Method for stabilizing ion exchange resins

By washing virgin ion exchange resin materials with nonionic detergents or alcoholic solvents and rinsing with deoxygenated water, followed by storage in gas-impermeable containers, the method effectively stabilizes the resin, reducing oxidative degradation and organic contaminant release.

JP7656426B2Active Publication Date: 2025-04-03EVOQUA WATER TECHNOLOGIES LLC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020539717
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-02-12
Filing Date
2019-02-12
Publication Date
2025-04-03
Estimated Expiration
2039-02-12

AI Technical Summary

Technical Problem

Virgin ion exchange resin materials are prone to oxidative degradation during handling, storage, and transport, leading to reduced stability and increased release of organic contaminants.

Method used

The method involves washing the virgin ion exchange resin material with a preparation containing a nonionic detergent or an alcoholic solvent at concentrations below their critical micelle concentrations, followed by rinsing with deoxygenated water and sealing it in a gas-impermeable container to minimize exposure to oxygen.

Benefits of technology

This approach significantly reduces the rate of oxidative degradation, maintaining the stability of the ion exchange resin and minimizing the release of organic contaminants, thereby extending its usability and reducing wastewater production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007656426000004
    Figure 0007656426000004
  • Figure 0007656426000005
    Figure 0007656426000005
  • Figure 0007656426000006
    Figure 0007656426000006
Patent Text Reader

Abstract

A method for stabilizing virgin ion exchange resin material is provided. The method includes washing the virgin ion exchange resin material with a formulation comprising a non-ionic detergent. The method includes washing the virgin ion exchange resin material with a formulation comprising an alcohol solvent. The method includes rinsing the virgin ion exchange resin material with deoxygenated water. The method includes introducing the washed / rinsed virgin ion exchange resin material into a gas-impermeable container and sealing the container. The method includes introducing an oxygen-removing material into the gas-impermeable container and sealing the container. Also disclosed is a method for facilitating water treatment at a location where it is needed by providing the washed virgin ion exchange resin material in deoxygenated water.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Aspects and embodiments disclosed herein relate to the stabilization of virgin ion exchange resin material. More specifically, the disclosed aspects and embodiments relate to methods for reducing the rate of oxidative degradation of virgin ion exchange resin material. The disclosed aspects and embodiments relate to the handling, storage, and transportation of stabilized virgin ion exchange resin material. Summary of the Invention

[0002] According to one aspect, a method of stabilizing virgin ion exchange resin material is provided. The method may include washing the virgin ion exchange resin material with a formulation comprising a non-ionic detergent to produce a washed virgin ion exchange resin material. The formulation may comprise the non-ionic detergent at a concentration less than the critical micelle concentration (CMC) of the non-ionic detergent. The method may include introducing the virgin ion exchange resin material into a gas impermeable container. The method may include sealing the container.

[0003] In some embodiments, the method may further include rinsing the washed virgin ion exchange resin material with deoxygenated water.

[0004] The non-ionic detergent may comprise at least one of ethoxylated octylphenol, polysorbate, polyoxyethylene and metabolites thereof.

[0005] According to certain embodiments, the preparation may comprise less than about 0.125 g / L of ethoxylated octylphenol.

[0006] The method may include introducing the washed virgin ion exchange resin material into a liquid impermeable container of a gas impermeable container.

[0007] In another aspect, a method of stabilizing virgin ion exchange resin material is provided. The method can include washing the virgin ion exchange resin material with a preparation comprising an alcohol solvent to produce a washed virgin ion exchange resin material. The method can include introducing the washed virgin ion exchange resin material into a gas impermeable container. The method can include sealing the container.

[0008] In some embodiments, the method may further include rinsing the washed virgin ion exchange resin material with deoxygenated water.

[0009] According to certain embodiments, the alcohol solvent may comprise at least one of isopropanol, methanol, ethanol, n-butanol, isooctanol, methyl isobutyl carbinol, isoamyl alcohol, isobutyl alcohol, cyclohexanol, methyl cyclohexanol, and aqueous ammonia.

[0010] The preparation may comprise less than about 0.5% isopropanol.

[0011] In some embodiments, the method may include introducing the washed virgin ion exchange resin into a liquid impermeable vessel of a gas impermeable vessel.

[0012] According to another aspect, a method of stabilizing virgin ion exchange resin material is provided. The method may include washing the virgin ion exchange resin material with a formulation comprising a non-ionic detergent to produce a washed virgin ion exchange resin material. The formulation may comprise the non-ionic detergent at a concentration below the critical micelle concentration of the non-ionic detergent. The method may include rinsing the washed virgin ion exchange resin material with deoxygenated water to produce a rinsed virgin ion exchange resin material.

[0013] The method may include rinsing the washed ion exchange resin material with deoxygenated water having a dissolved oxygen concentration of less than about 10 ppb.

[0014] In some embodiments, the non-ionic detergent may comprise at least one of ethoxylated octylphenol, polysorbate, polyoxyethylene, and metabolites thereof.

[0015] The method may further include introducing the rinsed virgin ion exchange resin material into a gas impermeable container and sealing the container.

[0016] According to another aspect, a method of stabilizing virgin ion exchange resin material is provided. The method may include washing the virgin ion exchange resin material with a formulation comprising an alcohol solvent to produce a washed virgin ion exchange resin material. The method may include rinsing the washed virgin ion exchange resin material with deoxygenated water to produce a rinsed virgin ion exchange resin material.

[0017] In some embodiments, the method may include rinsing the washed ion exchange resin material with deoxygenated water having a dissolved oxygen concentration of less than about 10 ppb.

[0018] The alcohol solvent may comprise at least one of isopropanol, methanol, ethanol, n-butanol, isooctanol, methyl isobutyl carbinol, isoamyl alcohol, isobutyl alcohol, cyclohexanol, methyl cyclohexanol, and aqueous ammonia.

[0019] The method may further include introducing the rinsed virgin ion exchange resin material into a gas impermeable container and sealing the container.

[0020] According to another aspect, a method for facilitating water treatment is provided at a location in need thereof. The method may include providing a washed virgin ion exchange resin material in deoxygenated water. The washed virgin ion exchange resin material may be a polystyrene-based ion exchange resin material. The washed virgin ion exchange resin material may have less than about 25 ppb of oxygen-containing total organic carbon species.

[0021] In some embodiments, the method may further include providing the washed virgin ion exchange resin material and deoxygenated water in a liquid impermeable compartment of the sealed gas impermeable container.

[0022] The method may further include providing an oxygen scavenging material disposed between an outer wall of the liquid impermeable compartment and an inner wall of the gas impermeable container.

[0023] In some embodiments, the method may further include providing an indication of oxygen contamination.

[0024] The method can include providing deoxygenated water in an amount of about 40% to about 50% of the washed virgin ion exchange resin material.

[0025] The method can include providing deoxygenated water having less than about 10 ppb of dissolved oxygen. [Brief description of the drawings]

[0026] The accompanying drawings are not intended to be drawn to scale. In the drawings, each identical or nearly identical component that is illustrated in various figures is represented by a like numeral. For clarity, not every component is indexed in every drawing. Shown in the drawings are:

[0027] [Figure 1] FIG. 1 is a schematic diagram of a container according to an embodiment disclosed herein. [Diagram 2] FIG. 1 is a schematic diagram of a system including a container according to an embodiment disclosed herein. [Diagram 3] FIG. 1 is a schematic diagram of a container according to an embodiment disclosed herein. [Figure 4] 1 is a graph of the comparative amount of oxygen-containing total organic carbon on an ion exchange resin after washing with various detergents according to one embodiment disclosed herein. [Figure 5A] 1 is a graph of the concentration of oxygen-containing total organic carbon on an ion exchange resin after washing with various concentrations of percarbonate. [Figure 5B] 1 is a graph of the concentration of oxygen-containing total organic carbon on an ion exchange resin after washing with various concentrations of isopropanol. [Figure 5C] 1 is a graph of the concentration of oxygen-containing total organic carbon on an ion exchange resin after washing with various concentrations of ethoxylated octylphenol. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Ion exchange resins may generally be used to separate components contained in liquid mixtures. Conventional ion exchange resins may be prepared by functionalizing a copolymer matrix with groups having cationic and anionic sites. Anions or cations may be able to exchange or associate with ions or molecules in the liquid having the same charge when the resin is in contact with the liquid mixture. The ions are exchanged stoichiometrically to maintain the electrical neutrality of the system. Resins that exchange one cation (or a proportional amount based on valence), such as hydrogen, for another cation, such as copper, iron, sodium, etc., are cationic resins. Resins that exchange one anion (or a proportional amount based on valence), such as hydroxide, for another anion, such as chloride, sulfate, chromate, etc., are anionic resins. Often, both types of resins are used to remove various salts, such as sodium chloride and calcium sulfate, from solutions. Mixed bed ion exchange resins include a combination of cationic and anionic resins, providing treated water of higher purity. The resins may be used until the removed ions are saturated. Many resins may also be regenerated and reused. For example, resins used in water treatment can be regenerated using a strong acid (in the case of a cationic resin) or a strong base (in the case of anionic resins).

[0029] Ion exchange is often used in water treatment, where ions in an aqueous solution are converted to hydrogen (H) that is usually attached to a substrate, e.g. an ion exchange resin. + ) or hydroxide (OH -) ions. This is sometimes called "water desalination" or "water deionization." Ion exchange resins can be commonly used, for example, in water purification, nuclear power generation, microelectronics manufacturing, semiconductor manufacturing, food processing, pharmaceutical manufacturing, chemical processing, and metal extraction.

[0030] Under certain conditions, ion exchange resins may undergo oxidative degradation of the copolymer matrix over an extended period of time. For example, during purification of a liquid mixture, the liquid mixture placed in contact with the resin may contain oxidizing species such as molecular oxygen, dissolved oxygen, dissolved chlorine, or may be at elevated temperatures. Each of these may promote undesirable degradation of the copolymer matrix. In some cases, ion exchange resins may undergo oxidative degradation during handling, storage, or transportation prior to use. For example, water or air in contact with the ion exchange resin prior to use may also promote degradation of the copolymer matrix.

[0031] Specifically, it is believed that during oxidative degradation, carbon-carbon bonds are broken, destroying cross-links between individual polymer chains and / or bonds between individual styrene moieties. As used herein, "oxidative degradation" of an ion exchange resin material refers to the loss of carbon-carbon bonds of cross-links between individual polymer chains or styrene moieties of the copolymer matrix of the material. Without wishing to be bound by a particular theory, it is believed that such loss of bonds can cause an increase in water-holding capacity and, ultimately, the release of organic contaminants, such as functionalized linear polystyrene segments. Oxidative degradation of a copolymer matrix may be undesirable for commercial operation of an ion exchange or chromatography process. For example, a resin that loses cross-links may become relatively soft and may swell and become larger. The increased softness and swelling of the resin as a result of oxidative degradation may ultimately cause one or more of an increase in bed pressure drop, a decrease in the flow rate of the liquid mixture being treated, and a decrease in the operational ability to remove chemical species from the liquid being treated.

[0032] Additionally, loss of crosslinking in the copolymer matrix increases the release of organic contaminants into the column effluent, which may be unacceptable in some applications, such as the nuclear power industry. For example, organic contaminants from degraded ion exchange resins can create potential sources of corrosion in process equipment and can contaminate other ion exchange resins associated with the process. Ionic contaminants can also arise from degraded ion exchange resins. For example, in an exemplary treatment process, a cation exchange resin may contain sulfonic acid charges anchored on a styrene backbone. The sulfonic acid is negatively charged. A positively charged ion, such as sodium or calcium, can be exchanged for another ion, e.g., a hydrogen ion (H+), from the ion exchange resin, such that the sodium or calcium is removed from the liquid being treated. However, in some instances, the resin may degrade to such an extent that sulfate ions leach out of the cation exchange resin. The leached sulfate ions can adversely affect the water quality of the treated water.

[0033] Previously, industry personnel have attempted to improve the oxidative degradation and associated problems of ion exchange resins by increasing the amount of crosslinking monomer used in the preparation of the copolymer matrix. However, increasing the number of crosslinks generally reduces the compatibility of the resulting resin beads with liquid mixtures, thereby resulting in reduced diffusion into the beads and poor operation capabilities. Highly crosslinked resins may exhibit poor regeneration efficiency and be impermeable to large molecules such as glucose, fructose, and other sugars. Furthermore, increasing the crosslink density may not address issues associated with the release of organic contaminants, as degradation still occurs.

[0034] Others in the industry have attempted to improve the oxidative degradation of ion exchange resins by replacing the hydrogen on the tertiary carbon adjacent to the benzene ring of the styrene moiety with halogens. Briefly, as envisioned in U.S. Pat. No. 3,342,755, which is incorporated by reference in its entirety for all purposes, a possible mechanism for degradation of the copolymer matrix is ​​related to a "weak link" defined by the tertiary carbon adjacent to the benzene ring of the styrene moiety. The tertiary carbon is considered a weak link because its attached hydrogen has a tendency to form hydroperoxides with oxidizing agents such as molecular oxygen and chlorine. The hydroperoxides can ultimately lead to the scission of the carbon chain associated with the copolymer. In U.S. Pat. No. 3,342,755, the inventors attempted to improve degradation by using monomers such as orthochlorostyrene that do not contribute to the stability of the resin.

[0035] When degradation of ion exchange resins occurs, conventionally, attempts may be made to flush the degradation products from the ion exchange resins, as long as the resin's performance is not compromised. If rinsed with standard rinse water (non-deoxygenated water), the ion exchange resins may continue to undergo oxidative degradation and / or contamination. Polymer fragments and impurities remaining from the polymerization and activation steps in the manufacture of ion exchange resins may become entangled and slowly leach out of the resin. These must also be flushed away to levels acceptable for the particular industrial application. Furthermore, in certain instances, rinsing ion exchange resins generates large amounts of waste. For example, in the nuclear industry, rinsing ion exchange resins may generate large amounts of waste and / or radioactive wastewater that is complex to treat. Virgin ion exchange resins must be left offline to stabilize before use.

[0036] Ion exchange resins may be stabilized and oxidative degradation of the ion exchange resins may be prevented by limiting exposure of the resins to oxidizing agents such as molecular oxygen, dissolved oxygen, and chlorine. Conventionally, ion exchange resins are often stored in moist containers before being used to treat liquids. The inventors have recognized that ion exchange resins may be stabilized prior to use by preventing exposure of the ion exchange resins to oxygen and / or chlorine dissolved in standard rinse water, limiting the rate of oxidative degradation of the resins. Additionally, conventional ion exchange resin storage containers may generally allow air ingress into the container, which may cause a rapid rate of oxidative degradation of the ion exchange resins. The inventors have recognized that ion exchange resins may be further stabilized by preventing contact with oxygen, e.g., from the ambient air, further limiting oxidative degradation of the ion exchange resins. Stabilization allows the ion exchange resins to remain usable for a predetermined period of time off-line compared to ion exchange resins that are conventionally stored prior to use. The methods disclosed herein may also reduce the amount of wastewater generated during rinsing.

[0037] Analysis was performed on polystyrene-based resins to determine several contaminants released by the oxidative degradation of the resin. Some of the contaminants identified included 5-methyl-3-hexanone, methoxyphenyloxime, benzaldehyde, acetophenone, 2-methylbenzaldehyde, benzenemethanimine, and tributylamine. Without wishing to be bound by a particular theory, it is believed that at least some of these contaminants arise from the oxidation of styrene and orthoxylene moieties present from the manufacture of the resin.

[0038] [ka]

[0039] Such contaminants may have varying degrees of water solubility. For example, acetophenone, benzaldehyde, and 2-methylbenzaldehyde have water solubility of 5.5 g / L, 3.0 g / L, and 1.2 g / L, respectively. Contaminants with high water solubility can generally be washed away with water. However, contaminants with lower water solubility may not be able to be washed away with water or may only be partially washed away with water.

[0040] Aspects and embodiments disclosed herein relate to the stabilization of virgin ion exchange resin materials. In some embodiments, stabilization of an ion exchange resin may refer to maintaining the stability of the ion exchange resin over time, for example, during handling, storage, and / or transportation. Stabilization and maintained stability may relate to a reduction in the rate of oxidative degradation of the virgin ion exchange resin material. Specifically as used herein, a "stabilized" ion exchange resin material may refer to an ion exchange resin material that has a reduced rate of oxidative degradation over a period of time.

[0041] Systems and methods for stabilizing virgin ion exchange resin material are disclosed. The method of stabilizing ion exchange resin may include rinsing the virgin ion exchange resin material with deionized water to produce a rinsed virgin ion exchange resin material. The method of stabilizing ion exchange resin may include introducing the rinsed virgin ion exchange resin material into a gas impermeable container. The method of stabilizing virgin ion exchange resin material may include sealing the gas impermeable container.

[0042] In some embodiments, a method of stabilizing an ion exchange resin may include rinsing a virgin ion exchange resin material with deoxygenated water having a dissolved oxygen concentration of less than about 10 ppb. A method of stabilizing an ion exchange resin may include rinsing a virgin ion exchange resin material with deoxygenated water having a dissolved oxygen concentration of about 1 ppb. A method of stabilizing an ion exchange resin may include rinsing a virgin ion exchange resin material with deoxygenated water having a chlorine concentration of less than about 10 ppb. A method of stabilizing an ion exchange resin may include rinsing a virgin ion exchange resin material with deoxygenated water having a chlorine concentration of about 1 ppb.

[0043] In certain embodiments, the methods disclosed herein may include rinsing the virgin ion exchange resin material by introducing deoxygenated water into a gas impermeable container having the virgin ion exchange resin material and removing the interstitial deoxygenated water from the container. Rinsing with non-deoxygenated deionized water may be an improvement over not rinsing immediately prior to using the water at the consumer's site. A pre-rinse may be designed to remove residual polymer and organic compound debris that may be entangled in the resin. Deoxygenating the deionized water minimizes the generation of oxygen in the deionized rinse water, which may degrade the resin itself. This may generally be responsible for organic (measured by total organic carbon - TOC) impurity levels from the ion exchange resin.

[0044] In some embodiments, the methods disclosed herein may include maintaining a moisture content in the rinsed virgin ion exchange resin material. Maintaining the moisture content may be associated with cross-linking of polymers necessary for resin function, minimizing leaching of organic compounds, and increasing physical strength. For example, in some embodiments, the methods may include maintaining a moisture content of at least about 40% in the rinsed virgin ion exchange resin material. In some embodiments, the methods may include maintaining a moisture content of about 50% in the rinsed virgin ion exchange resin material. In some embodiments, the methods may include maintaining a moisture content of about 40% to about 50% in the rinsed virgin ion exchange resin material.

[0045] According to certain embodiments, the methods disclosed herein may further include producing deoxygenated water. For example, the deoxygenated water may be produced by deoxygenating non-deoxygenated water. The non-deoxygenated water may be deoxygenated by a process to remove dissolved oxygen. In some embodiments, the non-deoxygenated water may be deoxygenated by passing through a deoxygenating membrane. In some embodiments, the non-deoxygenated water may be deoxygenated by subjecting the non-deoxygenated water to vacuum degassing.

[0046] In some embodiments, the methods disclosed herein may include rinsing the virgin ion exchange resin material with deoxygenated water having a concentration of dissolved oxygen effective to reduce a rate of oxidative degradation of the virgin ion exchange resin material. For example, the rate of oxidative degradation may be reduced such that a first volume of water treated by the virgin ion exchange resin material comprises less than about 10 ppb total organic carbon. In some embodiments, after maintaining the virgin ion exchange resin material in a vessel for a predetermined period of time, the rate of oxidative degradation may be reduced such that a first volume of water treated by the virgin ion exchange resin material comprises less than about 10 ppb total organic carbon.

[0047] In some embodiments, the rate of oxidative degradation may be reduced such that the first volume of water treated by the virgin ion exchange resin material comprises less than about 10 ppb sulfate. In some embodiments, the rate of oxidative degradation may be reduced such that the first volume of water treated by the virgin ion exchange resin material comprises less than about 10 ppb chloride. After maintaining the virgin ion exchange resin material in the vessel for a predetermined period of time, the rate of oxidative degradation may be reduced such that the first volume of water treated by the virgin ion exchange resin material comprises less than about 10 ppb sulfate and / or less than about 10 ppb chloride. Organically bound chlorides and sulfates are measured collectively as TOC. Individual organic sulfates and organic chlorides contained in untreated virgin resin may decompose to form ionic chlorides and sulfates. These compounds may be analytically measured by UV light, which breaks down the organic compounds, leaving ionic chlorides and sulfates that can be analyzed using conventional methods.

[0048] In some embodiments, after maintaining the virgin ion exchange resin material in the container for at least about six months, the rate of oxidative degradation may be reduced such that the first volume of water treated by the virgin ion exchange resin material comprises less than about 10 ppb total organic carbon, less than about 10 ppb sulfate, and / or less than about 10 ppb chloride.

[0049] In some embodiments, the methods disclosed herein may further include opening the container and rinsing the virgin ion exchange resin material. The method may further include opening the container after maintaining the virgin ion exchange resin material in the container for a predetermined time and rinsing the virgin ion exchange resin material. For example, the method may further include opening the container and rinsing the virgin ion exchange resin material after maintaining the virgin ion exchange resin material in the container for at least about six months. The method may further include opening the container and rinsing the virgin ion exchange resin material with deoxygenated water and / or deionized water (deoxygenated or non-deoxygenated) prior to use.

[0050] According to another aspect, a method of facilitating water treatment is provided at a location in need thereof. The method of facilitating on-site water treatment may include rinsing virgin ion exchange resin material with deoxygenated water to produce rinsed virgin ion exchange resin material. The method of facilitating water treatment may include introducing the rinsed virgin ion exchange resin material into a gas impermeable container. The method may include sealing the container. In some embodiments, the method may include providing the gas impermeable container with the rinsed virgin ion exchange resin material and residual moisture to a location, such as a water treatment location. The residual moisture content may include, for example, a moisture content of about 40% to about 50%.

[0051] In some embodiments, a method of facilitating water treatment at a location in need thereof may include rinsing a virgin ion exchange resin material with deoxygenated water having a dissolved oxygen concentration of less than about 10 ppb. A method of facilitating water treatment may include rinsing a virgin ion exchange resin material with deoxygenated water having a dissolved oxygen concentration of about 1 ppb. A method of facilitating water treatment may include rinsing a virgin ion exchange resin material with deoxygenated water having a chlorine concentration of less than about 10 ppb. A method of facilitating water treatment may include rinsing a virgin ion exchange resin material with deoxygenated water having a chlorine concentration of about 1 ppb.

[0052] According to certain embodiments, the methods disclosed herein may further include providing a procedure. The method may include providing a procedure for maintaining the virgin ion exchange resin material in a sealed container for a predetermined period of time. For example, the method may include providing a procedure for maintaining the virgin ion exchange resin material in a sealed container until ready for use. In some embodiments, the method may further include providing a procedure for opening the container and rinsing the virgin ion exchange resin material with deoxygenated water, e.g., before use. The method may include providing a procedure for opening the container and rinsing the virgin ion exchange resin material before use, e.g., before use in water treatment.

[0053] According to another aspect, a container is provided that includes virgin ion exchange resin material and deoxygenated water. In some embodiments, the container can be sealed. In some embodiments, the container can include deoxygenated water having less than about 10 ppb of dissolved oxygen. The container can include deoxygenated water having less than about 10 ppb of chlorine.

[0054] In some embodiments, the container may include a packaged desiccant medium. For example, the container may include a packaged desiccant medium within the container. In some embodiments, the container may be constructed from a gas impermeable material. For example, the container may be constructed from at least one of stainless steel and epoxy-lined carbon steel.

[0055] In some embodiments, the virgin ion exchange resin material can be a cation exchange resin, hi some embodiments, the virgin ion exchange resin material can be an anion exchange resin or a mixture of cation and anion exchange resins.

[0056] According to one aspect, a method of stabilizing virgin ion exchange resin material is provided. The method includes rinsing the virgin ion exchange resin material with deoxygenated water to produce a rinsed virgin ion exchange resin material. The method may further include introducing the rinsed virgin ion exchange resin material into a gas-impermeable container. The method may include introducing the rinsed virgin ion exchange resin material into a designated compartment of the container, e.g., a liquid-impermeable compartment. The method may include introducing a preservative, an oxygen-scavenging material, and / or an indicator of oxygen contamination into the gas-impermeable container. The method may further include sealing the container. The method may further include purging oxygen from the gas-impermeable container. In certain embodiments, the method may include removing the preservative, the oxygen-scavenging material, and the indicator of oxygen contamination prior to using the ion exchange resin.

[0057] A system and method for stabilizing virgin ion exchange resin material is disclosed. The method may include rinsing the virgin ion exchange resin material with deoxygenated water to produce a rinsed virgin ion exchange resin material. The method may include introducing the rinsed virgin ion exchange resin material into a liquid impermeable compartment of a gas impermeable container. The method may include sealing the container.

[0058] According to certain embodiments, the method may further include introducing an oxygen scavenging material into the gas impermeable container. The method may include disposing the oxygen scavenging material between an exterior wall of the liquid impermeable compartment and an interior wall of the gas impermeable container.

[0059] In some embodiments, the method may include introducing the rinsed virgin ion exchange resin material into a gas impermeable vessel comprising at least one of polyethylene terephthalate, stainless steel, and epoxy-lined carbon steel.

[0060] The method can include rinsing the virgin ion exchange resin material with deoxygenated water having a dissolved oxygen concentration of less than about 10 ppb.

[0061] The method may include rinsing virgin ion exchange resin material within a gas impermeable container.

[0062] According to another aspect, a method of stabilizing virgin ion exchange resin material is provided. The method may include rinsing the virgin ion exchange resin material with deoxygenated water to produce a rinsed virgin ion exchange resin material. The method may include introducing the rinsed virgin ion exchange resin material into a gas impermeable container. The method may include introducing an oxygen scavenging material into the gas impermeable container, the oxygen scavenging material positioned to avoid direct contact with moisture. The method may include sealing the container.

[0063] In some embodiments, the method may further include introducing the rinsed virgin ion exchange resin material into a liquid impermeable compartment of a gas impermeable container. The method may include disposing an oxygen scavenging material between an outer wall of the liquid impermeable compartment and an inner wall of the gas impermeable container.

[0064] According to certain embodiments, the oxygen scavenging material may include ferrous compounds, catechol, ascorbate, ascorbic acid, sodium bicarbonate, citrus extracts, oxidase enzymes, unsaturated hydrocarbons, polyamides, or combinations thereof.

[0065] The method may further include introducing an indication of oxygen contamination. The indication of oxygen contamination may be a redox midpoint potential E of about -0.05 V to about +0.06 V at pH 7 and 25°C. 0 The visual indicator may have the following characteristics:

[0066] According to another aspect, methods are provided for facilitating water treatment at a location where it is needed. These methods may include providing a rinsed virgin ion exchange resin material in deoxygenated water, the rinsed virgin ion exchange resin material being disposed in a liquid impermeable compartment of a sealed gas impermeable container.

[0067] In some embodiments, the method may further include providing an oxygen scavenging material within the gas impermeable container and disposed such that the material is not in direct contact with the deoxygenated water. The method may include providing an oxygen scavenging material disposed between an outer wall of the liquid impermeable compartment and an inner wall of the gas impermeable container. The method may include providing an oxygen scavenging material selected from ferrous compounds, catechol, ascorbate, ascorbic acid, sodium bicarbonate, citrus extracts, oxidase enzymes, unsaturated hydrocarbons, polyamides, and combinations thereof.

[0068] In some embodiments, the method can include providing deoxygenated water in an amount of about 40% to about 50% of the virgin ion exchange resin material.

[0069] The method can include providing deoxygenated water having less than about 10 ppb of dissolved oxygen.

[0070] In some embodiments, the method may include providing an indication of oxygen contamination within the gas impermeable container.

[0071] According to another aspect, a sealed container is provided. The container can include virgin ion exchange resin material in deoxygenated water having less than about 10 ppb of dissolved oxygen. The container can also include an oxygen scavenging material.

[0072] In some embodiments, virgin ion exchange resin material in deoxygenated water may be placed in a liquid impermeable compartment of a sealed container.

[0073] The oxygen scavenging material may be disposed between the outer wall of the liquid impermeable compartment and the inner wall of the container. The oxygen scavenging material may include ferrous compounds, catechol, ascorbate, ascorbic acid, sodium bicarbonate, citrus extracts, oxidases, unsaturated hydrocarbons, polyamides, and combinations thereof.

[0074] The vessel may be constructed from materials comprising at least one of polyethylene terephthalate, stainless steel, and epoxy-lined carbon steel.

[0075] The container may further comprise an indicator of oxygen contamination. The indicator of oxygen contamination is a redox midpoint potential E of about -0.05 V to +0.06 V at pH 7 and 25° C. 0 The device may include a visual indicator having:

[0076] As used herein, "virgin ion exchange resin" material may refer to unused or unconsumed ion exchange resin material. Virgin ion exchange resin material may include freshly manufactured resin and / or used resin that has been processed to meet the required specifications for new use. For example, raw or unpurified resin may be processed for new use by treatment with high purity water. Used resin may also be regenerated for reuse by treatment with strong acid or strong base. Virgin ion exchange resin material may comprise cation exchange resin, anion exchange resin, and mixtures of cation exchange resin and anion exchange resin.

[0077] According to yet another aspect, a system and method for stabilizing virgin ion exchange resin material is provided that includes washing the virgin ion exchange resin material. The virgin ion exchange resin material may be washed with a formulation comprising a suitable detergent.

[0078] As used herein, "washed ion exchange resin" material may refer to an ion exchange resin material that has been treated for the removal of water-insoluble oxygen-containing impurities. According to certain embodiments, the water-insoluble oxygen-containing impurities may be oxygen-decomposed contaminants having a water solubility of less than about 10.0 g / L. The water-insoluble oxygen-containing impurities may have a water solubility of less than about 7.0 g / L, less than about 5.0 g / L, less than about 4.0 g / L, less than about 3.0 g / L, less than about 2.0 g / L, less than about 1.0 g / L, or less than about 0.5 g / L.

[0079] The washed ion exchange resin may have a concentration of oxygen-containing impurities or contaminants less than about 50 ppb, which may be measured as oxygen-containing total organic carbon (TOC). In some embodiments, the washed ion exchange resin may have an oxygen-containing TOC of less than 40 ppb, an oxygen-containing TOC of less than 30 ppb, an oxygen-containing TOC of less than 25 ppb, an oxygen-containing TOC of less than 20 ppb, an oxygen-containing TOC of less than 15 ppb, an oxygen-containing TOC of less than 10 ppb, or an oxygen-containing TOC of less than 5 ppb. The concentration of oxygen-containing TOC in the ion exchange resin may generally depend on the particular cleaning agent, the cleaning agent concentration in the formulation, and the cleaning method used.

[0080] The water-insoluble oxygen-containing impurities may generally be oxidized derivative molecules of the resin material. According to certain embodiments, the ion exchange resin material may be a polystyrene-based resin material. Exemplary oxidized derivative molecules of polystyrene-based resin materials include benzaldehyde and acetophenone. Other derivative molecules may result from oxidized degradation of polystyrene or other materials of the resin. Such oxidized molecules may be similarly removed by the methods disclosed herein.

[0081] In certain embodiments, the ion exchange resin material may contain one or more antioxidants from manufacture. For example, a polystyrene-based resin may contain orthoxylene. Exemplary oxidized derivative molecules of such antioxidants include 5-methyl-3-hexanone, methoxyphenyloxime, 2-methylbenzaldehyde, benzenemethanimine, and tributylamine. Other oxidized derivative molecules may result from oxidative degradation of orthoxylene or other resin molecular species. Such oxidized molecules may be similarly removed by the methods disclosed herein.

[0082] In some embodiments, the oxygen-containing impurities may include one or more of 5-methyl-3-hexanone, methoxyphenyloxime, benzaldehyde, acetophenone, 2-methylbenzaldehyde, benzenemethanimine, and tributylamine.

[0083] The ion exchange resin material may be rinsed with water to remove water soluble oxygen-containing impurities and contaminants.

[0084] The embodiments disclosed herein may incorporate ion exchange resin materials rinsed with deionized water. Deoxygenated water is water that has been treated to remove molecular oxygen, e.g., dissolved oxygen. In general, non-deoxygenated water may contain more than about 1 ppm of molecular dissolved oxygen, and up to about 20 ppm of dissolved oxygen. Dissolved oxygen in water may vary with temperature, salinity, pH, conductivity, dissolved solids concentration, and pressure changes. Dissolved oxygen concentration may be measured with one or more of a meter, a sensor, Winkler titration, and colorimetry. The embodiments disclosed herein may incorporate measuring one or more of temperature, pressure, salinity, pH, conductivity, total dissolved solids (TDS) concentration, and dissolved oxygen concentration of water.

[0085] According to certain embodiments, the methods disclosed herein may further include producing deoxygenated water. Deoxygenated water may be produced, for example, by deoxygenating non-deoxygenated water from a source of non-deoxygenated water. Deoxygenated water may be produced by treating non-deoxygenated water to remove dissolved oxygen. In some embodiments, the deoxygenated non-deoxygenated water may have at least about 75% of the dissolved oxygen removed. Deoxygenating the non-deoxygenated water may remove at least about 75%, at least about 80%, at least about 85%, at least about 90%, at least about 95%, at least about 99%, or about 100% of the dissolved oxygen from the non-deoxygenated water. Deoxygenating the non-deoxygenated water may remove about 90% to about 100% of the dissolved oxygen from the non-deoxygenated water. Non-deoxygenated water may include deionized water, ultrapure water, high purity water, distilled water, microfiltered water, ultrafiltered water, water that has undergone reverse osmosis or ultraviolet oxidation, granular activated carbon treated water, or water that has been treated in other ways to remove contaminants.

[0086] Non-deoxygenated water may be deoxygenated by passing it through a deoxygenation membrane. For example, the deoxygenation membrane may comprise a Liqui-Cel® membrane contactor (manufactured by 3M Industrial Group, Maplewood, Minnesota). Briefly, a deoxygenation membrane may remove dissolved gas from a liquid with a mass transfer driving force. According to Henry's law, the amount of gas dissolved in a liquid at equilibrium is proportional to the partial pressure of the gas in the gas phase in contact with the liquid. At standard temperature and pressure (25° C. and 1 atm), equilibrium water may contain approximately 8.5 ppm of dissolved oxygen, 14.5 ppm of dissolved nitrogen, and some dissolved carbon dioxide. Reducing the partial pressure of the gas in contact with the liquid may correspondingly reduce the amount of gas dissolved in the liquid. The partial pressure of the gas may be reduced by lowering the total pressure of the gas phase or by changing the concentration of the gas in the gas phase. Each of these changes may be applied to the gas side of the membrane and may drive the dissolved gas out of the liquid through the membrane.

[0087] Non-deoxygenated water can be deoxygenated by subjecting it to vacuum degassing. Vacuum degassing can be accomplished in a vacuum degassing tower or a dedicated vacuum chamber. To reduce the concentration of dissolved gas in a liquid with vacuum degassing, the total pressure of the gas phase can be reduced by applying a vacuum to the gas. Mass transfer can drive the dissolved gas out of the liquid in contact with the gas.

[0088] Non-deoxygenated water can be deoxygenated by exposing it to an oxygen-scavenging resin. The oxygen-scavenging resin can be contained in a column or other device. In some embodiments, the oxygen-scavenging resin can include a catalyst. The catalyst can comprise a metal halide. In some embodiments, the catalyst can include sodium chloride. The catalyst can include palladium or a palladium compound, for example, palladium chloride.

[0089] In some embodiments, the methods disclosed herein include rinsing the virgin ion exchange resin material with deoxygenated water having a concentration of dissolved oxygen effective to reduce the rate of oxidative degradation of the virgin ion exchange resin material. In general, a reduced rate of oxidative degradation may contribute to improved resin stability, liquid purification capability, reduced rate of crosslink degradation, reduced incidence of impurities, improved bead integrity, and / or reduced concentration of ionic contaminants in the treated liquid. For example, in some embodiments, the stabilized ion exchange resin may have a reduced crosslink degradation rate of about 90% to about 70% over a given storage period, e.g., at least 6 months storage period. The stabilized ion exchange resin may have about a 100% reduction in crosslink degradation rate, about a 90% reduction in crosslink degradation rate, about an 80% reduction in crosslink degradation rate, about a 70% reduction in crosslink degradation rate, or about a 60% reduction in crosslink degradation rate. The percent reduction in degradation (and decrosslinking) may depend on the concentration of oxidizing agent present and the concentration of iron and other metals in or on the resin that act as catalysts for degradation.

[0090] The water insoluble oxygen-containing impurities and contaminants may be removed by washing the ion exchange resin material with a surfactant. In some embodiments, the water insoluble oxygen-containing impurities and contaminants may be removed with a washing agent, for example a non-ionic washing agent.

[0091] The embodiments disclosed herein may incorporate the cleaning ion exchange resin material into a preparation that includes a non-ionic detergent. The preparation may be an aqueous preparation or may include a buffer or other solvent. The detergent generally includes a surfactant with cleaning properties, often in a dilute solution. In some embodiments, the non-ionic detergent may include polyoxyethylene (POE), polyethylene glycol (PEG), polyethylene oxide (PEO), or a glycoside backbone with an uncharged hydrophilic head group. Suitable non-ionic detergents include, for example, ethoxylated octylphenol, polysorbate, polyoxyethylene, and their metabolites.

[0092] Detergents are often foaming agents. The critical micelle concentration (CMC) of a surfactant or detergent is the concentration above which micelles are formed. Thus, at concentrations above the CMC, the surfactant may begin to form bubbles, which contribute to the oxidative degradation of the ion exchange resin. According to certain embodiments, the formulation may comprise a surfactant or detergent at a concentration below its CMC. For example, according to certain embodiments, the formulation may comprise ethoxylated octylphenol at a concentration below about 0.125 g / L. The CMC of a surfactant or detergent may vary with temperature and pressure. As disclosed herein, exemplary CMCs are for formulations at about room temperature (25° C.) and about atmospheric pressure.

[0093] Additionally or alternatively, water insoluble oxygen-containing impurities and contaminants can be removed by washing the ion exchange resin material with an alcohol solvent.

[0094] The embodiments disclosed herein may incorporate the washing ion exchange resin material with a preparation comprising an alcohol solvent. The preparation may be an aqueous preparation or may comprise a buffer or other solvent. The alcohol solvent may be slightly polar, making them suitable solvents for non-polar hydrocarbons, polar organic molecules, and certain ionic compounds. Exemplary alcohol solvents may include, for example, isopropanol, methanol, ethanol, n-butanol, isooctanol, methyl isobutyl carbinol, isoamyl alcohol, isobutyl alcohol, cyclohexanol, methyl cyclohexanol, and aqueous ammonia.

[0095] Isopropanol can be used as a solvent and cleaning agent for ion exchange resins, since it does little harm to the ion exchange resins while removing water-insoluble contaminants. According to certain embodiments, the preparation may comprise less than 2.0% isopropanol. For example, the preparation may comprise less than about 1.5% isopropanol, less than about 1.0% isopropanol, less than about 0.5% isopropanol, or less than about 0.25% isopropanol.

[0096] In some embodiments, the stabilized ion exchange resin may have less than about 100 ppm metal impurities (dry weight), including, for example, aluminum, copper, iron, sodium, and lead, and / or less than about 10 ppm organic impurities (soak), including, for example, total organic carbon (TOC), sulfate, and chloride, after a storage period, for example, at least 6 months. Specifically, the stabilized ion exchange resin may have iron impurities of about 50 ppm or less, about 40 ppm or less, about 30 ppm or less, about 20 ppm or less, about 10 ppm or less, about 5 ppm or less, or about 1 ppm or less. The stabilized ion exchange resin may have less than about 5 ppm TOC, sulfate, or chloride impurities, less than about 4 ppm, less than about 3 ppm, less than about 2 ppm, less than about 1 ppm, less than about 0.5 ppm, less than about 0.1 ppm TOC, sulfate, or chloride impurities, or less than about 1 ppb TOC, or even less than about 0.5 ppb TOC. These concentrations are measured analytically in rinse water that passes through and / or bathes the resin, and measures the TOC in the effluent. Levels are measured to less than 1 ppb, or even less than 0.5 ppb TOC. In some embodiments, stabilized ion exchange resin material stored for a given storage period may be substantially similar to new or regenerated ion exchange resin material, for example, in bead integrity, concentration of impurities, and / or concentration of ionic contaminants in the treated liquid.

[0097] The methods disclosed herein may include a predetermined storage period. The predetermined storage period may generally include any time that the ion exchange resin is held in a sealed container. The storage period may include storage, handling, transportation, or any use for maintaining the ion exchange resin in a sealed container. As used herein, the predetermined storage period may include a storage period of at least about 15 days, a storage period of at least about 30 days, a storage period of at least about 1 month, a storage period of at least about 2 months, a storage period of at least about 3 months, a storage period of at least about 6 months, a storage period of at least about 9 months, a storage period of at least about 12 months, a storage period of at least about 18 months, or a storage period of at least about 24 months.

[0098] In some embodiments, the rate of oxidative degradation of the virgin ion exchange resin material may be reduced such that a first volume of water treated with the virgin ion exchange resin material contains less than about 1 ppb TOC to less than about 10 ppb TOC. In some embodiments, after maintaining the virgin ion exchange resin material in a vessel for a predetermined period of time, the rate of oxidative degradation may be reduced such that the first volume of water treated with the virgin ion exchange resin material contains less than about 1 ppb TOC to less than about 10 ppb TOC. For example, the first volume of water to be treated may comprise less than about 30 ppb TOC, less than about 20 ppb TOC, less than about 10 ppb TOC, less than about 5 ppb TOC, less than about 1 ppb TOC, less than about 0.5 ppb TOC, or less than about 0.1 ppb TOC.

[0099] As disclosed herein, the first volume of water to be treated by the ion exchange resin material includes a soak or rinse of the ion exchange resin material that is observed initially once the ion exchange resin material is placed in line to treat the water. In some embodiments, the concentration of the contaminant in the first volume of water to be treated can be measured from the water in contact with the ion exchange resin material. In other embodiments, the concentration of the contaminant in the first volume of water to be treated can be measured downstream of the ion exchange resin material contact, for example, such that the water is diluted or concentrated in a downstream process. In some embodiments, the water can be diluted or concentrated by at least about 100, about 200, or about 300 times. In such embodiments, the concentration of the contaminant in the undiluted or unconcentrated first volume of treated water can be extrapolated from the concentration of the contaminant measured in the diluted water or the concentrated water. Thus, as disclosed herein, the concentration of the contaminant in the first volume of treated water can refer to the concentration of the undiluted and unconcentrated contaminant. The first volume of treated water can include, for example, between about 25 gallons and about 150 gallons of treated water. In some embodiments, the undiluted, unconcentrated first volume of process water comprises about 25 gallons, about 50 gallons, about 75 gallons, about 100 gallons, about 125 gallons, or about 150 gallons of process water. Alternatively, the first 15-20 resin bed volumes of rinse water passed through the ion exchange resin material may contain high ppb or low ppm levels of organics, including organic sulfates and chlorides.

[0100] In some embodiments, the rate of oxidative degradation may be reduced such that the first volume of water treated with the virgin ion exchange resin material comprises less than about 10 ppb of sulfate. The rate of degradation during use may be affected by temperature, nuclear radiation, oxidation, and / or metals present on the resin. In some embodiments, the rate of oxidative degradation may be reduced such that the first volume of water treated with the virgin ion exchange resin material comprises less than about 10 ppb of chloride. After maintaining the virgin ion exchange resin material in the container for a predetermined period of time, the rate of oxidative degradation may be reduced such that the first volume of water treated with the virgin ion exchange resin material comprises less than about 10 ppb of sulfate and / or less than about 10 ppb of chloride. For example, the first volume of water to be treated may comprise less than about 30 ppb sulfate or chloride, less than about 20 ppb sulfate or chloride, less than about 10 ppb sulfate or chloride, less than about 5 ppb sulfate or chloride, 1 ppb sulfate or chloride, less than about 0.5 ppb sulfate or chloride, or less than about 0.1 ppb sulfate or chloride.

[0101] In some embodiments, the rate of oxidative degradation may be reduced such that a first volume of water treated by the virgin ion exchange resin material after maintaining the virgin ion exchange resin material in a container for a predetermined storage period, e.g., at least about six months, contains less than about 10 ppb TOC, less than about 10 ppb sulfate, and / or less than about 10 ppb chloride.

[0102] In some embodiments, the deoxygenated water may contain less than about 0.1 ppm dissolved oxygen. For example, the deoxygenated water may comprise less than about 0.1 ppm, less than about 50 ppb, less than about 40 ppb, less than about 30 ppb, less than about 20 ppb, less than about 10 ppb, less than about 8 ppb, less than about 6 ppb, less than about 5 ppb, less than about 4 ppb, less than about 3 ppb, less than about 2 ppb, less than about 1 ppb, or less than about 0.5 ppb dissolved oxygen.

[0103] Deoxygenation can remove other dissolved gases in the water, such as dissolved carbon dioxide, dissolved nitrogen, and other ambient air gases. In some embodiments, the deoxygenated water can contain less than about 0.1 ppm of dissolved carbon dioxide or nitrogen. For example, the deoxygenated water can have less than about 0.1 ppm, less than about 50 ppb, less than about 40 ppb, less than about 30 ppb, less than about 20 ppb, less than about 10 ppb, less than about 8 ppb, less than about 6 ppb, less than about 5 ppb, less than about 4 ppb, less than about 3 ppb, less than about 2 ppb, less than about 1 ppb, or less than about 0.5 ppb of dissolved carbon dioxide or nitrogen.

[0104] The methods disclosed herein may include treating deoxygenated or non-deoxygenated water to remove oxidative contaminants. Deoxygenated or non-deoxygenated water may comprise small amounts of other oxidative contaminants, such as chlorine, chloramines, and / or hydrogen peroxide. Deoxygenated or non-deoxygenated water may be treated with membrane filtration, reverse osmosis, high purity reducing agents (such as sodium bisulfite), or granular activated carbon to remove oxidative contaminants such as chlorine. In some embodiments, deoxygenated or non-deoxygenated water may comprise less than about 0.1 ppm chlorine. For example, deoxygenated water may comprise less than about 0.1 ppm, less than about 50 ppb, less than about 40 ppb, less than about 30 ppb, less than about 20 ppb, less than about 10 ppb, less than about 8 ppb, less than about 6 ppb, less than about 5 ppb, less than about 4 ppb, less than about 3 ppb, less than about 2 ppb, less than about 1 ppb, or less than about 0.5 ppb chlorine, chloramines, and hydrogen peroxide.

[0105] The methods disclosed herein may include rinsing the virgin ion exchange resin material by introducing deoxygenated water into a gas-impermeable container with the virgin ion exchange resin material and removing the interstitial (oxygen) water from the container. For example, a container with virgin ion exchange resin material may be filled with deoxygenated water, the deoxygenated water may be substantially drained, and the deoxygenated water may replace the oxygenated water. In some embodiments, the methods disclosed herein may include maintaining the moisture content in the rinsed virgin ion exchange resin material. As disclosed herein, moisture content may refer to the amount of liquid or water contained in the material. Moisture content may be defined as the ratio of the mass of liquid (e.g., water) in the sample to the mass of solids (e.g., ion exchange resin) in the sample. Interstitial moisture is the water in the voids between the individual resin beads. The moisture of the beads themselves is the moisture or hydration within the resin beads measured in percent moisture. Most plastics (and other materials) have an inherent amount of moisture within the material that can be dried, and the difference in weight is measured. The deoxygenation portion of the methods disclosed herein replaces or otherwise removes both sites of oxygenated water.

[0106] In some embodiments, the method includes maintaining a moisture content in the rinsed virgin ion exchange resin material of at least about 20%. The method may include maintaining a moisture content in the rinsed ion exchange resin material of at least about 20%, at least about 30%, at least about 40%, at least about 50%, at least about 60%, or at least about 70%. In some embodiments, the method includes maintaining a moisture content in the rinsed virgin ion exchange resin material of less than about 50%. The method may include maintaining a moisture content in the rinsed ion exchange resin material of less than about 80%, less than about 70%, less than about 60%, less than about 50%, less than about 40%, or less than about 30%. In some embodiments, the method includes maintaining a moisture content in the rinsed virgin ion exchange resin material of between about 20% and about 80%, between about 30% and about 60%, or between about 40% and about 50%. Residual moisture content may be maintained in the virgin ion exchange resin material while the container is sealed, e.g., while the container containing the rinsed virgin ion exchange resin material is handled, stored, or transported. In some embodiments, the moisture content may contribute to stabilizing the rinsed virgin ion exchange resin material over time. For example, the moisture content may contribute to reducing the rate of oxidative degradation of the virgin ion exchange resin material.

[0107] Higher cross-linking of resins can counteract the dominance of oxidative degradation. High cross-linking contains entangled organic matter, resulting in lower TOC levels over a period of time. This effect can be negated by continued exposure of the resin to oxidizing agents.

[0108] In some embodiments, the methods disclosed herein may further include opening the container and rinsing the virgin ion exchange resin material. The methods may further include opening the container and rinsing the virgin ion exchange resin material after maintaining the virgin ion exchange resin material in the container for a predetermined period of time, as described above. For example, the methods may further include opening the container and rinsing the virgin ion exchange resin material after maintaining the virgin ion exchange resin material in the container for at least about six months. The methods may further include opening the container and rinsing the virgin ion exchange resin material before use. The virgin ion exchange resin material may be rinsed with deoxygenated water before use. In some embodiments, the virgin ion exchange resin material may be rinsed with deoxygenated water having any concentration of dissolved oxygen, dissolved gas, or oxidizing contaminants previously disclosed herein before use. The virgin ion exchange resin material may be rinsed with deoxygenated water produced by any of the methods previously disclosed herein before use.

[0109] According to another aspect, a method is provided to facilitate water treatment at a location in need thereof, which may be associated with, for example, nuclear power generation, microelectronics manufacturing, semiconductor manufacturing, food manufacturing, pharmaceutical manufacturing, chemical processing, and metal extraction, or any location requiring water treatment that may benefit from ion exchange water treatment technology.

[0110] A method of facilitating on-site water treatment may include providing a virgin ion exchange resin material that has been rinsed in deoxygenated water as previously described herein. The rinsed virgin ion exchange resin material may be provided in a sealed gas impermeable container. In some embodiments, the rinsed virgin ion exchange resin material may be provided in a liquid impermeable compartment of the sealed container. The method may further include providing one or more of a preservative, an oxygen scavenging material, or an indicator of oxygen contamination in the sealed container.

[0111] A method for facilitating on-site water treatment may include providing a washed virgin ion exchange resin material in deoxygenated water as previously described herein. The washed virgin ion exchange resin material may be a polystyrene-based ion exchange resin material. As previously described, the polystyrene-based resin material may decompose to form oxygen-containing impurities and contaminants in the form of total organic carbon (TOC). In some embodiments, the provided washed virgin ion exchange resin material may have less than about 25 ppb of oxygen-containing TOC species. For example, the provided washed virgin ion exchange resin material may have less than about 20 ppb of oxygen-containing TOC, less than about 15 ppb of oxygen-containing TOC, less than about 10 ppb of oxygen-containing TOC, or less than about 5 ppb of oxygen-containing TOC.

[0112] The washed virgin ion exchange resin material may be placed in a sealed gas impermeable container. In some embodiments, the washed virgin ion exchange resin material may be provided in a liquid impermeable compartment of a sealed container. The method may further include providing one or more of a preservative, an oxygen scavenging material, or an indicator of oxygen contamination in the sealed container. The washed virgin ion exchange material may be rinsed with deoxygenated water before or after washing.

[0113] Generally, the method of facilitating on-site water treatment may include washing the virgin ion exchange resin material with deoxygenated water to produce a rinsed virgin ion exchange resin material. Additionally or alternatively, the method may include washing the virgin ion exchange resin material with a surfactant, detergent, or alcohol solvent. The method may include introducing the virgin ion exchange resin material into a gas-impermeable container, sealing the container, and purging oxygen from the container, as previously described herein. The method of facilitating water treatment may include providing the gas-impermeable container comprising the rinsed and / or washed virgin ion exchange resin material and residual moisture to a location, such as, for example, a water treatment location. In some embodiments, the method of facilitating water treatment may further include providing instructions regarding the use of the container comprising the virgin ion exchange resin material.

[0114] As discussed above, the residual moisture content may include maintaining the moisture content of the rinsed ion exchange resin. For example, the residual moisture content may include a moisture content of about 40% to about 50%. The residual moisture content may include a moisture content of about 20% to about 80%, about 30% to about 60%, or about 40% to about 50% in the rinsed virgin ion exchange resin material, or any of the moisture contents discussed above.

[0115] In some embodiments, a method for facilitating water treatment at a location in need thereof may include rinsing a virgin ion exchange resin material with deionized water, for example deionized water having a dissolved oxygen concentration of less than about 10 ppb. In some embodiments, the virgin ion exchange resin material may be rinsed with deoxygenated water having any concentration of dissolved oxygen, dissolved gas, or oxidizing contaminants, as previously disclosed herein.

[0116] In some embodiments, the method of facilitating water treatment in a location where it is needed may include, for example, washing a virgin ion exchange resin material with a formulation having a non-ionic detergent at a concentration below its CMC. For example, the method may include washing a virgin ion exchange resin material with a formulation having an ethoxylated octylphenol at a concentration of less than about 0.125 g / L. In some embodiments, the method may include washing a virgin ion exchange resin material with a formulation comprising, for example, an alcohol solvent. For example, the method may include washing a virgin ion exchange resin material with a formulation having an isopropanol at a concentration of less than about 0.5%. In some embodiments, a virgin ion exchange resin material may be washed with a formulation having a surfactant, detergent, or alcohol solvent at any concentration as previously disclosed herein.

[0117] According to certain embodiments, the methods disclosed herein may further include providing a procedure for maintaining the virgin ion exchange resin material in a sealed container for a predetermined period of time. For example, the method may include providing a procedure for maintaining the virgin ion exchange resin material in a sealed container until ready for use. The predetermined period of time may include any length of storage, handling, and / or shipping time required prior to use of the ion exchange resin. The predetermined period of time may include any predetermined period of time as previously described herein.

[0118] The methods disclosed herein may include providing procedures for maintaining the sealed container under certain conditions. For example, the methods may include providing procedures for maintaining the container with the cation exchange resin at a temperature of at least less than about 210°F (99°C), at least less than about 200°F (93°C), or at least less than about 190°F (88°C). The methods may include providing procedures for maintaining the container with the anion exchange resin or a mixture of anion exchange resin and cation exchange resin at a temperature of at least less than about 130°F (54°C) or at least less than about 120°F (49°C) and down to ambient temperature. The methods may include providing procedures for maintaining the sealed container at ambient pressure. The methods may include providing procedures for avoiding a temperature rise of more than 10°C, such as a temperature rise of more than 7°C or more than 5°C.

[0119] In some embodiments, the method may further include providing a procedure for opening the container and rinsing the virgin ion exchange resin material with deoxygenated water, e.g., prior to use. As previously described herein, the virgin ion exchange resin material may be rinsed with deoxygenated water containing any concentration of dissolved oxygen, dissolved gas, or oxidizing contaminants. The method disclosed herein may include a procedure for rinsing the virgin ion exchange resin material immediately prior to use. In some embodiments, the method may include providing a procedure for rinsing the virgin ion exchange resin material immediately prior to use while the ion exchange resin is still contained within the container. For example, the method may include providing a procedure for filling the container with deoxygenated water and removing interstitial water from the container, thus rinsing the virgin ion exchange resin material. The method may include providing a procedure for opening the container and rinsing the virgin ion exchange resin material, e.g., prior to use in water treatment.

[0120] In some embodiments, the method of facilitating water treatment may include a procedure for returning the vessel after removal of the ion exchange resin material. Such a procedure may reduce vessel waste and reduce operation time.

[0121] According to another aspect, a container is provided that includes virgin ion exchange resin material and deoxygenated water. In some embodiments, the container may be sealed. The container may include an opening having a hermetic seal. The container may further include an inlet and an outlet. The inlet and outlet may include an airtight seal. The inlet may be connected to a source of ion exchange resin material or a source of deoxygenated water. The outlet may be connected to a drain for the deoxygenated water or to a point of use of the ion exchange resin material. For example, the outlet may be connected to a hose configured to deliver the ion exchange resin material to a point of use.

[0122] The vessel may be a container, tank, barrel, basin, chamber, or receptacle configured to hold the ion exchange resin and deoxygenated water. The vessel generally has a volume of about 20 cubic feet (0.57 m 3 ) ~ Approximately 50 cubic feet (1.42 m 3For example, the volume of the vessel may be about 20 cubic feet (0.57 m 3 ), 25 cubic feet (0.71 m 3 ), 30 cubic feet (0.85 m 3 ), 35 cubic feet (1.0 m 3 ), 40 cubic feet (1.13 m 3 ), 45 cubic feet (1.27 m 3 ), or 50 cubic feet (1.42 m 3 ) The vessel will generally have a volume in which the headspace restriction associated with where the ion exchange resin material is required can be observed.

[0123] In some embodiments, the container may be constructed from a gas-impermeable material. The container may be composed of a material with a high flash point. For example, the container may be constructed from or lined with at least one of stainless steel and epoxy-lined carbon steel. The container may be constructed from or lined with polyethylene terephthalate. Traditionally, ion exchange resin storage and transport containers may be constructed from fiber, plastic, or wood. Such materials are relatively inexpensive, but are not gas-impermeable and may contribute to oxidative degradation of the ion exchange resin material within the container. Additionally, traditional materials may have low flash points and may be unsafe and / or undesirable in certain locations requiring ion exchange resin materials.

[0124] The container may include one or more compartments. According to certain embodiments, the container may include a liquid-impermeable compartment. Virgin ion exchange resin and deoxygenated water may be packed into the liquid-impermeable compartment. The liquid-impermeable compartment may have substantially no head space or interstitial space between the resin beads and the water. In some embodiments, the liquid-impermeable compartment may have a water content of about 40% to about 50% in the form of deoxygenated water. In some embodiments, the liquid-impermeable compartment may also be gas-impermeable. The liquid-impermeable compartment may be constructed from gas-impermeable materials as described above. Alternatively, the liquid-impermeable compartment may be constructed from polymeric or metallic materials that are liquid-impermeable. In some embodiments, the one or more compartments are integral with the container. In other embodiments, the one or more compartments are removable from the container. For example, the liquid-impermeable compartment containing the ion-exchange resin may be an ion-exchange resin package that is removable from the container.

[0125] In some embodiments, the container may contain deoxygenated water having any concentration of dissolved oxygen, dissolved gas, or oxidizing contaminants as previously described herein. In some embodiments, the container may contain a void volume of deoxygenated water. In some embodiments, the container may contain deoxygenated water as a residual moisture content, e.g., as a moisture content as previously described herein.

[0126] The container or a compartment thereof may comprise a void space of a predetermined volume, for example, the container or compartment may comprise interstitial void space between the ion exchange resin beads and / or head space. In some embodiments, the void space is limited. The container or compartment may comprise substantially no head space between the resin beads and / or may comprise limited interstitial space. Limiting the void space may contribute to the stability of the ion exchange resin stored, handled, or transported within the container.

[0127] In some embodiments, the container may include a preservative. The container may include a packaged desiccant medium. For example, the container may include a packaged desiccant medium contained within the container. The packaged desiccant medium may be configured to remove oxygen from void spaces within the container. In some embodiments, the desiccant / oxygen scavenging medium is packaged in a fiber pillow having a porous design that can allow oxygen exchange.

[0128] The preservative or desiccant / oxygen scavenging medium may be an oxygen scavenging material. The container may comprise an oxygen scavenging material. The oxygen scavenging material may be capable of removing or reducing the level of oxygen within the sealed container. In some embodiments, the oxygen scavenging material may be in the form of an oxygen scavenging compound. For example, the oxygen scavenging material may be an oxidizing compound. In some embodiments, the oxygen scavenging material comprises a ferrous compound, a catechol, an ascorbate salt, an ascorbic acid, sodium bicarbonate, a citrus extract, an oxidase enzyme, an unsaturated hydrocarbon, a polyamide, or a combination thereof. The oxygen scavenging material may further comprise a catalyst that promotes oxidation. For example, the oxygen scavenging material may comprise a metal halide catalyst. The oxygen scavenging material may comprise sodium chloride or palladium.

[0129] The oxygen scavenging material may be packaged in a gas-permeable container. The gas-permeable container may be water-permeable or water-impermeable. The gas-permeable container may comprise a gas-permeable pouch, a perforated container, a fabric container, a cardboard or paper container, or a polymer container. In other embodiments, the oxygen scavenging material may be part of a packaging film or structure. For example, the oxygen scavenging material may line or be part of a container structure. The gas-permeable container may be attached to a liquid-impermeable compartment that holds the ion exchange resin. In some embodiments, the gas-permeable container may be included on a layered strip around the liquid-impermeable compartment. In some embodiments, a portion of the liquid-impermeable compartment may be removable to expose the oxygen scavenging material.

[0130] The container may include an indicator of oxygen contamination. In some embodiments, the indicator may include a redox indicator in a transparent package. When reduced, the redox indicator may be a first color. When exposed to a predetermined concentration of an oxidizing agent, such as oxygen, the redox indicator may be oxidized and turn to a second color. Thus, the redox indicator may provide a visual indicator of oxygen contamination in the container. The indicator of oxygen contamination may be positioned such that it reacts with potential oxidizing agents in the container but is visible from the outside of the container, for example, through a window. Thus, the indicator may be visible without opening the hermetic seal of the container.

[0131] An indication of oxygen contamination is the redox midpoint potential E of approximately -0.05 V to approximately +0.06 V at pH 7 and 25 °C. 0 For example, an indication of oxygen contamination may be a redox midpoint potential E of about -0.05 V to about -0.04 V, about -0.02 V to about +0.02 V, or about +0.05 V to +0.06 V at pH 7 and 25°C. 0 Indicators of oxygen contamination may include, for example, indigotetrasulfonic acid, methylene blue, or thionine.

[0132] The preservative, oxygen scavenging material, or indicator of oxygen contamination may be placed in a designated compartment within the container, either independently or together. In some embodiments, the preservative, oxygen scavenging material, or indicator of oxygen contamination may be placed within the gas-impermeable container, but outside the liquid-impermeable compartment that holds the ion-exchange resin and deoxygenated water. In general, the preservative, oxygen scavenging material, or indicator of oxygen contamination may be placed so as not to be in direct contact with moisture. Thus, in some embodiments, the preservative, oxygen scavenging material, or indicator of oxygen contamination may be placed between the outer wall of the liquid-impermeable compartment that holds the ion-exchange resin and deoxygenated water and the inner wall of the gas-impermeable container.

[0133] In some embodiments, the virgin ion exchange resin material can be a cation exchange resin. In some embodiments, the virgin ion exchange resin material can be an anion exchange resin. In yet other embodiments, the virgin ion exchange resin material can be a mixture of cation exchange resin and anion exchange resin. The storage conditions of the container, such as temperature, pressure, and / or concentration of dissolved gas in the deoxygenated water, can vary depending on the type of ion exchange resin contained within the container. For example, in general, continuous exposure of the anion resin to free chlorine in excess of about 0.05 ppm should be avoided. At a supply temperature of about 5° C. to about 10° C., standard crosslinked anion resins can be capable of withstanding free chlorine levels up to about 0.3 ppm, highly crosslinked anion resins can be capable of withstanding free chlorine levels up to about 0.5 ppm, and macroporous anion resins can be capable of withstanding free chlorine levels up to about 1 ppm. At feed temperatures of about 20°C to about 30°C, standard crosslinked anion resins may be able to withstand free chlorine levels of only less than 0.1 ppm, highly crosslinked anion resins may be able to withstand free chlorine levels up to about 0.1 ppm, and macroporous anion resins may be able to withstand free chlorine levels up to about 0.5 ppm. Some cation exchange resins, such as DIAION® SK1B resins available from Mitsubishi Chemical Corporation, may have a free chlorine tolerance of about 0.6 mg / L at temperatures between about 5°C to about 10°C and about 0.1 mg / L at temperatures between about 20°C to about 25°C. The presence of a catalyst, such as iron or copper, may reduce the oxidant levels to which the resin may be exposed without significantly degrading the resin.

[0134] According to another aspect, a system is provided that includes a container containing virgin ion exchange resin material and deoxygenated water. The container may be gas impermeable and sealable as described above. The container may be connected or connectable downstream to a source of deoxygenated water. The container may be connected or connectable downstream to a source of ion exchange resin material. In some embodiments, the container may be connected or connectable upstream to a drain for used deoxygenated water. The container may be connected or connectable upstream to a point of use of the virgin ion exchange resin material, for example via a hose.

[0135] In some embodiments, the system includes an oxygen monitor. The oxygen monitor may be connected to the vessel and configured to measure the oxygen concentration in the vessel. The system may include a degasser, for example, an in-line degasser. The degasser may be an oxygen scavenging membrane. For example, the oxygen scavenging membrane may be provided by Liqui-Cel® membrane contactors (3M Industrial Group, Maplewood, Minn.). The degasser may be a vacuum degasser. The degasser may be a column or other device that includes an oxygen scavenging resin. The oxygen scavenging resin may include an oxygen scavenging material as described above. In some embodiments, the oxygen scavenging resin may include a catalyst. The catalyst may include a metal halide. In some embodiments, the catalyst may include sodium chloride. The catalyst may include palladium or a palladium compound, for example, palladium chloride. The degasser may be fluidly connected or connectable upstream of the vessel. The degasser may be fluidly connected or connectable downstream of a source of non-deoxygenated water and configured to perform deoxygenation of the non-deoxygenated water.

[0136] The system may further include a sensor or monitor, such as, for example, a pressure sensor or a thermometer. The sensor and / or monitor may be disposed upstream of the vessel and configured to measure the temperature, pressure, pH, conductivity, and / or composition of the deoxygenated or non-deoxygenated water. The sensor and / or monitor may be electrically connected to a control module. The control module may be configured to control one or more parameters of the in-line degasser in response to measurements received from the sensor and / or monitor. The control module may be connected to an oxygen monitor. The control module may be configured to control one or more parameters of the in-line degasser in response to measurements received from the oxygen monitor.

[0137] As shown in Figure 1, a container 100 may contain virgin ion exchange resin material and deoxygenated water. The container 100 may have an opening 110, an inlet 120, and an outlet 130. The opening, inlet, and / or outlet may be sealable. The inlet may be connectable to a source of deoxygenated water 140 or a source of ion exchange resin material 150. The outlet may be connectable to a drain 160 or a point of use of the ion exchange resin material 170.

[0138] 2, system 200 may include a vessel 100 having an opening 110, an inlet 120, and an outlet 130. The system may further include an oxygen monitor 210, a degasser 220, a sensor or monitor 230, and a control module 240.

[0139] As shown in Figure 3, the container 100 may have a compartment 105 configured to hold virgin ion exchange resin material and deoxygenated water. A container 180 holding a preservative or oxygen scavenging material may be disposed in the interstitial space outside of the compartment 105. An indicator 190 of oxygen contamination is visible through an observation window 195 in the container 100. The container of Figure 3 may have an inlet and an outlet (not shown) in fluid communication with the container 180. For example, the container may include an inlet or outlet in fluid communication with a liquid impermeable container holding the ion exchange resin and deoxygenated water. EXAMPLES

[0140] (Example 1: Application of a gas-impermeable container with a cationic resin) In one exemplary application, cation exchange resins used in denitrification applications have had problems with sulfate leaching from the resin prior to use. Traditionally, the resins are rinsed before being placed into service, and the rinse water is discharged into a radioactive hot well. Radioactive hot wells are limited in the amount of rinse water they can accept. Additionally, treatment of radioactive water from the hot wells is expensive.

[0141] The use of a gas-impermeable container with ion exchange resin material and deoxygenated water may, for example, allow rinsing of the ion exchange resin before use in non-hot areas of the plant without limiting the amount of rinse water produced. The rinse water may flow to a common drain and the resin may be transported by hose to a container in the radioactive area.

[0142] Example 2: Stability of stored virgin ion exchange resin material Experiments were conducted to test whether various methods would reduce or prevent degradation of ion exchange resins. After treating and storing the ion exchange resins for specified periods, the resins were tested for degradation. Organic sulfate (SO4) concentrations were measured by UV light adsorption to determine the extent of resin degradation. The results are shown in Table 1.

[0143] Experimental lots (E) were rinsed with deoxygenated water and packaged in gas impermeable containers with oxygen scavenging pouches as described above. Comparative lots (C) were processed and stored in various conventional ways.

[0144] [Table 1]

[0145] The results show a reduced rate of degradation when treating and storing ion exchange resins by the methods disclosed herein. The experimental samples exhibited significantly lower rates of SO4 increase than the comparative samples measured. Thus, the experimental samples were found to be 20-1500 times more stable when measured in comparison to conventional ion exchange resin samples. Thus, the methods disclosed herein improve the stability of ion exchange resins after extended periods of storage.

[0146] Example 3: Effect of Temperature on Stored Virgin Ion Exchange Resin Material Experiments were conducted to test the rate of degradation of ion exchange resins with increasing temperature. The ion exchange resins were tested by measuring the total organic carbon (TOC) after heating in 500 mL of water for one week while bubbling air through the solution. Table 2 shows the equivalent degradation of the ion exchange resins kept at room temperature.

[0147] [Table 2]

[0148] For every 10°C increase in temperature, the rate of degradation increased by a factor of two compared to when the ion exchange resin was kept at room temperature for the same time. Thus, temperature appears to have a detrimental effect on the rate of degradation of ion exchange resins. Thus, as disclosed herein, degradation can be reduced or prevented by refraining from increasing the temperature beyond 10°C.

[0149] (Example 4: TOC reduction test) Batch testing was conducted to determine the appropriate cleaning agent for the ion exchange resin. The samples contained 150 mL of industrial grade polystyrene-based anion exchange resin in the chloride form and sample cleaning agent (at various concentrations) in 400 mL of deionized water. The samples were stirred at 60°C and 150 rpm for 2 hours. After stirring, the ion exchange resin samples were rinsed with deionized water. The samples were scanned by UV / Vis spectroscopy at 1 and 2 hours of stirring and then tested by gas chromatography / mass spectrometry.

[0150] The detergents tested were isopropanol, ammonia, and ethoxylated octylphenol (Triton TM The oxidizers tested were X-100, available from Sigma-Aldrich, St. Louis, Missouri), ammonia peroxide (oxidizer control), ethanolamine, methanol, and sodium percarbonate. An additional control was tested with high purity deionized water. The concentrations of oxygen-containing TOC species found after treatment were added together to determine the final concentration of TOC in the resin after washing. The results are shown in the graphs in Figures 4 and 5A-C.

[0151] Briefly, as shown in Figure 4, treatment with isopropanol reduced the concentration of oxygenated TOC compared to the water control, treatment with ammonia reduced the concentration of oxygenated TOC compared to the water control, treatment with ethoxylated octylphenol produced results similar to the water control, treatment with ammonia peroxide control also produced results similar to the water control, treatment with ethanolamine slightly increased the concentration of oxygenated TOC compared to the water control, treatment with methanol slightly increased the concentration of oxygenated TOC compared to the water control, and treatment with percarbonate significantly increased the concentration of oxygenated TOC compared to the water control.

[0152] It should be noted that the concentrations tested were above the critical micelle concentration (CMC) of the particular detergent. Thus, it is believed that the ethoxylated octylphenol, ethanolamine, and methanol detergents can provide better results than the water control when used at low concentrations, e.g., below the critical micelle concentration (for detergents).

[0153] As shown in Figure 5A-C, percarbonate, isopropanol, and ethoxylated octylphenol were each tested at two concentrations for comparison. Results for cleaning formulations with 1 g and 1.91 g (2.5 g / L and 4.775 g / L, respectively) of percarbonate are shown in Figure 5A. Percarbonate is believed to increase oxidative degradation of ion exchange resins at all tested and extrapolated concentrations.

[0154] Results for wash preparations with 1 mL and 1.325 mL (0.25% and 0.33%, respectively) of isopropanol are shown in FIG. 5B. Both isopropanol concentrations tested yielded excellent results. However, lower concentrations of isopropanol yielded slightly better results. For example, when washed with 0.33% isopropanol, 0.16 μg of acetophenone was detected. When washed with 0.25% isopropanol, 0.14 μg of acetophenone was detected.

[0155] The results of cleaning preparations with 0.1 g and 0.2 g (0.25 g / L and 0.5 g / L, respectively) of ethoxylated octylphenol are shown in Figure 5C. Lower concentrations of ethoxylated octylphenol gave better results. For example, when cleaning with 0.5 g / L of ethoxylated octylphenol, 0.3 μg of acetophenone was detected. When cleaning with 0.25 g / L of ethoxylated octylphenol, 0.12 μg of acetophenone was detected. When the data shown in Figure 5C is extrapolated to a concentration of 0.05 g (0.125 g / L) of ethoxylated octylphenol, the concentration of oxygen-containing TOC is greatly reduced and almost negligible. It should be noted that 0.125 g / L of ethoxylated octylphenol is at its critical micelle concentration.

[0156] Thus, many of the detergents tested are capable of removing oxygen-containing impurities from ion exchange resins. Isopropanol and ethoxyoctylphenol provide better impurity removal at lower concentrations. In particular, ethoxyoctylphenol is believed to provide superior impurity removal below its critical micelle concentration. Based on the detergents tested, other soluble alcohols and nonionic detergents are expected to provide similar results at dilute concentrations.

[0157] The phraseology and terminology used herein are for purposes of explanation and should not be considered limiting. As used herein, the term "plurality" refers to two or more items or components. The terms "comprises," "includes," "performs," ​​"has," "contains," and "comprises," whether in the specification or claims, are open-ended terms, i.e., meaning "including, but not limited to." Thus, the use of such terms is meant to encompass the items listed thereafter and their equivalents, as well as additional items. With respect to the claims, only the transitional phrases "consisting of" and "consisting essentially of" are closed or semi-closed transitional phrases, respectively. The use of ordinal terms such as "first," "second," "third," and the like in a claim to modify a claim element does not, in and of itself, imply a priority, precedence, or order of a claim element over other elements or the chronological order in which certain procedural actions are performed, but is used only as a label to distinguish a particular named claim element from another element of the same name (but in common use of the term).

[0158] Those skilled in the art should understand that the parameters and configurations described herein are exemplary, and that the actual parameters and / or configurations will depend on the particular application in which the disclosed methods and materials are used. Those skilled in the art should also recognize, or be able to ascertain, equivalents to the specific embodiments disclosed without using more than routine experimentation. For example, those skilled in the art may recognize that the methods and components thereof according to the present disclosure may further comprise a network or system including an ion exchange resin or a gas impermeable container as disclosed herein. Accordingly, it should be understood that the embodiments described herein are presented by way of example only and are within the scope of the appended claims and their equivalents. The disclosed embodiments may be practiced in other ways than as specifically described. The present systems and methods are directed to each individual feature, system, or method described herein. Moreover, any combination of two or more such features, systems, or methods is included within the scope of the present disclosure, if such features, systems, or methods are not mutually inconsistent. The steps of the methods disclosed herein may be performed in the illustrated order or in an alternate order, and the methods may include additional or alternative acts, or may be practiced with the omission of one or more of the illustrated acts.

[0159] Further, it should be understood that various changes, modifications, and improvements will readily occur to those skilled in the art. Such changes, modifications, and improvements are intended to be part of this disclosure and are intended to be within the spirit and scope of this disclosure. In other examples, existing equipment may be modified to utilize or incorporate any one or more aspects of the methods and systems described herein. Thus, in some examples, a system may include connecting or configuring existing equipment to perform a method for reducing the rate of oxidative degradation of ion exchange resins or to contain or utilize ion exchange resins or gas impermeable containers as described herein. Thus, the foregoing description and figures are by way of example only. Furthermore, the depictions in the figures do not limit the disclosure to the specific illustrated representations.

[0160] While exemplary embodiments of the present disclosure have been disclosed, many modifications, additions, and deletions may be made thereto without departing from the spirit and scope of the disclosure and its equivalents, as set forth in the following claims.

Claims

1. 1. A method for stabilizing virgin ion exchange resin material, comprising: washing the virgin ion exchange resin material with a formulation comprising a non-ionic detergent at a concentration less than the critical micelle concentration of the non-ionic detergent measured at 25° C. and atmospheric pressure to produce a washed virgin ion exchange resin material, the non-ionic detergent consisting of ethoxylated octylphenol, the formulation comprising less than 0.125 g / L of ethoxylated octylphenol; introducing the washed virgin ion exchange resin material into a gas impermeable container; and sealing the container.

2. 10. The method of claim 1 further comprising rinsing the washed virgin ion exchange resin material with deoxygenated water.

3. 2. The method of claim 1 including the step of introducing said washed virgin ion exchange resin material into a liquid impermeable vessel of said gas impermeable vessel.

4. 10. The method of claim 1 for stabilizing virgin ion exchange resin material, comprising: and rinsing the washed virgin ion exchange resin material with deoxygenated water to produce a rinsed virgin ion exchange resin material.

5. 5. The method of claim 4, comprising rinsing the washed virgin ion exchange resin material with deoxygenated water having a concentration of dissolved oxygen less than 10 ppb.

6. 5. The method of claim 4 further comprising the steps of introducing said rinsed virgin ion exchange resin material into a gas impermeable container and sealing said container.

Citation Information

Patent Citations

  • Method for conditioning ion exchanger

    JP2003514657A

  • Method for purifying basic anion exchange resin

    JP2007313506A

  • Method for stabilizing cation exchange resins prior to use as acid catalysts and use of stabilized cation exchange resins in chemical processes

    JP2008528276A

  • Cation exchange resin and method of producing bisphenol compound

    JP2011098301A

  • Composition for regenerating an ion exchange resin

    US20020132866A1