solid-state batteries

By using a Li composite oxide and oxide glass-based solid electrolyte in the negative electrode layer with specific density and content ratios, the interfacial resistance is reduced, improving lithium ion conduction and energy density in solid-state batteries.

JP7948420B2Active Publication Date: 2026-11-11MURATA MFG CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2025509760
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-12-27
Publication Date
2026-11-11
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

Conventional solid-state batteries face challenges in reducing interfacial resistance between the negative electrode active material and the solid electrolyte, which hinders the movement of lithium ions and limits the volume energy density.

Method used

The solid-state battery incorporates a negative electrode layer composed of a Li composite oxide and an oxide glass-based solid electrolyte, with a solid electrolyte content of 20-60% by mass and a density ratio of 0.3-0.6, ensuring a dense contact interface for lithium ion conduction.

Benefits of technology

This configuration reduces interfacial resistance, enhances lithium ion mobility, and improves the volumetric energy density and charge/discharge efficiency to 85% or more.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948420000003
    Figure 0007948420000003
  • Figure 0007948420000004
    Figure 0007948420000004
  • Figure 0007948420000001
    Figure 0007948420000001
Patent Text Reader

Abstract

One embodiment of the present invention provides a solid state battery comprising a negative electrode layer containing an oxide glass-based solid electrolyte and a negative electrode active material that contains a Li composite oxide, wherein the content of the solid electrolyte in the negative electrode layer relative to the total amount of the solid electrolyte and the negative electrode active material is 20-60 mass%, and the ratio (B / A) of the actual density B of the negative electrode active material to the true density A of the negative electrode active material is 0.3-0.6.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a solid-state battery. [Background technology]

[0002] Rechargeable batteries, which can be repeatedly charged and discharged, have long been used in a variety of applications. For example, rechargeable batteries are used as power sources for electronic devices such as smartphones and laptop computers.

[0003] In secondary batteries, liquid electrolytes are generally used as a medium for ion transfer that contributes to charging and discharging. In other words, so-called electrolyte solutions are used in secondary batteries. However, safety is generally required in such secondary batteries in terms of preventing electrolyte leakage. Furthermore, since organic solvents used in electrolytes are flammable substances, safety is required in that respect as well. Therefore, research is progressing on solid-state batteries that use solid electrolytes instead of liquid electrolytes.

[0004] A solid-state battery comprises a battery element having a positive electrode layer, a negative electrode layer, and a solid electrolyte interposed between the electrode layers of the positive and negative electrode layers. The positive electrode layer contains a positive electrode active material and a solid electrolyte, and the negative electrode layer contains a negative electrode active material and a solid electrolyte. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2015-144061 [Patent Document 2] Japanese Patent Publication No. 2019-77573 [Patent Document 3] Japanese Patent Publication No. 2020-068188 [Overview of the project] [Problems that the invention aims to solve]

[0006] The inventors of the present application have newly found that conventional solid-state batteries have points that can be improved, and there is a need to take countermeasures for such points.

[0007] Specifically, in a solid-state battery, the electrode layer that is a constituent element thereof, particularly the negative electrode layer, may consist of a combination of a negative electrode active material containing a Li composite oxide and a garnet-type oxide-based solid electrolyte. However, the garnet-type oxide-based solid electrolyte is difficult to form a dense interface with the particles of the negative electrode active material, and it is difficult to reduce the porosity inside the electrode. As a result, the interfacial resistance between the active material and the solid electrolyte in the negative electrode increases, which may make it difficult for lithium ions to move across this interface. As a result, there is a risk that the volume energy density of the solid-state battery cannot be increased.

[0008] The present invention has been made in view of such problems. That is, an object of the present invention is to provide a solid-state battery provided with a negative electrode layer capable of reducing the interfacial resistance between the active material and the solid electrolyte. [Means for Solving the Problems]

[0009] To achieve the above object, in one embodiment of the present invention, the solid-state battery comprises a negative electrode layer including a negative electrode active material containing a Li composite oxide and an oxide glass-based solid electrolyte, the content of the solid electrolyte is 20 mass% or more and 60 mass% or less with respect to the total amount of the negative electrode active material and the solid electrolyte in the negative electrode layer, and the ratio (B / A) of the actual density B of the negative electrode active material to the true density A of the negative electrode active material is 0.3 or more and 0.6 or less. [Effects of the Invention]

[0010] According to the solid-state battery according to one embodiment of the present invention, it is possible to provide a negative electrode layer capable of reducing the interfacial resistance between the active material and the solid electrolyte. [Brief Description of the Drawings]

[0011] [Figure 1] Figure 1 is a schematic external perspective view of a solid-state battery according to one embodiment of the present invention. [Figure 2] Figure 2 is a schematic cross-sectional view of the AA cross-section of the solid-state battery shown in Figure 1, viewed in the direction of the arrow. [Modes for carrying out the invention]

[0012] The solid-state battery of the present invention will be described in detail below. Although the description will be made with reference to the drawings as necessary, the illustrations are for illustrative purposes only to help understand the present invention, and the appearance and dimensional ratios may differ from the actual product.

[0013] In this specification, "cross-sectional view" refers to the form of a solid-state battery's stacked structure as viewed from a direction approximately perpendicular to the stacking direction (simply put, the form when cut by a plane parallel to the thickness direction of the layers). Furthermore, in this specification, "plan view" or "plan view shape" refers to a sketch of the object as viewed from above or below along the thickness direction of the layers (i.e., the stacking direction mentioned above).

[0014] In this specification, “up and down” and “left and right” as used directly or indirectly correspond to the up and down and left and right directions in the figures, respectively. Unless otherwise specified, the same reference numeral or symbol indicates the same member, part, or has the same meaning. In a preferred embodiment, the vertical downward direction (i.e., the direction in which gravity acts) can be considered as “downward,” and the opposite direction as “upward.”

[0015] In this invention, the term "solid-state battery" broadly refers to a battery whose constituent elements are solid, and narrowly refers to an all-solid-state battery whose constituent elements (particularly preferably all constituent elements) are solid. In one preferred embodiment, the solid-state battery in this invention is a stacked solid-state battery configured such that each layer constituting the battery constituent unit is stacked on top of each other, and preferably each such layer is made of a fired body. The "solid-state battery" is a so-called "rechargeable battery" that can be repeatedly charged and discharged. The term "rechargeable battery" is not overly restrictive and may also include, for example, energy storage devices.

[0016] The features of this invention relate to the positive electrode layer contained in a solid-state battery. Below, in order to understand the overall structure of the solid-state battery, the basic configuration of the solid-state battery of this invention will be described. However, the configuration of the solid-state battery described here is merely an example for understanding the invention and does not limit the invention.

[0017] [Basic Configuration of Solid-State Batteries] Figure 1 is a schematic external perspective view of a solid-state battery according to one embodiment of the present invention. Figure 2 is a schematic cross-sectional view of the AA cross section of the solid-state battery of Figure 1, viewed in the direction of the arrow. The solid-state battery has at least positive electrode and negative electrode layers and a solid electrolyte. Specifically, as shown in Figures 1 and 2, the solid-state battery 200 includes a solid-state battery stack 100 which includes a battery component unit consisting of a positive electrode layer 10A, a negative electrode layer 10B, and a solid electrolyte 20 interposed at least between them.

[0018] The solid battery 200 according to the present invention is a solid battery stack 100 comprising at least one battery component unit consisting of a positive electrode layer 10A, a negative electrode layer 10B, and a solid electrolyte layer 20 interposed between them, along the stacking direction L; and The solid battery stack 100 has a positive electrode terminal 40A and a negative electrode terminal 40B provided on opposite sides of the stack. In the solid-state battery stack 100, the positive electrode layer 10A and the negative electrode layer 10B are stacked alternately via a solid electrolyte layer 20.

[0019] In solid-state batteries, each constituent layer may be formed by firing, and the positive electrode layer, negative electrode layer, and solid electrolyte layer may form fired layers. Preferably, the positive electrode layer, negative electrode layer, and solid electrolyte layer are each fired integrally with each other, so that the solid-state battery laminate forms an integrally fired body.

[0020] The positive electrode layer is an electrode layer containing at least a positive electrode active material. The positive electrode layer may further contain a solid electrolyte. In one preferred embodiment, the positive electrode layer is composed of a sintered body containing at least positive electrode active material particles and solid electrolyte particles. On the other hand, the negative electrode layer is an electrode layer containing at least a negative electrode active material. The negative electrode layer may further contain a solid electrolyte. In one preferred embodiment, the negative electrode layer is composed of a sintered body containing at least negative electrode active material particles and solid electrolyte particles. A positive electrode layer having such a configuration may be called a "composite positive electrode," and similarly, a negative electrode layer may be called a "composite negative electrode."

[0021] The positive electrode active material and the negative electrode active material are materials that are involved in electron transfer in a solid-state battery. Charging and discharging occur when ions move (conduce) between the positive electrode layer and the negative electrode layer via a solid electrolyte, resulting in electron transfer. It is preferable that each electrode layer of the positive and negative electrode layers is capable of intercalating and deintercalating lithium ions or sodium ions. In other words, it is preferable that the solid-state battery is an all-solid-state secondary battery in which charging and discharging occur through the movement of lithium ions or sodium ions between the positive and negative electrode layers via a solid electrolyte.

[0022] Examples of positive electrode active materials included in the positive electrode layer include lithium-containing layered oxides and lithium-containing oxides having a spinel-type structure. Examples of lithium-containing layered oxides include LiCoO2 and LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 Examples include O2. Examples of lithium-containing oxides having a spinel-type structure include LiMn2O4 and LiNi 0.5 Mn 1.5 Examples include O4.

[0023] Furthermore, the positive electrode active material capable of intercalating and deintercalating sodium ions can be selected from sodium-containing layered oxides, sodium-containing oxides having a spinel-type structure, and the like.

[0024] The positive electrode layer and / or negative electrode layer may contain a conductive material. Examples of conductive materials included in the positive electrode layer and negative electrode layer include at least one of metallic materials such as silver, palladium, gold, platinum, aluminum, copper, and nickel, as well as carbon.

[0025] Furthermore, the positive electrode layer and / or negative electrode layer may contain a sintering aid. Examples of sintering aids include at least one selected from the group consisting of lithium oxide, sodium oxide, potassium oxide, boron oxide, silicon oxide, bismuth oxide, and phosphorus oxide.

[0026] The thicknesses of the positive electrode layer and the negative electrode layer are not particularly limited, but for example, they may be 2 μm or more and 50 μm or less, and especially 5 μm or more and 30 μm or less, respectively.

[0027] (Positive electrode current collecting layer / Negative electrode current collecting layer) Although not essential elements of the electrode layer, the positive electrode layer and the negative electrode layer may each comprise a positive electrode current collector layer 11A and a negative electrode current collector layer 11B, respectively. The positive electrode current collector layer and the negative electrode current collector layer may each be in the form of foil. However, if greater emphasis is placed on aspects such as improved electronic conductivity through integral firing, reduction of manufacturing costs for solid-state batteries, and / or reduction of internal resistance of solid-state batteries, the positive electrode current collector layer and the negative electrode current collector layer may each be in the form of a fired body.

[0028] It is preferable to use materials with high conductivity for the positive electrode current collector that constitutes the positive electrode current collector layer and the negative electrode current collector that constitutes the negative electrode current collector. For example, silver, palladium, gold, platinum, aluminum, copper, and / or nickel may be used. The positive electrode current collector and the negative electrode current collector may each have an electrical connection part for electrically connecting to the outside, and may be configured to be electrically connectable to terminals.

[0029] Furthermore, if the positive electrode current collector layer and the negative electrode current collector layer are in the form of a fired body, they may be composed of a fired body containing a conductive material and a sintering aid. The conductive material included in the positive electrode current collector layer and the negative electrode current collector layer may be selected from materials similar to those that may be included in the positive electrode layer and the negative electrode layer. The sintering aid included in the positive electrode current collector layer and the negative electrode current collector layer may be selected from materials similar to those that may be included in the positive electrode layer and the negative electrode layer.

[0030] (solid electrolyte) The solid electrolyte is a material that can conduct lithium ions or sodium ions. This solid electrolyte can form a lithium-ion conductive layer between the positive electrode layer and the negative electrode layer. Furthermore, the solid electrolyte can also be contained within the positive electrode layer and the negative electrode layer.

[0031] The solid electrolyte layer may contain a sintering aid. The sintering aid included in the solid electrolyte layer may be selected from materials similar to those that may be included in the positive electrode layer and the negative electrode layer.

[0032] The thickness of the solid electrolyte layer is not particularly limited. The thickness of the solid electrolyte layer located between the positive electrode layer and the negative electrode layer may be, for example, 1 μm to 15 μm, and more particularly 1 μm to 5 μm.

[0033] (electrode separation part) The solid battery 200 of the present invention may further have electrode separation portions (also referred to as "margin layers" or "margin portions") 30 (30A, 30B).

[0034] The electrode separation section 30A (positive electrode separation section) is positioned around the positive electrode layer 10A, thereby separating the positive electrode layer 10A from the negative electrode terminal 40B. The electrode separation section 30B (negative electrode separation section) is positioned around the negative electrode layer 10B, thereby separating the negative electrode layer 10B from the positive electrode terminal 40A. Although not particularly limited, the electrode separation section 30 may be composed of one or more materials selected from the group consisting of, for example, solid electrolytes, insulating materials, and mixtures thereof.

[0035] The solid electrolyte that can constitute the electrode separation section 30 can be made of the same material as the solid electrolyte that can constitute the solid electrolyte layer.

[0036] The insulating material that may constitute the electrode separation section 30 may be a material that does not conduct electricity, i.e., a non-conductive material. Although not particularly limited, the insulating material may be, for example, glass or ceramic material. For example, glass material may be selected as the insulating material. Although not particularly limited, the glass material may be at least one selected from the group consisting of soda-lime glass, potash glass, borate glass, borosilicate glass, barium borosilicate glass, borite glass, barium borate glass, bismuth borosilicate glass, bismuth zinc borate glass, bismuth silicate glass, phosphate glass, aluminophosphate glass, and phosphate glass. Furthermore, although not particularly limited, ceramic materials include at least one selected from the group consisting of aluminum oxide (Al2O3), boron nitride (BN), silicon dioxide (SiO2), silicon nitride (Si3N4), zirconium oxide (ZrO2), aluminum nitride (AlN), silicon carbide (SiC), and barium titanate (BaTiO3).

[0037] (Terminals) The solid-state battery 200 of the present invention is generally provided with terminals (external terminals) 40 (40A, 40B). In particular, positive and negative terminals 40A and 40B are provided in pairs on the side surface of the solid-state battery. More specifically, a positive terminal 40A connected to the positive electrode layer 10A and a negative terminal 40B connected to the negative electrode layer 10B are provided in pairs. Since terminals 40A and 40B can be provided so as to cover at least one side surface of the solid-state battery, they can also be called "end electrodes". Such terminals 40 (40A, 40B) can be made of a material with high conductivity. The material of the terminals 40 is not particularly limited, but examples include at least one conductive material selected from the group consisting of silver, gold, platinum, aluminum, copper, tin, and nickel.

[0038] Terminals 40 (40A, 40B) may further contain a sintering aid. Examples of sintering aids include materials similar to those that may be included in the positive electrode layer 10A. In one preferred embodiment, terminals 40 (40A, 40B) are composed of a sintered body containing at least a conductive material and a sintering aid.

[0039] (outer layer material) The solid-state battery 200 of the present invention typically further comprises an outer layer material 60. The outer layer material 60 is generally formed on the outermost surface of the solid-state battery and is intended to provide electrical, physical, and / or chemical protection. The material constituting the outer layer material 60 is preferably excellent in insulating properties, durability, and / or moisture resistance, and is environmentally safe. For example, glass, ceramics, thermosetting resins, photocurable resins, and mixtures thereof can be used.

[0040] The glass material that can constitute the outer layer can be the same material as the glass material that can constitute the electrode separation section. Similarly, the ceramic material that can constitute the outer layer can be the same material as the ceramic material that can constitute the electrode separation section.

[0041] [Features of the Solid-State Battery of the Present Invention] The inventors of the present invention have diligently studied solutions to reduce interfacial resistance between the active material and the solid electrolyte in the negative electrode layer of a solid-state battery. As a result, the inventors have newly devised the present invention, which has technical features related to a specific combination of negative electrode active material and solid electrolyte in the negative electrode layer, as well as a specific range of density of the negative electrode active material and content of the solid electrolyte.

[0042] Specifically, the present invention has the technical features that the negative electrode layer comprises a negative electrode active material containing a Li composite oxide and an oxide glass-based solid electrolyte, wherein the content of the solid electrolyte in the negative electrode layer is 20% by mass or more and 60% by mass or less relative to the total amount of the negative electrode active material and the solid electrolyte, and the ratio of the actual density B of the negative electrode active material to the true density A of the negative electrode active material (B / A) is 0.3 or more and 0.6 or less.

[0043] In this specification, "negative electrode active material and solid electrolyte in the negative electrode layer" refers to the negative electrode active material and solid electrolyte located in areas other than the voids that can be formed in the negative electrode layer of the final solid-state battery (corresponding to the finished product).

[0044] According to the above technical features, when the solid electrolyte content in the negative electrode layer is 20% by mass or more and 60% by mass or less, the actual density B of the negative electrode active material in the manufactured battery can be ensured at a predetermined ratio (0.3 or more and 0.6 or less) to the true density A of the negative electrode active material. For example, the true density A of the negative electrode active material is 3.0 g / cm³. 3 More than 4.0g / cm 3 The following is an example: 3.5 g / cm³ 3 This is possible. Furthermore, when the solid electrolyte content in the negative electrode layer is 20% by mass or more, a predetermined amount of solid electrolyte is ensured compared to when it is less than 20% by mass.

[0045] As a result, the contact interface between the negative electrode active material and the solid electrolyte in the negative electrode layer can be made denser, allowing for the suitable formation of lithium ion conduction paths. In other words, the interfacial resistance between the negative electrode active material and the solid electrolyte in the negative electrode layer can be reduced, making it easier for lithium ions to move across this interface. As a result, the internal resistance of the battery can be reduced, and the volumetric energy density can be improved.

[0046] Furthermore, when the solid electrolyte content in the negative electrode layer is 60% by mass or less, the ratio of the actual density B of the negative electrode active material to the true density A (B / A) can be ensured to be 0.3 or higher, compared to when it exceeds 60% by mass. As a result, in the manufactured battery, the negative electrode active material occupies a predetermined amount in the negative electrode layer, and the interparticle distance of the negative electrode active material in the negative electrode layer can be kept to a distance that allows for the formation of suitable electron paths.

[0047] Based on the above, it becomes possible to secure a discharge capacity that can achieve a charge / discharge efficiency of 85% or more (above a predetermined standard value), thereby effectively improving the battery characteristics of the solid-state battery.

[0048] In this specification, "true density of negative electrode active material" refers to the density inherent to a given type of negative electrode active material, and "true density of solid electrolyte" refers to the density inherent to a given type of solid electrolyte. The true densities of the negative electrode active material and solid electrolyte can be calculated by a gas-phase displacement method using helium gas. The volume of the sample is determined by changing the pressure and volume, and then the weight is measured to calculate the true density. In addition, in this specification, "actual density of negative electrode active material" refers to the volume density of the negative electrode active material in the negative electrode layer of a solid-state battery after fabrication.

[0049] Furthermore, the actual density B of the negative electrode active material after battery fabrication can be calculated using the true density A of the negative electrode active material, the true density C of the solid electrolyte, the porosity E within the negative electrode, and the content F of the negative electrode active material and the content G of the solid electrolyte in the negative electrode layer. The calculation formula is as follows. The volume ratio of the negative electrode active material (V1) = (100-E) × F / A / (F / A + G / C) Actual density of the negative electrode active material after molding (B) = (A × V1) / 100

[0050] Note that the porosity inside the electrode can be calculated by subjecting the obtained solid-state battery to ion milling to form a smooth cross-section, and observing the cross-section at a magnification of 5000 times using an SEM. For this calculation, software called Image J can be used. In addition, the content rate F of the negative electrode active material and the content rate G of the solid electrolyte can also be calculated by the same method.

[0051] Note that in the present invention, the content rate of the solid electrolyte relative to the total amount of the negative electrode active material and the solid electrolyte described above is preferably 30 mass% or more and 50 mass% or less. In this case, compared with the case where the content rate is 20 mass%, the content rate of the solid electrolyte in the negative electrode layer increases by 10 mass%, whereby the contact interface between the negative electrode active material and the solid electrolyte in the negative electrode layer can be made denser, and the lithium ion conduction path can be formed more favorably.

[0052] When the content rate of the solid electrolyte in the negative electrode layer is 50 mass% or less, compared with the case where the content rate is 60 mass%, the amount of the negative electrode active material increases by 10 mass%, whereby the inter-particle distance of the negative electrode active material in the negative electrode layer can be suppressed to a distance that allows an electron path to be formed more favorably. According to the above, it is possible to secure a discharge capacity that can achieve a charge-discharge efficiency equal to or higher than a predetermined reference value (95% or more), and it is possible to more favorably improve the battery characteristics of the solid-state battery.

[0053] In addition, when the content rate of the solid electrolyte relative to the total amount of the negative electrode active material and the solid electrolyte in the negative electrode layer is uniformly a predetermined amount (for example, 40 mass%), the ratio (C / A) of the true density C of the solid electrolyte to the true density A of the negative electrode active material can be 0.55 or more and 0.9 or less. For example, the true density C of the solid electrolyte is 2.0 g / cm 3 or more and 3.0 g / cm 3 or less, preferably 2.0 g / cm 3 or more and 2.5 g / cm 3 or less.

[0054] If the ratio C / A is within this range, the actual density B of the negative electrode active material in the manufactured battery can be secured at a predetermined ratio (0.3 or more and 0.6 or less) to the true density A of the negative electrode active material. On the other hand, if the ratio C / A is outside this range (specifically, 0.51), the actual density B of the negative electrode active material in the manufactured battery cannot be secured at a predetermined ratio (0.3 or more and 0.6 or less) to the true density A of the negative electrode active material.

[0055] Based on the above, in the manufactured battery, a predetermined amount of negative electrode active material (and solid electrolyte) is secured in the negative electrode layer, making it possible to create a dense contact interface between the negative electrode active material and the solid electrolyte in the negative electrode layer, and thus suitably form lithium ion conduction paths.

[0056] Furthermore, when the above ratio C / A is 0.6 or more and 0.75 or less, the above ratio B / A may be 0.35 or more and 0.5 or less. In this case, the above ratio B / A can be increased compared to when the ratio C / A is less than 0.6. As a result, in the manufactured battery, the negative electrode active material (and solid electrolyte) is more suitably secured in a predetermined amount in the negative electrode layer, so that the contact interface between the negative electrode active material and the solid electrolyte in the negative electrode layer can be made denser, and lithium ion conduction paths can be formed more suitably.

[0057] The Li composite oxide included in the above-mentioned negative electrode active material can be an oxide containing Li and a transition metal element. For example, it can be an oxide containing Li and at least one metal element selected from the group consisting of titanium (Ti), silicon (Si), tin (Sn), chromium (Cr), iron (Fe), niobium (Nb), and molybdenum (Mo). For instance, the Li composite oxide included in the above-mentioned negative electrode active material can be an oxide containing Li and Ti. When an oxide containing Li and Ti is used, a high energy density can be obtained while suppressing the expansion and contraction of the negative electrode layer during charging and discharging.

[0058] The oxide glass-based solid electrolyte for the negative electrode layer has the advantage of contributing to a reduction in the porosity within the negative electrode, and can be, for example, lithium borosilicate glass. Lithium borosilicate glass is an oxide-based glass material containing at least lithium (Li), silicon (Si), and boron (B) as constituent elements, and can be, for example, 50Li4SiO4·50Li3BO3. Lithium borosilicate glass may be advantageous in that it has a low glass transition temperature and can form a dense negative electrode layer.

[0059] Furthermore, the above-mentioned solid electrolyte may further include, in addition to lithium borosilicate glass as a glass-based solid electrolyte, other solid electrolytes used in known solid batteries. Such solid electrolytes may be one or more of the following: crystalline solid electrolytes, glass-based solid electrolytes different from lithium borosilicate glass, and glass-ceramic solid electrolytes. Crystalline solid electrolytes include, for example, oxide-based crystalline materials. Examples of oxide-based crystalline materials include lithium-containing phosphate compounds having a nasicone structure, oxides having a perovskite structure, oxides having a garnet-type or garnet-type similar structure, and oxide glass-ceramic lithium-ion conductors.

[0060] Li x M y Examples include (PO4)3 (1≦x≦2, 1≦y≦2, where M is at least one selected from the group consisting of titanium (Ti), germanium (Ge), aluminum (Al), gallium (Ga), and zirconium (Zr)). An example of a lithium-containing phosphate compound having a nastycon structure is, for example, Li 1.2 Al 0.2 Ti 1.8 Examples include (PO4)3. An example of an oxide having a perovskite structure is La 0.55 Li 0.35 Examples include TiO3. An example of an oxide having a garnet-type or garnet-type similar structure is Li7La3Zr2O. 12Examples include the following. The crystalline solid electrolyte may contain polymer materials (for example, polyethylene oxide (PEO)).

[0061] Other glass-based solid electrolytes that can be used besides lithium borosilicate glass include 30Li2S·26B2S3·44LiI, 63Li2S·36SiS2·1Li3PO4, 57Li2S·38SiS2·5Li4SiO4, 70Li2S·30P2S5, and 50Li2S·50GeS2.

[0062] Glass-ceramic solid electrolytes include, for example, oxide-based glass-ceramic materials. Examples of oxide-based glass-ceramic materials include phosphate compounds containing lithium, aluminum, and titanium (LATP) and phosphate compounds containing lithium, aluminum, and germanium (LAGP). For example, LATP is Li 1.07 Al 0.69 Ti 1.46 Examples include (PO4)3. Also, LAGP is, for example, Li 1.5 Al 0.5 Ge 1.5 (PO4), etc.

[0063] For example, in addition to lithium borosilicate glass, the solid electrolyte may further contain an oxide having a garnet-type or garnet-type similar structure, from the viewpoint of improving ionic conductivity.

[0064] [Manufacturing method for solid-state batteries] The solid-state battery of the present invention can be manufactured by a printing method such as screen printing, a green sheet method using a green sheet, or a combination of these methods. The following details will describe the cases where the printing method and the green sheet method are employed for the purpose of understanding the present invention, but the present invention is not limited to these methods. In other words, the solid-state battery may be manufactured in accordance with conventional solid-state battery manufacturing methods. Furthermore, the chronological order of the following descriptions is merely for explanatory purposes and is not necessarily binding.

[0065] (Formation process of solid-state battery stack precursor) In this process, several types of pastes are used as inks, such as paste for the positive electrode layer, paste for the negative electrode layer, paste for the solid electrolyte layer, paste for the positive electrode current collector layer, paste for the negative electrode current collector layer, paste for the electrode separation section, and paste for the outer layer material. In other words, a solid-state battery stacking precursor with a predetermined structure is formed on a support substrate by applying and drying the paste using a printing method.

[0066] During printing, a solid-state battery stacking precursor corresponding to a predetermined solid-state battery structure can be formed on a substrate by sequentially stacking printed layers with predetermined thickness and pattern shape. The type of pattern formation method is not particularly limited as long as it is a method capable of forming the predetermined pattern, but for example, it may be one or more of the following: screen printing and gravure printing.

[0067] The paste can be prepared by wet mixing predetermined constituent materials for each layer, appropriately selected from the group consisting of positive electrode active material particles, negative electrode active material particles, conductive material, solid electrolyte material, current collector layer material, insulating material, and sintering aid, as well as other materials mentioned above, with an organic vehicle in which an organic material is dissolved in a solvent.

[0068] The paste for the positive electrode layer includes, for example, positive electrode active material particles, a solid electrolyte material, an organic material and a solvent, and optionally a sintering aid.

[0069] The paste for the negative electrode layer includes, for example, negative electrode active material particles, a solid electrolyte material, an organic material and a solvent, and optionally a sintering aid.

[0070] The paste for the solid electrolyte layer comprises, for example, a solid electrolyte material, an organic material, and a solvent, and optionally a sintering aid.

[0071] The paste for the positive electrode current collector layer comprises a conductive material, an organic material, and a solvent, and optionally a sintering aid.

[0072] The paste for the negative electrode current collector layer comprises a conductive material, an organic material, and a solvent, and optionally a sintering aid.

[0073] The paste for the electrode separation section includes, for example, a solid electrolyte material, an insulating material, an organic material, and a solvent, and optionally a sintering aid.

[0074] The paste for the outer layer material includes, for example, an insulating material, an organic material, and a solvent, and optionally a sintering aid.

[0075] The organic material contained in the paste is not particularly limited, but at least one polymer material selected from the group consisting of polyvinyl acetal resin, cellulose resin, polyacrylic resin, polyurethane resin, polyvinyl acetate resin, and polyvinyl alcohol resin can be used.

[0076] The type of solvent is not particularly limited, but may be one or more of the following organic solvents: butyl acetate, N-methylpyrrolidone, toluene, terpineol, and N-methylpyrrolidone.

[0077] In wet mixing, media can be used, specifically the ball mill method or the visco mill method. Alternatively, wet mixing methods that do not use media may be used, such as the sand mill method, high-pressure homogenizer method, or kneader dispersion method.

[0078] The support substrate is not particularly limited as long as it is a support capable of supporting each paste layer, but for example, it may be a release film with a release treatment applied to one surface. Specifically, a substrate made of a polymer material such as polyethylene terephthalate can be used. If the paste layers are to be subjected to the firing process while remaining on the substrate, the substrate may be one that exhibits heat resistance to the firing temperature.

[0079] Alternatively, a green sheet can be formed from each paste, and the resulting green sheets can be stacked to create a solid-state battery stacking precursor.

[0080] In detail, the support substrates to which each paste is applied are dried on a hot plate heated to 30°C to 90°C, thereby forming positive electrode layer green sheets, negative electrode layer green sheets, solid electrolyte layer green sheets, positive electrode current collector layer green sheets, negative electrode current collector layer green sheets, electrode separation section green sheets, and / or outer layer material green sheets, each having a predetermined shape and thickness, on each support substrate (e.g., PET film).

[0081] Next, each green sheet is peeled off the substrate. After peeling, the green sheets of each component are stacked sequentially along the stacking direction to form a solid-state battery stacking precursor. After stacking, a solid electrolyte layer, insulating layer, and / or protective layer may be applied to the side regions of the electrode green sheets by screen printing.

[0082] (Firing process) In the firing process, the solid-state battery stacking precursor is subjected to firing. Although this is merely an example, firing is carried out by removing organic materials by heating in a nitrogen gas atmosphere containing oxygen gas or in air at, for example, 200°C or higher, and then heating in a nitrogen gas atmosphere or in air at, for example, 300°C to 500°C. Firing can be carried out while pressurizing the solid-state battery stacking precursor at 20 to 100 MPa in the stacking direction (and possibly in the stacking direction and perpendicular to the stacking direction).

[0083] Through such firing processes, a solid-state battery stack is formed, ultimately resulting in the desired solid-state battery.

[0084] (Process for forming positive and negative terminals) For example, the positive electrode terminal is bonded to the solid-state battery stack using a conductive adhesive, and the negative electrode terminal is also bonded to the solid-state battery stack using a conductive adhesive. This attaches both the positive and negative electrode terminals to the solid-state battery stack. As a result, the desired solid-state battery can be obtained.

[0085] The embodiments of the present invention have been described above, but these are merely typical examples. Therefore, the present invention is not limited thereto, and those skilled in the art will easily understand that various embodiments are conceivable without altering the essence of the invention. [Examples]

[0086] The following describes some examples.

[0087] <Example 1> (Process for manufacturing green sheets for solid electrolyte layers) First, a solid electrolyte consisting of halogen-containing lithium borosilicate glass (60Li2O-10SiO2-30B2O3, in which 10% of the oxygen is replaced with chlorine) and an acrylic binder was mixed in a mass ratio of lithium borosilicate glass:acrylic binder = 70:30. The true density of the solid electrolyte used in Example 1 was 2.5 g / cm³. 3 That was the case.

[0088] Next, the obtained mixture was mixed with butyl acetate as a solvent to a solid content of 30% by mass. This mixture was then stirred with 5 mm diameter zirconia balls for 4 hours to obtain a paste for the solid electrolyte layer. Subsequently, this paste was applied onto a release film and dried at 80°C for 20 minutes to produce a green sheet for the solid electrolyte layer as a precursor for the solid electrolyte layer.

[0089] (Process for manufacturing green sheets for positive electrode material layer) First, lithium cobalt oxide (LiCoO2) was prepared. Next, LiCoO2 as the positive electrode active material, the solid electrolyte used in the green sheet for the solid electrolyte layer mentioned above, and an acrylic binder were mixed in a mass ratio of LiCoO2:solid electrolyte:binder = 70:20:10. Then, the resulting mixture was mixed with terpineol so that the solid content was 60% by mass. The resulting mixture was then stirred with 5 mm diameter zirconia balls for 1 hour to obtain a paste for the positive electrode material layer. Subsequently, this paste was applied onto a release film and dried at 80°C for 20 minutes to prepare a green sheet for the positive electrode material layer, which served as a precursor for the positive electrode layer.

[0090] (Process for manufacturing the green sheet for the negative electrode material layer) First, as the negative electrode active material, Li4Ti5O 12 (Merck, part number 915939), and the solid electrolyte used in the above-mentioned green sheet for the solid electrolyte layer, along with an acrylic binder, are combined as Li4Ti5O 12 The solid electrolyte and binder were mixed in a mass ratio of 72:18:10. The true density of the negative electrode active material used was 3.5 g / cm³. 3 That was the case.

[0091] Next, the obtained mixture was mixed with terpineol so that the solid content was 60% by mass. Then, the obtained mixture was stirred with 5 mm diameter zirconia balls for 1 hour to obtain a paste for the negative electrode material layer. Subsequently, this paste was applied onto a release film and dried at 80°C for 20 minutes to prepare a green sheet for the negative electrode material layer as a precursor for the negative electrode material layer.

[0092] (Process for manufacturing the green sheet for the positive electrode current collector) First, carbon powder (manufactured by Resonaq, product code VGCF(registered trademark)-F) was mixed as a conductive material, along with the solid electrolyte used in the above-mentioned green sheet for the solid electrolyte layer and an acrylic binder, in a mass ratio of carbon powder:solid electrolyte:binder = 70:20:10. Next, the resulting mixture was mixed with terpineol so that the solid content was 60% by mass. Then, the resulting mixture was stirred with 5 mm diameter zirconia balls for 1 hour to obtain a paste for the positive electrode current collector layer. Subsequently, this paste was applied onto a release film and dried at 80°C for 20 minutes to produce a green sheet for the positive electrode current collector layer as a precursor for the positive electrode current collector layer.

[0093] (Process for manufacturing the green sheet for the negative electrode current collector) A green sheet for the negative electrode current collector was fabricated using the same process as described above for fabricating the green sheet for the positive electrode current collector.

[0094] (Process for manufacturing the green sheet for the outer layer) First, alumina particle powder (manufactured by Kojun Kagaku Kenkyusha, product number γ-Al2O3 alumina), the solid electrolyte used in the above-mentioned solid electrolyte layer green sheet, and an acrylic binder were mixed in a mass ratio of carbon powder:solid electrolyte:binder = 70:20:10. Next, the resulting mixture was mixed with terpineol so that the solid content was 60% by mass. Then, the resulting mixture was stirred with 5 mm diameter zirconia balls for 1 hour to obtain a paste for the main surface exterior material. Subsequently, this paste was applied onto a release film and dried to prepare a green sheet for the outer layer material as a precursor for the outer layer material.

[0095] (Process for manufacturing the green sheet for the electrode separation section) Similar to the process for producing the outer layer green sheet described above, a green sheet for the electrode separation section was produced as a precursor for the electrode separation section.

[0096] (Laminate fabrication process) Using the green sheets obtained as described above, a laminate having the configuration shown in Figures 1 and 2 was fabricated as follows. Specifically, first, each green sheet was processed into the shape shown in Figures 1 and 2, and then released from the release film. Next, each green sheet was stacked in order corresponding to the configuration of the battery element shown in Figures 1 and 2, and then thermocompressed by heating to 100°C while applying pressure in the thickness direction. This yielded a laminate as a precursor for a battery element.

[0097] (Degreasing and sintering process of the laminate) The resulting laminate was heated at 300°C for 10 hours to remove the acrylic binder contained in each green sheet. Then, the laminate from which the acrylic binder had been removed was heated at 350°C for 10 minutes under pressure in the thickness direction at 20-100 MPa, and subsequently cooled in air for 1 hour to obtain a sintered laminate.

[0098] (Terminal manufacturing process) Next, a solid-state battery was fabricated by bonding a silver plate to the first and second end faces (or sides) of a laminate, where the positive electrode current collector layer and the negative electrode current collector layer are exposed, using a conductive adhesive (thermosetting silver paste), thereby forming the positive and negative electrode terminals.

[0099] In addition, along with, or instead of, the above-mentioned laminate fabrication, degreasing, and sintering processes, multiple green sheets for the solid electrolyte layer, punched out to a diameter of φ16 mm, and the above-mentioned green sheets for the negative electrode material layer, punched out to a diameter of φ8 mm were sequentially bonded onto SUS304 (φ16 mm, thickness 0.3 mm). Subsequently, the binder contained in the green sheets was degreased at 300°C using a muffle furnace KDF P-90 (manufactured by Denken). The degreased sample was heated at 350°C for 10 minutes under pressure in the thickness direction at 20-100 MPa in a pressure sintering machine P-5058-00 (manufactured by NPA Systems), and then sintered by cooling in air for 30 minutes to obtain a cell element. Subsequently, a half-cell used in this evaluation was fabricated by punching out a 100 μm thick Li foil to a diameter of φ10 mm and bonding it to the cell element. Furthermore, in the fabricated cells, the mass-based content ratio of the negative electrode active material to the solid electrolyte became 80:20 after the removal of the acrylic binder.

[0100] <Example 2> In Example 2, in the process of manufacturing the green sheet for the negative electrode material layer in Example 1, Li4Ti5O 12 The solid electrolyte and binder were mixed in a mass ratio of 63:27:10. Apart from this, the solid battery was manufactured using the same method as in Example 1. In the manufactured cell, the mass-based content ratio of the negative electrode active material to the solid electrolyte became 70:30 after the removal of the acrylic binder.

[0101] <Example 3> In Example 3, in the process of manufacturing the green sheet for the negative electrode material layer in Example 1, Li4Ti5O 12 The solid electrolyte and binder were mixed in a mass ratio of 54:36:10. Apart from this, the solid battery was manufactured using the same method as in Example 1. In the manufactured cell, the mass-based content ratio of the negative electrode active material to the solid electrolyte became 60:40 after the removal of the acrylic binder.

[0102] <Example 4> In Example 4, in the process of manufacturing the green sheet for the negative electrode material layer in Example 1, Li4Ti5O 12 The solid electrolyte and binder were mixed in a mass ratio of 45:45:10. Apart from this, the solid battery was manufactured using the same method as in Example 1. In the manufactured cell, the mass-based content ratio of the negative electrode active material to the solid electrolyte became 50:50 after the removal of the acrylic binder.

[0103] <Example 5> In Example 5, in the process of manufacturing the green sheet for the negative electrode material layer in Example 1, Li4Ti5O 12 The solid electrolyte and binder were mixed in a mass ratio of 36:54:10. Apart from this, the solid battery was manufactured using the same method as in Example 1. In the manufactured cell, the mass-based content ratio of the negative electrode active material to the solid electrolyte became 40:60 after the removal of the acrylic binder.

[0104] <Example 6> In Example 6, similar to Example 3, in the process of manufacturing the green sheet for the negative electrode material layer, Li4Ti5O 12 The solid electrolyte and binder were mixed in a mass ratio of 54:36:10. That is, in the fabricated cell, as the acrylic binder was removed, the mass-based content ratio of the negative electrode active material to the solid electrolyte became 60:40. On the other hand, in Example 6, unlike Example 3, the composition ratio of the main components of the solid electrolyte, Li, B, and Si, was adjusted. For example, by reducing the Si content, the true density of the solid electrolyte was 2.2 g / cm³. 3 We used the following:

[0105] <Example 7> In Example 7, similar to Example 3, in the process of manufacturing the green sheet for the negative electrode material layer, Li4Ti5O 12The solid electrolyte and binder were mixed in a mass ratio of 54:36:10. That is, in the fabricated cell, as the acrylic binder was removed, the mass-based content ratio of the negative electrode active material to the solid electrolyte became 60:40. On the other hand, in Example 7, unlike Example 3, the composition ratio of the main components of the solid electrolyte, Li, B, and Si, was adjusted, for example, by further reducing the Si content ratio, resulting in a true density of 2.0 g / cm³ for the solid electrolyte. 3 We used the following:

[0106] <Comparative Example 1> In Comparative Example 1, in the process of manufacturing the green sheet for the negative electrode material layer in Example 1, Li4Ti5O 12 The solid electrolyte and binder were mixed in a mass ratio of 81:9:10. Apart from this, the solid battery was manufactured using the same method as in Example 1. In the manufactured cell, the mass-based content ratio of the negative electrode active material to the solid electrolyte became 90:10 after the removal of the acrylic binder.

[0107] <Comparative Example 2> In Comparative Example 2, in the process of manufacturing the green sheet for the negative electrode material layer in Example 1, Li4Ti5O 12 The solid electrolyte and binder were mixed in a mass ratio of 27:63:10. Apart from this, the solid battery was manufactured using the same method as in Example 1. In the manufactured cell, the mass-based content ratio of the negative electrode active material to the solid electrolyte became 30:70 after the removal of the acrylic binder.

[0108] <Comparative Example 3> In Comparative Example 3, similar to Example 3, in the process of manufacturing the green sheet for the negative electrode material layer, Li4Ti5O 12 The solid electrolyte and binder were mixed in a mass ratio of 54:36:10. That is, in the prepared cell, as the acrylic binder was removed, the mass-based content ratio of the negative electrode active material to the solid electrolyte became 60:40. On the other hand, in Comparative Example 3, unlike Example 3, the composition ratio of the main components of the solid electrolyte, Li, B, and Si, was adjusted, for example, by further reducing the Si content ratio, resulting in a true density of 1.8 g / cm³ as a solid electrolyte.3 We used the following:

[0109] [Measurement details] (Measurement of battery characteristics) The above half-cell was placed in a low-temperature incubator (Yamato Scientific Co., Ltd., model number: IQ822), and then a charge-discharge test was performed using a charge-discharge evaluation device (Toyo System Co., Ltd., model number: TOSCAT-3100). The charge-discharge conditions were as follows: The cell's rated capacity was set to 1C, and it was charged to a predetermined potential with a constant current of 0.05C (cutoff voltage 4V). It was then discharged to a predetermined potential with a constant current of 0.05C, and after reaching the predetermined potential, it was discharged in constant voltage mode until the current could be reduced to 0.005C (cutoff voltage 1.0V). The charge-discharge capacity of the half-cell was confirmed by this charge-discharge test.

[0110] [Measurement result 1] Table 1 shows the measurement results for Examples 1 to 5 and Comparative Examples 1 to 2. In these examples and comparative examples, the charging capacity was approximately 170 mAh / g. Based on this value, the charge / discharge efficiency was calculated from the ratio of discharge capacity to charging capacity. A charge / discharge efficiency of 85% or higher was judged as ○, a charge / discharge efficiency of 95% or higher was judged as ◎, and a charge / discharge efficiency of less than 85% or where the discharge capacity could not be measured was judged as ×.

[0111] [Table 1]

[0112] As shown in Examples 1 to 5 of Table 1, it was found that in the obtained batteries, when the content ratio (by mass) of negative electrode active material to solid electrolyte is 80:20 to 40:60, that is, when the content of solid electrolyte is 20% by mass or more and 60% by mass or less relative to the total amount of negative electrode active material and solid electrolyte, and the ratio of the actual density B of the negative electrode active material to the true density A of the negative electrode active material (B / A) is 0.3 or more and 0.6 or less, the charge-discharge efficiency is 85% or more.

[0113] In particular, it was found that when the content ratio of the negative electrode active material to the solid electrolyte is 70:30 to 50:50, that is, when the content of the solid electrolyte is between 30% and 50% by mass relative to the total amount of the negative electrode active material and solid electrolyte, the charge-discharge efficiency is 95% or more. The density of the negative electrode active material B after fabrication in this case is 0.3 g / cm³. 3 More than 0.5g / cm 3 The results were as follows:

[0114] On the other hand, as shown in Comparative Example 1, when the mass content ratio of the negative electrode active material to the solid electrolyte was 90:10, that is, when the solid electrolyte content was 10% by mass relative to the total amount of the negative electrode active material and solid electrolyte, and the porosity in the negative electrode layer was 20.0% by volume or less, a battery could be manufactured, but the discharge capacity could not be measured. From the above, it was found that because the content of the negative electrode active material was high and the content of the solid electrolyte was low, the contact interface between the negative electrode active material and the solid electrolyte could not be made dense, and thus a lithium ion conduction path could not be formed.

[0115] Furthermore, as shown in Comparative Example 2, when the mass content ratio of the negative electrode active material to the solid electrolyte is 30:70, that is, when the solid electrolyte content is 70% by mass relative to the total amount of the negative electrode active material and solid electrolyte, and the ratio of the actual density B of the negative electrode active material to the true density A (B / A) is less than 0.3, it was found that the charge-discharge efficiency is less than 85%. From the above, it was found that when the solid electrolyte content in the negative electrode layer exceeds 60% by mass and the ratio (B / A) is less than 0.3, the interparticle distance of the negative electrode active material cannot be set to a distance that allows for the formation of electron paths.

[0116] From the above, it was found that in the range of Examples 1 to 5 described above, the contact interface between the negative electrode active material and the solid electrolyte can be made dense, suitable lithium ion conduction paths can be formed, and the interparticle distance of the negative electrode active material in the negative electrode layer can be set to a distance suitable for the formation of electron paths.

[0117] [Measurement result 2] Table 2 shows the measurement results for Examples 3, 6, 7, and Comparative Example 3. In these examples and comparative examples, as with Example 1, the charging capacity was approximately 170 mAh / g, and the charge / discharge efficiency was calculated from the ratio of discharge capacity to charging capacity based on this value. A charge / discharge efficiency of 85% or higher was judged as ○, a charge / discharge efficiency of 95% or higher was judged as ◎, and a charge / discharge efficiency of less than 85% or where the discharge capacity could not be measured was judged as ×.

[0118] [Table 2]

[0119] As shown in Examples 3, 6, and 7 of Table 2, in the obtained batteries, when the content ratio of negative electrode active material to solid electrolyte is uniformly 60:40, that is, when the content of solid electrolyte is uniformly 40% by mass relative to the total amount of negative electrode active material and solid electrolyte, and the ratio of the true density C of the solid electrolyte to the true density A of the negative electrode active material (C / A) is 0.55 or more and 0.9 or less, the above ratio B / A becomes 0.3 or more and 0.5 or less, and it was found that a charge / discharge efficiency of 85% or more is ensured. In particular, as shown in Examples 3 and 6, when the above ratio C / A is 0.6 or more and 0.75 or less, the ratio B / A becomes 0.35 or more and 0.5 or less, and it was found that a charge / discharge efficiency of 95% or more is ensured. On the other hand, when the ratio (C / A) is less than 0.55, the above ratio B / A becomes less than 0.3, and it was found that the charge / discharge efficiency is less than 85%.

[0120] From the above, it was found that in the negative electrode layer, when a predetermined amount of solid electrolyte is contained relative to the total amount of negative electrode active material and solid electrolyte, the ratio of the true density C of the solid electrolyte to the true density A of the negative electrode active material (C / A) is also related to the charge-discharge efficiency, i.e., the battery characteristics.

[0121] Furthermore, the present invention may take the following embodiments. <1> The negative electrode layer comprises a negative electrode active material containing a Li composite oxide and a solid electrolyte made of an oxide glass system. The content of the solid electrolyte in the negative electrode layer is 20% by mass or more and 60% by mass or less, relative to the total amount of the negative electrode active material and the solid electrolyte. A solid-state battery in which the ratio (B / A) of the actual density B of the negative electrode active material to the true density A of the negative electrode active material is 0.3 or more and 0.6 or less. <2> The solid electrolyte content is 30% by mass or more and 50% by mass or less relative to the total amount of the negative electrode active material and the solid electrolyte. <1> Solid-state batteries as described above. <3> The ratio (C / A) of the true density C of the solid electrolyte to the true density A of the negative electrode active material is 0.55 or more and 0.9 or less. <1> or <2> Solid-state batteries as described above. <4> If the C / A is 0.6 or more and 0.75 or less, then the B / A is 0.35 or more and 0.5 or less. <3> Solid-state batteries as described above. <5> The true density A of the aforementioned negative electrode active material is 3.0 g / cm³. 3 More than 4.0g / cm 3 The following is: <1> ~ <4> A solid-state battery as described in any of the following. <6> The true density C of the solid electrolyte is 2.0 g / cm³. 3 More than 3.0g / cm 3 The following is: <3> or <4> Solid-state batteries as described above. <7> The Li composite oxide is an oxide containing Li and a transition metal element. <1> ~ <6> A solid-state battery as described in any of the following. <8> The Li composite oxide is an oxide containing Li and Ti. <7> Solid-state batteries as described above. <9> The solid electrolyte is lithium borosilicate glass. <1> ~ <8> A solid-state battery as described in any of the following. <10> The positive electrode further comprises a positive electrode layer, wherein the positive electrode layer comprises a positive electrode active material containing a Li composite oxide and an oxide glass-based solid electrolyte. <1> ~ <9> A solid-state battery as described in any of the following. <11> The Li composite oxide of the positive electrode active material is an oxide containing Li and Co. <10> Solid-state batteries as described above. [Industrial applicability]

[0122] The solid-state battery of the present invention can be used in a variety of fields where energy storage is anticipated. While this is merely an example, the solid-state battery of the present invention can be used in the electrical, information, and communication fields where mobile devices are used (e.g., the electrical and electronic equipment field or mobile device field, including small electronic devices such as mobile phones, smartphones, laptops and digital cameras, activity trackers, arm computers, electronic paper, RFID tags, card-type electronic money, and smartwatches), household and small-scale industrial applications (e.g., power tools, golf carts, household, caregiving, and industrial robots), large-scale industrial applications (e.g., forklifts, elevators, and port cranes), transportation systems (e.g., hybrid vehicles, electric vehicles, buses, trains, electric assist bicycles, electric motorcycles, etc.), power grid applications (e.g., various power generation, road conditioners, smart grids, and general household energy storage systems), medical applications (medical equipment such as earphones and hearing aids), pharmaceutical applications (medication management systems, etc.), as well as IoT fields and space and deep-sea applications (e.g., space probes, submersible research vessels, etc.). [Explanation of symbols]

[0123] 10: Electrode layer 10A: Positive electrode layer 10B: Negative electrode layer 11: Electrode current collecting layer 11A: Positive electrode current collecting layer 11B: Negative electrode current collecting layer 20: Solid electrolyte layer 30: Electrode separation part 30A: Positive electrode separation section 30B: Negative electrode separation section 40: Terminals 40A: Positive terminal 40B: Negative terminal 60: Outer layer material 100: Solid-state battery stack 200: Solid state battery

Claims

1. The negative electrode layer comprises only a negative electrode active material containing a Li composite oxide and a solid electrolyte containing an oxide glass-based solid electrolyte. The content of the solid electrolyte in the negative electrode layer relative to the total amount of the negative electrode active material and the solid electrolyte is 20% by mass or more and 60% by mass or less. A solid-state battery in which the ratio (B / A) of the actual density B of the negative electrode active material to the true density A of the negative electrode active material is 0.3 or more and 0.6 or less.

2. The solid battery according to claim 1, wherein the solid electrolyte content is 30% by mass or more and 50% by mass or less relative to the total amount of the negative electrode active material and the solid electrolyte.

3. The solid battery according to claim 1, wherein the ratio (C / A) of the true density C of the solid electrolyte to the true density A of the negative electrode active material is 0.55 or more and 0.9 or less.

4. The solid battery according to claim 3, wherein when the C / A is 0.6 or more and 0.75 or less, the B / A is 0.35 or more and 0.5 or less.

5. The true density A of the aforementioned negative electrode active material is 3.0 g / cm³. 3 4.0g / cm or more 3 The solid battery according to claim 1, which is as follows:

6. The true density C of the solid electrolyte is 2.0 g / cm³. 3 3.0g / cm or more 3 The solid battery according to claim 3, which is as follows:

7. The solid-state battery according to claim 1, wherein the Li composite oxide is an oxide containing Li and a transition metal element.

8. The solid-state battery according to claim 7, wherein the Li composite oxide is an oxide containing Li and Ti.

9. The solid battery according to claim 1, wherein the solid electrolyte is lithium borosilicate glass.

10. The solid-state battery according to claim 1, further comprising a positive electrode layer, wherein the positive electrode layer comprises a positive electrode active material containing a Li composite oxide and an oxide glass-based solid electrolyte.

11. The solid battery according to claim 10, wherein the Li composite oxide of the positive electrode active material is an oxide containing Li and Co.

Citation Information

Patent Citations

  • Lithium battery

    JP2001126757A

  • Method for manufacturing electrode complex, electrode complex and battery

    JP2015144061A

  • Method of manufacturing sintered body containing spinel type lithium titanate

    JP2019077573A

  • Solid-state lithium ion secondary battery

    JP2020068188A

  • Lithium ion cell and method for manufacturing same

    WO2018123479A1