Sealed battery

The sealing plate design with an inclined thin wall portion and thicker base portion in sealed batteries ensures stable and efficient pressure relief at low operating pressures, addressing high pressure issues and stress corrosion in existing designs.

JP7607222B2Active Publication Date: 2024-12-27PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022511613
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-01
Filing Date
2021-02-10
Publication Date
2024-12-27
Estimated Expiration
2041-02-10

AI Technical Summary

Technical Problem

Existing sealed batteries face issues with high operating pressures and variations in pressure when the inner peripheral side of the sealing plate is deviated toward the bottom of the battery can, leading to potential stress corrosion cracking and inconsistent explosion-proof function activation.

Method used

The sealing plate design includes an inclined portion with a thin wall portion arranged in the radial direction and a base portion thicker than the thin wall portion, ensuring that tensile stress is applied when internal pressure increases, thereby activating the explosion-proof function at lower pressures and reducing pressure variations.

Benefits of technology

The design achieves a stable explosion-proof function at low operating pressures with minimal variations, preventing swelling and bursting, and reduces the likelihood of stress corrosion cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007607222000004
    Figure 0007607222000004
  • Figure 0007607222000005
    Figure 0007607222000005
  • Figure 0007607222000006
    Figure 0007607222000006
Patent Text Reader

Abstract

This hermetically sealed battery is provided with a battery can in the shape of a bottomed cylinder having an opening, an electrode body accommodated in the battery can, and a sealing plate which blocks the opening in the battery can, wherein: the sealing plate is provided with a flat plate-shaped outer circumferential portion, an inner circumferential portion, and an inclined portion interposed therebetween, and is provided with a first main surface facing the outside of the battery can, and a second main surface on the opposite side to the first main surface; and the inclined portion is inclined in such a way that the inner circumferential portion is disposed further toward the outside of the battery can than the outer circumferential portion, and the inclined portion is provided with a thin-walled portion and a base portion which is thicker than the thin-walled portion, arranged side-by-side in the radial direction of the sealing plate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sealed battery comprising a battery can, an electrode assembly housed in the battery can, and a sealing plate that closes the opening of the battery can. [Background technology]

[0002] In the event of abnormal charging / discharging or misuse such as dropping into a fire, gas may be generated inside a sealed battery, causing the internal pressure to rise. As a safety device in such cases, a sealed battery is usually provided with an explosion-proof valve. When the explosion-proof valve opens, the battery is prevented from exploding or swelling. The explosion-proof valve is, for example, a thin-walled portion formed by pressing a part of a sealing plate that seals the battery can.

[0003] Patent Document 1 teaches that the inner periphery side of the sealing plate is offset toward the bottom of the battery can relative to the outer periphery side, with the thin wall portion as the boundary. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-177877 A Summary of the Invention

[0005] When the inner periphery of the sealing plate is displaced more toward the bottom of the battery can than the outer periphery as in Patent Document 1, the operating pressure becomes higher.

[0006] One aspect of the present invention relates to a sealed battery comprising: a bottomed cylindrical battery can having an opening; an electrode body contained in the battery can; and a sealing plate that closes the opening of the battery can, wherein the sealing plate has a flat outer peripheral portion, an inner peripheral portion, and an inclined portion interposed between them, and also has a first main surface facing an outside of the battery can and a second main surface opposite to the first main surface, the inclined portion is inclined so as to position the inner peripheral portion closer to the outside of the battery can than the outer peripheral portion, and comprises a thin-walled portion aligned in a radial direction of the sealing plate and a base portion that is thicker than the thin-walled portion.

[0007] According to the present invention, it is possible to provide a sealed battery that operates at a low operating pressure and has a small variation in explosion-proof function. [Brief description of the drawings]

[0008] [Figure 1] 1 is a schematic cross-sectional view showing a main part of a sealed battery according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic top view showing a sealing plate according to one embodiment of the present invention. [Diagram 3] 3 is a cross-sectional view of the sealing plate taken along line XX in FIG. 2. [Figure 4A] FIG. 4 is an enlarged schematic cross-sectional view of a main portion of a sealing plate according to another embodiment of the present invention. [Figure 4B] FIG. 13 is an enlarged schematic cross-sectional view of a main portion of a sealing plate according to still another embodiment of the present invention. [Figure 4C] FIG. 13 is an enlarged schematic cross-sectional view of a main portion of a sealing plate according to still another embodiment of the present invention. [Diagram 5] 1 is a schematic cross-sectional view of a main part of a battery according to one embodiment of the present invention. [Figure 6] FIG. 4 is an enlarged schematic cross-sectional view of a main portion of the sealing plate produced in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The sealed battery according to this embodiment (hereinafter, may be simply referred to as the battery) comprises a bottomed cylindrical battery can having an opening, an electrode body housed in the battery can, and a sealing plate that closes the opening of the battery can. The sealing plate has a first main surface facing the outside of the battery can and a second main surface opposite the first main surface. The sealing plate further comprises a flat outer periphery, an inner periphery, and an inclined portion interposed between them. The inclined portion is inclined so that the inner periphery is located closer to the outside of the battery can than the outer periphery. The inclined portion comprises a thin portion aligned in the radial direction of the sealing plate, and a base portion that is thicker than the thin portion.

[0010] When the internal pressure of the battery rises, pressure is applied to the sealing plate in a direction that causes it to bulge outward. This pressure causes the sealing plate to break at the thin part, releasing the internal pressure. This is the explosion-proof function. The explosion-proof function prevents the battery from exploding or swelling.

[0011] When the inner periphery of the sealing plate is recessed as in Patent Document 1, compressive stress acts on the thin-walled portion first, and then tensile stress acts on it. Therefore, the pressure (operating pressure) until the thin-walled portion breaks tends to be large. Furthermore, the thin-walled portion is formed on the entire inclined portion of the sealing plate. Therefore, stress concentration is unlikely to occur, and the operating pressure tends to vary.

[0012] In this embodiment, an inclined portion is provided on the sealing plate to raise the inner periphery. This allows only tensile stress to act on the inclined portion when the internal pressure rises. Therefore, the explosion-proof function can be activated at low internal pressure. Furthermore, the thin-walled portion is provided on a part of the inclined portion. Therefore, the tensile stress is more likely to concentrate on the thin-walled portion. Therefore, the variation in the activation pressure is also suppressed.

[0013] Moreover, the battery of this embodiment can provide high reliability even in an environment where an external load is applied. For example, if the inner periphery of the sealing plate is recessed as in Patent Document 1, tensile stress acts on the thin wall portion due to the external load. If this tensile stress is applied for a long period of time, stress corrosion cracking may occur in the thin wall portion. On the other hand, according to this embodiment, tensile stress does not act on the thin wall portion. Therefore, stress corrosion cracking is unlikely to occur.

[0014] From the viewpoint of preventing scattering of the contents, the operating pressure of the explosion-proof function is desirably 5.5 MPa or less, more desirably 5.3 MPa or less, and particularly desirably 5.0 MPa or less. The operating pressure of the sealed battery according to this embodiment may be within this range.

[0015] (slanted part) The inclined portion is inclined so that the inner periphery is disposed closer to the outside of the battery can than the outer periphery The inclined portion is formed by, for example, pressing.

[0016] The inclination angle of the inclined portion is not particularly limited. For example, the exterior angle A formed by the second main surface of the outer periphery and the second main surface of the inclined portion (hereinafter, sometimes referred to as the inclination angle A) is greater than 0° and less than 90°. The exterior angle formed by the second main surface of the inner periphery and the second main surface of the inclined portion is also greater than 0° and less than 90°.

[0017] In other words, the inclined portion is a region between the point where the angle A between the second main surface at the outer circumferential portion exceeds 0° and the point where the angle A between the second main surface at the inner circumferential portion exceeds 0°. The second main surface at the outer circumferential portion and the second main surface at the inner circumferential portion are approximately parallel to each other.

[0018] In order to facilitate the application of tensile stress to the thin-walled portion, the inclination angle A is preferably 25° or more, and more preferably 30° or more. Similarly, the inclination angle A is preferably 75° or less, more preferably 70° or less, and particularly preferably 65° or less. The inclination angle A is, for example, 25° or more and 75° or less. The inclination angle A is the average value of the inclination angles A measured using three different cross sections (hereinafter referred to as cross sections R) obtained by cutting the sealing plate in the radial direction R.

[0019] The arrangement of the inclined portion is not particularly limited and may be appropriately set depending on the radius of the sealing plate, etc. In a projection view of the sealing plate seen from the normal direction of the first main surface of the inner peripheral portion, the length from the outer edge of the outer peripheral portion to the inner edge of the inner peripheral portion is referred to as the total width W. The inclined portion is arranged, for example, so as to be contained in a region from the outer edge of the outer peripheral portion to 3% of the total width W inside and from the outer edge of the outer peripheral portion to 90% of the total width W, preferably from the outer edge of the outer peripheral portion to 70% of the total width W.

[0020] The width of the inclined portion is not particularly limited and may be appropriately set according to the radius of the sealing plate. The width W3 of the inclined portion may be, for example, 5% to 90% of the total width W, 10% to 50% of the total width W, or 15% to 30% of the total width W. The width W3 of the inclined portion is the average value of the length between the outer edge and the inner edge of the inclined portion measured by drawing straight lines extending in three different radial directions R on the projection diagram. The width W3 of the inclined portion may be calculated by subtracting the width W1 of the outer periphery and the width W2 of the inner periphery from the total width W. The outer edge of the inclined portion is synonymous with the boundary between the outer periphery and the inclined portion. The inner edge of the inclined portion is synonymous with the boundary between the inclined portion and the inner periphery.

[0021] The inclined portion includes a thin portion aligned in the radial direction R of the sealing plate, and a base portion that is thicker than the thin portion. This makes it easier for tensile stress to be concentrated in the thin portion, thereby suppressing variations in operating pressure.

[0022] <Thin-walled section> The thin-walled portion is formed by a groove arranged in an arc shape on a first main surface of the inclined portion facing the outside of the battery can. The groove is formed by recessing the first main surface at a part of the inclined portion by pressing, cutting, or the like. From the viewpoint of improving productivity and easily suppressing variations in operating pressure, it is desirable that no recess or protrusion is formed on the second main surface of the inclined portion and that the second main surface of the inclined portion is flat.

[0023] The press working for forming the inclined portion tends to increase the strength at the boundary between the outer periphery and the inclined portion, and at the boundary between the inclined portion and the inner periphery. Therefore, when the sealing plate has the inclined portion according to this embodiment, when the internal pressure rises, the difference in the deformation amount of the sealing plate between the inner periphery side and the outer periphery side of the boundary becomes large, and as a result, stress concentration occurs in the area sandwiched between both boundaries, i.e., the inclined portion. However, since the outer edge of the sealing plate is fixed to the battery can, the deformation amount of the outer periphery itself is small. Therefore, the difference in the deformation amount at the boundary between the outer periphery and the inclined portion is larger than the difference in the deformation amount at the boundary between the inclined portion and the inner periphery. Therefore, the stress is concentrated more on the outer periphery side of the inclined portion.

[0024] From the above viewpoint, it is preferable that the bottom of the groove is disposed on the outer peripheral side of the inclined portion. Tensile stress is concentrated at the bottom of the groove. When the internal pressure increases, the inclined portion and the inner peripheral portion are pushed up toward the outside starting from the bottom of the groove. On the other hand, the deformation amount of the outer peripheral portion itself is small. Therefore, the sealing plate is quickly broken at the bottom of the groove. At least a part of the bottom of the groove may be in a region from the outer edge of the inclined portion to 50% of the width W3 of the inclined portion.

[0025] In particular, it is preferable that the height h from the second main surface in the outer periphery to the bottom of the groove and the height H from the second main surface in the outer periphery to the first main surface in the inner periphery satisfy the relationship h / H≦45%. When this relationship is satisfied, it can be said that the bottom of the groove is sufficiently close to the boundary between the outer periphery and the inclined portion. It is preferable to satisfy the relationship h / H≦40%, and it is more preferable to satisfy the relationship h / H≦35%.

[0026] The bottom of the groove is the deepest part of the groove. Specifically, it is the point on the first main surface that is closest to the second main surface in the cross section R. When there are multiple points on the first main surface that are closest to the second main surface, the entire straight line connecting the two closest points is the bottom.

[0027] The height h is the height from the second main surface at the outer periphery to the bottom of the groove. If the bottom is linear, the height h is the height from the second main surface at the outer periphery to the midpoint of the bottom.

[0028] The height H is the height from the second main surface at the outer periphery to the point on the first main surface at the inner periphery that is closest to the inclined portion. The heights h and H are the average values ​​of the heights measured using three different cross sections R.

[0029] The arrangement of the entire groove is not particularly limited and may be appropriately set depending on the arrangement of the inclined portion, etc. In order to make it easier for tensile stress to concentrate in the groove, it is preferable that the entire groove is also located on the outer periphery side of the inclined portion. For example, at least a part of the groove may be located in a region from the outer edge of the inclined portion to 50% of its width.

[0030] The cross-sectional shape of the groove is not particularly limited. In the cross section R, the inner wall of the groove has, for example, a bottom portion, and a first side portion and a second side portion that respectively connect the bottom portion and the first main surface. The shape of the bottom portion of the groove may be linear, arc-shaped, or dot-shaped. From the viewpoint of processability, the shape of the bottom portion of the groove may be linear or arc-shaped. The radius of curvature of the arc-shaped bottom portion is not particularly limited, and may be, for example, 0.01 mm or more and 1 mm or less.

[0031] When the bottom is linear, it is desirable that the width of the bottom of the groove is narrow. This is because tensile stress tends to concentrate at the bottom of the groove. For example, it is preferable that the width Wb of the bottom of the groove and the thickness D of the base portion satisfy the relationship Wb / D≦50%. It is preferable that the relationship Wb / D≦40%, and it is preferable that the relationship Wb / D≦30%.

[0032] The width Wb of the bottom of the groove may be, for example, 0.5 mm or less. The width Wb of the bottom of the groove may be, for example, 0.01 mm or more, and may be 0.03 mm or more. When the width Wb of the bottom is 0.01 mm, the cross-sectional shape of the bottom is a point.

[0033] The cross-sectional shape of the groove is the shape of the groove at cross-section R. The width Wb of the bottom of the groove is the average value of the lengths of the first main surface at the bottom of the groove measured using three different cross-sections R. The thickness D of the base portion is the average value of the thicknesses of the base portion measured using three different cross-sections R.

[0034] In order to make it easier for tensile stress to concentrate at the bottom of the groove, it is preferable that the width of the groove is narrower toward the second main surface. In other words, it is preferable that the first side portion and the second side portion are inclined so that the width of the groove increases from the bottom toward the first main surface.

[0035] The angle B between the first side portion and the second side portion (hereinafter, sometimes referred to as the opening angle B) is preferably 30° or more, and more preferably 45° or more. The opening angle B is preferably 120° or less, and more preferably 100° or less. The opening angle B is, for example, 30° or more and 120° or less.

[0036] The opening angle B is the angle between two straight lines respectively connecting two intersections between the inner wall of the groove and the first main surface and the midpoint of the bottom of the groove on the cross section R. The opening angle B is the average value of the opening angles B measured using three different cross sections R.

[0037] The central angle C of the groove (hereinafter, sometimes referred to as the vent angle C) is not particularly limited. The vent angle C is preferably 60° or more. This makes it easier for the sealing plate to be torn open, and the operating pressure is further reduced. Therefore, scattering of the contents is also suppressed. The vent angle C may be 180° or more. The vent angle C may be 360°, less than 360°, or 270° or less. In particular, the vent angle C is preferably 60° or more and 270° or less.

[0038] The bent angle C of the groove is the angle between a line drawn through one circumferential end of the groove in the radial direction R of the sealing plate and a line drawn through the other circumferential end of the groove in the radial direction R of the sealing plate.

[0039] The thickness of the thin-walled portion is not particularly limited. The thickness d of the thin-walled portion may be 5% or more and 30% or less of the thickness D of the base portion. If the thickness of the thin-walled portion is within the above range, it becomes easy to exhibit the explosion-proof function at a low operating pressure while maintaining the strength of the sealing plate. The thickness d of the thin-walled portion may be 7% or more, or may be 10% or more of the thickness D of the base portion. The thickness d of the thin-walled portion may be 25% or less of the thickness D of the base portion.

[0040] The thickness of the thin portion is the shortest distance from the second main surface to the point closest to the thin portion in the cross section R. The thickness d of the thin portion is the average value of the thicknesses of the thin portion measured using three different cross sections.

[0041] <Base section> The base portion is thicker than the thin portion. The thickness D of the base portion is not particularly limited and may be approximately the same as the thickness D1 of the outer periphery portion and / or the thickness D2 of the inner periphery portion. The thickness D is, for example, approximately ±10% of the thickness D1 and / or the thickness D2.

[0042] (Outer periphery) The outer peripheral portion is a flat, doughnut-shaped portion of the sealing plate that surrounds the inclined portion. The width of the outer peripheral portion is not particularly limited and may be set appropriately depending on the radius of the sealing plate, etc. The width of the outer peripheral portion may be, for example, 3% to 80% of the total width W. The thickness D1 of the outer peripheral portion is also not particularly limited. The thickness D1 of the outer peripheral portion is, for example, 0.2 mm to 0.5 mm.

[0043] (Inner circumference) The inner periphery is a donut-shaped portion of the sealing plate surrounded by the inclined portion. The width of the inner periphery is not particularly limited and may be set appropriately depending on the radius of the sealing plate, etc. The width of the inner periphery may be, for example, 10% to 90% of the total width W. The thickness D2 of the inner periphery is also not particularly limited. The thickness D2 of the inner periphery is, for example, 0.2 mm to 0.5 mm.

[0044] The sealed battery according to the present embodiment will be described below with reference to the drawings. However, the present embodiment is not limited thereto. Fig. 1 is a schematic cross-sectional view showing the main part of the sealed battery according to the present embodiment. In the following illustrated examples, the same reference numerals are used for members having the same functions.

[0045] The sealing plate 300 is fixed near the opening of the battery can 100 to close the opening. The sealing plate 300 has a first main surface 300X facing the outside of the battery can and a second main surface 300Y opposite to the first main surface 300X, and is doughnut-shaped with a through hole S (see FIG. 2, etc.) in the center. An external terminal 330 with a crushed tip is fixed to the through hole in the center of the sealing plate 300 via an insulating gasket 310 and a washer 320. An end of an internal lead wire 210 led from a positive electrode or a negative electrode constituting an electrode body is connected to the external terminal 330. Hereinafter, a member constituted by the sealing plate 300, the gasket 310, the washer 320, and the external terminal 330 may be referred to as a sealing body. However, the shapes of the sealing plate 300 and the sealing body are not limited to this.

[0046] The sealing plate 300 has an outer circumferential portion 301, an inner circumferential portion 302, and an inclined portion 303 interposed therebetween. The inclined portion 303 has a thin portion. When the internal pressure of the battery increases, pressure is applied in a direction in which the sealing plate 300 bulges outward. At this time, tensile stress is concentrated in the thin portion. Then, the sealing plate breaks at the thin portion, thereby activating the explosion-proof function and releasing the internal pressure.

[0047] Next, the sealing plate will be specifically described with reference to Fig. 2 and Fig. 3. However, the sealing plate according to this embodiment is not limited thereto. Fig. 2 is a schematic top view showing the sealing plate according to this embodiment. Fig. 3 is a cross-sectional view of the sealing plate of Fig. 2 taken along line XX. In Fig. 2, the inclined portion and the thin portion are hatched for convenience. The line XX is along the radial direction R. In Figs. 2 and 3, the outer edge portion of the sealing plate used for fixing to the battery case is omitted.

[0048] The sealing plate 300 includes an outer peripheral portion 301, an inner peripheral portion 302, and an inclined portion 303 interposed therebetween. A through hole S is formed in the center of the sealing plate 300. The inclined portion is disposed so as to be located inside 3% of the total width W and within a region from the outer edge of the outer peripheral portion 301 to 90% of the total width W. The width W3 of the inclined portion is 5% to 90% of the total width W. The bent angle C is 60° to 270°. The inclination angle A of the inclined portion 303 is 25° to 75°.

[0049] The inclined portion 303 includes thin portions 303a aligned in the radial direction R, and a base portion 303b thicker than the thin portions 303a. The thin portions 303a are formed by grooves arranged in an arc shape on the first main surface 300X of the inclined portion 303.

[0050] The inner wall of the groove includes a bottom portion 3031, a first side portion 3032, and a second side portion 3033. The bottom portion 3031 is an intersection of the two side portions. The thickness d of the bottom portion 3031 is 5% to 30% of the thickness D of the base portion 303b. The thickness D of the base portion 303b is approximately the same as the thickness D1 of the outer circumferential portion 301 and the thickness D2 of the inner circumferential portion 302. The opening angle B between the first side portion 3032 and the second side portion 3033 is approximately 90°.

[0051] A height h from the second main surface 300Y in the outer circumferential portion 301 to the bottom 3031 of the groove and a height H from the second main surface 300Y in the outer circumferential portion 301 to the first main surface 300X in the inner circumferential portion 302 satisfy the relationship h / H≦45%. At least a part of the groove and the bottom 3031 of the groove are in a region from the outer edge of the inclined portion 303 to 50% of its width W3.

[0052] Next, the thin-walled portion will be specifically described with reference to Fig. 4A to Fig. 4C. Fig. 4A to Fig. 4C are schematic cross-sectional views showing enlarged main parts of another sealing plate according to the present embodiment. In Fig. 4A to Fig. 4C, the outer edge portion of the sealing plate used for fixing to the battery case is omitted.

[0053] Sealing plate 300A shown in Fig. 4A has the same configuration as the sealing plate shown in Fig. 3, except that the groove has an arc-shaped bottom 3031. The radius of curvature of bottom 3031 is not less than 0.01 mm and not more than 1 mm.

[0054] 3, except that the groove has a linear bottom 3031. The width Wb of the bottom 3031 and the thickness D of the base portion 303b satisfy the relationship Wb / D≦50%.

[0055] Sealing plate 300C shown in Fig. 4C has the same configuration as the sealing plate shown in Fig. 3, except that the groove is U-shaped. The radius of curvature of bottom 3031 is 0.01 mm or more and 1 mm or less. The opening angle between first side portion 3032 and second side portion 3033 is 30° or more and 120° or less.

[0056] FIG. 5 is a schematic vertical cross-sectional view of an example of a sealed battery.

[0057] The battery 10 includes a cylindrical battery can 100 with a bottom, a cylindrical electrode body 200 housed in the battery can 100, and a sealing plate 300 that closes the opening of the battery can 100. The sealing plate 300 is fixed to the vicinity of the opening of the battery can 100 by, for example, laser welding. The sealing plate 300 may be crimped to the vicinity of the opening of the battery can 100.

[0058] The material of the battery can 100 and the sealing plate 300 is not particularly limited, and examples include iron and / or iron alloys (including stainless steel), aluminum, and aluminum alloys (including alloys containing trace amounts of other metals such as manganese and copper), etc.

[0059] Next, the configuration of the electrode body 200 will be described by way of example using a lithium primary battery.

[0060] The cylindrical electrode body 200 is a wound type, and is constructed by spirally winding a positive electrode 201 and a negative electrode 202 with a separator 203 interposed therebetween. An internal lead wire 210 is connected to one of the positive electrode 201 and the negative electrode 202 (the positive electrode 201 in the illustrated example). The internal lead wire 210 is connected to an external terminal 330 by welding or the like. Another internal lead wire 220 is connected to the other of the positive electrode 201 and the negative electrode 202 (the negative electrode 202 in the illustrated example). The internal lead wire 220 is connected to the inner surface of the battery can 100 by welding or the like.

[0061] The electrode body 200, together with an electrolyte (not shown), is housed inside the battery can 100. To prevent internal short circuits, an upper insulating plate 230A and a lower insulating plate 230B are disposed on the upper and lower parts of the electrode body 200, respectively.

[0062] (positive electrode) The positive electrode includes a positive electrode active material, and manganese dioxide can be used as the positive electrode active material. The positive electrode includes, for example, a positive electrode current collector and a positive electrode mixture layer attached to the positive electrode current collector. The positive electrode mixture layer may include a resin material such as a fluororesin as a binder in addition to the positive electrode active material. The positive electrode mixture layer may include a conductive material such as a carbon material as a conductive material. The positive electrode current collector is, for example, an expanded metal, a net, or a punched metal made of stainless steel.

[0063] (Negative electrode) The negative electrode includes a negative electrode active material, and metallic lithium or a lithium alloy can be used as the negative electrode active material. The metallic lithium or lithium alloy is extruded, for example, into a long sheet shape and used as the negative electrode. As the lithium alloy, an alloy such as Li-Al, Li-Sn, Li-Ni-Si, or Li-Pb is used, and Li-Al alloy is preferable. The content of metal elements other than lithium contained in the lithium alloy is preferably 0.1% by mass or more and 5% by mass or less from the viewpoint of ensuring discharge capacity and stabilizing internal resistance.

[0064] (Separator) As the separator, a resin microporous film or nonwoven fabric is preferably used. As the material (resin) of the separator, polyolefin, polyamide, polyamideimide, etc. are preferable.

[0065] (electrolyte) The electrolyte may be a non-aqueous solvent in which a lithium salt is dissolved. The non-aqueous solvent is not particularly limited, but may be propylene carbonate, ethylene carbonate, 1,2-dimethoxyethane, γ-butyrolactone, or the like. The lithium salt may be lithium borofluoride, lithium hexafluorophosphate, lithium trifluoromethanesulfonate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, or the like.

[0066] The present invention will be specifically described below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0067] Example 1 (1) Creation of the sealing body A sealing plate (diameter 17 mm) was prepared.

[0068] A sealing plate (made of SUS316L) was pressed to form an inclined portion as shown in Fig. 2 and a groove (thin portion) having a cross-sectional shape as shown in Fig. 3. The inclined portion was formed so as to be contained in an area that was 33% of the total width W from the outer edge of the outer periphery and 54% of the total width W from the outer edge of the outer periphery. The width W3 of the inclined portion was 22% of the total width W. The inclination angle A was 45°.

[0069] The grooves were formed so that the ratio of height h to height H was h / H = 31%. The bottom of the groove was dot-like. The bent angle C of the groove was 270°. The opening angle B between the side portions of the groove was 90°. The width Wb of the bottom of the groove was 0.01 mm.

[0070] The thickness D1 of the outer periphery, the thickness D2 of the inner periphery and the thickness D of the base are all 0.2 mm. The thickness d of the thin portion is 0.05 mm.

[0071] A through hole with a diameter of about 3 mm was formed in the center of the sealing plate, and an external terminal was fixed into the through hole via an insulating gasket and washer to obtain a sealing body.

[0072] (2) Preparation of the positive electrode 92 parts by mass of electrolytic manganese dioxide as the positive electrode active material was mixed with 3.5 parts by mass of Ketjen black as the conductive agent, 4.5 parts by mass of polytetrafluoroethylene as the binder, and an appropriate amount of pure water to prepare a wet positive electrode mixture.

[0073] Next, the wet positive electrode mixture was applied to a positive electrode current collector made of stainless steel expanded metal to prepare a positive electrode precursor, which was then dried, rolled by a roll press, and cut to a predetermined size to obtain a strip-shaped positive electrode.

[0074] (3) Preparation of the negative electrode A sheet-like Li-Al alloy (Al content: 0.3 mass %) was cut to a predetermined size to obtain a strip-like negative electrode.

[0075] (4) Preparation of electrode groups The positive electrode mixture was peeled off from a part of the positive electrode to expose the positive electrode current collector, and a stainless steel positive electrode tab lead was welded to the exposed part. A nickel negative electrode tab lead was welded to a predetermined part of the negative electrode. The positive electrode and the negative electrode were wound in a spiral shape with a separator interposed between them to form a columnar electrode group. A polyethylene microporous film was used as the separator.

[0076] (5) Preparation of electrolyte The electrolyte was prepared by dissolving lithium trifluoromethanesulfonate as a lithium salt at a concentration of 0.5 mol / L in a non-aqueous solvent made by mixing propylene carbonate (PC), ethylene carbonate (EC), and 1,2-dimethoxyethane (DME) in a volume ratio of 2:1:2.

[0077] (6) Assembling cylindrical batteries The electrode group was inserted into a cylindrical battery can (made of SUS316L) with a bottom, with a ring-shaped lower insulating plate disposed at the bottom of the electrode group. The negative electrode tab lead was welded to the inner bottom surface of the battery can, and a ring-shaped upper insulating plate was disposed on the top of the electrode group, and then the positive electrode tab lead was welded to an external terminal fixed to a sealing plate. Next, an electrolyte was poured into the battery can, and then the sealing plate was laser welded near the opening of the battery can. In this way, 10 sealed cylindrical lithium batteries having the structure shown in FIG. 4 were produced. Separately, 10 sealed evaluation batteries were produced for operating pressure evaluation in the same manner, except that the electrode group and electrolyte were not contained.

[0078] [Working pressure evaluation] A hole was drilled in the side of the battery can of the evaluation battery, water was supplied through it, and the water pressure increased the pressure inside the battery, activating the explosion-proof function.

[0079] The average value (n=10), standard deviation (σ), and average value + 6σ of the operating pressure were calculated. The results are shown in Table 1. When the standard deviation is 0.22 or less, preferably 0.20 or less, more preferably 0.15 or less, and the average value + 6σ is 6.5 MPa or less, it can be said that the operating pressure is low and its variation is small.

[0080] Comparative Example 1 In the production of the sealing body (1), a slanted portion was formed to recess the inner periphery into the battery can, and a strip-shaped thin portion having a constant thickness was formed on the entire slanted portion, except that a sealing plate was produced in the same manner as in Example 1. The slanted angle was 45°. The width Wb of the bottom of the groove (width of the thin portion) was 0.37 mm.

[0081] 6 is an enlarged schematic cross-sectional view of a main portion of the sealing plate produced in Comparative Example 1. Thin portion 1303a is formed in a strip shape. The width of bottom 13031 of thin portion 1303a is the same as the width of inclined portion 1303. First and second side portions 13032, 13033 are approximately parallel to each other.

[0082] Using the obtained sealing plate, ten cylindrical lithium batteries and ten evaluation batteries were produced and evaluated in the same manner as in Example 1. The results are shown in Table 1. Since the tilt direction was opposite to that of Example 1, in Table 1 the tilt angle A is shown as -45°.

[0083] Comparative Example 2 In the production of the sealing body (1), except that the inclination angle A was set to 0°, a sealing plate was produced in the same manner as in Comparative Example 1. The width Wb of the bottom of the groove (width of the thin portion) was set to 0.72 mm.

[0084] Comparative Example 3 In the preparation of the sealing body (1), a sealing plate was prepared in the same manner as in Comparative Example 1, except that the direction of inclination was the same as in Example 1. The inclination angle A was 25°. The width Wb (width of the thin portion) of the bottom of the groove was 0.61 mm. Using the obtained sealing plate, 10 cylindrical lithium batteries and 10 evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 1.

[0085] Comparative Example 4 A sealing plate was prepared in the same manner as in Comparative Example 3, except that in the preparation of the sealing body (1), the inclination angle A was set to 45° and the width Wb (width of the thin portion) of the bottom of the groove was set to 0.36 mm. Using the obtained sealing plate, 10 cylindrical lithium batteries and 10 evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 1.

[0086] [Table 1]

[0087] In Example 1, the average value of the working pressure is 5 MPa or less, the standard deviation is 0.15 or less, and the average value + 6σ is 6.5 MPa or less. Therefore, the working pressure is low and its variation is small. On the other hand, in Comparative Examples 1 to 4, the average value of the working pressure, σ, and the average value + 6σ are all high. In particular, it can be seen that the average value + 6σ is large and the variation is large.

[0088] Example 2 A sealing plate was prepared in the same manner as in Example 1, except that in the preparation of the sealing body (1), the inclination angle A was set to 15°. Using the obtained sealing plate, ten cylindrical lithium batteries and ten evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 2.

[0089] Example 3 A sealing plate was prepared in the same manner as in Example 1, except that in the preparation of the sealing body (1), the inclination angle A was set to 25°. Using the obtained sealing plate, 10 cylindrical lithium batteries and 10 evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 2.

[0090] Example 4 A sealing plate was prepared in the same manner as in Example 1, except that in the preparation of the sealing body (1), the inclination angle A was set to 35°. Using the obtained sealing plate, ten cylindrical lithium batteries and ten evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 2.

[0091] Example 5 A sealing plate was prepared in the same manner as in Example 1, except that in the preparation of the sealing body (1), the inclination angle A was set to 55°. Using the obtained sealing plate, ten cylindrical lithium batteries and ten evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 2.

[0092] Example 6 A sealing plate was prepared in the same manner as in Example 1, except that in the preparation of the sealing body (1), the inclination angle A was set to 65°. Using the obtained sealing plate, ten cylindrical lithium batteries and ten evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 2.

[0093] Example 7 A sealing plate was prepared in the same manner as in Example 1, except that in the preparation of the sealing body (1), the inclination angle A was set to 75°. Using the obtained sealing plate, ten cylindrical lithium batteries and ten evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 2.

[0094] Example 8 A sealing plate was prepared in the same manner as in Example 1, except that in the preparation of the sealing body (1), the inclination angle A was set to 85°. Using the obtained sealing plate, ten cylindrical lithium batteries and ten evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 2.

[0095] Comparative Example 5 A sealing plate was prepared in the same manner as in Example 1, except that in the preparation of the sealing body (1), the inclination angle A was set to 0°. Using the obtained sealing plate, 10 cylindrical lithium batteries and 10 evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 2.

[0096] [Table 2]

[0097] In Examples 1 to 8, the average value of the working pressure is 5.5 MPa or less, the standard deviation is 0.20 or less, and the average value + 6σ is 6.5 MPa or less. In particular, the standard deviation is small in Examples 1 and 3 to 7, and the variation in the working pressure is effectively suppressed. On the other hand, in Comparative Example 5, the average value + 6σ exceeds 6.5 MPa.

[0098] Example 9 In the preparation of the sealing body (1), except that the position of the groove was changed so that h / H was 25%, a sealing plate was prepared in the same manner as in Example 1. Using the obtained sealing plate, 10 cylindrical lithium batteries and 10 evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 3.

[0099] Example 10 In the preparation of the sealing body (1), except that the position of the groove was changed so that h / H was 44%, a sealing plate was prepared in the same manner as in Example 1. Using the obtained sealing plate, 10 cylindrical lithium batteries and 10 evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 3.

[0100] Example 11 In the preparation of the sealing body (1), except that the position of the groove was changed so that h / H was 56%, a sealing plate was prepared in the same manner as in Example 1. Using the obtained sealing plate, 10 cylindrical lithium batteries and 10 evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 3.

[0101] Example 12 In the preparation of the sealing body (1), except that the position of the groove was changed so that h / H was 69%, a sealing plate was prepared in the same manner as in Example 1. Using the obtained sealing plate, 10 cylindrical lithium batteries and 10 evaluation batteries were prepared in the same manner as in Example 1, and evaluated. The results are shown in Table 3.

[0102] [Table 3]

[0103] In Examples 1, 9, and 12, the average value of the working pressure is 5.5 MPa or less, the standard deviation is 0.21 or less, and the average value +6σ is 6.5 MPa or less. In particular, the average value +6σ in Examples 1, 9, and 10 is small, and the variation in the working pressure is effectively suppressed. [Industrial Applicability]

[0104] The sealed battery according to the present invention exhibits stable explosion-proof function and is therefore suitable as a power source for various electronic devices. [Explanation of symbols]

[0105] 10:Battery 100: Battery can 200: Electrode body 201: Positive electrode 202:Negative electrode 203: Separator 210, 220: Internal lead wire 230A: Upper insulating plate 230B: Lower insulating plate 300, 300A, 300B, 300C: Sealing plate 300X: 1st main surface 300Y: Second main surface 301: Outer periphery 302: Inner circumference 303: Inclined part 303a: Thin wall part 3031: Bottom 3032:First side part 3033:Second side part 303b: Base section 310: Gasket 320: Washer 330: External terminal 1303: Inclined section (thin section) 13031: Bottom 13032:First side part 13033:Second side part

Claims

1. a cylindrical battery can having an opening and a bottom; An electrode assembly accommodated in the battery can; a sealing plate that closes the opening of the battery can, the sealing plate has a flat outer peripheral portion, an inner peripheral portion, and an inclined portion interposed therebetween, and also has a first main surface facing an outside of the battery can and a second main surface opposite to the first main surface, The inclined portion is inclined so that the inner peripheral portion is positioned outside the battery can relative to the outer peripheral portion, and the sealed battery has a thin-walled portion aligned in the radial direction of the sealing plate and a base portion thicker than the thin-walled portion.

2. The sealed battery according to claim 1 , wherein the thin portion is formed by a groove arranged in an arc shape on the first main surface of the inclined portion.

3. 3. The sealed battery according to claim 2, wherein a height h from the second main surface in the outer circumferential portion to a bottom of the groove and a height H from the second main surface in the outer circumferential portion to the first main surface in the inner circumferential portion satisfy a relationship of h / H≦45%.

4. 4. The sealed battery according to claim 2, wherein a width Wb of the bottom of the groove and a thickness D of the base portion satisfy a relationship of Wb / D≦50%.

5. 5. The sealed battery according to claim 2, wherein a central angle C of the groove is equal to or greater than 60° and equal to or less than 270°.

6. an inner wall of the groove includes a bottom portion, and a first side portion and a second side portion respectively connecting the bottom portion and the first main surface; The sealed battery according to any one of claims 2 to 5, wherein the first side portion and the second side portion are inclined so that the width of the groove increases from the bottom portion toward the first main surface.

7. The sealed battery according to claim 6 , wherein an angle B between the first side surface portion and the second side surface portion is equal to or greater than 30° and equal to or less than 120°.

8. 8. The sealed battery according to claim 1, wherein an exterior angle A formed between the second main surface at the outer circumferential portion and the second main surface at the inclined portion is 25° or more and 75° or less.

Citation Information

Patent Citations

  • Sealing plate for cylindrical battery and cylindrical battery

    JP2016177877A

  • Sealed battery

    JP2020047536A

  • Secondary battery

    KR1020160149861A

  • Cylindrical hermetically sealed battery

    WO2015146077A1