Manufacturing method of insulated wires
The vinyl chloride resin composition with hydrotalcite, polyethylene oxide, and phenolic antioxidant, crosslinked by electron beam irradiation, addresses the issues of extrusion molding and heat resistance in insulated wires, achieving stable and durable insulating layers for electronic devices.
Patent Information
- Application Number
- JP2025029657
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-02-27
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-03-30
AI Technical Summary
Existing vinyl chloride resin compositions used for insulated wires face challenges in maintaining extrusion molding characteristics and long-run heat resistance, particularly when the insulating layer thickness is reduced for miniaturization and weight reduction in electronic devices, with properties like flame retardancy, electrical properties, and heat deformation properties deteriorating due to the addition of plasticizers.
A vinyl chloride resin composition for insulated wires containing hydrotalcite, polyethylene oxide and/or calcium laurate, phenolic antioxidant, and TMPT, with specific ratios of phenolic antioxidant to TMPT, and crosslinked by electron beam irradiation, improves extrusion molding characteristics and long-run heat resistance.
The composition enhances extrusion molding stability and heat resistance of the insulating layer, ensuring consistent thickness and preventing degradation during high-speed extrusion and electron beam treatment.
Smart Images

Figure 0007948352000005 
Figure 0007948352000006 
Figure 0007948352000001
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a vinyl chloride resin composition, an insulated wire using the same, and a method for producing the insulated wire. BACKGROUND ART
[0002] As a stabilizer for improving the stability of vinyl chloride polymers against heat and light, there is a technique of adding surface-treated hydrotalcites to a vinyl chloride polymer (see, for example, Patent Document 1). PRIOR ART DOCUMENTS PATENT DOCUMENTS
[0003] PATENT DOCUMENT 1 Japanese Unexamined Patent Application Publication No. 2003-40614 SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION
[0004] For example, for insulated wires used for internal wiring of electronic devices, there is a need to reduce the coating thickness of the insulating layer covering the conductor from the perspective of miniaturization and weight reduction of electronic devices. A vinyl chloride resin composition is used as the coating material for insulated wires. Vinyl chloride resin (polyvinyl chloride; PVC) contains chlorine, which is a halogen, in its chemical structure, and the vinyl chloride resin alone has high flame retardancy. Since vinyl chloride resin is rigid, when used as a wire coating material, a plasticizer for softening the vinyl chloride resin composition is added to the base polymer of the vinyl chloride resin for use. However, due to the influence of additives such as plasticizers, the properties of the vinyl chloride resin composition (such as flame retardancy, heat deformation properties, electrical properties, extrusion line speed during wire coating processing, and heat resistance) may change, and the properties may deteriorate. The inventors of the present application have studied the improvement of the properties of vinyl chloride resin compositions, particularly vinyl chloride resin compositions that are particularly suitable when used as wire coating materials.
[0005] The object of the present invention is to provide an insulated wire and a method for manufacturing the same that can improve the extrusion molding characteristics and long-run heat resistance of the insulating layer. [Means for solving the problem]
[0006] An insulated wire according to one embodiment comprises a conductor and an insulating layer covering the conductor, wherein the insulating layer contains, per 100 parts by mass of polyvinyl chloride, 4 parts by mass or more of hydrotalcite, 0.03 parts by mass or more of polyethylene oxide and / or calcium laurate, 0.1 parts by mass or more of a phenolic antioxidant, a plasticizer, and TMPT (trimethylolpropane triacrylate), wherein the phenolic antioxidant includes a phenolic antioxidant added to the plasticizer, and the value obtained by dividing the amount of the phenolic antioxidant added by the amount of TMPT (trimethylolpropane triacrylate) added is 0.033, 0.034, 0.029, or 0.042 (rounded to the fourth decimal place) That is the case.
[0007] Another embodiment of an insulated wire is a method for manufacturing an insulated wire having a conductor and an insulating layer covering the conductor, comprising the steps of: preparing a polyvinyl chloride resin composition comprising 4 parts by mass or more of hydrotalcite, 0.03 parts by mass or more of polyethylene oxide and / or calcium laurate, 0.1 parts by mass or more of a phenolic antioxidant, a plasticizer, and TMPT (trimethylolpropane triacrylate) per 100 parts by mass of polyvinyl chloride, wherein the phenolic antioxidant includes a phenolic antioxidant added to the plasticizer, and the value obtained by dividing the amount of the phenolic antioxidant added by the amount of TMPT (trimethylolpropane triacrylate) added is 0.02 or less; forming the insulating layer by extrusion molding of the polyvinyl chloride resin composition; and crosslinking the polyvinyl chloride resin composition by irradiating the insulating layer with an electron beam. [Effects of the Invention]
[0008] According to a typical embodiment of the present invention, the extrusion molding characteristics and long-run heat resistance of the insulating layer can be improved. [Brief explanation of the drawing]
[0009] [Figure 1] This is a cross-sectional view showing an example of the structure of an electric wire, which is one embodiment of the present. [Figure 2] Figure 1 is a cross-sectional view showing an example of the structure of a cable including the electric wires shown. [Modes for carrying out the invention]
[0010] Embodiments of the present invention will be described below with reference to the drawings.
[0011] <Examples of basic structures for electric wires and cables> Figure 1 is a cross-sectional view showing an example of the structure of an electric wire according to one embodiment. Figure 2 is a cross-sectional view showing an example of the structure of a cable including the electric wire shown in Figure 1.
[0012] The electric wire (insulated wire) 10 shown in Figure 1 has a conductor 11, and an insulating layer 12 covering the conductor 11. The electric wire 10 is an insulated wire. The insulating layer 12 is, for example, cross-linked. The electric wire 10 can be described as a cross-linked insulated wire.
[0013] The cable 20 shown in Figure 2 has multiple wires 10 and a sheath (insulating layer) 21 that covers the multiple wires 10 together. In the example shown in Figure 2, the sheath 21 covers two wires 10. However, the number of wires 10 inside the sheath 21 is not limited to two; for example, there may be three or more. Also, as shown in Figure 2, it is preferable that all wires covered by the sheath 21 are wires 10, but as a variation, there may be cases where wires with a different structure from the wires 10 are covered together with the wires 10 in the sheath 21.
[0014] Furthermore, the following describes a vinyl chloride resin composition as the material for the insulating layer 12, but the vinyl chloride resin composition described below can also be used as the material for the sheath 21 shown in Figure 2.
[0015] <Vinyl chloride resin composition> The inventors of this application are working to improve the properties of polyvinyl chloride resin compositions that are particularly suitable for use as insulating layers in insulated electric wires. The following embodiments describe techniques for improving the properties of polyvinyl chloride resin compositions obtained by adding additives to polyvinyl chloride resin as a base polymer. The following describes a polyvinyl chloride resin composition used for the insulating layer 12 of an electric wire 10 shown in Figure 1. For electric wires 10 used for internal wiring of electronic equipment, there is a growing need for small-diameter electric wires with a thinner insulating layer 12 covering the conductor 11, from the viewpoint of making electronic equipment more compact or lighter. When a plasticizer is added to improve the processability of polyvinyl chloride resin, the properties of the polyvinyl chloride resin composition change. For example, the flame retardancy of the polyvinyl chloride resin composition tends to decrease compared to polyvinyl chloride resin alone. Also, for example, the electrical properties (insulation properties, properties related to electrical noise, etc.) or heat deformation properties of the polyvinyl chloride resin composition may decrease compared to polyvinyl chloride resin alone. In particular, when the thickness of the insulating layer 12 is reduced, a semi-rigid polyvinyl chloride resin composition with a reduced amount of plasticizer may be used. In this case, compared to a flexible polyvinyl chloride resin composition to which a sufficient amount of plasticizer has been added, the extrusion molding characteristics of the coating material, particularly the stability of the outer diameter dimensions, long-run heat resistance (no burning (carbide) occurring when continuous extrusion molding is performed under the specified conditions described in the examples), and the linear velocity during extrusion molding tend to decrease. Furthermore, when crosslinking an insulating layer made of a semi-rigid polyvinyl chloride resin composition by irradiating it with an electron beam, the degree of crosslinking tends to be suppressed.
[0016] Therefore, the inventors of the present invention investigated a vinyl chloride resin composition that can improve the extrusion molding characteristics and long-run heat resistance of the insulating layer 12 when the coating thickness of the insulating layer 12 is reduced.
[0017] The vinyl chloride resin composition constituting the insulating layer 12 shown in Figure 1 includes (A) polyvinyl chloride (vinyl chloride resin) as a base polymer, (D) hydrotalcite, and (E) polyethylene oxide and calcium laurate. More specifically, it contains 4 parts by mass or more of hydrotalcite and a total of 0.03 parts by mass or more of polyethylene oxide and calcium laurate per 100 parts by mass of polyvinyl chloride. Furthermore, it is preferable that the vinyl chloride resin composition constituting the insulating layer 12 further contains 0.1 parts by mass or more of (C) a phenolic antioxidant and (F) a plasticizer per 100 parts by mass of polyvinyl chloride. The (C) phenolic antioxidant includes the phenolic antioxidant added to the (F) plasticizer, and the value obtained by dividing the amount of phenolic antioxidant added by the amount of TMPT (trimethylolpropane triacrylate) added is 0.033, 0.034, 0.029, or 0.042 (rounded to the fourth decimal place) It is preferable that the mixture contains at least 1 part by mass of (B) stearic acid-based metal soap in total, per 100 parts by mass of polyvinyl chloride.
[0018] [Base polymer] The vinyl chloride resin composition of this embodiment contains (A) polyvinyl chloride as a base polymer. One or more types of polyvinyl chloride with a K value of 71.6 or higher can be selected and used as the base polymer. The K value is a value measured by the test method specified in JIS K7367-2 or ISO 1628-2. The K value can be used as an indicator of the degree of polymerization. When crosslinking the vinyl chloride resin composition by electron beam irradiation, it is preferable to use a polyvinyl chloride with a K value of 75.7 to 78.1 rather than using a polyvinyl chloride with a K value of 71.6 alone, from the viewpoint of providing likelihood for the heat resistance and heat deformation characteristics after electron beam irradiation.
[0019] [Flame retardant] As flame retardants, antimony trioxide, aluminum hydroxide, brominated flame retardants, amorphous silica and the like are added. Further, the aforementioned (D) hydrotalcite also functions as a flame retardant. When a large amount of aluminum hydroxide is added as a flame retardant, the heat resistance of the vinyl chloride resin composition decreases. By adding hydrotalcite which functions as a flame retardant and a hydrogen chloride scavenger, both heat resistance and flame retardancy can be achieved. As described above, the addition amount of hydrotalcite is preferably 4 parts by mass or more relative to 100 parts by mass of polyvinyl chloride. Thereby, the long-run heat resistance of the vinyl chloride resin composition can be obtained. Further, by adding 4 parts by mass or more of hydrotalcite, the voltage resistance of the vinyl chloride resin composition after the crosslinking treatment by electron beam irradiation can be improved. Although details will be described later, according to the results of experimental evaluations by the inventors of the present application, by adding 4 parts by mass or more of hydrotalcite, the insulating layer 2 having dielectric breakdown voltage performance against a spark voltage of 6000 V can be obtained each during extrusion molding and after electron beam irradiation for crosslinking. Further, by adding 4 parts by mass or more of hydrotalcite, the long-run heat resistance of the vinyl chloride resin composition can be improved.
[0020] Note that as the addition amount of hydrotalcite increases, the lubricity of the vinyl chloride resin composition increases. If the addition amounts of (E) polyethylene oxide and calcium laurate are increased, the increase in lubricity can be suppressed, but from the viewpoint of the electrical characteristics of the vinyl chloride resin composition (and from the viewpoint of raw material cost), relative to 100 parts by mass of polyvinyl chloride, the addition amounts of polyethylene oxide and calcium laurate are preferably 1 part by mass or less. Therefore, the addition amount of hydrotalcite is preferably less than 10 parts by mass relative to 100 parts by mass of polyvinyl chloride.
[0021] On the other hand, from the viewpoint of reducing the lubricity of a vinyl chloride resin composition containing 4 parts by mass or more of hydrotalcite, when polyvinyl chloride is taken as 100 parts by mass, the total amount of component (E), which is oxidized polyethylene and calcium laurate, to be added needs to be 0.03 parts by mass or more. By setting the total amount of oxidized polyethylene and calcium laurate to 0.03 parts by mass or more, the thickness uniformity when the polyvinyl chloride resin composition is molded as the insulating layer 12 can be improved. Although details will be described later, for example, according to the results of experimental evaluations by the inventors of the present application, when the linear velocity during extrusion molding is 200 m / min, the maximum error in the coating thickness of the insulating layer 12 set to 0.1 mm to 0.2 mm can be 30 μm or less. Further, the total amount of oxidized polyethylene and calcium laurate added is preferably 0.6 parts by mass or less.
[0022] [Stabilizer] When the dehydrochlorination reaction is accelerated by the flame retardant, the vinyl chloride resin composition may be discolored when irradiated with an electron beam as a crosslinking treatment. Therefore, a stabilizer is added to suppress discoloration of the vinyl chloride resin composition caused by electron beam irradiation. The stabilizer contains (B) a stearic acid-based metal soap. Examples of this stearic acid-based metal soap include zinc stearate, calcium stearate, magnesium stearate, and stearoylbenzoylmethane. As described above, the total amount of the stearic acid-based metal soap added is 1 part by mass or more when polyvinyl chloride is taken as 100 parts by mass. The total amount of the stearic acid-based metal soap added is preferably 1.5 parts by mass or less when polyvinyl chloride is taken as 100 parts by mass.
[0023] [Plasticizer] (F) The plasticizer is not particularly limited, and known plasticizers can be used. However, it is preferable to use a trimellitate plasticizer. Examples of trimellitate plasticizers include tri-2-ethylhexyl trimellitate, tri-normal alkyl trimellitate, triisononyl trimellitate, or isodecyl trimellitate. In the examples described later, TOTM (tri-normal alkyl trimellitate) (Trimex N-08, manufactured by Kao Corporation: 0.5% by mass of phenolic antioxidant) or TINTM (isononyl trimellitate) (manufactured by UPC Corporation: 0.35% by mass of phenolic antioxidant) were used, but other trimellitate esters can also be used by adjusting the irradiation intensity and amount added during the crosslinking treatment.
[0024] [Other additives] The vinyl chloride resin composition of this embodiment contains (C) a phenolic antioxidant as an antioxidant. Examples of phenolic antioxidants include 1,3,5-tris[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], stearyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and 4,4'-butylidenebis-(6-tert-butyl-3-methylphenol). When polyvinyl chloride is 100 parts by mass, the amount of phenolic antioxidant added is preferably 0.15 parts by mass or less.
[0025] In addition to the base polymer and additives described above, one or more of the following may be used in combination as needed: lubricants, colorants, fillers, processing aids, UV absorbers, light stabilizers, crosslinking aids, and other modifiers. Lubricants include metal soap-based magnesium stearate, fatty acid-based stearic acid, silicones, fatty acid amides, hydrocarbons, esters, and alcohols. The above-mentioned (E) polyethylene oxide and calcium laurate function as processing aids. Fillers include carbon, clay (including calcined clay), zinc oxide, tin oxide, titanium oxide, magnesium oxide, molybdenum oxide, silicon compounds, quartz, calcium carbonate, magnesium carbonate, and white carbon.
[0026] Examples of crosslinking aids include trimethylolpropane trimethacrylate (TMPT), triallyl isocyanurate, dipentaerythritol hexaacrylate, triallyl cyanurate, N,N'-metaphenylene bismaleimide, ethylene glycol dimethacrylate, zinc acrylate, and zinc methacrylate.
[0027] Of the crosslinking aids described above, the addition of TMPT offers the following advantages. For this reason, the vinyl chloride resin composition of this embodiment preferably contains TMPT. TMPT is an acrylate monomer with three functional groups. Upon electron beam irradiation, TMPT itself bonds between the molecules of polyvinyl chloride, forming a crosslinked structure, making it effective as a crosslinking aid. Because TMPT monomers are highly reactive, this reaction occurs even at low doses.
[0028] As mentioned above, the value obtained by dividing the amount of phenolic antioxidant added by the amount of TMPT (trimethylolpropane triacrylate) added is: 0.033, 0.034, 0.029, or 0.042 (rounded to the fourth decimal place)It is necessary that the following conditions are met. By adding a phenolic antioxidant, the degradation of polyvinyl chloride resin due to electron beam irradiation can be suppressed. However, the phenolic antioxidant acts as a crosslinking inhibitor because it captures and stabilizes the radical site that is the starting point of the crosslinking reaction of TMPT. The ratio of the phenolic antioxidant to the amount of TMPT added is 0.033, 0.034, 0.029, or 0.042 (rounded to the fourth decimal place) This allows for adjusting the degree of crosslinking without compromising performance. The ratio of the phenolic antioxidant to the amount of TMPT added is preferably 0.01 or higher.
[0029] Furthermore, as will be described in detail later, when performing a crosslinking test by irradiating the insulating layer 12 shown in Figure 1 with an electron beam, it is preferable that the thickness of the insulating layer 12 covering the conductor 11 is 0.2 mm or less, and that the insulating layer 12 is crosslinked by irradiating it with an electron beam of an intensity of 5 Mrad or less. This makes it possible to improve the heat resistance when evaluating the insulating layer 12.
[0030] Furthermore, it is preferable that the insulating layer 12 further contains a calcined clay and a clay in which the SiO2 content is greater than the Al2O3 content. By using a combination of calcined clay and a clay in which the SiO2 content is greater than the Al2O3 content, the anionic electrolyte capture ability is increased. As a result, the electrical properties can be improved.
[0031] Furthermore, the insulating layer 12 preferably contains a black processing pigment, and the black processing pigment preferably contains diisononyl phthalate (DINP). This promotes plasticization when kneading the vinyl chloride resin composition, thereby improving moldability.
[0032] <Rating> Next, we will describe several examples of the electric wire 10 shown in Figure 1, as well as comparative examples to those examples, and explain the results of the evaluation for each. Table 1 shows the mixing ratios and evaluation results for Examples 1 to 6. Table 2 shows the mixing ratios and evaluation results for Examples 7 to 12. Table 3 shows the mixing ratios and evaluation results for Comparative Examples 1 to 6.
[0033] Each of the multiple examples shown in Tables 1 and 2 and the multiple comparative examples shown in Table 3 was manufactured to have the same structure as the electric wire 10 shown in Figure 1 by following the procedure below. The conductor 11 is a tin-plated conductor made by twisting together seven strands of tin-plated soft copper wire with an outer diameter of 0.127 mmφ. The diameter of the conductor 11 is, for example, 0.38 mm. The insulating layer 12 was made by kneading the formulations shown in Tables 1 to 3 in an open-roll mixer heated to 170°C, and then pelletizing them in a granulator to obtain a polyvinyl chloride resin composition. Subsequently, the obtained polyvinyl chloride resin composition was used as a raw material to perform extrusion molding using an extruder and coated the conductor 11. The thickness (coating thickness) of the insulating layer 12 made of the polyvinyl chloride resin composition was, for example, 0.1 mm. The extrusion molding conditions were, for example, by setting the cylinder temperature to 170°C and the head temperature to 180°C, and performing the extrusion molding process at a line speed of 300 m / min. Subsequently, the obtained electric wire 10 was subjected to a crosslinking treatment by irradiating it with an electron beam. The electron beam irradiation dose was set to 3.5 Mrad. Examples of cases where the coating thickness of the insulating layer 12 and the electron beam irradiation conditions were changed will be described later.
[0034] Of the evaluation items in Tables 1 to 3, the item "Stability of outer diameter dimensions during high-speed extrusion" was evaluated as follows: Extrusion molding was performed at a linear speed of 300 m / min, and wire 10 was collected at 5 minutes, 30 minutes, and 60 minutes. The diameters of four points on the cross-section of wire 10 were measured using a microscope. At 5 minutes, 30 minutes, and 60 minutes, if the difference between the maximum and minimum values of the four measured diameters was within 30 μm, it was evaluated as ○. If any one of them exceeded 30 μm, it was evaluated as ×.
[0035] Of the evaluation items in Tables 1 to 3, the "heat resistance during extrusion" item was evaluated as follows: Extrusion molding was performed continuously for 60 minutes at a linear speed of 300 m / min, and no burning (carbonization) was observed. Extrusions that met the following three conditions were evaluated as "○": no foaming was observed in the insulating layer 12, and no carbonization was observed around the breaker plate after the extruder was dismantled. Extrusions that did not meet even one of the above three conditions were evaluated as "×".
[0036] Of the evaluation items in Tables 1 to 3, the "Withstand Voltage (Extrusion / After Electron Beam Irradiation)" item was evaluated as follows: Specifically, the evaluation during extrusion was performed using a 6000V charged spark tester while the extrusion molding machine was in operation, to test the withstand voltage (insulation withstand voltage). The evaluation after electron beam irradiation was performed using a 6000V charged spark tester on the wire 10 whose insulating layer 12 had been cross-linked by electron beam irradiation. Tests where no continuity was confirmed by sparking were evaluated as ○. Tests where continuity was confirmed by sparking were evaluated as ×.
[0037] Of the evaluation items in Tables 1 to 3, the "degree of crosslinking" item was evaluated as follows: The insulating layer 12 was removed from the electric wire 10 after irradiation with an electron beam, and the gel fraction was measured using this as a sample. Tetrahydrofuran was used as the solvent, and extraction was performed by immersion in the solvent at 70°C for 24 hours. The weight of the sample was measured before and after extraction, and the gel fraction was calculated as (weight after extraction / weight before extraction) × 100. Samples with a calculated gel fraction of 50% or more were evaluated as ○, and those with a value less than 50% were evaluated as ×.
[0038] Furthermore, among the raw materials shown in Tables 1 to 3, Insurite LHM-103HP, manufactured by Mizusawa Chemical Industries, Ltd., was used as the SiO2-rich surface-treated clay. In addition, the black processing pigment (MXE9749 black) is a processing pigment with 20-45% carbon added, consisting of PVC, DINP, and a dispersant. In addition, the black processing pigment (EP4715 black) is a processing pigment with 10-40% carbon, consisting of PVC, plasticizers other than DINP, and other additives.
[0039] [Table 1]
[0040] [Table 2]
[0041] [Table 3]
[0042] As shown in Tables 1 and 2, the vinyl chloride resin compositions constituting the insulating layer of the insulated wires of Examples 1 to 12 contain, as raw materials, (A) polyvinyl chloride (vinyl chloride resin) as a base polymer, (B) stearic acid-based metal soap, (C) phenolic antioxidant, (D) hydrotalcite, (E) oxidized polyethylene and calcium laurate, and (F) plasticizer. Specifically, per 100 parts by mass of polyvinyl chloride, the composition contains a total of 1 part by mass or more of stearic acid-based metal soap, 0.1 parts by mass or more of phenolic antioxidant, 4 parts by mass or more of hydrotalcite, a total of 0.03 parts by mass or more of oxidized polyethylene and calcium laurate, and a plasticizer. (C) Phenolic antioxidant includes the phenolic antioxidant added to (F) plasticizer. The value obtained by dividing the amount of phenolic antioxidant added by the amount of TMPT (trimethylolpropane triacrylate) added is: 0.033, 0.034, 0.029, or 0.042 (rounded to the fourth decimal place) That is the case.
[0043] As shown in Comparative Examples 1-4 of Table 3, if the amount of phenolic antioxidant added was divided by the amount of TMPT (trimethylolpropane triacrylate) added, the degree of crosslinking was evaluated as "×".
[0044] As shown in Comparative Examples 1, 4, and 5 of Table 3, when the amount of hydrotalcite added was less than 4 parts by mass, the heat resistance during extrusion was evaluated as "X".
[0045] Furthermore, as shown in Examples 1-12 in Tables 1 and 2, and Comparative Examples 1-5 in Table 3, by setting the total amount of added polyethylene oxide and calcium laurate to 0.03 parts by mass or more, the stability of the outer diameter during high-speed extrusion can be evaluated as "○". This is thought to be due to improved internal lubricity of the admixture, resulting in a more stable supply condition in the extruder, especially in the metering zone, which led to the stabilization of the outer diameter.
[0046] Next, we will explain the relationship between the processing conditions for the insulating layer 12 of the electric wire 10 shown in Figure 1 and the evaluation items described above. Table 4 is a table showing the relationship between the processing conditions for the insulating layer of the insulated electric wire and the evaluation results of its characteristics. The composition of each example shown in Table 4 was the same as that of Example 3 shown in Table 1. In each example shown in Table 4, the coating thickness of the insulating layer and the irradiation amount when irradiating with an electron beam were changed during the test. In addition, the "heat aging resistance test" item shown in Table 4 was evaluated as follows. That is, after irradiation with an electron beam, the polyvinyl chloride resin composition constituting the insulating layer of the electric wire was heated under conditions of maintaining 136°C for 168 hours, and the change in the elongation rate of the polyvinyl chloride resin composition before and after heating was evaluated. An elongation rate after heating of 65% or more compared to the elongation rate before heating was evaluated as ○, and an elongation rate of less than 65% was evaluated as ×.
[0047] [Table 4]
[0048] As shown in Examples 13-17 of Table 4, the "Stability of outer diameter dimensions during high-speed extrusion," "Heat resistance during extrusion," "Pressure resistance during extrusion / after electron beam irradiation," and "Degree of crosslinking" all received a "○" rating even when the conditions of the insulating layer were changed. However, the "Heat aging test" result for Examples 16 and 17 was "×". Examples 16 and 17 are examples where electron beam irradiation was performed at a high irradiation intensity. It was found that while the degree of crosslinking can be improved by irradiating with an electron beam at a high irradiation intensity, a decrease in heat resistance can be confirmed. The degree of crosslinking value for Example 16 was 1.4 times that of Example 15, and the degree of crosslinking value for Example 17 was 1.6 times that of Example 15. Based on these results, when performing a crosslinking test by irradiating the insulating layer 12 shown in Figure 1 with an electron beam, it is preferable that the thickness of the insulating layer 12 covering the conductor 11 is 0.2 mm or less, and that the insulating layer 12 is crosslinked by irradiating it with an electron beam of an intensity of 5 Mrad or less.
[0049] The present invention is not limited to the embodiments and examples described above, and can be modified in various ways without departing from its spirit. [Industrial applicability]
[0050] The present invention is applicable to electric wires and cables. [Explanation of Symbols]
[0051] 10 Electric wire 11 Conductors 12 Insulating layer 20 Cables 21. Sheath (insulating layer)
Claims
1. A method for manufacturing an insulated electric wire having a conductor and an insulating layer covering the conductor, A step of preparing a polyvinyl chloride resin composition comprising 100 parts by mass of polyvinyl chloride, 4 parts by mass or more of hydrotalcite, 0.03 parts by mass or more of polyethylene oxide and / or calcium laurate, 0.1 parts by mass or more of a phenolic antioxidant, a plasticizer, and TMPT (trimethylolpropane triacrylate), wherein the phenolic antioxidant includes a phenolic antioxidant added to the plasticizer, and the value obtained by dividing the amount of the phenolic antioxidant added by the amount of TMPT (trimethylolpropane triacrylate) added is 0.033 (rounded to the fourth decimal place), A step of forming the insulating layer by extruding the polyvinyl chloride resin composition, The process includes a step of crosslinking the polyvinyl chloride resin composition by irradiating the insulating layer with an electron beam. A method for manufacturing insulated electric wires.
2. A method for manufacturing an insulated electric wire having a conductor and an insulating layer covering the conductor, A step of preparing a polyvinyl chloride resin composition comprising 100 parts by mass of polyvinyl chloride, 4 parts by mass or more of hydrotalcite, 0.03 parts by mass or more of polyethylene oxide and / or calcium laurate, 0.1 parts by mass or more of a phenolic antioxidant, a plasticizer, and TMPT (trimethylolpropane triacrylate), wherein the phenolic antioxidant includes a phenolic antioxidant added to the plasticizer, and the value obtained by dividing the amount of the phenolic antioxidant added by the amount of TMPT (trimethylolpropane triacrylate) added is 0.034 (rounded to the fourth decimal place), A step of forming the insulating layer by extruding the polyvinyl chloride resin composition, The process includes a step of crosslinking the polyvinyl chloride resin composition by irradiating the insulating layer with an electron beam. A method for manufacturing insulated electric wires.
3. A method for manufacturing an insulated electric wire having a conductor and an insulating layer covering the conductor, A step of preparing a polyvinyl chloride resin composition comprising 100 parts by mass of polyvinyl chloride, 4 parts by mass or more of hydrotalcite, 0.03 parts by mass or more of polyethylene oxide and / or calcium laurate, 0.1 parts by mass or more of a phenolic antioxidant, a plasticizer, and TMPT (trimethylolpropane triacrylate), wherein the phenolic antioxidant includes a phenolic antioxidant added to the plasticizer, and the value obtained by dividing the amount of the phenolic antioxidant by the amount of TMPT (trimethylolpropane triacrylate) added is 0.029 (rounded to the fourth decimal place), A step of forming the insulating layer by extruding the polyvinyl chloride resin composition, The process includes a step of crosslinking the polyvinyl chloride resin composition by irradiating the insulating layer with an electron beam. A method for manufacturing insulated electric wires.
4. A method for manufacturing an insulated electric wire having a conductor and an insulating layer covering the conductor, A step of preparing a polyvinyl chloride resin composition comprising 100 parts by mass of polyvinyl chloride, 4 parts by mass or more of hydrotalcite, 0.03 parts by mass or more of polyethylene oxide and / or calcium laurate, 0.1 parts by mass or more of a phenolic antioxidant, a plasticizer, and TMPT (trimethylolpropane triacrylate), wherein the phenolic antioxidant includes a phenolic antioxidant added to the plasticizer, and the value obtained by dividing the amount of the phenolic antioxidant added by the amount of TMPT (trimethylolpropane triacrylate) added is 0.042 (rounded to the fourth decimal place), A step of forming the insulating layer by extruding the polyvinyl chloride resin composition, The process includes a step of crosslinking the polyvinyl chloride resin composition by irradiating the insulating layer with an electron beam. A method for manufacturing insulated electric wires.
5. The method for manufacturing an insulated wire according to any one of Claims 1 to 4, wherein the step of crosslinking the polyvinyl chloride resin composition is to crosslink the polyvinyl chloride resin composition by irradiating the insulating layer with an electron beam of an intensity of 5 Mrad or less.
Citation Information
Patent Citations
Vinyl chloride resin composition
JP1994032956A
Surface-treated hydrotalcite and polyvinyl chloride resin composition containing it
JP2003040614A
Adhesive tape
JP2017119806A
Vinyl chloride resin composition, insulated wire, cable, method for producing insulated wire, and method for producing cable
JP2020186286A