷ (Content of ethylene-vinyl ester copolymer (A) [mass%] + Content of ethylene-unsaturated carboxylate copolymer (B) [mass%])
[0042] <Tackifying resin (C)> The heat-sealable resin composition of the present disclosure contains a tackifier resin (C). The tackifier resin (C) further contains an alicyclic hydrocarbon resin (C1) and an aromatic hydrocarbon resin (C2). The alicyclic hydrocarbon resin (C1) and the aromatic hydrocarbon resin (C2) may each independently be used alone or in combination of two or more kinds.
[0043] Examples of the alicyclic hydrocarbon resin (C1) include resins obtained by cyclodimerizing and then polymerizing diene components in spent C4-C5 fractions, resins obtained by polymerizing cyclic monomers such as cyclopentadiene, and resins obtained by internally hydrogenating aromatic hydrocarbon resins. Among these, resins obtained by internally hydrogenating aromatic hydrocarbon resins are more preferred.
[0044] Examples of the aromatic hydrocarbon resin (C2) include resins mainly composed of C8-C10 vinyl aromatic hydrocarbons such as vinyltoluene, indene, and α-methylstyrene, styrene, isopropenyltoluene, and the like, and resins (aliphatic-aromatic copolymer hydrocarbon resins) obtained by copolymerizing these C8-C10 vinyl aromatic hydrocarbons, styrene, and isopropenyltoluene with C4 or C5 mono- or diolefins described below. Among these, resins mainly composed of α-methylstyrene and resins mainly composed of styrene are more preferred, and resins mainly composed of α-methylstyrene are even more preferred. The term "mainly composed of" means that the content of the constituent unit derived from the component exceeds 50% by mass with respect to the total constituent units of the resin.
[0045] The heat-sealable resin composition of the present disclosure may contain a tackifier resin other than the alicyclic hydrocarbon resin (C1) and the aromatic hydrocarbon resin (C2). Examples of the other tackifier resin include an aliphatic hydrocarbon resin, a coumarone-indene resin, a terpene resin, and a rosin.
[0046] Examples of the aliphatic hydrocarbon resin include polymers mainly composed of C4 or C5 mono- or diolefins such as 1-butene, isobutylene, butadiene, 1,3-pentadiene, isoprene, and piperylene.
[0047] Examples of the terpene resin include α-pinene polymers, β-pinene polymers, dipentene polymers, terpene-phenol copolymers, α-pinene-phenol copolymers, and hydrogenated terpene resins (hydrogenated terpene resins).
[0048] Examples of rosins include gum rosin, wood rosin, tall oil rosin, and modified products thereof, etc. Modified products include those modified by hydrogenation, disproportionation, dimerization, esterification, etc.
[0049] From the viewpoints of thermal stability and flexibility, the softening point of the alicyclic hydrocarbon resin (C1) is preferably 85°C or more and 155°C or less, more preferably 100°C or more and 145°C or less, and even more preferably 110°C or more and 130°C or less. In the present disclosure, the softening point means the ring and ball softening point measured in accordance with JIS K 6863:1994.
[0050] From the viewpoint of thermal stability and flexibility, the softening point of the aromatic hydrocarbon resin (C2) is preferably 70°C or more and 140°C or less, more preferably 85°C or more and 130°C or less, and even more preferably 95°C or more and 115°C or less.
[0051] From the viewpoints of the peel strength against APET and si-APET when used as a heat-sealing material, as well as the processability and handleability of the resin composition, the content of the tackifier resin (C) in the heat-sealable resin composition is preferably from 1 to 40% by mass, more preferably from 10 to 35% by mass, and even more preferably from 15 to 30% by mass, when the total mass of the resin components contained in the heat-sealable resin composition is taken as 100% by mass.
[0052] In the heat-sealable resin composition, the mass ratio (C2 / (C1+C2)) of the content of the aromatic hydrocarbon resin (C2) to the total content of the alicyclic hydrocarbon resin (C1) and the aromatic hydrocarbon resin (C2) is, from the viewpoint of the balance between the transparency when used as a heat-sealable material and the peel strength against si-APET, preferably from 0.05 to 0.8, more preferably from 0.08 to 0.6, and even more preferably from 0.1 to 0.5.
[0053] The heat-sealable resin composition may or may not contain other tackifier resins. The mass ratio of the content of the other tackifier resins to the total content of the alicyclic hydrocarbon resin (C1), the aromatic hydrocarbon resin (C2) and the other tackifier resins (hereinafter also referred to as the "total content of tackifier resins (C)") (content of other tackifier resins / total content of tackifier resins (C)) may be 0 or more and 0.1 or less, or 0 or more and 0.05 or less.
[0054] In the heat-sealable resin composition of the present disclosure, the total content of the ethylene-vinyl ester copolymer (A), the ethylene-unsaturated carboxylic acid ester copolymer (B) and the tackifier resin (C) is preferably 80% by mass to 100% by mass, more preferably 85% by mass to 100% by mass, even more preferably 90% by mass to 100% by mass, even more preferably 95% by mass to 100% by mass, particularly preferably 98% by mass to 100% by mass, and especially preferably more than 99% by mass to 100% by mass or less, when the total mass of the resin components contained in the heat-sealable resin composition is 100% by mass.
[0055] <Other ingredients> The heat-sealable resin composition of the present disclosure may contain components other than the ethylene-vinyl ester copolymer (A), the ethylene-unsaturated carboxylic acid ester copolymer (B), and the tackifier resin (C) (hereinafter also referred to as "other components") within the scope of not impairing the effects of the present invention. The other components are not particularly limited, and examples thereof include additives, other resins such as thermoplastic resins and thermosetting resins. Examples of additives include plasticizers, antioxidants, ultraviolet absorbers, antistatic agents, surfactants, colorants, light stabilizers, foaming agents, lubricants, crystal nucleating agents, crystallization accelerators, crystallization retarders, catalyst deactivators, inorganic fillers, organic fillers, impact resistance improvers, slip agents, crosslinking agents, crosslinking assistants, silane coupling agents, processing assistants, release agents, hydrolysis inhibitors, heat stabilizers, antiblocking agents, antifogging agents, flame retardants, flame retardant assistants, light diffusing agents, antibacterial agents, antifungal agents, dispersants, etc. The other components may be used alone or in combination of two or more.
[0056] <Method for preparing heat-sealable resin composition> The method for preparing the heat-sealable resin composition of the present disclosure is not particularly limited, and examples thereof include a method for preparing the composition by dry blending and mixing the ethylene-vinyl ester copolymer (A), the ethylene-unsaturated carboxylic acid ester copolymer (B), the tackifier resin (C) containing the alicyclic hydrocarbon resin (C1) and the aromatic hydrocarbon resin (C2), and other components added as necessary, and a method for preparing the composition by melt-kneading these components in an extruder or the like.
[0057] <Physical Properties of Heat-Sealable Resin Composition> In the heat-sealable resin composition of the present disclosure, from the viewpoint of transparency of the heat-sealing material, the haze measured by the method described below is preferably less than 6.0%, more preferably 5.8% or less, and even more preferably 5.5% or less. (method) Using a 40mmφ 3-type 3-layer cast molding machine, co-extruded low-density polyethylene (density = 917kg / m 3 The heat-sealable resin composition is laminated by cast molding with an air knife at a processing temperature of 200° C. and a processing speed of 30 m / min to obtain a packaging material of low-density polyethylene (thickness 22 μm) / heat-sealable resin composition layer (thickness 8 μm). Next, the haze of the obtained packaging material is measured by a haze meter in accordance with JIS K 7136:2000.
[0058] In the heat-sealable resin composition of the present disclosure, the lower limit of the haze measured by the above method is not particularly limited, and may be, for example, 1.0% or more, or 2.0% or more.
[0059] [Heat seal material] The heat seal material of the present disclosure is composed of the heat sealable resin composition of the present disclosure. The heat seal material of the present disclosure has excellent transparency and excellent peel strength against APET and si-APET. Since the heat seal material of the present disclosure has excellent peel strength against APET and si-APET, it can be particularly suitably used as a lid material for a container body made of APET or si-APET.
[0060] The method for producing the heat seal material is not particularly limited, and includes conventionally known methods, such as press molding, extrusion molding, injection molding, compression molding, cast molding, calendar molding, and inflation molding.
[0061] [Packaging and lid materials] The packaging material of the present disclosure comprises a base layer and a heat seal layer including the heat seal material of the present disclosure provided on one side of the base layer. The packaging material of the present disclosure has excellent transparency and excellent peel strength against APET and si-APET because it includes a heat seal layer including the heat seal material of the present disclosure. Therefore, a lid material including the packaging material of the present disclosure can be particularly suitably used as a lid material for a container body.
[0062] In the packaging material, the thickness of the heat seal layer is preferably 5 μm or more and 200 μm or less, and more preferably 10 μm or more and 100 μm or less.
[0063] The heat seal layer may be a single layer or a multi-layer structure of two or more layers. When the heat seal layer is two or more layers, the heat seal layer may be a laminate of two or more layers of the heat seal material of the present disclosure, or may be a laminate of at least one layer of the heat seal material of the present disclosure and at least one layer of another heat seal material. Examples of resins used in other heat seal materials include low-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-acrylic acid copolymer or ionomer thereof, ethylene-methacrylic acid copolymer or ionomer thereof, ethylene-(meth)acrylic acid ester copolymer, ethylene-vinyl ester copolymer, ethylene-vinyl alcohol copolymer, crystalline or amorphous polyester modified product, or a multi-component copolymer or mixture thereof.
[0064] The base layer is a layer provided for the purpose of improving the properties of the packaging material, such as the handling property, mechanical properties, electrical conductivity, heat insulation, heat resistance, moisture resistance, etc. Examples of the base layer include paper, nonwoven fabric, metal layers (aluminum foil, etc.), polyester films, nylon films, polyethylene films, polypropylene films, polyamide films, polyimide films, polyvinylidene chloride films, ethylene-vinyl alcohol copolymer films, aluminum films, etc. Examples of the substrate layer include aluminum-deposited plastic film, silica-deposited plastic film, alumina-deposited plastic film, and amorphous polyethylene terephthalate film. The substrate layer may be a single layer or a combination of two or more layers. The substrate layer may be uniaxially or biaxially stretched at any ratio.
[0065] In order to improve the adhesion between the base layer and the heat seal layer, the base layer may be subjected to a surface treatment, specifically, corona treatment, plasma treatment, undercoat treatment, primer coat treatment, etc.
[0066] The thickness of the substrate layer is preferably from 1 μm to 100 μm, more preferably from 2 μm to 50 μm, and further preferably from 5 μm to 40 μm. The shape of the substrate layer is not particularly limited, and examples thereof include a sheet shape, a film shape, and the like.
[0067] The packaging material of the present disclosure may be a packaging material consisting of only a base layer and a heat seal layer, or may be a packaging material having layers other than the base layer and the heat seal layer (hereinafter also referred to as "other layers") from the viewpoint of imparting various functions to the packaging material. Examples of the other layers include a foam layer, a metal layer, an inorganic layer, a gas barrier resin layer, an antistatic layer, a hard coat layer, an adhesive layer, an antireflection layer, an antifouling layer, etc. The other layers may be a single layer or a combination of two or more layers. The adhesive layer is, for example, a layer provided to increase the adhesion between the layers.
[0068] When the heat seal layer has two or more layers, the method of laminating the layers, the method of laminating the base material layer and the heat seal layer, or the method of laminating the base material layer, the heat seal layer and another layer can be a known method, such as an extrusion lamination method, a co-extrusion inflation method, or a co-extrusion T-die method.
[0069] The wrapping materials of the present disclosure may be uniaxially or biaxially stretched at any rate.
[0070] The packaging material of the present disclosure can be formed into various shapes by molding the heat-sealable resin composition of the present disclosure using a molding method such as extrusion molding, injection molding, blow molding, film molding, or sheet molding. The shape of the packaging material is not particularly limited, and examples thereof include a sheet shape, a film shape, and the like.
[0071] The packaging material of the present disclosure can be suitably used as a packaging material for packaging, for example, food, medicines, industrial products, daily necessities, cosmetics, etc., and can be particularly suitably used as a packaging material for food or medicines.
[0072] [Packaging container] The packaging container of the present disclosure includes, for example, a container body having an opening and the above-described lid material of the present disclosure that covers the opening of the container body. The lid material of the present disclosure has excellent transparency and excellent peel strength against APET and si-APET.
[0073] The component contained in at least a part of the container body having an opening is not particularly limited, and examples thereof include amorphous polyethylene terephthalate (APET), polypropylene, polyester, polycarbonate, polyvinyl chloride, etc. Among them, amorphous polyethylene terephthalate (APET) is preferable, and amorphous polyethylene terephthalate coated with silicone (si-APET) is more preferable. The aforementioned components need only be contained in at least a portion of the container body having an opening, and are preferably contained in the portion that comes into contact with the lid material of the present disclosure, and more preferably contained in the portion that comes into contact with the heat seal material contained in the packaging material of the lid material.
[0074] The packaging container of the present disclosure can be suitably used as a packaging container for packaging, for example, food, medicines, industrial products, daily necessities, cosmetics, etc., and can be particularly suitably used as a packaging container for food or medicines.
[0075] The heat-sealable resin composition, heat-sealing material, packaging material, lid material, and packaging container of the present disclosure have been described above, but these are merely examples of the present invention, and various configurations other than those described above can also be adopted. EXAMPLES
[0076] Hereinafter, the present disclosure will be described more specifically with reference to examples. However, the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure.
[0077] Details of the components used in the preparation of the heat-sealable resin composition are as follows.
[0078] <Other ethylene vinyl ester copolymers> EVA1: Ethylene-vinyl acetate copolymer (MFR = 7.5 g / 10 min, content of structural units derived from ethylene = 94 mass%, content of structural units derived from vinyl acetate = 6 mass%) <Ethylene-vinyl ester copolymer (A)> EVA2: ethylene-vinyl acetate copolymer (MFR = 3.0 g / 10 min, content of structural units derived from ethylene = 90% by mass, content of structural units derived from vinyl acetate = 10% by mass) EVA3: Ethylene-vinyl acetate copolymer (MFR = 1.3 g / 10 min, content of structural units derived from ethylene = 86 mass%, content of structural units derived from vinyl acetate = 14 mass%) EVA4: Ethylene-vinyl acetate copolymer (MFR = 2.5 g / 10 min, content of structural units derived from ethylene = 81 mass%, content of structural units derived from vinyl acetate = 19 mass%) EVA5: Ethylene-vinyl acetate copolymer (MFR = 2.5 g / 10 min, content of structural units derived from ethylene = 75% by mass, content of structural units derived from vinyl acetate = 25% by mass)
[0079] <Ethylene-unsaturated carboxylic acid ester copolymer (B)> EMA1: Ethylene-methyl acrylate copolymer (MFR=6g / 10min, content of structural units derived from ethylene=91% by mass, content of structural units derived from methyl acrylate=9% by mass, produced by tubular high-pressure polymerization method) EMA2: Ethylene-methyl acrylate copolymer (MFR=8g / 10min, content of structural units derived from ethylene=80% by mass, content of structural units derived from methyl acrylate=20% by mass, produced by tubular high-pressure polymerization method) EMA3: Ethylene-methyl acrylate copolymer (MFR=20g / 10min, content of structural units derived from ethylene=76% by mass, content of structural units derived from methyl acrylate=24% by mass, produced by tubular high-pressure polymerization method) EMA4: Ethylene-methyl acrylate copolymer (MFR=18g / 10min, content of structural units derived from ethylene=80% by mass, content of structural units derived from methyl acrylate=20% by mass, produced by autoclave high pressure polymerization)
[0080] <Alicyclic hydrocarbon resin (C1)> Tackifying resin 1: Resin obtained by internally hydrogenating aromatic hydrocarbon resin (Arakawa Chemical Industries, Alcon AM-1, ring and ball softening point = 115°C)
[0081] <Aromatic Hydrocarbon Resin (C2)> Tackifying resin 2: Resin mainly composed of α-methylstyrene (manufactured by Air Brown, SYLVARES SA100, ring and ball softening point = 100°C)
[0082] <Additives> Slip agent: Erucamide (ELA, NOF Corporation)
[0083] [Examples 1 to 9, Comparative Examples 1 to 5] <Preparation of evaluation samples> (1) Preparation of heat-sealable resin composition The components were melt-kneaded at 160° C. in an extruder (65 mmφ, L / D=28, Dulmage flight screw tip) in the blending ratios shown in Table 1 to obtain heat-sealable resin compositions for each of the Examples and Comparative Examples.
[0084] (2) Preparation of packaging materials Using a 40 mmφ single-layer cast molding machine, the above-mentioned various heat-sealable resin compositions were formed into a molten film by extrusion lamination at a processing temperature of 200°C and a processing speed of 25 m / min, and the above-mentioned heat-sealable resin composition was laminated to a thickness of 30 μm on a previously prepared PET (thickness 12 μm) / PE (thickness 15 μm) substrate to obtain a packaging material (1) of PET (thickness 12 μm) / PE (thickness 15 μm) / heat-sealable resin composition layer (thickness 30 μm). The resulting packaging material (1) was subjected to the following evaluations, the results of which are shown in Table 1.
[0085] [Peel strength against silicone-coated APET] The packaging material (1) was heat-sealed onto a 0.4 mm thick silicone-coated APET sheet (hereinafter also referred to as "silicone-coated APET") under conditions of a pressing force of 0.2 MPa, a heating temperature of 180°C, and a heating time of 1.0 second, and left at room temperature for 24 hours. After that, both sides of a 15 mm wide test piece cut out from the packaging material were pulled in opposite directions (180° peeling direction) to determine the maximum stress.
[0086] The peel strength of the packaging material (1) from the silicone-coated APET was evaluated according to the following evaluation criteria: If the evaluation was A, the peel strength from the silicone-coated APET was good, and if the evaluation was B, the peel strength from the silicone-coated APET was poor. -Evaluation criteria- A: Peel strength is 9N / 15mm or more B: Peel strength is less than 9N / 15mm
[0087] [Peel strength against uncoated APET] The packaging material (1) was heat-sealed to a 0.4 mm thick sheet of APET not coated with silicone (hereinafter also referred to as "silicone-uncoated APET") under conditions of a pressing force of 0.2 MPa, a heating temperature of 180°C, and a heating time of 1.0 second, and left at room temperature for 24 hours. After that, both sides of a 15 mm wide test piece cut out from the packaging material were pulled in opposite directions (180° peeling direction) to determine the maximum stress.
[0088] The peel strength of the packaging material (1) from APET not coated with silicone was evaluated according to the following evaluation criteria: If the evaluation was A, the peel strength from APET not coated with silicone was good, and if the evaluation was B, the peel strength from APET not coated with silicone was poor. -Evaluation criteria- A: Peel strength is 9N / 15mm or more B: Peel strength is less than 9N / 15mm
[0089] [Transparency] Using a 40mmφ 3-type 3-layer cast molding machine, co-extruded low-density polyethylene (density = 917kg / m3 A low-density polyethylene (thickness: 22 μm) / heat-sealable resin composition layer (thickness: 8 μm) was laminated on the above-mentioned various heat-sealable resin compositions by air knife cast molding at a processing temperature of 200° C. and a processing speed of 30 m / min to obtain a packaging material (2) having a low-density polyethylene (thickness: 22 μm) / heat-sealable resin composition layer (thickness: 8 μm). The haze (cloudiness, unit: %) of the obtained packaging material (2) was measured in accordance with JIS K 7136: 2000 using a haze meter HM-150 manufactured by Murakami Color Co., Ltd. If the evaluation was A, the transparency of the packaging material (2) was good, and if the evaluation was B, the transparency of the packaging material (2) was poor.
[0090] The transparency of the packaging material (2) was evaluated according to the following evaluation criteria. -Evaluation criteria- A: Haze is less than 6.0% B: Haze is 6.0% or more
[0091] [Table 1]
[0092] As is clear from Table 1, the packaging materials using the heat-sealable resin compositions of Examples 1 to 9 were excellent in peel strength from silicone-coated APET, peel strength from silicone-uncoated APET, and transparency. In contrast, the packaging materials using the heat-sealable resin compositions of Comparative Examples 1 to 5 were poor in at least one of the peel strength from silicone-coated APET, peel strength from silicone-uncoated APET, and transparency. From the above, it was confirmed that the heat-sealable resin composition according to this embodiment can realize a packaging material that is excellent in peel strength from silicone-coated APET, peel strength from silicone-uncoated APET, and transparency.
[0093] The disclosure of Japanese Patent Application No. 2021-044950, filed on March 18, 2021, is incorporated by reference in its entirety into this specification. All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference.
Claims
1. An ethylene-vinyl ester copolymer (A), An ethylene-unsaturated carboxylic acid ester copolymer (B); A tackifier resin (C); Including, the content of structural units derived from vinyl ester contained in the ethylene-vinyl ester copolymer (A) is 8 mass% or more based on all structural units of the copolymer constituting the ethylene-vinyl ester copolymer (A); The tackifier resin (C) contains an alicyclic hydrocarbon resin (C1) and an aromatic hydrocarbon resin (C2), A heat-sealable resin composition having a content of the ethylene-vinyl ester copolymer (A) of 20% by mass or more and 80% by mass or less, when the total mass of the resin components contained in the heat-sealable resin composition is taken as 100% by mass.
2. 2. The heat-sealable resin composition according to claim 1, wherein the content of the tackifier resin (C) is 1% by mass or more and 40% by mass or less, when the total mass of the resin components contained in the heat-sealable resin composition is 100% by mass.
3. 3. The heat-sealable resin composition according to claim 1, wherein the aromatic hydrocarbon resin (C2) has a softening point of 70° C. or higher and 140° C. or lower.
4. 4. The heat-sealable resin composition according to any one of claims 1 to 3, wherein a mass ratio (C2 / (C1+C2)) of a content of the aromatic hydrocarbon resin (C2) to a total content of the alicyclic hydrocarbon resin (C1) and the aromatic hydrocarbon resin (C2) is 0.05 or more and 0.8 or less.
5. The heat-sealable resin composition according to any one of claims 1 to 4, wherein a mass ratio (B / A) of a content of the ethylene-unsaturated carboxylic acid ester copolymer (B) to a content of the ethylene-vinyl ester copolymer (A) is 0.20 or more and 1.0 or less.
6. The heat-sealable resin composition according to any one of claims 1 to 5, which has a haze of less than 6.0% as measured by the following method. (method) Using a 40 mm diameter three-type three-layer cast molding machine, co-extruded low-density polyethylene (density = 917 kg / m 3 A low-density polyethylene (thickness: 22 μm) / heat-sealable resin composition layer (thickness: 8 μm) is laminated on a low-density polyethylene (thickness: 22 μm) / heat-sealable resin composition layer (thickness: 8 μm) at a processing temperature of 200° C. and a processing speed of 30 m / min by cast molding with an air knife at a processing temperature of 200° C. The haze of the obtained packaging material is then measured using a haze meter in accordance with JIS K 7136:2000.
7. A heat-sealing material comprising the heat-sealable resin composition according to any one of claims 1 to 6.
8. A packaging material comprising: a base layer; and a heat seal layer comprising the heat seal material according to claim 7 and provided on one surface of the base layer.
9. A lid material comprising the packaging material according to claim 8.
10. A packaging container comprising: a container body having an opening; and the lid material according to claim 9 for covering the opening of the container body.
11. The packaging container according to claim 10, wherein at least a portion of the container body comprises amorphous polyethylene terephthalate.
12. A container body having an opening, and a lid material for covering the opening of the container body, At least a portion of the container body contains amorphous polyethylene terephthalate, The lid material includes a packaging material including a base material layer and a heat seal layer including a heat seal material provided on one surface of the base material layer, The heat seal material is An ethylene-vinyl ester copolymer (A), An ethylene-unsaturated carboxylic acid ester copolymer (B); A tackifier resin (C); Including, the content of structural units derived from vinyl ester contained in the ethylene-vinyl ester copolymer (A) is 8 mass% or more based on all structural units of the copolymer constituting the ethylene-vinyl ester copolymer (A); The packaging container, wherein the tackifier resin (C) is a heat-sealable material composed of a heat-sealable resin composition containing an alicyclic hydrocarbon resin (C1) and an aromatic hydrocarbon resin (C2).
13. The packaging container according to any one of claims 10 to 12, wherein at least a portion of the container body comprises amorphous polyethylene terephthalate coated with silicone.
Citation Information
Patent Citations
Adhesive material for pocket warmer and disposable pocket warmer provided with the same
JP2001123135A
Floor tile
JP2002294996A
Sealant material, cover tape and package for conveying electronic parts
JP2012188133A
Hot-melt adhesive, and coated material using the same
JP2013018826A
Adhesive, film, and lid material for polyethylene terephthalate-made container
JP2017132851A