All-solid-state battery and method for manufacturing the same, and conductive coated current collector

The method for manufacturing all-solid-state batteries using a conductive coated current collector with a peelable second layer addresses sagging issues, improving performance and structure integrity by removing deformed portions and aligning layers.

JP7948164B2Active Publication Date: 2026-11-11TOYOTA JIDOSHA KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023221279
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2026-11-11
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

Existing methods for manufacturing all-solid-state batteries result in performance degradation due to coating sagging, leading to deviations from the ideal shape and reduced energy density.

Method used

A method involving the formation of a conductive coated current collector with distinct coating layers, where a second coating layer is easily peeled off, allowing for the removal of deformed peripheral portions during the manufacturing process, and alignment of electrode and electrolyte layers to minimize sagging effects.

Benefits of technology

Reduces performance degradation by eliminating coating sagging-induced deformations, enhances workability, and maintains the integrity of the battery structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948164000002
    Figure 0007948164000002
  • Figure 0007948164000003
    Figure 0007948164000003
  • Figure 0007948164000001
    Figure 0007948164000001
Patent Text Reader

Abstract

To provide a manufacturing method of an all-solid battery capable of reducing performance degradation caused by coating sagging.SOLUTION: A manufacturing method of an all-solid battery includes the steps (a) to (h) of: (a) forming a conductive first coating layer in a first region occupying a part of a first surface of a first collector; (b) forming a second coating layer adjacently to the first coating layer in a second region occupying an outer peripheral side of the first coating layer, the second coating layer being easier to peel than the first coating layer; (c) forming a first electrode layer continuously over surfaces of the first and second coating layers; (d) forming a solid electrolyte layer on a surface of the first electrode layer; (e) forming a second electrode layer on a surface of the solid electrolyte layer; (f) thermally pressing an obtained collector-electrode assembly; (g) removing the second coating layer from a collector 1 together with the layers thereon; and (h) laminating a second collector on a surface of the second electrode layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This application relates to an all-solid-state battery, a method for manufacturing the same, and a conductive coated current collector. [Background technology]

[0002] Patent Document 1 describes an all-solid-state battery and a method for manufacturing the same. [Prior art documents] [Patent Documents]

[0003] [Patent Document 1] Japanese Patent Publication No. 2019-200947 [Overview of the project] [Problems that the invention aims to solve]

[0004] Patent Document 1 describes the production of an all-solid-state battery by stacking a positive electrode, a solid electrolyte layer, and a negative electrode to obtain a laminate, and then by hot-pressing the laminate. However, since the positive electrode active material layer, the negative electrode active material layer, and the solid electrolyte layer are manufactured by coating them with a slurry, deformation (sagging) occurs due to the flow of the slurry after coating, resulting in a deviation from the ideal shape. Sagging in each layer leads to a decrease in energy density.

[0005] This invention provides a method for manufacturing an all-solid-state battery that can reduce performance degradation due to coating sagging. It also provides a conductive coated current collector and an all-solid-state battery. [Means for solving the problem]

[0006] The present invention includes the following embodiments [1] to [3]. [1] A method for manufacturing an all-solid-state battery, (a) A step of forming a conductive first coating layer on a first region that occupies a part of the first surface of the first current collector, (b) A step of forming a second coating layer adjacent to the first coating layer in a second region of the first surface of the first current collector, which occupies the outer periphery of the first coating layer, wherein the second coating layer is a coating layer that is more easily peeled off from the first surface of the first current collector than the first coating layer. (c) A step of forming a first electrode layer containing a first active material and having a first polarity on the surfaces of the first coating layer and the second coating layer of the conductive coated current collector obtained by going through steps (a) and (b), wherein the first electrode layer is formed continuously across the surface of the first coating layer and the surface of the second coating layer. (d) A step of forming a solid electrolyte layer containing a solid electrolyte on the surface of the first electrode layer, (e) A step of forming a second electrode layer on the surface of the solid electrolyte layer, the second electrode layer comprising a second active material and having a second polarity, wherein the second polarity is the opposite polarity to the first polarity. (f) A step of heat-pressing the current collector-electrode composite obtained by going through steps (a) to (e), (g) The step of removing the second coating layer from the current collector 1 together with the portion of the first electrode layer laminated on the second coating layer, the portion of the solid electrolyte layer laminated on the second coating layer, and the portion of the second electrode layer laminated on the second coating layer. (h) A step of laminating a second current collector onto the surface of the second electrode layer of the current collector-electrode composite that has undergone steps (f) and (g) above, A method for manufacturing an all-solid-state battery, characterized by including the following:

[0007] [2] A current collector having a conductive coating layer, A conductive substrate in the form of a plate, sheet, or foil, A conductive first coating layer is provided in a first region occupying a part of the first surface of the conductive substrate, A second coating layer is provided adjacent to the first coating layer in a second region of the first surface of the conductive substrate, which occupies the outer periphery of the first coating layer. Equipped with, A conductive coated current collector, characterized in that the second coating layer is a coating layer that is more easily peeled off from the first surface of the conductive substrate than the first coating layer.

[0008] [3] The first current collector and, A conductive coating layer is provided on a first region occupying a part of the first surface of the first current collector, A first electrode layer is provided in contact with the coating layer without directly contacting the first current collector, and comprises a first active material and having a first polarity. A solid electrolyte layer containing a solid electrolyte, A second electrode layer comprising a second active material and having a second polarity opposite to the first polarity, A second current collector is electrically connected to the second electrode layer, The laminated structure is provided in which the above order is stacked in the first direction, On the outer periphery side of the first surface of the first current collector, there exists a second region that is not covered by the coating layer. An all-solid-state battery characterized in that the end face of the coating layer, the end face of the first electrode layer, the end face of the solid electrolyte layer, and the end face of the second electrode layer are aligned. [Effects of the Invention]

[0009] In the method for manufacturing an all-solid-state battery of the present invention, a first coating layer is provided on a first region of the surface of a first current collector (step (a)), a second coating layer is provided adjacent to the first coating layer and in a region outside the first coating layer (step (b)), a first electrode layer, a solid electrolyte layer, and a second electrode layer are formed on the first and second coating layers (steps (c) to (e)), and in step (g), the second coating layer is removed from the first current collector. This makes it possible to remove the peripheral portions of each layer, where coating sagging is likely to occur, along with the second coating layer. Therefore, according to the method for manufacturing an all-solid-state battery of the present invention, it is possible to remove the portion deformed by coating sagging and reduce the performance degradation caused by coating sagging.

[0010] The conductive coated current collector of the present invention is in a state where steps (a) and (b) of the above-described method for manufacturing an all-solid-state battery are completed. Therefore, the conductive coated current collector of the present invention can be suitably used for manufacturing all-solid-state batteries in which performance degradation due to coating sagging is reduced.

[0011] In the all-solid-state battery of the present invention, since the respective end faces of the first electrode layer, the solid electrolyte layer, and the second electrode layer are aligned, it is possible to reduce performance degradation derived from deformation caused by coating sagging. Furthermore, the coat layer is provided on a part of the first surface of the first current collector, and the first electrode layer is provided in contact with the coat layer without directly contacting the first current collector, so a portion that can be used as a terminal is exposed at the outer peripheral portion of the first current collector. Thereby, it is possible to improve the workability of electrically connecting the all-solid-state battery. [Brief Description of the Drawings]

[0012] [Figure 1] Figure 1 is a flowchart illustrating a method S10 for manufacturing an all-solid-state battery according to one embodiment. [Figure 2] Figure 2(A) and Figure 2(C) are cross-sectional views schematically illustrating the first coating step S1. Figure 2(B) is a plan view taken along the line B-B in Figure 2(A). Figure 2(D) is a plan view taken along the line D-D in Figure 2(C). Figure 2(E) is a cross-sectional view schematically illustrating the second coating step S2. Figure 2(F) is a plan view taken along the line F-F in Figure 2(E). Figure 2(G) is a cross-sectional view schematically illustrating the first electrode layer forming step S3. Figure 2(H) is a plan view taken along the line H-H in Figure 2(G). Figure 2(I) is a cross-sectional view schematically illustrating the solid electrolyte layer forming step S4. Figure 2(J) is a plan view taken along the line J-J in Figure 2(I). Figure 2(K) is a cross-sectional view schematically illustrating the second electrode layer forming step S5. Figure 2(L) is a plan view taken along the line L-L in Figure 2(K). Figure 2(M) is a cross-sectional view schematically illustrating the hot pressing step S6 and the removing step S7. Figure 2(N) is a plan view taken along the line N-N in Figure 2(M). Figure 2(O) is a cross-sectional view schematically illustrating the second current collector laminating step S8. Figure 2(P) is a plan view taken along the line P-P in Figure 2(O). [Modes for carrying out the invention]

[0013] Embodiments of the present invention will be described below with reference to the drawings. However, the present invention is not limited to these embodiments. Note that the drawings do not necessarily reflect accurate dimensions. Also, some reference numerals may be omitted in the drawings. In this specification, unless otherwise specified, the notation "A~B" for numerical values ​​A and B means "A or more and B or less". If a unit is attached only to numerical value B in such notation, that unit shall also apply to numerical value A. Also, unless otherwise specified, the words "or" and "or else" mean logical OR. Also, the notation "E1 and / or E2" for elements E1 and E2 means "E1 or E2, or a combination thereof", and elements E1, ..., E N For (N is an integer greater than or equal to 3), "E1, ..., E N-1 , and / or E N The notation " is "E1, ..., E N-1 , or E N This shall mean ", or a combination thereof."

[0014] Figure 1 is a flowchart illustrating a manufacturing method S10 (hereinafter referred to as "manufacturing method S10") for an all-solid-state battery according to one embodiment. Manufacturing method S10 comprises, in this order, a first coating step S1, a second coating step S2, a first electrode layer formation step S3, a solid electrolyte layer formation step S4, a second electrode layer formation step S5, a hot pressing step S6, a removal step S7, a second current collector lamination step S8, and a housing step S9. Each step will be described in order below.

[0015] Figures 2(A) to 2(P) are schematic diagrams illustrating the manufacturing method S10. Figures 2(A) and 2(C) are schematic cross-sectional views illustrating the first coating process S1 (hereinafter referred to as "process S1"). Figure 2(B) is a plan view taken along the arrow BB in Figure 2(A), and Figure 2(D) is a plan view taken along the arrow DD in Figure 2(C). Process S1 is a process of forming a conductive first coating layer 2 on a first region R1 that occupies a part of the first surface 1a of the first current collector 1.

[0016] As the first current collector 1 (hereinafter referred to as "current collector 1"), a current collector made of an appropriate conductive material can be used, depending on whether the first electrode layer, described later, is a positive electrode layer or a negative electrode layer. The current collector 1 comprises, for example, a plate-shaped, sheet-shaped, or foil-shaped conductive substrate. As such a current collector 1, for example, a member made of a metallic material containing one or more elements selected from Cu, Ni, Al, V, Au, Pt, Mg, Fe, Ti, Pb, Co, Cr, Zn, Ge, In, Sn, and Zr can be used. As another example, a member comprising a conductive or electrically insulating substrate (for example, a resin film, etc.) and the above-mentioned metallic material on which the surface of the substrate is vapor-deposited or plated may be used as the current collector 1.

[0017] As the composition for coating the first coat layer 2 (hereinafter referred to as "coat layer 2"), a composition containing a binder and a conductive filler can be preferably used. In step S1, the conductive first coat layer 2 can be formed, for example, by coating a slurry containing the binder and the conductive filler. The slurry may further contain a suitable solvent. One or more binders can be used alone or in combination. From the viewpoint of suppressing peeling of the first coat layer 2 in the hot pressing step S6 described later, a thermoplastic resin with a melting point of 165°C or higher can preferably be used as the binder. There is no particular upper limit to the melting point of the binder resin, but in one embodiment it may be 200°C or lower. Examples of thermoplastic resins that can be included in the first coat layer 2 include halogen-containing polymers such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polychlorotrifluoroethylene (PCTFE). One or more conductive fillers can be used alone or in combination. Preferably, carbon material fillers such as furnace black, carbon black (CB), Ketjenblack (KB), acetylene black (AB), activated carbon, carbon, graphite, vapor-grown carbon fiber (VGCF), carbon nanotubes (CNT), and carbon nanofibers (CNF) can be used as conductive fillers. The average primary particle diameter of the carbon material filler may be, for example, 10 nm to 20 μm. Here, the average primary particle diameter is obtained, for example, as the arithmetic mean of the results of measuring the primary particle diameters (average of short and long diameters) of 30 or more particles based on image analysis using an electron microscope such as a scanning electron microscope (SEM).

[0018] Examples of conductive fillers other than carbon material fillers include metal particles such as Cu, Ni, Al, V, Au, Pt, Mg, Fe, Ti, Pb, Co, Cr, Zn, Ge, In, Sn, and Zr. Average particle size (D) of inorganic fillers. 50 The average particle size (D) can be, for example, 50 nm to 5 μm. 50) refers to the median diameter, which corresponds to the median value of the volume distribution measured based on the spherical approximation using the laser diffraction-scattering particle size distribution method.

[0019] The content of conductive filler in the first coating layer 2 is preferably 15% by volume or more, based on the total amount of the first coating layer 2 at 25°C (100% by volume), from the viewpoint of increasing the conductivity of the first coating layer 2, and preferably 60% by volume or less, from the viewpoint of increasing the adhesion of the first coating layer 2 to the current collector 1. The content of binder in the first coating layer 2 is preferably 85% by volume or less, based on the total amount of the first coating layer 2 at 25°C (100% by volume), from the viewpoint of increasing the conductivity of the first coating layer 2, and preferably 40% by volume or more, from the viewpoint of increasing the adhesion of the first coating layer 2 to the current collector 1.

[0020] In one embodiment, the thickness of the first coating layer 2 is preferably 0.5 μm or more from the viewpoint of enhancing the anchoring effect and preventing peeling, and preferably 4 μm or less from the viewpoint of suppressing peeling due to elongation in the in-plane direction.

[0021] Figure 2(E) is a schematic cross-sectional view illustrating the second coating process S2 (hereinafter referred to as "process S2"), and Figure 2(F) is a plan view taken along the FF arrow in Figure 2(E). Process S2 is a process in which, in the current collector 10pre having the first coating layer 2 after process S1, a second coating layer 3 is formed adjacent to the first coating layer 2 in the second region R2 of the first surface 1a of the first current collector 1, which occupies the outer periphery of the first coating layer 2. In process S2, the second coating layer 3 is a coating layer that is more easily peeled off from the first surface 1a of the first current collector 1 than the first coating layer 2.

[0022] The second coating layer 3 (hereinafter referred to as "coating layer 3") preferably contains a binder and a filler. In step S2, the second coating layer 3 can be formed, for example, by coating a slurry containing the binder and the filler. The slurry may further contain a suitable solvent. One or more binders may be used alone or in combination. As the binder in the second coating layer 3, (a) a binder having a melting point of 110°C or less (hereinafter referred to as "binder (a)") and / or (b) a binder having a Young's modulus of 2.34 GPa or more at 25°C and a relative permittivity of 3.45 or less at 25°C (hereinafter referred to as "binder (b)"). In one embodiment, the melting point of binder (a) may be 110°C or less, for example, 40 to 110°C. In one embodiment, the melting point of binder (a) may be 55°C or more lower than the hot pressing temperature in the hot pressing process S6 described later. In one embodiment, the Young's modulus of binder (b) at 25°C may be 2.34 GPa or more, for example 2.34 to 4.50 GPa, as the tensile modulus measured at 25°C in accordance with JIS K7161. In one embodiment, the relative permittivity of the binder resin at 25°C may be 3.45 or less, for example 3.10 to 3.45, as the relative permittivity measured at 25°C and 1 MHz in accordance with JIS C2138. Examples of binder (a) include acrylic adhesives, silicone adhesives, rubber adhesives, polypropylene (PP), polyethylene (PE), etc. Examples of binder (b) include polysulfone (PSU), polyphenylsulfone (PPSU), etc.

[0023] In the second coating layer 3, one or more fillers may be used individually or in combination. In one embodiment, the second coating layer 3 preferably contains a carbon material filler. As the carbon material filler, the carbon material filler described above in relation to the first coating layer 2 may be used. In other embodiments, the second coating layer 3 may contain an inorganic filler other than a carbon material. As the inorganic filler, the inorganic filler described above in relation to the first coating layer 2 may be used. The carbon material filler and the inorganic filler may be used in combination.

[0024] The filler content in the second coating layer 3 is preferably 20% by volume or more, based on the total volume of the second coating layer 3 at 25°C (100% by volume), from the viewpoint of facilitating the peeling of the second coating layer 3 from the current collector 1, and preferably 90% by volume or less, from the viewpoint of handling ease when peeling the coating layer. In one embodiment, from the viewpoint of facilitating the suppression of adhesion of the second coating layer 3 to the roll in the hot pressing process S6 described later, the filler content in the second coating layer 3 is 40% by volume or more, based on the total volume of the second coating layer 3 at 25°C (100% by volume), and the second coating layer 3 can be formed such that the edge of the second coating layer 3 and the edge of the current collector are aligned.

[0025] In one embodiment, from the viewpoint of facilitating the lamination of each layer constituting the battery on the first coating layer 2 and the second coating layer 3, the thickness of the second coating layer 3 can be the same as that of the first coating layer 2. From the viewpoint of ensuring the strength of the second coating layer 3 and facilitating its removal together with the layer above it in the removal step S7 described later, the thickness of the second coating layer 3 can be, for example, 0.5 μm to 5.0 μm.

[0026] The second coating layer 3 is removed from the surface of the current collector 1 in the removal step S7 described later. The phenomenon of loss of the bonding state between the second coating layer 3 and the current collector 1 may occur in the hot pressing step S6, the second electrode formation step S5 or the solid electrolyte layer formation step S4, or the first electrode formation step S3.

[0027] By going through steps S1 and S2, a conductive coated current collector 10 according to one embodiment is obtained. The conductive coated current collector 10 comprises a plate-shaped, sheet-shaped, or foil-shaped conductive substrate 1, a conductive first coating layer 2 provided in a first region R1 occupying a part of the first surface 1a of the conductive substrate 1, and a second coating layer 3 provided adjacent to the first coating layer 2 in a second region R2 of the first surface 1a of the conductive substrate 1, occupying the outer periphery of the first coating layer 2. In the conductive coated current collector 10, the second coating layer 3 is a coating layer that is more easily peeled off than the first coating layer 2. In one embodiment, the second coating layer 3 may be a coating layer that is more easily peeled off from the current collector 1 than the first coating layer 2 when heat, shear stress, or stress in a direction intersecting the first surface 1a of the current collector 1 is applied. In another embodiment, the second coating layer 3 may be a coating layer that is more easily peeled off from the current collector 1 than the first coating layer 2 when subjected to shear stress or stress in a direction intersecting the first surface 1a of the current collector 1.

[0028] Figure 2(G) is a schematic cross-sectional view illustrating the first electrode layer formation step S3 (hereinafter referred to as "step S3"), and Figure 2(H) is a plan view taken along the line HH in Figure 2(G). Step S3 is a step of forming a first electrode layer 4 containing a first active material and having a first polarity on the surfaces of the first coat layer 2 and the second coat layer 3 of a conductive coated current collector 10 having a first coat layer 2 and a second coat layer 3. In step S3, the first electrode layer 4 is formed continuously across the surface of the first coat layer 2 and the surface of the second coat layer 3. In this embodiment, the first electrode layer 4 is a negative electrode layer containing a negative electrode active material (hereinafter referred to as "negative electrode layer 4").

[0029] The negative electrode layer 4 comprises a negative electrode active material, a conductive additive, and a binder, and optionally further comprises a solid electrolyte as described later. For example, when a lithium-ion secondary battery is manufactured as an all-solid-state battery, examples of negative electrode active materials include carbon materials such as graphite, artificial graphite, highly oriented graphite, mesocarbon microbeads, hard carbon, and soft carbon, and Li4Ti5O 12、 Examples include metallic compounds, elements that can alloy with lithium or compounds of such elements, and boron-doped carbon. Examples of elements that can alloy with lithium include silicon and tin.

[0030] The binder plays the role of tying the active material or conductive additive to the surface of the conductive coated current collector 10 and maintaining the conductive network in the electrode. One or more binders may be used alone or in combination. Examples of binders include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and fluororubber; thermoplastic resins such as polypropylene (PP) and polyethylene (PE); imide resins such as polyimide (PI) and polyamideimide (PAI); alkoxysilyl group-containing resins; acrylic resins containing monomer units such as acrylic acid and methacrylic acid; styrene-butadiene rubber (SBR), carboxymethylcellulose (CMC), alginates such as sodium alginate and ammonium alginate; water-soluble cellulose ester crosslinked polymers; and starch-acrylic acid graft polymers.

[0031] Examples of conductive additives include acetylene black, carbon black, and graphite. A viscosity-adjusting solvent such as N-methyl-2-pyrrolidone (NMP) may be used in the negative electrode layer 4.

[0032] The negative electrode layer 4 can be formed by first kneading a negative electrode active material, a conductive additive, a binder, and optionally a solid electrolyte in a solvent to obtain a slurry-like negative electrode mixture, and then applying the negative electrode mixture to the surfaces of the first coat layer 2 and the second coat layer 3 of the conductive coated current collector 10 and drying it.

[0033] Figure 2(I) is a schematic cross-sectional view illustrating the solid electrolyte layer formation step S4 (hereinafter referred to as "step S4"), and Figure 2(J) is a plan view taken along the JJ arrow in Figure 2(I). Step S4 is a step of forming a solid electrolyte layer 5 containing a solid electrolyte on the surface of the first electrode layer (negative electrode layer) 4. One or more solid electrolytes may be used individually or in combination. The solid electrolyte layer 5 contains a solid electrolyte that has conductivity for ions absorbed and released by the negative electrode active material contained in the negative electrode layer 4 and the positive electrode active material contained in the positive electrode layer 6, which will be described later. For example, examples of solid electrolytes that have conductivity for lithium ions include oxide solid electrolytes such as Li3PO4; and sulfide solid electrolytes such as Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Si2S-P2S5, LiI-Li2S-P2O5, and LiI-Li3PO4-P2S5.

[0034] The solid electrolyte layer 5 can be prepared by adding a solid electrolyte and optionally a binder to a solvent and kneading to obtain a slurry-like electrolyte mixture, and then following procedures such as coating and drying the electrolyte composition. As the binder in the solid electrolyte 5, the binder described above in relation to the first electrode layer (negative electrode layer) 4 can be used. The solid electrolyte layer 5 may be formed, for example, by directly coating the surface of the first electrode layer (negative electrode layer) 4 with the electrolyte mixture, or, for example, by coating the surface of a substrate such as metal foil (e.g., Al foil) with the electrolyte mixture to form a solid electrolyte layer 5 on the surface of the substrate, and then the solid electrolyte layer 5 formed on the surface of the substrate may be placed on the surface of the first electrode layer 4 of the composite 20 in which the first electrode layer 4 is formed on the conductive coated current collector 10, and the solid electrolyte layer 5 may be transferred from the substrate surface to the surface of the first electrode layer 4 by press processing such as a roll press.

[0035] Figure 2(K) is a schematic cross-sectional view illustrating the second electrode layer formation step S5 (hereinafter referred to as "step S5"), and Figure 2(L) is a plan view taken along the LL arrow in Figure 2(K). Step S5 is a step of forming a second electrode layer 6 containing a second active material and having a second polarity on the surface of the solid electrolyte layer 5. In step S5, the second polarity (+ / -) is the opposite polarity to the first polarity (- / +). In this embodiment, the second electrode layer 6 is a positive electrode layer containing a positive electrode active material (hereinafter referred to as "positive electrode layer 6"). The positive electrode layer 6 comprises a positive electrode active material, a conductive additive, and a binder. For example, when the all-solid-state battery manufactured in manufacturing method S10 is a lithium-ion secondary battery, examples of positive electrode active materials include composite oxides, metallic lithium, and sulfur. The composition of the composite oxide includes, for example, at least one of iron, manganese, titanium, nickel, cobalt, and aluminum, and lithium. Examples of composite oxides include olivine-type lithium iron phosphate (LiFePO4), LiCoO2, and LiNiMnCoO2. The conductive additive and binder in the positive electrode layer 6 can be the same as those used in the negative electrode layer 4. The positive electrode layer 6 may further contain a solid electrolyte. The solid electrolyte in the positive electrode layer 6 can be the solid electrolyte described above in relation to the solid electrolyte layer 5.

[0036] The positive electrode layer 6 can be manufactured by kneading a positive electrode active material, a conductive additive, a binder, and optionally a solid electrolyte in a solvent to obtain a slurry-like positive electrode mixture, and then applying and drying this positive electrode mixture. The positive electrode layer 6 may be formed, for example, by directly coating the surface of the solid electrolyte layer 5 with the positive electrode mixture, or, for example, by coating the surface of a substrate such as metal foil (e.g., Al foil) with the positive electrode mixture to form the positive electrode layer 6 on the surface of the substrate, and then placing the positive electrode layer 6 formed on the surface of the substrate onto the surface of the solid electrolyte layer 5 of a composite 30 in which the negative electrode layer 4 and solid electrolyte layer 5 are formed on a conductive coated current collector 10, and transferring the positive electrode layer 6 from the substrate surface to the surface of the solid electrolyte layer 5 by press processing such as a roll press. Examples of solvents for forming each layer include N-methyl-2-pyrrolidone, methanol, methyl isobutyl ketone, and water. In one embodiment, the second electrode layer 6 may be formed straddling the boundary between the first coating layer 2 and the second coating layer 3 in a plan view. In one embodiment, the boundary between the first coating layer 2 and the second coating layer 3 may be formed on the current collector 1 at a location where the first electrode layer 4, the solid electrolyte layer 5, and the second electrode layer 6 are not cut together (for example, in a straight line).

[0037] Figure 2(M) is a schematic cross-sectional view illustrating the hot pressing process S6 (hereinafter referred to as "process S6") and the removal process S7 (hereinafter referred to as "process S7"), and Figure 2(N) is a plan view taken along the NN arrow in Figure 2(M). Process S6 is a process of hot pressing the current collector-electrode composite 40 obtained through processes S1 to S5. By going through process S6, the current collector-electrode composite is densified. The hot pressing can be carried out by, for example, a roll press. The temperature of the hot pressing can be, for example, a temperature that does not exceed the melting point of the binder contained in the first coating layer 2 by 10°C or more, or a temperature that does not exceed the melting point of the binder contained in the first coating layer 2, and in one embodiment it can be 130 to 200°C. The pressure of the hot pressing can be, for example, a linear pressure of 3 to 10 t / cm when the hot pressing is carried out by a roll press.

[0038] Step S7 is the step of removing the second coating layer 2 from the current collector 1 together with the portion of the first electrode layer (negative electrode layer) 4 laminated on the second coating layer 3, the portion of the solid electrolyte layer 5 laminated on the second coating layer 3, and the portion of the second electrode layer (positive electrode layer) 6 laminated on the second coating layer 3. In one embodiment, the second coating layer 3 loses its bonding state with the first current collector 1 due to the heat and stress of the hot press in step S6. In another embodiment, the second coating layer 3 loses its bonding state with the first current collector 1 due to the stress of the press when the solid electrolyte layer 5, which is coated on a substrate such as Al foil, is bonded to the first electrode layer (negative electrode layer) 4 in step S4. In another embodiment, the second coating layer 3 loses its bond with the first current collector 1 due to the stress of pressing when the second electrode layer (positive electrode layer) 6, which is coated and formed on a substrate such as Al foil, is joined to the solid electrolyte layer 5 in step S5. In any embodiment, the bond between the second coating layer 3 and the first current collector 1 is lost by the end of step S6. Therefore, the operation of removing the second coating layer 3 from the current collector 1 in step S7 can be easily performed. By going through step S7, the first electrode layer (negative electrode layer) 4, the solid electrolyte layer 5, and the peripheral portions of the second electrode layer (positive electrode layer) 6 where coating sagging has occurred can be removed together with the second coating layer 3. In the current collector-electrode composite 50 after steps S6 and S7, it is possible to obtain a state in which the end faces of the first coat layer 2, the first electrode layer (negative electrode layer) 4, the solid electrolyte layer 5, and the second electrode layer (positive electrode layer) 6 are aligned in the portion where the second coat layer 3 has been removed, without cutting the current collector-electrode composite.

[0039] Figure 2(O) is a schematic cross-sectional view illustrating the second current collector lamination process S8 (hereinafter sometimes referred to as "process S8"), and Figure 2(P) is a plan view taken along the PP arrow in Figure 2(O). Process S8 is a process of laminating a second current collector (positive electrode current collector) 7 onto the surface of the second electrode layer (positive electrode layer) 6 of the current collector-electrode composite 50 that has gone through processes S6 and S7. As the second current collector 7, for example, a plate-shaped, sheet-shaped, foil-shaped, or porous current collector formed from the conductive material described above in relation to the first current collector can be used.

[0040] The housing step S9 (hereinafter sometimes referred to as "step S9") is a step of housing and sealing the all-solid-state battery 100 obtained through steps S1 to S8 in an outer casing material (not shown). As the outer casing material, an outer casing material usable for all-solid-state batteries can be used. Examples of materials that can constitute such an outer casing material include metal materials such as aluminum and stainless steel, as well as resin materials such as polyphenylene sulfide resin and polyimide resin. Furthermore, the shape of the outer casing material is not particularly limited and may be circular (cylindrical, coin-shaped, button-shaped), hexahedral (cuboidal, cubic), bag-shaped, or a shape obtained by processing and deforming these. After step S8, before housing the all-solid-state battery 100 in the outer casing material, the all-solid-state battery 100 may be partially cut as needed.

[0041] The all-solid-state battery 100 has a laminated structure in which a first current collector 1; a conductive coat layer 2 provided in a first region R1 occupying a part of the first surface 1a thereof; a first electrode layer (negative electrode layer) 4 that is provided in contact with the coat layer 2 without being in direct contact with the first current collector 1, contains a first active material (negative electrode active material), and has a first polarity (-); a solid electrolyte layer 5 containing a solid electrolyte; a second electrode layer (positive electrode layer) 6 that contains a second active material (positive electrode active material) and has a polarity (+) opposite to the first polarity (-); and a second current collector 7 electrically connected to the second electrode layer 6 are laminated in the above order. In the all-solid-state battery 100, the end face of the coat layer 2, the end face of the first electrode layer 4, the end face of the solid electrolyte layer 5, and the end face of the second electrode layer 6 are aligned. Such a configuration cannot be obtained if coating sagging remains. Further, on the outer peripheral side of the first region R1 on the first surface 1a of the first current collector, there exists a second region R2 where the first current collector not covered with the coat layer 2 is exposed. The exposed portion of the first current collector can be preferably utilized as a terminal.

[0042] In the above description relating to the present invention, the manufacturing method S10 for an all-solid-state battery, the conductive coat current collector 10, and the all-solid-state battery 100, in the form where the first electrode layer 4 is a negative electrode layer containing a negative electrode active material and the second electrode layer 6 is a positive electrode layer containing a positive electrode active material, have been mainly cited as examples, but the present invention is not limited to these forms. For example, it is also possible to adopt a manufacturing method for an all-solid-state battery, a conductive coat current collector, and an all-solid-state battery in a form where the first electrode layer 4 is a positive electrode layer containing a positive electrode active material, and the second electrode layer 6 is a negative electrode layer containing a negative electrode active material.

[0043] In the above description relating to the present invention, the manufacturing method S10 in the form of manufacturing an all-solid-state battery that is a lithium ion secondary battery, and the all-solid-state battery 100 in the form of a lithium ion secondary battery have been mainly cited as examples, but the present invention is not limited to these forms. For example, ions other than lithium ions (for example, Na + , K + , Mg 2+ , Ca 2+ , Al 3+ , Zn 2+By using an active material that intercepts and releases ions (etc.), and by using a solid electrolyte that has conductivity for the ions intercepted and released by the active material, it is possible to create an all-solid-state battery other than a lithium-ion secondary battery, and it is also possible to provide a method for manufacturing such an all-solid-state battery. [Examples]

[0044] The present invention will be described in more detail below based on the examples. However, the present invention is not limited to these examples.

[0045] <Example 1> The following procedure was used to manufacture the all-solid-state battery. (1. Fabrication of negative electrode current collector foil with carbon coating layer) A negative electrode current collector foil (double-sided CC foil) with carbon coating layers on both sides was fabricated by the following procedure. A composition for the central carbon coating layer (central CC layer; first CC layer) (first CC composition) was prepared by weighing acetylene black and polyvinylidene fluoride (PVDF) in a mixed weight ratio of 20:80 and mixing them with N-methylpyrrolidone (NMP). Similarly, a composition for the edge CC layer (second CC layer) (second CC composition) was prepared by weighing acetylene black and an acrylic binder with a melting point of 110°C in a mixed weight ratio of 20:80 and mixing them with N-methylpyrrolidone (NMP). The central CC layer (first CC layer) was formed by center coating of the first CC composition with a width of 62 mm on both sides of a 120 mm wide Al foil. Then, the edge CC layer (second CC layer) was formed by coating of the second CC composition with a width of 5 mm on both sides of each central CC layer.

[0046] (2. Formation of the negative electrode layer) A negative electrode mixture was prepared by adding PVDF, negative electrode active material (lithium titanium oxide (LTO)) particles, and sulfide solid electrolyte (Li2S-P2S5 glass ceramic) to a polypropylene container and stirring with an ultrasonic dispersion device for 30 minutes. A negative electrode layer was formed by coating the surface (both sides) of the CC layer of the double-sided CC foil prepared in step 1 with the negative electrode mixture in a width of 70 mm, thereby creating a double-sided CC foil-negative electrode layer laminate.

[0047] (3. Formation of Solid Electrolyte Layer) A solid electrolyte mixture was prepared by adding heptane, butadiene rubber (BR), and the same sulfide solid electrolyte as in step 2 to a polypropylene container and stirring with an ultrasonic disperser for 15 minutes. A solid electrolyte (SE) layer was formed on the surface of the Al foil by coating the solid electrolyte mixture with a width of 70 mm, thereby creating an Al foil-SE layer laminate. Multiple Al foil-SE layer laminates were prepared.

[0048] (4. Formation of the positive electrode layer) Using a rolling fluid coating apparatus (manufactured by Powrec), positive electrode active material particles (Li) are formed in an atmospheric environment. 1.15 Ni 1 / 3 Co 1 / 3 Mn 1 / 3 Positive electrode active material particles having a lithium niobate coating layer were obtained by coating particles (mainly composed of O2) with lithium niobate and firing them in an atmospheric environment. A positive electrode mixture was prepared by adding PVDF, the above positive electrode active material particles, the sulfide solid electrolyte used in step 2, and vapor-grown carbon fiber (VGCF; manufactured by Showa Denko Corporation) to a polypropylene container and stirring for 20 minutes using an ultrasonic dispersion device. A positive electrode layer was formed by coating the surface of an Al foil with a width of 65 mm to create an Al foil-positive electrode layer laminate. Multiple Al foil-positive electrode layer laminates were prepared.

[0049] (5. Fabrication of Negative Electrode Current Collector-Electrode Composite: Transfer Pressing Process) The double-sided CC foil-negative electrode layer laminate fabricated in step 2, the Al foil-SE layer laminate fabricated in step 3, and the Al foil-positive electrode layer laminate fabricated in step 4 were each cut to a length of 80 mm. The Al foil-SE layer laminates were placed on both sides of the double-sided CC foil-negative electrode layer laminate and stacked so that the center positions of the coated areas coincided, and the solid electrolyte layer was transferred by roll pressing at a linear pressure of 0.4 t / cm, obtaining an SE layer-negative electrode layer-double-sided CC foil-negative electrode layer-SE layer laminate. Furthermore, the Al foil-positive electrode layer laminates were placed on both sides and stacked, and the positive electrode layer was transferred by roll pressing at a linear pressure of 0.4 t / cm, obtaining a negative electrode current collector-electrode composite having a structure in which the positive electrode layer-SE layer-negative electrode layer-double-sided CC foil-negative electrode layer-SE layer-positive electrode layer are laminated in this order.

[0050] (6. Hot Pressing Process) The negative electrode current collector-electrode composite obtained in step 5 was densified by roll pressing at a temperature of 165°C and a linear pressure of 5 t / cm for 10 minutes. At that time, the peeling of the end CC layer (second CC layer) was confirmed. After that, the negative electrode current collector-electrode composite was cut so that the dimensions of the positive electrode layer were 60 mm wide x 60 mm long.

[0051] (7. Preparation and application of positive electrode current collector foil) Acetylene black and PVDF, which are conductive materials, were weighed to a mixed weight ratio of 20:80, and NMP was added to prepare a carbon coating (CC) composition (third CC composition). The third CC composition was coated to a thickness of 2 μm on one side of the Al foil and dried at 100°C for 1 hour to obtain an Al foil (positive electrode current collector foil) having a CC layer (third CC layer) on one side. The positive electrode current collector foil was cut so that the dimensions of its CC layer were 57 mm in length and 57 mm in width. Styrene-butadiene rubber (SBR) binder was used to attach it to both sides of the current collector-electrode composite obtained in step 6, thereby creating a battery with a laminated structure of Al foil - third CC layer - positive electrode layer - SE layer - negative electrode layer - double-sided CC foil (first CC layer - Al foil - first CC layer) - negative electrode layer - SE layer - positive electrode layer - third CC layer - Al foil. After joining terminals to the positive electrode current collector foil and the negative electrode current collector foil, the battery was vacuum-sealed in a laminate film (outer packaging material).

[0052] <Examples 2 and 3> Except for changing the compositions of the first and second CC compositions used to produce the double-sided CC foil in step 1, as shown in Table 1, batteries were produced in the same manner as in Example 1. In both Examples 2 and 3, peeling of the edge CC layer (second CC layer) was observed during the transfer press process (step 5).

[0053] <Comparative Examples 1-5> Except for changing the compositions of the first and second CC compositions used to produce the double-sided CC foil in Step 1 as shown in Table 1, batteries were manufactured in the same manner as in Example 1. However, in Comparative Examples 1, 2, 4, and 5, since peeling of the end CC layer (second CC layer) was not observed, when joining the terminals to the negative electrode current collector foil in Step 7, the terminals were welded to the outside of the end CC layer (second CC layer). In Comparative Example 3, peeling of the end CC layer was observed during the hot pressing process (Step 6).

[0054] <Charge and Discharge Test> For each battery manufactured in Examples 1-3 and Comparative Examples 1-5, a charge and discharge test was performed according to the following procedure, and the internal resistance was measured. The battery under evaluation was charged with constant current and constant voltage at a charging voltage of 2.95V and a charging speed (C rate) of 0.3C, and then discharged to a cutoff voltage of 1.5V. Next, it was charged to 2.17V, and then discharged with constant current at a discharge speed of 5C, and the internal resistance was calculated from the voltage change ΔV.

[0055] <Evaluation Results> In Example 1, the end CC layer (second CC layer) could be peeled off during the hot pressing process (step 6), whereas in Example 2, peeling of the end CC layer was confirmed during the transfer pressing process (step 5). In Comparative Examples 1, 2, 4, and 5, the end CC layer could not be peeled off in any of the processes. The high internal resistance of the battery in Comparative Example 3 is thought to be due to the low electronic conductivity of the CC layer in the central part. In Example 1, it is thought that the binder in the end CC layer melted during the hot pressing process (step 6), and the presence of carbon in the end CC layer made the end CC layer slippery, causing it to peel off. In Examples 2 and 3, because the binder in the end CC layer was hard, it is thought that the difference in elongation due to the pressing stress occurred during the transfer pressing process (step 7), causing the end CC layer to peel off. Even when a binder with a low melting point was used in the end CC layer, the end CC layer did not peel off when there was no conductive material (carbon) (Comparative Examples 1 and 2). This is thought to be because no slippage occurred between the binder and the aluminum foil. Even when a thermosetting resin with a low dielectric constant was used as the binder for the edge CC layer, the edge CC layer could not be peeled off when only the binder was used (Comparative Examples 1 and 2). This is thought to be due to the high adhesive strength. When polyamide-imide (PAI) or PVDF was used as the binder for the edge CC layer (Comparative Examples 4 and 5), the edge CC layer could not be peeled off. This is thought to be due to the high dielectric constant and high adhesive strength of these binders.

[0056] [Table 1] [Explanation of symbols]

[0057] 1: First current collector, 1a: First surface, R1: First region, R2: Second region, 2: First coating layer, 3: Second coating layer, 4: First electrode layer, 5: Solid electrolyte layer, 6: Second electrode layer, 7: Second current collector, 10: Conductive coated current collector, 20, 30, 40, 50: Current collector-electrode composite, 100: All-solid-state battery

Claims

1. A method for manufacturing an all-solid-state battery, (a) A step of forming a conductive first coating layer on a first region that occupies a part of the first surface of the first current collector, (b) A step of forming a second coating layer adjacent to the first coating layer in a second region of the first surface of the first current collector that occupies the outer periphery of the first coating layer, wherein the second coating layer is a coating layer that is more easily peeled off from the first surface of the first current collector than the first coating layer. (c) A step of forming a first electrode layer containing a first active material and having a first polarity on the surfaces of the first coating layer and the second coating layer of the conductive coated current collector obtained by going through steps (a) and (b), wherein the first electrode layer is formed continuously across the surface of the first coating layer and the surface of the second coating layer. (d) A step of forming a solid electrolyte layer containing a solid electrolyte on the surface of the first electrode layer, (e) A step of forming a second electrode layer on the surface of the solid electrolyte layer, the second electrode layer comprising a second active material and having a second polarity, wherein the second polarity is the opposite polarity to the first polarity. The process, (f) A step of heat-pressing the current collector-electrode composite obtained by going through steps (a) to (e), (g) The step of removing the second coating layer from the first current collector together with the portion of the first electrode layer laminated on the second coating layer, the portion of the solid electrolyte layer laminated on the second coating layer, and the portion of the second electrode layer laminated on the second coating layer. (h) A step of laminating a second current collector onto the surface of the second electrode layer of the current collector-electrode composite that has undergone steps (f) and (g) above, A method for manufacturing an all-solid-state battery, characterized by including the following:

2. The first coating layer is A binder which is a thermoplastic resin with a melting point of 165°C or higher, The carbon material filler is present in an amount of 15% by volume or more, based on the total volume of the first coating layer at 25°C. Includes, The second coating layer is A binder having a melting point of 110°C or less, and / or a binder having a Young's modulus of 2.34 GPa or more at 25°C and a relative permittivity of 3.45 or less at 25°C, The carbon material filler is present in an amount of 20% by volume or more, based on the total volume of the second coating layer at 25°C. A method for manufacturing an all-solid-state battery according to claim 1, including the method described in claim 1.

3. The first electrode layer is a negative electrode layer containing a negative electrode active material, The second electrode layer is a positive electrode layer containing a positive electrode active material. A method for manufacturing an all-solid-state battery according to claim 1 or 2.

4. A current collector having a conductive coating layer, A conductive substrate in the form of a plate, sheet, or foil, A conductive first coating layer is provided in a first region occupying a part of the first surface of the conductive substrate, A second coating layer is provided adjacent to the first coating layer in a second region of the first surface of the conductive substrate, which occupies the outer periphery of the first coating layer. Equipped with, A conductive coated current collector, characterized in that the second coating layer is a coating layer that is more easily peeled off from the first surface of the conductive substrate than the first coating layer.

5. The first coating layer is A binder which is a thermoplastic resin with a melting point of 165°C or higher, The carbon material filler is present in an amount of 15% by volume or more, based on the total volume of the first coating layer at 25°C. Includes, The second coating layer is A binder having a melting point of 110°C or less, and / or a binder having a Young's modulus of 2.34 GPa or more at 25°C and a relative permittivity of 3.45 or less at 25°C, The carbon material filler is present in an amount of 20% by volume or more, based on the total volume of the second coating layer at 25°C. The current collector according to claim 4, including the following:

6. The first current collector and A conductive coating layer is provided in a first region that occupies a part of the first surface of the first current collector, A first electrode layer is provided in contact with the coating layer without directly contacting the first current collector, and contains a first active material and has a first polarity, A solid electrolyte layer containing a solid electrolyte, A second electrode layer comprising a second active material and having a second polarity opposite to the first polarity, A second current collector is electrically connected to the second electrode layer, The laminated structure is provided in which the above order is stacked in the first direction, On the outer periphery side of the first surface of the first current collector, there exists a second region that is not covered by the coating layer. An all-solid-state battery characterized in that the end face of the coating layer, the end face of the first electrode layer, the end face of the solid electrolyte layer, and the end face of the second electrode layer are aligned.

7. The aforementioned coating layer A binder which is a thermoplastic resin with a melting point of 165°C or higher, The carbon material filler is present in an amount of 15% by volume or more, based on the total volume of the coating layer at 25°C. The all-solid-state battery according to claim 6, including the above.

Citation Information

Patent Citations

  • Manufacture of electrode plate for non-aqueous electrolyte secondary battery

    JP1998144300A

  • Electrode plate for nonaqueous electrolyte secondary battery and manufacture thereof

    JP1998144301A

  • Masking device and manufacturing method of electrode for use in nonaqueous electrolytic battery

    JP2002313328A

  • Electrode plate for nonaqueous secondary battery and method of manufacturing the same, and nonaqueous secondary battery using the electrode plate

    JP2009283270A

  • Manufacturing method of electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery using the same

    JP2010277798A