tire

The tire design addresses high-speed cornering and fuel efficiency by using a specific rubber composition and belt layer configuration, enhancing performance through optimized contact pressure distribution.

JP7947783B2Active Publication Date: 2026-11-11SUMITOMO RUBBER INDUSTRIES LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022117374
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-07-22
Publication Date
2026-11-11
Estimated Expiration
2042-07-22

AI Technical Summary

Technical Problem

Existing tire compositions do not adequately address high-speed cornering performance and fuel efficiency, particularly in the context of modern vehicles traveling long distances at high speeds.

Method used

A tire design incorporating a tread portion with a specific rubber composition containing a multi-component copolymer and a styrene-based thermoplastic elastomer, along with a defined ratio of thermoplastic elastomer content, and a belt layer configuration that optimizes contact pressure distribution during high-speed cornering.

Benefits of technology

The tire design enhances high-speed cornering performance and reduces rolling resistance, leading to improved fuel efficiency and overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007947783000005
    Figure 0007947783000005
  • Figure 0007947783000006
    Figure 0007947783000006
  • Figure 0007947783000001
    Figure 0007947783000001
Patent Text Reader

Abstract

To provide a tire having improved total performance of high speed turning performance and low fuel consumption performance.SOLUTION: A tire has a tread part and a belt layer, wherein a rubber composition constituting the tread part contains a rubber component and a thermoplastic elastomer, the rubber component contains a multi-component copolymer having an aromatic vinyl unit and a conjugated diene unit, the thermoplastic elastomer contains a styrenic thermoplastic elastomer having an alkylene unit, in a normal state, a cross-sectional width of the tire when a normal load is applied to the tire and a tread is pressed against a plane is represented by Wt (mm), a belt layer width of the tire is represented by B (mm), and it is defined as Y=(B-16) / Wt, Y is 0.75 or less, and a ratio (X / Y) of a total content X (pts.mass) of the thermoplastic elastomer with respect to 100 pts.mass of the rubber component to Y is 3.0 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to tires. [Background technology]

[0002] In recent years, there has been a growing demand for more fuel-efficient automobiles. To meet this demand, tires are required to have low rolling resistance for improved fuel efficiency. Furthermore, there is a need to improve the overall performance of tires, including both fuel efficiency and other performance characteristics.

[0003] For example, Patent Document 1 describes how natural rubber is used as the rubber component in a tread rubber composition, and how resins and softeners are blended in larger amounts than in conventional methods, thereby suppressing an increase in rolling resistance while improving the braking performance of the tire. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] International Publication No. 2015 / 079703 [Overview of the project] [Problems that the invention aims to solve]

[0005] In recent years, with the development of expressways and improvements in vehicle performance, it has become common to travel long distances at high speeds. In this context, the aforementioned rubber compositions and tires do not take into account cornering performance at high speeds.

[0006] The present invention aims to provide a tire that improves the overall performance of high-speed cornering performance and fuel efficiency. [Means for solving the problem]

[0007] The present invention relates to a tire having a tread portion and a belt layer, The rubber composition constituting the tread portion contains a rubber component and a thermoplastic elastomer, The rubber component includes a multi-component copolymer having aromatic vinyl units and conjugated diene units, The thermoplastic elastomer includes a styrene-based thermoplastic elastomer having alkylene units, In a normal state, when the tread is pressed against a flat surface under a normal load, the cross-sectional width of the tire is defined as Wt (mm), and the belt layer width of the tire is defined as B (mm), Y=(B-16) / Wt when defined as such, Y is 0.75 or less, and the ratio (X / Y) of the total content X (parts by mass) of the thermoplastic elastomer relative to 100 parts by mass of the rubber component to Y is 3.0 or more. The present invention relates to a tire. [[ID=14】Effects of the Invention]

[0008] According to the present invention, a tire with improved overall performance of high-speed cornering performance and low fuel consumption performance is provided. Brief Description of the Drawings]

[0009] [Figure 1] It is a schematic partial cross-sectional view of a tire according to one embodiment of the present invention. [Figure 2] It is a developed view of the tread pattern on the tread surface. [[ID=33】Mode for Carrying Out the Invention]

[0010] The tire according to the present invention is a tire having a tread portion and a belt layer, wherein the rubber composition constituting the tread portion contains a rubber component and a thermoplastic elastomer, the rubber component includes a multi-component copolymer having aromatic vinyl units and conjugated diene units, the thermoplastic elastomer includes a styrene-based thermoplastic elastomer having alkylene units, and when the tread is pressed to a plane under normal conditions with a normal load applied, the cross-sectional width of the tire is Wt (mm) and the belt layer width of the tire is B (mm), and Y = (B-16) / Wt, Y is 0.75 or less, and the ratio (X / Y) of the total content X (parts by mass) of the thermoplastic elastomer to 100 parts by mass of the rubber component relative to Y is 3.0 or more. Although not intended to be theoretically bound, the mechanism by which the effects of the present invention are exerted can be considered as follows, for example.

[0011] The rubber composition constituting the tread contains (1) a multi-component copolymer having aromatic vinyl units and conjugated diene units as rubber components, which causes interactions such as π-π stacking between aromatic rings in the multi-component copolymer, improving reinforcement. Furthermore, (2) by containing a styrene-based thermoplastic elastomer having alkylene units, the alkylene units prevent contact between styrene blocks and suppress heat generation, thus reducing the amount of filler and lowering rolling resistance. In addition, (3) by satisfying the relationship (B-16) / Wt≦0.75 between the tire cross-sectional width Wt (mm) and the tire belt layer width B (mm), it is possible to suppress an excessive rise in contact pressure at the tread shoulder, thus equalizing the contact pressure of the tread during high-speed cornering, increasing the force generated across the entire contact surface, improving the road-following ability of the tread, and making it easier for the force generated at the tread to be transmitted to the inside of the tire. Furthermore, by setting the ratio of the total thermoplastic elastomer content to (4)(B-16) / Wt to ​​a predetermined value, the contact pressure of the tread increases during high-speed driving, and some of the aromatic vinyl units crystallize, making it easier to obtain reaction force during cornering. And it is believed that the combined effect of (1) to (4) above achieves a remarkable improvement in the overall performance of the tire, including high-speed cornering performance and fuel efficiency.

[0012] The glass transition temperature of the styrene-based thermoplastic elastomer having the alkylene units is preferably -30°C or lower.

[0013] It is believed that a glass transition temperature of -30°C or lower for styrene-based thermoplastic elastomers containing alkylene units can reduce the heat generation of the rubber composition, lower rolling resistance, and improve fuel efficiency.

[0014] The styrene content of the styrene-based thermoplastic elastomer having the alkylene units is preferably 20% by mass or more.

[0015] By setting the styrene content of the thermoplastic elastomer within the above range, the reinforcing properties of the rubber composition can be improved, and the filler content can be reduced, which is thought to reduce rolling resistance and improve fuel efficiency.

[0016] The aforementioned rubber composition, further measured by the BET method, has an N2SA of 170m. 2 / g super 240m 2 It is preferable that the silica content be less than / g.

[0017] N2SA is 170m 2 / g super 240m 2 By including silica at a level of less than 1g / g, the reinforcing properties of the rubber composition can be improved, and excessive heat generation can be suppressed, thus enabling both high-speed cornering performance and low fuel consumption.

[0018] The rubber composition further contains CTAB at 160m 2 / g super 210m 2 It is preferable that the silica content be less than / g.

[0019] CTAB is 160m 2 / g super 210m 2By containing silica at a content of less than / g, the reinforcing property of the rubber composition can be improved and excessive heat generation can be suppressed, so it is considered that both high-speed cornering performance and low fuel consumption performance can be achieved.

[0020] The ratio of tanδ at 70°C (70°C tanδ) to tanδ at 0°C (0°C tanδ) of the rubber composition, i.e., 70°C tanδ / 0°C tanδ, is preferably 0.05 or more and 0.80 or less.

[0021] By setting 70°C tanδ / 0°C tanδ within the above range, it is considered that the high-speed cornering performance and the low fuel consumption performance are further improved.

[0022] It is preferable that the rubber composition further contains a resin component. By containing the resin component, it is considered that the high-speed cornering performance can be improved while suppressing an increase in rolling resistance.

[0023] It is preferable that the rubber component further contains butadiene rubber.

[0024] By containing butadiene rubber, the Tg of the rubber composition does not become too low, a certain level of heat build-up can be obtained even during high-speed cornering, and it is considered that high-speed cornering performance and reduction of rolling resistance can be achieved at a high level.

[0025] The tread portion preferably includes a base rubber layer adjacent to the outer side in the tire radial direction of the belt layer, and the base rubber layer is preferably composed of a rubber composition containing a rubber component including at least one of isoprene-based rubber and butadiene rubber. By forming the tread portion with two or more layers of rubber compositions, it is considered that the high-speed cornering performance and the low fuel consumption performance are further improved.

[0026] When the tire outer diameter is defined as Dt (mm), Wt and Dt preferably satisfy the following formula (1). (π / 4)×(Dt 2 / Wt)≧1500···(1)

[0027] By setting the value of equation (1) above within the aforementioned range and reducing the width of the tread portion relative to the lateral area of ​​the tire, heat generation originating from the tread portion can be reduced. This suppresses the temperature rise caused by heat generated in the tread portion, which contributes most to heat generation in the tire, preventing the tire temperature and sidewall temperature from becoming too high, and is thought to reduce rolling resistance.

[0028] The tread portion has land areas separated by one or more circumferential grooves that extend continuously in the circumferential direction of the tire, and at least one of the land areas has an opening area of ​​0.1 to 15 mm to the tread surface. 2 It is preferable that it has one or more small holes.

[0029] The tread portion having one or more of the small holes allows water to be removed between the tread surface and the road surface when the tire makes contact with a wet road surface, making it easier to follow the road surface and improving cornering performance, especially at high speeds.

[0030] <Definition> "Thermoplastic elastomer (TPE)" refers to a thermoplastic resin material that is an elastic polymer compound, comprising a copolymer having a crystalline, high-melting-point hard segment and an amorphous, low-glass transition-temperature soft segment. In thermoplastic elastomers, the crystalline, high-melting-point hard segment acts as a pseudo-crosslinking point, exhibiting elasticity. Thermoplastic elastomers (TPEs) can be reused because the pseudo-crosslinking points can be regenerated by heating to melt the hard segment and then cooling it. On the other hand, rubber has double bonds in its molecular chains, and elasticity is exhibited by crosslinking (vulcanizing) it with sulfur, etc., to create a three-dimensional network structure. Therefore, once rubber is crosslinked (vulcanized), it loses its fluidity due to this three-dimensional network structure, making it difficult to reuse even when heated. The thermoplastic elastomer (TPE) of the present invention is defined as not containing the above-mentioned rubber components.

[0031] An "aromatic vinyl unit" is a monomeric unit derived from aromatic vinyl compounds.

[0032] A "regular rim" is the rim specified for each tire in the standards system that the tire is based on. For example, it is called a "standard rim" for JATMA, a "design rim" for TRA, and a "measuring rim" for ETRTO. Refer to JATMA, ETRTO, and TRA in that order, and if an applicable size is found at the time of reference, follow that standard. In the case of a tire size not specified in the aforementioned standards system, it refers to the narrowest rim with the smallest diameter that can be mounted on that tire without causing air leakage between the rim and tire.

[0033] "Regular internal pressure" refers to the air pressure specified for each tire by the tire standard, which is part of the tire standard system on which the tire is based. For example, it is the "maximum air pressure" for JATMA, the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES" for TRA, and "INFLATION PRESSURE" for ETRTO. For tires not specified in any standard, the regular internal pressure is 250kPa.

[0034] "Normal condition" refers to a tire mounted on a normal rim, filled to the normal internal pressure, and under no load. In the case of tires of sizes not specified in the aforementioned standard system, it refers to a tire mounted on the smallest rim, filled to 250 kPa, and under no load. Unless otherwise specified in this specification, the dimensions of each part of the tire (tire section width Wt, etc.) are measured under the normal condition.

[0035] "Regular load" refers to the load specified in the standards system, including the standard on which the tire is based. The "maximum load capacity" in the JATMA standard, the "maximum value" listed in "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES" in the TRA standard, and the "LOAD CAPACITY" in the ETRTO standard are all considered regular loads.

[0036] "Tire section width Wt" refers to the maximum width of the tire section in its normal state. However, if there are patterns or letters on the tire sidewall, these are excluded, and it is the maximum width between the outer surfaces of the sidewalls. Alternatively, it can be measured by cutting the tire in a plane containing the tire's axis of rotation, and determining the maximum straight distance in the width direction of the cross section, excluding letters and other markings on the sidewall, with the bead portion aligned to the normal rim width.

[0037] "Tire belt layer width B" refers to the maximum length in the width direction of the tire's belt layer in its normal state. Simply put, similar to the tire cross-sectional width Wt described above, it can be measured by determining the straight-line distance in the width direction between the endpoints of the belt layer in a cross-section obtained by cutting the tire in a plane containing the tire's rotation axis, with the bead sections aligned to the normal rim width. If the belt layer consists of multiple layers, the longest of these layers is considered the "total tire belt width B".

[0038] "Tire outer diameter Dt" refers to the diameter of the tire in its normal state.

[0039] "Small holes" are tiny holes present on the tread surface, extending from the inside of the tread and opening onto the tread surface. Each small hole exists independently and does not communicate with circumferential grooves, lateral grooves, etc.

[0040] <Measurement method> The glass transition temperature (Tg) of thermoplastic elastomers is measured according to JIS K 7121 using a differential scanning calorimeter (Q200) manufactured by T.A. Instruments Japan Co., Ltd., under a heating rate of 10°C / min. The glass transition temperature (Tg) of rubber components is measured in the same manner.

[0041] "Aromatic vinyl unit amount" is, 1 It is calculated by 1H-NMR measurement. For example, it is applied to the content of aromatic vinyl compounds in conjugated diene polymers. "Styrene content" is, 1 It is calculated by 1H-NMR measurement. For example, it is applied to styrene-based thermoplastic elastomers and styrene-containing rubbers.

[0042] The "vinyl bond content (amount of 1,2-bonded butadiene units)" is measured by infrared absorption spectroscopy. This method is applied, for example, to styrene-butadiene rubber, butadiene rubber, etc.

[0043] "Cis content (amount of cis-1,4-bonded butadiene units)" is a value calculated by infrared absorption spectroscopy in accordance with JIS K 6239-2:2017, and is applied to rubber components having repeating units derived from butadiene, such as butadiene rubber.

[0044] The "weight-average molecular weight (Mw)" can be determined by converting it to standard polystyrene based on measurements obtained by gel permeation chromatography (GPC) (for example, the GPC-8000 series from Tosoh Corporation, with a differential refractometer as the detector and TSKGEL SUPERMALTIPORE HZ-M column from Tosoh Corporation). This method is applicable, for example, to rubber components, thermoplastic elastomers, resin components, etc.

[0045] The "average primary particle size of carbon black" can be determined by observing with a transmission or scanning electron microscope, measuring 400 or more primary particles of carbon black observed within the field of view, and averaging the results. The "N2SA of carbon black" is measured in accordance with JIS K 6217-2:2017.

[0046] The "average primary particle size of silica" can be determined by observing with a transmission or scanning electron microscope, measuring 400 or more primary silica particles observed within the field of view, and averaging the results. The "CTAB (cetyltrimethylammonium bromide) specific surface area of ​​silica" is measured according to ASTM D3765-92. The "N2SA of silica" is measured by the BET method according to ASTM D3037-93.

[0047] "tanδ at 70°C (70°C tanδ)" is the loss tangent measured using a dynamic viscoelasticity measuring device (e.g., the Iplexer series from GABO) under conditions of 70°C, 10Hz frequency, and 1% dynamic strain amplitude. The sample for loss tangent measurement is a vulcanized rubber composition measuring 20mm in length, 4mm in width, and 1mm in thickness. When preparing the sample by cutting it from a tire, it should be cut from the tire tread so that the tire circumference is the longer side and the tire radius is the thickness direction.

[0048] "tanδ at 0°C (0°C tanδ)" is the loss loss tangent measured using a dynamic viscoelasticity measuring instrument (e.g., the Iplexer series from GABO) under the conditions of 0°C temperature, 10% initial strain, 2.5% dynamic strain, and 10 Hz frequency. The sample for this measurement is prepared in the same manner as for 70°C tanδ.

[0049] The "softening point of the resin component" is the temperature at which the sphere drops when the softening point specified in JIS K 6220-1:2001 is measured using a ring-type softening point measuring device.

[0050] ≪Tires≫ A tire, which is one embodiment of the present invention, will be described in detail below with reference to the drawings. However, the following description is illustrative for explaining the present invention and is not intended to limit the technical scope of the present invention to this scope only. In this specification, when a numerical range is indicated using "~", it includes the numerical values ​​at both ends of the range.

[0051] <Tire dimensions> Figure 1 is a cross-sectional view showing a part of the tire according to the present invention. The vertical direction is the radial direction of the tire, the horizontal direction is the tire width direction, and the direction perpendicular to the plane of the paper is the tire circumferential direction.

[0052] The cross-sectional width Wt of the tire of the present invention is preferably 125 mm or more, more preferably 150 mm or more, and even more preferably 175 mm or more. Furthermore, the cross-sectional width Wt of the tire is preferably less than 305 mm, more preferably less than 245 mm, and even more preferably less than 210 mm.

[0053] The belt layer width B is preferably 120 mm or more, more preferably 130 mm or more, even more preferably 140 mm or more, and particularly preferably 150 mm or more. Furthermore, the belt layer width B is preferably less than 205 mm, more preferably less than 200 mm, even more preferably less than 190 mm, even more preferably less than 180 mm, and particularly preferably less than 170 mm.

[0054] The present invention is characterized in that, in a normal state, when the tread is pressed against a plane under a normal load, the cross-sectional width of the tire is Wt (mm) and the belt layer width of the tire is B (mm), and Y = (B-16) / Wt is defined as Y being 0.75 or less.

[0055] From the viewpoint of the effects of the present invention, the value of Y is preferably 0.74 or less, more preferably 0.73 or less, and even more preferably 0.72 or less. The lower limit of Y is not particularly limited, but is preferably 0.50 or more, more preferably 0.60 or more, and even more preferably 0.65 or more.

[0056] In the present invention, the ratio (X / Y) of the total content X (parts by mass) of thermoplastic elastomer to 100 parts by mass of rubber component in the rubber composition constituting the tread portion relative to Y is 3.0 or more, preferably 5.0 or more, more preferably 8.0 or more, even more preferably 10.0 or more, even more preferably 12.0 or more, even more preferably 14.0 or more, even more preferably 18.0 or more, even more preferably 20.0 or more, even more preferably 25.0 or more, even more preferably 28.0 or more, even more preferably 30.0 or more, and even more preferably 35.0 or more. Furthermore, the upper limit of X / Y is preferably 100 or less, more preferably 94 or less, and even more preferably 67 or less. The total content X (parts by mass) of thermoplastic elastomer relative to 100 parts by mass of rubber component will be described later.

[0057] The outer diameter Dt of the tire is preferably 585 mm or more, more preferably 600 mm or more, and even more preferably 625 mm or more. Furthermore, the outer diameter Dt of the tire is preferably less than 843 mm, more preferably less than 725 mm, and even more preferably less than 685 mm.

[0058] In the present invention, when the tire section width is Wt (mm) and the tire outer diameter is Dt (mm), it is preferable that Wt and Dt satisfy the following formula (1). (π / 4) × (Dt 2 / Wt)≧1500 ···(1)

[0059] Here, as Dt increases, the value of equation (1) increases, and conversely, as Dt decreases, the equivalent value decreases. On the other hand, as Wt increases, the value of equation (1) decreases, and conversely, as Wt decreases, the equivalent value increases. Focusing on this point, we can adjust Dt and Wt so that they satisfy equation (1).

[0060] The value of formula (1) is preferably 1500 or more, more preferably 1520 or more, and even more preferably 1525 or more. Furthermore, there is no particular upper limit to the value of formula (1), but it is preferably 2800 or less, more preferably 2700 or less, and even more preferably 2600 or less.

[0061] Examples of tire sizes that satisfy equation (1) include 125 / 65R19, 145 / 60R18, 145 / 60R19, 155 / 55R18, 155 / 55R19, 155 / 70R17, 155 / 70R19, 165 / 55R20, 165 / 55R21, 165 / 60R19, 165 / 65R19, 165 / 70R18, 175 / 55R19, 175 / 55R20, 175 / 55R22, 175 / 60R18, 185 / 55R19, 185 / 60R20, 195 / 50R20, 195 / 55R20, 205 / 55R16, 195 / 65R15, 205 / 55R16, etc.

[0062] <Tread structure> The tread portion of the tire shown in Figure 1 comprises a base rubber layer 6 adjacent to the radially outer side of the belt layer 3. The tire of the present invention preferably comprises a base rubber layer 6 adjacent to the radially outer side of the belt layer 3. The cap rubber layer 4 may have two or more layers, and there may be one or more additional rubber layers between the cap rubber layer 4 and the base rubber layer 6, as long as the objective of the present invention is achieved.

[0063] <Tread Pattern> Figure 2 is an unfolded view of the tread pattern of the tread surface. In Figure 2, the tread surface 10 constituting the tire has, as shown in Figure 2, a circumferential groove 1 that extends continuously in the tire circumferential direction C (in the example of Figure 2, it extends linearly along the tire circumferential direction), and transverse grooves 21 and sipes 22, 23 that extend in the width direction. The tire of the present invention preferably has circumferential grooves.

[0064] In Figure 2, three circumferential grooves 1 are provided, but the number of circumferential grooves is not particularly limited and may be, for example, two to five. Furthermore, the circumferential grooves 1 are not limited to this configuration and may extend in a wavy, sinusoidal, or zigzag pattern along the circumferential direction.

[0065] In Figure 2, the tread surface 10 has a land area 2 separated by a plurality of circumferential grooves 1 in the tire width direction W. It is preferable that the tread surface 10 is provided with lateral grooves (widthwise grooves) and / or sipes. In Figure 2, the land area 2 is provided with a plurality of shoulder lateral grooves 21 whose ends open into the circumferential grooves 1, a plurality of shoulder sipes 22 whose one end opens into the circumferential grooves 1, and a plurality of center sipes 23 whose one end opens into the circumferential grooves 1.

[0066] The land portion 2 preferably has one or more small holes. In Figure 2, there are two small holes 24 in each portion of the land portion separated by adjacent center sipes 23. The opening area of ​​the small holes to the tread surface is 0.1 to 15 mm². 2 Preferably, 0.5 to 10 mm 2 More preferably, 1.0 to 7.0 mm 2 More preferably, 1.5 to 5.0 mm 2 This is particularly preferable. By providing small holes with the aforementioned opening area, when the tire makes contact with a wet road surface, water can be removed between the tread surface and the road surface, making it easier to follow the road surface and improving cornering performance, especially at high speeds. Furthermore, since it is possible to increase the surface area of ​​the tread without adversely affecting other performance, it is thought that heat dissipation in the tread area will improve, and the temperature rise in the tire and sidewall will be suppressed.

[0067] In this specification, "groove," including circumferential grooves and widthwise grooves, refers to a recess with a width of at least 2.0 mm. On the other hand, in this specification, "sipe" refers to a narrow cut with a width of 2.0 mm or less, preferably 0.5 to 1.5 mm.

[0068] [Physical properties of rubber compositions] From the viewpoint of the effects of the present invention, the 0°C tanδ of the rubber composition constituting the tread portion of the tire of the present invention (hereinafter referred to as the "rubber composition according to the present invention") is preferably greater than 0.25, more preferably greater than 0.28, even more preferably greater than 0.30, and particularly preferably greater than 0.32. Furthermore, from the viewpoint of reducing heat generation during driving and improving fuel efficiency, the 0°C tanδ of the rubber composition of the present invention is preferably less than 1.50, more preferably less than 1.40, even more preferably less than 1.30, even more preferably less than 1.20, and particularly preferably less than 1.10. Note that the 0°C tanδ of the rubber composition can be appropriately adjusted depending on the type and amount of rubber components, plasticizers, etc.

[0069] From the viewpoint of the effects of the present invention, the 70°C tanδ of the rubber composition according to the present invention is preferably greater than 0.08, more preferably greater than 0.10, even more preferably greater than 0.11, and particularly preferably greater than 0.12. Furthermore, from the viewpoint of reducing heat generation during driving and improving fuel efficiency, the 70°C tanδ of the rubber composition according to the present invention is preferably less than 0.45, more preferably less than 0.42, even more preferably less than 0.39, even more preferably less than 0.36, and particularly preferably less than 0.33.

[0070] The values ​​of 0°C tanδ and 70°C tanδ can be adjusted by conventional methods in the tire industry. For example, the value of 70°C tanδ can be decreased by reducing the filler content, and conversely, it can be increased by increasing it. Therefore, those skilled in the art can appropriately adjust the value of 70°C tanδ according to the target 70°C tanδ.

[0071] In the rubber composition according to the present invention, the ratio of 70°C tanδ to 0°C tanδ (70°C tanδ / 0°C tanδ) is preferably 1.80 or less, and more preferably 1.50 or less. 、 More preferably 1.00 or less, even more preferably 0.80 or less, even more preferably 0.75 or less, and 0.70 or less. underThis is particularly preferable. Furthermore, from the viewpoint of the effects of the present invention, the lower limit of 70°C tanδ / 0°C tanδ is preferably 0.05 or higher, more preferably 0.07 or higher, and even more preferably 0.10 or higher.

[0072] [Rubber composition formulation] The rubber composition according to the present invention contains a rubber component and a thermoplastic elastomer. The rubber component includes a polypolymer having aromatic vinyl units and conjugated diene units, and the thermoplastic elastomer includes a styrene-based thermoplastic elastomer having alkylene units.

[0073] <Rubber components> Suitable rubber components used in the production of the rubber composition according to the present invention include a polypolymer having aromatic vinyl units and conjugated diene units, butadiene rubber (BR), and isoprene-based rubber. Furthermore, if the rubber composition according to the present invention comprises a base rubber layer, it is preferable that the rubber components of the rubber composition constituting the base rubber layer include at least one of isoprene-based rubber and BR.

[0074] Examples of polypolymers having aromatic vinyl units and conjugated diene units include styrene-butadiene rubber (SBR), styrene-isoprene-butadiene rubber (SIBR), and styrene-isoprene rubber (SIR), with SBR being preferred. There are no particular limitations on SBR, and examples include solution-polymerized SBR (S-SBR), emulsion-polymerized SBR (E-SBR), and modified SBRs thereof (modified S-SBR, modified E-SBR). Modified SBRs include SBRs with modified terminals and / or main chains, and modified SBRs coupled with tin, silicon compounds, etc. (condensates, those with branched structures, etc.). Among these, S-SBR and modified SBRs are preferred. Furthermore, hydrogenated versions of these SBRs (hydrogenated SBRs) can also be used. These SBRs may be used individually or in combination of two or more types.

[0075] As for SBR, either stretchable SBR or non-stretchable SBR can be used. When stretchable SBR is used, the amount of stretchable SBR, that is, the amount of stretchable plasticizer contained in the SBR, is preferably 10 to 50 parts by mass per 100 parts by mass of rubber solids in the SBR.

[0076] S-SBRs that can be used in this invention are commercially available from companies such as JSR Corporation, Sumitomo Chemical Co., Ltd., Ube Industries, Ltd., Asahi Kasei Corporation, and ZS Elastomer Co., Ltd.

[0077] Modified SBR may be one in which the main chain and / or terminals are modified with a modifying agent, or it may be modified with a polyfunctional modifying agent such as tin tetrachloride or silicon tetrachloride and have a partially branched structure, but SBR modified with a modifying agent having functional groups that interact with silica in the main chain and / or terminals (silica-modified SBR) is preferred. It is particularly preferable to contain modified SBR in the first layer and / or second layer.

[0078] Examples of functional groups that interact with silica include amino groups, amide groups, alkoxysilyl groups, isocyanate groups, imino groups, imidazole groups, urea groups, ether groups, carbonyl groups, oxycarbonyl groups, sulfide groups, disulfide groups, sulfonyl groups, sulfinyl groups, thiocarbonyl groups, ammonium groups, imide groups, hydrazo groups, azo groups, diazo groups, carboxyl groups, nitrile groups, pyridyl groups, alkoxy groups, hydrocarbon groups, hydroxyl groups, oxy groups, and epoxy groups. These functional groups may have substituents. Among these, amino groups, epoxy groups, hydroxyl groups, alkoxy groups, and alkoxysilyl groups are preferred from the viewpoint of improving the dispersibility of silica, and amino groups and alkoxysilyl groups are more preferred.

[0079] In a multi-component polymer having aromatic vinyl units and conjugated diene units, the amount of aromatic vinyl units is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, from the viewpoint of high-speed swirling performance. Furthermore, from the viewpoint of temperature dependence of grip performance and blow resistance, it is preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 50% by mass or less. In this specification, the styrene content is determined by the measurement method described above.

[0080] The vinyl content of a multi-component polymer having aromatic vinyl units and conjugated diene units is preferably 10 mol% or more, more preferably 15 mol% or more, and even more preferably 20 mol% or more, from the viewpoint of ensuring reactivity with silica, wet grip performance, rubber strength, and abrasion resistance. Furthermore, the vinyl content of SBR is preferably 70 mol% or less, more preferably 65 mol% or less, and even more preferably 60 mol% or less, from the viewpoint of preventing increased temperature dependence, elongation at break, and abrasion resistance. The vinyl content (amount of 1,2-bonded butadiene units) is determined by the measurement method described above.

[0081] The weight-average molecular weight (Mw) of the multi-component polymer having aromatic vinyl units and conjugated diene units is preferably 200,000 or more, more preferably 250,000 or more, and even more preferably 300,000 or more, from the viewpoint of wet grip performance. Furthermore, from the viewpoint of crosslinking uniformity, the weight-average molecular weight is preferably 2,000,000 or less, more preferably 1,800,000 or less, and even more preferably 1,500,000 or less. The weight-average molecular weight of the multi-component polymer having aromatic vinyl units and conjugated diene units is determined by the measurement method described above.

[0082] From the viewpoint of low fuel consumption performance, the content of the polypolymer having aromatic vinyl units and conjugated diene units in the rubber component of the rubber composition according to the present invention is preferably 50% by mass or more, more preferably 55% by mass or more, even more preferably 60% by mass or more, even more preferably 65% ​​by mass or more, even more preferably 70% by mass or more, even more preferably 75% by mass or more, and particularly preferably 80% by mass or more. Furthermore, there is no particular upper limit to the content of the polypolymer having aromatic vinyl units and conjugated diene units in the rubber component; for example, it can be 90% by mass or less, 95% by mass or less, or even 100% by mass, i.e., the rubber component can consist only of the polypolymer having aromatic vinyl units and conjugated diene units.

[0083] (BR) BR is not particularly limited, and for example, BR with a cis content of less than 50 mol% (low-cis BR), BR with a cis content of 90 mol% or more (high-cis BR), rare-earth butadiene rubber synthesized using a rare-earth element catalyst (rare-earth BR), BR containing syndiotactic polybutadiene crystals (SPB-containing BR), modified BR (high-cis modified BR, low-cis modified BR), etc., which are common in the tire industry, can be used. These BRs may be used individually or in combination of two or more types.

[0084] High-cis BR can be commercially available from companies such as Nippon Zeon Co., Ltd., Ube Industries, Ltd., and JSR Corporation. Including high-cis BR can improve low-temperature properties and wear resistance. The cis content is preferably 95 mol% or more, more preferably 96 mol% or more, even more preferably 97 mol% or more, and particularly preferably 98 mol% or more. In this specification, the cis content (amount of cis-1,4-bonded butadiene units) is a value calculated by infrared absorption spectroscopy.

[0085] Rare earth-based BR is synthesized using a rare earth element catalyst, and has a vinyl content of preferably 1.8 mol% or less, more preferably 1.0 mol% or less, and even more preferably 0.8 mol or less, and a cis content of preferably 95 mol% or more, more preferably 96 mol% or more, even more preferably 97 mol% or more, and particularly preferably 98 mol% or more. As rare earth-based BR, commercially available products from companies such as Lanxess can be used.

[0086] SPB-containing BR refers to a type in which 1,2-syndiotactic polybutadiene crystals are not simply dispersed in BR, but are chemically bonded to and dispersed in BR. Such SPB-containing BR can be commercially available from companies such as Ube Industries, Ltd.

[0087] Modified BRs include those obtained by polymerizing 1,3-butadiene with a lithium initiator and then adding a tin compound, with the ends of the modified BR molecule being linked by tin-carbon bonds (tin-modified BR), and butadiene rubber modified with a modifying agent having functional groups that interact with silica on the main chain and / or ends of the butadiene rubber (silica-modified BR). Furthermore, the modified BR may be either unhydrogenated or hydrogenated.

[0088] From the viewpoint of wear resistance, the weight-average molecular weight (Mw) of BR is preferably 300,000 or more, more preferably 350,000 or more, and even more preferably 400,000 or more. From the viewpoint of crosslinking uniformity, it is preferably 2,000,000 or less, and more preferably 1,000,000 or less. The weight-average molecular weight of BR is measured by the measurement method described above.

[0089] When BR is included as a rubber component, its content in the rubber component is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 25% by mass or less, from the viewpoint of increasing the amount of the multi-component polymer having aromatic vinyl units and conjugated diene units. Furthermore, there is no particular lower limit to the content when BR is included, but for example, it can be 1% by mass or more, 3% by mass or more, 5% by mass or more, 10% by mass or more, or 15% by mass or more.

[0090] (Isoprene rubber) As isoprene-based rubbers, for example, isoprene rubber (IR) and natural rubber, which are common in the tire industry, can be used. Natural rubber includes not only unmodified natural rubber (NR), but also modified natural rubbers such as epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), deproteinized natural rubber (DPNR), high-purity natural rubber, and grafted natural rubber. These isoprene-based rubbers may be used individually or in combination of two or more types.

[0091] NR is not particularly limited and can use any tire that is common in the tire industry, such as SIR20, RSS#3, and TSR20.

[0092] When isoprene-based rubber is included as a rubber component, its content in the rubber component is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 20% by mass or less, from the viewpoint of increasing the amount of a multi-component polymer having aromatic vinyl units and conjugated diene units. Furthermore, there is no particular lower limit to the content when isoprene-based rubber is included, but for example, it can be 1% by mass or more, 3% by mass or more, 5% by mass or more, 10% by mass or more, or 15% by mass or more.

[0093] (Other rubber components) The rubber component according to the present invention may include rubber components other than the aforementioned multipolymer having aromatic vinyl units and conjugated diene units, BR, and isoprene-based rubber. Other rubber components that can be crosslinked are commonly used in the tire industry, and examples include chloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), hydrogenated nitrile rubber (HNBR), butyl rubber (IIR), ethylene propylene rubber, polynorbornene rubber, silicone rubber, polyethylene chloride rubber, fluororubber (FKM), acrylic rubber (ACM), and hydrin rubber. These other rubber components may be used individually or in combination of two or more.

[0094] Thermoplastic elastomer (TPE) The rubber composition according to the present invention contains a thermoplastic elastomer (TPE). Examples of thermoplastic elastomers (TPEs) include styrene-based thermoplastic elastomers, urethane-based thermoplastic elastomers, olefin-based thermoplastic elastomers, polyester-based thermoplastic elastomers, and polyamide-based thermoplastic elastomers. One or more types of thermoplastic elastomers (TPEs) can be used.

[0095] (Styrene-based thermoplastic elastomer) The rubber composition according to the present invention contains a styrene-based thermoplastic elastomer. The styrene-based thermoplastic elastomer is a copolymer having at least one styrene block (hard segment) and at least one elastomer block (soft segment). The molecular structure of the styrene-based thermoplastic elastomer is not particularly limited, but it is preferable to have a molecular structure in which styrene blocks are present at one or both ends and elastomer blocks elsewhere. Having a styrene block at at least one end tends to result in better grip performance. Furthermore, it is more preferable that the styrene-based thermoplastic elastomer does not have styrene blocks in the main chain portion other than the ends. With such a structure, the hardness of the thermoplastic elastomer in the room temperature range does not become too high, and better fracture characteristics and twisting performance tend to be obtained.

[0096] Examples of styrene-based thermoplastic elastomers include styrene-isobutylene block copolymer (SIB), styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), styrene-ethylene-butylene block copolymer (SEB), styrene-ethylene-propylene block copolymer (SEP), styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-ethylene-butylene-ethylene block copolymer (SEBC), hydrogenated styrene-butadiene copolymer (HSBR), styrene-ethylene-propylene-styrene block copolymer (SEPS), styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS), styrene-butadiene-butylene-styrene block copolymer (SBBS), and styrene-alkylene block copolymer.

[0097] The styrene-based thermoplastic elastomer contained in the rubber composition according to the present invention has alkylene units. Examples of alkylene units include methylene, ethylene, propylene, and butylene. Specifically, examples of elastomer blocks include vinyl-polydienes such as styrene-butadiene (SB), polyisoprene (IP), polybutadiene, polyethylene, polychloroprene, and poly2,3-dimethylbutadiene. Furthermore, hydrogenated elastomer blocks may also be used.

[0098] The glass transition temperature (Tg) of a styrene-based thermoplastic elastomer containing alkylene units is preferably -20°C or lower, more preferably -30°C or lower, and even more preferably -35°C or lower, from the viewpoint of lowering the tanδ of the rubber composition and reducing rolling resistance. There is no particular upper limit to the glass transition temperature (Tg) of a styrene-based thermoplastic elastomer containing alkylene units, but it is usually -60°C or higher.

[0099] The styrene content (styrene unit content) of the styrene-based thermoplastic elastomer having alkylene units is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more, from the viewpoint of high-speed turning performance. Furthermore, from the viewpoint of suppressing heat generation, it is preferably 75% by mass or less, more preferably 70% by mass or less, and even more preferably 65% ​​by mass or less.

[0100] The rubber composition according to the present invention contains a styrene-based thermoplastic elastomer having alkylene units, and may also contain thermoplastic elastomers other than the styrene-based thermoplastic elastomer having alkylene units.

[0101] (Urethane-based thermoplastic elastomer) The urethane-based thermoplastic elastomer is not particularly limited, but for example, those prepared from polyols and diisocyanates can be suitably used. Examples of polyols include polyester polyols, polyester ether polyols, polycarbonate polyols, and polyether polyols. Examples of diisocyanates include tolylene diisocyanate (TDI) and 4,4'-diphenylmethane diisocyanate (MDI).

[0102] (Olefin-based thermoplastic elastomer) Examples of olefin-based thermoplastic elastomers include ethylene-α-olefin copolymers such as ethylene-propylene copolymer (EPR), ethylene-butene copolymer (EBR), ethylene-hexene copolymer (EHR), and ethylene-octene copolymer (EOR); and ethylene-α-olefin-diene ternary copolymers such as ethylene-propylene-ethylidene norbornene copolymer, ethylene-propylene-butadiene copolymer, and ethylene-propylene-isoprene copolymer.

[0103] Thermoplastic elastomers (TPEs) may be hydrogenated. Examples of hydrogenated thermoplastic elastomers include hydrogenated styrene-based thermoplastic elastomers.

[0104] Thermoplastic elastomers (TPEs) can also be modified with a modifying agent to introduce a modifying group, if desired. Any of the modifying groups commonly used in this field can be suitably used, such as alkoxysilyl groups (e.g., trimethoxysilyl group, triethoxysilyl group). For example, by synthesizing a styrene-based thermoplastic elastomer having a styrene terminus at least one end, and then treating it with chlorotriethoxysilane as a modifying agent, a modified styrene-based thermoplastic elastomer can be obtained in which a triethoxysilyl group is introduced at the active end of the styrene-based thermoplastic elastomer.

[0105] As the thermoplastic elastomer (TPE), either a commercially available product or one obtained through synthesis may be used. Examples of commercially available products include those manufactured and sold by JSR Corporation, Asahi Kasei Corporation, Kuraray Co., Ltd., and Nippon Miractran Co., Ltd.

[0106] The amount of thermoplastic elastomer (TPE) X (parts by mass) per 100 parts by mass of rubber component is preferably more than 5 parts by mass, more preferably more than 9 parts by mass, even more preferably 10 parts by mass or more, even more preferably more than 15 parts by mass, even more preferably more than 20 parts by mass, and particularly preferably 30 parts by mass or more, from the viewpoint of reducing rolling resistance and improving fuel efficiency. Furthermore, the amount of thermoplastic elastomer X (parts by mass) is preferably less than 100 parts by mass, more preferably less than 90 parts by mass, even more preferably less than 80 parts by mass, and particularly preferably less than 70 parts by mass, from the viewpoint of wear resistance.

[0107] <Filler> The rubber composition according to the present invention preferably contains a filler, which preferably contains carbon black or silica, more preferably silica, and even more preferably both silica and carbon black.

[0108] (Carbon Black) The carbon black used is not particularly limited and can be any that is common in the tire industry, such as GPF, FEF, HAF, ISAF, SAF, etc. Specifically, N110, N115, N120, N125, N134, N135, N219, N220, N231, N234, N293, N299, N326, N330, N339, N343, N347, N351, N356, N358, N375, N539, N550, N582, N630, N642, N650, N660, N683, N754, N762, N765, N772, N774, N787, N907, N908, N990, N991, etc. can be suitably used, as can other proprietary synthetic products. These can be used individually or in combination of two or more types.

[0109] The nitrogen adsorption specific surface area (N2SA) of carbon black is 50m², considering weather resistance and reinforcement properties. 2 Preferably 80m / g or more. 2 More preferably 100m / g or more, 2 A value of 250m or more is even more preferable. Furthermore, from the viewpoint of dispersibility, reduced rolling resistance, fracture characteristics, and durability, 250m is preferable. 2 Preferably less than / g, 220m 2 A value of less than / g is more preferable. The N2SA of carbon black in this specification can be measured by the measurement method described above.

[0110] When carbon black is included, the content per 100 parts by mass of rubber component is preferably more than 1 part by mass, more preferably more than 3 parts by mass, and even more preferably more than 4 parts by mass, from the viewpoint of weather resistance and reinforcing properties. Furthermore, from the viewpoint of reducing heat generation and rolling resistance, it is preferably less than 30 parts by mass, more preferably less than 20 parts by mass, and even more preferably less than 10 parts by mass.

[0111] (silica) By incorporating silica into the rubber composition according to the present invention, rolling resistance can be reduced and fuel efficiency can be improved. The silica used is not particularly limited; for example, silica prepared by a dry process (anhydrous silica) or silica prepared by a wet process (hydrated silica), which are common in the tire industry, can be used. Among these, hydrated silica prepared by a wet process is preferred because it contains a large number of silanol groups. Silica may be used alone or in combination of two or more types. Furthermore, in addition to silica made from hydrated silica, silica made from biomass materials such as rice husks may also be used.

[0112] The nitrogen adsorption specific surface area (N2SA) of silica, measured by the BET method, is 150 m² in terms of elongation at break. 2 Preferably more than / g, 170m 2 More preferably than / g, 200m 2 A value greater than / g is even more preferable. Also, from the viewpoint of reducing rolling resistance and processability, 300m 2Less than / g is preferable, 250m 2 Less than / g is more preferable, 240m 2 Less than / g is even more preferable, 236m 2 A value of less than / g is even more preferable. The N2SA content of silica can be measured by the measurement method described above.

[0113] The specific surface area of ​​silica CTAB (cetyltrimethylammonium bromide) (hereinafter referred to as silica CTAB) is 150 m² from the viewpoint of dispersibility. 2 Preferably more than / g, 160m 2 More preferably than / g, 170m 2 More preferably than / g, 190m 2 A concentration of more than / g is even more preferable. Furthermore, the silica CTAB is 350m from the viewpoint of silica dispersibility in the rubber phase. 2 Less than / g is preferable, 300m 2 Less than / g is more preferable, 250m 2 It is even more preferable that the amount be less than / g, and 210m 2 A value of less than / g is particularly preferred. The CTAB of silica is measured by the measurement method described above.

[0114] The average primary particle diameter of silica is preferably 20 nm or less, more preferably 18 nm or less, and even more preferably 17 nm or less. While there is no particular lower limit to the average primary particle diameter, from the viewpoint of silica dispersibility, it is preferably 1 nm or more, more preferably 3 nm or more, and even more preferably 5 nm or more. By having the average primary particle diameter of silica within the above range, the dispersibility of silica can be further improved, and the reinforcing properties, fracture characteristics, and wear resistance can be further improved. The average primary particle diameter of silica can be determined by the measurement method described above.

[0115] When silica is included, the silica content per 100 parts by mass of rubber component is preferably more than 40 parts by mass, more preferably more than 50 parts by mass, and more preferably more than 60 parts by mass, from the viewpoint of reducing rolling resistance. Furthermore, from the viewpoint of suppressing the increase in rolling resistance due to the deterioration of silica's dispersibility in rubber, it is preferably less than 150 parts by mass, more preferably less than 140 parts by mass, and even more preferably less than 130 parts by mass.

[0116] (Other fillers) Other fillers besides carbon black and silica can be added, including aluminum hydroxide, calcium carbonate, alumina, clay, talc, and other materials commonly used in the tire industry.

[0117] (Silane coupling agent) Silica is preferably used in combination with a silane coupling agent. The silane coupling agent is not particularly limited, and any silane coupling agent that has conventionally been used in combination with silica in the tire industry can be used, for example: mercapto-based silane coupling agents such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, and 2-mercaptoethyltriethoxysilane; sulfide-based silane coupling agents such as bis(3-triethoxysilylpropyl) disulfide and bis(3-triethoxysilylpropyl) tetrasulfide; 3-octanoylthio-1-propyltriethoxysilane, 3-hexanoylthio-1-propyltriethoxysilane, and 3-octanoylthio-1-propyltrimethoxysilane. Examples include thioester silane coupling agents such as lan; vinyl silane coupling agents such as vinyltriethoxysilane and vinyltrimethoxysilane; amino silane coupling agents such as 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and 3-(2-aminoethyl)aminopropyltriethoxysilane; glycidoxy silane coupling agents such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro silane coupling agents such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro silane coupling agents such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Among these, it is preferable to contain a sulfide silane coupling agent and / or a mercapto silane coupling agent. As silane coupling agents, for example, those commercially available from Momentive, etc., can be used. These silane coupling agents may be used individually or in combination of two or more.

[0118] When a silane coupling agent is included, its content per 100 parts by mass of the rubber component is preferably more than 3.0 parts by mass, more preferably more than 4.0 parts by mass, and even more preferably more than 5.0 parts by mass. Furthermore, the content of the silane coupling agent is preferably less than 20 parts by mass, more preferably less than 15 parts by mass, and even more preferably less than 10 parts by mass.

[0119] When a silane coupling agent is included, its content per 100 parts by mass of silica is preferably 0.5 parts by mass or more, more preferably 1.0 part by mass or more, even more preferably 2.0 parts by mass or more, and particularly preferably 3.0 parts by mass or more, in order to react with the silica. Furthermore, from the viewpoint of preventing a decrease in wear resistance, the content of the silane coupling agent per 100 parts by mass of silica is preferably less than 20 parts by mass, more preferably less than 15 parts by mass, and even more preferably less than 10 parts by mass.

[0120] (Other combination drugs) In addition to the components mentioned above, the rubber composition according to the present invention may appropriately contain compounding agents commonly used in the tire industry, such as oils, resin components, antioxidants, waxes, zinc oxide, stearic acid, crosslinking agents such as sulfur, and vulcanization accelerators.

[0121] (Resin components) The rubber composition according to the present invention preferably contains a resin component. The resin component is not particularly limited, but examples include petroleum resins, terpene resins, rosin resins, phenolic resins, etc., which are commonly used in the tire industry. These resin components may be used individually or in combination of two or more.

[0122] The resin component is not particularly limited, and resins commonly used in conventional tire rubber compositions, such as aromatic petroleum resins, terpene resins, rosin resins, and phenolic resins, can be used.

[0123] Suitable aromatic petroleum resins include, for example, coumarone indene resin, coumarone resin, indene resin, and aromatic vinyl resins. As aromatic vinyl resins, α-methylstyrene or a homopolymer of styrene, or a copolymer of α-methylstyrene and styrene is preferred, and a copolymer of α-methylstyrene and styrene is more preferred, due to their economical nature, ease of processing, and excellent heat generation properties. Aromatic vinyl resins that are commercially available from companies such as Kraton Corporation and Eastman Chemical Corporation can be used.

[0124] Examples of terpene resins include polyterpene resins consisting of at least one terpene compound selected from α-pinene, β-pinene, limonene, dipentene, etc.; aromatically modified terpene resins made from the terpene compound and an aromatic compound; terpene-phenol resins made from the terpene compound and a phenolic compound; and these terpene resins that have been hydrogenated (hydrogenated terpene resins). Examples of aromatic compounds used as raw materials for aromatically modified terpene resins include styrene, α-methylstyrene, vinyltoluene, and divinyltoluene. Examples of phenolic compounds used as raw materials for terpene-phenol resins include phenol, bisphenol A, cresol, and xylenol.

[0125] Rosin-based resins are not particularly limited, but examples include natural resin rosin and rosin-modified resins obtained by hydrogenation, disproportionation, dimerization, esterification, etc.

[0126] Phenolic resins are not particularly limited, but examples include phenol-formaldehyde resin, alkylphenol-formaldehyde resin, alkylphenol-acetylene resin, and oil-modified phenol-formaldehyde resin.

[0127] From the viewpoint of grip performance, the softening point of the resin component is preferably 40°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher. Furthermore, from the viewpoint of processability and improved dispersibility between the rubber component and filler, it is preferably 150°C or lower, more preferably 140°C or lower, and even more preferably 130°C or lower. The softening point of the resin component is measured by the measurement method described above.

[0128] When a resin component is included, its content per 100 parts by mass of rubber component is preferably more than 3 parts by mass, more preferably more than 5 parts by mass, and even more preferably more than 8 parts by mass. Furthermore, from the viewpoint of processability, the resin component content is preferably less than 30 parts by mass, more preferably less than 20 parts by mass, and even more preferably less than 15 parts by mass.

[0129] (oil) Examples of oils include process oils, vegetable oils, and animal oils. Examples of process oils include paraffinic process oils, naphthenic process oils, and aromatic process oils. For environmental reasons, process oils with a low content of polycyclic aromatic compounds (PCA) can also be used. Examples of low-PCA process oils include light extraction solvates (MES), processed distillate aromatic extracts (TDAEs), and heavy naphthenic oils. Furthermore, from a life cycle assessment perspective, waste oil from rubber mixers and engines, or refined waste cooking oil from restaurants, may also be used. Oils may be used individually or in combination of two or more types. Examples of oils that can be used include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., ENEOS Corporation, Orisoy Co., Ltd., H&R Co., Ltd., Toyokuni Oil Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., etc.

[0130] When oil is included, the oil content per 100 parts by mass of rubber component is preferably more than 5 parts by mass, more preferably more than 10 parts by mass, even more preferably more than 15 parts by mass, and particularly preferably 20 parts by mass or more, from the viewpoint of processability. Furthermore, from the viewpoint of wear resistance, it is preferably less than 120 parts by mass, more preferably less than 100 parts by mass, even more preferably less than 80 parts by mass, and particularly preferably less than 60 parts by mass. In this specification, the oil content also includes the amount of oil contained in the stretched rubber.

[0131] (Anti-aging agent) Anti-aging agents are not particularly limited, but examples include amine-based, quinoline-based, quinone-based, phenol-based, and imidazole-based compounds, as well as metal carbamate salts. Examples include N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, N-cyclohexyl-N'-phenyl-p-phenylenediamine, N,N'-bis(1-methylheptyl)-p-phenylenediamine, and N,N'-bis(1,4-di Phenylenediamine-based antioxidants such as methylpentyl)-p-phenylenediamine, N,N'-bis(1-ethyl-3-methylpentyl)-p-phenylenediamine, N-4-methyl-2-pentyl-N'-phenyl-p-phenylenediamine, N,N'-diaryl-p-phenylenediamine, hindereddiaryl-p-phenylenediamine, phenylhexyl-p-phenylenediamine, and phenyloctyl-p-phenylenediamine, and quinoline-based antioxidants such as 2,2,4-trimethyl-1,2-dihydroquinoline polymer and 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline are preferred. These antioxidants may be used alone or in combination of two or more.

[0132] When an anti-aging agent is included, the total content per 100 parts by mass of rubber component is preferably more than 0.5 parts by mass, more preferably more than 1.0 part by mass, and even more preferably more than 1.5 parts by mass, from the viewpoint of the rubber's resistance to ozone cracking. Furthermore, from the viewpoint of wear resistance and wet grip performance, it is preferably less than 10.0 parts by mass, and more preferably less than 5.0 parts by mass.

[0133] When stearic acid is included, its content per 100 parts by mass of the rubber component is preferably more than 0.5 parts by mass, more preferably more than 1.0 part by mass, and even more preferably more than 1.4 parts by mass, from the viewpoint of processability. Furthermore, from the viewpoint of vulcanization rate, it is preferably less than 10.0 parts by mass, and more preferably less than 5.0 parts by mass.

[0134] When zinc oxide is included, its content per 100 parts by mass of rubber component is preferably more than 0.5 parts by mass, more preferably more than 1.0 part by mass, and even more preferably more than 1.4 parts by mass, from the viewpoint of processability. Furthermore, from the viewpoint of wear resistance, it is preferably less than 10.0 parts by mass, and more preferably less than 5.0 parts by mass.

[0135] (Crosslinking agent) Sulfur is preferably used as a crosslinking agent. Suitable sulfur varieties include powdered sulfur, oil-treated sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, and highly dispersible sulfur.

[0136] When sulfur is included, the sulfur content per 100 parts by mass of rubber component is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, from the viewpoint of ensuring a sufficient vulcanization reaction. Furthermore, from the viewpoint of preventing deterioration, it is preferably 5.0 parts by mass or less, more preferably 4.0 parts by mass or less, even more preferably 3.0 parts by mass or less, and particularly preferably 2.5 parts by mass or less. When oil-containing sulfur is used as a crosslinking agent, the content of the vulcanizing agent shall be the total content of pure sulfur contained in the oil-containing sulfur.

[0137] As a crosslinking agent other than sulfur, known organic crosslinking agents can also be used. The organic crosslinking agent is not particularly limited as long as it can form crosslinking chains other than polysulfide bonds, but examples include alkylphenol-sulfur chloride condensate, 1,6-hexamethylene-dithiosulfate sodium dihydrate, 1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane, dicumyl peroxide, etc., with 1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane being preferred. These organic crosslinking agents can be used if they are commercially available from companies such as Taoka Chemical Industries, Ltd., Lanxess Corporation, Flexis, etc.

[0138] While there are no particular limitations on the vulcanization accelerators, examples include sulfenamide, thiazole, thiram, thiourea, guanidine, dithiocarbamate, aldehyde-amine or aldehyde-ammonia, imidazoline, and xanthate vulcanization accelerators. Among these, sulfenamide and thiram vulcanization accelerators are preferred because they more favorably produce the desired effects, and using these two in combination is even more preferable.

[0139] Examples of sulfenamide-based vulcanization accelerators include CBS (N-cyclohexyl-2-benzothiadylsulfenamide), TBBS (Nt-butyl-2-benzothiadylsulfenamide), N-oxyethylene-2-benzothiadylsulfenamide, N,N'-diisopropyl-2-benzothiadylsulfenamide, and N,N-dicyclohexyl-2-benzothiadylsulfenamide. Examples of thiazole-based vulcanization accelerators include 2-mercaptobenzothiazole and dibenzothiazolyl disulfide. Examples of thiuram-based vulcanization accelerators include tetramethylthiuram monosulfide, tetramethylthiuram disulfide, and tetrabenzylthiuram disulfide (TBzTD). Examples of guanidine-based vulcanization accelerators include diphenylguanidine (DPG), diortotolylguanidine, and orthotolylbiguanidine. These may be used individually or in combination of two or more. Among these, the combination of CBS and TBzTD is particularly preferred because it more favorably yields the desired effect.

[0140] When a vulcanization accelerator is included, its content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, and more preferably 2 parts by mass or more. Furthermore, the content of the vulcanization accelerator per 100 parts by mass of the rubber component is preferably 8 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 6 parts by mass or less. By keeping the content of the vulcanization accelerator within the above range, it tends to be possible to ensure fracture strength and elongation.

[0141] The rubber composition according to the present invention can be manufactured by known methods. For example, it can be manufactured by kneading the components other than the vulcanizing agent (crosslinking agent) and vulcanization accelerator in a known kneading machine commonly used in the tire industry, such as a Banbury mixer, kneader, or open roll, then adding the vulcanizing agent and vulcanization accelerator and kneading further, and then vulcanizing.

[0142] <Tires> The tire of the present invention comprises a tread portion made of the above-mentioned rubber composition and is suitably used for passenger car tires, high-performance passenger car tires, heavy-duty tires, and the like. In particular, it is preferred for use as a passenger car tire.

[0143] A tire having a tread made of the above rubber composition can be manufactured using the above rubber composition by conventional methods. Specifically, an unvulcanized rubber composition, in which the above components are blended with the rubber component as needed, is extruded to match the shape of the tread, bonded together with a belt layer and other tire components on a tire molding machine, and molded in a conventional method to form an unvulcanized tire. This unvulcanized tire is then heated and pressurized in a vulcanizing machine to manufacture the tire. [Examples]

[0144] The following examples (implementations) are considered preferable for implementation, but the scope of the present invention is not limited to these examples.

[0145] We investigated tires having a tread made of rubber compositions obtained according to the formulations shown in Tables 1 and 2 using the various chemicals listed below, and the results calculated based on the various analysis and evaluation methods described below are shown in Tables 1 to 4.

[0146] NR:TSR20 SBR1: SBR1502 manufactured by JSR Corporation (unmodified E-SBR, styrene content: 23.5% by mass, vinyl content: 18 mol%, Tg: -56℃, Mw: 440,000, non-oil-based) SBR2: HPR850 manufactured by JSR Corporation (S-SBR, styrene content: 26% by mass, vinyl content: 59 mol%, Tg: -25℃, Mw: 190,000, non-oil-based) BR: UBEPOL BR(registered trademark) 150B manufactured by Ube Industries, Ltd. (Vinyl binding content: 1.5 mol%, cis-1,4- content: 97%, Mw: 440,000) TPE1: Dynalon (registered trademark) manufactured by JSR Corporation (styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene content: 53% by mass, alkylene unit content: 47% by mass, Tg: -50℃) TPE2: Septon (registered trademark) manufactured by Kuraray Co., Ltd. (Hydrogenated styrene-alkylene block copolymer (SEBS), styrene content: 32% by mass, alkylene unit content: 68% by mass, Tg: -50℃) Carbon black: Diablack N220 (N2SA: 115m) manufactured by Mitsubishi Chemical Corporation. 2 / g) Silica 1: 9100GR (N2SA: 235m) manufactured by Evonik Tegusa. 2 / g, CTAB:200m 2 / g, average primary particle diameter: 15.6nm) Silica 2: Evonik Degussa's UltraSil VN3 (N2SA: 175m 2 / g, CTAB:165m 2 / g, average primary particle diameter: 15nm) Silane coupling agent: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa. Oil: H&R VivaTec400 (TDAE oil) Resin component: Sylvatraxx® 4401 (a copolymer of α-methylstyrene and styrene, manufactured by Arizona Chemical Corporation; softening point: 85°C, Tg: 43°C) Anti-aging agent 1: Nocrack 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Anti-aging agent 2: Nocrack RD (poly(2,2,4-trimethyl-1,2-dihydroquinoline)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Stearic acid: Beads of stearic acid manufactured by NOF Corporation Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: HK-200-5 (5% oil-containing powdered sulfur) manufactured by Hosoi Chemical Industry Co., Ltd. Vulcanization accelerator 1: Noxellar CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide (CBS)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 2: Sunceller TBZTD (Tetrabenzylthioram disulfide (TBzTD)) manufactured by Sanshin Chemical Industry Co., Ltd.

[0147] (Examples and Comparative Examples) According to the formulations shown in Tables 1 and 2, chemicals other than sulfur and vulcanization accelerators were mixed in a 1.7 L closed Banbury mixer for 1 to 10 minutes until the discharge temperature reached 150 to 160°C to obtain a mixture. Next, using a twin-screw open roll mixer, sulfur and vulcanization accelerators were added to the mixture and mixed for 4 minutes until the temperature reached 105°C to obtain an unvulcanized rubber composition. Using the obtained unvulcanized rubber composition, it was molded to the shape of the tread section and bonded together with other tire components such as a belt layer to produce an unvulcanized tire. The tire was then vulcanized at 170°C to obtain the test tires (sizes: 205 / 65R16 or 195 / 65R15) listed in Tables 3 and 4.

[0148] <Measurement of tanδ at 0℃> Each rubber test piece, cut from the rubber layer of the tread of each test tire to a length of 20 mm, width of 4 mm, and thickness of 1 mm, with the tire circumference as the longer side, is measured using a GABO Iplexer series under the conditions of 0°C, 10 Hz, initial strain of 10%, dynamic strain of 2.5%, and extension mode.

[0149] <Measurement of tanδ at 70°C> Each rubber test piece, cut from the rubber layer of the tread of each test tire to a length of 20 mm, width of 4 mm, and thickness of 1 mm, with the tire circumference as the longer side, is measured using a GABO Iplexer series under the conditions of a temperature of 70°C, a frequency of 10 Hz, an initial strain of 10%, a dynamic strain of 1%, and the extension mode.

[0150] <High-speed turning performance> The obtained test tires were mounted on regular rims, inflated with air, and then installed on all wheels of a domestic FF vehicle (2000cc). With the test tires installed, the vehicle was driven on a road surface at 100 km / h, and its cornering performance was subjectively evaluated on a scale of 5 points. The same evaluation was performed by 20 drivers, and the total score of the evaluation results was calculated. From the obtained results, the results of Comparative Example 3 were indexed with 100, and the evaluation results for each tire were obtained. A higher index indicates better high-speed cornering performance. (High-speed cornering performance index) = (Total score of each evaluated tire) / (Total score of Comparative Example 5) × 100

[0151] <Fuel efficiency> Using a rolling resistance tester, the rolling resistance of each test tire was measured while it was driven at a speed of 80 km / h. The reciprocal of this value was then expressed as an exponential value, with Comparative Example 6 set to 100. A higher value indicates lower rolling resistance and superior fuel efficiency.

[0152] The overall performance index is the sum of high-speed cornering performance and fuel efficiency performance.

[0153] [Table 1]

[0154] [Table 2]

[0155] [Table 3]

[0156] [Table 4]

[0157] <Embodiment> Examples of embodiments of the present invention are shown below.

[0158] [1] A tire having a tread portion and a belt layer, The rubber composition constituting the tread portion contains a rubber component and a thermoplastic elastomer, The rubber component comprises a multi-component copolymer having aromatic vinyl units and conjugated diene units. The thermoplastic elastomer includes a styrene-based thermoplastic elastomer having alkylene units. Under normal conditions, when the tire is subjected to a normal load and pressed against a flat surface, the cross-sectional width of the tire is Wt (mm), and the width of the tire's belt layer is B (mm). Y=(B-16) / Wt When defined as such, Y is less than or equal to 0.75, A tire in which the ratio (X / Y) of the total content X (parts by mass) of the thermoplastic elastomer to 100 parts by mass of the rubber component Y is 3.0 or greater. [2] The tire according to [1], wherein the glass transition temperature of the styrene-based thermoplastic elastomer having alkylene units is -30°C or lower. [3] The tire according to [1] or [2] above, wherein the styrene content of the styrene-based thermoplastic elastomer having alkylene units is 20% by mass or more. [4] A tire as described in any of [1] to [3] above, wherein X is 10 parts by mass or more. [5] The tire according to any one of [1] to [4] above, wherein the rubber component contains 50% by mass or more of a polypolymer having aromatic vinyl units and conjugated diene units. [6] The rubber composition further has an N2SA of 170m as measured by the BET method. 2 / g super 240m 2 A tire containing less than 1 / g of silica, as described in any of the above [1] to [5]. [7] The rubber composition further contains CTAB 160m 2 / g super 210m 2 A tire containing less than 1 / g of silica, as described in any of the above [1] to [6]. [8] The tire according to any one of [1] to [7] above, wherein the ratio of the tanδ at 70°C (70°C tanδ) to the tanδ at 0°C (0°C tanδ) of the rubber composition, 70°C tanδ / 0°C tanδ, is 0.05 or more. [9] The tire according to any one of [1] to [8] above, wherein the ratio of the tanδ at 70°C (70°C tanδ) to the tanδ at 0°C (0°C tanδ) of the rubber composition, 70°C tanδ / 0°C tanδ, is 1.80 or less.

[10] A tire as described in any of [1] to [9] above, in which Y is less than 0.73.

[11] The tire according to any one of [1] to

[10] above, wherein the rubber composition further contains a resin component.

[12] The tire according to any one of [1] to

[11] above, wherein the rubber component further contains butadiene rubber.

[13] The tire according to any one of [1] to

[12] above, wherein the tread portion comprises a base rubber layer adjacent to the radially outer side of the belt layer, and the base rubber layer is composed of a rubber composition containing a rubber component that includes at least one of isoprene rubber and butadiene rubber.

[14] A tire as described in any of [1] to

[13] above, wherein when the outer diameter of the tire is Dt (mm), Wt and Dt satisfy the following formula (1). (π / 4) × (Dt 2 / Wt)≧1500···(1)

[15] The tread portion has land portions separated by one or more circumferential grooves that extend continuously in the circumferential direction of the tire, and at least one of the land portions has an opening area to the tread surface of 0.1 to 15 mm 2 A tire having one or more small holes, as described in any of the above [1] to

[14] . [Explanation of Symbols]

[0159] Wt Section width B Belt layer width DT Tire Outer Diameter 1 Circumferential groove 2 Land 3 Belt Layer 4. Cap rubber layer 6. Base rubber layer 7 Sidewall 8 Inner Liner 9. Clinch 10 Tread surface C Tire circumferential direction W (Tire width direction) Te tread edge 21 Yokomizo 22 sipes 23 Center Sipe 24 Small hole 30 bead 31 Bead Core 32 rim

Claims

1. A tire having a tread section and a belt layer, The rubber composition constituting the tread portion contains a rubber component and a thermoplastic elastomer, The rubber component comprises a multi-component copolymer having aromatic vinyl units and conjugated diene units. The thermoplastic elastomer includes a styrene-based thermoplastic elastomer having alkylene units. Under normal conditions, when the tire is subjected to a normal load and pressed against a flat surface, the cross-sectional width of the tire is Wt (mm), and the width of the tire's belt layer is B (mm). Y=(B-16) / Wt When defined as such, Y is less than or equal to 0.75, A tire in which the ratio (X / Y) of the total content X (parts by mass) of the thermoplastic elastomer to 100 parts by mass of the rubber component contained in the rubber composition constituting the tread portion Y is 3.0 or more.

2. The tire according to claim 1, wherein the glass transition temperature of the styrene-based thermoplastic elastomer having the alkylene units is -30°C or lower.

3. The tire according to claim 1 or 2, wherein the styrene content of the styrene-based thermoplastic elastomer having alkylene units is 20% by mass or more.

4. The tire according to claim 1 or 2, wherein X is 10 parts by mass or more.

5. The tire according to claim 1 or 2, wherein the rubber component contains 50% by mass or more of a polypolymer having aromatic vinyl units and conjugated diene units.

6. The aforementioned rubber composition, further measured by the BET method, has an N2SA of 170 m 2 / g over 240m 2 A tire according to claim 1 or 2, containing less than 1g of silica.

7. The aforementioned rubber composition further contains CTAB at 160 m 2 / g over 210m 2 A tire according to claim 1 or 2, containing less than 1g of silica.

8. The tire according to claim 1 or 2, wherein the ratio of the loss loss tangent (0°C tanδ) measured under conditions of temperature 70°C, frequency 10 Hz, initial strain 10%, and dynamic strain 1% to the loss loss tangent (70°C tanδ) measured under conditions of temperature 70°C, frequency 10 Hz, initial strain 10%, and dynamic strain 2.5% of the rubber composition, 70°C tanδ / 0°C tanδ, is 0.05 or more.

9. The tire according to claim 1 or 2, wherein the ratio of the loss loss tangent (0°C tanδ) measured under conditions of temperature 70°C, frequency 10Hz, initial strain 10%, and dynamic strain 1% to the loss loss tangent (70°C tanδ) measured under conditions of temperature 70°C, frequency 10Hz, initial strain 10%, and dynamic strain 2.5% of the rubber composition, 70°C tanδ / 0°C tanδ, is 1.80 or less.

10. The tire according to claim 1 or 2, wherein Y is less than 0.

73.

11. The tire according to claim 1 or 2, wherein the rubber composition further contains a resin component.

12. The tire according to claim 1 or 2, wherein the rubber component further contains butadiene rubber.

13. The tire according to claim 1 or 2, wherein the tread portion comprises a base rubber layer adjacent to the radially outer side of the belt layer, and the base rubber layer is composed of a rubber composition containing a rubber component that includes at least one of isoprene rubber and butadiene rubber.

14. The tire according to claim 1 or 2, wherein when the outer diameter of the tire is Dt (mm), Wt and Dt satisfy the following formula (1). (π / 4)×(Dt 2 / Wt)≧1500・・・(1)

15. The tire according to claim 1 or 2, wherein the tread portion has land portions separated by one or more circumferential grooves extending continuously in the circumferential direction of the tire, and at least one of the land portions has one or more small holes with an opening area to the tread surface of 0.1 to 15 mm².

16. The tire according to claim 1 or 2, wherein the ratio X / Y is 13.9 or greater.

Citation Information

Patent Citations

  • Tire having a tread comprising a diene elastomer and a thermoplastic elastomer system

    JP2018519384A

  • Rubber composition and tire

    WO2015079703A1

  • Pneumatic tire

    WO2021075469A1

  • Tire

    WO2021166904A1