Coating agent and coating method
A coating agent with boric acid, zinc compounds, mica, metal sources, and silicon carbide, applied with an alkali metal silicate solution, addresses refractory deterioration by enhancing heat resistance and reducing gas penetration and clinker formation in high-temperature environments.
Patent Information
- Application Number
- JP2025219023
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-12-02
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-12-02
AI Technical Summary
Refractories used in high-temperature environments suffer from porous surfaces that allow penetration of corrosive gases, leading to spalling and clinker formation, which deteriorate the materials.
A coating agent comprising powdered components such as boric acid compounds, zinc compounds, mica, metal sources, inorganic heat-resistant aggregates, and silicon carbide, applied with an alkali metal silicate solution, forms a coating that enhances heat resistance and reduces gas penetration, oxidation, and clinker formation.
The coating agent provides high heat resistance, reducing defects like oxidation, spalling, and clinker formation, while maintaining structural integrity under high temperatures.
Smart Images

Figure 0007948651000001_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a coating agent and a coating method. BACKGROUND ART
[0002] Conventionally, refractory bricks, precast refractory bricks, and castable refractories are used in high-temperature atmospheres. These refractories are produced, for example, by molding fine particle powders of high-melting-point materials such as zirconia, alumina, and silica, followed by firing at high temperatures. Therefore, these refractories usually have porous surfaces, into which high-temperature corrosive gas easily penetrates. In addition, when molten fly ash adheres to the refractories, clinkers are formed. The refractories deteriorate due to spalling caused by high-temperature corrosive gas and collapse of the clinkers.
[0003] Patent Document 1 discloses a coating treatment method for a heat-resistant and oxidation-resistant coating material, characterized in that an aqueous solution containing at least aluminum oxide, zirconium dioxide, silicic anhydride, kaolinite, graphite, and potassium silicate, as well as one or more components selected from tricobalt tetroxide, cobaltous oxide, cobaltic oxide, Raney cobalt, and manganese dioxide, one or more components selected from sodium borate, metaborate, tetraborate, pyroborate, borate, tetraborate, boron trioxide, sodium pentaborate, and ammonium borate, one or more components selected from zinc hydroxide, zinc carbonate, lead trioxide, and lead silicate, or one or more components selected from magnesium oxide, magnesium borate, magnesium sulfate, and magnesium fluoride, is applied to an object to be treated, and the resultant is fired at a temperature lower than the melting point of the object to be treated.
[0004] Patent Document 2 discloses an aqueous solution of a heat-resistant and oxidation-resistant coating material, which contains an aqueous alkali metal silicate compound solution, a boric acid compound, a zinc compound, and mica, and further contains a powdered inorganic heat-resistant aggregate having a predetermined particle size in the range of 20 μm to 100 μm, with a particle size distribution in which 90% or more of the particles have a particle size within ±10% of the predetermined particle size. PRIOR ART DOCUMENTS PATENT DOCUMENTS
[0005] [Patent Document 1] Patent No. 3399650 [Patent Document 2] Patent No. 4716196 [Overview of the project] [Problems that the invention aims to solve]
[0006] The purpose of this disclosure is to provide a coating agent that can impart high heat resistance. [Means for solving the problem]
[0007] This disclosure includes the following aspects: [1] (A) Powdered components and (B) Alkali metal silicate solution, The aforementioned (A) powder component is At least one of a boric acid compound and a zinc compound, Mica and, One or more metal sources selected from the group consisting of ferrosilicon, manganese compounds, and cobalt compounds, Inorganic heat-resistant aggregate, A coating agent containing silicon carbide. [2] The coating agent according to [1] above, wherein the powder component (A) further comprises glass frit. [3] The inorganic heat-resistant aggregate comprises one or more selected from the group consisting of magnesium compounds, zirconium dioxide, aluminum oxide, anhydrous silicic acid, kaolinite, titanium dioxide, and silicon nitride, as described in the coating agent of [1] or [2] above. [4] Applying one of the above coating agents [1] to [3] to the object to be treated, A coating method comprising applying the coating agent and then firing the workpiece at a temperature lower than its melting point. [Effects of the Invention]
[0008] According to the present disclosure, a coating agent capable of imparting high heat resistance, and a coating method using this coating agent are provided. [Brief Description of the Drawings]
[0009] [Figure 1A] This is a photograph of a slag outlet weir with a formed coating before use (Application Example 1). [Figure 1B] This is a photograph of a slag outlet weir with a formed coating 12 months after the start of use (Application Example 1). [Figure 2A] This is a photograph of an uncoated slag outlet weir before use (Application Example 1). [Figure 2B] This is a photograph of an uncoated slag outlet weir 10 months after the start of use (Application Example 1). [Figure 3] This is a photograph of a precast refractory brick with a formed coating 210 days after the start of use (Application Example 2). [Figure 4] This is a photograph of an uncoated precast refractory brick 210 days after the start of use (Application Example 2). [Figure 5] This is a photograph of a water wall of a biomass boiler with a formed coating 314 days after the start of use (Application Example 3). [Modes for Carrying Out the Invention]
[0010] [Coating Agent] The coating agent of the present disclosure comprises (A) a powder component and (B) an alkali metal silicate solution. Since component (A) and component (B) undergo a chemical reaction to cure, they are mixed before use. By separating component (A) and component (B), long-term storage (for example, 2 to 4 years) becomes possible.
[0011] The powder component (A) includes at least one of a boric acid compound and a zinc compound, mica, one or more metal sources selected from the group consisting of ferrosilicon, manganese compounds and cobalt compounds, an inorganic heat-resistant aggregate, and silicon carbide. Such a coating agent can form a coating film having excellent heat resistance.
[0012] Heat resistance refers to the performance of reducing defects caused by heating at high temperatures (for example, 600°C or higher). Examples of the above defects include oxidation, thermal deterioration, occurrence of spalling, formation of clinker, and strength reduction. The performance of reducing at least one of oxidation, thermal deterioration, spalling, clinker, and strength reduction is referred to as heat resistance.
[0013] The coating agent of the present disclosure can particularly suppress oxidation and thermal deterioration that may occur in a workpiece containing an iron component and a carbon component under heating at 700°C or higher (further 800°C or higher).
[0014] The coating agent of the present disclosure contains silicon carbide. Silicon carbide suppresses penetration of high-temperature corrosive gas into the interior of the workpiece (refractory). This improves the oxidation resistance of the workpiece. Therefore, various metals can be used as the workpiece. Silicon carbide also increases the far-infrared emissivity of the coating film. As a result, heat conduction into the interior of the workpiece is suppressed to reduce the thermal load, and energy for cooling can be reduced.
[0015] Silicon carbide hardly forms bonds with other components of the coating agent. Therefore, fly ash hardly adheres to the surface of the coating agent, and clinker formation is reduced. Furthermore, even when clinker is formed, it easily peels off from the surface of the coating agent under its own weight. These effects suppress deterioration of the workpiece.
[0016] The coating agent of the present disclosure includes a metal source and a silicon source (for example, an alkali metal silicate solution). The coating film obtained by the coating agent of the present disclosure may contain a ceramic metal compound obtained by reacting a metal and silicon. While the coating film softens at high temperatures, it cures and shrinks when the temperature decreases, so it can follow the expansion or contraction of the workpiece. Therefore, even with a rapid temperature change, cracking and peeling caused by the difference in expansion coefficient from the workpiece (particularly, a metal refractory) are unlikely to occur.
[0017] The solid content concentration of the coating agent in this disclosure is not particularly limited and is set as appropriate depending on the application and purpose. The solid content concentration of the coating agent is adjusted by the mixing ratio of (B) alkali metal silicate solution.
[0018] The coating agents of this disclosure are preferably substantially free of organic substances. The coating agents may be inorganic. "Organic substance" means a compound containing carbon atoms (C) and hydrogen atoms (H). "Inorganic coating agent" means a coating agent that is substantially free of organic substances. In inorganic coating agents, the presence of unavoidable organic substances is permissible. In inorganic coating agents, the presence of organic substances below the detection limit is permissible.
[0019] Solids are also called non-volatile components. Solids are the residue after heating. The solids concentration can be calculated according to JIS K 5601-1-2, the method for measuring residue after heating, for example, from the residue after heating a coating agent at 200°C for 20 minutes.
[0020] The average particle size is the particle size (D50) at which the cumulative volume, measured by a laser diffraction particle size analyzer, reaches 50%.
[0021] The coating agent and coating method in the embodiments of this disclosure will be described in detail below, but the present invention is not limited to these embodiments.
[0022] (A) Powdered ingredients (A) The powder component comprises at least one of a boric acid compound and a zinc compound, mica, one or more metal sources selected from the group consisting of ferrosilicon, manganese compounds and cobalt compounds, an inorganic heat-resistant aggregate, and silicon carbide. (A) Each component contained in the powder component is usually in powder form.
[0023] (Silicon carbide) As mentioned above, silicon carbide (SiC) imparts high heat resistance to the coating. The silicon carbide may have a purity of 90% or higher.
[0024] The silicon carbide content is set appropriately according to the application and purpose. Preferably, the silicon carbide content is 2.0 to 30.0 parts by mass per 100 parts by mass of the powder component (A). This can further improve the adhesion between the coating and the object to be treated. The silicon carbide content may be 4.0 parts by mass or more, 5.0 parts by mass or more, or 6.0 parts by mass or more. The silicon carbide content may be 25.0 parts by mass or less, or 15.0 parts by mass or less. The silicon carbide content may be 4.0 to 25.0 parts by mass, 5.0 to 25.0 parts by mass, 5.0 to 15.0 parts by mass, or 6.0 to 15.0 parts by mass.
[0025] The average particle size of silicon carbide is, for example, 0.5 to 50.0 μm. The average particle size of silicon carbide may be 0.7 μm or more, 1.0 μm or more, or 1.5 μm or more. The average particle size of silicon carbide may be 30.0 μm or less, 20.0 μm or less, 10.0 μm or less, or 8.0 μm or less. The average particle size of silicon carbide may be 0.7 to 30.0 μm, 0.7 to 20.0 μm, 1.0 to 10.0 μm, or 1.5 to 8.0 μm.
[0026] (Borate compounds and zinc compounds) Boric acid compounds and zinc compounds can melt metal sources and inorganic heat-resistant aggregates at temperatures lower than their melting points. Therefore, the heat load on the workpiece is reduced during construction, and melting of the workpiece is avoided.
[0027] The product may contain at least one of a boric acid compound or a zinc compound (hereinafter referred to as the promoting component), and it is preferable that it contains at least a boric acid compound. It may also contain both a boric acid compound and a zinc compound. The effect of the zinc compound is more pronounced in the presence of a boric acid compound. When both a boric acid compound and a zinc compound are included, the mass ratio of the boric acid compound to the zinc compound (boric acid compound:zinc compound) may be, for example, 90:10 to 40:60, or 80:20 to 50:50.
[0028] The content of the accelerating component is set appropriately according to the application and purpose. The total content of the accelerating component is preferably 0.5 to 20.0 parts by mass per 100 parts by mass of (A) powder component. This makes the inorganic heat-resistant aggregate softer. The above content of the accelerating component may be 1.0 part by mass or more, 1.2 parts by mass or more, or 1.5 parts by mass or more. The above content of the accelerating component may be 18.0 parts by mass or less, or 15.0 parts by mass or less. The above content of the accelerating component may be 1.0 to 18.0 parts by mass, 1.2 to 18.0 parts by mass, or 1.5 to 15.0 parts by mass.
[0029] Examples of boric acid compounds include oxides, salts, and dehydration condensates of boric acid. Specific examples include boron trioxide, borates, diborates, tetraborates, pentaborates, metaboric acid, and polyboric acid. These can be used individually or in combination of two or more.
[0030] Substances that form salts with boric acid include, for example, sodium, ammonia, zinc, manganese, cobalt, nickel, potassium, lithium, and calcium. Zinc borate is treated as a boric acid compound.
[0031] The average particle size of borate compounds is, for example, 40.0 to 150.0 μm. The average particle size of borate compounds may be 50.0 μm or more, 55.0 μm or more, 60.0 μm or more, or 65.0 μm or more. The average particle size of borate compounds may be 120.0 μm or less, 100.0 μm or less, 90.0 μm or less, or 85.0 μm or less. The average particle size of borate compounds may be 50.0 to 120.0 μm, 55.0 to 100.0 μm, 60.0 to 90.0 μm, or 65.0 to 85.0 μm.
[0032] Examples of zinc compounds include zinc oxide, zinc hydroxide, zinc carbonate, and zinc silicate. These can be used individually or in combination of two or more.
[0033] The average particle size of the zinc compound may be 0.3 to 1.5 μm. The average particle size of the zinc compound may be 0.4 μm or more, or 0.5 μm or more. The average particle size of the zinc compound may be 1.2 μm or less, or 1.0 μm or less, or 0.9 μm or less. The average particle size of the zinc compound may be 0.3 to 1.2 μm, or 0.4 to 1.0 μm, or 0.5 to 0.9 μm.
[0034] (Maika) Mica plays a role in reducing cracks caused by the expansion and contraction of the coating.
[0035] The mica content is set appropriately according to the application and purpose. Preferably, the mica content is 0.2 to 20.0 parts by mass per 100 parts by mass of the powder component (A). This is expected to further reduce cracks. The mica content may be 0.3 parts by mass or more, 0.4 parts by mass or more, or 0.5 parts by mass or more. The mica content may be 15.0 parts by mass or less, or 12.0 parts by mass or less. The mica content may be 0.3 to 20.0 parts by mass, 0.4 to 15.0 parts by mass, or 0.5 to 12.0 parts by mass.
[0036] The average particle size of mica is, for example, 3.0 to 30.0 μm. The average particle size of mica may be 4.0 μm or more, 5.0 μm or more, 6.0 μm or more, or 6.5 μm or more. The average particle size of mica may be 28.0 μm or less, 25.0 μm or less, or 22.0 μm or less. The average particle size of mica may be 4.0 to 30.0 μm, 5.0 to 28.0 μm, 6.0 to 25.0 μm, or 6.5 to 22.0 μm.
[0037] (Ferrosilicon, manganese compounds, or cobalt compounds) Ferrosilicon, manganese compounds, and cobalt compounds are metal sources for coatings. These are used individually or in combination of two or more.
[0038] These metal sources can react with silicon atoms in the coating agent to form ceramic metal compounds. These ceramic metal compounds densify the coating. By covering the surface of the workpiece with a dense coating, the penetration of high-temperature corrosive gases into the workpiece is reduced. Furthermore, the ceramic metal compounds are resistant to oxidation, thus reducing oxidation of the coating.
[0039] Coatings containing ceramic metal compounds soften at high temperatures and harden and shrink as the temperature decreases, allowing them to follow the expansion or contraction of the treated object. Therefore, delamination between the coating and the treated object, especially metals, can be reduced. In addition, clinker is less likely to adhere to ceramic metal compounds.
[0040] Ferrosilicon is an iron alloy containing silicon. The iron component in ferrosilicon softens and melts during the firing process, forming a dense metallic film. Ferrosilicon may have an oxide coating. The oxide film suppresses the bonding between clinker and the iron component, further reducing clinker adhesion.
[0041] Examples of manganese compounds include natural manganese dioxide and electrolytic manganese. The purity of natural manganese dioxide should preferably be 65% or higher.
[0042] Examples of cobalt compounds include cobalt tetraoxide (Co3O4), cobalt trioxide (Co2O3), cobalt(II) oxide (CoO), and Raney cobalt.
[0043] The total content of these metal sources is set appropriately according to the application and purpose. Preferably, the total content of these metal sources is 10.0 to 80.0 parts by mass per 100 parts by mass of (A) powder component. This is expected to further suppress oxidation. The above content of these metal sources may be 15.0 parts by mass or more, and may be 20.0 parts by mass or more. The above content of these metal sources may be 75.0 parts by mass or less, and may be 60.0 parts by mass or less. The above content of these metal sources may be 15.0 to 75.0 parts by mass, and may be 20.0 to 60.0 parts by mass.
[0044] The average particle size of these metal sources is, for example, 2.0 to 150.0 μm. The average particle size of these metal sources may be 20.0 μm or more, 30.0 μm or more, or 50.0 μm or more. The average particle size of these metal sources may be 150.0 μm or less, 120.0 μm or less, or 100.0 μm or less. The average particle size of these metal sources may be 20.0 to 150.0 μm, 30.0 to 120.0 μm, or 50.0 to 100.0 μm.
[0045] (Inorganic heat-resistant aggregate) Inorganic heat-resistant aggregate is an inorganic material that does not melt under refractory operating conditions (e.g., above 600°C) on its own. Inorganic heat-resistant aggregate has a melting point of 1800°C or higher. Inorganic heat-resistant aggregate is a particulate inorganic material and does not contain mica. Inorganic heat-resistant aggregate has the function of reducing cracks caused by expansion and contraction of the coating. During firing, inorganic heat-resistant aggregate is incorporated into the above-mentioned metal source and melts together with it to form a ceramic metal compound. As a result, the coating can be made even denser.
[0046] Examples of inorganic heat-resistant aggregates include one or more selected from the group consisting of magnesium compounds, zirconium dioxide, aluminum oxide, anhydrous silicic acid, kaolinite, titanium oxide, and silicon nitride. Titanium oxide is particularly preferred because it enhances the corrosion resistance of the coating.
[0047] Examples of magnesium compounds include magnesium oxide, magnesium borate, magnesium sulfate, and magnesium fluoride. Magnesium borate is treated as a magnesium compound.
[0048] The amount of inorganic heat-resistant aggregate is set appropriately according to the application and purpose. Preferably, the amount of inorganic heat-resistant aggregate is 20.0 to 65.0 parts by mass per 100 parts by mass of the powder component (A). This is expected to further suppress the occurrence of cracks. The above amount of inorganic heat-resistant aggregate may be 30.0 parts by mass or more, 35.0 parts by mass or more, or 38.0 parts by mass or more. The above amount of inorganic heat-resistant aggregate may be 65.0 parts by mass or less, 55.0 parts by mass or less, or 53.0 parts by mass or less. The above amount of inorganic heat-resistant aggregate may be 30.0 to 65.0 parts by mass, 35.0 to 55.0 parts by mass, or 38.0 to 53.0 parts by mass.
[0049] The average particle size of inorganic heat-resistant aggregate is, for example, 2.0 to 150.0 μm. The average particle size of inorganic heat-resistant aggregate may be 15.0 μm or more, 20.0 μm or more, or 23.0 μm or more. The average particle size of inorganic heat-resistant aggregate may be 120.0 μm or less, or 100.0 μm or less. The average particle size of inorganic heat-resistant aggregate may be 15.0 to 120.0 μm, 20.0 to 120.0 μm, or 23.0 to 100.0 μm.
[0050] (Glass frit) The coating agent preferably further contains glass frit. The glass frit is obtained by crushing glass.
[0051] Glass frit has a low bending point of approximately 700°C or less. During firing, volatile components (e.g., solvents) contained in the coating agent evaporate, forming microscopic pores in the film. High-temperature corrosive gases can reach the surface of the workpiece through these pores. Glass frit rapidly coats the surface of the workpiece during firing, suppressing this corrosion (oxidation). In particular, workpieces containing iron and carbon components are easily oxidized, and suppressing this oxidation is useful.
[0052] Glass frit works even more effectively when the treated material remains at a temperature of 700-800°C for an extended period during firing. This is because a large amount of volatile components evaporate at 700-800°C, making it easier for pores to form.
[0053] Glass frit is particularly effective on materials (such as metals) that begin to oxidize at 700-800°C. This is because a glass frit coating is formed before oxidation of the material begins.
[0054] The inflection point of the glass frit is preferably less than 700.0°C. This allows the surface of the workpiece to be easily covered with glass frit before oxidation of the iron and carbon components contained in the workpiece occurs. The inflection point of the glass frit may be 400.0°C or higher, 450.0°C or higher, 500.0°C or higher, or 550.0°C or higher. The inflection point of the glass frit may be 690.0°C or lower, 680.0°C or lower, 650.0°C or lower, or 600.0°C or lower. The inflection point of the glass frit may be 400.0 to 690.0°C, 450.0 to 680.0°C, 500.0 to 650.0°C, or 550.0 to 600.0°C.
[0055] The bending point of glass frit should be the value specified in the manufacturer's specifications.
[0056] The glass frit content is set appropriately according to the application and purpose. Preferably, the glass frit content is 3.0 to 35.0 parts by mass per 100 parts by mass of the powder component (A). This can further improve the oxidation suppression effect. The glass frit content may be 4.0 parts by mass or more, 4.5 parts by mass or more, or 5.0 parts by mass or more. The glass frit content may be 30.0 parts by mass or less, 28.0 parts by mass or less, or 25.0 parts by mass or less. The glass frit content may be 4.0 to 30.0 parts by mass, 4.5 to 28.0 parts by mass, or 5.0 to 25.0 parts by mass.
[0057] The average particle size of glass frit is, for example, 10.0 to 200.0 μm. The average particle size of glass frit may be 20.0 μm or more, 30.0 μm or more, 40.0 μm or more, or 45.0 μm or more. The average particle size of glass frit may be 150.0 μm or less, 120.0 μm or less, 100.0 μm or less, or 85.0 μm or less. The average particle size of glass frit may be 20.0 to 150.0 μm, 30.0 to 120.0 μm, 40.0 to 100.0 μm, or 45.0 to 85.0 μm.
[0058] The type of glass is not particularly limited. Examples of glass include silicate glass, borate glass, bismuth silicate glass, borosilicate glass, vanadium oxide glass, and phosphate glass. These can be used individually or in combination of two or more types.
[0059] (Colloidal silica or silica powder) The coating agent may contain colloidal silica or silica powder. These facilitate the formation of siloxane bonds by alkali metal silicates.
[0060] Colloidal silica is also called silica sol. Colloidal silica is a colloidal particle mainly composed of silicon dioxide (SiO2) or hydrated silica. Colloidal silica can be amorphous. The particle shape is not limited and may be spherical or crushed.
[0061] The average particle size of colloidal silica is not limited and can be appropriately selected depending on the application and purpose. For example, the average particle size of colloidal silica may be between 3.0 and 100.0 nm. Multiple types of colloidal silica with different average particle sizes may be used in combination.
[0062] The average particle size of silica powder is, for example, 3.0 to 100.0 nm. The average particle size of silica powder may be 5.0 nm or larger, and may be 6.0 nm or larger. The average particle size of silica powder may be 50.0 nm or smaller, and may be 30.0 nm or smaller. The average particle size of silica powder may be 5.0 to 50.0 nm, and may be 6.0 to 30.0 nm.
[0063] The content of colloidal silica or silica powder is set appropriately according to the application and purpose. Preferably, the content of colloidal silica solids and silica powder is 20.0 to 28.0 parts by mass per 100 parts by mass of (A) powder component. This is expected to further improve adhesion. The above content of colloidal silica solids and silica powder may be 22.0 parts by mass or more. The above content of colloidal silica solids and silica powder may be 26.0 parts by mass or less, and may be 24.0 parts by mass or less. The above content of colloidal silica solids and silica powder may be 20.0 to 26.0 parts by mass, and may be 22.0 to 24.0 parts by mass.
[0064] (B) Alkali metal silicate solution (B) The alkali metal silicate solution contains alkali metal silicate and a solvent. The alkali metal silicate solution adjusts the viscosity of the coating agent, improves workability, and enhances adhesion.
[0065] The concentration of the alkali metal silicate solution is preferably 26 to 45 Bh. When the concentration of the alkali metal silicate solution is 26 Bh or higher, a glassy film is more easily formed. When the concentration of the alkali metal silicate solution is 45 Bh or lower, the coating agent is more easily mixed uniformly. Bh (Baume) can be calculated as (1 - 1 / specific gravity of alkali metal silicate) × 144.3). The concentration of the alkali metal silicate solution may be 18 Bh or higher, or 20 Bh or higher. The concentration of the alkali metal silicate solution may be 40 Bh or lower, or 35 Bh or lower. The concentration of the alkali metal silicate solution may be 18 to 40 Bh, or 20 to 35 Bh.
[0066] (Alkali metal silicates) Alkali metal silicates enhance the adhesion between the coating agent and the workpiece. They also act as an adhesive, bonding the other components of the coating agent to the workpiece, both before and after the metal source melts. Furthermore, because alkali metal silicates form siloxane bonds, they reduce the penetration of high-temperature corrosive gases into the workpiece and the oxidation of the workpiece.
[0067] Examples of alkali metals include one or more selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and francium (Fr).
[0068] Examples of alkali metal silicates include sodium silicate, potassium silicate, and lithium silicate. These can be used individually or in combination of two or more. Potassium silicate is particularly suitable.
[0069] Potassium silicate (K2SiO3) is a mixture of silicon dioxide (SiO2), potassium oxide (K2O), and water (H2O). The molar ratio of SiO2 to K2O is not limited.
[0070] (solvent) A typical solvent is water. Examples of water include purified water, deionized water, tap water, and deionized water.
[0071] The mixing ratio (A:B) of (A) the powder component and (B) the alkali metal silicate solution is set appropriately according to the application and purpose. The above mixing ratio (A:B) is preferably 60:40 to 30:70 by mass. This is expected to further improve adhesion. The above mixing ratio (A:B) may be 55:45 to 35:65.
[0072] [Object to be processed] Examples of materials to be processed include refractories. Refractories are materials used at high temperatures (e.g., 600°C or higher). Examples of refractories include refractory bricks, precast refractory bricks, castable refractories, metals, and C / C composites (Carbon Fiber Reinforced Carbon Composite).
[0073] By applying the coating agent of this disclosure to a C / C composite, it becomes possible to replace metal with a lighter material.
[0074] Specific examples of metal refractories include incinerator grates, heat exchanger pipes, heating furnace pipes, shochu furnaces, turbine cases, gas turbines, jet engine turbine blades, and internal combustion engines.
[0075] The melting point of the material to be treated is not particularly limited. The melting points of refractory bricks, precast refractory bricks, and castable refractories are, for example, 1800°C to 2800°C. The melting point of metallic refractories is, for example, 1300°C to 1800°C.
[0076] When used on refractory bricks, precast refractory bricks, and castable refractories, the coating agent is particularly useful as a gas barrier, sealing pores on the surface of the refractory material and preventing gas intrusion.
[0077] The following are examples of coating agents particularly suitable for refractory bricks, precast refractory bricks, castable refractories, and C / C composites. In the examples below, zinc borate can be substituted with other boric acid compounds or zinc compounds. Ferrosilicon and manganese dioxide can be substituted with other metal sources. Anhydrous silicic acid, etc., can be substituted with other inorganic heat-resistant aggregates.
[0078] [Table 1-1]
[0079] [Table 1-2]
[0080] The coating agent of this disclosure can follow the expansion and contraction of metals. Therefore, the coating agent of this disclosure is also suitable for metallic refractories. The coating agent of this disclosure softens gradually upon heating, allowing it to follow the expansion of metals. The coating agent of this disclosure also contracts as the temperature decreases, allowing it to follow the contraction of metals.
[0081] The following are examples of coating agents particularly suitable for metallic refractories. In the examples below, zinc borate can be substituted with other boric acid compounds. Zinc oxide can be substituted with other zinc compounds. Manganese dioxide can be substituted with other metal sources. Anhydrous silicic acid, etc., can be substituted with other inorganic heat-resistant aggregates.
[0082] [Table 2-1]
[0083] [Table 2-2]
[0084] [Coating Method] The coating method of this disclosure includes applying the above-mentioned coating agent to a workpiece and firing the workpiece at a temperature lower than its melting point (main firing) after applying the coating agent.
[0085] (1) Preparation of coating agent The coating agent is prepared, for example, as follows: First, the powder components are weighed in a predetermined mixing ratio and thoroughly mixed in a powder mixer to prepare (A) the powder components. Separately, alkali metal silicate is diluted with a solvent (water) to a predetermined concentration (for example, 26-45 Bh) to prepare (B) the alkali metal silicate solution. The powder components (A) and the alkali metal silicate solution (B) are mixed and thoroughly mixed. This yields the coating agent.
[0086] (A) The powder component and (B) the alkali metal silicate solution undergo a rapid curing reaction, so it is desirable to mix them immediately before use. They may also be mixed using a dispersion medium.
[0087] (2) Grant The method of applying the coating agent to the object to be treated is not limited. Application can be carried out, for example, by a spray gun such as an airless gun or a stucco gun, a brush, or a roller. Among these, an airless gun is preferred because it can apply the coating over a wide area in a short time.
[0088] For metal workpieces, it is desirable to degrease or blast-treat the surface before application. This improves the adhesion of the coating and removes oil. Chamfering the edges of the workpiece is also desirable from the viewpoint of suppressing peeling.
[0089] The amount of coating agent applied is not limited. The amount of coating agent applied can be determined so that the thickness of the coating is, for example, 70 to 300 μm. If the thickness of the coating is 70 μm or more, sufficient heat resistance can be obtained. If the thickness of the coating is 300 μm or less, cracks and fractures in the coating are reduced. In particular, it is desirable that the amount of coating agent applied to metal workpieces be within the above range. The thickness of the coating may be 100 μm or more. The thickness of the coating may be 250 μm or less. The thickness of the coating may be 100 to 250 μm.
[0090] The amount of coating agent applied can be appropriately set depending on the type of object to be treated, its application, and its surface condition. Typically, the amount of coating agent applied is 1.0 to 2.5 kg / m². 2 It is acceptable for it to be 1.5~2.0 kg / m 2 That's fine.
[0091] The coating agent may be applied multiple times. In this case, it is desirable to apply the coating agent again after the surface of the previously applied coating agent has dried. The number of applications is not limited, for example, 4 to 8 times. The application of the coating agent may be repeated until the desired thickness is obtained.
[0092] (3) Firing After applying the coating agent, the workpiece is fired at a temperature lower than its melting point. If glass frit is included, it is preferable to fire the workpiece at a temperature lower than its melting point and above the bending point of the glass frit.
[0093] The final firing is carried out at a temperature lower than the melting point of the material to be treated (if necessary, and at a temperature above the yield point of the glass frit). The coating agent is sintered by the firing. The final firing may be carried out when the material to be treated is in use. For example, if the material to be treated is part of an incinerator, the coating agent may be applied to the material, dried as necessary, and then the incinerator may be operated. The final firing is carried out during this operation.
[0094] The firing temperature is, for example, 600 to 1500°C. In particular, it is desirable that the firing conditions for coatings on metal workpieces be within the above range. The firing temperature may be 700°C or higher, or 800°C or higher. The firing temperature may be 1400°C or lower, or 1350°C or lower. The firing temperature may be 600 to 1400°C, 700 to 1400°C, or 800 to 1350°C. The firing time is not particularly limited. The firing time may be, for example, at least 40 minutes, or 60 minutes. The firing time may be 120 minutes or less.
[0095] Before the final firing, the moisture contained in the coating agent may be evaporated. The moisture can be evaporated, for example, by natural drying, low-temperature forced drying, or by cold air.
[0096] Prior to the main firing, pre-firing may be performed at 200-300°C for about 20-30 minutes. This allows the alkali metal silicate to form siloxane bonds, reducing chalking and enabling long-term storage of the pre-fired treated material. In addition, pre-firing reduces peeling and cracking of the coating agent during the main firing. However, with respect to the coating agent of this disclosure, pre-firing can be omitted.
[0097] The coating agent of this disclosure forms a film on the surface of a workpiece, improving its heat resistance. The film also has a high far-infrared emissivity. Therefore, heat conduction into the workpiece is suppressed, reducing the heat load and potentially reducing energy required for cooling, thus contributing to a reduction in CO2 emissions. [Examples]
[0098] The present invention will be further described in detail by the following examples, but the present invention is not limited thereto.
[0099] [Example 1] According to the table below, each component was measured to the specified mixing ratio and thoroughly mixed in a powder mixer to obtain the coating agent. Alkali metal silicate (potassium silicate) was used diluted with water to 30 Bh. This coating agent is suitable for, for example, refractory bricks, precast refractory bricks, and castable refractories.
[0100] [Table 3-1]
[0101] [Table 3-2]
[0102] [Construction example 1] The coating agent obtained using the formulation shown in Table 3-1 was applied by roller to one of the outlet weirs of a precast refractory brick (made of chromium oxide block) in a waste incineration gasification melting furnace. After application, it was allowed to air dry at room temperature for about 6 hours, and then the melting furnace was operated at 800-1350°C (main firing). The outlet weirs of the other precast refractory bricks were left uncoated. During use, the above precast refractory bricks were constantly in contact with molten slag at approximately 1300°C.
[0103] Figure 1A is a photograph of the tailings outlet weir before use, after the protective coating was formed. Figure 1B is a photograph of the tailings outlet weir 12 months after it began use. As can be seen from Figure 1B, the tailings outlet weir has been maintained without collapsing. The tailings outlet weir was then able to be used for another two years.
[0104] Figure 2A is a photograph of the unconstructed slag outlet weir before it was put into use. Figure 2B is a photograph of the unconstructed slag outlet weir 10 months after it began to be put into use. As can be seen from Figure 2B, the slag outlet weir has completely collapsed.
[0105] The coating agent disclosed herein is expected to reduce maintenance costs. In addition, it is expected to reduce the frequency of furnace shutdowns for maintenance, thereby improving the operating rate.
[0106] [Construction example 2] The coating agent obtained using the formulation shown in Table 3-1 was applied by roller to a precast refractory brick located in one of the two openings in the flue section of the incinerator. After application, it was allowed to air dry at room temperature for about 6 hours, and then the incinerator was operated at 800-1350°C (main firing). The other opening was left uncoated.
[0107] The flue opening was opened once every 30 days to compare the amount of clinker adhering to the coated and uncoated areas. This comparison was performed a total of seven times over a period of 210 days.
[0108] Although there were traces of clinker adhering to the coated precast refractory bricks, most of it had fallen off due to its own weight. The amount of adhering clinker was extremely small and could be removed by hand. Removal of clinker from the coated areas was unnecessary for at least 330 days. The coating agent disclosed herein is expected to improve work efficiency and reduce maintenance costs. Figure 3 is a photograph of the precast refractory bricks 210 days after the start of use following the formation of the coating.
[0109] The precast refractory bricks in the uncoated areas were repeatedly coated with clinker, which had to be forcibly removed. Figure 4 is a photograph of the uncoated precast refractory bricks 210 days after they were put into use.
[0110] [Example 2] A coating agent was obtained by mixing each component in the same manner as in Example 1, according to the table below. Zinc oxide was added as a mixture with water. This coating agent is suitable, for example, for metallic refractories.
[0111] [Table 4-1]
[0112] [Table 4-2]
[0113] [Construction example 3] The coating agent obtained using the formulation shown in Table 4-1 was applied to the water-cooled wall of a biomass boiler. After application, it was allowed to air dry at room temperature for about 6 hours, and then the boiler was operated at 800-1100°C (main firing).
[0114] Figure 5 is a photograph taken 314 days after the start of use of the biomass boiler water-cooled wall with the coating formed on it. Clinker adhesion was suppressed in the coated area.
[0115] [Evaluation 1] Total emissivity A coating agent according to the formulation in Table 3-1 was applied to a boiler steel plate (iron plate), and fired at 250°C to obtain test specimen A. A coating agent according to Table 4-1 was applied to a boiler steel plate (iron plate), and fired at 250°C to obtain test specimen B. A boiler steel plate (iron plate) without any coating agent was used as a comparison test specimen.
[0116] The perpendicular spectral emissivity (%) of far-infrared radiation was measured at room temperature using each test specimen in accordance with JIS R 1693-2. Based on these measurement results, the perpendicular total emissivity (%) at 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, and 1100°C was calculated. The optical path from the light source to the detector was filled with N2 gas and purged. The results are shown in Table 5. Table 5 also shows the perpendicular total emissivity (%) of test specimens A and B, with the perpendicular total emissivity of the comparative test specimen set as the baseline (100%). A larger value indicates improved emissivity.
[0117] (FTIR device) PerkinElmer System2000 model Integrating sphere: Labsphere, PAS-PE-200-ID, gold-plated interior. Integrating sphere entrance aperture: 16mm Measuring part diameter: 24mm
[0118] (Measurement conditions) Measurement area: 370~7800cm -1 (Effective range 400~6000cm) -1 ) Total number of times: 200 Light source: MIR Detector: MIR-TGS Resolution: 16cm -1 Beam splitter: optimized KBr
[0119] [Table 5]
[0120] As can be seen from the table, the coating made with the coating agent disclosed herein has a high total emissivity. Therefore, it is expected to reduce fuel costs and CO2 emissions.
[0121] [Evaluation 2] Heat cycle test The coating agent obtained using the formulation shown in Table 4-1 was applied to the entire front and back surfaces of nickel alloy, iron plate, and stainless steel (SUS304) to a total thickness of approximately 200 μm. Pre-firing was performed in a firing furnace at 250°C for 30 minutes. Subsequently, firing was performed in an electric furnace, raising the temperature from room temperature to 1000°C for 60 minutes.
[0122] Afterward, the fired material was removed from the electric furnace and allowed to cool to room temperature. It was then placed back into the electric furnace and heated to 1000°C. This heat cycle of cooling to room temperature and heating to 1000°C was repeated 50 times. No cracks or peeling were observed in the coating.
[0123] [Evaluation 3] Rapid Cooling Test The fired material obtained in the same manner as in Evaluation 2 was heated to 1000°C in an electric furnace, and then immersed in water for a rapid cooling test. In this case as well, no cracks or peeling were observed in the coating. [Industrial applicability]
[0124] The coating agent of this disclosure can form a highly heat-resistant film on refractories used in high-temperature atmospheres. The coating agent of this disclosure can be used, for example, on refractories in heat furnaces such as industrial waste incinerators, gasification and melting furnaces, incinerators, biomass power plants, thermal power plants, scorching furnaces, heating furnaces, reheating furnaces, and boilers.
Claims
1. (A) Powdered components and (B) Alkali metal silicate solution, The aforementioned (A) powder component is At least one of a boric acid compound and a zinc compound, Mica and, One or more metal sources selected from the group consisting of ferrosilicon, manganese compounds, and cobalt compounds, Inorganic heat-resistant aggregate, An inorganic coating agent containing silicon carbide.
2. The coating agent according to claim 1, wherein the powder component (A) further comprises glass frit.
3. The coating agent according to claim 1, wherein the inorganic heat-resistant aggregate comprises one or more selected from the group consisting of magnesium compounds, zirconium dioxide, aluminum oxide, anhydrous silicic acid, kaolinite, titanium oxide, and silicon nitride.
4. Applying the coating agent described in claim 1 to the object to be treated, A coating method comprising applying the coating agent and then firing the workpiece at a temperature lower than its melting point.
Citation Information
Patent Citations
Coating method of heat resistant and oxidation resistant coating material
JP1996053775A
Combustion-preventive material and refractory material using the same
JP1996060159A
Aqueous solution of heat resistive / oxidation resistive covering material, and method for covering
JP2009102212A
Coating treatment method for heat-resistant and oxidation-resistant coating materials
JP3399650B2
Aqueous solution of heat-resistant and oxidation-resistant coating material and coating treatment method
JP4716196B2