Tire tread

The tire treads are enhanced with specific elastomer and filler combinations to achieve improved material strength, low rolling resistance, and reduced heat generation, addressing the balance of performance and efficiency challenges.

JP7948762B2Active Publication Date: 2026-11-11BEYOND LOTUS LLC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021572284
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-05
Filing Date
2020-06-04
Publication Date
2026-11-11
Estimated Expiration
2040-06-04

Smart Images

  • Figure 0007948762000001
    Figure 0007948762000001
  • Figure 0007948762000002
    Figure 0007948762000002
  • Figure 0007948762000003
    Figure 0007948762000003
Patent Text Reader

Abstract

Tire treads and tires are provided, and more particularly, tires having treads or other elastomeric components within ranges of improved composite material properties, including, but not limited to, modulus ratio, percent elongation at break, and / or loss tangent, wherein the tire, tread, or other elastomeric component comprises a composite characterized by well-dispersed reinforcing fillers, which may be indicated by macrodispersion.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to tire treads and tires. The tire treads and / or tires preferably have improved material properties, such as, but not limited to, modulus ratio, percentage elongation at break, and / or loss tangent. The tire treads and tires comprise an elastomeric material and well-dispersed reinforcing fillers. The tire may be a pneumatic tire having radial carcass reinforcements and further layers or zones of elastomeric material, intended to be mounted on vehicles that carry heavy loads and operate at sustained speeds, such as trucks, tractors, trailers, or buses. Alternatively, the tires and tire treads of the present invention may fit other vehicles, such as light trucks, passenger cars, high-performance vehicles, motorcycles, vehicles used off-road, construction machinery vehicles, aircraft, and road-fit vehicles having road-mounted rubber treads. [Background technology]

[0002] In heavy-duty tires used for trucks and buses, as well as in other tire types, it is known that the tire tread has a multi-layer structure, for example, a cap rubber layer that provides the outer surface of the tread and a base rubber layer radially arranged inside the cap rubber layer, with rubber having excellent wear resistance used in the cap rubber layer and low heat generation rubber with low loss tangent used in the base rubber layer. In other higher stress areas of the tire, for example, in the shoulder area of ​​the tread, a selected rubber compound with improved properties is used. See, for example, U.S. Patent No. 10,399,386. It is desirable to manufacture tire treads that achieve improved fuel efficiency along with improved tire life and durability in the original replacement tire tread by simultaneously achieving high levels of wear and stress resistance, low heat generation (low loss tangent), and low rolling resistance.

[0003] Many tire and tread designs and formulations have been proposed to balance the mechanical and tensile strength rubber material properties with respect to heat, e.g., vehicle weight and speed, surface condition and operating temperature, to obtain acceptable tire performance and life under typical stresses. See, for example, U.S. Patent No. 6,247,512, U.S. Patent No. 10,479,037, U.S. Patent No. 10,308,073 and U.S. Patent Application Publication No. 2009 / 0255613. Some propose using different materials axially to form the tread. The central equatorial material may be different from the lateral planar material, and these materials may be different from the materials used in the various inner zones of the tread. See, for example, U.S. Patent No. 9,713,942. In many cases, the outer material in contact with the ground exhibits better wear performance, while the inner material exhibits hysteresis properties that allow for less heat generation and lower operating temperatures in the crown region when these materials are superimposed on the tread. The void pattern in the tread can vary axially, often having a lower void ratio in the central equatorial plane and a higher groove or sipe surface area in the outer axial portion of the tread. Further inner layers of elastomer materials have been proposed for target ranges in terms of mechanical strength and thermal management, and the thickness of each material layer is selected to optimize tire life and performance. To improve tire performance metrics, several designs and formulations identify elastomer materials with improved filler dispersion levels achieved by liquid elastomer masterbatch processes as a means of optimizing tire performance. See, for example, U.S. Patent No. 10,308,073B2, U.S. Patent No. 10,017,612, U.S. Patent No. 9,834,658 and U.S. Patent No. 9,713,942B2. [Overview of the Initiative] [Problems that the invention aims to solve]

[0004] The present invention preferably provides a tire that has both excellent material strength and sufficiently low rolling resistance, as well as low heat generation to meet fuel efficiency targets.

[0005] The feature of the present invention is to provide a tire tread having one or more advantageous characteristics.

[0006] A further feature of the present invention is to provide a tire tread that provides excellent material strength and / or sufficiently low rolling resistance, and / or low heat generation to meet fuel efficiency targets. [Means for solving the problem]

[0007] To achieve these and other advantages, the present invention, as embodied and described herein, relates to a tire tread comprising at least one elastomer and at least one filler of 40 to 80 phr, wherein the filler comprises at least one carbon black of at least 40 phr, and the tire tread is: a) Modulus ratio > 5.60; b) Percent elongation at break > 470, and c) Loss tangent ≥ 0.10 and < 0.25 at 60℃ (333.15K) The above-mentioned tire tread has the above-mentioned characteristics.

[0008] The present invention relates to a tire tread comprising at least one elastomer and at least one filler of 20 to 80 phr, wherein the filler comprises at least one carbon black of 40 phr or less, and the tread is: a) Modulus ratio ≥ 5.43; b) Percent elongation at break > 400, and c) Loss tangent ≥ 0.09 and < 0.15 at 60℃ (333.15K) The present invention relates to the above tire tread having the above-mentioned features.

[0009] Further, the present invention relates to a tire tread comprising at least one elastomer and from 20 to 80 phr of at least one filler, wherein the filler comprises at least one carbon black, and the tread is characterized by a macrodispersion value V, which is the area percentage of undispersed carbon black particles larger than 10 μm, determined by optical microscopy in transmission mode according to the formula 0.01<V<0.15, said tire tread.

[0010] In addition, the present invention relates to a tire tread comprising at least one elastomer and from 20 to 80 phr of at least one filler, wherein the filler comprises at least one carbon black, and the tread is characterized in that a macrodispersion value V, which is the area percentage of undispersed carbon black particles larger than 10 μm, determined by optical microscopy in transmission mode, is greater than 0.01, said tread: a) has a modulus of elasticity ratio ≥ 5.43; or b) has a percent elongation at break > 400, or c) has a loss tangent at 60°C (333.15 K) < 0.25 has at least one of the above, said tire tread.

[0011] Further, the present invention relates to a tire tread comprising at least one elastomer and from 20 to 80 phr of at least one filler, wherein the filler comprises at least 40 phr of at least one carbon black, and the tire tread: a) has a modulus of elasticity ratio > 5.60; b) has a percent elongation at break > 400, and c) has a loss tangent at 60°C (333.15 K) > 0.09 and < 0.15, and said tread is characterized by a macrodispersion value V, which is the area percentage of undispersed carbon black particles larger than 10 μm, determined by optical microscopy in transmission mode according to the formula 0.01<V<0.15, said tire tread.

[0012] The present invention further relates to a tire tread which may comprise at least one elastomer and at least one filler in an amount of 20 to 80 phr. The filler may comprise at least one carbon black in an amount of at least 40 phr. The tire tread is: a) Modulus ratio > 5.60; b) Percentage elongation at break > 480, and optionally c) Loss tangent <0.25 at 60℃ (333.15K) It may have. The tire tread is further characterized by a macrodispersion value V greater than 0.01, which is the area percentage of undispersed carbon black particles larger than 10 μm, as determined by optical microscopy in transmission mode.

[0013] The present invention also relates to a tire including the tire tread of the present invention.

[0014] Further features and advantages of the present invention are, in part, described in the following detailed description, some of which are evident from the detailed description, or may be taught by the practical application of the present invention. The object and other advantages of the present invention are realized and achieved by the elements and combinations specifically pointed out in the detailed description and the appended claims.

[0015] It should be understood that both the above overview and the following detailed description are illustrative and for illustrative purposes only, and are intended to provide further explanation of the invention as described in the claims. [Modes for carrying out the invention]

[0016] The tires and tire treads of the present invention comprise a composite compound mixed with a rubber compound selected for a desired tire size, grade, and purpose. In one embodiment of the present invention, the tire treads of the present invention may be characterized by an improved combination of material strength, low heat generation, and low rolling resistance, as indicated by an increased modulus ratio and elongation at break, which unexpectedly increases in relation to a decrease in hysteresis (loss tangent). The tire treads of the present invention may be used in tires for heavy-duty vehicles, e.g., tires for off-road use, agricultural vehicles and trucks and buses; tires for lighter vehicles, e.g., light trucks, passenger cars, high-performance vehicles and motorcycles; aircraft tires; and other tires in road-fitting vehicles having road-mounted rubber treads.

[0017] Various tire treads form part of the present invention. A tire tread may be characterized by the amount of filler phr, the amount of carbon black which is part of the filler phr, the modulus ratio value or range, the percentage elongation at break value or range, the loss tangent value or range, and / or the macrodispersion value or range, and any combination of any two or more of these parameters further described herein.

[0018] For example, the tire tread of the present invention may include at least one elastomer and at least one filler in an amount of 40 to 80 phr (tire tread A). The filler may include at least one carbon black in an amount of at least 40 phr. The tire tread is: a) Modulus ratio > 5.60; b) Percent elongation at break > 470, and c) Loss tangent ≥ 0.10 and < 0.25 at 60℃ (333.15K) It may have.

[0019] Generally, with respect to tire treads and tire tread A, the values ​​of modulus ratio, percent elongation at break, and loss tangent can be based on tests in which the tire tread being tested has carbon black present at 50 phr.

[0020] In general, with respect to tire treads and tire tread A, the modulus ratio may be, for example, 5.61 or higher, 5.62 or higher, 5.63 or higher, 5.64 or higher, 5.65 or higher, 5.65 or higher, 5.66 or higher, 5.67 or higher, 5.68 or higher, 5.69 or higher, 5.7 or higher, 5.71 or higher, 5.75 or higher, for example, 5.61 to 6.3, or 5.62 to 6.3, or 5.63 to 6.3, or 5.67 to 6.3, or 5.7 to 6.3, or any other value within one of these ranges.

[0021] Generally speaking, with respect to tire treads and tire tread A, the percentage elongation at break may be 471 or higher, 472 or higher, 473 or higher, 474 or higher, 475 or higher, 480 or higher, 485 or higher, 490 or higher, 495 or higher, 500 or higher, for example, 475 to 550, or 480 to 525, or 480 to 500, or any other value within one of these ranges.

[0022] Generally, with respect to tire tread and tire tread A, the loss tangent may be 0.10 to 0.249, or 0.10 to 0.245, or 0.10 to 0.24, or 0.10 to 0.23, or 0.10 to 0.22, or 0.11 to 0.245, or 0.11 to 0.24, or 0.12 to 0.2, or any other value within one of these ranges.

[0023] In general, with respect to tire treads and tire tread A, the elastomer may include natural rubber, functionalized natural rubber, styrene-butadiene rubber, functionalized styrene-butadiene rubber, polybutadiene rubber, functionalized polybutadiene rubber, or any blend thereof. Alternatively, the elastomer may be any of the elastomers or a blend thereof, as described herein in further detail below.

[0024] The present invention further relates to a tire tread (tire tread B) which may include at least one elastomer and at least one filler in an amount of 20 to 80 phr. The filler may include at least one carbon black in an amount of 40 phr or less. The tire tread is: a) Modulus ratio ≥ 5.43; b) Percent elongation at break > 400, and c) Loss tangent >0.09 and <0.15 at 60℃ (333.15K) It may have.

[0025] Generally, for tire treads and tire tread B, the values ​​of modulus ratio, percent elongation at break, and loss tangent can be based on tire treads tested with a carbon black content of 40 phr.

[0026] Generally speaking, with respect to tire tread and tire tread B, the modulus ratio can be 5.43 or higher, 5.5 or higher, 5.6 or higher, 5.7 or higher, 5.8 or higher, 5.9 or higher, 6.0 or higher, for example, 5.43 to 6.25, or 5.43 to 6.2, or any value within one of these ranges.

[0027] Generally speaking, with respect to tire tread and tire tread B, the percentage elongation at break may be 401 or higher, 402 or higher, 403 or higher, 404 or higher, 405 or higher, 410 or higher, 415 or higher, 420 or higher, 425 or higher, 430 or higher, 435 or higher, 440 or higher, 445 or higher, 450 or higher, 455 or higher, 460 or higher, 465 or higher, 470 or higher, 475 or higher, 480 or higher, 485 or higher, 490 or higher, 495 or higher, 500 or higher, for example, 405 to 550, or 425 to 525, or 425 to 500, or any value within one of these ranges.

[0028] In general, with respect to tire treads, and tire tread B, the loss tangent may be 0.091 to 0.149, or 0.091 to 0.145, or 0.091 to 0.14, or 0.092 to 0.14, or 0.095 to 0.13, or 0.095 to 0.14, or 0.10 to 0.12, or 0.10 to 0.11, or any value within one of these ranges.

[0029] In general, with respect to tire treads and tire tread A and / or B, the tire tread may be further characterized by a macro-dispersion value V. This value V is the area percentage of undispersed carbon black particles exceeding 10 μm, as determined by an optical microscope in transmission mode. The macro-dispersion value V may satisfy the formula: 0.01<V<0.15. The macro-dispersion value V may be 0.011<V<0.15, or 0.012<V<0.15, or 0.013<V<0.15, or 0.014<V<0.15, or 0.015<V<0.15, or 0.02<V<0.15, or 0.05<V<0.15, or 0.07<V<0.15, or 0.08<V<0.15, or 0.09<V<0.12, or any value within one of these ranges.

[0030] The present invention further relates to a tire tread (tire tread C) that may comprise at least one elastomer and 20 to 80 phr of at least one filler. The filler may comprise at least one carbon black. The tire tread may be characterized by the macrodispersion value V as defined herein, which is the area percentage of undispersed carbon black particles larger than 10 μm, determined by optical microscopy in transmission mode. The macrodispersion value V may satisfy the formula: 0.01 < V < 0.15. The macrodispersion value V may be 0.011 < V < 0.15, or 0.012 < V < 0.15, or 0.013 < V < 0.15, or 0.014 < V < 0.15, or 0.015 < V < 0.15, or 0.016 < V < 0.15, or 0.017 < V < 0.15, or 0.018 < V < 0.15, or 0.019 < V < 0.15, or 0.02 < V < 0.15, or 0.05 < V < 0.15, or 0.07 < V < 0.15, or 0.08 < V < 0.15, or 0.09 < V < 0.14, or 0.01 < V < 0.13, or 0.01 < V < 0.12, or 0.01 < V < 0.11, or 0.01 < V < 0.1, or any value within one of these ranges.

[0031] For any of the macrodispersion values V, V may be based on a test in which the tire tread tested has a carbon black content of 50 phr.

[0032] The present invention further relates to a tire tread (tire tread D) that may comprise at least one elastomer and 20 to 80 phr of at least one filler. The filler may comprise no more than 40 phr of at least one carbon black. The tread may be characterized by a macrodispersion value V (the area percentage of undispersed carbon black particles larger than 10 μm, determined by optical microscopy in transmission mode) of greater than 0.01, as described previously. The tire tread has one or more of the following (or two, or all three of the following): a) Elastic modulus ratio ≥ 5.43; or b) percent elongation at break > 400, or c) loss tangent at 60°C (333.15 K) < 0.25 can have.

[0033] Generally with respect to the tire tread and the tire tread D, the tire tread may have values of modulus ratio, percent elongation at break, and loss tangent based on a test in which the tested tire tread comprises carbon black in an amount of 40 phr.

[0034] Generally with respect to the tire tread and the tire tread D, the macro-dispersion value V may be 0.011 or more, 0.012 or more, 0.013 or more, greater than 0.014, or greater than 0.015, or greater than 0.016, or greater than 0.017, or greater than 0.02, or greater than 0.03, or greater than 0.05, or greater than 0.1, or greater than 0.11, or greater than 0.12, or greater than 0.13, or greater than 0.14, or 0.011 < V < 0.14, or 0.012 < V < 0.13, or 0.01 < V < 0.14, or 0.015 < V < 0.14, or 0.02 < V < 0.13, or 0.05 < V < 0.12, or 0.07 < V < 0.11, or 0.01 < V < 0.1, or 0.01 < V < 0.09, or any value within one of these ranges.

[0035] Generally with respect to the tire tread and the tire tread D, the modulus ratio may be 5.43 or more, greater than 5.45, or greater than 5.5, or greater than 5.6, or greater than 5.7, or greater than 5.8, or greater than 5.9, or greater than 5.9, for example, 5.43 to 6.25, or 5.43 to 6.5, or 5.43 to 6.5, or 5.45 to 6.5, or 5.00 to 6.2, or any value between any one of these ranges.

[0036] Generally speaking, with respect to tire treads and tire tread D, the percentage elongation at break may be 401 or higher, 402 or higher, 403 or higher, 404 or higher, 405 or higher, 410 or higher, 415 or higher, 420 or higher, 425 or higher, 430 or higher, 435 or higher, 440 or higher, 445 or higher, 450 or higher, 455 or higher, 460 or higher, 465 or higher, 470 or higher, 475 or higher, 480 or higher, 485 or higher, 490 or higher, 495 or higher, 500 or higher, for example, 405 to 550, or 425 to 525, or 425 to 500, or any value within one of these ranges.

[0037] Generally, with respect to the tire tread and tire tread D, the loss tangent may be 0.249 or less, or 0.245 or less, 0.24 or less, or less than 0.24, or less than 0.23, or less than 0.22, or less than 0.21, or less than 0.2, or less than 0.18, or less than 0.16, or less than 0.14, or less than 0.12, or less than 0.1, for example, 0.09 to 0.249, or 0.09 to 0.245, or 0.09 to 0.22, or 0.10 to 0.2, or any value within any one of these ranges.

[0038] The present invention further relates to a tire tread (tire tread E) which may comprise at least one elastomer and at least one filler in an amount of 40 to 80 phr. The filler may comprise at least one carbon black in an amount of at least 40 phr. The tire tread may have an elastic modulus ratio > 5.60, a percent elongation at break > 470, and loss loss tangents > 0.10 and < 0.25 at 60°C (333.15 K).

[0039] Generally, with respect to the tire tread and tire tread E, the modulus ratio may be greater than 5.61, or greater than 5.62, or greater than 5.65, or greater than 5.7, or greater than 5.8, or greater than 5.9, or greater than 6, or greater than 6.1, or greater than 6.2, for example, 5.61 to 6.2, or 5.65 to 6.1, or 5.7 to 6, or any value within any one of these ranges.

[0040] Generally, with respect to tire tread and tire tread E, the percentage elongation at break may be 471 or higher, 472 or higher, 473 or higher, 474 or higher, 475 or higher, 480 or higher, 485 or higher, 490 or higher, 495 or higher, 500 or higher, for example, 475 to 550, or 480 to 525, or 480 to 500, or any other value within one of these ranges.

[0041] Generally, with respect to the tire tread and tire tread E, the loss loss tangent at 60°C (333.15K) may be 0.101-0.249, or 0.105-0.245, 0.11-0.24, 0.12-0.24, 0.13-0.24, or 0.14-0.24, or 0.15-0.24, or 0.16-0.23, or 0.17-0.23, or 0.18-0.22, or any other value within one of these ranges.

[0042] The present invention further relates to a tire tread (tire tread F) which may include at least one elastomer and at least one filler in an amount of 20 to 80 phr. The filler may include at least one carbon black in an amount of at least 40 phr. The tire tread is: a) Modulus ratio > 5.60; b) Percentage elongation at break > 480, and optionally c) Loss tangent <0.25 at 60℃ (333.15K) It may have. In the tire tread F, the loss tangent parameter is arbitrarily selected. Furthermore, generally speaking, with respect to the tire tread F, the tire tread can be characterized by having a macrodispersion value V (area percentage of undispersed carbon black particles larger than 10 μm, determined by optical microscopy in transmission mode) greater than 0.01, as previously described.

[0043] In general, with respect to tire treads and tire tread F, the tire tread may have values ​​for modulus ratio, percent elongation at break, and loss tangent based on a test in which the tire tread being tested has carbon black in an amount of 50 phr.

[0044] Generally speaking, with respect to tire treads and tire tread F, the modulus ratio of elasticity can be 5.61 or greater, 5.62 or greater, 5.63 or greater, 5.64 or greater, 5.65 or greater, 5.66 or greater, 5.67 or greater, 5.68 or greater, 5.69 or greater, 5.7 or greater, greater than 5.8, or greater than 5.9, or greater than 6.0, or greater than 6.1, or greater than 6.2, or greater than 5.65, or greater than 5.75, for example, 5.61 to 6.25, or 5.65 to 6.5, or 5.63 to 6.2, or any value within any one of these ranges.

[0045] Generally speaking, with respect to tire treads and tire tread F, the percentage elongation at break may be 481 or higher, 482 or higher, 483 or higher, 484 or higher, 485 or higher, 490 or higher, 495 or higher, 500 or higher, 505 or higher, 510 or higher, for example, 481 to 550, or 485 to 525, or 490 to 500, or any other value within one of these ranges.

[0046] Generally, with respect to the tire tread and tire tread F, the loss loss tangent is less than 0.25, or less than 0.24, or less than 0.23, or less than 0.22, or less than 0.21, or less than 0.2, or less than 0.19, or less than 0.18, or less than 0.17, or less than 0.16, or less than 0.15, for example, 0.09 to 0.249, or 0.09 to 0.24, or 0.09 to 0.23, or 0.09 to 0.22, or 0. It may be greater than 0.09 and less than 0.24, or greater than 0.1 and less than 0.24, or 0.1 to 0.24, or 0.1 to 0.23, or 0.11 to 0.23, 0.09 to 0.145, or 0.095 to 0.14, or 0.095 to 0.13, or 0.11 to 0.14, or 0.09 to 0.13, or any value within any one of these ranges.

[0047] Generally, with respect to tire tread and tire tread F, the macrovariance V is 0.011~0.149, or 0.012~0.145, or 0.014~0.145, 0.015~0.14, 0.02~0.14, 0.03~0.14, 0.04~0.14, 0.03~0.06, 0.02~0.12, 0.02~0.11, 0.02~0.1, 0.02~0.09, 0.02~0.08, 0.02~0. It may be 0.7, 0.02 to 0.06, 0.011 to 0.099, greater than 0.01 and less than 0.1, 0.011 to 0.099, or 0.012 to 0.095, or 0.012 to 0.09, or 0.015 to 0.09, or 0.02 to 0.09, or 0.02 to 0.085, or 0.02 to 0.08, or 0.025 to 0.07, or any value within any one of these ranges.

[0048] For any tire tread, including one of tire treads A through F, the filler may include at least one material selected from carbonaceous materials, carbon black, silica, nanocellulose, lignin, clay, nanoclay, metal oxides, metal carbonates, pyrolysis carbon, graphene, graphene oxide, reduced graphene oxide, carbon nanotubes, single-walled carbon nanotubes, multi-walled carbon nanotubes, or combinations thereof, as well as coatings and treated materials thereof, or any combination thereof.

[0049] For any tire tread, including any one of tire treads A through F, the filler may contain carbon black and silica in a weight ratio greater than 2.7:1, or greater than 2.8:1, or greater than 2.9:1, or greater than 3:1, or greater than 3.5:1, or greater than 4:1, or greater than 4.5:1, or greater than 5:1, for example, a carbon black to silica weight ratio of 2.75:1 to 10:1, or any other weight ratio within any one of these ranges.

[0050] For any tire tread, including one of tire treads A through F, the elastomer may be selected from natural rubber, functionalized natural rubber, styrene-butadiene rubber, functionalized styrene-butadiene rubber, polybutadiene rubber, functionalized polybutadiene rubber, polyisoprene rubber, ethylene-propylene rubber, isobutylene-based elastomer, polychloroprene rubber, nitrile rubber, hydrogenated nitrile rubber, polysulfide rubber, polyacrylate elastomer, fluoroelastomer, perfluoroelastomer, silicone elastomer, or any blend of two or more of these.

[0051] For any tire tread, including one of tire treads A through F, the tire tread may further contain one or more rubber chemicals selected from degradation inhibitors, processing aids and activators, zinc oxide, fatty acids, zinc salts of fatty acids, waxes, accelerators, resins, and / or processing oils. One or more of these may be present.

[0052] For any one of the tire treads, including any one of tire treads A to F, the tire tread may comprise carbon black present as a filler or as one of the fillers. The carbon black may have an STSA of greater than 140 m 2 / g, or an STSA of greater than 150 m 2 / g, or 110 m 2 / g to 220 m 2 / g, or an STSA of 120 m 2 / g to 180 m 2 / g, or an STSA of 140 m 2 / g to 180 m 2 / g, or an STSA of 150 m 2 / g to 160 m 2 / g. Further details of fillers comprising carbon black are provided below and may be used in any of the tire tread formulations.

[0053] The tire tread of the present invention may be formed by using one or more of the following process steps to form an elastomer composite, which may then be incorporated into a tire tread formulation to fabricate the tire tread. The present invention includes any tire tread and / or tire formed by any one of the processes described herein or any combination thereof.

[0054] Process step (1) may be used to make the tire tread of the present invention as follows: (a) charging into a mixer a material comprising one or more solid elastomer(s), as well as one or more wet filler(s) comprising filler(s) and at least 15% by weight of liquid based on the total weight of the wet filler(s); (b) Mixing the introduced materials to form a mixture, while removing at least a portion of the liquid, optionally at least 50% by weight of the liquid, from the mixture by evaporation, at a mixer temperature controlled by at least one temperature control means, optionally set to a temperature Tz in the range of 30°C (303.15K) to 150°C (423.15K), and at a mixer rotor tip speed of at least 0.6 m / s for at least 50% of the mixing duration; and (c) Discharge from the mixer an elastomer composite containing fillers dispersed in elastomers at a rate of at least 20 phr with a filler yield loss of 10% or less, and the composite having a liquid content of 10% by weight or less based on the total weight of the elastomer composite.

[0055] Process step (2) may be used to produce the tire tread of the present invention as follows: (a) Put into the first mixer one or more solid elastomers and one or more wet fillers containing fillers and liquids in a weight basis of at least 15% by weight of the total wet fillers; (b) Mixing materials to form a mixture in one or more mixing steps, and in at least one of the mixing steps, removing at least a portion of the liquid, optionally at least 50% by weight of the liquid, from the mixture by evaporation, while performing the mixing at a mixer rotor tip speed of at least 0.6 m / s for at least 50% of the duration of the mixing; (c) Discharge from a first mixer a mixture containing at least 20 phr of filler dispersed in elastomer(s), the mixture having a reduced liquid content to less than the initial liquid content, and the mixture having a material temperature in the range of 100°C (373.15K) to 180°C (453.15K); (d) The mixture from (c) is introduced into a second mixer and mixed to obtain an elastomer composite, the second mixer being operated under at least one of the following conditions: (i) 5 psi (3.448275 × 10 -2 Ram pressure below Pa; (ii) Ram raised to at least 75% of its highest level; (iii) Rams that operate in a floating configuration; (iv) Rams positioned so as not to be substantially in contact with the mixture; (v) The mixer is ramless; and / or (vi) The fill factor of the mixture is in the range of 25% to 70%; and (e) Discharge from the second mixer an elastomer composite having a liquid content of less than 3% by weight on a total elastomer composite weight basis.

[0056] More detailed examples of processes that may be used or included in the production of the tire tread of the present invention may be as follows:

[0057] One method for producing a tire tread according to the present invention may include the following: (a) to impart a wet mixed complex, the wet mixed complex being prepared by: (i) Putting a wet filler into a mixer having one or more rotors, which includes at least a solid elastomer and a liquid present in an amount ranging from 15% to 65% by weight based on the total weight of the filler and the wet filler; (ii) in one or more mixing steps, at least a solid elastomer and a wet filler are mixed to form a mixture, and in at least one of the mixing steps, the mixing is performed, the mixer has at least one temperature control means set to a temperature Tz of 65°C (338.15K) or higher, and at least a portion of the liquid is removed from the mixture by evaporation; and (iii) Discharge from the mixer a wet mixed composite containing a filler dispersed in an elastomer at a charge volume of at least 20 phr with a filler yield loss of 10% or less, and the wet mixed composite shall have a liquid content of 5% by weight or less based on the total weight of the composite; (b) in at least one mixing step, the wet mixed composite is mixed with the tire tread compound; and (c) Manufacturing tire treads from tire tread compounds.

[0058] Another method for producing the tire tread of the present invention may include the following: (a) to impart a wet mixed complex, the wet mixed complex being prepared by: (i) Putting into a mixer at least a solid elastomer containing at least 50% by weight of natural rubber, and a wet filler containing a filler and a liquid present in an amount of at least 15% by weight based on the total weight of the wet filler, the fill factor of at least the solid elastomer and wet filler on a dry weight basis is 68% or less, (ii) in one or more mixing steps, mixing at least a solid elastomer and a wet particulate filler to form a mixture, and in at least one of the mixing steps, performing the mixing at a mixer temperature controlled by at least one temperature control means, and removing at least a portion of the liquid from the mixture by evaporation; (iii) Discharge from the mixer a composite containing a filler dispersed in an elastomer at a charge volume of at least 20 phr with a filler yield loss of 10% or less, and the composite shall have a liquid content of 10% by weight or less based on the total weight of the composite; (b) in at least one mixing step, the wet mixed composite is mixed with the tire tread compound; and (c) Manufacturing tire treads from tire tread compounds.

[0059] Further methods for producing the tire tread of the present invention may include the following: (a) to impart a wet mixed complex, the wet mixed complex being prepared by: (i) Putting into a mixer at least a solid elastomer and a wet filler containing a liquid present in an amount of at least 15% by weight based on the total weight of the filler and the wet filler. (ii) in one or more mixing steps, mixing at least a solid elastomer and a wet filler to form a mixture, and in at least one of the mixing steps, for at least 50% of the mixing time, performing the mixing at a mixer temperature controlled by at least one temperature control means using one or more rotors operating at a tip speed of at least 0.6 m / s, thereby removing at least a portion of the liquid from the mixture by evaporation; and (iii) Discharge from the mixer a wet mixed composite containing a filler dispersed in an elastomer at a charge volume of at least 20 phr with a filler yield loss of 10% or less, and the wet mixed composite shall have a liquid content of 10% by weight or less based on the total weight of the wet mixed composite; (b) in at least one mixing step, the wet mixed composite is mixed with the tire tread compound; and (c) Manufacturing tire treads from tire tread compounds.

[0060] Further methods for producing the tire tread of the present invention may include the following: (a) to impart a wet mixed complex, the wet mixed complex being prepared by: (i) A wet filler comprising at least a solid elastomer and a liquid present in an amount of at least 15% by weight based on the total weight of the filler and the wet filler is introduced into a first mixer having one or more rotors; (ii) in one or more mixing steps, mixing at least a solid elastomer and a wet filler to form a mixture, and in at least one of the mixing steps, for at least 50% of the mixing time, performing the mixing at a mixer temperature controlled by at least one temperature control means using one or more rotors operating at a tip speed of at least 0.6 m / s, thereby removing at least a portion of the liquid from the mixture by evaporation. (iii) Discharge from a first mixer a mixture containing a filler dispersed in an elastomer in a charge of at least 20 phr, wherein the mixture has a liquid content in the range of 1% to 20% by weight based on the total weight of the composite, and the mixture has a material temperature in the range of 100°C (373.15K) to 180°C (453.15K); (iv) Mixing the mixture from (iii) in a second mixer to obtain a complex, the second mixer being operated under at least one of the following conditions: -5psi (3.448275 x 10 -2 Ram pressure below Pa; - Ram raised to at least 75% of its highest level; - A ram operating in a floating configuration; - A ram positioned so as not to be substantially in contact with the mixture; - The mixer must be ram-free; and / or - The fill factor of the mixture is in the range of 25% to 70%; and (v) Discharge from the second mixer a wet mixed complex having a liquid content of less than 3% by weight based on the total weight of the wet mixed complex; (b) in at least one mixing step, the wet mixed composite is mixed with the tire tread compound; and (c) Manufacturing tire treads from tire tread compounds.

[0061] Further methods for producing the tire tread of the present invention may include the following: (a) to impart a wet mixed complex, the wet mixed complex being prepared by: (i) A wet filler comprising at least a solid elastomer and a liquid present in an amount of at least 15% by weight based on the total weight of the filler and the wet filler is introduced into a first mixer having one or more rotors; (ii) in one or more mixing steps, mixing at least a solid elastomer and a wet filler to form a mixture; in at least one of the mixing steps, performing the mixing at a mixer temperature controlled by at least one temperature control means; applying an average specific power of at least 2.5 kW / kg over the mixing time; and removing at least a portion of the liquid from the mixture by evaporation; (iii) Discharge from the first mixer a mixture containing a filler dispersed in an elastomer in a charge of at least 20 phr, wherein the mixture has a reduced liquid content to less than the liquid content at the beginning of step (ii), and the mixture has a material temperature in the range of 100°C (373.15K) to 180°C (453.15K); (iv) Mixing the mixture from (iii) in a second mixer to obtain a complex, the second mixer being operated under at least one of the following conditions: -5psi (3.448275 x 10 -2 Ram pressure below Pa; - Ram raised to at least 75% of its highest level; - A ram operating in a floating configuration; - A ram positioned so as not to be substantially in contact with the mixture; - The mixer must be ram-free; and / or - The fill factor of the mixture is in the range of 25% to 70%; and (v) Discharge from the second mixer a composite having a liquid content of less than 3% by weight based on the total weight of the above composite; (b) in at least one mixing step, the wet mixed composite is mixed with the tire tread compound; and (c) Manufacturing tire treads from tire tread compounds.

[0062] In addition, as used herein, the term “wet-mixed composite” means an elastomer composite material produced from a solid elastomer and a wet filler by an optional further processing step combined with any set of process steps (1) or (2) or any other process described herein. Further processing steps include, but are not limited to, the following: (a) The filler contains at least 50% by weight, or at least 40% by weight, of carbon black material; and / or the carbon black material is dispersed in the elastomer(s) in a charge of 30 to 150 phr; and / or the carbon black material is 60 m 2 / g~200m 2 Selection of a filler having STSA in the range of / g and / or COAN in the range of 60mL / 100g to 120mL / 100g; (b) Selection of a liquid that is volatile at the elastomer composite mixing temperature; and / or selection of a liquid containing water; and / or selection of a liquid containing a component selected from acids, bases, salts, surfactants and processing aids; (c) Selection of mixer conditions to obtain a total specific energy of at least 1,400 kJ / kg of elastomer composite; and / or applying energy to the mixer to obtain a time-averaged liquid discharge rate of 0.01 to 0.14 kg / (min·kg) based on the dry weight (kg) of the elastomer composite; and / or obtaining a liquid content of the discharged elastomer composite of 5% by weight or less based on the total weight of the elastomer composite; (d) Selection of batch, semi-continuous and / or continuous mixers and mixing process; and / or exclusion of one or more rubber chemicals and extruded elastomer composites from the mixing process; and / or 5 psi (3.448275 × 10 -2Operated by the second mixer at a ram pressure of less than or equal to Pa) and / or at a temperature Tz in the range of 60°C (333.15K) to 110°C (383.15K), or 65°C (338.15K) to 100°C (373.15K), or 50°C (323.15K) to 100°C (373.15K); and / or operated by the first mixer at a fill factor of 50-70%; and / or (e) Selection of a mixer as a second mixer that operates under at least one of the following conditions (i) 5 psi (3.448275 × 10 -2 Ram pressure below Pa; (ii) Ram raised to at least 75% of its highest level; (iii) Rams that operate in a floating configuration; (iv) Rams positioned so as not to be substantially in contact with the mixture; (v) The mixer is ramless; and / or (vi) The fill factor of the mixture is in the range of 25% to 70%.

[0063] In addition, as used herein, the term “wet-mixed composite” means any elastomeric composite material produced from a solid elastomer and a wet-filler by any process disclosed in U.S. Provisional Patent Application No. 62 / 857,779 and PCT Application No. 20 / 36168, entitled “METHODS OF PREPARING A COMPOSITE HAVING ELASTOMER AND FILLER,” as incorporated herein by reference.

[0064] In the detailed description of the present invention, the terms “rubber” and “elastomer” are used interchangeably unless otherwise specified. The terms “rubber composition,” “compound,” “admixtured rubber,” and “rubber compound” are used interchangeably as used herein to mean “rubber blended or mixed with various components,” and the term “compound” means “rubber composition” unless otherwise specified. Such terms are well known to those skilled in the art of rubber mixing or admixture. The term “phr” refers to parts of each material per 100 parts by dry weight of rubber or elastomer. The terms “cured” and “vulcanized” or “vulcanized product” are used interchangeably with respect to crosslinked rubber compounds in tires unless otherwise specified.

[0065] The tire tread of the present invention is characterized by excellent filler dispersion. Filler dispersion can be measured in a cured or vulcanized rubber compound by a technique using an optical microscope in a transmission mode for determining a macrodispersion value "V" representing the area percentage of undispersed carbon black particles larger than 10 μm. Such a composite has distinctive product properties. The tire tread of the present invention, comprising at least one elastomer and at least one filler of 20 to 80 phr, wherein the filler comprises at least one carbon black, can be characterized by a macrodispersion value V, modulus ratio, percent elongation at break, or loss tangent at 60°C (333.15 K), which can be determined by typical industrial test methods described in the following examples.

[0066] Solid elastomer Examples of solid elastomers useful in wet filler composites include, but are not limited to, natural or synthetic elastomers in any solid form suitable for tire components or tire treads.

[0067] Optionally, the solid elastomer used in the composite of the present invention may be natural rubber and at least one of its treated and functionalized derivatives. For example, natural rubber may be treated to chemically or enzymatically modify or reduce various non-rubber components, or the rubber molecule itself may be modified with various monomers or other chemical groups, such as chlorine. Optionally, epoxidized natural rubber may be used, as described in PCT International Publication No. 2017 / 207912, where the natural rubber has a nitrogen content of up to 0.3% by weight. A useful technical description of natural rubber is readily available, for example, in Rubber World Magazine's Blue Book, published by Lippincott and Peto, Inc. (Akron, Ohio, USA). The solid elastomer used in the composite of the present invention may be at least one elastomer selected from natural rubber, functionalized natural rubber, styrene-butadiene rubber, functionalized styrene-butadiene rubber, polybutadiene rubber, functionalized polybutadiene rubber, polyisoprene rubber, ethylene-propylene rubber, isobutylene-based elastomer, polychloroprene rubber, nitrile rubber, hydrogenated nitrile rubber, polysulfide rubber, polyacrylate elastomer, fluoroelastomer, perfluoroelastomer, silicone elastomer, and blends thereof.

[0068] Exemplary elastomers include, but are not limited to, rubbers and polymers (e.g., homopolymers, copolymers, and / or terpolymers) of 1,3-butadiene, styrene, isoprene, isobutylene, and 2,3-dialkyl-1,3-butadiene, where alkyl may be methyl, ethyl, propyl, etc., or acrylonitrile, ethylene, propylene, etc. The elastomers may have a glass transition temperature (Tg) in the range of about -120°C (153.15K) to about 0°C (273.15K), as measured by differential scanning calorimetry (DSC). Examples include, but are not limited to, styrene-butadiene rubber (SBR), natural rubber and its derivatives, e.g., chlorinated rubber, polybutadiene, polyisoprene, poly(styrene-co-butadiene), and oil-extracted derivatives of any of these. Any blend of the above may be used. Particularly suitable synthetic rubbers include: styrene and butadiene copolymers containing about 10% to about 70% by weight of styrene and about 90% to about 30% by weight of butadiene, for example, copolymers of 19 parts styrene and 81 parts butadiene, 30 parts styrene and 70 parts butadiene, 43 parts styrene and 57 parts butadiene, and 50 parts styrene and 50 parts butadiene; conjugated dienes, for example, polybutadiene, polyisoprene, polychloroprene and polymers and copolymers thereof. Furthermore, copolymers of such conjugated dienes with copolymerizable ethylenically active monomers, such as styrene, methylstyrene, chlorostyrene, acrylonitrile, 2-vinylpyridine, 5-methyl-2-vinylpyridine, 5-ethyl-2-vinylpyridine, 2-methyl-5-vinylpyridine, allyl-substituted acrylates, vinyl ketones, methyl isopropenyl ketones, methyl vinyl ethers, alpha-methylene carboxylic acids, and their esters and amides, such as acrylic acid and dialkylacrylamide. Copolymers of ethylene with other higher alpha-olefins, such as propylene, 1-butene, and 1-pentene, are also suitable for use herein.Other polymers are disclosed in U.S. Patent Application Publication No. 2018 / 0282523 and European Patent No. 2423253(B1), the disclosures of which are incorporated herein by reference. Other polymers include silicone elastomers or hybrid systems having silicone and hydrocarbon domains. With respect to solid elastomers used and mixed with wet fillers, the solid elastomers may be dry elastomers or substantially dry elastomers. The solid elastomers have a water content (or moisture content) of 5% by weight or less, for example, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.1% to 5% by weight, 0.5% to 5% by weight, 1% to 5% by weight, 0.5% to 4% by weight and equivalent amounts based on the total weight of the solid elastomer. The solid elastomer may be an elastomer as a whole (having an initial water content of 5% by weight or less), or it may be a solid elastomer masterbatch containing one or more fillers and / or other components. For example, the solid elastomer may be 50% to 99.9% by weight of elastomer, with 0.1% to 50% by weight of fillers pre-dispersed in the elastomer, the pre-dispersed fillers being present in addition to the wet fillers incorporated into the composite.

[0069] With respect to solid elastomer masterbatches used and mixed with wet fillers, the solid elastomer masterbatch may be a dry elastomer masterbatch or a substantially dry elastomer masterbatch. The solid elastomer masterbatch has a water content (or moisture content) of 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.1% to 5% by weight, 0.5% to 5% by weight, 1% to 5% by weight, 0.5% to 4% by weight and equivalent.

[0070] A solid elastomer masterbatch (e.g., a starting solid elastomer masterbatch) is an elastomer containing one or more fillers and, optionally, other components. For example, a solid elastomer masterbatch may contain 1 phr to 100 phr of filler pre-dispersed in the elastomer, or 20 phr to 80 phr of filler pre-dispersed in the elastomer, or 30 phr to 70 phr of filler pre-dispersed in the elastomer, or 40 phr to 60 phr of filler pre-dispersed in the elastomer, and the like. Other components, such as further elastomers, antioxidants, and other rubber chemicals and additives, may be present in the solid elastomer in amounts of 0.1 phr to less than 50 phr. A solid elastomer masterbatch may contain any elastomer, any filler, any additive, and any combination thereof in any amount described and illustrated herein, and known in the art. The total fillers contained in the finishing rubber compound include, in addition to added wet fillers, fillers pre-dispersed in a solid elastomer masterbatch. The solid elastomer masterbatch may be a dry and / or wet mixed composite, or a dry mixture or compound produced by a dry masterbatch process.

[0071] The second elastomeric material may be combined with the solid elastomer (or masterbatch) before, simultaneously with, or after the wet filler is combined with the solid elastomer (or masterbatch). The second elastomeric material may consist of at least one solid elastomer; at least one further solid elastomer masterbatch. The second elastomeric material may consist of the same elastomer as the solid elastomer, or at least one different elastomer selected from one or more elastomers described herein or known in the art. The second elastomeric material may consist of at least one rubber chemical described herein or known in the art.

[0072] filler When preparing the rubber compound for the tire tread of the present invention, a wet-mix composite may be used. A wet-mix composite utilizing a wet filler (e.g., including filler and liquid) allows batch time and temperature to be controlled beyond those achievable in known dry-mix processes, providing other benefits, such as improved filler dispersion and / or facilitated rubber-filler interaction and / or improved rubber compound performance. The wet filler may be effective when sufficient liquid is used to wet substantially a portion or substantially all of the filler surface before mixing with the solid elastomer. Generally, as described herein, the mixing process can be controlled by controlling one or more mixers or process parameters, such as mixer surface temperature and / or rotor speed, fill factor, incorporation of rubber chemicals (if any) at time after the mixing cycle, composite discharge temperature, and / or application of two or more mixing stages.

[0073] A method for preparing a wet-mix composite comprises adding or introducing at least a solid elastomer and a wet filler, for example, a) one or more solid elastomers and b) one or more fillers, into a rubber mixer, wherein at least one filler or a portion of at least one filler is wet with a liquid before mixing with the solid elastomer (wet filler). The solid elastomer and the wet filler are combined to form a mixture during a mixing step(s). The method further comprises performing the mixing in one or more mixing steps, wherein at least a portion of the liquid is removed by evaporation or an evaporation process performed during mixing. The liquid of the wet filler may be removed by evaporation (and at least a portion may be removed under the listed mixing conditions) and may be a volatile liquid, for example, volatile at the bulk mixture temperature. For example, a liquid may have a boiling point at 1 atm (101325 Pa) of 60°C (333.15 K) to 110°C (383.15 K), 60°C (333.15 K) to 100°C (373.15 K), 60°C (333.15 K) to 90°C (363.15 K), 90°C (363.15 K) to 110°C (383.15 K), 90°C (363.15 K) to 100°C (373.15 K), 95°C (368.15 K) to 120°C (393.15 K), or 95°C (368.15 K) to 110°C (383.15 K). For example, volatile liquids can be distinguished from oils (e.g., extender oils, process oils) that may be present during at least a portion of the mixing process, and such oils are intended to be present in the discharged complex and therefore do not evaporate during a substantial portion of the mixing time.

[0074] With respect to the wet filler, in one embodiment, the wet filler has the consistency of a solid. Preferably, the dry filler is wet only to the extent that the resulting wet filler is in the form of a powder, particulate matter, pellets, cake, or paste, or maintains a similar consistency, and / or has the appearance of a powder, particulate matter, pellets, cake, or paste. The wet filler does not flow like a liquid (for example, under zero applied stress). Optionally, the wet filler, whether in the form of individual particles, aggregates, pellets, cake, or paste, can maintain its shape at 25°C (298.15K) when molded into such shape. The wet filler is not a composite produced by a liquid masterbatch process, nor is it any other pre-blended composite of fillers dispersed in a solid elastomer in which the elastomer is a continuous phase. In another embodiment, the wet filler may be a slurry. In yet another embodiment, the wet filler is not a slurry of fillers and does not have the consistency of a liquid or slurry.

[0075] In its dry state, the filler may contain a small amount of liquid (e.g., water) adsorbed on its surface. For example, carbon black may have 1-3% or 4% by weight of water, and precipitated silica may have a water content of 4-7% by weight. Such fillers are referred to herein as dry or non-wet fillers. With respect to the wet filler, an additional liquid is added to the filler and present on the surface of the filler, including the inner surface or pores that are accessible to the liquid. During mixing, at least a portion of the liquid is removed by evaporation as the wet filler disperses in the solid elastomer, and the surface of the filler may become available for subsequent interaction with the solid elastomer. The wet filler may have a liquid content of at least 20% by weight relative to the total weight of the wet filler, for example, at least 30%, at least 40%, at least 50% by weight relative to the total weight of the wet filler, or 20% to 80%, 30% to 80%, 30% to 70%, 30% to 60%, 40% to 80%, 40% to 70%, or 40% to 60%.

[0076] The liquid used to wet the filler may be an aqueous liquid, for example, water, or may contain water. The liquid may contain at least one other component, for example, a base(s), an acid(s), a salt(s), a solvent(s), a surfactant(s), a coupling agent(s), and / or a processing aid(s), and / or any combination thereof.

[0077] Optionally, the mixture may further comprise one or more non-wetting fillers (e.g., any filler that is not wet as described herein, e.g., dry fillers, e.g., fillers having 10% by weight or less of liquid).

[0078] The fillers used to fabricate the wet filler composite may be any conventional fillers used with the elastomer, including, but not limited to, carbon black, silica, carbon black-containing fillers, silica-containing fillers, and / or any combination thereof. The fillers may be particulate, fibrous, or plate-like. For example, particulate fillers are made of separate objects. Such fillers may often have aspect ratios (e.g., length to diameter) of 3:1 or less, or 2:1 or less, or 1.5:1 or less. Fibrous fillers may have aspect ratios of, for example, 2:1 or more, 3:1 or more, 4:1 or more, or greater. Typically, fillers used to reinforce the elastomer have dimensions that are microscopic (e.g., several hundred microns or less) or nanoscale (e.g., less than 1 micron). In the case of carbon black, separate particulate carbon black bodies refer to aggregates or clumps formed from primary particles but not the primary particles themselves. In other embodiments, the filler may have a plate-like structure and may be, for example, graphene and reduced graphene oxide.

[0079] The carbon black used in the tire tread of the present invention may be untreated carbon black, treated carbon black, or a mixture thereof. The filler may be, or may contain, wet carbon black in the form of pellets, a fluffy powder, granules, and / or agglomerates. The wet carbon black may be formed into pellets, granules, or agglomerates in, for example, a pelletizer, a fluidized bed, or other apparatus for producing wet filler.

[0080] The filler used in the tire tread of the present invention may be chemically treated (e.g., chemically treated carbon black, chemically treated silica, silicon-treated carbon black) and / or chemically modified. The filler may be or may contain carbon black to which organic groups are bonded. The filler may have one or more coatings present on the filler (e.g., silicon-coated material, silica-coated material, carbon-coated material). The filler may be oxidized and / or may have other surface treatments. The filler may include carbonaceous materials, carbon black, silica, nanocellulose, lignin, nanoclay, metal oxides, metal carbonates, pyrolytic carbon, recycled carbon, recovered carbon, rCB, graphene, graphene oxide, reduced graphene oxide, carbon nanotubes, single-walled carbon nanotubes, multi-walled carbon nanotubes, or combinations thereof, or at least one material selected from the corresponding coated or chemically treated materials thereof. The types of silica, carbon black, or other usable fillers are not limited. Further details regarding the filler are provided in other sections of this specification. The filler may be, or may contain, a blend of carbon black and silica in any weight ratio, for example, in the weight ratio range of 1:99 to 99:1 or 25:75 to 75:25 or 45:55 to 55:45.

[0081] Wet carbon black can be one or more of the following: - Undried carbon black pellets; and / or - For example, dry carbon black pellets moistened with water in a pelletizer; and / or - Dry carbon black pellets that are crushed in a pelletizer and then re-moistened with water; and / or - Dry carbon black pellets combined with water; and / or - A fluffy powder, granules, or aggregate combined with water.

[0082] In the typical production of carbon black, carbon black is initially prepared as a dry, finely particulate (fluffy) material. The fluffy carbon black can be densified by conventional pelletizing processes, for example, by combining the carbon black with a liquid, such as by adding water and feeding the mixture into a pin pelletizer. Pin pelletizers are well known in the art, including those described in U.S. Patent No. 3,528,785. The resulting wet pellets are then heated under controlled temperatures and parameters to remove the liquid from the pellets before further handling and transport. In an alternative process, carbon black pellets may be produced by a process that omits the drying step. In such a process, the pelletized carbon black contains at least 20% by weight of process water based on the total weight of the wet carbon black. These “undried carbon black” pellets can be used directly in the claimed process after pelletizing. Alternatively, dry carbon black pellets (e.g., commercially available carbon black pellets) can be re-moistened in a pelletizer. The pellets can be granulated, crushed, sorted, and / or crushed, for example, in a jet mill. The resulting carbon black is in a fluffy form and can be re-pelletized in a pelletizer, or, in other cases, compressed or agglomerated in the presence of water to wet the carbon black. Alternatively, the fluffy carbon black can be compressed into other forms, such as brick-like forms, by apparatus known in the art. Another optional choice is to wet the fluffy carbon black by using a fluidized bed, sprayer, mixer, or rotating drum and the like. When the liquid is water, the undried or re-wet carbon black can achieve a moisture content of 20% to 80%, 30% to 70% by weight, or other ranges, for example, 55% to 60% by weight, relative to the total weight of the wet carbon black.

[0083] The carbon black used in the tire tread of the present invention may be of any grade from reinforced carbon black and semi-reinforced carbon black. Examples of ASTM grade reinforced grades are N110, N121, N134, N220, N231, N234, N299, N326, N330, N339, N347, N351, N358, and N375 carbon black. Examples of ASTM grade semi-reinforced grades are N539, N550, N650, N660, N683, N762, N765, N774, N787, N990 carbon black and / or N990 grade thermal black.

[0084] Carbon black, for example, 20m 2 / g~250m 2 / g or more, for example, at least 60m 2 / g, for example, 60m 2 / g~150m 2 / g, or 70m 2 / g~250m 2 / g, or 80m 2 / g~200m 2 / g, or 90m 2 / g~200m 2 / g, or 100m 2 / g~180m 2 / g, 110m 2 / g~150m 2 / g, 120m 2 / g~150m 2 / g etc, 140m 2 / g~180m 2 / g, 150m 2 / g~180m 2 / g, 140m 2 / g~170m 2 / g, 150m 2 / g~170m 2 / g, 140m 2 / g~160m 2 / g, or 150m 2 / g~160m 2It may have any statistical thickness specific surface area (STSA) within the range of / g. STSA (statistical thickness specific surface area) is determined based on ASTM test procedure D-6556 (measured by nitrogen adsorption).

[0085] Carbon black is available in quantities of approximately 30 mL / 100 g to approximately 150 mL / 100 g, for example, approximately 30 mL / 100 g to approximately 125 mL / 100 g, approximately 30 mL / 100 g to approximately 115 mL / 100 g, approximately 50 mL / 100 g to approximately 150 mL / 100 g, approximately 50 mL / 100 g to approximately 125 mL / 100 g, approximately 50 mL / 100 g to approximately 115 mL / 100 g, and approximately 70 mL / 100 g to approximately 150 mL / 100 g. The Compression Oil Absorption (COAN) may be in the range of mL / 100g, approximately 70mL / 100g to approximately 125mL / 100g, approximately 70mL / 100g to approximately 115mL / 100g, approximately 80mL / 100g to approximately 150mL / 100g, approximately 80mL / 100g to approximately 125mL / 100g, approximately 80mL / 100g to approximately 115mL / 100g, or approximately 80mL / 100g to approximately 100mL / 100g. The Compression Oil Absorption (COAN) is determined according to ASTM D3493. Optionally, carbon black may have a COAN of 70mL / 100g to 115mL / 100g and a 60mL COAN. 2 / g~1555m 2 It may have an STSA in the range of / g.

[0086] As described, carbon black may be rubber black, in particular a reinforced or semi-reinforced grade of carbon black. Trademarks Regal®, Black Pearls®, Spheron®, Sterling®, Propel®, Endure®, and Vulcan® available from Cabot Corporation; trademarks Raven®, Statex®, Furnex®, and Neotex® available from Birla Carbon (formerly available from Columbia Chemicals), as well as the CD and HV series; trademarks Corax®, Durax®, Ecorax®, and Purex® available from Orion Engineered Carbons (formerly Evonik and Degussa Industries), as well as carbon black sold under the CK series; and other fillers suitable for use in rubber or tire applications may also be utilized for use in various implements. Suitable chemically functionalized carbon blacks include those disclosed in International Publication No. 96 / 18688 and U.S. Patent Application Publication No. 2013 / 0165560, which are incorporated herein by reference. Mixtures of any of these carbon blacks may be used. Carbon blacks having surface area and structure exceeding typical values ​​selected for ASTM grade and rubber mixing, such as those described in U.S. Patent Application Publication No. 2018 / 0282523, whose disclosure is incorporated herein by reference, may be used in the tire treads of the present invention.

[0087] Carbon black may be oxidized carbon black, for example, carbon black that has been surface-treated with an oxidizing agent. Oxidizing agents include, but are not limited to, air, oxygen gas, ozone, NO2 (including mixtures of NO2 and air), peroxides, such as hydrogen peroxide, sodium persulfate, potassium, or persulfates including ammonium, hypohalites, such as hypochlorous acid, halogenous acid, or sodium perhalate (e.g., sodium chlorite, sodium chlorate, or sodium perchlorate), oxidizing acids, such as nitric acid, and transition metal-containing oxidizing agents, such as permanganates, osmium tetroxide, chromium oxide, or cerium ammonium nitrate. Mixtures of oxidizing agents, particularly gaseous oxidizing agents, such as mixtures of oxygen and ozone, may be used. In addition, carbon black prepared using other surface modification methods for introducing ionic or ionizable groups into the pigment surface, such as chlorination and sulfonation, may be used. Processes that can be used to produce oxidized carbon black are known in the art, and several types of oxidized carbon black are commercially available.

[0088] Carbon black can be furnace black, gas black, thermal black, acetylene black, lamp black, plasma black, or recycled black (or rCB), or a carbon product containing silicon-containing species and / or metal-containing species and / or similar. For the purposes of the present invention, carbon black can be a multiphase aggregate comprising at least one carbon phase and at least one metal-containing species phase or silicon-containing species phase, i.e., silicon-treated carbon black. In silicon-treated carbon black, silicon-containing species, such as silicon oxides or carbides, are distributed throughout at least a portion of the carbon black aggregate as an essential part of the carbon black. Although silicon-treated carbon black is not a coated or otherwise modified carbon black aggregate, it actually represents a two-phase aggregate particle, where one phase is carbon still present as graphite crystals and / or amorphous carbon, while the second phase is silica and possibly other silicon-containing species). Therefore, the silicon-containing species phase of silicon-treated carbon black is an essential part of the aggregate, distributed throughout at least a portion of the aggregate. ECOBLACK (商標) Siliconized carbon black is available from Cabot Corporation. The manufacturing and properties of these siliconized carbon blacks are described in U.S. Patent No. 6,028,137, which is incorporated herein by reference.

[0089] Siliconized carbon black may contain silicon-containing regions primarily on the aggregate surface of the carbon black, but which are still parts of the carbon black, and / or siliconized carbon black may contain silicon-containing regions distributed throughout the entire carbon black aggregate. Siliconized carbon black can be oxidized. Siliconized carbon black may contain about 0.1% to about 50% by weight of silicon, based on the weight of the siliconized carbon black. These amounts can all be about 0.5% to about 25% by weight, about 1% to about 15% by weight of silicon, about 2% to about 10% by weight, about 3% to about 8% by weight, about 4% to about 5% by weight, or about 6% by weight, based on the weight of the siliconized carbon black.

[0090] Those skilled in the art will recognize that, apart from the silicon content of siliconized carbon black, the surface of the particles can also vary in the amounts of silica and carbon black. For example, the surface area of ​​siliconized carbon black may contain about 5% to about 95% silica, e.g., about 10% to about 90%, about 15% to about 80%, about 20% to about 70%, about 25% to about 60%, about 30% to about 50%, or about 35% to about 40%, e.g., a maximum of about 20% or a maximum of about 30% silica. The amount of silica on the surface can be determined by the difference in surface area between particles, as measured by iodine value (ASTM D-1510) and nitrogen adsorption (i.e., BET, ASTM D6556).

[0091] Alternatively, a filler, such as carbon black, may be chemically treated. For example, carbon black may have at least one bonded organic group. The bond may arise via a diazonium reaction having a diazonium salt substituent, as detailed in U.S. Patent Nos. 5,554,739; 5,630,868; 5,672,198; 5,707,432; 5,851,280; 5,885,335; 5,895,522; 5,900,029; and 5,922,118, the disclosure of which is incorporated herein by reference.

[0092] In the tire tread of the present invention, a combination of more than one filler may be used in the composite of the present invention or a compound containing said composite. The combination may include rubber-reinforced carbon black(s) and silica, for example, precipitated silica, and the combination may contain a carbon black to silica weight ratio of at least 2.7 to 1.0.

[0093] With respect to the filler, one or more types of silica, or any combination of silica(s), may be used in any embodiment of the present invention. Silica may include, or may be, precipitated silica, fumed silica, silica gel, and / or colloidal silica. Silica may be, or may be, untreated silica and / or chemically treated silica. Silica may be suitable for reinforcing elastomer composites, about 20 m 2 / g ~ approx. 450m 2 / g; approx. 30m 2 / g ~ approx. 450m 2 / g; approx. 30m 2 / g~about 400m 2 / g; or approximately 60ml 2 / g ~ approx. 250m 2 / g, approx. 60m 2 / g ~ approx. 250m 2 / g, approx. 80m 2 / g~about 200m 2It can be characterized by the Brunauer-Emmett Teller surface area (BET) per g. Highly dispersible precipitated silica can be used as a filler in this method. Highly dispersible precipitated silica ("HDS") is understood to mean any silica that has substantial ability to dissociate and disperse in an elastomeric matrix. The determination of such dispersion can be observed by known methods using an electron or optical microscope in a thin section of the elastomeric composite. Examples of commercially available grades of HDS include Perkasil® GT3000GRAN silica from WR Grace & Co, Ultrasil® 7000 silica from Evonik Industries, Zeosil® 1165MP, 1115MP, Premium and 1200MP silica from Solvay SA, Hi-Sil® EZ160G silica from PPG Industries, Inc., and Zeopol® 8741 or 8745 silica from Evonik Industries. Conventional non-HDS precipitated silica may also be used. Examples of commercially available grades of conventional precipitated silica include Perkasil® KS408 silica from WR Grace & Co, Zeosil® 175GR silica from Solvay SA, Ultrasil® VN3 silica from Evonik Industries, and Hi-Sil® 243 silica from PPG Industries, Inc. Precipitated silica with a silane coupling agent attached to the surface may also be used. Examples of commercially available grades of chemically treated precipitated silica include Agilon® 400, 454, or 458 silica from PPG Industries, Inc., and Coupsil silica from Evonik Industries, such as Coupsil® 6109 silica.

[0094] While the amounts of liquid in the fillers described above can be applied equally to silica, as a more specific example, when silica is used as a wet filler in part or in whole, the silica may have liquid present in amounts of about 25% to about 75% by weight, for example, about 30% to about 75%, about 40% to about 75%, about 45% to about 75%, about 50% to about 75%, about 30% to about 70%, about 40% to about 70%, about 45% to about 70%, about 50% to about 70%, about 30% to about 65%, about 40% to about 65%, about 45% to about 65%, about 50% to about 65%, about 30% to about 60%, about 40% to about 60%, about 45% to about 60%, or about 50% to about 60% by weight.

[0095] Typically, silica (e.g., silica particles) has a silica content of at least 20% by weight, at least 25% by weight, at least 30% by weight, at least 35% by weight, at least 40% by weight, at least 50% by weight, at least 60% by weight, at least 70% by weight, at least 80% by weight, at least 90% by weight, or approximately 100% by weight or 100% by weight, or about 20% to about 100% by weight, based on the total weight of all particles. Any silica(s) may be chemically functionalized to have, for example, bonded or adsorbed chemical groups, for example, bonded or adsorbed organic groups. Any combination of silica(s) may be used. Silica may be silica that is partially or entirely hydrophobic, or silica that becomes hydrophobic by making the surface of the silica hydrophobic through treatment (e.g., chemical treatment). Hydrophobic surfaces may be obtained by chemically modifying silica particles by hydrophobicizing a silane that does not have ionic groups, such as bis-triethoxysilylpropyltetrasulfide. Hydrophobic surface-treated silica particles suitable for use herein may be obtained from commercially available sources, such as Agilon® 454 silica and Agilon® 400 silica from PPG Industries. Silica with a low surface silanol density, such as silica obtained by dehydroxylation at temperatures above 150°C (423.15K) via a calcination process, may be used herein. Intermediate forms of silica (undried silica) obtained from the precipitation process in cake or paste form without drying can be added directly to the mixer as a wet filler, thus eliminating the complex drying process and other downstream processing steps used in the conventional production of precipitated silica.

[0096] In any embodiment and in any step, a coupling agent may be introduced in any step (or in multiple steps or locations) insofar as there is an opportunity for the coupling agent to be dispersed in the complex. The coupling agent may be one or more silane coupling agents, one or more zirconate coupling agents, one or more titanate coupling agents, one or more nitro coupling agents, or any combination thereof. The coupling agents are bis(3-triethoxysilylpropyl)tetrasulfan (e.g., Si69 from Evonik Industries, Struktol SCA98 from Struktol Company), bis(3-triethoxysilylpropyl)disulfan (e.g., Si75 and Si266 from Evonik Industries, Struktol SCA985 from Struktol Company), 3-thiocyanatopropyl-triethoxysilane (e.g., Si264 from Evonik Industries), gamma-mercaptopropyl-trimethoxysilane (e.g., VP Si163 from Evonik Industries, Struktol SCA989 from Struktol Company), gamma-mercaptopropyl-triethoxysilane (e.g., VP from Evonik Industries) The coupling agents may be, or may include, Si263), zirconium dineoalkanolato di(3-mercapto)propionato-O, N,N'-bis(2-methyl-2-nitropropyl)-1,6-diaminohexane, S-(3-(triethoxysilyl)propyl)octanthioate (e.g., NXT coupling agents from Momentive, Friendly, WV), and / or coupling agents having one or more of the same chemical groups. Further specific examples of coupling agents by commercial name include, but are not limited to, NXT Z and NXT Z-50 from Momentive and VP Si363 from Evonik Industries. The coupling agents described herein may be used to impart hydrophobic surface modification (pre-coupled or pre-treated silica) to silica.It should be recognized that any combination of elastomers, additives, and further composites may be added to the elastomer composite, for example, in a mixer.

[0097] The amount of silica (parts per 100 units of rubber, or phr) present in the formed elastomer composite is approximately 0 phr to approximately 200 phr, approximately 1 phr to approximately 200 phr, or 1 phr to 10 phr, or 1 phr to 20 phr, or 1 phr to 25 phr, or 5 to 190 phr, or 10 to 180 phr, or approximately 15 phr to approximately 180 phr, or approximately 55 phr to approximately 150 phr, or approximately Possible ranges include 10 phr to approximately 100 phr, approximately 20 phr to approximately 150 phr, approximately 30 phr to approximately 100 phr, approximately 25 phr to approximately 100 phr, approximately 25 phr to approximately 80 phr, approximately 35 phr to approximately 115 phr, approximately 35 phr to approximately 100 phr, approximately 40 phr to approximately 110 phr, approximately 40 phr to approximately 100 phr, approximately 40 phr to approximately 90 phr, approximately 40 phr to approximately 80 phr, and equivalent levels.

[0098] Other fillers are disclosed in U.S. Patent Application Publication No. 2018 / 0282523 and European Patent No. 2423253(B1), which are incorporated herein by reference.

[0099] The amount of filler (e.g., wet filler alone or wet filler with other fillers) incorporated into the wet filler composite and tread rubber compound is 30 phr to 150 phr, for example, about 5 phr to 100 phr, 10 phr to 100 phr, 20 phr to 100 phr, 30 phr to 100 phr, 40 phr to 100 phr, 50 phr to 100 phr, or 5 phr to 70 phr, 10 phr to 70 phr, 20 phr to 70 phr, 30 phr to 70 phr, 35 It may be in the range of phr~70phr, 40phr~70phr, 5phr~65phr, 10phr~65phr, 20phr~65phr, 30phr~65phr, 35phr~65phr, 40phr~65phr, 5phr~60phr, 10phr~60phr, 20phr~60phr, 30phr~60phr, 35phr~60phr, 40phr~60phr, or other quantities within or outside one or more of these ranges. Other ranges include approximately 15 phr to approximately 180 phr, approximately 20 phr to approximately 150 phr, approximately 25 phr to approximately 80 phr, approximately 30 phr to approximately 150 phr, approximately 35 phr to approximately 115 phr, approximately 35 phr to approximately 100 phr, approximately 40 phr to approximately 100 phr, approximately 40 phr to approximately 90 phr, approximately 40 phr to approximately 80 phr, approximately 29 phr to approximately 175 phr, approximately 40 phr to approximately 110 phr, approximately 50 phr to approximately 175 phr, approximately 60 phr to approximately 175 phr, and equivalent ranges. The filler may be any filler disclosed herein, such as carbon black, silica, or silicon-treated carbon black, whether alone or with one or more other fillers.

[0100] For example, carbon black can be dispersed in an elastomer in a charge amount ranging from 30 phr to 70 phr, or 40 phr to 65 phr, or 40 phr to 60 phr. More specifically, the elastomer may be natural rubber alone or containing one or more other elastomers, and the filler may be carbon black alone or containing one or more other fillers (e.g., silica or silicon-treated carbon black), and the carbon black can be dispersed in the natural rubber in a charge amount ranging from 30 phr to 70 phr, or 40 phr to 65 phr, or 40 phr to 60 phr.

[0101] The tires and treads of the present invention may be manufactured using a compound prepared by curing a particular wet-mix composite. Such a composite may be manufactured by adding a solid elastomer and a wet filler to a mixer in one or more steps or additions. The solid elastomer may be masticated to a temperature of about 90°C (363.15K) or 100°C (373.15K) or higher before the wet filler is added to the mixer. Alternatively, the solid elastomer may be masticated to a temperature of about 90°C (363.15K) or 100°C (373.15K) or higher by at least a portion of the wet filler before any actual dispersion of the filler begins.

[0102] With respect to mixing, mixing may be carried out in one or more mixing steps. Mixing begins when at least the solid elastomer and wet filler are introduced into the mixer and energy is applied to the mixing system that drives one or more rotors of the mixer. One or more mixing steps may be performed after the introduction step is completed, or may overlap with the introduction step for any length of time. For the purposes of the present invention, the introduction step is completed before the mixing step is completed.

[0103] During mixing, at least some of the liquid present in the introduced mixture and / or wet filler is at least partially removed by evaporation. Optionally, a majority (in weight percent) of any liquid from the mixture is removed by evaporation. For example, at least 50% by weight of liquid is removed based on the total weight of liquid removed during mixing. The total weight of liquid removed can be determined from the difference between the liquid content of the wet filler and any liquid remaining in the complex when discharged from the mixer, and any liquid present in or discharged from the mixer when the complex is discharged from the mixer. For example, when the complex is discharged, additional liquid (e.g., unevaporated liquid) may be discharged either with or within the complex, or through an outlet provided in the mixer. Liquid removal by evaporation may represent at least 70% by weight, at least 80% by weight, or 51% to 100% by weight, or 51% to 95% by weight of the total liquid contained in the wet filler introduced into the mixer. Optionally, one or more mixing steps or stages may further remove a portion of the liquid from the mixture by pressing, compressing, and / or squeezing, or any combination thereof.

[0104] With respect to the mixers that may be used to prepare the composite, any suitable mixer capable of combining (e.g., mixing or blending together) the filler with the solid elastomer may be used. The mixer(s) may be a batch mixer or a semi-continuous or continuous mixer. A mixer and process combination may be used, and the mixers may be used in tandem order and / or integrated with other processing equipment. The mixer may be an internal or closed mixer or an open mixer, or an extruder or continuous mixer or kneading mixer or a combination thereof. The mixer may be capable of incorporating the filler into the solid elastomer and / or dispersing the filler in the elastomer and / or distributing the filler in the elastomer. Any one or a combination of commercially available mixers for making rubber compounds may be used in this method.

[0105] The top of a typical batch mixing chamber can be raised or lowered by an air or hydraulic piston commonly referred to as a "floating weight" or "ram." The ram is raised to supply material (e.g., at least a solid elastomer and a wet filler) and lowered to apply pressure to the mixture to keep it within the mixing chamber. Typically, by selecting the batch fill factor and ram pressure, the ram can reach its lowest position to minimize the gap between the ram and the rotor, thereby enabling good filler dispersion. The vertical distance of the ram beyond its minimum position is known as "ram deflection."

[0106] A mixer may have one or more rotors (at least one rotor). For example, each rotor may rotate within its own cylindrical chamber, which may be connected to the chambers of other rotors. The shaft is controlled by a mixing system to which energy (electrical energy) is applied. The rotor may be a device that imparts energy to the mixture and / or a component that forms the mixture. The rotor may be designed to have internal circuits or channels for steam or water or other fluids for cooling and / or heating. At least one rotor or one or more rotors may be a screw rotor, a cross-reversing rotor, a tangential rotor, a kneading rotor, a rotor used in an extruder, a roll mill that imparts significant total specific energy, or a creeper mill.

[0107] One or more mixing steps may be a single mixing step, e.g., a one-stage or single-stage mixing step or process, and the mixing is carried out under one or more of the following conditions: at least one of the mixer temperatures is controlled by a temperature-controlled means having one or more rotors operating at a tip speed of at least 0.6 m / s for at least 50% of the mixing time, or by at least one temperature control means set to a temperature Tz of 65°C (338.15 K) or higher, or the mixing is carried out in the substantial absence of one or more rubber chemicals before the mixer reaches the indicated temperature. In certain cases, in a single-stage or single-mixing step, the composite may be discharged with a liquid content of 10% by weight or less. In other embodiments, two or more mixing steps or stages may be carried out, insofar as one of the mixing steps is carried out under one or more of the conditions described above.

[0108] In multi-stage mixing, the compound (or composite) properties can be improved by a second or any number of subsequent mixing stages, as an optional choice, compared to a composite mixed by the first stage of material mixing alone. In other words, a composite formed from a single-stage mixing can be comparable to a composite formed from further mixing processes, for example, one subjected to a second stage. When such multi-stage mixing is utilized, one or more of the composite properties (e.g., loss tangent and / or modulus ratio) can be improved. The improvement may be 5%, 10%, or 15% or more compared to a composite from a single-stage mixing alone. This improvement can be obtained independently of the type of filler used and independently of the type of elastomer filler.

[0109] In a particular embodiment, the method includes performing mixing at a controlled mixer temperature, for example, through the use of at least one temperature control means. Controlling the mixer temperature means controlling the temperature of at least one surface of the mixer. Optionally, the mixer temperature may be controlled during both the loading and at least one of the mixing steps. The temperature control means may be a temperature control device on and / or within the mixer, or in other cases, may be attached to the mixer (e.g., connected to the mixer) to heat or cool at least one surface and / or one or more parts of the mixer.

[0110] The temperature control means, but are not limited to, the flow or circulation of a heat-conducting fluid through channels in one or more parts of the mixer. For example, the heat-conducting fluid may be water or heat-conducting oil. For example, the heat-conducting fluid may flow through the rotor, the mixing chamber walls, the ram, and the drop door.

[0111] The temperature of at least one temperature control means may be set and maintained, for example, by one or more temperature control units ("TCU"). This set temperature, or TCU temperature, is also referred to herein as "T z It is also called "." In the case of a temperature control means that incorporates a heat-conducting fluid, T z This is an indicator of the temperature of the fluid itself. Heating or cooling provided by the temperature control means is T z Depending on the circumstances, the heat is conducted to at least one surface of the mixer or to one or more parts of the mixer; the heat is then conducted to or from at least one surface, and subsequently to or from the material in the mixer, affecting the temperature of the mixture or a portion thereof, for example, the local temperature of the mixture.

[0112] The mixer may have thermocouples located in different parts of the mixer to provide more accurate measurement of the temperature of the mixer section(s) or the mixture.

[0113] The optimal Tz value can be selected based on the type of filler. For example, in fillers containing carbon black and silicon-treated carbon black (e.g., at least 50%, at least 75%, at least 90%, or all or substantially all of the filler is carbon black), the Tz may have the values ​​specified herein, for example, 65°C (338.15K) or higher or 65°C (338.15K) to 100°C (373.15K). When the filler is silica, the Tz value can be in the range of 40°C (313.15K) to 100°C (373.15K), for example, 40°C (313.15K) to 90°C (363.15K), 40°C (313.15K) to 80°C, 40°C (313.15K) to 75°C (348.15K), 50°C (323.15K) to 100°C (373.15K), 50°C (323.15K) to 90°C (363.15K), 50°C (323.15K) to 80°C, or 50°C (323.15K) to 75°C (348.15K).

[0114] The energy applied to the mixture during the mixing process can be controlled through mixer settings and process control. For example, in a batch mixer, the total specific energy takes into account the energy applied to the rotor(s) between the input of the solid elastomer and / or wet filler and the discharge of the composite per kg on a dry weight basis. In a continuous mixer, the total specific energy is the input per kg of output on a dry weight basis under steady-state conditions. In a process with multi-stage mixing, the total specific energy is the sum of the specific energies from each mixing process. Determining the total specific energy preferably does not include the amount of energy used to mold or form the discharged composite (e.g., excluding the energy of roll milling of the composite). The resulting “total specific energy” is the energy E applied to the mixing system driving one or more rotors per mass of the composite on a dry weight basis, as defined herein. R (For example, electrical energy). This total specific energy is also E 合計It may also be written as follows. As described herein, the current process imparts total specific energy under selected operating conditions that balance a longer mixing time with a reasonable amount of evaporation or removal of water over time.

[0115] Optionally, the process includes, in at least one of the mixing steps, mixing such that the resulting total specific energy is at least 1,400 kJ or at least 1,500 kJ per kg of the composite, for example, at least 1,600 kJ / kg, at least 1,700 kJ / kg, at least 1,800 kJ / kg, at least 1,900 kJ / kg, at least 2,000 kJ / kg, at least 2,500 kJ / kg, or at least 3,000 kJ / kg. As an optional choice, the total specific energy is approximately 1,400 kJ / kg of composite or approximately 1,500 kJ / kg of composite (or per kg of mixture present in the mixer) to approximately 10,000 kJ / kg of composite (or per kg of mixture present in the mixer), for example, 2,000 kJ / kg to approximately 5,000 kJ or 1,500 kJ / kg to 8,000 kJ / kg, 1,500 kJ / kg to 7,000 kJ / kg, 1,500 kJ / kg to 6,000 kJ / kg. This could be a range of 1,500 kJ / kg to 5,000 kJ / kg, 1,500 kJ / kg to 3,000 kJ / kg, 1,600 kJ / kg to 8,000 kJ / kg, 1,600 kJ / kg to 7,000 kJ / kg, 1,600 kJ / kg to 6,000 kJ / kg, 1,600 kJ / kg to 5,000 kJ / kg, 1,600 kJ / kg to 4,000 kJ / kg, 1,600 kJ / kg to 3,000 kJ / kg, or any other value within these ranges.

[0116] Optionally, the process includes, in at least one of the mixing steps, mixing such that one or more rotors operate at a tip velocity of at least 0.5 m / s for at least 50% of the mixing time or at a tip velocity of at least 0.6 m / s for at least 50% of the mixing time. The energy input to the mixing system is at least partially a function of the velocity and type of at least one rotor. The tip velocity, considering the rotor diameter and rotor velocity, can be calculated by the following formula: Tip velocity m / s = π × (rotor diameter, m) × (rotational speed, rpm) / 60.

[0117] Since the tip velocity may vary throughout the mixing process, optionally, a tip velocity of at least 0.5 m / s or at least 0.6 m / s is achieved for at least 50% of the mixing time, e.g., at least 60%, at least 70%, at least 75%, at least 80%, at least 85%, at least 90%, at least 95%, or substantially all of the mixing time. The tip velocity may be at least 0.6 m / s, at least 0.7 m / s, at least 0.8 m / s, at least 0.9 m / s, at least 1.0 m / s, at least 1.1 m / s, at least 1.2 m / s, at least 1.5 m / s, or at least 2 m / s for at least 50% of the mixing time or for the other parts of the mixing listed above. The tip velocity may be selected to minimize the mixing time, or to be 0.6 m / s to 10 m / s, 0.6 m / s to 8 m / s, 0.6 to 6 m / s, 0.6 m / s to 4 m / s, 0.6 m / s to 3 m / s, 0.6 m / s to 2 m / s, 0.7 m / s to 4 m / s, 0.7 m / s to 3 m / s, 0.7 m / s to 2 m / s, or 0.7 m / s to 10 m / s (for example, for at least 50% of the mixing time or during other mixing times as specified herein). Alternatively, or in addition, the tip velocity may be selected to maximize the overall rate.

[0118] The wet-mixed composite can be discharged from the mixer with fillers dispersed in the elastomer in a charge of at least 20 phr, with a filler yield loss of 10% or less and a liquid content of 10% by weight or less of the total composite. Discharge ("damping" in batch mixing) may be performed based on a time or temperature or specific energy or output parameter selected to minimize rubber degradation. In one embodiment, the mixing time may be determined from the period from when the loading is completed to the time of discharge. In a batch-internal mixer, the mixing time may be determined from the ram downtime, the time it takes for the ram to operate at its lowest position and be fully closed. In other embodiments, the lowest position of the ram (i.e., its fully set position) may allow for a certain amount of ram deflection. The mixing time does not include the period when additional components are added, for example, when one or more additional portions of elastomer and / or fillers are added. Optionally, in a continuous mixer, the nominal mixing time (or residence time) may be calculated from the mixer chamber volume and the volumetric production rate.

[0119] Optionally, dispensing is performed based on a specified mixing time. The mixing time between the start of mixing and dispensing may be approximately 1 minute or more, for example, approximately 1 to 40 minutes, approximately 1 to 30 minutes, approximately 1 to 20 minutes, or 1 to 15 minutes, or 5 to 30 minutes, or 5 to 20 minutes, or 5 to 15 minutes, or 1 to 12 minutes, or 1 to 10 minutes, or 3 to 30 minutes, or other times. Alternatively, for batch internal mixers, ram downtime may be used as a parameter to monitor the time related to batch mixing time. For example, ram downtime may be in the range of 3 to 30 minutes, 3 to 20 minutes, 3 to 10 minutes, 5 to 30 minutes, 5 to 20 minutes, or 5 to 10 minutes.

[0120] Optionally, dispensing is performed based on damping or dispensing temperature. For example, a mixer may have a damping temperature in the range of 120°C (393.15K) to 180°C (453.15K), 120°C (393.15K) to 190°C (463.15K), 130°C (403.15K) to 180°C (453.15K), for example, 140°C (413.15K) to 180°C (453.15K), 150°C (423.15K) to 180°C (453.15K), 130°C (403.15K) to 170°C (443.15K), 140°C (413.15K) to 170°C (443.15K), 150°C (423.15K) to 170°C (443.15K), or other temperatures within or outside these ranges.

[0121] The extruded complex may have a liquid content of 10% by weight or less, based on the total weight of the complex, as outlined by the following formula: Liquid content of the complex (%) = 100 * [Mass of liquid] / [Mass of liquid + Mass of dry composite]

[0122] The extruded wet mixed complex may have a liquid content of 10% by weight or less based on the total weight of the complex, for example, 9% by weight or less, 8% by weight or less, 7% by weight or less, 6% by weight or less, 5% by weight or less, 2% by weight or less, or 1% by weight or less based on the total weight of the complex. This amount may range from about 0.1% by weight to 10% by weight, or about 0.5% by weight to 9% by weight, or about 0.5% by weight to about 7% by weight, based on the total weight of the complex extruded from the mixer at the end of the process. The liquid content (or "moisture content") may be a measured weight percentage of liquid present in the complex, based on the total weight of the complex. There may optionally be additional liquid present in the mixer that is not retained in the extruded complex. This excess liquid is not part of any liquid content calculated from the complex.

[0123] Filler yield loss is determined by subtracting the measured filler phr in the extruded composite from the theoretical maximum phr of filler in the elastomer (assuming all filler introduced into the mixer is incorporated into the composite). Filler that detaches from the composite surface due to insufficient integration into the elastomer is included in the filler yield loss. This measurement can be obtained from thermogravimetric analysis (TGA). Therefore, the filler yield loss (%) is calculated as follows: [((Theoretical filler phr) - (Measured filler phr)) / ((Theoretical filler phr))] × 100

[0124] Optionally, the fill factor (on a dry weight basis) of the wet filler and the solid elastomer containing natural rubber may be 70% or less, or 68% or less, for example, in the range of 60% to 70%, 60% to 68%, or 65% to 68%. Such conditions may be used for a solid elastomer containing at least 50%, at least 75%, at least 90%, or at least 95% natural rubber, for example, a blend of natural rubber and at least one further elastomer, for example, polybutadiene and / or styrene-butadiene rubber, or other elastomers disclosed herein.

[0125] Optionally, and not necessarily limited to, the liquid release rate, including the evaporation rate of the liquid from the complex during mixing, may be measured as the time-averaged release rate of liquid per kg of the complex, which may be 0.01–0.14 kg / (min·kg) or 0.01–0.07 kg / (min·kg) or other rates below or above this range. This release rate may be the overall release rate of liquid removal by any means during mixing, or it may be the release rate due to evaporation alone. In the case of aqueous liquids, the evaporation rate may be the vapor release or vapor generation rate. Release rates below 0.01 kg / (min·kg) may generally indicate longer times to remove the liquid, for example, at a Tz below 65°C (338.15 K) and / or a specific energy level below 1,500 kJ / kg, and / or a tip velocity below 0.5 m / s or 0.6 m / s. Release rates above 0.15 kg / (min·kg) may indicate shorter mixing times. If the time-averaged release rate is not optimized, it can result in insufficient dispersion and rubber properties.

[0126] Optionally, the maximum pressure can be controlled. When the mixer is a batch mixer with a ram, the pressure in the mixer chamber can be affected by controlling the pressure applied to the ram cylinder.

[0127] Optionally, a multi-step mixing process may be used to produce a wet-mixed composite having at least two mixing steps or stages. These two (or more) mixing steps may be a multi-step or multi-step mixing process having a first mixing step or stage and at least a second mixing step or stage. One or more of the multi-step mixing processes may be batch, continuous, semi-continuous, or a combination thereof.

[0128] With respect to a multi-step process, a method for preparing a composite comprises the step of adding or introducing at least a) one or more solid elastomers and b) one or more fillers to a first mixer, wherein at least one filler or a portion of at least one filler is a wet filler as described herein (e.g., a wet filler comprising a filler and a liquid present in an amount of at least 15% by weight based on the total weight of the wet filler). The solid elastomers are combined with the wet fillers to form a mixture or composite during this mixing step(s), which may be considered a first mixing step or step. The method further comprises mixing the mixture in this first mixing step to such an extent that at least a portion of the liquid is removed by evaporation or an evaporation process performed during mixing. This first mixing step(s) or step is performed using one or more of the processes described above for forming a composite, with the understanding that after the completion of the first mixing, the mixture discharged from the mixer after the first mixing step(e.g., the discharged mixture) does not need to have a liquid content of 10% by weight or less. In other words, the mixture obtained by a multi-stage process (or multiple stages) from the first mixer (or first mixing step) to the completion of the first mixing may have a liquid content exceeding 10% by weight, but not a liquid content reduced (in weight%) compared to the liquid content of the combined solid elastomer and wet filler at the start of the first mixing step, for example, a liquid content reduced to less than the liquid content at the beginning of any subsequent mixing step, for example, a liquid content reduced by at least 50% by weight.

[0129] The method then includes mixing or further mixing the mixture in at least a second mixing step or stage using the same mixer (i.e., a first mixer) and / or using a second(or more) mixer different from the first mixer.

[0130] After the first mixing, any further mixing steps(s) performed for multi-stage mixing may utilize one or more of the mixing procedures, parameters, or steps used in the first mixing step as described herein. Therefore, when performing further mixing steps or stages, the same or different mixer design and / or the same or different operating parameters as those of the first mixer may be used in the further mixing steps. The mixers and any selection thereof described prior to the first mixing step, and / or the operating parameters described prior to the mixing step, may be optionally used in further or second mixing steps (e.g., mixing steps described herein including a tip velocity of at least 0.5 m / s for at least 50% of the time or at least 0.6 m / s for at least 50% of the time, and / or a Tz of 50°C (323.15 K) or higher, 60°C (333.15 K) or higher, or 65°C (338.15 K) or higher). Therefore, in a method for preparing a composite by multi-stage mixing, one or more of the following parameters may be used in at least one mixing step, at least two mixing steps, or all of the mixing steps: At least one temperature control means is set to a temperature Tz of 65°C (338.15K) or higher during the mixing; and / or During the above mixing, one or more rotors operate at a tip speed of at least 0.5 m / s for at least 50% of the mixing time to perform mixing such that the resulting composite has a total specific energy of at least 1500 kJ / kg; and / or During the above input (a) or mixing (b), at least one additive selected from degradation inhibitors and coupling agents is optionally added, and after the mixer reaches a temperature of 120°C (393.15K) or higher, one or more rubber chemicals are optionally added; and / or The above input (a) and mixing (b) are carried out in the substantially absence of one or more rubber chemicals before the mixer reaches the indicated temperature; and / or The mixer has a fill factor, which is 72% or less based on the dry weight of at least the solid elastomer and wet filler.

[0131] During mixing in the second mixer, the ram pressure can be reduced under one or more of the following conditions, for example: (i) The ram may be installed, but the ram must be under pressure (e.g., 5 psi (3.448275 × 10) -2 No pressure (below Pa) is essentially applied. (ii) The ram is raised to at least 75% of its highest level. Some mixers allow the ram to be positioned at a specific height. The ram in the fully set position is at 0% of its highest level, as opposed to being raised to its highest level or fully open position, which is the typical position of the ram when material is introduced into the mixer. The ram positioned at at least 75% of its highest level is raised to, for example, at at least 80%, at least 85%, at least 90%, at least 95%, or fully, relative to its highest level (100%), so as to ensure that contact between the ram and the elastomer introduced into the mixer is minimized. (iii) When no pressure is applied to the mixing chamber, certain rams may act as floating weights, for example, in a floating form. The rams may come into contact with the elastomer, but the pressure applied is minimal. (iv) The ram is positioned so as not to be in substantially contact with the mixture. When the content has a low fill factor, for example, 25%, it may not be necessary to position the ram height to at least 75% of its highest level. The ram may be positioned at a height such that it is not in substantially contact with the mixture, for example, 10% or less of the surface area of ​​the ram is in contact with the mixture, for example, 5% or less of the surface area of ​​the ram, or 0% of the surface area of ​​the ram is not in contact with the mixture. (v) Select a mixer that does not have a ram. (vi) The fill factor of the mixture is in the range of 25% to 70% on a dry weight basis, for example, 25% to 60%, 25% to 55%, 25% to 50%, 25% to 45%, 25% to 40%, 30% to 70%, 30% to 60%, 30% to 55%, 30% to 50%, 30% to 45%, 30% to 40%, 35% to 70%, 35% to 60%, 35% to 55%, 35% to 50%, 35% to 45%, or 35% to 40%. By controlling the fill factor, it may not be necessary to manipulate the ram or position.

[0132] Optionally, after the complex is discharged from the second mixer, it may be subjected to further mastication by mixing in, for example, the first or second mixer, or the third mixer.

[0133] Tires, treads, and compounds Treads and tires can be mixed, assembled, molded, shaped and cured by various methods readily apparent to those skilled in the art.

[0134] The tire tread of the present invention may include one or more overlapping elastomer layers, such as a tire carcass or belt, and one or more rubber compounds extruded into an inner or lower layer between the outer layer or cap that contacts the road surface. One or more further layers or zoned layers overlapping within the cap or inner layer may be used. Alternatively, the tire tread of the present invention may include a multi-zone elastomer layer. For example, an axial zone traversing the tire tread may be made of one rubber compound in the equatorial plane and one or more different rubber compounds in the lateral outer plane. A similar zoned configuration may be used in one or more inner layers of the tread. The volume of voids (grooves or sipes) may vary across the multi-zone configuration, with or without the selection of different rubber compounds in such zones. The thickness of the elastomer layer may vary. The composite material of the present invention can be used in rubber compounds for the outer layer of a tread and for the equatorial zone of a multi-zone tread, improving wear resistance and rubber performance in the region of maximum stress during tire operation without generating excessive heat.

[0135] In addition, the tire and tire tread of the present invention may include a composite rubber compound in the shoulder region of the inner tread and carcass configuration, where mechanical stress tends to be high, particularly in trucks and heavy-duty vehicles. Such a zone or bead of rubber compound may be used in a multi-zone inner layer design, for example, together with a low-heat-generating rubber compound in the lower mechanical stress portion of the inner layer of the tread, which has a very low loss tangent. The use of the present invention in such a shoulder region also extends the tire life useful for truck and other heavy-duty vehicle tires, as it facilitates retreading.

[0136] The rubber compounds for treads and tires according to the present invention may, in addition to the composite of the present invention, include, for example, a plasticizer including processing oil and resin, a pigment, an antioxidant, an anti-ozone wax, a crosslinking system based on sulfur and / or peroxide and / or bismaleimide, a crosslinking activator including zinc monoxide and stearic acid, an extender oil, and one or more agents for coating silica, such as alkoxysilane, polyol, or amine.

[0137] It will be readily apparent to those skilled in the art that rubber compositions (e.g., those made from the composites of the present invention) can be admixtured by methods generally known in the field of rubber admixture, for example, by mixing a sulfur-vulcanizable constituent rubber with a variety of commonly used rubber additives, such as crosslinking aids, e.g., sulfur, activators, retarders and accelerators; processing additives, e.g., rubber processing oils, resins including tackifying resins, silica and plasticizers; fillers, pigments, fatty acids, zinc oxide, waxes, antioxidants and ozone degradation inhibitors; compounding accelerators and reinforcing materials, e.g., reinforcing particles, fibers, granules and platelets, e.g., carbon black and silica and combinations thereof. As is known to those skilled in the art, depending on the intended use of the sulfur-vulcanizable material (rubber) and the sulfur-vulcanizable material (rubber), the additives mentioned above are generally used in selected and effective amounts and incorporated into the compound during an optimized mixing process stage.

[0138] The rubber compound may be developed using paraffin, aromatic, or naphthenic oils in amounts of extender oil between 0 and 50 phr. As an optional choice made possible by the composite of the present invention, the extender oil and resin may be used in smaller amounts, for example, 5 phr or less, or 2 phr or less, to obtain better mechanical properties and wear resistance in the rubber compound and tire tread, and to improve the processability of compounds having very low oil or resin levels.

[0139] When used in a compound, fatty acids, such as stearic acid, may be added in an amount of about 0.5 to about 3 phr. A typical amount of zinc oxide may be about 1 to about 5 phr. A typical amount of wax may be about 1 to about 5 phr. Microcrystalline wax can be used. A typical amount of thiglioside may be about 0.1 to about 1 phr. Typical thigliosides may be, for example, pentachlorothiophenol and dibenzamide diphenyl disulfide.

[0140] Vulcanization is carried out in the presence of a sulfur vulcanizing agent. Examples of suitable sulfur vulcanizing agents include elemental sulfur (free sulfur) or sulfur-donating vulcanizing agents, such as amine disulfides, polymeric polysulfides, or sulfur olefin adducts. Preferably, the sulfur vulcanizing agent is elemental sulfur. As is known to those skilled in the art, the sulfur vulcanizing agent is used in amounts ranging from about 0.5 to about 4 phr, or even, in some situations, up to about 8 phr, about 1.5 to about 2.5 phr, and occasionally, preferably, about 2 to about 2.5 phr.

[0141] Accelerators are used to control the time and / or temperature required for vulcanization and to improve the properties of the vulcanized product. In one embodiment, a single accelerator system, i.e., a primary accelerator, may be used. Primary accelerators may be used in a total amount ranging from about 0.5 to about 4 phr, preferably from about 0.8 to about 2.5 phr. In another embodiment, a combination of primary and secondary accelerators may be used, with a second accelerator used in a smaller amount (about 0.05 to about 3 phr) to activate and improve the properties of the vulcanized product. These accelerator combinations are expected to produce a synergistic effect on the final properties, which may be somewhat better than those produced by using either accelerator alone. In addition, retarding accelerators may be used that are not affected by the normal processing temperature but produce a sufficient effect at normal vulcanization temperatures. Vulcanization retarders may also be used.

[0142] Suitable types of accelerators that may be used are amines, disulfides, guanidine, thiourea, thiazole, thiuram, sulfenamides, dithiocarbamates, and xanthetes. Preferably, the primary accelerator is a sulfenamide. When a second accelerator is used, the secondary accelerator is preferably a guanidine, dithiocarbamate, or thiuram compound.

[0143] In practice, the tread rubber composition may be prepared, for example, in at least one non-productive mixing step in an internal rubber mixer, and often in a series of at least one, usually two, separate and individual preliminary internal rubber mixing steps or stages, in which the composite is first mixed with any further fillers or elastomers or other additives ("minor portions"), and then in a finishing mixing step ("productive" mixing step), in an internal rubber mixer, or optionally in an open mill mixer, the curing agents (sulfur and sulfur vulcanization accelerators) are blended in at a lower temperature and for a substantially shorter period of time.

[0144] Typically, after each internal rubber mixing step, the rubber mixture (composition) is removed from the rubber mixer and cooled to a temperature below 40°C (313.15K), for example, in the range of about 20°C (293.15K) to about 40°C (313.15K), and then returned to the internal rubber mixer for the next sequential mixing step or stage. Such temperature selection and handling techniques in non-productive mixing stages and subsequent productive mixing stages are well known to those skilled in the art.

[0145] The mixing of the finishing rubber composition can be achieved by such a sequential mixing process. The components can be mixed in at least two stages, namely at least one “non-productive” or preliminary stage followed by a productive mixing stage. The finishing curing agent is typically mixed in a productive or finishing mixing stage, where the mixing typically occurs at a temperature (maximum or highest temperature) lower than the mixing temperature (possibly) of the preceding non-productive mixing step(s).

[0146] The formation of tire treads or other components is completed by conventional means, for example, by extrusion, calendering, or molding of a rubber composition, to give a molded, unvulcanized rubber article or component, such as a tire tread layer, or a complete tread ready for assembly. Such forming and manufacturing operations are well known to those skilled in the art.

[0147] It is understood that tires, as manufactured articles, are prepared by molding and curing an assembly of their components in a suitable mold at high temperatures (e.g., 140°C (413.15K) to 170°C (443.15K)) and high pressures.

[0148] In general, any tire tread described herein, or a tire containing one of the tire treads, is another embodiment of the present invention.

[0149] The tires and tire treads may be fitted to vehicles, for example, vehicles that carry heavy loads and operate at sustained speeds, such as trucks, tractors, trailers, or buses.

[0150] For example, the tire of the present invention may be a pneumatic tire having a tread with radial carcass reinforcements and further layers or zones of elastomerous material (i.e., rubber compound), intended to fit vehicles that carry heavy loads and operate at sustained speeds, such as trucks, tractors, trailers, or buses.

[0151] Alternatively, the tires and tire treads may fit other vehicles, such as light trucks, passenger cars, high-performance vehicles, motorcycles, vehicles used off-road, construction machinery, aircraft, and vehicles fitted to roads that have rubber treads mounted on roads.

[0152] Specific examples of the tire, filler, elastomer, and / or other parameters of the present invention include the following:

[0153] The tire may be a tire for a vehicle used off-road or for construction machinery, and the tread may be an elastomer of 60-100 phr containing at least one natural or synthetic polyisoprene, and at least 130 m 2 It contains at least 40 phr of filler, which includes at least one carbon black having a BET of 115 ml / g and a COAN of 115 ml / g or less.

[0154] The tire may be a tire for a vehicle used on a road or for a construction machinery vehicle, and the tread further comprises at least one styrene-butadiene copolymer, or a butadiene polymer, or a combination thereof.

[0155] The tire may be a tire for a vehicle used off-road or for construction machinery, and the tread may be an elastomer of 60-100 phr containing at least one natural or synthetic polyisoprene, and at least 130 m 2 It contains at least one carbon black having a BET of 115 ml / g and a COAN of 115 ml / g or less, and at least 40 phr of filler containing at least one silica of 5 to 10 phr. For example, the tire may be a tire for a vehicle used off-road or for construction machinery, and the tread may be 150 m 2 Further comprising at least one carbon black having a BET greater than / g, an OAN less than 100ml / g, and a COAN less than 90ml / g.

[0156] The tire may be a high-performance car or motorcycle tire, and the tread is made of a 100 phr elastomer containing at least one polymer selected from solution styrene-butadiene copolymer and butadiene polymer and combinations thereof, and 150-220 m 2 At least one carbon black with STSA of / g and 150-200m 2 It contains at least 40 phr of filler, which includes at least one silica having a BET of / g.

[0157] The tire may be a truck or bus tire, and the tread shall consist of at least one natural or synthetic polyisoprene elastomer of 60-100 phr, and at least 115 m 2 The filler comprises at least 30 phr of filler containing at least one carbon black having STSA of 1 / g and COAN of less than 110 ml / g, and at least one silica filler of 1 to 25 phr.

[0158] The tire may be a truck or bus tire, and the tread shall consist of at least one natural or synthetic polyisoprene elastomer of 60-100 phr, and at least 115 m 2 The filler comprises 45-60 phr containing at least one carbon black having STSA at 1 / g and COAN at less than 110 ml / g, and at least one silica filler at 1-25 phr.

[0159] The tire may be a truck or bus tire, and the tread is made of at least one natural or synthetic polyisoprene elastomer of 60-100 phr, and 150 m 2 The filler comprises at least 30 phr of carbon black having a BET greater than / g, an OAN less than 100 ml / g, and a COAN less than 90 ml / g, as well as at least one silica filler of 1 to 25 phr.

[0160] The tire may be a truck or bus tire, and the tread shoulder component shall consist of at least one natural or synthetic polyisoprene elastomer of 60-100 phr, and at least 120 m 2 The filler comprises at least 40 phr of carbon black having a BET of 1 / g and a COAN of less than 110 ml / g, and at least one silica filler of 1 to 20 phr.

[0161] The tire may be a truck or bus tire, and the tread shoulder component is at least one natural or synthetic polyisoprene elastomer of 60-100 phr, and 150 m2 The filler comprises at least 40 phr of carbon black having a BET greater than / g, an OAN less than 100 ml / g, and a COAN less than 90 ml / g, as well as at least one silica filler of 1 to 25 phr.

[0162] The tire's tread's lower layer consists of at least one natural or synthetic polyisoprene elastomer, polybutadiene elastomer, or a combination thereof, in a quantity of 60-100 phr, and 100 m 2 It may contain at least 40 phr of filler, including at least one carbon black with a BET of less than 110 g / kg and an I2 valency of less than 110 g / kg.

[0163] The tire may have a tire tread containing at least 20 phr of filler, which includes at least one carbon black selected from surface-modified carbon black, oxidized carbon black, multiphase aggregated carbon black (e.g., ECOBLACK® material), and carbon black having a surface hydrogen content of at least 2000 ppm.

[0164] Optionally, wet-mix composites may be used in pneumatic tires and non-pneumatic or solid tires in various parts of the tire other than the tire tread, such as the base, undertread, inner liner, tire sidewall, tire sidewall insert, tire wire skim, and cushion rubber for retreaded tires, or may be manufactured for use (for example, to form a vulcanized product to be incorporated).

[0165] In some embodiments, the composites and formulations described herein are used in various tire designs, for example, U.S. Patent Nos. 3,157,218; 6,247,512; 8,936,056; 9,713,943; 10,308,073; 6,540,858; 9,649,883; 8,302,643; 9,713,942; 8,720,508; 8,939,183; 9,387,728; 9,783,004; 10,245,891; 10,336,14 It is used in, or manufactured for use in, the specifications described in U.S. Patent No. 0; U.S. Patent No. 7,028,734; U.S. Patent No. 7,735,533; U.S. Patent No. 8,695,662; U.S. Patent No. 8,936,056; U.S. Patent No. 10,399,386; U.S. Patent No. 10,543,718; U.S. Patent Application Publication No. 2019 / 0351716 and U.S. Patent Application Publication No. 2020 / 0070577; and International Publication Brochure No. 2018 / 122496A1; International Publication Brochure No. 2014 / 102136A1; International Publication Brochure No. 2019 / 092361A1; and International Publication Brochure No. 2019 / 122618A1.

[0166] With respect to the present invention, any “optional” or “optional feature” can be combined with other optional features. The disclosures herein refer to certain shown examples, which are presented as examples and should be understood not to be limiting. The above detailed description considers preferred examples, but should be construed to cover all variations, substitutions, and equivalents of such examples, which may fall within the spirit and scope of the invention as defined by further disclosures.

[0167] The entire contents of all listed references in this disclosure are incorporated herein by reference to the extent that they do not contradict this disclosure.

[0168] The present invention may include any combination of the various features or embodiments described in the text and / or paragraphs described above and / or in the claims. Any combination of the features disclosed herein shall be part of the present invention, and no limitation is intended with respect to the combinatable features.

[0169] Other embodiments of the present invention will be apparent to those skilled in the art from consideration of this specification and practices of the present invention disclosed herein. This specification and examples are intended to be merely illustrative, with the true scope and spirit of the invention being shown below by its claims and equivalents. [Examples]

[0170] The example describes the preparation of a wet-mix composite (masterbatch), a compound prepared from the masterbatch, and the corresponding vulcanized tire treads of the present invention (Samples E1 and E3), as well as comparative materials (Samples C1 and C2).

[0171] Examples 1-3 Preparation of Sample E1 Wet Mixture For the wet-mixed composite used to prepare the rubber compound for the tire tread (Sample E1) of the present invention, the wet carbon black was obtained by jet milling N234 carbon black pellets (Vulcan® 7H carbon black obtained from Cabot Corporation), and then re-pelletizing and wetting the dried milled carbon black in a pin pelletizer with reverse osmosis (RO) treated water. The moisture content of the wet carbon black was in the range of 54-60% by weight.

[0172] The wet composite using wet carbon black and solid natural rubber was mixed in a two-stage mixing process with a target filler charge of 51 phr. The first stage of mixing to form the composite was carried out in a Kobelco BB-72 tangential mixer fitted with a 4WN rotor, with a net capacity of 66.2 L, according to the mixing protocol in Table 1A. The resulting mixture was transferred to a TSR-125 twin-screw damping extruder (Kobelco Kobe Steel Group) fitted with a fixed blade, further processed, and discharged into a second mixer for the second stage of mixing. The second stage of mixing was carried out in a Kobelco BB-16 tangential mixer (14.4 L capacity) fitted with a 6WI rotor, according to the mixing protocol in Table 1B. In this protocol, mastication and water evaporation were completed to obtain the composite by using an automatic control unit that maintained the mixture temperature (at a constant value of 135°C (408.15K)) by varying the mixer rpm. The resulting mixture was transferred to a twin-screw damping extruder (Kobelco Kobe Steel Group) fitted with a roller die and converted into a composite sheet. Standard grade RSS3 natural rubber (Von Bundit Co., Thailand) was used, and a degradation inhibitor (2phr 6PPD) was added during the first stage of mixing. [Table 1A] [Table 1B]

[0173] Preparation of Sample C2 Dry Mixture The comparative dry-mixed composite and compound were mixed and blended as described later in Tables 2 and 4-5. Unless otherwise specified, the rubber used was standard grade RSS3 natural rubber (Von Bundit Co., Thailand).

[0174] Preparation of Sample C1 Solid Elastomer Masterbatch C1 comparative solid elastomer masterbatch samples were prepared by the liquid masterbatch process of U.S. Patent No. 8,586,651, Example 2, unless otherwise described below.

[0175] The elastomer latex (diluted and sludge-free MVL Field latex) had a dry rubber content of 28% by weight, and the filler slurry contained 13-14% by weight of carbon black (Vulcan® 7H carbon black (N234 grade) obtained from Cabot Corporation, Boston, MA). By adjusting the flow rate, the target, finish carbon black charge of 50 phr was obtained at the desired production rate. The average carbon black charge level of the resulting complex was 50.8 phr. The dehydrated complex was masticated and mixed with 2 phr of antioxidant (6 PPD) in a continuous mixer (Farrel Unimix Continuous Mixer (FCM) with two #15 rotors; operating at 190-320 rpm, Farrel Corporation, Ansonia, CT), dried, further masticated, cooled and dried in an open mill.

[0176] The resulting solid elastomer masterbatch composites were mixed according to the formulations shown in Table 3 and the processes outlined in Tables 2 and 4.

[0177] Compound preparation All compound mixing processes were carried out as described in Tables 2 and 4-5 below. The composites and compound batches were mixed using a 320-liter cross-reverse mixer (Harburg Feudenberger GK 320) and a 55-liter cross-reverse mixer (Carter 55L with a swirling rotor and cross-reverse). The first stage mixing of Comparative Examples C1 and C2 was achieved using the 320L mixer, and the downstream mixing operation was performed using the 55L mixer. All mixing stages for Sample E1 of the present invention were performed using the 55L mixer. The mixing stages were selected to achieve the desired Mooney viscosity value in the range of 6565-80 MU (ML(1+4) at 100°C (373.15K)) in the finishing compound.

[0178] The first stage of mixing the compounds (C1, E1, and C2 samples) was carried out as described in Table 2. [Table 2]

[0179] The water content of the extruded composite before treatment was measured using a water balance (Model: HE53, Manufacturer: Mettler Toledo NA, Ohio). The composite was sliced ​​into small pieces (size: length, width, height < 5 mm), and 2-2.5 g of material was placed on a disposable aluminum disc / plate and placed in the water balance. Weight loss was recorded at 125°C (398.15 K) for 30 minutes. At the end of the 30 minutes, the water content of the composite was recorded as follows: Water content of the composite = ((Initial weight - Final weight) / Initial weight) * 100

[0180] The amount of carbon black in the composite was determined by thermogravimetric analysis (Model Q500 units, manufacturer: TA Instruments, DE). Approximately 15-20 mg of rubber sample was used. First, the sample was heated from room temperature to 125°C (398.15K) at 30°C (303.15K) / min under a nitrogen atmosphere, and kept isothermable for 30 minutes to remove moisture. Then, it was heated to a maximum of 550°C (823.15K) at 30°C (303.15K) / min and kept isothermable for 5 minutes to determine the rubber content. After switching the atmosphere to air, the sample was then heated to a maximum of 800°C (1073.15K) at 30°C (303.15K) / min and kept isothermable for 15 minutes to determine the carbon black (CB) content and other residues. The amount of CB added was then calculated based on the rubber and CB content data.

[0181] The following tests were used to obtain the rubber properties for each of the vulcanized tire treads: - Tensile stress at 100% elongation (M100) and 300% elongation (M300) was evaluated by ASTM D412 at 23°C (296.15K) (RT) and 50% relative humidity. The loss tangent was measured in tensile mode under a pre-tension of 0.5N, at 10Hz with a 0.5% strain, by temperature sweep of dynamic mechanical analysis. The results are reported at a temperature of 60°C (333.15K).

[0182] Tread mixing procedure The finishing compound was prepared using the formulations shown in Table 3. These formulations were mixed as described in Tables 2 and 4.

[0183] To convert and blend the C2 dry mixed composite into a vulcanized tire tread, at least one further mixing step was performed as described in Table 5.

[0184] The components used in all formulations included carbon black filler (Vulcan® 7H(N234) carbon black obtained from Cabot Corporation), antioxidant 6PPD [N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine] and TMQ, standard rubber grades of zinc oxide, stearic acid, and sulfur, and TBBS accelerators, all obtained from Akrochem, Akron, Ohio. The solid-dry RSS3 natural rubber had a moisture content of <1% by weight. [Table 3] [Table 4] [Table 5]

[0185] Tires made with tread compounds C1, E1, and C2. The manufacture of tires made using the tread compound and comparative compound of the present invention was carried out by a known process.

[0186] A tire (tire size: 195 / 55R15) was assembled using the ORBITREAD® retreading device (McNeil & NRM, Inc., Akron, Ohio) and process. The tire was assembled and cured according to standard techniques known in the art, including the following steps: (1) a new commercial tire was polished to remove the tread compound; (2) a rubber compound was extruded and applied to the tire; (3) the stripped tire was cured at 150°C (423.15K) using predetermined curing conditions (curing time) based on curing curves, thermocouple measurements of the tire temperature profile, and modeling of the tire curing behavior.

[0187] Table 6 lists the tested properties of the experimental C1, E1, and C2 hardened tire treads, along with the same properties measured on a series of 32 comparative commercially available tire treads designed for heavy-duty vehicles, such as trucks, containing natural rubber and carbon black as sole rubber and reinforcing fillers, respectively. [Table 6]

[0188] The data in Table 6 demonstrate that the tire tread compound according to the present invention, comprising natural rubber and wet carbon black, has the following characteristics: (a) a higher tensile stress ratio (M300 / M100) and (b) a lower δ value than Comparative Example C2 prepared by a dry mixing process; and (a) equivalent elongation at break and (b) a close M300 / M100 value compared to Comparative Example C1 prepared by a liquid masterbatch process, while having significant wet mixing composite processing advantages obtained by eliminating the complexity and limitations of liquid masterbatches.

[0189] The data in Table 6 further demonstrate that the tire tread of the present invention has one of the following combinations: (a) higher elongation at break and, in all but two cases, a higher tensile stress ratio (M300 / M100); and (b) lower or comparable tanδ values ​​compared to a wide range of commercially available truck tire tread compounds made from natural rubber / carbon black formulations with comparable reinforcing grade carbon black filler at similar filler content levels.

[0190] Example 4 Filler dispersion in tread compounds The amount of carbon black filler dispersed in tire treads prepared using the compounds of Examples 1-3 was measured together with samples of commercially available truck tire treads containing comparable rubber compounds using the following method. The macrodispersion of the vulcanized compound was shown by V, and the area percentage of undispersed carbon black particles larger than 10 μm was determined in the tread samples using a transmission-mode optical microscope.

[0191] Macro-dispersion testing methods: The characteristics of macrodispersion were determined by optical microscopy in transmission mode. A 1 μm thick cryomicrotome section of a rubber sample was cut using a diamond knife in a PTPC PowerTome ultramicrotome instrument (RMC Boeckeler). The section was placed on a glass slide and measured at 0.55 mm. 2 Transmission optical imaging was performed at a resolution of 0.65 μm / pixel within the field of view. At least 10 optical images were acquired for each sample, each image taken from a different thin section of the same sample. The images were first processed by correcting the non-uniform background of the images using pseudo-flat-field correction based on Gaussian blur. Image noise was reduced using edge-preserving bidirectional filters, and image contrast enhancement was applied as needed. Dark and bright objects in the images represent non-dispersive particles and voids, respectively, while the gray image background represents areas of rubber due to well-dispersed carbon black. Objects were separated from the image by segmenting the image using a suitable whole or local thresholding method to create two binary images representing non-dispersive particles and voids, respectively. Image filtering and segmentation were optimized to ensure that the boundaries between voids and non-dispersive particles were clearly defined by visual comparison between the segmented image and the original image. The size distribution of non-dispersive particles was then analyzed from each binary image. The size of non-dispersive particles was determined using the area-equivalent diameter of the corresponding object in the binary image. The area-equivalent diameter is: area-equivalent diameter = (4 * Area of ​​the dark object / π) 1 / 2In this specification, the term "particle" refers to aggregated carbon black particles, not individual primary carbon black particles. Table 7 shows the area percentage (value "V") of undispersed carbon black particles larger than 10 μm. [Table 7]

[0192] In investigating the macrodispersion characteristics, Sample C1, a comparative liquid masterbatch sample, exhibited greater macrodispersion compared to Sample E1 of the present invention, as indicated by a smaller number of undispersed large particles. The tire tread of the present invention had more undispersed large filler particles than the C1 liquid masterbatch sample, but exhibited better dispersion and fewer undispersed large filler particles than all of the comparative samples of commercially available treads. Despite demonstrating slightly less beneficial macrodispersion characteristics compared to Sample C1, which was prepared by a process known to deliver excellent carbon black macrodispersion and associated excellent rubber material properties to tire treads, Sample E1 of the present invention unexpectedly exhibited rubber properties comparable to those of Sample C1, as shown by the data in Table 6.

[0193] In line with the superior macro-dispersion characteristics of Sample E1 of the present invention compared to comparable commercially available tire treads, the rubber material properties of Sample E1 are superior to those of comparable commercially available tread compounds.

[0194] Example 5 Tread compound made from a blend of elastomers and fillers. Preparation of a wet mixed complex In this example, Sample E3, a wet-mixed composite, was prepared using a blend of two elastomers (RSS1 natural rubber from RCMA Group, Singapore and Buna® CB22 butadiene rubber from Lanxess, Germany, at an NR / BR ratio of 80 / 20 phr) and two fillers (PROPEL® X25 carbon black from Cabot Corporation and ZEOSIL® Z1165 MP precipitated silica from Solvay USA Inc., Cranbury, NJ). Two wet-mixed composites (Part A and Part B) were prepared to create the E3 sample compound. Undried carbon black pellets with a moisture content of 55-58% by weight of total wet carbon black were mixed with natural rubber to prepare the Part A formulation described in Table 8A. To prepare the formulation of Part B described in Table 8A, Z1165 MP silica (5-7% moisture) was placed in a 5-gallon container, and water (reverse osmosis treated) was slowly added while mixing at a variable speed using a Warner Paint stirrer attached to an Ika laboratory mixer until the water and silica became a homogeneous system forming a wet paste. After sealing the container of wet silica for 24 hours, it was added to the other components of Part B, including the silane (Si69) coupling agent, during the preparation of the wet mixed composite of Part B. [Table 8A]

[0195] Wet-mixed composite sections A and B were prepared using a BR-1600 Banbury® laboratory mixer ("BR1600" mixer; Farrel Corporation, Ansonia, CT). The BR1600 mixer was operated by two 2-blade tangential rotors (2WL) to provide a volume of 1.6 L. The process used to prepare the two wet-mixed composite sections is shown in Table 8B. [Table 8B]

[0196] Compound Preparation The formulations used for the E3 sample compounds are set forth in Table 9. The components used included standard rubber grades of antioxidant 6PPD [N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine] (also used in Part A and Part B) and TMQ, zinc oxide, stearic acid, wax beads, sulfur, and TBBS accelerator, all obtained from Akrochem, Akron, Ohio. The solid dry natural rubber had a moisture content of <1 wt%.

[0197] The E3 sample compounds were mixed using a tangential mixer (Carter 55L tangential mixer with orbiting rotors from Carter, Manchester, UK). The mixing process was carried out as described in Table 10.

[0198] Tires with treads comprising the E3 sample compounds were prepared as described in Examples 1 to 3. [Table 9] [Table 10] [Table 11]

[0199] As can be observed from the macro-dispersion data in Table 7 for the E3 sample treads of the present invention, the tire treads of the present invention comprising a blend of elastomers and silica and carbon black fillers exhibit higher quality filler dispersion, demonstrating unique product characteristics, as compared to comparable commercial tire treads. The data set forth in Table 11 shows that the rubber properties of such tire treads comprising a blend of elastomers and a blend of carbon black and silica fillers were superior to those of a broad range of 13 comparable commercial truck tire treads.

[0200] The applicants refer specifically to the entire contents of all listed references in this disclosure. Furthermore, where a quantity, concentration, or other value or parameter is given as a range, a preferred range, or a list of preferred upper and lower limits, this should be understood to specifically disclose all ranges formed from any pair of any upper or preferred value and any lower or preferred value, regardless of whether the range is disclosed separately. Where numerical ranges are listed herein, unless otherwise stated, the range is intended to include its endpoint, as well as all integers and fractions within that range. The scope of the present invention is not intended to be limited to the specific values ​​listed when defining a range.

[0201] Other embodiments of the present invention will be apparent to those skilled in the art from consideration of this specification and practice of the present invention disclosed herein. This specification and examples are intended to be used only as examples to illustrate the true scope and spirit of the present invention by its claims and equivalents below. The present invention includes the following embodiments. (1) A tire tread comprising at least one elastomer and at least one filler in an amount of 40 to 80 phr, wherein the filler comprises at least 40 phr of at least one carbon black, and the tire tread comprises: a. Modulus ratio > 5.60; b. Percentage elongation at break > 470, and c. Loss tangent ≥ 0.10 and < 0.25 at 60℃ (333.15K) The tire tread having the above-mentioned features. (2) The tire tread according to (1), wherein the values ​​of the modulus ratio, the percentage elongation at break, and the loss tangent are based on the tire tread having the carbon black at 50 phr. (3) The tire tread according to (1), wherein the modulus of elasticity ratio is 5.60 to 6.30. (4) The tire tread according to (1), wherein the elastic modulus ratio is 5.70 to 6.30. (5) The tire tread according to (1), wherein the percentage elongation at break is 475 to 550. (6) The tire tread according to (1), wherein the percentage elongation at break is 480 to 525. (7) The tire tread according to (1), wherein the percentage elongation at break is 480 to 500. (8) The tire tread described in (1), wherein the loss tangent is 0.10 to 0.22. (9) The tire tread according to (1), wherein the loss tangent is 0.12 to 0.20. (10) The tire tread according to (1), wherein the elastomer comprises a blend of elastomers selected from natural rubber, functionalized natural rubber, styrene-butadiene rubber, functionalized styrene-butadiene rubber, polybutadiene rubber, functionalized polybutadiene rubber, and blends thereof. (11) A tire tread comprising at least one elastomer and at least one filler in an amount of 20 to 80 phr, wherein the filler comprises at least one carbon black in an amount of 40 phr or less, and the tread is: a) Modulus ratio ≥ 5.43; b) Percent elongation at break > 400, and c) Loss tangent >0.09 and <0.15 at 60℃ (333.15K) The tire tread having the above-mentioned features. (12) The tire tread according to (11), wherein the values ​​of the modulus ratio, the percentage elongation at break, and the loss tangent are based on the tire tread having the carbon black at 40 phr. (13) The tire tread according to (11), wherein the elastic modulus ratio is 5.43 to 6.25. (14) The tire tread according to (11), wherein the elastic modulus ratio is 5.43 to 6.20. (15) The tire tread according to (11), wherein the percent elongation at break is 405 to 550. (16) The tire tread according to (11), wherein the percent elongation at break is 425 to 525. (17) The tire tread according to (11), wherein the percent elongation at break is 425 to 500. (18) The tire tread according to (11), wherein the loss tangent is 0.095 to 0.14. (19) The tire tread according to (11), wherein the loss tangent is 0.10 to 0.12. (20) The tire tread according to any one of (1) to (19), characterized by a macro dispersion value V, which is the area percentage of undispersed carbon black particles larger than 10 μm, determined by an optical microscope in transmission mode according to the formula: 0.01<V<0.15. (21) A tire tread comprising at least one elastomer and 20 to 80 phr of at least one filler, wherein the filler comprises at least one carbon black, and the tread is characterized by a macro dispersion value V, which is the area percentage of undispersed carbon black particles larger than 10 μm, determined by an optical microscope in transmission mode according to the formula 0.01<V<0.15. (22) The tire tread according to (21), wherein V is based on the tire tread having the carbon black at 50 phr. (23) A tire tread comprising at least one elastomer and 20 to 80 phr of at least one filler, wherein the filler comprises at least one carbon black in an amount of 40 phr or less, the tread is characterized in that a macro dispersion value V, which is the area percentage of undispersed carbon black particles larger than 10 μm determined by an optical microscope in transmission mode, is greater than 0.01, and the tread has: a) an elastic modulus ratio ≧5.43; or b) a percent elongation at break >400, or c) a loss tangent at 60°C (333.15 K) <0.25 at least one of the above, the tire tread. (24) The tire tread according to (23), wherein the values ​​of the modulus ratio, the percentage elongation at break, and the loss tangent are based on the tire tread having the carbon black at 40 phr. (25) The tire tread according to (23), wherein the modulus ratio of elasticity is 5.43 to 6.25. (26) The tire tread according to (23), wherein the modulus ratio of elasticity is 5.43 to 6.2. (27) The tire tread according to (23), wherein the percentage elongation at break is 405 to 550. (28) The tire tread according to (23), wherein the percentage elongation at break is 425 to 525. (29) The tire tread according to (23), wherein the percentage elongation at break is 425 to 500. (30) The tire tread according to (23), wherein the loss tangent is 0.09 to 0.22. (31) The tire tread according to (23), wherein the loss tangent is 0.10 to 0.20. (32) A tire tread according to any one of (1) to (31), wherein the filler comprises at least one material selected from carbonaceous materials, carbon black, silica, nanocellulose, lignin, clay, nanoclay, metal oxides, metal carbonates, pyrolysis carbon, graphene, graphene oxide, reduced graphene oxide, carbon nanotubes, single-walled carbon nanotubes, multi-walled carbon nanotubes, or combinations thereof, and coated and treated materials thereof. (33) The tire tread according to any one of (1) to (31), wherein the filler comprises at least one material selected from carbon black, silica, and coated and treated materials thereof. (34) The tire tread according to any one of (1) to (31), wherein the filler contains carbon black and silica in a weight ratio of carbon black to silica greater than 2.7:1. (35) A tire tread according to any one of (1) to (31), wherein the elastomer is selected from natural rubber, functionalized natural rubber, styrene-butadiene rubber, functionalized styrene-butadiene rubber, polybutadiene rubber, functionalized polybutadiene rubber, polyisoprene rubber, ethylene-propylene rubber, isobutylene-based elastomer, polychloroprene rubber, nitrile rubber, hydrogenated nitrile rubber, polysulfide rubber, polyacrylate elastomer, fluoroelastomer, perfluoroelastomer, silicone elastomer, and blends thereof. (36) The tire tread according to any one of (1) to (31), wherein the elastomer is styrene-butadiene rubber, functionalized styrene-butadiene rubber, polybutadiene rubber, polyisoprene rubber, ethylene-propylene rubber, nitrile rubber, hydrogenated nitrile rubber, or a blend thereof. (37) The tire tread according to any one of items (1) to (31), wherein the elastomer is natural rubber, functionalized natural rubber, or both. (38) The tire tread according to (37), wherein the filler is selected from carbon black, silica, and coated and treated materials thereof. (39) The tire tread according to any one of (1) to (38), further comprising one or more rubber chemicals selected from deterioration inhibitors, processing aids and activators, zinc oxide, fatty acids, zinc salts of fatty acids, waxes, accelerators, resins, and processing oils. (40) The carbon black is STSA > 140m 2 A tire tread according to any one of items (1) to (39), having a value of / g. (41) The carbon black is STSA > 150m 2 A tire tread according to any one of items (1) to (39), having a value of / g. (42) The carbon black is 120m 2 / g~180m 2 A tire tread as described in any one of items (1) to (39), having an STSA of / g. (43) The carbon black is 150m 2 / g~160m 2 A tire tread as described in any one of items (1) to (39), having an STSA of / g. (44) A tire tread comprising at least one elastomer and at least one filler in an amount of 20 to 80 phr, wherein the filler comprises at least 40 phr of at least one carbon black, and the tire tread is: a) Modulus ratio > 5.60; b) Percentage elongation at break > 480, and optionally, c) Loss tangent <0.25 at 60℃ (333.15K) The tire tread having the following characteristics: the tread has a macrodispersion value V greater than 0.01, which is the area percentage of undispersed carbon black particles larger than 10 μm, as determined by an optical microscope in transmission mode. (45) The tire tread according to (44), wherein V is greater than 0.02. (46) The tire tread according to (44) or (45), having the loss tangent, wherein the loss tangent at 60°C (333.15K) is ≤0.20. (47) A tire having a tire tread as described in any one of the items (1) to (46). (48) Tires as described in (47), selected from tires for trucks, tractors, trailers, buses, passenger cars, high-performance vehicles, motorcycles, vehicles used off-road, construction machinery vehicles, and aircraft. (49) The tire is a tire for a vehicle used on a road other than a road or for a construction machinery vehicle, and the tread is made of an elastomer of 60 to 100 phr containing at least one type of natural or synthetic polyisoprene, and at least 130 m 2 The tire according to (47), comprising at least 40 phr of filler, which includes at least one type of carbon black having a BET of 115 ml / g or less and a COAN of 115 ml / g or less. (50) The tire according to (49), wherein the tire is a tire for a vehicle used on a road other than a road or for a construction machinery vehicle, and the tread further comprises at least one styrene-butadiene copolymer or butadiene polymer, or a combination thereof. (51) The tire is a tire for a vehicle used on a road other than a road or for a construction machinery vehicle, and the tread is made of an elastomer of 60 to 100 phr containing at least one type of natural or synthetic polyisoprene, and at least 130 m 2 The tire according to (47), comprising at least one carbon black having a BET of 115 ml / g or less and a COAN of 115 ml / g or less, and at least 40 phr of filler containing at least one silica of 5 to 10 phr. (52) The tire is a tire for a vehicle used on a road other than a road or for a construction machinery vehicle, and the tread is 150m 2 The tire according to (49), further comprising at least one type of carbon black having a BET greater than / g, an OAN of less than 100 ml / g, and a COAN of less than 90 ml / g. (53) The tire is a tire for a high-performance car or motorcycle, and the tread is an elastomer of 100 phr containing at least one polymer selected from solution styrene-butadiene copolymer and butadiene polymer and combinations thereof, and 150-220 m 2 At least one type of carbon black having STSA of / g and 150-200m 2 The tire according to (47), comprising at least 40 phr of filler containing at least one silica having a BET of / g. (54) The tire is a truck or bus tire, and the tread is made of at least one natural or synthetic polyisoprene elastomer of 60 to 100 phr, and at least 115 m 2 The tire according to (47), comprising at least 30 phr of filler containing at least one carbon black having STSA of 1 / g and COAN of less than 110 ml / g, and at least one silica filler of 1 to 25 phr. (55) The tire is a truck or bus tire, and the tread is made of at least one natural or synthetic polyisoprene elastomer of 60 to 100 phr, and at least 115 m 2 The tire according to (54), comprising 45 to 60 phr of filler containing at least one carbon black having STSA at 1 / g and COAN at less than 110 ml / g, and at least one silica filler at 1 to 25 phr. (56) The tire is a truck or bus tire, and the tread is made of at least one natural or synthetic polyisoprene elastomer of 60 to 100 phr, and 150 m 2 The tire according to (54), comprising at least 30 phr of filler containing at least one type of carbon black having a BET greater than / g, an OAN of less than 100 ml / g, and a COAN of less than 90 ml / g, and at least one type of silica filler of 1 to 25 phr. (57) The tire is a truck or bus tire, and the shoulder component of the tread is at least one natural or synthetic polyisoprene elastomer of 60 to 100 phr, and at least 120 m 2 The tire according to (47), comprising at least 40 phr of filler containing at least one carbon black having a BET of 1 / g and a COAN of less than 110 ml / g, and at least one silica filler of 1 to 20 phr. (58) The tire is a truck or bus tire, and the shoulder component of the tread is at least one natural or synthetic polyisoprene elastomer of 60 to 100 phr, and 150 m 2 The tire according to (57), comprising at least 40 phr of filler containing at least one type of carbon black having a BET greater than / g, an OAN of less than 100 ml / g, and a COAN of less than 90 ml / g, and at least one silica filler of 1 to 25 phr. (59) The lower layer of the tread is at least one natural or synthetic polyisoprene elastomer, polybutadiene elastomer, or a combination thereof in a quantity of 60 to 100 phr, and 100 m 2 BET less than / g and I less than 110g / kg 2 The tire according to (47), comprising at least 40 phr of filler containing at least one carbon black having a value. (60) The tire according to (47), wherein the tread comprises at least 20 phr of filler containing at least one carbon black selected from surface-modified carbon black, oxidized carbon black, multiphase aggregated carbon black, and carbon black having a surface hydrogen content of at least 2000 ppm. (61) A vehicle that fits a road and includes a rubber tread mounted on the road, wherein the tread is a tire tread as described in any one of (1) to (46).

Claims

1. A tire tread comprising at least one elastomer and at least one filler in an amount of 40 to 80 phr, wherein the filler comprises at least 40 phr of at least one carbon black, and the tire tread is: a. Tensile stress ratio (M300 / M100) > 5.60; b. Percent elongation at break > 470, and c. Loss tangent ≥ 0.10 and < 0.25 at 60°C (333.15K) It has, The aforementioned tire tread is characterized by a macrodispersion value V, which is the area percentage of undispersed carbon black particles larger than 10 μm, determined by optical microscopy in transmitted light mode using the formula: 0.01 < V < 0.

15. The aforementioned tire tread.

2. The tire tread according to claim 1, wherein the tensile stress ratio (M300 / M100) is greater than 5.60 and 6.30 or less.

3. The tire tread according to claim 1, wherein the percentage elongation at break is 475 to 550.

4. The tire tread according to claim 1, wherein the loss tangent is 0.10 to 0.

22.

5. A tire tread comprising at least one elastomer and at least one filler in an amount of 20 to 80 phr, wherein the filler does not contain at least one carbon black in an amount greater than 40 phr, and the tire tread is characterized by a macrodispersion value V, which is the area percentage of undispersed carbon black particles greater than 10 μm, as determined by optical microscopy in transmitted light mode, having the formula: 0.01 < V < 0.15, and the tire tread is: a) Tensile stress ratio (M300 / M100) ≥ 5.43; b) Percent elongation at break > 400, and c) Loss tangent > 0.09 and < 0.15 at 60°C (333.15K) The tire tread having the above-mentioned features.

6. A tire tread comprising at least one elastomer and at least one filler in an amount of 20 to 80 phr, wherein the filler does not contain at least one carbon black in an amount greater than 40 phr, and the tire tread is characterized by a macrodispersion value V, which is the area percentage of undispersed carbon black particles greater than 10 μm, as determined by optical microscopy in transmitted light mode, having the formula: 0.01 < V < 0.15, and the tire tread is: a) Tensile stress ratio (M300 / M100) ≥ 5.43; or b) Percentage elongation at break > 400, or c) Loss tangent < 0.25 at 60°C (333.15K) The tire tread having at least one of the following.

7. The tire tread according to any one of claims 1 to 6, wherein the filler comprises at least one material selected from carbonaceous materials, carbon black, silica, nanocellulose, lignin, clay, nanoclay, metal oxides, metal carbonates, pyrolysis carbon, graphene, graphene oxide, reduced graphene oxide, carbon nanotubes, single-walled carbon nanotubes, multi-walled carbon nanotubes, or combinations thereof, and coated and treated materials thereof.

8. The tire tread according to any one of claims 1 to 6, wherein the filler comprises at least one material selected from carbon black, silica, and coated and treated materials thereof.

9. The tire tread according to any one of claims 1 to 6, wherein the filler contains carbon black and silica in a weight ratio of carbon black to silica greater than 2.7:

1.

10. The tire tread according to any one of claims 1 to 6, wherein the elastomer is selected from natural rubber, functionalized natural rubber, styrene-butadiene rubber, functionalized styrene-butadiene rubber, polybutadiene rubber, functionalized polybutadiene rubber, polyisoprene rubber, ethylene-propylene rubber, isobutylene-based elastomer, polychloroprene rubber, nitrile rubber, hydrogenated nitrile rubber, polysulfide rubber, polyacrylate elastomer, fluoroelastomer, perfluoroelastomer, silicone elastomer, and blends thereof.

11. The tire tread according to any one of claims 1 to 6, wherein the elastomer is styrene-butadiene rubber, functionalized styrene-butadiene rubber, polybutadiene rubber, polyisoprene rubber, ethylene-propylene rubber, nitrile rubber, hydrogenated nitrile rubber, or a blend thereof.

12. The tire tread according to any one of claims 1 to 6, wherein the elastomer is natural rubber, functionalized natural rubber, or both.

13. The carbon black has an STSA of > 140m. 2 A tire tread according to any one of claims 1 to 12, having / g.

14. The carbon black is 120 m 2 / g to 180m 2 A tire tread according to any one of claims 1 to 12, having an STSA of / g.

15. A tire tread comprising at least one elastomer and at least one filler in an amount of 20 to 80 phr, wherein the filler comprises at least 40 phr of at least one carbon black, and the tire tread is characterized by a macrodispersion value V, which is the area percentage of undispersed carbon black particles larger than 10 μm, determined by optical microscopy in transmitted light mode, according to the formula: 0.01 < V < 0.15, wherein the tire tread is: a) Tensile stress ratio (M300 / M100) > 5.60; b) Percentage elongation at break > 480, and optionally, c) Loss tangent < 0.25 at 60°C (333.15K) The tire tread having the above-mentioned features.

16. The tire tread according to claim 15, having the loss tangent, wherein the loss tangent at 60°C (333.15K) is ≤0.

20.

17. A tire having the tire tread described in any one of claims 1 to 16.

18. The tire according to claim 17, selected from tires for trucks, tractors, trailers, buses, passenger cars, high-performance vehicles, motorcycles, vehicles used off-road, construction machinery vehicles, and aircraft.

Citation Information

Patent Citations

  • Elastomer composite compound and method of making same

    JP2001518401A

  • Rubber composition, its manufacturing process, and products made therefrom

    JP2010518229A

  • Elastomer composites, formulations, and methods for preparing the same.

    JP2016519196A