Secondary battery, electronic device and vehicle
Patent Information
- Application Number
- JP2022569310
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2020-12-16
- Filing Date
- 2021-12-02
- Publication Date
- 2024-12-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium-ion secondary batteries face challenges in achieving high capacity, excellent charge/discharge cycle characteristics, safety, and long-term reliability, particularly at high voltages and temperatures, due to issues with transition metal elution and crystal structure instability.
A lithium-ion secondary battery design incorporating a positive electrode active material with a layered rock salt crystal structure, optimized with additives like magnesium and fluorine, and a low-water electrolyte containing lithium salts and ionic liquids, which suppresses metal elution and maintains structural stability at high charging voltages and temperatures.
The battery exhibits improved capacity retention, safety, and long-term reliability, with enhanced energy density and stability, even under high voltage and temperature conditions, through the use of a stable crystal structure and controlled electrolyte composition.
Abstract
Description
Secondary battery, electronic device and vehicle
[0001] One embodiment of the present invention relates to an object, a method, or a manufacturing method. Alternatively, one embodiment of the present invention relates to a process, a machine, a manufacture, or a composition of matter. One embodiment of the present invention relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, or an electronic device, or a manufacturing method thereof. In particular, the present invention relates to a positive electrode active material that can be used in a secondary battery, a secondary battery, an electronic device having a secondary battery, and a vehicle having a secondary battery.
[0002] Another embodiment of the present invention relates to a power storage system including a secondary battery and a battery control circuit, or to an electronic device and a vehicle including the power storage system.
[0003] In this specification, the term "power storage device" refers to elements and devices in general that have a power storage function, including, for example, storage batteries (also called secondary batteries) such as lithium ion secondary batteries, lithium ion capacitors, and electric double layer capacitors.
[0004] In this specification, the term "electronic device" refers to any device having a power storage device, and includes electro-optical devices having a power storage device, information terminal devices having a power storage device, and the like.
[0005] In recent years, various types of power storage devices have been actively developed, such as lithium-ion secondary batteries, lithium-ion capacitors, and air batteries. In particular, demand for high-power, high-energy-density lithium-ion secondary batteries has rapidly expanded in conjunction with the development of the semiconductor industry, and they are now indispensable in the modern information society as a rechargeable energy source, as they are used in portable information terminals such as mobile phones, smartphones, tablets, and notebook computers, portable music players, digital cameras, medical devices, and next-generation clean energy vehicles (hybrid vehicles (HVs), electric vehicles (EVs), plug-in hybrid vehicles (PHVs), etc.).
[0006] The characteristics required of lithium ion secondary batteries include higher energy density, improved cycle characteristics, safety in various operating environments, and improved long-term reliability.
[0007] Therefore, improvements to the positive electrode active material have been investigated to improve the cycle characteristics and capacity of lithium-ion secondary batteries (Patent Documents 1 and 2). Research on the crystal structure of the positive electrode active material has also been conducted (Non-Patent Documents 1 to 3).
[0008] Non-Patent Document 4 describes the physical properties of metal fluorides.
[0009] X-ray diffraction (XRD) is one of the techniques used to analyze the crystalline structure of positive electrode active materials. XRD data can be analyzed using the Inorganic Crystal Structure Database (ICSD) introduced in Non-Patent Document 5.
[0010] JP 2002-216760 A JP 2006-261132 A
[0011] Toyoki Okumura et al,”Correlation of lithium ion distribution and X−ray absorption near−edge structure in O3−and O2−lithium cobalt oxides from first−principle calculation”,Journal of Materials Chemistry,2012,22,p.17340−17348Motohashi,T.et al,”Electronic phase diagram of the layered cobalt oxide system LixCoO▲2▼(0.0≦x≦1.0)”,Physical Review B,80(16);165114Zhaohui Chen et al,“Staging Phase Transitions in LixCoO▲2▼,”Journal of The Electrochemical Society,2002,149(12)A1604−A1609W.E.Counts et al,“Flouride Model Systems:II、The Binary Systems CaF▲2▼−BeF▲2▼,MgF▲2▼−BeF▲2▼,and LiF−MgF▲2▼,”Journal of the American Ceramic Society,(1953)36[1]12−17.Fig.01471Belsky,A.et al.,“New developments in the Inorganic Crystal Structure Database(ICSD):accessibility in support of materials research and design”,Acta Cryst.,(2002)B58 364−369
[0012] An object of one embodiment of the present invention is to provide a lithium ion secondary battery having high capacity and excellent charge / discharge cycle characteristics, and a manufacturing method thereof. Another object of one embodiment of the present invention is to provide a secondary battery capable of rapid charge and a manufacturing method thereof. Another object of one embodiment of the present invention is to provide a high-capacity secondary battery and a manufacturing method thereof. Another object of one embodiment of the present invention is to provide a secondary battery having excellent charge / discharge characteristics and a manufacturing method thereof. Another object of one embodiment of the present invention is to provide a secondary battery in which a decrease in capacity is suppressed even when the battery is maintained in a charged state at a high voltage for a long period of time, and a manufacturing method thereof. Another object of one embodiment of the present invention is to provide a safe or highly reliable secondary battery and a manufacturing method thereof. Another object of one embodiment of the present invention is to provide a secondary battery in which a decrease in capacity is suppressed even at high temperatures, and a manufacturing method thereof. Another object of one embodiment of the present invention is to provide a secondary battery having a long lifetime, and a manufacturing method thereof.
[0013] An object of one embodiment of the present invention is to provide an excellent secondary battery that can be rapidly charged, can be used at high temperatures, can have a high energy density by increasing the charging voltage, and is safe and has a long life.
[0014] An object of one embodiment of the present invention is to provide a positive electrode active material for a lithium ion secondary battery that has high capacity and excellent charge-discharge cycle characteristics, and a manufacturing method thereof. Another object is to provide a manufacturing method of the positive electrode active material with high productivity. Another object is to provide a positive electrode active material that, when used in a lithium ion secondary battery, suppresses a decrease in capacity during charge-discharge cycles. Another object is to provide a positive electrode active material that suppresses elution of a transition metal such as cobalt even when the battery is maintained in a charged state at a high voltage for a long period of time.
[0015] Another object of one embodiment of the present invention is to provide a novel substance, active material particles, a power storage device, or a manufacturing method thereof.
[0016] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these can be extracted from the description in the specification, drawings, and claims.
[0017] One embodiment of the present invention is a secondary battery that includes a positive electrode, a negative electrode, and an electrolyte, the electrolyte having a water content of less than 1000 ppm.
[0018] Another embodiment of the present invention is a secondary battery that includes a positive electrode, a negative electrode, and an electrolyte, in which the water content of the electrolyte is less than 1000 ppm, and the water content of the electrolyte is measured using a Karl Fischer moisture meter.
[0019] In the above configuration, the electrolyte preferably contains a lithium salt and a cyclic carbonate.
[0020] In the above configuration, the electrolyte preferably includes a lithium salt and an ionic liquid.
[0021] In the above configuration, it is preferable to have one or more cations selected from imidazolium cations, pyridinium cations, quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations, and one or more anions selected from monovalent amide anions, monovalent methide anions, fluorosulfonate anions, perfluoroalkylsulfonate anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, and perfluoroalkylphosphate anions.
[0022] Another embodiment of the present invention is an electronic device including any one of the above secondary batteries, a display portion, and a sensor.
[0023] Alternatively, one aspect of the present invention is a vehicle having any one of the secondary batteries described above, an electric motor, and a control device, wherein the control device has the function of supplying power from the secondary battery to the electric motor.
[0024] According to one embodiment of the present invention, a lithium-ion secondary battery having a high capacity and excellent charge-discharge cycle characteristics and a manufacturing method thereof can be provided. According to another embodiment of the present invention, a secondary battery capable of rapid charging and a manufacturing method thereof can be provided. Furthermore, a secondary battery in which a decrease in capacity is suppressed even when the battery is maintained in a high-voltage charged state for a long period of time and a manufacturing method thereof can be provided. According to another embodiment of the present invention, a safe or highly reliable secondary battery and a manufacturing method thereof can be provided. According to another embodiment of the present invention, a secondary battery in which a decrease in capacity is suppressed even at high temperatures and a manufacturing method thereof can be provided. According to another embodiment of the present invention, a secondary battery having a long life and a manufacturing method thereof can be provided.
[0025] According to one embodiment of the present invention, it is possible to provide an extremely excellent secondary battery that can be rapidly charged, can be used at high temperatures, can have a high energy density by increasing the charging voltage, and is safe and has a long life.
[0026] According to one embodiment of the present invention, a positive electrode active material for a lithium ion secondary battery having high capacity and excellent charge-discharge cycle characteristics, and a manufacturing method thereof can be provided. Furthermore, a manufacturing method of the positive electrode active material with high productivity can be provided. Furthermore, according to one embodiment of the present invention, a positive electrode active material that, when used in a lithium ion secondary battery, suppresses a decrease in capacity during charge-discharge cycles can be provided. Furthermore, according to one embodiment of the present invention, a positive electrode active material in which elution of a transition metal such as cobalt is suppressed even when the battery is maintained in a charged state at a high voltage for a long period of time can be provided.
[0027] Another embodiment of the present invention can provide a novel substance, active material particles, a power storage device, or a manufacturing method thereof.
[0028] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract other effects from the description in the specification, drawings, claims, etc.
[0029] FIG. 1 is a diagram illustrating the crystal structure of a positive electrode active material. FIG. 2 is a diagram illustrating the crystal structure of a positive electrode active material. FIG. 3 is a cross-sectional schematic diagram of a positive electrode active material particle. FIGS. 4A and 4B are diagrams illustrating an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention. FIGS. 5A to 5C are diagrams illustrating an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention. FIG. 6 is a diagram illustrating an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention. FIGS. 7A to 7C are diagrams illustrating an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention. FIGS. 8A, 8B, 8C, and 8D are cross-sectional schematic diagrams of negative electrode active material particles. FIGS. 9A, 9B, 9C, and 9D are cross-sectional views of an example of a secondary battery. FIGS. 10A and 10B are diagrams illustrating an external appearance of a secondary battery. FIGS. 11A and 11B are diagrams illustrating a method for manufacturing a secondary battery. FIGS. 12A and 12B are diagrams illustrating a method for manufacturing a secondary battery. FIG. 13 is a diagram illustrating an external appearance of a secondary battery. FIG. 14 is a top view showing an example of a manufacturing apparatus for a secondary battery. FIG. 15 is a cross-sectional view showing an example of a method for manufacturing a secondary battery. FIGS. 16A to 16C are perspective views showing an example of a method for manufacturing a secondary battery. FIG. 16D is a cross-sectional view corresponding to FIG. 16C. FIGS. 17A to 17F are perspective views showing an example of a method for manufacturing a secondary battery. FIG. 18 is a cross-sectional view showing an example of a secondary battery. FIG. 19A is a diagram showing an example of a secondary battery. FIGS. 19B and 19C are diagrams showing an example of a method for manufacturing a stack. FIGS. 20A to 20C are diagrams showing an example of a method for manufacturing a secondary battery. FIGS. 21A and 21B are cross-sectional views showing an example of a stack. FIG. 21C is a cross-sectional view showing an example of a secondary battery. FIGS. 22A and 22B are diagrams showing an example of a secondary battery. FIG. 22C is a diagram showing the interior of a secondary battery. FIGS. 23A to 23C are diagrams showing an example of a secondary battery. Fig. 24A is an exploded perspective view of a coin-type secondary battery, Fig. 24B is a perspective view of the coin-type secondary battery, and Fig. 24C is a cross-sectional perspective view thereof. Figs. 25A and 25B are examples of cylindrical secondary batteries, Fig. 25C is an example of multiple cylindrical secondary batteries, and Fig. 25D is an example of a power storage system having multiple cylindrical secondary batteries. Fig. 26A is a perspective view showing an example of a battery pack. Fig. 26B is a block diagram showing an example of a battery pack.FIG. 26C is a block diagram showing an example of a vehicle having a motor. FIGS. 27A to 27E are diagrams showing an example of a transportation vehicle. FIG. 28A is a diagram showing an electric bicycle, FIG. 28B is a diagram showing a secondary battery for the electric bicycle, and FIG. 28C is a diagram explaining an electric motorcycle. FIGS. 29A and 29B are diagrams showing an example of a power storage device. FIGS. 30A to 30E are diagrams explaining an example of an electronic device. FIGS. 31A to 31H are diagrams explaining an example of an electronic device. FIGS. 32A to 32C are diagrams explaining an example of an electronic device. FIG. 33 is a diagram explaining an example of an electronic device. FIGS. 34A to 34C are diagrams explaining an example of an electronic device. FIGS. 35A to 35C are diagrams showing an example of an electronic device. FIGS. 36A and 36B are diagrams showing an example of charge and discharge characteristics of a secondary battery. FIGS. 37A and 37B are diagrams showing an example of cycle characteristics of a secondary battery. FIG. 38 is a diagram showing an NMR spectrum. FIGS. 39A and 39B are diagrams showing NMR spectra.
[0030] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various modifications can be made to the embodiments and details. Furthermore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.
[0031] Furthermore, in this specification and the like, crystal planes and directions are indicated using Miller indices. In crystallography, crystal planes and directions are represented by a superscript bar after the number, but in this specification and the like, due to limitations on application notation, numbers may be represented by a minus sign (-) before them instead of a bar above them. Furthermore, individual orientations indicating directions within a crystal are represented by [ ], collective orientations indicating all equivalent directions are represented by < >, individual planes indicating crystal planes are represented by ( ), and collective planes with equivalent symmetry are represented by {}.
[0032] In this specification and the like, segregation refers to a phenomenon in which a certain element (for example, B) is spatially distributed non-uniformly in a solid composed of a plurality of elements (for example, A, B, C).
[0033] In this specification, the surface layer of particles of active material or the like refers to the region from the surface to a depth of about 10 nm. Surfaces formed by cracks or fissures may also be referred to as the surface. The region deeper than the surface layer is referred to as the interior.
[0034] In this specification, the layered rock-salt type crystal structure belonging to the space group R-3m, which is possessed by a composite oxide containing lithium and a transition metal such as cobalt, refers to a crystal structure having a rock-salt type ion arrangement in which cations and anions are alternately arranged, and in which the transition metal and lithium are regularly arranged to form a two-dimensional plane, allowing two-dimensional diffusion of lithium. Defects such as vacancies of cations or anions may also be present. Furthermore, strictly speaking, the layered rock-salt type crystal structure may have a structure in which the lattice of the rock-salt type crystal is distorted.
[0035] In this specification and the like, the term "rock salt type crystal structure" refers to a structure having a cubic crystal structure such as the space group Fm-3m, in which cations and anions are arranged alternately. Note that there may be a deficiency of cations or anions.
[0036] In this specification and the like, the O3'-type crystal structure of a composite oxide containing lithium and a transition metal is a space group R-3m, and ions of cobalt, magnesium, etc. occupy hexacoordinated oxygen positions. In the O3'-type crystal structure, light elements such as lithium may occupy tetracoordinated oxygen positions.
[0037] A secondary battery has, for example, a positive electrode and a negative electrode. A material constituting the positive electrode is a positive electrode active material. The positive electrode active material is, for example, a substance that undergoes a reaction that contributes to the charge / discharge capacity. Note that the positive electrode active material may partially contain a substance that does not contribute to the charge / discharge capacity.
[0038] In this specification and the like, the positive electrode active material of one embodiment of the present invention may be referred to as a positive electrode material, a positive electrode material for a secondary battery, or the like. Also, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a compound. Also, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a composition. Also, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a composite.
[0039] Embodiment 1 In this embodiment, an example of a secondary battery of one embodiment of the present invention will be described.
[0040] As will be described in the Examples below, it has been found that the characteristics of a secondary battery according to one embodiment of the present invention are extremely stable even when charged at a high voltage. In addition, the secondary battery according to one embodiment of the present invention can operate stably over a wide temperature range. The secondary battery according to one embodiment of the present invention can achieve a secondary battery with significantly excellent characteristics.
[0041] A positive electrode active material of one embodiment of the present invention is an oxide containing an element A and a metal M.
[0042] The element A can be at least one selected from alkali metals such as lithium, sodium, and potassium, and Group 2 elements such as calcium, beryllium, and magnesium. The element A is preferably an element that functions as a carrier metal.
[0043] For example, a transition metal can be used as the metal M. The positive electrode active material of one embodiment of the present invention includes, for example, one or more of cobalt, nickel, and manganese, particularly cobalt, as the metal M. Furthermore, the metal M may include an element such as aluminum that does not change valence and can have the same valence as the metal M, more specifically, for example, a trivalent typical element.
[0044] The positive electrode active material of one embodiment of the present invention is represented by the chemical formula AM y O Z (y>0, z>0). Lithium cobalt oxide is LiCoO 2 Lithium nickel oxide is sometimes expressed as LiNiO 2 It may be expressed as:
[0045] The positive electrode active material of one embodiment of the present invention preferably includes an additional element X. Examples of the additional element X include magnesium, calcium, zirconium, lanthanum, barium, titanium, and yttrium. Examples of the additional element X include nickel, aluminum, cobalt, manganese, vanadium, iron, chromium, and niobium. Examples of the additional element X include copper, potassium, sodium, zinc, chlorine, fluorine, hafnium, silicon, sulfur, phosphorus, boron, and arsenic. Two or more of the above elements may be used in combination as the additional element X.
[0046] For example, a part of the additional element X may be substituted at the position of the element A. Alternatively, for example, a part of the additional element X may be substituted at the position of the metal M.
[0047] The positive electrode active material of one embodiment of the present invention is represented by chemical formula A 1−w X w M y O Z (y>0, z>0, 0<w<1). y−j X j O Z (y>0, z>0, 0<j<y). 1−w X w M y−j X j O Z It may be expressed as (y>0, z>0, 0<w<1, 0<j<y).
[0048] The positive electrode active material of one embodiment of the present invention preferably contains a halogen in addition to the additional element X. The positive electrode active material of one embodiment of the present invention preferably contains a halogen such as fluorine or chlorine. When the positive electrode active material of one embodiment of the present invention contains the halogen, substitution of the additional element X at the position of the element A may be promoted.
[0049] As the charging voltage of a secondary battery increases, the crystal structure of the positive electrode active material becomes unstable, which can lead to a deterioration in the characteristics of the secondary battery. For example, a material having a layered crystal structure in which metal A is released from between the layers upon charging will be described. In such a positive electrode active material, the charge capacity and discharge capacity can be increased by increasing the charging voltage. On the other hand, as the charging voltage increases, a large amount of metal A may be released from the positive electrode active material, resulting in significant changes in the crystal structure, such as changes in the interlayer distance and layer misalignment. If the change in crystal structure accompanying the insertion and release of metal A is irreversible, the crystal structure may gradually collapse with repeated charging and discharging, resulting in a significant decrease in capacity with charge and discharge cycles.
[0050] Furthermore, increasing the charging voltage may cause the metal M contained in the positive electrode active material to easily leach into the electrolyte. When the metal M leach out of the positive electrode active material into the electrolyte, the amount of the metal M in the positive electrode active material decreases, which may lead to a decrease in the capacity of the positive electrode.
[0051] In the positive electrode active material of one embodiment of the present invention, the metal M is mainly bonded to oxygen. When oxygen is desorbed from the positive electrode active material, the metal M may be significantly eluted.
[0052] During charging, if the oxidation number of the metal M contained in the positive electrode active material increases, the reactivity of the positive electrode active material increases, and the positive electrode active material becomes highly reactive with impurities in the electrolyte. For example, oxygen is released from the positive electrode active material, and the electrolyte is oxidized. When oxygen is released, the metal M is more likely to be eluted.
[0053] Charging and discharging under high voltage conditions of 4.5 V or higher or at high temperatures (45°C or higher) can cause progressive defects (also called pits) in the positive electrode active material particles. Furthermore, defects such as fissures (also called cracks) can occur due to the expansion and contraction of the positive electrode active material particles during charging and discharging. Figure 3 shows a schematic cross-sectional view of a positive electrode active material particle 51. In the positive electrode active material particle 51, pits are shown as holes at 54 and 58, but the openings are not circular but have depth, and cracks are shown at 57. Reference numeral 55 denotes a crystal plane, 52 denotes a recess, and 53 and 56 denote barrier films.
[0054] Positive electrode active material particles may have defects, and these defects may change before and after charge and discharge. When used in a secondary battery, positive electrode active material particles may be chemically or electrochemically eroded by environmental substances (such as electrolytes) surrounding the positive electrode active material particles, or the material may deteriorate. This deterioration does not occur uniformly on the particle surface but occurs in a locally concentrated manner, and repeated charge and discharge of the secondary battery may cause deep defects, for example, from the surface to the interior.
[0055] The phenomenon in which defects progress to form holes in the positive electrode active material particles may be called pitting corrosion, and the holes formed by this phenomenon are also referred to as pits in this specification.
[0056] In this specification, cracks and pits are different. Immediately after the production of positive electrode active material particles, cracks may be present, but pits are not. For example, in lithium cobalt oxide, pits can be described as holes formed by the loss of several layers of cobalt and oxygen due to charging and discharging under high voltage conditions of 4.5 V or higher or at high temperatures (45°C or higher), and can also be described as locations where cobalt has dissolved. Cracks refer to new surfaces formed by the application of physical pressure, or fissures caused by grain boundaries. Cracks can also occur due to particle expansion and contraction caused by charging and discharging. Pits can also occur from cracks or cavities within particles.
[0057] When charging and discharging at high voltage or high temperature, cobalt dissolves from lithium cobalt oxide, and a crystalline phase different from lithium cobalt oxide may form in the surface layer. For example, Co with a spinel structure 3 O 4 , spinel structure LiCo 2 O 4 and CoO with a rock salt structure may be formed. These materials have a smaller discharge capacity than, for example, lithium cobalt oxide, or are materials that do not contribute to charge and discharge. Therefore, the formation of these materials in the surface layer may lead to a decrease in the discharge capacity of the secondary battery. Furthermore, this may lead to a decrease in the output characteristics and low-temperature characteristics of the secondary battery. Furthermore, these materials may be formed in the vicinity of pits.
[0058] Furthermore, metal M may be eluted from the positive electrode active material, and the electrolyte may transport ions of metal M, resulting in the deposition of metal M on the surface of the negative electrode. Furthermore, a coating may be formed on the surface of the negative electrode from decomposition products of metal M and the electrolyte. The formation of this coating may make it difficult for carrier ions to be inserted into and removed from the negative electrode active material, which may result in a deterioration in the rate characteristics, low-temperature characteristics, etc. of the secondary battery.
[0059] The positive electrode active material of one embodiment of the present invention can have an O3' structure described later during charging, and thus can be charged to a deep charge depth. By increasing the charge depth, the capacity of the positive electrode can be increased, thereby increasing the energy density of the secondary battery. Furthermore, repeated charge and discharge can be performed even when an extremely high charge voltage is used.
[0060] Furthermore, the positive electrode active material of one embodiment of the present invention can be made extremely pure by minimizing the amount of impurities mixed in raw materials and during the manufacturing process. Increasing the purity of the positive electrode active material can sometimes further improve the structural stability of the positive electrode active material at high charging voltages.
[0061] However, when charging is performed at a higher charging voltage, the oxidation number of the metal M becomes higher. In such a state, as described above, the metal M is more likely to dissolve.
[0062] In the secondary battery of one embodiment of the present invention, the charging voltage is extremely high, which makes it easy for the metal M to dissolve, but the dissolution of the metal M can be suppressed by reducing impurities in the electrolyte in some cases. Thus, both a high charging voltage and suppression of the dissolution of the metal M can be achieved.
[0063] An example of an impurity in the electrolyte is water.
[0064] Here, the surface layer is preferably a region within 50 nm from the surface, more preferably within 35 nm, and even more preferably within 20 nm. The region deeper than the surface layer is referred to as the interior.
[0065] A positive electrode active material of one embodiment of the present invention includes an additive element X. In the positive electrode active material of one embodiment of the present invention, the additive element X preferably has a concentration gradient. The additive element X preferably has a concentration gradient that increases from the inside toward the surface. The concentration gradient of the additive element X can be evaluated using, for example, energy dispersive X-ray spectroscopy (EDX).
[0066] For example, when irreversible changes occur in the crystalline structure of the material constituting the positive electrode active material due to charging at high temperatures, deterioration of the secondary battery occurs significantly. For example, a significant decrease in capacity with repeated charge / discharge cycles may occur. When the temperature is high and the charging voltage is also high, the crystalline structure of the positive electrode may become even more unstable.
[0067] In the secondary battery of one embodiment of the present invention, by using a positive electrode active material whose crystal structure is extremely stable at high charging voltages and high temperatures, excellent characteristics can be achieved even at high temperatures and high charging voltages, and the effect of an electrolyte with an extremely reduced water content can be fully exerted. In other words, the remarkable improvement in characteristics obtained by using the configuration of the secondary battery of one embodiment of the present invention is found by combining it with the positive electrode active material of one embodiment of the present invention.
[0068] As will be described later, the positive electrode active material of one embodiment of the present invention preferably contains an additional element X, and preferably contains a halogen in addition to the additional element X. When the positive electrode active material of one embodiment of the present invention contains the additional element X or a halogen in addition to the additional element X, it is suggested that a reaction between the surface of the positive electrode active material and an electrolyte is suppressed.
[0069] Furthermore, the secondary battery of one embodiment of the present invention has an extremely wide range of reaction potentials. In such a wide reaction potential, there is a concern that the surface of the active material may react with impurities in the electrolyte. By using the electrolyte of one embodiment of the present invention, it is possible to suppress the reaction between the electrolyte and the surface of the active material, thereby realizing a more stable secondary battery.
[0070] The secondary battery of one embodiment of the present invention is preferably used in combination with a battery control circuit. The battery control circuit preferably has, for example, a function of controlling charging. Controlling charging refers to, for example, monitoring parameters of the secondary battery and changing charging conditions according to the state. Examples of the monitored parameters of the secondary battery include the voltage, current, temperature, charge amount, and impedance of the secondary battery.
[0071] The secondary battery according to one embodiment of the present invention is preferably used in combination with a sensor, which preferably has a function of measuring one or more of displacement, position, velocity, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substance, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor, and infrared light.
[0072] In addition, it is preferable that the charging of the secondary battery of one embodiment of the present invention be controlled in accordance with a value measured by a sensor. An example of controlling the secondary battery using a temperature sensor will be described later.
[0073] [Positive Electrode Active Material] Hereinafter, a positive electrode active material that is preferably used in the secondary battery of one embodiment of the present invention will be described.
[0074] <Structure of Positive Electrode Active Material> The positive electrode active material preferably contains a metal (hereinafter referred to as element A) that serves as a carrier ion. Examples of element A that can be used include alkali metals such as lithium, sodium, and potassium, and Group 2 elements such as calcium, beryllium, and magnesium.
[0075] In a positive electrode active material, carrier ions are desorbed from the positive electrode active material during charging. The greater the desorption of element A, the greater the number of ions that contribute to the capacity of the secondary battery, resulting in an increased capacity. On the other hand, the greater the desorption of element A, the more likely the crystalline structure of the compound contained in the positive electrode active material is to be deformed. The destructive collapse of the crystalline structure of the positive electrode active material may result in a decrease in discharge capacity with charge-discharge cycles. When the positive electrode active material of one embodiment of the present invention contains an additive element X, the destructive collapse of the crystalline structure when carrier ions are desorbed during charging of the secondary battery may be suppressed. For example, a portion of the additive element X is substituted at the position of element A. Elements such as magnesium, calcium, zirconium, lanthanum, and barium can be used as the additive element X. Elements such as copper, potassium, sodium, zinc, titanium, yttrium, nickel, aluminum, cobalt, manganese, vanadium, iron, chromium, niobium, and hafnium can also be used as the additive element X. Elements such as silicon, sulfur, phosphorus, boron, and arsenic can also be used as the additive element X. Further, as the additional element X, two or more of the elements listed above may be used in combination.
[0076] The positive electrode active material of one embodiment of the present invention preferably contains a halogen in addition to the additional element X. The positive electrode active material of one embodiment of the present invention preferably contains a halogen such as fluorine or chlorine. When the positive electrode active material of one embodiment of the present invention contains the halogen, substitution of the additional element X at the position of the element A may be promoted.
[0077] When the positive electrode active material of one embodiment of the present invention contains an additional element X or contains a halogen in addition to the additional element X, the electrical conductivity on the surface of the positive electrode active material might be suppressed in some cases.
[0078] Furthermore, a positive electrode active material according to one embodiment of the present invention includes a metal (hereinafter, metal M) whose valence changes upon charging and discharging of a secondary battery. The metal M is, for example, a transition metal. The positive electrode active material according to one embodiment of the present invention includes, for example, one or more of cobalt, nickel, and manganese as the metal M, and particularly includes cobalt. Furthermore, an element that does not change valence and can have the same valence as the metal M, such as aluminum, may be present at the position of the metal M, more specifically, a trivalent typical element, for example. The aforementioned additional element X may be substituted at the position of the metal M, for example. Furthermore, when the positive electrode active material according to one embodiment of the present invention is an oxide, the additional element X may be substituted at the position of oxygen.
[0079] As the positive electrode active material of one embodiment of the present invention, for example, a lithium composite oxide having a layered rock salt crystal structure is preferably used. More specifically, examples of the lithium composite oxide having a layered rock salt crystal structure include lithium cobalt oxide, lithium nickel oxide, a lithium composite oxide containing nickel, manganese, and cobalt, and a lithium composite oxide containing nickel, cobalt, and aluminum. These positive electrode active materials are preferably represented by the space group R-3m.
[0080] In a positive electrode active material having a layered rock-salt crystal structure, increasing the depth of charge can cause the crystal structure to collapse. Here, the collapse of the crystal structure refers to, for example, layer misalignment. If the collapse of the crystal structure is irreversible, repeated charging and discharging can cause a decrease in the capacity of the secondary battery.
[0081] The positive electrode active material of one embodiment of the present invention contains the additive element X, which suppresses the above-described layer misalignment, even at a deep charge depth. Suppressing the misalignment can reduce volume change during charge and discharge. Therefore, the positive electrode active material of one embodiment of the present invention can achieve excellent cycle characteristics. Furthermore, the positive electrode active material of one embodiment of the present invention can have a stable crystal structure in a high-voltage charged state. Therefore, the positive electrode active material of one embodiment of the present invention may be less susceptible to short circuits when maintained in a high-voltage charged state. In such cases, safety is further improved, which is preferable.
[0082] In the positive electrode active material of one embodiment of the present invention, the change in crystal structure and the difference in volume per the same number of transition metal atoms between a fully discharged state and a high-voltage charged state are small.
[0083] The positive electrode active material of one embodiment of the present invention has the chemical formula AM y O Z (y>0, z>0). For example, lithium cobalt oxide is LiCoO 2 For example, lithium nickel oxide can be expressed as LiNiO 2 It may be expressed as:
[0084] Lithium cobalt oxide (LiCoO 2 Materials having a layered rock salt type crystal structure, such as LiMO, are known to have a high discharge capacity and are excellent as positive electrode active materials for secondary batteries. 2 Examples of the composite oxide include a composite oxide represented by the formula: The metal M includes a first metal. The first metal is one or more metals including cobalt. Furthermore, the metal M may include a second metal in addition to the first metal. As the second metal, an element selected from the elements exemplified as the additional element X can be used. For example, the second metal is one or more metals selected from magnesium, calcium, zirconium, lanthanum, barium, copper, potassium, sodium, and zinc.
[0085] It is known that the strength of the Jahn-Teller effect in transition metal compounds varies depending on the number of electrons in the d orbital of the transition metal.
[0086] In compounds containing nickel, distortion may easily occur due to the Jahn-Teller effect. 2 When LiCoO is charged and discharged at a high voltage, there is a concern that the crystal structure may be destroyed due to distortion. 2 It is suggested that the influence of the Jahn-Teller effect is small in this case, and the durability of charge and discharge at high voltages may be superior, which is preferable.
[0087] Here, LiMO 2The composition of the lithium composite oxide represented by the formula is not limited to Li:M:O=1:1:2. 2 Examples of the lithium composite oxide represented by the formula (I) include lithium cobalt oxide, lithium nickel-cobalt-manganese oxide, lithium nickel-cobalt-aluminate, and lithium nickel-cobalt-manganese-aluminate.
[0088] When cobalt is used as the element M in an amount of 75 atomic % or more, preferably 90 atomic % or more, and more preferably 95 atomic % or more, it has many advantages such as being relatively easy to synthesize and handle, and having excellent cycle characteristics.
[0089] On the other hand, when nickel is used as the element M in an amount of 33 atomic % or more, preferably 60 atomic % or more, and more preferably 80 atomic % or more, the raw material may be cheaper than when cobalt is used in large amounts, and the charge / discharge capacity per weight may increase, which is preferable.
[0090] Furthermore, the particle size may become small when nickel is used in an amount of 33 atomic % or more, preferably 60 atomic % or more, and more preferably 80 atomic % or more as the element M. Therefore, for example, it is preferable that the third particles described above contain nickel in an amount of 33 atomic % or more, preferably 60 atomic % or more, and more preferably 80 atomic % or more as the element M.
[0091] Furthermore, when nickel is present in part along with cobalt as element M, it may suppress the deviation of the layered structure consisting of octahedra of cobalt and oxygen. This is preferable because the crystal structure may become more stable, particularly in the charged state at high temperatures. This is because nickel easily diffuses deep into the lithium cobalt oxide, and while it is present on the cobalt site during discharge, it is thought to be able to be located on the lithium site through cation mixing during charge. The nickel present on the lithium site during charge is thought to function as a pillar supporting the layered structure consisting of octahedra of cobalt and oxygen, contributing to the stabilization of the crystal structure.
[0092] The element M does not necessarily have to contain manganese, nickel, or cobalt.
[0093] During charging, lithium is released from the surface of the particles, so the lithium concentration in the surface layer of the particles tends to be lower than in the interior, and the crystalline structure tends to collapse.
[0094] The particles of one embodiment of the present invention contain lithium, an element M, and oxygen. 2 The particle of one embodiment of the present invention includes a lithium composite oxide represented by the formula (where M is one or more metals including cobalt). Furthermore, the particle of one embodiment of the present invention has one or more elements selected from magnesium, fluorine, aluminum, and nickel in the surface layer portion. By having one or more of these elements in the surface layer portion of the particle of one embodiment of the present invention, structural changes accompanying charge and discharge can be reduced in the surface layer portion of the particle, and crack formation can be suppressed. Furthermore, irreversible structural changes in the surface layer portion of the particle can be suppressed, and capacity loss accompanying repeated charge and discharge can be suppressed. Furthermore, the concentration of these elements in the surface layer portion is preferably higher than the concentration of these elements in the entire particle. Furthermore, the particle of one embodiment of the present invention may have a structure in the surface layer portion in which, for example, some of the atoms in the lithium composite oxide are substituted with one or more elements selected from magnesium, fluorine, aluminum, and nickel.
[0095] In a positive electrode active material according to one embodiment of the present invention, which contains an additive element X, when the depth of charge is 0.8 or more, the material is represented by the space group R-3m, and although it is not a spinel-type crystal structure, ions of a metal M (e.g., cobalt), an additive element X (e.g., magnesium), or the like may occupy oxygen hexacoordination positions. This structure is referred to as an O3'-type crystal structure in this specification. Note that in the O3'-type crystal structure, light elements such as lithium may occupy oxygen tetracoordination positions.
[0096] The structure of the positive electrode active material becomes unstable due to the detachment of carrier ions during charging. It can be said that the O3'-type crystal structure is a structure that can maintain high stability even when carrier ions are detached.
[0097] The O3' type crystal structure has randomly interlayered Li atoms, but the CdCl 2 It can be said that this crystal structure is similar to that of the CdCl type. 2A crystal structure similar to the type was observed when lithium nickel oxide was charged to a charge depth of 0.94 (Li 0.06 NiO 2 ), but it is known that pure lithium cobaltate or layered rock salt-type positive electrode active materials containing a large amount of cobalt do not usually adopt this crystal structure.
[0098] The anions in the layered rock salt crystal and the rock salt crystal have a cubic close-packed structure (face-centered cubic lattice structure). It is estimated that the anions in the O3'-type crystal also have a cubic close-packed structure. Therefore, when the layered rock salt crystal and the rock salt crystal come into contact, there is a crystal plane where the orientation of the cubic close-packed structure formed by the anions is aligned. However, since the space group of the layered rock salt crystal and the O3'-type crystal is R-3m, which is different from the space group Fm-3m (the space group of a general rock salt crystal) of the rock salt crystal, the Miller indices of the crystal planes that satisfy the above conditions are different between the layered rock salt crystal and the O3'-type crystal and the rock salt crystal. In this specification, when the orientation of the cubic close-packed structure formed by the anions is aligned in the layered rock salt crystal, the O3'-type crystal, and the rock salt crystal, it may be said that the crystal orientations are approximately the same.
[0099] The crystal structure at a charge depth of 0 (discharged state) in Fig. 1 is the same as that in Fig. 2, R-3m(O3). On the other hand, the positive electrode active material of one embodiment of the present invention shown in Fig. 1 has a crystal structure different from the H1-3 type crystal structure (space group R-3m) shown in Fig. 2 when it is fully charged. This structure is in the space group R-3m, and ions such as cobalt and magnesium ions occupy the oxygen hexacoordination positions. In addition, the CoO in this structure 2 The symmetry of the layers is the same as that of the O3 type. Therefore, this structure is referred to as the O3' type crystal structure in this specification. In the diagram of the O3' type crystal structure shown in Figure 1, lithium can exist at any lithium site with a probability of about 20%, but this is not limited to this. It may exist only at a specific part of the lithium sites. In both the O3 type crystal structure and the O3' type crystal structure, CoO 2 It is preferable that magnesium is present in a dilute form between the layers, i.e., at the lithium sites, and it is also preferable that halogen such as fluorine is present randomly and dilutely at the oxygen sites.
[0100] In the O3' type crystal structure, a light element such as lithium may occupy the oxygen tetracoordination position.
[0101] In the positive electrode active material of one embodiment of the present invention, the change in the crystal structure when a large amount of lithium is released by charging at a high voltage is suppressed compared to the structure described later with reference to FIG. 2. For example, as shown by the dotted line in FIG. 1, in these crystal structures, CoO 2 There is almost no layer misalignment.
[0102] More specifically, the positive electrode active material of one embodiment of the present invention has high structural stability even at a high charge voltage. For example, in FIG. 2, the H1-3 crystal structure is formed at a voltage of about 4.6 V relative to the potential of lithium metal. However, the positive electrode active material shown in FIG. 1 can maintain the R-3m(O3) crystal structure even at a charge voltage of about 4.6 V. Even at a higher charge voltage, for example, a voltage of about 4.65 V to 4.7 V relative to the potential of lithium metal, the positive electrode active material shown in FIG. 1 can also have an O3' crystal structure. When the charge voltage is further increased above 4.7 V, the H1-3 crystal may be observed in the positive electrode active material shown in FIG. 1. Furthermore, even at a lower charge voltage (for example, when the charge voltage is 4.5 V or more and less than 4.6 V relative to the potential of lithium metal), the positive electrode active material shown in FIG. 1 may also have an O3' crystal structure.
[0103] In addition, when graphite is used as the negative electrode active material in a secondary battery, the voltage of the secondary battery drops below the voltage based on the potential of lithium metal by the amount of the graphite's potential. The potential of graphite is approximately 0.05 V to 0.2 V based on the potential of lithium metal. Therefore, even when the voltage of a secondary battery using graphite as the negative electrode active material is 4.3 V or higher and 4.5 V or lower, the positive electrode active material shown in FIG. 1 can maintain the R-3m(O3) crystal structure. Furthermore, even when the charge voltage is higher, for example, when the voltage of the secondary battery is higher than 4.5 V and lower than 4.6 V, the positive electrode active material shown in FIG. 1 can also adopt the O3'-type crystal structure. Furthermore, when the charge voltage is lower, for example, when the voltage of the secondary battery is 4.2 V or higher but lower than 4.3 V, the positive electrode active material shown in FIG. 1 can sometimes adopt the O3' structure.
[0104] Therefore, in the positive electrode active material shown in FIG. 1, the crystal structure is not easily broken even when charging and discharging are repeated at a high voltage.
[0105] The crystal structure shown in FIG. 4 is labeled R-3m(O3), and Li x CoO 2 This is the crystal structure of lithium cobalt oxide with x=1 in the unit cell. 2 There are three layers, and lithium is CoO 2 Lithium occupies an octahedral site where six oxygen atoms are coordinated. Therefore, this crystal structure is sometimes called an O3 type crystal structure. 2 The layer is defined as a structure in which octahedral structures in which oxygen is six-coordinated to cobalt are connected in a plane with edge sharing. This is sometimes called a layer consisting of cobalt and oxygen octahedra.
[0106] It is known that the lithium cobalt oxide shown in Figure 4 has a crystal structure that has high lithium symmetry when x = 0.5 or so and belongs to the monoclinic space group P2 / m. This structure has CoO 2 There is one layer, so it is sometimes called O1 type or monoclinic O1 type.
[0107] When x = 0, the positive electrode active material has a crystal structure of the trigonal space group P-3m1, and also contains CoO 2 There is one layer. Therefore, this crystal structure is sometimes called O1 type or trigonal O1 type. In addition, when the trigonal crystal is converted into a composite hexagonal lattice, it is sometimes called hexagonal O1 type.
[0108] When x is about 0.12, the lithium cobalt oxide shown in FIG. 4 has a crystal structure of the space group R-3m. This structure is similar to CoO, such as trigonal O1 type. 2 and LiCoO such as R-3m O 2It can also be said that the structure of and the structure of are stacked alternately. Therefore, this crystal structure is sometimes called an H1-3 crystal structure. Note that, since actual lithium insertion and extraction can be uneven, the H1-3 crystal structure is experimentally observed from about x = 0.25. In fact, the number of cobalt atoms per unit cell in the H1-3 crystal structure is twice that of other structures. However, in this specification and the like, to make it easier to compare with other crystal structures, the c-axis of the H1-3 crystal structure may be shown in a diagram where the c-axis is half the unit cell.
[0109] As an example of the H1-3 type crystal structure, as described in Non-Patent Document 1, the coordinates of cobalt and oxygen in the unit cell can be expressed as Co (0, 0, 0.42150 ± 0.00016), O1 (0, 0, 0.27671 ± 0.00045), and O2 (0, 0, 0.11535 ± 0.00045). O1 and O2 are each oxygen atoms. Which unit cell should be used to represent the crystal structure of the positive electrode active material can be determined, for example, by Rietveld analysis of the XRD pattern. In this case, it is sufficient to adopt a unit cell that results in a small GOF (goodness of fit) value.
[0110] The positive electrode active material shown in FIG. x CoO 2 The change in the crystal structure between the discharge state where x is 1 and the state where x is 0.24 or less is even smaller than that in Figure 4. More specifically, the change in the crystal structure between the discharge state where x is 1 and the state where x is 0.24 or less is even smaller than that in Figure 4. 2 The layer misalignment can be reduced, and the volume change per cobalt atom can be reduced.
[0111] In addition, in the positive electrode active material shown in FIG. 1, the difference in volume per the same number of cobalt atoms between R-3m(O3) in the discharged state and the O3′-type crystal structure is 2.5% or less, more specifically 2.2% or less, and typically 1.8%.
[0112] In the O3'-type crystal structure, the coordinates of cobalt and oxygen in the unit cell can be expressed within the ranges of Co(0,0,0.5), O(0,0,x), 0.20≦x≦0.25. Regarding the lattice constant of the unit cell, the a-axis is preferably 0.2797≦a≦0.2837 (nm), more preferably 0.2807≦a≦0.2827 (nm), and typically a=0.2817 (nm). The c-axis is preferably 1.3681≦c≦1.3881 (nm), more preferably 1.3751≦c≦1.3811 (nm), and typically c=1.3781 (nm).
[0113] CoO 2 Magnesium, which exists randomly and dilutely between the layers, i.e., at the lithium sites, turns into CoO when charged at a high voltage. 2 This has the effect of suppressing layer misalignment. 2 When magnesium is present between the layers, the O3' type crystal structure is easily formed.
[0114] However, if the heat treatment temperature is too high, cation mixing occurs, increasing the possibility that magnesium will enter the cobalt site. Magnesium present at the cobalt site may have little effect on maintaining the R-3m structure during high-voltage charging. Furthermore, if the heat treatment temperature is too high, there are concerns about adverse effects such as cobalt being reduced to divalent and lithium transpiration.
[0115] Therefore, it is preferable to add a halogen compound such as a fluorine compound to the lithium cobalt oxide before the heat treatment to distribute magnesium throughout the particles. Adding the halogen compound lowers the melting point of the lithium cobalt oxide. Lowering the melting point makes it easier to distribute magnesium throughout the particles at a temperature where cation mixing is unlikely to occur. Furthermore, the presence of a fluorine compound is expected to improve corrosion resistance to hydrofluoric acid produced by decomposition of the electrolyte.
[0116] Note that if the magnesium concentration is increased above a desired value, the effect on stabilizing the crystal structure may be reduced. This is thought to be because magnesium enters the cobalt site in addition to the lithium site. The number of magnesium atoms in the positive electrode active material produced according to one embodiment of the present invention is preferably 0.001 to 0.1 times the number of cobalt atoms, more preferably more than 0.01 to less than 0.04 times, and even more preferably about 0.02 times. The magnesium concentration shown here may be, for example, a value obtained by performing elemental analysis of the entire particles of the positive electrode active material using ICP-MS or the like, or may be based on the value of the raw material composition in the process of producing the positive electrode active material.
[0117] The number of nickel atoms in the positive electrode active material of one embodiment of the present invention is preferably 7.5% or less of the number of cobalt atoms, preferably 0.05% to 4%, and more preferably 0.1% to 2%. The nickel concentration shown here may be a value obtained by performing elemental analysis of the entire particles of the positive electrode active material using, for example, ICP-MS or the like, or may be based on a value obtained by mixing raw materials in the process of producing the positive electrode active material.
[0118] <Particle size> If the particle size of the positive electrode active material of one embodiment of the present invention is too large, problems such as difficulty in diffusing lithium and excessive roughness of the surface of the active material layer when applied to a current collector occur. On the other hand, if the particle size is too small, problems such as difficulty in supporting the active material layer when applied to a current collector and excessive reaction with the electrolyte occur. Therefore, the average particle size (D50: also referred to as median diameter) is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 40 μm or less, and even more preferably 5 μm or more and 30 μm or less.
[0119] <Analysis Method> Whether a certain positive electrode active material exhibits an O3'-type crystal structure when charged at a high voltage can be determined by analyzing the positive electrode charged at a high voltage using XRD, electron diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), etc. XRD is particularly preferred in that it can analyze the symmetry of transition metals such as cobalt contained in the positive electrode active material with high resolution, it can compare the level of crystallinity and the orientation of the crystals, it can analyze the periodic distortion of the lattice and the crystallite size, and it can obtain sufficient accuracy even when measuring a positive electrode obtained by disassembling a secondary battery as is.
[0120] As described above, the positive electrode active material of one embodiment of the present invention is characterized by minimal change in crystal structure between a high-voltage charged state and a discharged state. Materials in which a crystal structure that exhibits a significant change between a high-voltage charged state and a discharged state accounts for 50 wt % or more are undesirable because they cannot withstand high-voltage charging and discharging. It should be noted that the desired crystal structure may not be achieved simply by adding impurity elements. For example, even if both materials share the common feature of being lithium cobalt oxide containing magnesium and fluorine, there are cases in which the O3'-type crystal structure accounts for 60 wt % or more and cases in which the H1-3-type crystal structure accounts for 50 wt % or more when charged at a high voltage. Furthermore, at a certain voltage, the O3'-type crystal structure may be nearly 100 wt %, and further increasing the voltage may result in the H1-3-type crystal structure. Therefore, it is preferable to analyze the crystal structure of the positive electrode active material of one embodiment of the present invention using XRD or the like. By combining this with measurements such as XRD, a more detailed analysis can be performed.
[0121] However, when a positive electrode active material is charged or discharged at a high voltage, its crystal structure may change when exposed to air. For example, it may change from an O3'-type crystal structure to an H1-3-type crystal structure. Therefore, it is preferable to handle all samples in an inert atmosphere, such as an argon-containing atmosphere.
[0122] The positive electrode active material shown in FIG. 2 is a lithium cobalt oxide (LiCoO 2 The crystal structure of the lithium cobalt oxide shown in Figure 2 changes depending on the depth of charge.
[0123] As shown in FIG. 2, lithium cobalt oxide at a charge depth of 0 (discharged state) has a region having a crystal structure of the space group R-3m, and CoO 2 There are three layers. Therefore, this crystal structure is sometimes called an O3 type crystal structure. 2 The layer refers to a structure in which an octahedral structure in which cobalt is six-coordinated with oxygen atoms is continuous on a plane in an edge-sharing state.
[0124] At a charge depth of 1, the crystal structure has a space group of P-3m1, and the unit cell contains CoO 2 There is one layer, and therefore this crystal structure is sometimes called an O1-type crystal structure.
[0125] Furthermore, lithium cobalt oxide at a charge depth of about 0.8 has a crystal structure of the space group R-3m. This structure is similar to CoO such as P-3m1(O1). 2 and LiCoO such as R-3m(O3). 2 It can also be said that this crystal structure is a structure in which the structure of and are stacked alternately. For this reason, this crystal structure is sometimes called an H1-3 crystal structure. In reality, the number of cobalt atoms per unit cell in the H1-3 crystal structure is twice that of other structures. However, in Figure 2 and other parts of this specification, to make it easier to compare with other structures, the c-axis of the H1-3 crystal structure is shown as half the unit cell.
[0126] As an example of the H1-3 type crystal structure, the coordinates of cobalt and oxygen in the unit cell are Co(0, 0, 0.42150±0.00016), O 1 (0, 0, 0.27671±0.00045), O 2 It can be expressed as (0, 0, 0.11535±0.00045). 1 and O 2are oxygen atoms. In this way, the H1-3 crystal structure is represented by a unit cell using one cobalt and two oxygen atoms. On the other hand, the O3' crystal structure of one embodiment of the present invention is preferably represented by a unit cell using one cobalt and one oxygen atom. This indicates that the symmetry between cobalt and oxygen differs between the O3' crystal structure and the H1-3 structure, and the O3' crystal structure exhibits a smaller change from the O3 structure than the H1-3 structure. The unit cell that is more preferably used to represent the crystal structure of the positive electrode active material may be selected, for example, so that the GOF (good of fitness) value is smaller in Rietveld analysis of the XRD pattern.
[0127] When lithium cobalt oxide is repeatedly charged and discharged at a high voltage of 4.6 V or higher based on the redox potential of lithium metal, or when it is charged to a deep depth of charge of 0.8 or higher, the crystal structure of the lithium cobalt oxide changes repeatedly between the H1-3 crystal structure and the R-3m(O3) structure in the discharged state (i.e., a non-equilibrium phase change).
[0128] However, these two crystal structures are different from CoO 2 As shown by the dotted lines and arrows in Figure 2, in the H1-3 type crystal structure, CoO 2 The layers deviate significantly from R-3m(O3). Such dynamic structural changes can adversely affect the stability of the crystal structure.
[0129] Furthermore, the difference in volume is large: when compared per the same number of cobalt atoms, the difference in volume between the H1-3 type crystal structure and the O3 type crystal structure in a discharged state is 3.0% or more.
[0130] In addition, the H1-3 type crystal structure has CoO such as P-3m1(O1). 2 A structure with continuous layers is likely to be unstable.
[0131] Therefore, repeated high-voltage charging and discharging causes the crystalline structure of lithium cobalt oxide to collapse, which leads to a deterioration in cycle characteristics. This is thought to be because the collapse of the crystalline structure reduces the number of sites where lithium can exist stably and makes it difficult for lithium to be inserted and extracted.
[0132] An example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS. 4 to 7. Here, as an example, a method for manufacturing a positive electrode active material containing lithium, a transition metal, and an additional element X will be described.
[0133] 4A , a lithium source and a transition metal source are prepared as materials for lithium and transition metal. In the drawing, the lithium source is illustrated as a Li source, and the transition metal source is illustrated as an M source.
[0134] As the lithium source, for example, lithium carbonate, lithium fluoride, etc. can be used.
[0135] The transition metal source may be, for example, at least one of manganese, cobalt, and nickel. For example, the transition metal source may be a combination of cobalt alone, nickel alone, cobalt and manganese, cobalt and nickel, or cobalt, manganese, and nickel.
[0136] It is preferable to use a high-purity material as the transition metal source used in the synthesis. Specifically, the purity of the material is 3N (99.9%) or higher, preferably 4N (99.99%) or higher, more preferably 4N (99.995%) or higher, and even more preferably 5N (99.999%) or higher. The use of a high-purity material can increase the capacity and / or reliability of the secondary battery.
[0137] In addition, it is preferable that the transition metal source has high crystallinity. For example, it is preferable that the transition metal source has single crystal grains. The crystallinity of the transition metal source can be evaluated using, for example, a TEM (transmission electron microscope) image, a STEM (scanning transmission electron microscope) image, a HAADF-STEM (high-angle annular dark-field scanning transmission electron microscope) image, an ABF-STEM (annular bright-field scanning transmission electron microscope) image, or the like. The crystallinity of the transition metal source can also be evaluated using X-ray diffraction (XRD), electron beam diffraction, neutron beam diffraction, or the like. Note that the above-mentioned crystallinity evaluation can be applied not only to the transition metal source, but also to the evaluation of the crystallinity of primary particles or secondary particles.
[0138] Furthermore, when using metals capable of forming a layered rock-salt type composite oxide, it is preferable to set the mixing ratio of cobalt, manganese, and nickel within a range that allows a layered rock-salt type crystal structure to be formed. Furthermore, an additional element X may be added to these transition metals within a range that allows a layered rock-salt type crystal structure to be formed. An example of the process of adding the additional element X is shown in FIG. 4B. In step S11, a lithium source, a transition metal source, and an additional element X source are prepared, and then step S12 is performed.
[0139] The additive element X can be one or more selected from magnesium, calcium, zirconium, lanthanum, barium, titanium, yttrium, nickel, aluminum, cobalt, manganese, vanadium, iron, chromium, niobium, copper, potassium, sodium, zinc, chlorine, fluorine, hafnium, silicon, sulfur, phosphorus, boron, and arsenic. In addition to the above elements, bromine and beryllium may also be used as the additive element X. However, since bromine and beryllium are toxic to living organisms, it is preferable to use the additive element X described above.
[0140] The transition metal source may be an oxide or hydroxide of the metals exemplified above, and the cobalt source may be, for example, cobalt oxide or cobalt hydroxide.
[0141] As the manganese source, manganese oxide, manganese hydroxide, etc. can be used. As the nickel source, nickel oxide, nickel hydroxide, etc. can be used. As the aluminum source, aluminum oxide, aluminum hydroxide, etc. can be used.
[0142] <Step S12> Next, in step S12, the lithium source, transition metal source, and additive element X source are crushed and mixed. Crushing and mixing can be performed by dry or wet methods. It is particularly preferable to perform crushing using dehydrated acetone with a purity of 99.5% or higher, in which the water content is reduced to 10 ppm or less. Note that, in this specification, the term "crushing" may be interpreted as "pulverization." Mixing can be performed using, for example, a ball mill or a bead mill. When using a ball mill, it is preferable to use zirconia balls as the media. When using a ball mill or a bead mill, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less to suppress contamination from the media or materials. For example, the peripheral speed may be 838 mm / s (rotation speed: 400 rpm, ball mill diameter: 40 mm). Furthermore, using the dehydrated acetone described above in crushing and mixing can reduce impurities that may be mixed into the materials.
[0143] <Step S13> Next, in step S13, the mixed materials are heated. The heating temperature in this step is preferably 800°C or higher and lower than 1100°C, more preferably 900°C or higher and 1000°C or lower, and even more preferably about 950°C. If the temperature is too low, the decomposition and melting of the lithium source and transition metal source may be insufficient. On the other hand, if the temperature is too high, defects may occur due to factors such as lithium transpiration from the lithium source and / or excessive reduction of the metal used as the transition metal source. For example, when cobalt is used as the transition metal, defects may occur in which cobalt becomes divalent.
[0144] The heating time can be, for example, 1 hour or more and 100 hours or less, and preferably 2 hours or more and 20 hours or less. The heating is preferably carried out in an atmosphere with little water, such as dry air (for example, a dew point of -50°C or less, more preferably a dew point of -80°C or less). For example, the heating may be carried out in an atmosphere with a dew point of -93°C. The heating may also be carried out in a CH 4 , CO, CO 2 , and H 2 It is preferable to perform the treatment in an atmosphere in which the impurity concentrations of the above are 5 ppb (parts per billion) or less, since this can suppress impurities that may be mixed into the material.
[0145] For example, when heating at 1000°C for 10 hours, it is preferable to increase the temperature by 200°C / h and to supply dry air at a flow rate of 10 L / min. The heated material can then be cooled to room temperature. For example, it is preferable to set the cooling time from the specified temperature to room temperature to 10 hours or more and 50 hours or less. However, cooling to room temperature in step S13 is not essential.
[0146] The crucible used for heating in step S13 is preferably made of a material that does not easily release impurities. For example, a crucible made of alumina with a purity of 99.9% may be used.
[0147] Furthermore, when recovering the material after heating in step S13, it is preferable to transfer the material from the crucible to a mortar and then recover it, since this prevents impurities from being mixed into the material. It is also preferable that the mortar be made of a material that does not easily release impurities. Specifically, it is preferable to use a mortar made of alumina with a purity of 90% or more, preferably 99% or more. Note that conditions equivalent to those of step S13 can also be applied to heating steps other than step S13, which will be described later.
[0148] <Step S14> Through the above steps, the positive electrode active material 100 of one embodiment of the present invention can be manufactured (Step S14). Note that the positive electrode active material 100 is a composite oxide containing lithium, a transition metal, and oxygen (LiMO). 2 However, the positive electrode active material of one embodiment of the present invention may be represented by LiMO. 2The composition is not strictly limited to Li:M:O=1:1:2, so long as it has a crystalline structure of a lithium composite oxide represented by the formula:
[0149] By using a high-purity transition metal source material for synthesis and preparing a cathode active material through a synthesis process with minimal impurity contamination, a material with a low impurity concentration, in other words, a highly purified material, can be obtained. Furthermore, the cathode active material obtained by this method for preparing a cathode active material has high crystallinity. Furthermore, the cathode active material obtained by the method for preparing a cathode active material according to one embodiment of the present invention can increase the capacity and / or reliability of a secondary battery.
[0150] [Method 2 for Manufacturing Positive Electrode Active Material] Next, another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS. 5A, 5B, and 5C.
[0151] In FIG. 5A, steps S11 to S14 are performed in the same manner as in FIG. 4A to obtain a composite oxide containing lithium, a transition metal, and oxygen (LiMO). 2 ) to prepare.
[0152] It is also possible to use a pre-synthesized composite oxide in step S14. In this case, steps S11 to S13 can be omitted. When preparing a pre-synthesized composite oxide, it is preferable to use a high-purity material. The purity of the material is 99.5% or more, preferably 99.9% or more, and more preferably 99.99% or more.
[0153] A heating step may be provided between step S14 and the next step S20. This heating can smooth the surface of the composite oxide, for example. The heating may be performed, for example, under the same atmosphere and temperature conditions as in step S33 described below, with a treatment time shorter than that of step S33. A smooth surface refers to a surface with few irregularities, a rounded overall surface, and rounded corners. Furthermore, a surface with few foreign matter adhering to it is called smooth. Foreign matter is considered to be a cause of irregularities, so it is preferable that it does not adhere to the surface.
[0154] <Step S20> In step S20 of FIG. 5A, a source of the additive element X is prepared. The materials described above can be used as the source of the additive element X. Furthermore, a plurality of elements may be used as the additive element X. A case in which a plurality of elements is used as the additive element X will be described with reference to FIGS. 5B and 5C. The additive element X can be added by a solid-phase method, a liquid-phase method such as a sol-gel method, a sputtering method, a vapor deposition method, a CVD (chemical vapor deposition) method, a PLD (pulsed laser deposition) method, or the like.
[0155] 5B, a magnesium source (Mg source) and a fluorine source (F source) are prepared. A lithium source may also be prepared in addition to the magnesium source and the fluorine source.
[0156] As the magnesium source, for example, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. can be used.
[0157] Examples of fluorine sources include lithium fluoride (LiF) and magnesium fluoride (MgF 2 ), aluminum fluoride (AlF 3 ), titanium fluoride (TiF 4 ), cobalt fluoride (CoF 2 , CoF 3 ), nickel fluoride (NiF 2 ), zirconium fluoride (ZrF 4 ), vanadium fluoride (VF 5 ), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF 2 ), calcium fluoride (CaF 2 ), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF 2 ), cerium fluoride (CeF 2 ), lanthanum fluoride (LaF 3 ) Sodium aluminum hexafluoride (Na 3 AlF 6 The fluorine source is not limited to a solid, and may be, for example, fluorine (F 2 ), fluorocarbon, sulfur fluoride, oxygen fluoride (OF2 , O 2 F 2 , O 3 F 2 , O 4 F 2 , O 2 F), etc., may be used and mixed into the atmosphere in the heating step described below. A mixture of multiple fluorine sources may also be used. Among these, lithium fluoride is preferred because it has a relatively low melting point of 848°C and is easily melted in the heating step described below.
[0158] Examples of lithium sources that can be used include lithium fluoride and lithium carbonate. That is, lithium fluoride can be used as both a lithium source and a fluorine source. Magnesium fluoride can be used as both a fluorine source and a magnesium source.
[0159] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF) is prepared as the fluorine source and magnesium source. 2 ) Lithium fluoride LiF and magnesium fluoride MgF 2 is LiF:MgF 2 Mixing lithium fluoride (LiF) and magnesium fluoride (MgF) in a molar ratio of about 65:35 results in the greatest effect of lowering the melting point (Non-Patent Document 4). On the other hand, if the amount of lithium fluoride is too high, there is a concern that the lithium will be excessive and the cycle characteristics will deteriorate. Therefore, 2 The molar ratio of LiF:MgF 2 =x:1 (0≦x≦1.9), and LiF:MgF 2 =x:1 (0.1≦x≦0.5) is more preferable, and LiF:MgF 2 = x: 1 (x = 0.33 or its vicinity) is more preferable. In this specification, "or its vicinity" refers to a value that is greater than 0.9 times and smaller than 1.1 times the value.
[0160] When the subsequent mixing and crushing steps are performed in a wet system, a solvent is prepared. As the solvent, it is preferable to use a protic solvent that does not easily react with lithium, such as a ketone such as acetone, an alcohol such as ethanol or isopropanol, ether, dioxane, acetonitrile, or N-methyl-2-pyrrolidone (NMP).
[0161] <Step S22> Next, in step S22 of FIG. 5B, the above materials are mixed and crushed. Mixing can be performed by either a dry method or a wet method, but a wet method is preferred because it allows for smaller crushing. For example, a ball mill or a bead mill can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media. The conditions for the ball mill or bead mill can be the same as those for step S12.
[0162] <Step S23> Next, in step S23, the crushed and mixed material is recovered to obtain a source of the additional element X. Note that the source of the additional element X shown in step S23 may be called a mixture because it is formed from a plurality of materials.
[0163] The mixture preferably has a D50 (median diameter) of 600 nm or more and 20 μm or less, and more preferably 1 μm or more and 10 μm or less. Such a finely pulverized mixture facilitates uniform adhesion of the mixture to the surface of the composite oxide particles when mixed with a composite oxide containing lithium, a transition metal, and oxygen in a subsequent process. Uniform adhesion of the mixture to the surface of the composite oxide particles is preferred because it facilitates thorough distribution of halogen and magnesium near the surface of the composite oxide particles after heating. If there are regions near the surface that do not contain halogen and magnesium, the O3'-type crystal structure described below may be difficult to achieve in a charged state.
[0164] Although the method of mixing two materials in step S21 of FIG. 5B is illustrated, the present invention is not limited to this. For example, as shown in FIG. 5C , four materials (a magnesium source (Mg source), a fluorine source (F source), a nickel source (Ni source), and an aluminum source (Al source)) may be mixed to prepare the additive element X source. Alternatively, the additive element X source may be prepared using a single material, i.e., one type of material. Nickel oxide, nickel hydroxide, etc. may be used as the nickel source. Aluminum oxide, aluminum hydroxide, etc. may be used as the aluminum source.
[0165] <Step S31> Next, in step S31 of FIG. 5A, the LiMO obtained in step S14 is 2 and a source of an additional element X. The ratio of the number of transition metal atoms M in the composite oxide containing lithium, transition metal, and oxygen to the number of magnesium atoms Mg in the source of additional element X is preferably M:Mg=100:y (0.1≦y≦6), and more preferably M:Mg=100:y (0.3≦y≦3).
[0166] The mixing conditions in step S31 are preferably milder than those in step S12 so as not to destroy the composite oxide particles. For example, it is preferable to use conditions with a lower rotation speed or a shorter time than those in step S12. It can also be said that dry mixing provides milder conditions than wet mixing. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media.
[0167] In this embodiment, dry mixing is performed in a ball mill using zirconia balls with a diameter of 1 mm at 150 rpm for 1 hour in a dry room with a dew point of −100° C. or higher and −10° C. or lower.
[0168] <Step S32> Next, in step S32 of FIG. 5A, the mixed materials are collected to obtain a mixture 903.
[0169] Although this embodiment describes a method of adding a mixture of lithium fluoride and magnesium fluoride to lithium cobalt oxide with few impurities, one embodiment of the present invention is not limited thereto. Instead of the mixture 903 in step S32, a starting material for lithium cobalt oxide to which a magnesium source, a fluorine source, and the like have been added and heated may be used. In this case, there is no need to separate the steps S11 to S14 from the steps S21 to S23, which simplifies the process and increases productivity.
[0170] Alternatively, lithium cobalt oxide to which magnesium and fluorine have been added in advance may be used. If lithium cobalt oxide to which magnesium and fluorine have been added is used, the steps up to step S32 can be omitted, which is simpler.
[0171] Alternatively, a magnesium source and a fluorine source may be further added to lithium cobalt oxide to which magnesium and fluorine have been added in advance.
[0172] <Step S33> Next, in step S33, the mixture 903 is heated in an atmosphere containing oxygen. The heating is preferably performed in such a manner that the particles of the mixture 903 do not stick to each other.
[0173] It is preferable that the additive be added uniformly across the entire surface of the particles. However, if the particles of the mixture 903 stick together during heating, the additive may be added unevenly to only a portion of the surface. Furthermore, even though the surface of the particles is preferably smooth and has few irregularities, if the particles stick together, the surface may become more irregular, potentially increasing defects such as cracks and / or fissures. This is thought to be due to the fact that the adhesion of the particles of the mixture 903 reduces the contact area with oxygen in the atmosphere and obstructs the route for the additive to diffuse.
[0174] The heating in step S33 may be performed using a rotary kiln. The heating in a rotary kiln may be performed while stirring, whether it is a continuous or batch type. The heating in step S33 may be performed using a roller hearth kiln.
[0175] The heating temperature in step S33 is LiMO 2 The temperature must be equal to or higher than the temperature at which the reaction between LiMO and the source of the added element X proceeds. 2 The temperature may be lower than the melting point of these materials. For example, in the case of oxides, the melting point T m 0.757 times (Tammann temperature T d ) or more, solid-phase diffusion occurs. Therefore, the heating temperature in step S33 may be, for example, 500° C. or more.
[0176] However, if the temperature is equal to or higher than the temperature at which at least a part of the mixture 903 melts, the reaction proceeds more easily, which is preferable. For example, LiF and MgF are used as the source of the additive element X. 2 When LiF and MgF 2 Since the eutectic point of is around 742°C, it is preferable to set the heating temperature in step S33 to 742°C or higher.
[0177] Also, LiCoO 2 :LiF:MgF 2 In the mixture 903 in which the molar ratio is 100:0.33:1, an endothermic peak is observed around 830° C. in differential scanning calorimetry (DSC measurement). Therefore, the heating temperature is preferably 830° C. or higher.
[0178] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and productivity is higher.
[0179] However, the heating temperature is LiMO 2 Decomposition temperature of LiCoO 2 In addition, at temperatures close to the decomposition temperature, a small amount of LiMO 2 Therefore, the heating temperature in step S33 is preferably less than 1130°C, more preferably 1000°C or less, even more preferably 950°C or less, and even more preferably 900°C or less.
[0180] Therefore, the heating temperature in step S33 is preferably 500°C or higher and lower than 1130°C, more preferably 500°C or higher and lower than 1000°C, even more preferably 500°C or higher and lower than 950°C, and even more preferably 500°C or higher and lower than 900°C. Also, the heating temperature is preferably 742°C or higher and lower than 1130°C, more preferably 742°C or higher and lower than 1000°C, even more preferably 742°C or higher and lower than 950°C, and even more preferably 742°C or higher and lower than 900°C. Also, the heating temperature is preferably 830°C or higher and lower than 1130°C, more preferably 830°C or higher and lower than 1000°C, even more preferably 830°C or higher and lower than 950°C, and even more preferably 830°C or higher and lower than 900°C.
[0181] Furthermore, when the mixture 903 is heated, it is preferable to control the partial pressure of fluorine or fluoride in the atmosphere within an appropriate range.
[0182] In the manufacturing method described in this embodiment, some materials, for example, LiF, which is a fluorine source, may function as a flux. 2 The temperature can be lowered to a temperature below the decomposition temperature of the compound, for example, 742° C. to 950° C., and additives such as magnesium can be distributed near the surface, making it possible to produce a positive electrode active material with good characteristics.
[0183] However, since LiF has a lower specific gravity in a gaseous state than oxygen, when LiF volatilizes due to heating, the amount of LiF in the mixture 903 decreases. This weakens the function as a flux. Therefore, it is necessary to heat while suppressing the volatilization of LiF. Even if LiF is not used as a fluorine source, etc., LiMO 2 There is also a possibility that Li and F on the surface may react to produce LiF, which may then volatilize. Therefore, even if a fluoride with a higher melting point than LiF is used, it is still necessary to suppress volatilization.
[0184] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF is high in the heating furnace. By heating in this manner, it is possible to suppress the volatilization of LiF in the mixture 903.
[0185] Furthermore, when heating in a rotary kiln, it is preferable to control the flow rate of the oxygen-containing atmosphere in the kiln to heat the mixture 903. For example, it is preferable to reduce the flow rate of the oxygen-containing atmosphere, or to first purge the atmosphere and then not flow oxygen gas after introducing oxygen gas into the kiln.
[0186] When heating is performed using a roller hearth kiln, the mixture 903 can be heated in an atmosphere containing LiF by, for example, placing a lid on a container containing the mixture 903 .
[0187] The heating time is preferably determined by the heating temperature, the LiMO concentration in step S14, and the like. 2 The temperature and time required for the reaction may vary depending on the particle size, composition, etc. Small particles may be more suitable at lower temperatures or for shorter times than large particles.
[0188] For example, when the average particle size (D50) of the composite oxide in step S14 of Fig. 5A is about 12 µm, the heating temperature is preferably, for example, 600°C or higher and 950°C or lower. The heating time is, for example, preferably 3 hours or longer, more preferably 10 hours or longer, and even more preferably 60 hours or longer.
[0189] On the other hand, when the average particle size (D50) of the composite oxide in step S14 is about 5 μm, the heating temperature is preferably, for example, 600° C. or higher and 950° C. or lower. The heating time is preferably, for example, 1 hour or higher and 10 hours or lower, and more preferably about 2 hours. The temperature-lowering time after heating is preferably, for example, 10 hours or higher and 50 hours or lower.
[0190] <Step S34> Next, the heated material is recovered to produce the positive electrode active material 100. At this time, it is preferable to further sieve the recovered particles. Through the above steps, the positive electrode active material 100 of one embodiment of the present invention can be produced (Step S34).
[0191] [Method 3 for Manufacturing Positive Electrode Active Material] Next, another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS. 6, 7A, 7B, and 7C.
[0192] 6, steps S11 to S14 are performed in the same manner as in FIG. 4A to obtain a composite oxide containing lithium, a transition metal, and oxygen (LiMO 2 ) to prepare.
[0193] Alternatively, a composite oxide containing lithium, a transition metal, and oxygen that has been synthesized in advance may be used in step S14, in which case steps S11 to S13 can be omitted.
[0194] 5, a heating step may be provided between step S14 and step S20. The heating may be performed, for example, under the same atmosphere and temperature conditions as in step S33 described below, with the processing time being shorter than that in step S33.
[0195] <Step S20a> In step S20a of FIG. 6, a source of the additive element X1 is prepared. The source of the additive element X1 can be selected from the additive elements X described above. For example, one or more elements selected from magnesium, fluorine, and calcium can be suitably used as the additive element X1. In this embodiment, FIG. 7A illustrates a configuration in which magnesium and fluorine are used as the additive element X1. Steps S21 and S22 included in step S20a shown in FIG. 7A can be fabricated using the same processes as steps S21 and S22 shown in FIG. 5B. The additive element X1 can be added by a solid-phase method, a liquid-phase method such as a sol-gel method, a sputtering method, a vapor deposition method, a CVD (chemical vapor deposition) method, a PLD (pulsed laser deposition) method, or the like.
[0196] Step S23 shown in FIG. 7A is a process of recovering the material crushed and mixed in step S22 shown in FIG. 7A to obtain a source of the additional element X1.
[0197] 5. Steps S31 to S33 shown in FIG. 6 can be fabricated in the same manner as steps S31 to S33 shown in FIG.
[0198] <Step S34a> Next, the material heated in step S33 is recovered to produce a composite oxide.
[0199] <Step S40> In step S40 of FIG. 6 , a source of the additive element X2 is prepared. The additive element X2 source can be selected from the additive elements X described above. For example, the additive element X2 can be one or more elements selected from nickel, titanium, boron, zirconium, and aluminum. In this embodiment, FIG. 7B illustrates a configuration in which nickel and aluminum are used as the additive element X2. Steps S41 and S42 included in step S40 shown in FIG. 7B can be fabricated using the same processes as steps S21 and S22 shown in FIG. 5B . The additive element X2 can be added by a solid-phase method, a liquid-phase method such as a sol-gel method, a sputtering method, a vapor deposition method, a CVD (chemical vapor deposition) method, a PLD (pulsed laser deposition) method, or the like.
[0200] Step S43 shown in FIG. 7B is a process of recovering the material crushed and mixed in step S42 shown in FIG. 7B to provide a source of the additional element X2.
[0201] Step S40 shown in Fig. 7C is a modified example of step S40 shown in Fig. 7B. In Fig. 7C, a nickel source and an aluminum source are prepared (step S41), and each is independently crushed (step S42a), thereby preparing a plurality of sources of the additional element X2 (step S43).
[0202] Here, when the sol-gel method is used to add the additive element X2, a solvent to be used in the sol-gel method is prepared in addition to the additive element X2 source. For example, a metal alkoxide can be used as the metal source for the sol-gel method, and alcohol can be used as the solvent. For example, when aluminum is added, aluminum isopropoxide can be used as the metal source, and isopropanol (2-propanol) can be used as the solvent. For example, when zirconium is added, zirconium (IV) tetrapropoxide can be used as the metal source, and isopropanol can be used as the solvent.
[0203] <Steps S51 to S53> Next, step S51 in FIG. 6 is a step of mixing the composite oxide produced in step S34a with the source of the additive element X2 produced in step S40. Note that step S51 in FIG. 6 can be processed in a manner similar to step S31 shown in FIG. 5A. Note that step S52 in FIG. 6 can be processed in a manner similar to step S32 shown in FIG. 5A. Note that the material produced in step S52 in FIG. 6 is a mixture 904. Mixture 904 is a material containing the material of mixture 903 as well as the additive element X2 added in step S40. Note that step S53 in FIG. 6 can be processed in a manner similar to step S33 shown in FIG. 5A.
[0204] <Step S54> Next, the heated material is recovered to produce the positive electrode active material 100. At this time, it is preferable to further sieve the recovered particles. Through the above steps, the positive electrode active material 100 of one embodiment of the present invention can be produced (Step S54).
[0205] As shown in Figures 6 and 7A to 7C, by separating the steps of introducing the transition metal, the additive element X1, and the additive element X2, the depth profile of each element can sometimes be changed. For example, the concentration of the additive can be increased near the surface compared to the interior of the particle. Furthermore, the ratio of the number of atoms of the additive element to the reference number of transition metal atoms can be made higher near the surface than in the interior.
[0206] Furthermore, by using a high-purity material as the transition metal source for synthesis, employing a process with minimal impurity contamination during synthesis, thoroughly eliminating impurity contamination during synthesis, and controlling and introducing a desired additive element (additive element X, additive element X1, or additive element X2) into the positive electrode active material, a positive electrode active material can be obtained in which regions with low impurity concentrations and regions with the additive element introduced are controlled. Furthermore, a positive electrode active material with high crystallinity can be obtained. Furthermore, the positive electrode active material obtained by the method for manufacturing a positive electrode active material according to one embodiment of the present invention can increase the capacity and / or reliability of a secondary battery.
[0207] [Positive Electrode Active Material 2] The positive electrode active material of one embodiment of the present invention is not limited to the materials listed above. Alternatively, the positive electrode active material of one embodiment of the present invention may be a mixture of the above-listed materials and other materials.
[0208] For example, a composite oxide having a spinel crystal structure can be used as the positive electrode active material. Also, for example, a polyanion-based material can be used as the positive electrode active material. Examples of polyanion-based materials include materials having an olivine crystal structure and Nasicon-based materials. Also, for example, a material containing sulfur can be used as the positive electrode active material.
[0209] Examples of materials having a spinel-type crystal structure include LiM 2 O 4 It is preferable that the metal M contains Mn. For example, LiMn 2 O 4 Furthermore, by including Ni in addition to Mn as the metal M, the discharge voltage of the secondary battery may be improved, and the energy density may be improved, which is preferable. 2 O 4 A small amount of lithium nickel oxide (LiNiO) is added to a lithium-containing material having a spinel-type crystal structure containing manganese, such as 2 or LiNi 1−x M x O 2By mixing M (Co, Al, etc.), the characteristics of the secondary battery can be improved, which is preferable.
[0210] An example of a polyanion-based material that can be used is a composite oxide containing oxygen, a metal A, a metal M, and an element X. The metal A is one or more of Li, Na, and Mg, the metal M is one or more of Fe, Mn, Co, Ni, Ti, V, and Nb, and the element X is one or more of S, P, Mo, W, As, and Si.
[0211] Examples of materials having an olivine-type crystal structure include composite materials (general formula: LiMPO 4 (M is one or more of Fe(II), Mn(II), Co(II), and Ni(II)) can be used. The general formula is LiMPO 4 Representative examples include LiFePO 4 , LiNiPO 4 , LiCoPO 4 , LiMnPO 4 , LiFe a Ni b P.O. 4 , LiFe a Co b P.O. 4 , LiFe a Mn b P.O. 4 , LiNi a Co b P.O. 4 , LiNi a Mn b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1), LiFe c Ni d Co e P.O. 4 , LiFe c Ni d Mn e P.O. 4 , LiNi c Co d Mn e P.O. 4 (c+d+e is 1 or less, 0<c<1, 0<d<1, 0<e<1), LiFe f Ni g Co h Mn i P.O. 4(f+g+h+i is 1 or less, 0<f<1, 0<g<1, 0<h<1, 0<i<1) and other lithium compounds can be used.
[0212] Also, the general formula Li (2−j) MSiO 4 (M is one or more of Fe(II), Mn(II), Co(II), Ni(II), 0≦j≦2) and other composite materials can be used. (2−j) MSiO 4 Representative examples include Li (2−j) FeSiO 4 , Li (2−j) NiSiO 4 , Li (2−j) CoSiO 4 , Li (2−j) MnSiO 4 , Li (2−j) Fe k Ni l SiO 4 , Li (2−j) Fe k Co l SiO 4 , Li (2−j) Fe k Mn l SiO 4 , Li (2−j) Ni k Co l SiO 4 , Li (2−j) Ni k Mn l SiO 4 (k+l is 1 or less, 0<k<1, 0<l<1), Li (2−j) Fe m Ni n Co q SiO 4 , Li (2−j) Fe m Ni n Mn q SiO 4 , Li (2−j) Ni m Co n Mn q SiO 4 (m+n+q is 1 or less, 0<m<1, 0<n<1, 0<q<1), Li (2−j) Fe r Ni s Cot Mn u SiO 4 Lithium compounds such as (r+s+t+u is 1 or less, 0<r<1, 0<s<1, 0<t<1, 0<u<1) can be used as materials.
[0213] Also, A x M 2 (XO 4 ) 3 Nasicon type compounds represented by the general formula (A = Li, Na, Mg, M = Fe, Mn, Ti, V, Nb, X = S, P, Mo, W, As, Si) can be used. 2 (MnO 4 ) 3 , Fe 2 (SO 4 ) 3 , Li 3 Fe 2 (P.O. 4 ) 3 In addition, as a positive electrode active material, Li 2 MPO 4 F, Li 2 MP 2 O 7 , Li 5 MO 4 Compounds represented by the general formula (M=Fe, Mn) can be used.
[0214] In addition, NaFeF 3 , FeF 3 Perovskite-type fluorides such as TiS 2 , MoS 2 Metal chalcogenides (sulfides, selenides, tellurides), LiMVO 4 oxides having an inverse spinel type crystal structure, such as vanadium oxides (V 2 O 5 , V 6 O 13 , LiV 3 O 8 Materials such as manganese oxides and organic sulfur compounds may also be used.
[0215] In addition, as the positive electrode active material, 3A borate-based material represented by (M is Fe(II), Mn(II), or Co(II)) may also be used.
[0216] Examples of materials containing sodium include NaFeO 2 , Na 2/3 [Fe 1/2 Mn 1/2 ]O 2 , Na 2/3 [Ni 1/3 Mn 2/3 ]O 2 , Na 2 Fe 2 (SO 4 ) 3 , Na 3 V 2 (P.O. 4 ) 3 , Na 2 FePO 4 F, NaVPO 4 F, NaMPO 4 (M is Fe(II), Mn(II), Co(II), Ni(II)), Na 2 FePO 4 F, Na 4 Co 3 (P.O. 4 ) 2 P 2 O 7 Alternatively, a sodium-containing oxide such as , may be used as the positive electrode active material.
[0217] Furthermore, lithium-containing metal sulfides may be used as the positive electrode active material. 2 TiS 3 , Li 3 NbS 4 Examples include:
[0218] [Positive Electrode Active Material 3] Particles containing a plurality of the positive electrode active materials listed above may be used as the positive electrode active material. For example, one of the positive electrode active materials listed above may be used as the first material, and another of the positive electrode active materials listed above may be used as the second material, and the particles may have a structure in which at least a portion of the first material is covered with the second material. Such particles having a structure in which at least a portion of the first material is covered with the second material may be referred to as a positive electrode active material composite. The composite treatment may be one or more of the following: composite treatments using mechanical energy, such as mechanochemical, mechanofusion, and ball milling; composite treatments using liquid-phase reactions, such as coprecipitation, hydrothermal, and sol-gel; and composite treatments using gas-phase reactions, such as barrel sputtering, atomic layer deposition (ALD), vapor deposition, and chemical vapor deposition (CVD). It is preferable to perform a heat treatment after the composite treatment. The composite treatment may also be called a surface coating treatment or a coating treatment.
[0219] The positive electrode active material particles may form secondary particles.
[0220] [Electrolyte] The secondary battery of one embodiment of the present invention preferably includes an electrolyte. As the electrolyte, an organic electrolyte, an ionic liquid, a solid electrolyte, or the like can be used. The secondary battery of one embodiment of the present invention particularly preferably includes an ionic liquid.
[0221] When the electrolyte contains water, the water may react with the electrolyte to form compounds, which may react with battery components such as the current collector, active material, and conductive additive, resulting in a decrease in charge / discharge efficiency.
[0222] As an example, the electrolyte is LiPF 6 Consider the case where the electrolyte has LiPF 6 When the compound has the formula (I), it is presumed that the reaction with water will sequentially proceed as shown in the following reaction formulas (1) to (4).
[0223] H 2 O+LiPF 6 → LiF + POF3 +2HF(1)
[0224] H 2 O+POF 3 → HPO 2 F 2 +HF(2)
[0225] H 2 O + HPO 2 F 2 → H 2 P.O. 3 F+HF(3)
[0226] H 2 O + HPO 3 F → H 3 P.O. 4 +HF(4)
[0227] The reactions of the above reaction formulas (1) to (4) can be collectively represented by the following reaction formula (5).
[0228] H 2 O+LiPF 6 → LiF + H 3 P.O. 4 +HF(5)
[0229] In this way, the electrolyte is LiPF 6 In the case of a battery containing a lithium-ion battery, it is believed that the inclusion of water generates hydrofluoric acid. Hydrofluoric acid may react with, for example, the aluminum current collector of the positive electrode. If such a reaction occurs, the charge / discharge efficiency decreases, and the discharge capacity decreases.
[0230] The compounds produced by the reaction of water and electrolytes can sometimes be evaluated by nuclear magnetic resonance spectroscopy (NMR). For example, compounds containing fluorine can be 19 Phosphorus-containing compounds may be detected by F-NMR spectroscopy. 31 It may be detected by P-NMR spectroscopy.
[0231] The electrolyte in the secondary battery of one embodiment of the present invention has a water content of less than 1000 ppm, preferably less than 100 ppm, more preferably less than 50 ppm, even more preferably less than 20 ppm, still more preferably less than 10 ppm, still more preferably less than 5 ppm, and still more preferably less than 1 ppm.
[0232] The content of components such as impurities in the electrolyte of the present invention can be measured by, for example, ICP emission spectroscopy, ion chromatography, a Karl Fischer moisture meter, or gas chromatography.
[0233] The water content of the electrolyte can be measured, for example, by a Karl Fischer moisture meter.
[0234] The electrolyte in the secondary battery of one embodiment of the present invention contains hydrogen fluoride in an amount of 100 ppm or less, preferably 50 ppm or less, more preferably 20 ppm or less, still more preferably less than 10 ppm, still more preferably less than 5 ppm, and still more preferably less than 1 ppm.
[0235] The water content of the electrolyte can be reduced by, for example, treatment under reduced pressure, heat treatment, or the addition of a drying agent such as a molecular sieve. The molecular sieve is preferably removed from the electrolyte after treatment. Alternatively, a water-absorbing additive may be added to the electrolyte. These treatments may also be combined.
[0236] The electrolyte included in the secondary battery of one embodiment of the present invention contains a salt containing a metal that serves as a carrier ion.
[0237] The secondary battery of one embodiment of the present invention has, as a carrier ion, one or more ions selected from alkali metal ions such as sodium ions and potassium ions, and alkaline earth metal ions such as calcium ions, strontium ions, barium ions, beryllium ions, and magnesium ions.
[0238] When lithium ions are used as carrier ions, the electrolyte contains a lithium salt, for example, LiPF 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiAlCl 4 , LiSCN, LiBr, LiI, Li 2 SO 4 , Li 2 B 10 Cl 10 , Li 2 B12 Cl 12 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 4 F 9 SO 2 ) (CF 3 SO 2 ), LiN(C 2 F 5 SO 2 ) 2 etc. can be used.
[0239] The electrolyte of the secondary battery of one embodiment of the present invention can use, in addition to the above salts, one or more selected from esters, ethers, nitriles, sulfoxides, sulfones, sulfonate esters, and the like, in any combination and ratio.
[0240] The electrolyte solution included in the secondary battery of one embodiment of the present invention preferably contains one or more of a cyclic carbonate and a chain carbonate. For example, a solution containing one or more of a cyclic carbonate and a chain carbonate and the above-described salt can be used as the electrolyte. A fluorinated cyclic carbonate may be used as the cyclic carbonate. A fluorinated chain carbonate may be used as the chain carbonate. The electrolyte may contain multiple types of cyclic carbonates. The electrolyte may contain multiple types of chain carbonates.
[0241] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, and γ-valerolactone.
[0242] Examples of the chain carbonate include dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC).
[0243] Examples of fluorinated cyclic carbonates include fluorinated ethylene carbonates, such as monofluoroethylene carbonate (fluoroethylene carbonate, FEC, F1EC), difluoroethylene carbonate (DFEC, F2EC), trifluoroethylene carbonate (F3EC), and tetrafluoroethylene carbonate (F4EC). DFEC includes isomers such as cis-4,5 and trans-4,5 isomers.
[0244] Monofluoroethylene carbonate (FEC) is represented by the following structural formula (101): Tetrafluoroethylene carbonate (F4EC) is represented by the following structural formula (102): Difluoroethylene carbonate (DFEC) is represented by the following structural formula (103):
[0245]
[0246] Fluorinated cyclic carbonates can improve the non-flammability and safety of lithium-ion secondary batteries. The use of one or more fluorinated cyclic carbonates as the electrolyte to solvate lithium ions and transport them within the electrolyte contained in the electrodes during charge and discharge is important for low-temperature operation.
[0247] The use of a fluorinated cyclic carbonate in the electrolyte reduces the desolvation energy required for lithium ions solvated in the electrolyte contained in the electrode to enter active material particles. Reducing this desolvation energy facilitates insertion and desorption of lithium ions into active material particles, even at low temperatures. While lithium ions may migrate in a solvated state, they may also undergo a hopping phenomenon, in which the coordinated solvent molecules are swapped. When lithium ions are more easily desolvated, they may be more easily transported by hopping, which may facilitate the movement of lithium ions.
[0248] In addition to the above-described salts, the electrolyte of the secondary battery according to one embodiment of the present invention may include one or more of methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), diethyl ether, methyl diglyme, tetrahydrofuran, acetonitrile, benzonitrile, dimethyl sulfoxide, sulfolane, and sultone, in any combination and ratio. Furthermore, one or more of these may be used in combination with one or more of the above-described cyclic carbonates and chain carbonates.
[0249] In addition, additives such as vinylene carbonate (VC), propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), succinonitrile, adiponitrile, fluorobenzene, cyclohexylbenzene, biphenyl, etc. may be added to the electrolyte. The concentration of the added material may be, for example, 0.1 wt % to 5 wt % of the total solvent.
[0250] The electrolyte included in the secondary battery of one embodiment of the present invention preferably includes an ionic liquid and a salt containing a metal that serves as a carrier ion.
[0251] When the electrolyte contains an ionic liquid, the salt containing a metal that serves as a carrier ion is preferably a metal salt of a fluorosulfonate anion or a fluoroalkylsulfonate anion, and among these, (C n F 2n+1 SO 2 ) 2 N − Metal salts of amide anions represented by (n=0 or more and 3 or less) are preferred because they have high stability at high temperatures and high resistance to oxidation and reduction.
[0252] Ionic liquids are composed of cations and anions, and include organic cations and anions. Examples of organic cations used in the electrolyte include aromatic cations such as imidazolium cations and pyridinium cations, and aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations. Examples of anions used in the electrolyte include monovalent amide anions, monovalent methide anions, fluorosulfonate anions, perfluoroalkylsulfonate anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, and perfluoroalkylphosphate anions.
[0253] In addition to the ionic liquid, the electrolyte may contain an aprotic solvent such as one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, sulfolane, and sultone, or a mixture of two or more of these in any combination and ratio.
[0254] Furthermore, an additive such as vinylene carbonate (VC), propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), succinonitrile, adiponitrile, fluorobenzene, cyclohexylbenzene, biphenyl, etc. may be added to the electrolyte containing an ionic liquid. The concentration of the added material may be, for example, 0.1 wt % to 5 wt % of the total solvent.
[0255] As the ionic liquid having an imidazolium cation, for example, an ionic liquid represented by the following general formula (G1) can be used. In the general formula (G1), R 1 represents an alkyl group having 1 to 6 carbon atoms or a substituted or unsubstituted aryl group having 6 to 13 carbon atoms, preferably an alkyl group having 1 to 4 carbon atoms; R 2 ~R 4 each independently represents a hydrogen atom, an alkyl group having from 1 to 6 carbon atoms, or a substituted or unsubstituted aryl group having from 6 to 13 carbon atoms, preferably an alkyl group having from 1 to 4 carbon atoms; R 5 represents an alkyl group or a main chain composed of two or more atoms selected from C, O, Si, N, S, and P. 5 A substituent may be introduced into the main chain of R. Examples of the substituent to be introduced include an alkyl group and an alkoxy group. 5 The main chain of R may have a carboxy group. 5 The main chain may have a carbonyl group.
[0256]
[0257] As the ionic liquid having a pyridinium cation, for example, an ionic liquid represented by the following general formula (G2) may be used. In general formula (G2), R 6 represents an alkyl group or a main chain composed of two or more atoms selected from C, O, Si, N, S, and P; R 7 ~R 11 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 6 A substituent may be introduced into the main chain of the polymer. Examples of the substituent to be introduced include an alkyl group and an alkoxy group.
[0258]
[0259] As the ionic liquid having a quaternary ammonium cation, for example, ionic liquids represented by the following general formulae (G3), (G4), (G5) and (G6) can be used.
[0260]
[0261] In general formula (G3), R 28 ~R 31 each independently represents an alkyl group having 1 to 20 carbon atoms, a methoxy group, a methoxymethyl group, a methoxyethyl group, or a hydrogen atom.
[0262]
[0263] In general formula (G4), R 12 ~R 17 each independently represents an alkyl group having 1 to 20 carbon atoms, a methoxy group, a methoxymethyl group, a methoxyethyl group, or a hydrogen atom.
[0264]
[0265] In general formula (G5), R 18 ~R 24 each independently represents an alkyl group having 1 to 20 carbon atoms, a methoxy group, a methoxymethyl group, a methoxyethyl group, or a hydrogen atom.
[0266]
[0267] In general formula (G6), n and m are 1 or more and 3 or less. α is 0 or more and 6 or less, and when n is 1, α is 0 or more and 4 or less, when n is 2, α is 0 or more and 5 or less, and when n is 3, α is 0 or more and 6 or less. β is 0 or more and 6 or less, when m is 1, β is 0 or more and 4 or less, when m is 2, β is 0 or more and 5 or less, and when m is 3, β is 0 or more and 6 or less. When α or β is 0, this indicates unsubstituted. The case where both α and β are 0 is excluded. X or Y represents, as a substituent, a linear or side-chain alkyl group having 1 to 4 carbon atoms, a linear or side-chain alkoxy group having 1 to 4 carbon atoms, or a linear or side-chain alkoxyalkyl group having 1 to 4 carbon atoms.
[0268] As an ionic liquid having a tertiary sulfonium cation, for example, an ionic liquid represented by the following general formula (G7) can be used. In general formula (G7), R 25 ~R 27each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group. 25 ~R 27 A main chain composed of two or more atoms selected from C, O, Si, N, S, and P may be used as the main chain.
[0269]
[0270] As the ionic liquid having a quaternary phosphonium cation, for example, an ionic liquid represented by the following general formula (G8) can be used. In general formula (G8), R 32 ~R 35 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group. 32 ~R 35 A main chain composed of two or more atoms selected from C, O, Si, N, S, and P may be used as the main chain.
[0271]
[0272] A represented by general formulas (G1) to (G8) − As the anion, one or more of a monovalent amide anion, a monovalent methide anion, a fluorosulfonate anion, a perfluoroalkylsulfonate anion, a tetrafluoroborate anion, a perfluoroalkylborate anion, a hexafluorophosphate anion, and a perfluoroalkylphosphate anion can be used.
[0273] As the monovalent amide anion, (C n F 2n+1 SO 2 ) 2 N − (n=0 or more and 3 or less), and the monovalent cyclic amide anion is (CF 2 SO 2 ) 2 N − The monovalent methide anion can be, for example, (C n F 2n+1 SO 2 ) 3 C −(n=0 or more and 3 or less), and the monovalent cyclic methide anion is (CF 2 SO 2 ) 2 C − (CF 3 SO 2 ) and the like can be used. As the fluoroalkylsulfonate anion, (C m F 2m+1 SO 3 ) − (m=0 or more and 4 or less). Examples of the fluoroalkylborate anion include {BF n (C m H k F 2m+1−k ) 4−n} − (n = 0 or more and 3 or less, m = 1 or more and 4 or less, k = 0 or more and 2m or less). Examples of the fluoroalkyl phosphate anion include {PF n (C m H k F 2m+1−k ) 6−n} − (n=0 or more and 5 or less, m=1 or more and 4 or less, k=0 or more and 2m or less)
[0274] Furthermore, as the monovalent amide anion, for example, one or more of a bis(fluorosulfonyl)amide anion and a bis(trifluoromethanesulfonyl)amide anion can be used.
[0275] The ionic liquid may also have one or more of a hexafluorophosphate anion and a tetrafluoroborate anion.
[0276] From now on, (FSO 2 ) 2 N − The anion represented by the formula (CF) is an FSA anion. 3 SO 2 ) 2 N − The anion represented by the formula (I) may be referred to as a TFSA anion.
[0277] Specific examples of the cation of the general formula (G1) include structural formulae (111) to (174).
[0278]
[0279]
[0280]
[0281]
[0282]
[0283]
[0284] The ionic liquid represented by the general formula (G1) is a compound represented by the general formula (G2) − and an anion represented by the formula (I). Ionic liquids having an imidazolium cation have low viscosity and can be used over a wide temperature range. Furthermore, ionic liquids having an imidazolium cation are highly stable and have a wide potential window, making them suitable for use as electrolytes in secondary batteries.
[0285] The ionic liquid represented by the general formula (G1) can be mixed with a salt such as a lithium salt and used as an electrolyte for a secondary battery. The imidazolium cation represented by the general formula (G1) has high oxidation resistance and reduction resistance and a wide potential window, making it suitable as a solvent for use in an electrolyte. Here, the potential window refers to the range of potential within which an electrolyte is not electrolyzed. In a secondary battery, increasing the charging voltage can increase the energy density of the secondary battery. Therefore, by using an ionic liquid with a wide potential window and particularly excellent oxidation resistance, an excellent secondary battery can be realized.
[0286] In general formula (G1), R 1 is a methyl group, an ethyl group, or a propyl group, and R 2 , R 3 and R 4 one of which is a hydrogen atom or a methyl group, and the other two are hydrogen atoms; and an anion A − As, (FSO 2 ) 2 N − Anions represented by (FSA anion) and (CF 3 SO 2 ) 2 N− By using either one of the anions (TFSA anion) represented by the formula (I) or a mixture of two of them, it is possible to realize an electrolyte that has a wide potential window, excellent oxidation resistance, low viscosity, does not solidify even at low temperatures, and can be used over a wide temperature range.
[0287] In addition, as the salt used for the electrolyte, metal salts of fluorosulfonic acid anions and fluoroalkylsulfonic acid anions are particularly preferred in some cases, and among these, (C n F 2n+1 SO 2 ) 2 N − Metal salts of amide-based anions represented by (n = 0 to 3) are preferred because they have high stability at high temperatures and high resistance to oxidation and reduction. 2 ) 2 , LiN(CF 3 SO 2 ) 2 By using either one of these or a mixture of the two, a secondary battery that is highly stable and can operate over a wide temperature range can be realized.
[0288] Specific examples of the cation of the above general formula (G2) include structural formulae (701) to (719).
[0289]
[0290]
[0291] Specific examples of the cation of the general formula (G4) include structural formulae (501) to (520).
[0292]
[0293] Specific examples of the cation of the above general formula (G5) include structural formulae (601) to (630).
[0294]
[0295]
[0296] Specific examples of the cation of the general formula (G6) include structural formulae (301) to (309) and structural formulae (401) to (419).
[0297]
[0298]
[0299] In addition, structural formulas (301) to (309) and structural formulas (401) to (419) show examples in which m is 1 in general formula (G6), but m may be changed to 2 or 3 in structural formulas (301) to (309) and structural formulas (401) to (419).
[0300] Specific examples of the cation of the general formula (G7) include structural formulae (201) to (215).
[0301]
[0302] In the secondary battery of one embodiment of the present invention, even when the secondary battery is repeatedly used at a high charging voltage, a decrease in capacity can be suppressed and significantly excellent characteristics can be achieved.
[0303] [Negative Electrode Active Material] The negative electrode of one embodiment of the present invention includes a negative electrode active material. The negative electrode of one embodiment of the present invention preferably includes a conductive agent. The negative electrode of one embodiment of the present invention preferably includes a binder.
[0304] As the negative electrode active material, it is preferable to use a material capable of reacting with carrier ions of the secondary battery, a material capable of inserting and desorbing carrier ions, a material capable of alloying with a metal that becomes a carrier ion, a material capable of dissolving and precipitating a metal that becomes a carrier ion, or the like.
[0305] As the negative electrode active material, for example, carbon materials such as graphite, graphitizable carbon, non-graphitizable carbon, carbon nanotubes, carbon black, and graphene can be used.
[0306] As the negative electrode active material, for example, a material containing one or more elements selected from silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, and indium can be used.
[0307] Furthermore, impurity elements such as phosphorus, arsenic, boron, aluminum, and gallium may be added to silicon to lower its resistance.
[0308] Examples of silicon-containing materials include SiO x (x is preferably smaller than 2, more preferably 0.5 or more and 1.6 or less) can be used.
[0309] The silicon-containing material may have, for example, a plurality of crystal grains within a single particle. For example, a single particle may have one or more silicon crystal grains within it. The single particle may have silicon oxide around the silicon crystal grains. The silicon oxide may be amorphous.
[0310] Silicon nanoparticles can be used as the negative electrode active material. The average particle size of the silicon nanoparticles is preferably 5 nm or more and less than 1 μm, more preferably 10 nm or more and 300 nm or less, and even more preferably 10 nm or more and 100 nm or less.
[0311] The silicon nanoparticles may be crystalline, or may have a crystalline region and an amorphous region.
[0312] In addition, lithium silicate (Li 2c SiO (2+c) , 0<c<2) may be used. Furthermore, the lithium silicate phase may contain a zirconium compound, an yttrium compound, an iron compound, a nickel compound, or the like, and it is more preferable that these metal compounds are dispersed in the lithium silicate phase.
[0313] Examples of compounds containing silicon include Li 2 SiO 3 and Li 4 SiO 4 Li can be used.2 SiO 3 and Li 4 SiO 4 may each be crystalline or amorphous.
[0314] Furthermore, particles containing lithium silicate can be used as the negative electrode active material. The lithium silicate-containing particles may contain zirconium, yttrium, iron, etc. Furthermore, the lithium silicate-containing particles may have a form in which a plurality of silicon crystal grains are contained within one particle.
[0315] The average particle size of the particles containing lithium silicate is preferably 100 nm or more and 100 μm or less, and more preferably 500 nm or more and 50 μm or less.
[0316] The silicon-containing compound can be analyzed using NMR, XRD, Raman spectroscopy, or the like.
[0317] Examples of materials that can be used for the negative electrode active material include oxides containing one or more elements selected from titanium, niobium, tungsten, and molybdenum.
[0318] As the negative electrode active material, a combination of the above-mentioned metals, materials, compounds, etc. can be used.
[0319] The negative electrode active material of one embodiment of the present invention may have fluorine in the surface layer portion. The negative electrode active material having a halogen in the surface layer portion can suppress a decrease in charge / discharge efficiency. It is also believed that the reaction with the electrolyte on the active material surface is suppressed. Furthermore, the negative electrode active material of one embodiment of the present invention may have at least a portion of its surface covered with a region containing a halogen. The region may be, for example, in the form of a film. Fluorine is particularly preferred as the halogen.
[0320] <Example of Manufacturing Method> An example of a method for manufacturing a negative electrode active material having a halogen in the surface layer portion will be described.
[0321] The negative electrode active material can be manufactured by mixing the above-described material that can be used as a negative electrode active material as the first material and a compound having a halogen as the second material, and performing heat treatment.
[0322] In addition to the first and second materials, a third material may be mixed that undergoes a eutectic reaction with the second material. The eutectic point resulting from the eutectic reaction is preferably lower than at least one of the melting points of the second and third materials. The lowering of the melting point due to the eutectic reaction may facilitate the second and third materials to cover the surface of the first material during heat treatment, thereby improving the coating properties.
[0323] Furthermore, by using, as the second material and the third material, materials having a metal whose ions function as carrier ions in the reaction of the secondary battery, when the metal is contained in the negative electrode active material, the metal may contribute to charging and discharging as a carrier ion.
[0324] The third material may be, for example, a material containing oxygen and carbon, such as a carbonate, or an organic compound.
[0325] Alternatively, a hydroxide may be used as the third material.
[0326] Carbonates, hydroxides, etc. are preferred because they are inexpensive and highly safe materials, and carbonates, hydroxides, etc. are also preferred because they may have a eutectic point with a material containing a halogen.
[0327] A more specific example of the second material and the third material will be described. When lithium fluoride is used as the second material, when it is mixed with the first material and heated, the lithium fluoride may not cover the surface of the first material and may aggregate on its own. In such a case, the coverage of the surface of the first material may be improved by using a material that undergoes a eutectic reaction with lithium fluoride as the third material.
[0328] When the first material is heated, a reaction with oxygen in the atmosphere may occur during the heating, and an oxide film may be formed on the surface. In the preparation of the negative electrode active material of one embodiment of the present invention, a eutectic reaction between the material containing halogen and the material containing oxygen and carbon occurs in the annealing step described later, whereby heating can be performed at a low temperature, thereby suppressing an oxidation reaction on the surface.
[0329] Furthermore, when a carbon material is used as the first material, carbon dioxide is generated by a reaction between the carbon material and oxygen in the atmosphere during heating, which may result in a weight loss of the first material, damage to the surface of the first material, etc. In the preparation of the negative electrode active material of one embodiment of the present invention, heating can be performed at a low temperature, and therefore weight loss, surface damage, etc. can be suppressed even when a carbon material is used as the first material.
[0330] Here, graphite is prepared as the first material. Examples of graphite that can be used include flake graphite, spherical natural graphite, and MCMB. The surface of the graphite may be coated with a low-crystalline carbon material.
[0331] A material containing a halogen is prepared as the second material. A halogen compound containing a metal A1 can be used as the halogen material. For example, the metal A1 can be one or more selected from lithium, magnesium, aluminum, sodium, potassium, calcium, barium, lanthanum, cerium, chromium, manganese, iron, cobalt, nickel, zinc, zirconium, titanium, vanadium, and niobium. For example, a fluoride or a chloride can be used as the halogen compound. The halogen contained in the halogen material is represented by element Z.
[0332] Here, lithium fluoride is prepared as an example.
[0333] A material containing oxygen and carbon is prepared as the third material. For example, a carbonate containing a metal A2 can be used as the material containing oxygen and carbon. For example, the metal A2 can be one or more selected from the group consisting of lithium, magnesium, aluminum, sodium, potassium, calcium, barium, lanthanum, cerium, chromium, manganese, iron, cobalt, and nickel.
[0334] Here, lithium carbonate is prepared as an example.
[0335] The first material, the second material, and the third material are mixed to obtain a mixture.
[0336] The second material and the third material are preferably mixed in a ratio of (second material):(third material)=a1:(1-a1) [unit: mol], where a1 is preferably greater than 0.2 and less than 0.9, and more preferably greater than 0.3 and less than 0.8.
[0337] Furthermore, it is preferable that the first material and the second material are mixed in a ratio of (first material):(second material)=1:b1 [unit: mol], and b1 is preferably 0.001 or more and 0.2 or less.
[0338] Next, an annealing step is performed to obtain the negative electrode active material of one embodiment of the present invention.
[0339] The annealing step is preferably performed in a reducing atmosphere because it can suppress oxidation of the surface of the first material and reaction between the first material and oxygen. The reducing atmosphere may be, for example, a nitrogen atmosphere or a rare gas atmosphere. Alternatively, a mixture of two or more types of nitrogen and rare gas may be used. Heating may also be performed under reduced pressure.
[0340] The melting point of the second material is M 2 When expressed as [K], the heating temperature is, for example, (M 2 -550) [K] higher (M 2 +50) [K], and (M 2 -400) [K] or more (M 2 ) [K] or less is more preferable.
[0341] Furthermore, solid-state diffusion of a compound is likely to occur at temperatures equal to or higher than the Tammann temperature. For example, the Tammann temperature is 0.757 times the melting point of an oxide. Therefore, for example, the heating temperature is preferably 0.757 times the eutectic point or higher, or a temperature close to that temperature.
[0342] Furthermore, in the case of lithium fluoride, a representative example of a material containing a halogen, the amount of evaporation increases rapidly above the melting point, so for example, the heating temperature is preferably below the melting point of the material containing a halogen.
[0343] The eutectic point of the second material and the third material is M 23 When expressed as [K], the heating temperature is, for example, (M 23 ×0.7) [K] higher (M 2 +50) [K], and (M 23 ×0.75) [K] or more (M 2 +20) [K] or less, and (M 23 ×0.75) [K] or more (M 2 +20) [K] or less, and M 23 [K] higher (M 2 +10) [K], and (M 23 ×0.8) [K] or more M 2 [K] or less is more preferable, and (M 23 ) [K] or more M 2 It is more preferable that it is [K] or less.
[0344] When lithium fluoride is used as the second material and lithium carbonate is used as the third material, the heating temperature is, for example, preferably higher than 350°C and lower than 900°C, more preferably 390°C or higher and 850°C or lower, even more preferably 520°C or higher and 910°C or lower, still more preferably 570°C or higher and 860°C or lower, and still more preferably 610°C or higher and 860°C or lower.
[0345] The heating time is, for example, preferably 1 hour or more and 60 hours or less, and more preferably 3 hours or more and 20 hours or less.
[0346] 8A, 8B, 8C, and 8D show examples of cross sections of negative electrode active material 400. FIG.
[0347] By exposing a cross section of the negative electrode active material 400 by processing, the cross section can be observed and analyzed.
[0348] 8A has a region 401 and a region 402. The region 402 is located outside the region 401. The region 402 is preferably in contact with the surface of the region 401.
[0349] At least a portion of the region 402 preferably includes the surface of the negative electrode active material 400 .
[0350] The region 401 is, for example, a region including the inside of the negative electrode active material 400 .
[0351] Region 401 contains the first material described above. Region 402 contains, for example, element Z, oxygen, carbon, metal A1, and metal A2. Element Z is, for example, fluorine, chlorine, etc. Note that region 402 may not contain some of element Z, oxygen, carbon, metal A1, and metal A2. Alternatively, the concentration of some of element Z, oxygen, carbon, metal A1, and metal A2 in region 402 may be so low that they cannot be detected by analysis.
[0352] The region 402 may be referred to as a surface layer portion of the negative electrode active material 400 .
[0353] The negative electrode active material 400 may have various forms, such as a single particle, an aggregate of a plurality of particles, or a thin film.
[0354] The region 401 may be a particle of the first material, or an aggregate of a plurality of particles of the first material, or a thin film of the first material.
[0355] The region 402 may be a part of a particle. For example, the region 402 may be the surface layer of a particle. Alternatively, the region 402 may be a part of a thin film. For example, the region 402 may be the upper layer of a thin film.
[0356] Region 402 may be a coating layer formed on the surface of a particle.
[0357] Furthermore, the region 402 may be a region having a bond between an element constituting the first material and the element Z. For example, the surface of the first material may be modified with the element Z or a functional group having the element Z at the region 402 or the interface between the region 401 and the region 402. Therefore, in the negative electrode active material of one embodiment of the present invention, a bond between an element constituting the first material and the element Z may be observed. For example, when the first material is graphite and the element Z is fluorine, a C—F bond may be observed. For example, when the first material contains silicon and the element Z is fluorine, a Si—F bond may be observed.
[0358] For example, when graphite is used as the first material, region 401 is a graphite particle and region 402 is a coating layer of the graphite particle. Alternatively, when graphite is used as the first material, region 401 is a region including the inside of the graphite particle and region 402 is a surface layer of the graphite particle.
[0359] The region 402 has, for example, a bond between the element Z and carbon. The region 402 also has, for example, a bond between the element Z and a metal A1. The region 402 also has, for example, a carbonate group.
[0360] When analyzing the negative electrode active material 400 by X-ray photoelectron spectroscopy (XPS), it is preferable to detect element Z, and element Z is preferably detected at a concentration of 1 atomic % or more. In this case, the concentration of element Z can be calculated, for example, assuming that the sum of the concentrations of carbon, oxygen, metal A1, metal A2, and element Z is 100%. Alternatively, the concentration of element Z may be calculated by adding the concentration of nitrogen to the concentrations of these elements to 100%. Furthermore, the concentration of element Z is, for example, 60 atomic % or less, or, for example, 30 atomic % or less.
[0361] When analyzing the negative electrode active material 400 by XPS, it is preferable to detect a peak resulting from a bond between the element Z and carbon. Alternatively, a peak resulting from a bond between the element Z and metal A1 may be detected.
[0362] When element Z is fluorine and metal A1 is lithium, in the XPS F1s spectrum, a peak suggesting a carbon-fluorine bond (hereinafter referred to as peak F2) is observed at a position near 688 eV, for example, in an energy range higher than 686.5 eV and lower than 689.5 eV, and a peak suggesting a lithium-fluorine bond (hereinafter referred to as peak F1) is observed at a position near 685 eV, for example, in an energy range higher than 683.5 eV and lower than 686.5 eV. The intensity of peak F2 is preferably more than 0.1 times but less than 10 times the intensity of peak F1, for example, 0.3 times or more but 3 times or less.
[0363] When analyzing the negative electrode active material 400 by XPS, it is preferable that a peak corresponding to a carbonate or a carbonate group is observed. In the XPS C1s spectrum, the peak corresponding to a carbonate or a carbonate group is observed at a peak position near 290 eV, for example, in an energy range higher than 288.5 eV and lower than 291.5 eV.
[0364] In addition, when the negative electrode active material 400 is analyzed by XRD, Li, which is represented by the space group Fm-3m, 2 Spectra due to O may be observed.
[0365] In the example shown in Fig. 8B, region 401 has an area that is not covered by region 402. In the example shown in Fig. 8C, region 402 that covers the recessed area on the surface of region 401 has a large thickness.
[0366] 8D , region 401 includes regions 401a and 401b. Region 401a includes the interior of region 401, and region 401b is located outside region 401a. Region 401b is preferably in contact with region 402.
[0367] The region 401 b is the surface layer of the region 401 .
[0368] Region 401b contains one or more of element Z, oxygen, carbon, metal A1, and metal A2 contained in region 402. Furthermore, in region 401b, the elements contained in region 402, such as element Z, oxygen, carbon, metal A1, and metal A2, may have a concentration gradient in which the concentration gradually decreases from the surface or near the surface toward the interior.
[0369] The concentration of element Z in region 401b is higher than the concentration of element Z in region 401a. In addition, the concentration of element Z in region 401b is preferably lower than the concentration of element Z in region 402.
[0370] The oxygen concentration in the region 401b may be higher than the oxygen concentration in the region 401a, and may be lower than the oxygen concentration in the region 402.
[0371] When the negative electrode active material of one embodiment of the present invention is measured by energy dispersive X-ray spectroscopy using a scanning electron microscope, it is preferable to detect the element Z. Furthermore, the concentration of the element Z is preferably 10 atomic % to 70 atomic % when the total concentration of the element Z and oxygen is 100 atomic %.
[0372] The region 402 has a thickness of, for example, 50 nm or less, more preferably 1 nm or more and 35 nm or less, and even more preferably 5 nm or more and 20 nm or less.
[0373] The region 401b has a thickness of, for example, 50 nm or less, more preferably 1 nm or more and 35 nm or less, and even more preferably 5 nm or more and 20 nm or less.
[0374] When fluorine is used as element Z and lithium is used as metal A1 and metal A2, region 402 may have a region covered with a region having lithium fluoride and a region covered with a region having lithium carbonate relative to region 401. Furthermore, region 402 does not inhibit the insertion and extraction of lithium, and therefore an excellent secondary battery can be realized without deteriorating the output characteristics, etc., of the secondary battery.
[0375] This embodiment mode can be combined with the descriptions of other embodiment modes as appropriate.
[0376] In this embodiment, an example of a secondary battery of one embodiment of the present invention will be described with reference to Fig. 9. The secondary battery includes an outer casing (not shown), a positive electrode 503, a negative electrode 506, a separator 507, and an electrolyte in which a lithium salt or the like is dissolved. The separator 507 is provided between the positive electrode 503 and the negative electrode 506.
[0377] A positive electrode of one embodiment of the present invention includes a positive electrode active material layer. The positive electrode active material layer includes a positive electrode active material. The positive electrode active material layer may include a conductive agent, a binder, or the like. The positive electrode of one embodiment of the present invention preferably includes a current collector, and the positive electrode active material layer is preferably provided over the current collector.
[0378] 9A , a positive electrode 503 includes a positive electrode active material layer 502 and a positive electrode current collector 501. The positive electrode active material layer 502 includes a positive electrode active material 561, a conductive additive, and a binder. Fig. 9B shows an enlarged view of a region surrounded by a dashed line as a region 502a in Fig. 9A as an enlarged view of a portion of the positive electrode active material layer 502. Fig. 9B illustrates an example in which acetylene black 553 and graphene 554 are used as conductive additives.
[0379] A negative electrode of one embodiment of the present invention includes a negative electrode active material layer. The negative electrode active material layer includes a negative electrode active material. The negative electrode active material layer may include a conductive agent, a binder, or the like. The negative electrode of one embodiment of the present invention preferably includes a current collector, and the negative electrode active material layer is preferably provided over the current collector.
[0380] The negative electrode 506 includes a negative electrode active material layer 505 and a negative electrode current collector 504. The negative electrode active material layer 505 includes a negative electrode active material 563, a conductive additive, and a binder. Fig. 9B shows an enlarged view of a region surrounded by a dashed line as region 505a in Fig. 9A as an enlarged view of part of the negative electrode active material layer 505. Fig. 9D shows an example in which acetylene black 556 and graphene 557 are used as conductive additives.
[0381] The conductive agent may be a carbon material, a metal material, a conductive ceramic material, or the like. Alternatively, a fibrous material may be used as the conductive agent. The content of the conductive agent relative to the total amount of the active material layer is preferably 1 wt % to 10 wt %, more preferably 1 wt % to 5 wt %.
[0382] The conductive agent can form an electrically conductive network in the active material layer. The conductive agent can maintain electrical conduction paths between active materials. By adding the conductive agent to the active material layer, an active material layer with high electrical conductivity can be realized.
[0383] The conductive agent may be a graphene compound, natural graphite, artificial graphite such as mesocarbon microbeads, or carbon fiber.
[0384] Examples of usable carbon fibers include mesophase pitch-based carbon fibers and isotropic pitch-based carbon fibers. Examples of usable carbon fibers include carbon nanofibers and carbon nanotubes. Carbon nanotubes can be produced, for example, by vapor phase growth. Examples of usable conductive agents include carbon materials such as carbon black (e.g., acetylene black (AB)), graphite particles, graphene, and fullerene. Examples of usable conductive agents include metal powders, metal fibers, and conductive ceramic materials, such as copper, nickel, aluminum, silver, and gold.
[0385] [Graphene Compound] In this specification and the like, graphene compounds include graphene, multilayer graphene, multigraphene, graphene oxide, multilayer graphene oxide, multi-graphene oxide, reduced graphene oxide, reduced multilayer graphene oxide, reduced multi-graphene oxide, graphene quantum dots, and the like. Graphene compounds contain carbon, have a shape such as a plate or sheet, and have a two-dimensional structure formed by six-membered carbon rings. The two-dimensional structure formed by six-membered carbon rings may also be referred to as a carbon sheet. Graphene compounds may have functional groups. Furthermore, graphene compounds preferably have a curved shape. Furthermore, graphene compounds may be rolled up to resemble carbon nanofibers.
[0386] As the conductive agent, the above-mentioned materials can be used in combination.
[0387] In this specification and the like, graphene oxide refers to a material that contains carbon and oxygen, has a sheet shape, and has a functional group, in particular, an epoxy group, a carboxy group, or a hydroxy group.
[0388] In this specification, reduced graphene oxide refers to a material containing carbon and oxygen, having a sheet-like shape, and having a two-dimensional structure formed by six-membered carbon rings. It may also be called a carbon sheet. A single reduced graphene oxide can function, but multiple sheets may be stacked. Reduced graphene oxide preferably has a portion where the carbon concentration is greater than 80 atomic % and the oxygen concentration is 2 atomic % or more and 15 atomic % or less. By achieving these carbon and oxygen concentrations, even a small amount can function as a highly conductive conductive agent. Furthermore, reduced graphene oxide preferably has an intensity ratio G / D between the G band and the D band in a Raman spectrum of 1 or more. Reduced graphene oxide with such an intensity ratio can function as a highly conductive conductive agent even in a small amount.
[0389] In the longitudinal section of the active material layer, the sheet-like graphene compound is dispersed substantially uniformly in the inner region of the active material layer. The plurality of graphene compounds are formed so as to partially cover the plurality of granular active material particles or to be attached to the surfaces of the plurality of granular active material particles, and are in surface contact with each other.
[0390] Here, a plurality of graphene compounds are bonded together to form a mesh-like graphene compound sheet (hereinafter referred to as a graphene compound net or graphene net). When an active material is covered with a graphene net, the graphene net can also function as a binder that binds the active materials together. Therefore, the amount of binder can be reduced or no binder can be used, thereby improving the ratio of the active material to the electrode volume and electrode weight. In other words, the charge / discharge capacity of a secondary battery can be increased.
[0391] Here, it is preferable to use graphene oxide as the graphene compound, mix it with an active material to form a layer that will become the active material layer, and then reduce it. That is, the completed active material layer preferably contains reduced graphene oxide. By using graphene oxide, which has extremely high dispersibility in polar solvents, to form the graphene compound, it is possible to substantially uniformly disperse the graphene compound in the internal region of the active material layer. The solvent is volatilized and removed from the dispersion medium containing uniformly dispersed graphene oxide, and the graphene oxide is reduced. The graphene compounds remaining in the active material layer partially overlap and are dispersed to the extent that they are in surface contact with each other, thereby forming three-dimensional conductive paths. The reduction of graphene oxide may be performed, for example, by heat treatment or using a reducing agent. Unlike granular conductive agents such as acetylene black, which form point contact with the active material, graphene compounds enable surface contact with low contact resistance, and therefore can improve electrical conductivity within the electrode with a smaller amount than conventional conductive agents. This allows for an increased proportion of active material in the active material layer, thereby increasing the discharge capacity of the secondary battery.
[0392] [Binder] As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Furthermore, as the binder, fluororubber can be used.
[0393] Furthermore, it is preferable to use, for example, a water-soluble polymer as the binder. Examples of the water-soluble polymer that can be used include polysaccharides. Examples of the polysaccharide that can be used include one or more selected from cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, and regenerated cellulose, as well as starch. It is even more preferable to use these water-soluble polymers in combination with the rubber material described above.
[0394] Alternatively, it is preferable to use, as the binder, materials such as polystyrene, polymethyl acrylate, polymethyl methacrylate (polymethyl methacrylate, PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, and nitrocellulose.
[0395] The binder may be used in combination with two or more of the above.
[0396] For example, a material with particularly excellent viscosity adjusting effect may be used in combination with other materials. For example, while rubber materials have excellent adhesive strength and elasticity, it may be difficult to adjust the viscosity when mixed with a solvent. In such cases, it is preferable to mix them with a material with particularly excellent viscosity adjusting effect. For example, a water-soluble polymer may be used as a material with particularly excellent viscosity adjusting effect. Furthermore, as a water-soluble polymer with particularly excellent viscosity adjusting effect, one or more selected from the aforementioned polysaccharides, for example, carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, and diacetyl cellulose, cellulose derivatives such as regenerated cellulose, and starch may be used.
[0397] In addition, the solubility of cellulose derivatives such as carboxymethyl cellulose can be increased by converting them into salts such as sodium or ammonium salts of carboxymethyl cellulose, making them more effective as viscosity adjusters. Higher solubility can also improve dispersibility with the active material and other components when preparing electrode slurry. In this specification, the cellulose and cellulose derivatives used as electrode binders also include their salts.
[0398] Water-soluble polymers stabilize viscosity by dissolving in water and can stably disperse active materials and other materials combined as binders, such as styrene-butadiene rubber, in aqueous solutions. Furthermore, because they contain functional groups, they are expected to be easily and stably adsorbed onto the surface of active materials. Furthermore, many cellulose derivatives, such as carboxymethyl cellulose, contain functional groups, such as hydroxyl and carboxyl groups, and because of these functional groups, the polymers are expected to interact with each other and widely cover the surface of the active material.
[0399] When the binder covering or contacting the surface of the active material forms a film, it is expected to function as a passive film and suppress the decomposition of the electrolyte. Here, the passive film is a film with no electrical conductivity or a film with extremely low electrical conductivity. For example, when a passive film is formed on the surface of the active material, it can suppress the decomposition of the electrolyte at the battery reaction potential. Furthermore, it is more desirable that the passive film suppresses electrical conductivity while still allowing lithium ions to conduct.
[0400] The active material layer can be produced by mixing an active material, a binder, a conductive additive and a solvent to prepare a slurry, forming the slurry on a current collector, and volatilizing the solvent.
[0401] The solvent used for the slurry is preferably a polar solvent, such as water, methanol, ethanol, acetone, tetrahydrofuran (THF), dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO), or a mixture of two or more of these.
[0402] [Current Collector] The positive electrode current collector and the negative electrode current collector can be made of a highly conductive material that does not alloy with carrier ions such as lithium, such as metals such as stainless steel, gold, platinum, zinc, iron, copper, aluminum, and titanium, and alloys thereof. Aluminum alloys containing elements that improve heat resistance, such as silicon, titanium, neodymium, scandium, and molybdenum, can also be used. They may also be made of a metal element that reacts with silicon to form a silicide. Examples of metal elements that react with silicon to form a silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel. The current collector can be in a sheet, mesh, punched metal, expanded metal, or other shape. It is preferable to use a current collector with a thickness of 10 μm to 30 μm.
[0403] The negative electrode current collector is preferably made of a material that does not alloy with carrier ions such as lithium.
[0404] A titanium compound may be provided as a current collector by being laminated on the metal element shown above. Examples of titanium compounds include titanium nitride, titanium oxide, titanium nitride in which part of the nitrogen is substituted with oxygen, titanium oxide in which part of the oxygen is substituted with nitrogen, and titanium oxynitride (TiO x N y , 0 < x < 2, 0 < y < 1), or a mixture or stack of two or more of these can be used. Among these, titanium nitride is particularly preferred because of its high conductivity and excellent oxidation suppression function. By providing a titanium compound on the surface of the current collector, for example, reaction between the material of the active material layer formed on the current collector and metal can be suppressed. When the active material layer contains a compound containing oxygen, oxidation reaction between the metal element and oxygen can be suppressed. For example, when aluminum is used as the current collector and the active material layer is formed using graphene oxide described below, oxidation reaction between oxygen in graphene oxide and aluminum may be a concern. In such a case, providing a titanium compound on aluminum can suppress oxidation reaction between the current collector and graphene oxide.
[0405] As the graphene 554 and the graphene 557, graphene or a graphene compound can be used.
[0406] In this specification and the like, graphene compounds include multilayer graphene, multigraphene, graphene oxide, multilayer graphene oxide, multi-graphene oxide, reduced graphene oxide, reduced multilayer graphene oxide, reduced multi-graphene oxide, graphene quantum dots, etc. Graphene compounds contain carbon, have a shape such as a plate or sheet, and have a two-dimensional structure formed by six-membered carbon rings. The two-dimensional structure formed by six-membered carbon rings may also be called a carbon sheet. Graphene compounds may have functional groups. Furthermore, graphene compounds preferably have a curved shape. Furthermore, graphene compounds may be rolled up to resemble carbon nanofibers.
[0407] In the positive electrode or negative electrode of one embodiment of the present invention, graphene or a graphene compound can function as a conductive agent. Multiple graphenes or graphene compounds can form three-dimensional conductive paths in the positive electrode or negative electrode, thereby increasing the conductivity of the positive electrode or negative electrode. Furthermore, graphene or a graphene compound can cling to particles in the positive electrode or negative electrode, thereby suppressing particle collapse in the positive electrode or negative electrode and increasing the strength of the positive electrode or negative electrode. Graphene or a graphene compound has a thin sheet shape and can form an excellent conductive path even when its volume in the positive electrode or negative electrode is small. This allows the volume of the active material in the positive electrode or negative electrode to be increased. Therefore, the capacity of a secondary battery can be increased.
[0408] [Separator] The separator 507 may be made of, for example, paper, nonwoven fabric, glass fiber, ceramics, etc. Alternatively, it may be made of nylon (polyamide), vinylon (polyvinyl alcohol fiber), polyester, acrylic, polyolefin, polyurethane, polypropylene, polyethylene, etc. The separator is preferably processed into an envelope shape and disposed so as to encase either the positive electrode or the negative electrode.
[0409] Furthermore, a polymer film containing, for example, polypropylene, polyethylene, polyimide, etc. can be used for the separator 507. Polyimide has good wettability with ionic liquids, and may be a more preferable material for the separator 507 in some cases.
[0410] Polymer films containing polypropylene, polyethylene, etc. can be produced by either the dry method or the wet method. The dry method involves heating and stretching a polymer film containing polypropylene, polyethylene, polyimide, etc., to create gaps between the crystals and create fine holes. The wet method involves mixing a solvent into the resin beforehand, forming it into a film, and then extracting the solvent to create holes.
[0411] The left diagram in Figure 9C shows an enlarged view of region 507a as an example of separator 507 (produced by a wet method). In this example, a structure in which multiple holes 582 are formed in polymer film 581 is shown. The right diagram in Figure 9C shows an enlarged view of region 507b as another example of separator 507 (produced by a dry method). In this example, a structure in which multiple holes 585 are formed in polymer film 584 is shown.
[0412] The pore diameter of the separator may differ between the surface layer portion of the surface facing the positive electrode and the surface layer portion of the surface facing the negative electrode after charge and discharge. In this specification, the surface layer portion of the separator is preferably, for example, a region within 5 μm, more preferably within 3 μm, from the surface.
[0413] The separator may have a multi-layer structure, for example, a structure in which two types of polymer materials are laminated.
[0414] Alternatively, a structure can be used in which a ceramic material, a fluorine material, a polyamide material, or a mixture thereof is coated on a polymer film having, for example, polypropylene, polyethylene, polyimide, etc. Alternatively, a structure can be used in which a ceramic material, a fluorine material, a polyamide material, or a mixture thereof is coated on a nonwoven fabric, for example. Polyimide has good wettability with ionic liquids and may be more preferable as a coating material.
[0415] As the fluorine-based material, for example, PVdF, polytetrafluoroethylene, etc. can be used.
[0416] Examples of polyamide-based materials that can be used include nylon and aramid (meta-aramid, para-aramid).
[0417] [Exterior Body] The exterior body of the secondary battery can be made of one or more materials selected from a metal material such as aluminum and a resin material. A film-like exterior body can also be used. Examples of the film include a three-layer structure film in which a thin, flexible metal film such as aluminum, stainless steel, copper, or nickel is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, or polyamide, and an insulating synthetic resin film such as a polyamide resin or polyester resin is further provided on the thin metal film as the outer surface of the exterior body.
[0418] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0419] Embodiment Mode 3 In this embodiment mode, a method for manufacturing a secondary battery will be described.
[0420] <Method 1 for manufacturing laminated secondary battery> Here, an example of a method for manufacturing a laminated secondary battery whose external views are shown in Figures 10A and 10B will be described with reference to Figures 11A and 11B and Figures 12A and 12B. A secondary battery 500 shown in Figures 10A and 10B has a positive electrode 503, a negative electrode 506, a separator 507, an outer casing 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511. Note that, as a cross-sectional view of the laminated secondary battery shown in Figure 10A etc., for example, a structure in which a positive electrode, a separator, and a negative electrode are stacked and surrounded by an outer casing can be used, as shown in Figure 15 described later.
[0421] First, a positive electrode 503, a negative electrode 506, and a separator 507 are prepared. Fig. 11A shows an example of the positive electrode 503 and the negative electrode 506. The positive electrode 503 has a positive electrode active material layer 502 on a positive electrode current collector 501. The positive electrode 503 preferably has a tab region where the positive electrode current collector 501 is exposed. The negative electrode 506 has a negative electrode active material layer 505 on a negative electrode current collector 504. The negative electrode 506 preferably has a tab region where the negative electrode current collector 504 is exposed.
[0422] Next, negative electrodes 506, separators 507, and positive electrodes 503 are stacked. Fig. 11B shows the stacked negative electrodes 506, separators 507, and positive electrodes 503. Here, an example is shown in which five pairs of negative electrodes and four pairs of positive electrodes are used. This can also be called a stack consisting of negative electrodes, separators, and positive electrodes.
[0423] Next, the tab regions of the positive electrode 503 are joined together, and the positive electrode lead electrode 510 is joined to the tab region of the outermost positive electrode. For example, ultrasonic welding or the like may be used for joining. Similarly, the tab regions of the negative electrode 506 are joined together, and the negative electrode lead electrode 511 is joined to the tab region of the outermost negative electrode.
[0424] Next, the negative electrode 506 , the separator 507 and the positive electrode 503 are arranged on the outer casing 509 .
[0425] Next, as shown in Fig. 12A, the exterior body 509 is folded at the portion indicated by the dashed line. Thereafter, the outer periphery of the exterior body 509 is joined. For example, thermocompression bonding or the like may be used for joining. At this time, an area (hereinafter referred to as an inlet 516) that is not joined is provided in a part (or one side) of the exterior body 509 so that the electrolyte 508 can be introduced later.
[0426] Next, as shown in Fig. 12B, the electrolyte 508 is introduced into the inside of the exterior body 509 through an inlet 516 provided in the exterior body 509. The introduction of the electrolyte 508 is preferably performed under a reduced pressure atmosphere or an inert atmosphere. Finally, the inlet 516 is joined. In this manner, the laminated secondary battery 500 can be fabricated.
[0427] In the above, the positive electrode lead electrode 510 and the negative electrode lead electrode 511 are led out of the exterior of the outer casing from the same side to produce the secondary battery 500 shown in Fig. 10A. The positive electrode lead electrode 510 and the negative electrode lead electrode 511 can also be led out of the exterior of the outer casing from opposite sides to produce the secondary battery 500 shown in Fig. 10B.
[0428] <Method 2 for Manufacturing Laminated Secondary Battery> Next, an example of a method for manufacturing a laminated secondary battery 600 whose external view is shown in Fig. 13 will be described with reference to Fig. 14, Fig. 15, Fig. 16A to Fig. 16D, and Fig. 17A to Fig. 17F. The secondary battery 600 shown in Fig. 13 has a positive electrode 503, a negative electrode 506, a separator 507, an outer casing 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511. The outer casing 509 is sealed in a region 514.
[0429] The laminated secondary battery 600 can be fabricated using, for example, the manufacturing apparatus shown in FIG. 14 . The manufacturing apparatus 570 shown in FIG. 14 includes a material input chamber 571, a transfer chamber 572, a treatment chamber 573, and a material removal chamber 576. Each chamber can be connected to various exhaust mechanisms depending on the intended use. Each chamber can also be connected to various gas supply mechanisms depending on the intended use. To prevent impurities from entering the manufacturing apparatus 570, an inert gas is preferably supplied to the manufacturing apparatus 570. The gas supplied to the manufacturing apparatus 570 is preferably highly purified using a gas purifier before being introduced into the manufacturing apparatus 570. The material input chamber 571 is a chamber for loading a positive electrode, a separator, a negative electrode, an outer casing, and the like into the manufacturing apparatus 570. The transfer chamber 572 includes a transfer mechanism 580. The treatment chamber 573 includes a stage and an electrolyte dripping mechanism. The component removal chamber 576 is a chamber for removing the fabricated secondary battery to the outside of the manufacturing apparatus 570 .
[0430] The laminated secondary battery 600 is fabricated as follows.
[0431] First, an exterior body 509b is placed on a stage 591 of a processing chamber 573, and then a positive electrode 503 is placed on the exterior body 509b ( FIGS. 16A and 16B ). Next, an electrolyte 515a is dropped onto the positive electrode 503 from a nozzle 594 ( FIGS. 16C and 16D ). FIG. 16D is a cross section corresponding to the dashed-dotted line A-B in FIG. 16C . Note that the illustration of the stage 591 may be omitted to avoid cluttering the drawings. The dropping method may be, for example, any one of a dispensing method, a spray method, an inkjet method, or the like. The electrolyte may be dropped using an ODF (One Drop Fill) method.
[0432] By moving the nozzle 594, the electrolyte 515a can be dropped over the entire surface of the positive electrode 503. Alternatively, by moving the stage 591, the electrolyte 515a may be dropped over the entire surface of the positive electrode 503.
[0433] The electrolyte is preferably dropped from a position whose shortest distance from the receiving surface is greater than 0 mm and equal to or less than 1 mm.
[0434] It is also preferable to appropriately adjust the viscosity of the electrolyte dropped from a nozzle, etc. The electrolyte can be dropped from a nozzle if the viscosity of the entire electrolyte is within the range of 0.3 mPa·s to 1000 mPa·s at room temperature (25°C).
[0435] In addition, since the viscosity of the electrolyte changes depending on the temperature of the electrolyte, it is preferable to appropriately adjust the temperature of the electrolyte to be dropped. The temperature of the electrolyte is preferably equal to or higher than the melting point and equal to or lower than the boiling point or flash point of the electrolyte.
[0436] Next, a separator 507 is placed on the positive electrode 503 so as to overlap one entire surface of the positive electrode 503 ( FIG. 17A ). Subsequently, an electrolyte 515b is dripped onto the separator 507 using a nozzle 594 ( FIG. 17B ). Thereafter, a negative electrode 506 is placed on the separator 507 ( FIG. 17C ). The negative electrode 506 is placed on top of the separator 507 so as not to protrude from the separator 507 in a top view. Subsequently, an electrolyte 515c is dripped onto the negative electrode 506 using a nozzle 594 ( FIG. 17D ). Thereafter, the stack of the positive electrode 503, the separator 507, and the negative electrode 506 is further stacked to produce the stack 512 shown in FIG. 15 . Next, the positive electrode 503, the separator 507, and the negative electrode 506 are sealed with an exterior body 509a and an exterior body 509b ( FIGS. 17E and 17F ).
[0437] In FIG. 15 , the positive electrode and the negative electrode are arranged such that the positive electrode active material layer and the negative electrode active material layer sandwich a separator. Note that in a secondary battery according to one embodiment of the present invention, it is preferable that the negative electrode active material layer has few or no regions that do not face the positive electrode active material layer. When the electrolyte contains an ionic liquid and the negative electrode active material layer has regions that do not face the positive electrode active material layer, the charge / discharge efficiency of the secondary battery may decrease. Therefore, in a secondary battery according to one embodiment of the present invention, for example, it is preferable that the edge of the positive electrode active material layer and the edge of the negative electrode active material layer are as aligned as possible. Therefore, it is preferable that the areas of the positive electrode active material layer and the negative electrode active material layer are aligned as much as possible when viewed from above. Alternatively, it is preferable that the edge of the positive electrode active material layer is located more inward than the edge of the negative electrode active material layer.
[0438] Multiple laminates 512 can be obtained by arranging multiple laminates 512 on exterior body 509b. After sealing exterior bodies 509a and 509b at region 514 so as to surround the active material layer, each laminate 512 is cut outside region 514, thereby separating the multiple secondary batteries into individual ones.
[0439] During sealing, first, a frame-shaped resin layer 513 is formed on the exterior body 509b. Next, at least a portion of the resin layer 513 is irradiated with light under reduced pressure to harden at least a portion of the resin layer 513. Next, sealing is performed in the region 514 by thermocompression bonding or welding under atmospheric pressure. Alternatively, only sealing by thermocompression bonding or welding may be performed without performing the above-described sealing by light irradiation.
[0440] Although Figure 13 shows an example in which the exterior body 509 is sealed on all four sides (sometimes called four-sided sealing), it may also be sealed on three sides (sometimes called three-sided sealing) as shown in Figures 10A and 10B.
[0441] Through the above steps, the laminated secondary battery 600 can be fabricated.
[0442] <Another Secondary Battery and Manufacturing Method 1> An example of a cross-sectional view of a stack of one embodiment of the present invention is shown in Fig. 18. A stack 550 shown in Fig. 18 is manufactured by placing one separator between a positive electrode and a negative electrode while folding the separator.
[0443] In the laminate 550, one separator 507 is folded multiple times so as to be sandwiched between the positive electrode active material layers 502 and the negative electrode active material layers 505. In Fig. 18, six layers of positive electrodes 503 and six layers of negative electrodes 506 are stacked, and therefore the separator 507 is folded at least five times. The separator 507 may not only be provided so as to be sandwiched between the positive electrode active material layers 502 and the negative electrode active material layers 505, but also may have its extending portion further folded so as to bind the multiple positive electrodes 503 and negative electrodes 506 together with tape or the like.
[0444] In the method for manufacturing a secondary battery of one embodiment of the present invention, after the positive electrode 503 is disposed, an electrolyte can be dropped onto the positive electrode 503. Similarly, after the negative electrode 506 is disposed, an electrolyte can be dropped onto the negative electrode 506. Furthermore, in the method for manufacturing a secondary battery of one embodiment of the present invention, an electrolyte can be dropped onto the separator 507 before folding the separator or after folding the separator 507 and overlapping it with the negative electrode 506 or the positive electrode 503. By dropping the electrolyte onto at least one of the negative electrode 506, the separator 507, and the positive electrode 503, the negative electrode 506, the separator 507, or the positive electrode 503 can be impregnated with the electrolyte.
[0445] 19A has a stack 972 inside a housing 971. A terminal 973b and a terminal 974b are electrically connected to the stack 972. At least a portion of the terminal 973b and at least a portion of the terminal 974b are exposed to the outside of the housing 971.
[0446] The stack body 972 can have a structure in which a positive electrode, a negative electrode, and a separator are stacked. Alternatively, the stack body 972 can have a structure in which a positive electrode, a negative electrode, and a separator are wound, or the like.
[0447] For example, the laminate 972 may be a laminate having a structure in which separators are folded back as shown in FIG.
[0448] An example of a method for manufacturing the stacked body 972 will be described with reference to FIGS. 19B and 19C.
[0449] First, as shown in FIG. 19B , a strip-shaped separator 976 is placed on top of a positive electrode 975a, and then a negative electrode 977a is placed on top of the positive electrode 975a with the separator 976 sandwiched between them. The separator 976 is then folded back and placed on top of the negative electrode 977a. Next, as shown in FIG. 19C , a positive electrode 975b is placed on top of the negative electrode 977a with the separator 976 sandwiched between them. In this way, by folding back the separator and arranging the positive electrode and negative electrode in order, a stack 972 can be produced. A structure including a stack produced in this way is sometimes called a "zigzag structure."
[0450] Next, an example of a method for manufacturing the secondary battery 970 will be described with reference to FIGS. 20A to 20C.
[0451] 20A , a positive electrode lead electrode 973a is electrically connected to the positive electrode of the laminate 972. Specifically, for example, a tab region may be provided on each positive electrode of the laminate 972, and each tab region may be electrically connected to the positive electrode lead electrode 973a by welding or the like. In addition, a negative electrode lead electrode 974a is electrically connected to the negative electrode of the laminate 972.
[0452] One stack 972 or a plurality of stacks 972 may be arranged inside the housing 971. Fig. 20B shows an example in which two sets of stacks 972 are prepared.
[0453] Next, as shown in FIG. 20C , the prepared laminate 972 is housed in a housing 971, terminals 973b and 974b are attached, and the housing 971 is sealed. It is preferable that a conductor 973c is electrically connected to each positive electrode lead electrode 973a of the plurality of laminates 972. It is also preferable that a conductor 974c is electrically connected to each negative electrode lead electrode 974a of the plurality of laminates 972. The terminal 973b is electrically connected to the conductor 973c, and the terminal 974b is electrically connected to the conductor 974c. The conductor 973c may have a conductive region and an insulating region. The conductor 974c may have a conductive region and an insulating region.
[0454] A metal material (for example, aluminum) can be used for the housing 971. In the case where a metal material is used for the housing 971, the surface of the housing 971 is preferably covered with resin or the like. Alternatively, a resin material can be used for the housing 971.
[0455] It is preferable to provide a safety valve, an overcurrent protection element, or the like in the housing 971. The safety valve is a valve that releases gas when the pressure inside the housing 971 reaches a predetermined level in order to prevent the battery from exploding.
[0456] <Another Secondary Battery and Manufacturing Method 2> Fig. 21C shows an example of a cross-sectional view of a secondary battery of another embodiment of the present invention. A secondary battery 560 shown in Fig. 21C is manufactured using the stack 130 shown in Fig. 21A and the stack 131 shown in Fig. 21B. Note that for clarity, Fig. 21C only shows the stack 130, the stack 131, and the separator 507.
[0457] As shown in FIG. 21A , the laminate 130 includes a positive electrode 503 having positive electrode active material layers on both sides of a positive electrode current collector, a separator 507, a negative electrode 506 having negative electrode active material layers on both sides of a negative electrode current collector, the separator 507, and a positive electrode 503 having positive electrode active material layers on both sides of a positive electrode current collector laminated in this order.
[0458] As shown in FIG. 21B , the laminate 131 includes a negative electrode 506 having a negative electrode active material layer on both sides of a negative electrode current collector, a separator 507, a positive electrode 503 having a positive electrode active material layer on both sides of a positive electrode current collector, the separator 507, and a negative electrode 506 having a negative electrode active material layer on both sides of a negative electrode current collector laminated in this order.
[0459] The method for manufacturing a secondary battery according to one embodiment of the present invention can be applied to manufacturing a stack. Specifically, when the negative electrode 506, the separator 507, and the positive electrode 503 are stacked to manufacture a stack, an electrolyte is dropped onto at least one of the negative electrode 506, the separator 507, and the positive electrode 503. By dropping multiple drops of the electrolyte, the negative electrode 506, the separator 507, or the positive electrode 503 can be impregnated with the electrolyte.
[0460] As shown in FIG. 21C, the plurality of stacks 130 and the plurality of stacks 131 are covered with a wound separator 507 .
[0461] In addition, in the method for manufacturing a secondary battery of one embodiment of the present invention, after the stack 130 is arranged, an electrolyte can be dropped onto the stack 130. Similarly, after the stack 131 is arranged, an electrolyte can be dropped onto the stack 131. Furthermore, before the separator 507 is folded, or after the separator 507 is folded and overlapped with the stack, an electrolyte can be dropped onto the separator 507. By dropping multiple drops of the electrolyte, the stack 130, the stack 131, or the separator 507 can be impregnated with the electrolyte.
[0462] <Another Secondary Battery and Manufacturing Method 3> A secondary battery of another embodiment of the present invention will be described with reference to Fig. 22 and Fig. 23. The secondary battery described here can be called a wound secondary battery, or the like.
[0463] The secondary battery 913 shown in FIG. 22A has a wound body 950 provided with terminals 951 and 952 inside a housing 930. The wound body 950 is immersed in an electrolyte inside the housing 930. The terminal 952 contacts the housing 930, and the terminal 951 is not in contact with the housing 930 by using an insulating material or the like. Note that in FIG. 22A , for convenience, the housing 930 is shown separated, but in reality, the wound body 950 is covered by the housing 930, and the terminals 951 and 952 extend outside the housing 930. The housing 930 can be made of a metal material (e.g., aluminum) or a resin material.
[0464] 22B, the housing 930 shown in Fig. 22A may be formed from a plurality of materials. For example, the secondary battery 913 shown in Fig. 22B has a housing 930a and a housing 930b bonded together, and a wound body 950 is provided in the area surrounded by the housing 930a and the housing 930b.
[0465] The housing 930a can be made of an insulating material such as organic resin. In particular, by using a material such as organic resin on the surface on which the antenna is formed, it is possible to suppress shielding of the electric field by the secondary battery 913. Note that if the shielding of the electric field by the housing 930a is small, the antenna may be provided inside the housing 930a. The housing 930b can be made of, for example, a metal material.
[0466] 22C shows the structure of the wound body 950. The wound body 950 has a negative electrode 931, a positive electrode 932, and a separator 933. The wound body 950 is a wound body in which the negative electrode 931 and the positive electrode 932 are stacked on top of each other with the separator 933 sandwiched therebetween, and the laminated sheet is wound. Note that multiple layers of the negative electrode 931, the positive electrode 932, and the separator 933 may be stacked.
[0467] In a method for manufacturing a secondary battery according to one embodiment of the present invention, when the negative electrode 931, the separator 933, and the positive electrode 932 are stacked, an electrolyte is dropped onto at least one of the negative electrode 931, the separator 933, and the positive electrode 932. That is, the electrolyte is preferably dropped onto at least one of the negative electrode 931, the separator 933, and the positive electrode 932 before the laminate sheet is wound. By dropping multiple drops of the electrolyte, the negative electrode 931, the separator 933, or the positive electrode 932 can be impregnated with the electrolyte.
[0468] Alternatively, a secondary battery 913 may be provided that has a wound body 950a as shown in Fig. 23A. The wound body 950a shown in Fig. 23A has a negative electrode 931, a positive electrode 932, and a separator 933. The negative electrode 931 has a negative electrode active material layer 931a. The positive electrode 932 has a positive electrode active material layer 932a.
[0469] The separator 933 has a width wider than the negative electrode active material layer 931 a and the positive electrode active material layer 932 a, and is wound so as to overlap the negative electrode active material layer 931 a and the positive electrode active material layer 932 a. From the standpoint of safety, it is preferable that the negative electrode active material layer 931 a be wider than the positive electrode active material layer 932 a. A wound body 950 a having such a shape is preferable because of its high safety and productivity.
[0470] 23B, the negative electrode 931 is electrically connected to a terminal 951. The terminal 951 is electrically connected to a terminal 911a. The positive electrode 932 is electrically connected to a terminal 952. The terminal 952 is electrically connected to a terminal 911b.
[0471] 23C , the wound body 950a and the electrolyte are covered by the housing 930 to form the secondary battery 913. It is preferable to provide the housing 930 with a safety valve, an overcurrent protection element, etc. The safety valve opens temporarily only when the internal pressure of the housing 930 exceeds a predetermined value to prevent the battery from exploding.
[0472] 23B, the secondary battery 913 may have a plurality of wound bodies 950a. By using a plurality of wound bodies 950a, the secondary battery 913 can have a larger charge / discharge capacity.
[0473] [Coin-Type Secondary Battery] An example of a coin-type secondary battery will be described. Fig. 24A is an exploded perspective view of a coin-type (single-layer flat) secondary battery, Fig. 24B is an external view, and Fig. 24C is a cross-sectional view thereof. Coin-type secondary batteries are mainly used in small electronic devices.
[0474] 24A is a schematic diagram that shows the overlapping of components (upper and lower relationships and positional relationships) for ease of understanding. Therefore, FIGS. 24A and 24B are not completely identical corresponding views.
[0475] In Fig. 24A, a positive electrode 304, a separator 310, a negative electrode 307, a spacer 322, and a washer 312 are stacked. These are sealed by a negative electrode can 302 and a positive electrode can 301. Note that a gasket for sealing is not shown in Fig. 24A. The spacer 322 and the washer 312 are used to protect the inside or to fix the position inside the can when the positive electrode can 301 and the negative electrode can 302 are crimped together. The spacer 322 and the washer 312 are made of stainless steel or an insulating material.
[0476] A positive electrode 304 has a laminated structure in which a positive electrode active material layer 306 is formed on a positive electrode current collector 305 .
[0477] To prevent short-circuiting between the positive electrode and the negative electrode, a separator 310 and a ring-shaped insulator 313 are arranged so as to cover the side and top surfaces of the positive electrode 304. The separator 310 has a larger planar area than the positive electrode 304.
[0478] FIG. 24B is a perspective view of the completed coin-type secondary battery.
[0479] In the coin-type secondary battery 300, a positive electrode can 301, which also serves as a positive electrode terminal, and a negative electrode can 302, which also serves as a negative electrode terminal, are insulated and sealed by a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed by a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. The negative electrode 307 is formed by a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector. The negative electrode 307 is not limited to a laminated structure, and may be formed of lithium metal foil or a lithium-aluminum alloy foil.
[0480] It is to be noted that the positive electrode 304 and the negative electrode 307 used in the coin-type secondary battery 300 each only need to have an active material layer formed on one side.
[0481] The positive electrode can 301 and the negative electrode can 302 can be made of a material that is corrosion-resistant to the electrolyte. For example, metals such as nickel, aluminum, and titanium, alloys of these metals, or alloys of these metals with other metals (e.g., stainless steel) can be used. Furthermore, to prevent corrosion by the electrolyte, it is preferable to coat them with nickel, aluminum, or the like. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.
[0482] These negative electrode 307, positive electrode 304, and separator 310 are immersed in an electrolyte, and as shown in FIG. 24C , the positive electrode 304, separator 310, negative electrode 307, and negative electrode can 302 are stacked in this order with the positive electrode can 301 facing downwards, and the positive electrode can 301 and the negative electrode can 302 are crimped together via a gasket 303 to produce a coin-type secondary battery 300.
[0483] The secondary battery of one embodiment of the present invention can be the coin-type secondary battery 300 that has a large capacity, a large charge / discharge capacity, and excellent cycle characteristics. Note that the separator 310 may not be necessary in the secondary battery.
[0484] [Cylindrical Secondary Battery] An example of a cylindrical secondary battery will be described with reference to Fig. 25A . As shown in Fig. 25A , a cylindrical secondary battery 616 has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The battery can (external can) 602 is formed from a metal material and has excellent water barrier properties and gas barrier properties. The positive electrode cap 601 and the battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0485] 25B is a schematic diagram showing the cross section of a cylindrical secondary battery. The cylindrical secondary battery shown in Fig. 25B has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap and battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0486] A battery element is provided inside a hollow cylindrical battery can 602. The battery element is formed by winding a strip-shaped positive electrode 604 and a negative electrode 606 with a separator 605 sandwiched between them. Although not shown, the battery element is wound around a center pin. The battery can 602 is closed at one end and open at the other. The battery can 602 can be made of a material that is corrosion-resistant to the electrolyte. For example, metals such as nickel, aluminum, and titanium, alloys of these metals, or alloys of these metals with other metals (e.g., stainless steel, etc.) can be used. Furthermore, to prevent corrosion by the electrolyte, the battery can 602 is preferably coated with nickel, aluminum, or the like. Inside the battery can 602, the wound battery element, consisting of the positive electrode, negative electrode, and separator, is sandwiched between a pair of opposing insulating plates 608 and 609. An electrolyte (not shown) is injected into the battery can 602, where the battery element is provided. The electrolyte can be the same as that used in coin-type secondary batteries.
[0487] Since the positive and negative electrodes used in a cylindrical storage battery are wound up, it is preferable to form active materials on both sides of the current collector.
[0488] A positive electrode terminal (positive electrode current collector lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collector lead) 607 is connected to the negative electrode 606. Both the positive electrode terminal 603 and the negative electrode terminal 607 can be made of a metal material such as aluminum. The positive electrode terminal 603 is resistance-welded to a safety valve mechanism 613, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 613 is electrically connected to the positive electrode cap 601 via a PTC (Positive Temperature Coefficient) element 611. The safety valve mechanism 613 cuts off the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the increase in internal pressure of the battery exceeds a predetermined threshold. The PTC element 611 is a thermosensitive resistor whose resistance increases as the temperature increases, and the increased resistance limits the amount of current to prevent abnormal heat generation. The PTC element is made of barium titanate (BaTiO 3 )-based semiconductor ceramics, etc. can be used.
[0489] FIG. 25C shows an example of a power storage system 615. The power storage system 615 includes multiple secondary batteries 616. The positive electrodes of each secondary battery are electrically connected to a conductor 624 separated by an insulator 625. The conductor 624 is electrically connected to a control circuit 620 via wiring 623. The negative electrodes of each secondary battery are electrically connected to the control circuit 620 via wiring 626. The control circuit 620 may include a charge / discharge control circuit for charging and discharging, and a protection circuit for preventing overcharging or overdischarging. The control circuit 620 may have one or more functions, for example, controlling charging, controlling discharging, measuring charging voltage, measuring discharging voltage, measuring charging current, measuring discharging current, and measuring remaining capacity using integration of the charge. The control circuit 620 may also have one or more functions, for example, detecting overcharging, overdischarging, detecting charging overcurrent, and detecting discharging overcurrent. Based on these detection results, the control circuit 620 preferably has one or more functions, for example, stopping charging, stopping discharging, changing charging conditions, and changing discharging conditions.
[0490] 25D shows an example of a power storage system 615. The power storage system 615 has a plurality of secondary batteries 616, which are sandwiched between a conductive plate 628 and a conductive plate 614. The plurality of secondary batteries 616 are electrically connected to the conductive plate 628 and the conductive plate 614 by wiring 627. The plurality of secondary batteries 616 may be connected in parallel, in series, or in parallel and then further connected in series. By configuring the power storage system 615 to have a plurality of secondary batteries 616, it is possible to extract a large amount of power.
[0491]
[0492] A temperature control device may be provided between the multiple secondary batteries 616. When the secondary batteries 616 are overheated, they can be cooled by the temperature control device, and when the secondary batteries 616 are too cold, they can be heated by the temperature control device. This makes it difficult for the performance of the power storage system 615 to be affected by the outside air temperature.
[0493] 25D , the power storage system 615 is electrically connected to a control circuit 620 via wiring 621 and wiring 622. The wiring 621 is electrically connected to the positive electrodes of the plurality of secondary batteries 600 via a conductive plate 628, and the wiring 622 is electrically connected to the negative electrodes of the plurality of secondary batteries 600 via a conductive plate 614.
[0494] This embodiment mode can be combined with other embodiment modes as appropriate.
[0495] Embodiment 4 In this embodiment, application examples of a secondary battery of one embodiment of the present invention will be described with reference to FIGS.
[0496] [Vehicle] First, an example in which the secondary battery of one embodiment of the present invention is applied to an electric vehicle (EV) will be described.
[0497] 26C shows a block diagram of a vehicle having a motor. The electric vehicle is equipped with first batteries 1301a and 1301b as main driving secondary batteries, and a second battery 1311 that supplies power to an inverter 1312 that starts the motor 1304. The second battery 1311 is also called a cranking battery or starter battery. The second battery 1311 only needs to have high output, and does not need to have a large capacity, and the capacity of the second battery 1311 is smaller than that of the first batteries 1301a and 1301b.
[0498] For example, a secondary battery manufactured using a method for manufacturing a secondary battery according to one embodiment of the present invention can be used for one or both of the first batteries 1301a and 1301b.
[0499] In this embodiment, an example is shown in which two first batteries 1301a and 1301b are connected in parallel, but three or more batteries may be connected in parallel. Furthermore, if the first battery 1301a can store sufficient power, the first battery 1301b may be omitted. By configuring a battery pack having multiple secondary batteries, it is possible to extract large amounts of power. The multiple secondary batteries may be connected in parallel, in series, or in series after being connected in parallel. A plurality of secondary batteries is also called a battery pack.
[0500] In addition, in a secondary battery for vehicle use, a service plug or circuit breaker that can cut off high voltage without using tools is provided in the first battery 1301a in order to cut off power from multiple secondary batteries.
[0501] The power of the first batteries 1301a and 1301b is mainly used to rotate the motor 1304, but also supplies power to 42V system (high voltage system) on-board components (such as an electric power steering 1307, a heater 1308, and a defogger 1309) via a DCDC circuit 1306. When a rear motor 1317 is provided for the rear wheels, the first battery 1301a is also used to rotate the rear motor 1317.
[0502] In addition, the second battery 1311 supplies power to 14V (low voltage) in-vehicle components (audio 1313, power windows 1314, lamps 1315, etc.) via the DCDC circuit 1310.
[0503] The first battery 1301a will be described with reference to FIG. 26A.
[0504] 26A shows an example of a large battery pack 1415. One electrode of the battery pack 1415 is electrically connected to the control circuit unit 1320 by a wiring 1421. The other electrode is electrically connected to the control circuit unit 1320 by a wiring 1422. The battery pack may have a configuration in which a plurality of secondary batteries are connected in series.
[0505] A memory circuit including a transistor using an oxide semiconductor may be used for the control circuit portion 1320. A charge control circuit or a battery control system including a memory circuit including a transistor using an oxide semiconductor may be referred to as a battery operating system (BTOS) or a battery oxide semiconductor (BTOS).
[0506] The control circuit 1320 detects the terminal voltage of the secondary battery and manages the charge / discharge state of the secondary battery. For example, to prevent overcharging, it can turn off both the output transistor and the cutoff switch of the charging circuit almost simultaneously.
[0507] FIG. 26B shows an example of a block diagram of the battery pack 1415 shown in FIG. 26A.
[0508] The control circuit 1320 includes a switch unit 1324 including at least a switch for preventing overcharging and a switch for preventing overdischarging, a control circuit 1322 for controlling the switch unit 1324, and a voltage measurement unit for the first battery 1301a. The control circuit 1320 sets upper and lower voltage limits for the secondary battery used and limits the upper limit of external current or the upper limit of output current to the external device. The range between the lower and upper voltage limits for the secondary battery is within the recommended voltage range. If the secondary battery falls outside this range, the switch unit 1324 activates and functions as a protection circuit. The control circuit 1320 can also be called a protection circuit because it controls the switch unit 1324 to prevent overcharging or overdischarging. For example, if the control circuit 1322 detects a voltage that could cause overcharging, it turns off the switch unit 1324 to cut off the current. Furthermore, a PTC element may be provided in the charge / discharge path to provide a function for cutting off the current in response to an increase in temperature. The control circuit section 1320 also has an external terminal 1325 (+IN) and an external terminal 1326 (-IN).
[0509] The switch portion 1324 can be configured by combining one or both of an n-channel transistor and a p-channel transistor. The switch portion 1324 is not limited to a switch having a Si transistor using single crystal silicon. For example, the switch portion 1324 may be formed using a power transistor having Ge (germanium), SiGe (silicon germanium), GaAs (gallium arsenide), GaAlAs (gallium aluminum arsenide), InP (indium phosphide), SiC (silicon carbide), ZnSe (zinc selenide), GaN (gallium nitride), or GaOx (gallium oxide; x is a real number greater than 0). Furthermore, memory elements using OS transistors can be freely arranged by stacking them on circuits using Si transistors, for example, and thus can be easily integrated. Furthermore, OS transistors can be manufactured using the same manufacturing equipment as Si transistors, and therefore can be manufactured at low cost. That is, the control circuit portion 1320 using an OS transistor can be stacked on the switch portion 1324 and integrated into a single chip. The volume occupied by the control circuit section 1320 can be reduced, which allows for miniaturization.
[0510] The first batteries 1301a and 1301b mainly supply power to in-vehicle devices of the 42V system (high voltage system), and the second battery 1311 supplies power to in-vehicle devices of the 14V system (low voltage system). A lead-acid battery is often used as the second battery 1311 because of its cost advantage.
[0511] In this embodiment, an example is shown in which lithium ion secondary batteries are used as both the first battery 1301a and the second battery 1311. The second battery 1311 may be a lead storage battery, an all-solid-state battery, or an electric double layer capacitor.
[0512] Furthermore, regenerative energy generated by the rotation of the tire 1316 is sent to the motor 1304 via the gear 1305, and is then sent from the motor controller 1303 or the battery controller 1302 via the control circuit unit 1321 to charge the second battery 1311. Alternatively, the first battery 1301a is charged from the battery controller 1302 via the control circuit unit 1320. Alternatively, the first battery 1301b is charged from the battery controller 1302 via the control circuit unit 1320. In order to efficiently charge the regenerative energy, it is desirable that the first batteries 1301a and 1301b be capable of rapid charging.
[0513] The battery controller 1302 can set the charging voltage and charging current of the first batteries 1301a and 1301b. The battery controller 1302 can set charging conditions in accordance with the charging characteristics of the secondary battery used, and can perform rapid charging.
[0514] Although not shown, when an external charger is connected, the charger's outlet or the charger's connection cable is electrically connected to the battery controller 1302. Power supplied from the external charger is charged to the first batteries 1301a and 1301b via the battery controller 1302. Some chargers are provided with a control circuit, and although the functions of the battery controller 1302 may not be used, it is preferable to charge the first batteries 1301a and 1301b via the control circuit unit 1320 to prevent overcharging. The control circuit unit 1320 may also be provided in the connection cable or the charger's connection cable. The control circuit unit 1320 is sometimes called an ECU (Electronic Control Unit). The ECU is connected to a CAN (Controller Area Network) provided in the electric vehicle. CAN is one of the serial communication standards used as an in-vehicle LAN. The ECU includes a microcomputer. The ECU uses a CPU or a GPU.
[0515] Next, an example in which the secondary battery of one embodiment of the present invention is mounted on a vehicle, typically a transportation vehicle, will be described.
[0516] When a secondary battery according to one embodiment of the present invention is installed in a vehicle, next-generation clean energy vehicles such as hybrid vehicles (HVs), electric vehicles (EVs), and plug-in hybrid vehicles (PHVs) can be realized. Furthermore, the secondary battery can also be installed in agricultural machinery such as electric tractors, mopeds including electrically assisted bicycles, motorcycles, electric wheelchairs, electric carts, small or large ships, submarines, aircraft such as fixed-wing aircraft and rotary-wing aircraft, rockets, artificial satellites, space probes or planetary probes, and spacecraft. A large secondary battery can be fabricated by using the method for manufacturing a secondary battery according to one embodiment of the present invention. Therefore, the secondary battery according to one embodiment of the present invention can be suitably used in transportation vehicles.
[0517] 27A to 27E illustrate transportation vehicles using a secondary battery of one embodiment of the present invention. The automobile 2001 illustrated in FIG. 27A is an electric automobile using an electric motor as a power source for traveling. Alternatively, it is a hybrid automobile that can appropriately select and use an electric motor or an engine as a power source for traveling. When a secondary battery is installed in a vehicle, the secondary battery is installed in one or more locations. The automobile 2001 illustrated in FIG. 27A includes the battery pack 1415 illustrated in FIG. 24A. The battery pack 1415 includes a secondary battery module. The battery pack 1415 preferably further includes a charge control device electrically connected to the secondary battery module. The secondary battery module includes one or more secondary batteries.
[0518] Furthermore, automobile 2001 can charge its secondary battery by receiving power from an external charging facility using a plug-in system, a contactless power supply system, or the like. Charging can be performed using a predetermined charging method or connector standard, such as CHAdeMO (registered trademark) or Combo, as appropriate. The charging device may be a charging station installed in a commercial facility or a household power source. For example, plug-in technology can be used to charge the secondary battery installed in automobile 2001 using an external power supply. Charging can be performed by converting AC power to DC power via a conversion device, such as an AC-DC converter.
[0519] Furthermore, although not shown, a power receiving device can be mounted on a vehicle and power can be supplied contactlessly from a ground-based power transmitting device to charge the vehicle. In the case of this contactless power supply method, by incorporating a power transmitting device into a road or an exterior wall, charging can be performed not only while the vehicle is stopped but also while the vehicle is moving. This contactless power supply method can also be used to transmit and receive power between two vehicles. Furthermore, a solar cell can be installed on the exterior of the vehicle to charge the secondary battery while the vehicle is stopped or moving. For such contactless power supply, an electromagnetic induction method or a magnetic field resonance method can be used.
[0520] 27B shows a large transport vehicle 2002 having an electrically controlled motor as an example of a transport vehicle. The secondary battery module of the transport vehicle 2002 is a secondary battery module in which, for example, four secondary batteries of 3.5 V or more and 4.7 V or less are connected in parallel to form one cell, and 48 such cells are connected in series to achieve a maximum voltage of 170 V. Apart from the number of secondary batteries constituting the secondary battery module of the battery pack 2201, the secondary battery module has the same functions as those shown in FIG. 27A, and therefore a description thereof will be omitted.
[0521] FIG. 27C illustrates, as an example, a large transport vehicle 2003 having an electrically controlled motor. The secondary battery module of the transport vehicle 2003 has, for example, a maximum voltage of 600 V, which is obtained by connecting in series one hundred or more secondary batteries with a voltage of 3.5 V or higher and 4.7 V or lower. Therefore, a secondary battery with minimal variation in characteristics is required. By using the method for manufacturing a secondary battery according to one embodiment of the present invention, secondary batteries with stable battery characteristics can be manufactured, enabling low-cost mass production from the viewpoint of yield. Furthermore, except for the number of secondary batteries constituting the secondary battery module of the battery pack 2202, the same functions as those in FIG. 27A are provided, and therefore description thereof will be omitted.
[0522] Fig. 27D shows, as an example, an aircraft 2004 having an engine that burns fuel. Since the aircraft 2004 shown in Fig. 27D has wheels for takeoff and landing, it can also be said to be part of a transportation vehicle, and has a battery pack 2203 that includes a secondary battery module formed by connecting multiple secondary batteries and the secondary battery module and a charge control device.
[0523] The secondary battery module of the aircraft 2004 is, for example, eight 4 V secondary batteries connected in series to produce a maximum voltage of 32 V. Other than the number of secondary batteries constituting the secondary battery module of the battery pack 2203, the secondary battery module has the same functions as those shown in Fig. 27A, and therefore a description thereof will be omitted.
[0524] FIG. 27E shows an example of a transport vehicle 2005 for transporting cargo. The transport vehicle 2005 has an electrically controlled motor and performs various tasks by receiving power from a secondary battery constituting a secondary battery module of a battery pack 2204. The transport vehicle 2005 does not necessarily have to be driven by a human driver and can be unmanned via CAN communication or the like. While a forklift is shown in FIG. 27E , this is not a limitation, and a battery pack having a secondary battery according to one embodiment of the present invention can be mounted on industrial machinery that can be operated via CAN communication or the like, such as an automated transporter, a work robot, or a small construction machine.
[0525] 28A is an example of an electric bicycle using the secondary battery of one embodiment of the present invention. The secondary battery of one embodiment of the present invention can be applied to the electric bicycle 2100 shown in Fig. 28A. A power storage device 2102 shown in Fig. 28B includes, for example, a plurality of secondary batteries and a protection circuit.
[0526] The electric bicycle 2100 includes a power storage device 2102. The power storage device 2102 can supply electricity to a motor that assists a rider. The power storage device 2102 is portable and is shown in a state detached from the bicycle in FIG. 28B . The power storage device 2102 includes a plurality of secondary batteries 2101 of one embodiment of the present invention, and a display unit 2103 can display the remaining battery charge and other information. The power storage device 2102 also includes a control circuit 2104 that can control charging or detect an abnormality of the secondary battery, which is an example of one embodiment of the present invention. The control circuit 2104 is electrically connected to the positive and negative electrodes of the secondary battery 2101. A small solid-state secondary battery may be provided in the control circuit 2104. Providing a small solid-state secondary battery in the control circuit 2104 also allows power to be supplied to retain data in a memory circuit of the control circuit 2104 for a long period of time. Furthermore, a synergistic effect in terms of safety can be obtained by combining the positive electrode active material 100 of one embodiment of the present invention with a secondary battery using the positive electrode. The secondary battery and the control circuit 2104 in which the positive electrode active material 100 according to one embodiment of the present invention is used for a positive electrode can significantly contribute to preventing accidents such as fires caused by secondary batteries.
[0527] 28C illustrates an example of a two-wheeled vehicle using the secondary battery of one embodiment of the present invention. A scooter 2300 illustrated in FIG. 28C includes a power storage device 2302, a side mirror 2301, and a turn signal light 2303. The power storage device 2302 can supply electricity to the turn signal light 2303. Furthermore, the power storage device 2302, which includes a plurality of secondary batteries each using the positive electrode active material 100 of one embodiment of the present invention in its positive electrode, can have a high capacity and contribute to miniaturization. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery.
[0528] 28C is capable of storing a power storage device 2302 in under-seat storage 2304. The power storage device 2302 can be stored in under-seat storage 2304 even if the under-seat storage 2304 is small.
[0529] [Building] Next, an example in which the secondary battery of one embodiment of the present invention is mounted in a building will be described with reference to FIGS.
[0530] 29A includes a power storage device 2612 including a secondary battery with stable battery characteristics obtained by using a manufacturing method for a secondary battery according to one embodiment of the present invention, and a solar panel 2610. The power storage device 2612 is electrically connected to the solar panel 2610 via wiring 2611 or the like. The power storage device 2612 may also be electrically connected to a ground-mounted charging device 2604. The power obtained by the solar panel 2610 can be charged to the power storage device 2612. The power stored in the power storage device 2612 can be charged to a secondary battery included in the vehicle 2603 via the charging device 2604. The power storage device 2612 is preferably installed in an underfloor space. By installing the power storage device 2612 in the underfloor space, the space above the floor can be effectively utilized. Alternatively, the power storage device 2612 may be installed on the floor.
[0531] The power stored in the power storage device 2612 can also be supplied to other electronic devices in the house. Therefore, even when power cannot be supplied from a commercial power source due to a power outage or the like, the power storage device 2612 can be used as an uninterruptible power supply, allowing the use of electronic devices.
[0532] 29B illustrates an example of a power storage device according to one embodiment of the present invention. As illustrated in FIG. 29B , a large-sized power storage device 791 obtained by the method for manufacturing a secondary battery according to one embodiment of the present invention is installed in an underfloor space 796 of a building 799.
[0533] A control device 790 is installed in the power storage device 791, and the control device 790 is electrically connected to the distribution board 703, the power storage controller 705 (also called the control device), the display 706, and the router 709 by wiring.
[0534] Electric power is sent from commercial power source 701 to distribution board 703 via service line attachment portion 710. Electric power is also sent to distribution board 703 from power storage device 791 and commercial power source 701, and distribution board 703 supplies the sent electric power to general load 707 and power storage load 708 via outlets (not shown).
[0535] The general load 707 is, for example, an electrical appliance such as a television or a personal computer, and the power storage load 708 is, for example, an electrical appliance such as a microwave oven, a refrigerator, or an air conditioner.
[0536] The power storage controller 705 includes a measurement unit 711, a prediction unit 712, and a planning unit 713. The measurement unit 711 has a function of measuring the amount of power consumed by the general load 707 and the power storage load 708 during a day (e.g., from midnight to midnight). The measurement unit 711 may also have a function of measuring the amount of power of the power storage device 791 and the amount of power supplied from the commercial power source 701. The prediction unit 712 has a function of predicting the amount of power demand to be consumed by the general load 707 and the power storage load 708 during the next day based on the amount of power consumed by the general load 707 and the power storage load 708 during the previous day. The planning unit 713 has a function of creating a plan for charging and discharging the power storage device 791 based on the amount of power demand predicted by the prediction unit 712.
[0537] The amount of power consumed by the general load 707 and the power storage load 708 measured by the measurement unit 711 can be confirmed on the display 706. It can also be confirmed on an electrical device such as a television or a personal computer via the router 709. It can also be confirmed on a portable electronic device such as a smartphone or a tablet via the router 709. The amount of power demand for each time period (or each hour) predicted by the prediction unit 712 can also be confirmed on the display 706, the electrical device, or the portable electronic device.
[0538] The secondary battery of one embodiment of the present invention can be used in, for example, one or both of an electronic device and a lighting device, such as a mobile phone, a smartphone, a portable information terminal such as a laptop computer, a portable game console, a portable music player, a digital camera, or a digital video camera.
[0539] A personal computer 2800 shown in FIG. 30A includes a housing 2801, a housing 2802, a display portion 2803, a keyboard 2804, a pointing device 2805, and the like. A secondary battery 2807 is provided inside the housing 2801, and a secondary battery 2806 is provided inside the housing 2802. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 2807 may be electrically connected to the secondary battery 2807. A touch panel is applied to the display portion 2803. As shown in FIG. 30B, the housings 2801 and 2802 can be removed from the personal computer 2800, and the personal computer 2800 can be used as a tablet terminal using only the housing 2802.
[0540] A large secondary battery obtained by the method for manufacturing a secondary battery according to one embodiment of the present invention can be used as one or both of the secondary battery 2806 and the secondary battery 2807. The shape of the secondary battery obtained by the method for manufacturing a secondary battery according to one embodiment of the present invention can be freely changed by changing the shape of the exterior body. For example, by forming the secondary batteries 2806 and 2807 to match the shapes of the housings 2801 and 2802, the capacity of the secondary battery can be increased and the usage time of the personal computer 2800 can be extended. Furthermore, the weight of the personal computer 2800 can be reduced.
[0541] A flexible display is applied to the display portion 2803 of the housing 2802. A large-sized secondary battery obtained by the manufacturing method of a secondary battery according to one embodiment of the present invention is used as the secondary battery 2806. A large-sized secondary battery obtained by the manufacturing method of a secondary battery according to one embodiment of the present invention can be made into a bendable secondary battery by using a flexible film for the exterior body. This allows the housing 2802 to be folded and used as shown in FIG. 30C . In this case, part of the display portion 2803 can also be used as a keyboard as shown in FIG. 30C .
[0542] The housing 2802 can be folded so that the display portion 2803 faces inward as shown in FIG. 30D, or can be folded so that the display portion 2803 faces outward as shown in FIG. 30E.
[0543] The secondary battery of one embodiment of the present invention can be applied to a bendable secondary battery, and can be mounted in electronic devices and incorporated along the curved surfaces of the interior or exterior walls of houses or buildings, or the interior or exterior surfaces of automobiles.
[0544] 31A shows an example of a mobile phone. The mobile phone 7400 includes a display portion 7402 built into a housing 7401, operation buttons 7403, an external connection port 7404, a speaker 7405, a microphone 7406, and the like. Note that the mobile phone 7400 includes a secondary battery 7407. By using the secondary battery of one embodiment of the present invention as the secondary battery 7407, a lightweight mobile phone with a long life can be provided. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 7407 may be electrically connected to the secondary battery 7407.
[0545] FIG. 31B shows the mobile phone 7400 in a bent state. When the mobile phone 7400 is deformed by an external force and bent as a whole, the secondary battery 7407 installed inside is also bent. FIG. 31C shows the state of the bent secondary battery 7407 at that time. The secondary battery 7407 is a thin storage battery. The secondary battery 7407 is fixed in a bent state. The secondary battery 7407 has a lead electrode electrically connected to the current collector. For example, the current collector is copper foil, and a portion of the current collector is alloyed with gallium to improve adhesion with the active material layer in contact with the current collector, resulting in a configuration with high reliability when the secondary battery 7407 is bent.
[0546] FIG. 31D shows an example of a bangle-type display device. The portable display device 7100 includes a housing 7101, a display unit 7102, operation buttons 7103, and a secondary battery 7104. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 7104 may be electrically connected to the secondary battery 7104. FIG. 31E also shows a bent secondary battery 7104. When the secondary battery 7104 is worn on a user's wrist in a bent state, the housing deforms, causing a partial or complete change in curvature of the secondary battery 7104. The degree of bending at any point on the curve, expressed as the radius of the corresponding circle, is called the radius of curvature, and the reciprocal of the radius of curvature is called the curvature. Specifically, a partial or complete change in the main surface of the housing or secondary battery 7104 occurs within a radius of curvature range of 40 mm to 150 mm. High reliability can be maintained if the radius of curvature of the main surface of the secondary battery 7104 is within a range of 40 mm to 150 mm. By using the secondary battery of one embodiment of the present invention as the secondary battery 7104, a lightweight and long-life portable display device can be provided.
[0547] 31F shows an example of a wristwatch-type portable information terminal 7200. The portable information terminal 7200 includes a housing 7201, a display portion 7202, a band 7203, a buckle 7204, operation buttons 7205, an input / output terminal 7206, and the like.
[0548] The portable information terminal 7200 can execute various applications such as mobile phone calls, e-mail, document browsing and creation, music playback, internet communication, and computer games.
[0549] The display surface of the display portion 7202 is curved, and display can be performed along the curved display surface. The display portion 7202 also includes a touch sensor, and can be operated by touching the screen with a finger, a stylus, or the like. For example, an application can be started by touching an icon 7207 displayed on the display portion 7202.
[0550] The operation button 7205 can have various functions, such as time setting, power on / off operation, wireless communication on / off operation, silent mode activation / deactivation, power saving mode activation / deactivation, etc. For example, the functions of the operation button 7205 can be freely set by an operating system incorporated in the portable information terminal 7200.
[0551] The portable information terminal 7200 is also capable of performing standardized short-range wireless communication. For example, hands-free conversation is possible by communicating with a wirelessly enabled headset.
[0552] The portable information terminal 7200 also includes an input / output terminal 7206, and can directly exchange data with another information terminal via a connector. Charging can also be performed via the input / output terminal 7206. Note that charging may be performed by wireless power supply without using the input / output terminal 7206.
[0553] The display portion 7202 of the portable information terminal 7200 includes the secondary battery of one embodiment of the present invention. By using the secondary battery of one embodiment of the present invention, a lightweight portable information terminal with a long life can be provided. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. For example, the secondary battery 7104 shown in FIG. 31E can be installed in a curved state inside the housing 7201 or in a bendable state inside the band 7203.
[0554] The portable information terminal 7200 preferably has a sensor. For example, a fingerprint sensor, a pulse sensor, a human body sensor such as a body temperature sensor, a touch sensor, a pressure sensor, an acceleration sensor, or the like is preferably mounted as the sensor.
[0555] 31G shows an example of a wristband-type display device. The display device 7300 includes a display portion 7304 and a secondary battery of one embodiment of the present invention. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. The display device 7300 may also include a touch sensor in the display portion 7304 and can function as a portable information terminal.
[0556] The display surface of the display portion 7304 is curved, and display can be performed along the curved display surface. The display state of the display device 7300 can be changed by short-range wireless communication according to a communication standard.
[0557] The display device 7300 also includes an input / output terminal, and can directly exchange data with another information terminal via a connector. Charging can also be performed via the input / output terminal. Note that charging may be performed by wireless power supply without using the input / output terminal.
[0558] By using the secondary battery of one embodiment of the present invention as the secondary battery included in the display device 7300, a lightweight display device with a long lifetime can be provided.
[0559] Furthermore, examples in which a secondary battery with good cycle characteristics according to one embodiment of the present invention is mounted on an electronic device will be described with reference to FIGS. 31H, 32, and 33. FIG.
[0560] By using the secondary battery of one embodiment of the present invention as a secondary battery in an electronic device, a lightweight product with a long life can be provided. For example, examples of daily electronic devices include electric toothbrushes, electric shavers, and electric beauty devices. For the secondary battery of these products, a small, lightweight, and large-capacity stick-shaped secondary battery is desired for ease of holding by users.
[0561] FIG. 31H is a perspective view of a device also known as a tobacco-containing smoking device (electronic cigarette). In FIG. 31H, the electronic cigarette 7500 includes an atomizer 7501 including a heating element, a secondary battery 7504 that supplies power to the atomizer, and a cartridge 7502 including a liquid supply bottle or a sensor. To enhance safety, a protection circuit that prevents overcharging and / or over-discharging of the secondary battery 7504 may be electrically connected to the secondary battery 7504. The secondary battery 7504 shown in FIG. 31H has external terminals so that it can be connected to a charging device. Because the secondary battery 7504 is the tip portion when held, it is desirable that the total length be short and the weight be light. The secondary battery of one embodiment of the present invention has high capacity and good cycle characteristics, making it possible to provide a compact and lightweight electronic cigarette 7500 that can be used for a long period of time.
[0562] Next, an example of a foldable tablet terminal is shown in Figures 32A and 32B. The tablet terminal 7600 shown in Figures 32A and 32B includes a housing 7630a, a housing 7630b, a movable portion 7640 connecting the housings 7630a and 7630b, a display portion 7631 having display portions 7631a and 7631b, switches 7625 to 7627, a fastener 7629, and an operation switch 7628. Using a flexible panel for the display portion 7631 allows the tablet terminal to have a larger display area. Figure 32A shows the tablet terminal 7600 in an open state, and Figure 32B shows the tablet terminal 7600 in a closed state.
[0563] The tablet terminal 7600 also includes a power storage unit 7635 inside the housing 7630a and the housing 7630b. The power storage unit 7635 passes through the movable portion 7640 and is provided across the housing 7630a and the housing 7630b.
[0564] All or part of the display portion 7631 can be a touch panel area, and data can be input by touching an image including an icon, text, an input form, etc. displayed in the area. For example, keyboard buttons may be displayed on the entire surface of the display portion 7631a on the housing 7630a side, and information such as text and images may be displayed on the display portion 7631b on the housing 7630b side.
[0565] A keyboard may be displayed on the display portion 7631b of the housing 7630b, and information such as text and images may be displayed on the display portion 7631a of the housing 7630a. A keyboard display switch button of a touch panel may be displayed on the display portion 7631, and the keyboard may be displayed on the display portion 7631 by touching the button with a finger, a stylus, or the like.
[0566] In addition, touch input can be simultaneously performed on the touch panel area of the display portion 7631a on the housing 7630a side and the touch panel area of the display portion 7631b on the housing 7630b side.
[0567] Furthermore, the switches 7625 to 7627 may be interfaces capable of switching various functions in addition to interfaces for operating the tablet terminal 7600. For example, at least one of the switches 7625 to 7627 may function as a switch for turning the tablet terminal 7600 on and off. For example, at least one of the switches 7625 to 7627 may have a function for switching the display orientation, such as portrait or landscape, or a function for switching between black and white and color display. For example, at least one of the switches 7625 to 7627 may have a function for adjusting the brightness of the display unit 7631. The brightness of the display unit 7631 can be optimized depending on the amount of external light detected by an optical sensor built into the tablet terminal 7600 during use. The tablet terminal may also have built-in not only an optical sensor but also other detection devices, such as a gyroscope, an acceleration sensor, or other sensors for detecting tilt.
[0568] 32A shows an example in which the display areas of the display portion 7631a on the housing 7630a and the display portion 7631b on the housing 7630b are substantially the same, the display areas of the display portion 7631a and the display portion 7631b are not particularly limited, and the sizes of one and the other may be different, and the display qualities may also be different. For example, one display panel may be capable of displaying at a higher resolution than the other.
[0569] 32B shows a tablet terminal 7600 folded in half, and the tablet terminal 7600 includes a housing 7630, a solar cell 7633, and a charge / discharge control circuit 7634 including a DCDC converter 7636. In addition, a secondary battery of one embodiment of the present invention is used as a power storage unit 7635.
[0570] As described above, the tablet terminal 7600 can be folded in half, and thus can be folded so that the housing 7630a and the housing 7630b overlap when not in use. By folding, the display portion 7631 can be protected, thereby improving the durability of the tablet terminal 7600. Furthermore, the power storage unit 7635 using the secondary battery of one embodiment of the present invention has a high capacity and favorable cycle characteristics, and therefore the tablet terminal 7600 can be used for a long period of time. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery included in the power storage unit 7635 may be electrically connected to the secondary battery.
[0571] In addition, the tablet terminal 7600 shown in Figures 32A and 32B can have functions such as displaying various information (still images, videos, text images, etc.), displaying a calendar, date or time on the display unit, a touch input function for touch input operations or editing information displayed on the display unit, and controlling processing using various software (programs).
[0572] A solar cell 7633 attached to the surface of the tablet terminal 7600 can supply power to a touch panel, a display unit, a video signal processor, or the like. The solar cell 7633 can be provided on one or both surfaces of the housing 7630, and can be configured to efficiently charge the power storage unit 7635. Use of a lithium-ion battery as the power storage unit 7635 has the advantage of enabling miniaturization.
[0573] The configuration and operation of the charge / discharge control circuit 7634 shown in Fig. 32B are described with reference to a block diagram in Fig. 32C Fig. 32C shows a solar cell 7633, a power storage unit 7635, a DC / DC converter 7636, a converter 7637, switches SW1 to SW3, and a display unit 7631. The power storage unit 7635, the DC / DC converter 7636, the converter 7637, and switches SW1 to SW3 correspond to the charge / discharge control circuit 7634 shown in Fig. 32B .
[0574] First, an example of operation when power is generated by the solar cell 7633 using external light will be described. The power generated by the solar cell is stepped up or down by a DC-DC converter 7636 to a voltage for charging the power storage unit 7635. When power from the solar cell 7633 is used to operate the display unit 7631, a switch SW1 is turned on, and the converter 7637 steps up or steps down the voltage to a voltage required for the display unit 7631. When no display is to be performed on the display unit 7631, the switch SW1 may be turned off and the switch SW2 may be turned on to charge the power storage unit 7635.
[0575] Note that the solar cell 7633 is shown as an example of a power generation means, but is not particularly limited thereto, and a configuration in which the power storage unit 7635 is charged by other power generation means such as a piezoelectric element (piezo element) or a thermoelectric conversion element (Peltier element) may be used. For example, a configuration in which a contactless power transmission module that transmits and receives power wirelessly (contactlessly) for charging, or a combination of other charging means may be used.
[0576] FIG. 33 illustrates an example of another electronic device. In FIG. 33 , a display device 8000 is an example of an electronic device using a secondary battery 8004 according to one embodiment of the present invention. Specifically, the display device 8000 corresponds to a display device for receiving TV broadcasts and includes a housing 8001, a display portion 8002, a speaker portion 8003, a secondary battery 8004, and the like. To enhance safety, a protection circuit for preventing overcharging and / or overdischarging of the secondary battery 8004 may be electrically connected to the secondary battery 8004. The secondary battery 8004 according to one embodiment of the present invention is provided inside the housing 8001. The display device 8000 can receive power from a commercial power source or can use power stored in the secondary battery 8004. Therefore, even when power cannot be supplied from the commercial power source due to a power outage or the like, the display device 8000 can be used by using the secondary battery 8004 according to one embodiment of the present invention as an uninterruptible power source.
[0577] The display portion 8002 can be a liquid crystal display device, a light-emitting device having a light-emitting element such as an organic EL element in each pixel, an electrophoretic display device, a semiconductor display device such as a DMD (Digital Micromirror Device), a PDP (Plasma Display Panel), or an FED (Field Emission Display).
[0578] The display device includes all display devices for displaying information, such as those for receiving TV broadcasts, those for personal computers, and those for displaying advertisements.
[0579] In FIG. 33 , a stationary lighting device 8100 is an example of an electronic device using a secondary battery 8103 according to one embodiment of the present invention. Specifically, the lighting device 8100 includes a housing 8101, a light source 8102, a secondary battery 8103, and the like. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 8103 may be electrically connected to the secondary battery 8103. Although FIG. 33 illustrates the case where the secondary battery 8103 is provided inside a ceiling 8104 on which the housing 8101 and the light source 8102 are installed, the secondary battery 8103 may also be provided inside the housing 8101. The lighting device 8100 can receive power from a commercial power source or can use power stored in the secondary battery 8103. Therefore, even when power cannot be supplied from the commercial power source due to a power outage or the like, the lighting device 8100 can be used by using the secondary battery 8103 according to one embodiment of the present invention as an uninterruptible power supply.
[0580] Note that although Figure 33 illustrates an example of a stationary lighting device 8100 provided on the ceiling 8104, the secondary battery of one embodiment of the present invention can also be used in a stationary lighting device provided on a side wall 8105, a floor 8106, a window 8107, or the like other than the ceiling 8104, or can also be used in a tabletop lighting device.
[0581] Furthermore, an artificial light source that artificially obtains light using electric power can be used as the light source 8102. Specifically, examples of the artificial light source include a discharge lamp such as an incandescent lamp or a fluorescent lamp, an LED, and / or an organic EL element.
[0582] In FIG. 33 , an air conditioner including an indoor unit 8200 and an outdoor unit 8204 is an example of an electronic device using a secondary battery 8203 according to one embodiment of the present invention. Specifically, the indoor unit 8200 includes a housing 8201, an air outlet 8202, a secondary battery 8203, and the like. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 8203 may be electrically connected to the secondary battery 8203. Although FIG. 33 illustrates the case where the secondary battery 8203 is provided in the indoor unit 8200, the secondary battery 8203 may also be provided in the outdoor unit 8204. Alternatively, the secondary battery 8203 may be provided in both the indoor unit 8200 and the outdoor unit 8204. The air conditioner can receive power from a commercial power source or can use power stored in the secondary battery 8203. In particular, when a secondary battery 8203 is provided in both the indoor unit 8200 and the outdoor unit 8204, the air conditioner can be used by using the secondary battery 8203 of one embodiment of the present invention as an uninterruptible power supply even when power cannot be supplied from a commercial power source due to a power outage or the like.
[0583] Note that although Figure 33 illustrates an example of a separate-type air conditioner including an indoor unit and an outdoor unit, a secondary battery of one embodiment of the present invention can also be used in an integrated air conditioner in which the functions of the indoor unit and the outdoor unit are combined in one housing.
[0584] 33 , an electric refrigerator-freezer 8300 is an example of an electronic device using a secondary battery 8304 according to one embodiment of the present invention. Specifically, the electric refrigerator-freezer 8300 includes a housing 8301, a refrigerator compartment door 8302, a freezer compartment door 8303, a secondary battery 8304, and the like. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 8304 may be electrically connected to the secondary battery 8304. In FIG. 33 , the secondary battery 8304 is provided inside the housing 8301. The electric refrigerator-freezer 8300 can receive power from a commercial power source or can use power stored in the secondary battery 8304. Therefore, even when power cannot be supplied from the commercial power source due to a power outage or the like, the electric refrigerator-freezer 8300 can be used by using the secondary battery 8304 according to one embodiment of the present invention as an uninterruptible power supply.
[0585] Among the electronic devices described above, electronic devices such as microwave ovens and other high-frequency heating devices and electric rice cookers require a large amount of power for a short period of time. Therefore, by using a secondary battery according to one embodiment of the present invention as an auxiliary power source for supplementing the power that cannot be supplied by the commercial power source, it is possible to prevent the breaker of the commercial power source from tripping when the electronic device is in use.
[0586] Furthermore, by storing power in the secondary battery during times when electronic devices are not in use, particularly during times when the ratio of the amount of power actually used to the total amount of power that can be supplied by the commercial power supplier (referred to as the power usage rate) is low, it is possible to prevent the power usage rate from increasing outside of these times. For example, in the case of an electric refrigerator-freezer 8300, power is stored in the secondary battery 8304 during the night when the temperature is low and the refrigerator door 8302 and the freezer door 8303 are not opened or closed. Then, during the day when the temperature is high and the refrigerator door 8302 and the freezer door 8303 are opened and closed, the secondary battery 8304 is used as an auxiliary power source, thereby keeping the daytime power usage rate low.
[0587] According to one embodiment of the present invention, the cycle characteristics of the secondary battery can be improved, and the reliability can be improved. Furthermore, according to one embodiment of the present invention, a high-capacity secondary battery can be obtained, and therefore the characteristics of the secondary battery can be improved, and therefore the secondary battery itself can be made smaller and lighter. Therefore, by incorporating the secondary battery according to one embodiment of the present invention in the electronic device described in this embodiment, the electronic device can have a longer life and be lighter.
[0588] 34A shows an example of a wearable device. The wearable device uses a secondary battery as a power source. Furthermore, in order to improve splash-proof, water-resistant, or dust-proof performance when used at home or outdoors, a wearable device that can be charged wirelessly as well as via a wired connection with an exposed connector is desired.
[0589] For example, a secondary battery according to one embodiment of the present invention can be mounted on an eyeglasses-type device 9000 as shown in FIG. 34A . The eyeglasses-type device 9000 includes a frame 9000a and a display unit 9000b. Mounting a secondary battery on the temples of the curved frame 9000a allows the eyeglasses-type device 9000 to be lightweight, well-balanced in weight, and have a long continuous use time. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. By including a secondary battery according to one embodiment of the present invention, a configuration that can accommodate space savings due to a smaller housing can be realized.
[0590] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on a headset device 9001. The headset device 9001 includes at least a microphone unit 9001a, a flexible pipe 9001b, and an earphone unit 9001c. The secondary battery can be provided in the flexible pipe 9001b or the earphone unit 9001c. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. By including the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space savings due to a smaller housing can be realized.
[0591] Furthermore, a secondary battery according to one embodiment of the present invention can be mounted on a device 9002 that can be directly attached to the body. A secondary battery 9002b can be provided in a thin housing 9002a of the device 9002. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 9002b may be electrically connected to the secondary battery 9002b. By including the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space savings due to a smaller housing can be realized.
[0592] Furthermore, a secondary battery according to one embodiment of the present invention can be mounted on a device 9003 that can be attached to clothing. A secondary battery 9003b can be provided in a thin housing 9003a of the device 9003. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 9003b may be electrically connected to the secondary battery 9003b. By including the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space savings due to a smaller housing can be realized.
[0593] Furthermore, the secondary battery of one embodiment of the present invention can be mounted on a belt-type device 9006. The belt-type device 9006 has a belt portion 9006a and a wireless power receiving portion 9006b, and the secondary battery can be mounted inside the belt portion 9006a. To improve safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. By including the secondary battery of one embodiment of the present invention, a configuration that can accommodate space saving due to a miniaturized housing can be realized.
[0594] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on the wristwatch device 9005. The wristwatch device 9005 has a display portion 9005a and a belt portion 9005b, and the secondary battery can be provided on the display portion 9005a or the belt portion 9005b. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery may be electrically connected to the secondary battery. By including the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving due to a miniaturized housing can be realized.
[0595] The display portion 9005a can display not only the time but also various information such as incoming emails and / or phone calls.
[0596] Furthermore, since the wristwatch-type device 9005 is a wearable device that is worn directly on the arm, it may be equipped with sensors that measure the user's pulse, blood pressure, etc. Data on the user's exercise amount and health can be accumulated to manage the user's health.
[0597] FIG. 34B shows a perspective view of the wristwatch-type device 9005 removed from the wrist.
[0598] 34C shows a side view of the display device 9005. The display device 9005 includes a secondary battery 913 according to one embodiment of the present invention. The secondary battery 913 is small and lightweight and is provided so as to overlap with the display portion 9005a.
[0599] 35A shows an example of a cleaning robot. The cleaning robot 9300 includes a display unit 9302 arranged on the top surface of a housing 9301, multiple cameras 9303 arranged on the side surface, a brush 9304, operation buttons 9305, a secondary battery 9306, various sensors, and the like. To enhance safety, a protection circuit that prevents overcharging and / or over-discharging of the secondary battery 9306 may be electrically connected to the secondary battery 9306. Although not shown, the cleaning robot 9300 is provided with tires, a suction port, and the like. The cleaning robot 9300 can move by itself, detect dust 9310, and suck up the dust through a suction port provided on the bottom surface.
[0600] For example, the cleaning robot 9300 can analyze an image captured by the camera 9303 to determine whether or not there is an obstacle such as a wall, furniture, or a step. Furthermore, if an object that may become entangled in the brush 9304, such as a wire, is detected through image analysis, the cleaning robot 9300 can stop the rotation of the brush 9304. The cleaning robot 9300 includes a secondary battery 9306 according to one embodiment of the present invention and a semiconductor device or electronic component therein. By using the secondary battery 9306 according to one embodiment of the present invention in the cleaning robot 9300, the cleaning robot 9300 can be a highly reliable electronic device with a long operating time.
[0601] Fig. 35B shows an example of a robot. The robot 9400 shown in Fig. 35B includes a secondary battery 9409, an illuminance sensor 9401, a microphone 9402, an upper camera 9403, a speaker 9404, a display unit 9405, a lower camera 9406, an obstacle sensor 9407, a movement mechanism 9408, a computing device, etc. To enhance safety, a protection circuit that prevents overcharging and / or over-discharging of the secondary battery 9409 may be electrically connected to the secondary battery 9409.
[0602] The microphone 9402 has a function of detecting the user's voice, environmental sounds, etc. The speaker 9404 has a function of emitting sound. The robot 9400 can communicate with the user using the microphone 9402 and the speaker 9404.
[0603] The display portion 9405 has a function of displaying various information. The robot 9400 can display information desired by a user on the display portion 9405. The display portion 9405 may be equipped with a touch panel. The display portion 9405 may be a detachable information terminal, which can be installed in a fixed position on the robot 9400 to enable charging and data transfer.
[0604] The upper camera 9403 and the lower camera 9406 have the function of capturing images of the surroundings of the robot 9400. In addition, the obstacle sensor 9407 can detect the presence or absence of obstacles in the direction of travel when the robot 9400 moves forward using the movement mechanism 9408. The robot 9400 can recognize the surrounding environment and move safely using the upper camera 9403, the lower camera 9406, and the obstacle sensor 9407.
[0605] The robot 9400 includes a secondary battery 9409 according to one embodiment of the present invention and a semiconductor device or an electronic component inside the robot 9400. By using the secondary battery according to one embodiment of the present invention in the robot 9400, the robot 9400 can be a highly reliable electronic device with a long operating time.
[0606] Fig. 35C shows an example of an air vehicle. The air vehicle 9500 shown in Fig. 35C has a propeller 9501, a camera 9502, a secondary battery 9503, and the like, and has the function of flying autonomously. To enhance safety, a protection circuit that prevents overcharging and / or over-discharging of the secondary battery 9503 may be electrically connected to the secondary battery 9503.
[0607] For example, image data captured by the camera 9502 is stored in the electronic component 9504. The electronic component 9504 can analyze the image data and detect the presence or absence of an obstacle when moving. Furthermore, the electronic component 9504 can estimate the remaining battery charge from a change in the storage capacity of the secondary battery 9503. The flying object 9500 includes the secondary battery 9503 according to one embodiment of the present invention therein. By using the secondary battery according to one embodiment of the present invention in the flying object 9500, the flying object 9500 can be an electronic device with a long operating time and high reliability.
[0608] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0609] (Additional Notes Regarding the Description of the Present Specification, etc.) The following additional notes will be given regarding the above-described embodiments and the explanation of each configuration in the embodiments.
[0610] The configurations shown in each embodiment can be combined with the configurations shown in other embodiments as appropriate to form one aspect of the present invention. In addition, when multiple configuration examples are shown in one embodiment, the configuration examples can be combined as appropriate.
[0611] In addition, the content (or even a part of the content) described in one embodiment can be applied to, combined with, or replaced with another content (or even a part of the content) described in that embodiment, and / or the content (or even a part of the content) described in one or more other embodiments.
[0612] The contents described in the embodiments refer to the contents described in each embodiment using various figures or the contents described using text in the specification.
[0613] Furthermore, a figure (or even a part thereof) described in one embodiment can be combined with another part of that figure, another figure (or even a part thereof) described in that embodiment, and / or a figure (or even a part thereof) described in one or more other embodiments to form even more figures.
[0614] In addition, in the present specification and the like, in the block diagrams, components are classified by function and shown as independent blocks. However, in actual circuits, etc., it is difficult to separate components by function, and there may be cases where one circuit is involved in multiple functions, or where one function is involved across multiple circuits. Therefore, the blocks in the block diagrams are not limited to the components described in the specification, but may be rephrased appropriately depending on the situation.
[0615] In addition, in the drawings, the size, layer thickness, or region is shown at an arbitrary size for convenience of explanation. Therefore, it is not necessarily limited to the scale. Note that the drawings are shown schematically for clarity, and are not limited to the shapes or values shown in the drawings. For example, it is possible to include variations in signal, voltage, or current due to noise, or variations in signal, voltage, or current due to timing deviations.
[0616] In this specification and the like, when describing the connection relationship of a transistor, the term "one of the source or the drain" (or first electrode or first terminal) is used, and the other of the source and the drain is referred to as "the other of the source or the drain" (or second electrode or second terminal). This is because the source and drain of a transistor vary depending on the structure or operating conditions of the transistor. Note that the names of the source and drain of a transistor can be appropriately changed to source (drain) terminal or source (drain) electrode, etc., depending on the situation.
[0617] Furthermore, the terms "electrode" and "wiring" used in this specification and elsewhere do not limit the functionality of these components. For example, an "electrode" may be used as part of a "wiring," and vice versa. Furthermore, the terms "electrode" and "wiring" include cases where multiple "electrodes," multiple "wirings," or multiple "electrodes" and multiple "wirings" are integrally formed.
[0618] Furthermore, in this specification and the like, the terms voltage and potential can be interchanged as appropriate. Voltage refers to a potential difference from a reference potential. For example, if the reference potential is a ground voltage, voltage can be interchanged with potential. Ground potential does not necessarily mean 0 V. Note that potential is relative, and the potential applied to wiring, etc. may change depending on the reference potential.
[0619] In this specification and the like, terms such as "film" and "layer" can be interchangeable depending on the circumstances. For example, the term "conductive layer" can be changed to the term "conductive film." Or, for example, the term "insulating film" can be changed to the term "insulating layer."
[0620] In this specification, a switch refers to a device that has a function of controlling whether a current flows by being in a conductive state (on state) or a non-conductive state (off state), or a device that has a function of selecting and switching a path for a current to flow.
[0621] In this specification, the channel length refers to, for example, in a top view of a transistor, a region where a semiconductor (or a portion in the semiconductor through which current flows when the transistor is on) and a gate overlap, or a distance between a source and a drain in a region where a channel is formed.
[0622] In this specification, the channel width refers to, for example, the length of the region where the semiconductor (or the portion in the semiconductor through which current flows when the transistor is on) and the gate electrode overlap, or the length of the portion where the source and drain face each other in the region where the channel is formed.
[0623] In this specification, "A and B are connected" includes not only a direct connection between A and B, but also an electrical connection between A and B. Here, "A and B are electrically connected" means that when an object having some kind of electrical effect exists between A and B, transmission of an electrical signal between A and B is possible.
[0624] In this example, a secondary battery of one embodiment of the present invention was fabricated and evaluated.
[0625] [Preparation of Positive Electrode Active Material] Positive electrode active materials were prepared with reference to the preparation method shown in FIG.
[0626] LiMO in step S14 2 As the X1 source, commercially available lithium cobalt oxide (Cellseed C-10N, manufactured by Nippon Chemical Industry Co., Ltd.) containing cobalt as the transition metal M and no particular additives was prepared. As in step S20a, lithium fluoride and magnesium fluoride were prepared as X1 sources, and the lithium fluoride and magnesium fluoride were mixed using a solid-phase method, as in steps S31 and S32. The lithium fluoride and magnesium fluoride were added so that the number of lithium fluoride molecules was 0.33 and the number of magnesium fluoride molecules was 1, assuming that the number of cobalt atoms was 100. This was designated mixture 903.
[0627] Next, annealing was performed in the same manner as in step S33. 30 g of the mixture 903 was placed in a square alumina container, a lid was placed on it, and the mixture was heated in a muffle furnace. The furnace was purged, and oxygen gas was introduced, but no gas flow was observed during heating. The annealing temperature was 900°C, and the time was 20 hours.
[0628] In step S101, nickel hydroxide and aluminum hydroxide were added to the heated composite oxide and dry mixed. The number of nickel atoms was 0.5 and the number of aluminum atoms was 0.5, assuming that the number of cobalt atoms was 100. This was designated mixture 904.
[0629] Next, annealing was performed in the same manner as in step S33. 30 g of the mixture 903 was placed in a rectangular alumina container, a lid was placed, and the container was heated in a muffle furnace. The inside of the furnace was purged, and oxygen gas was introduced and flowed during heating. The annealing temperature was 850°C for 10 hours.
[0630] Thereafter, the powder was collected by sieving through a 53 μmφ sieve to obtain a positive electrode active material.
[0631] [Fabrication of Positive Electrode] Next, a positive electrode was fabricated using the positive electrode active material prepared above. The positive electrode active material prepared above, acetylene black (AB), and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of positive electrode active material:AB:PVDF = 95:3:2, and a slurry was prepared using NMP as a solvent. The prepared slurry was applied to a current collector, and the solvent was evaporated. Thereafter, a press of 120 kN / m was performed at 120°C to form a positive electrode active material layer on the current collector, thereby fabricating a positive electrode. A 20 μm thick aluminum foil was used as the current collector. The positive electrode active material layer was provided on one side of the current collector. The loading amount was approximately 10 mg / cm. 2 It was.
[0632] [Fabrication of Secondary Battery] Next, for evaluation, a coin-type secondary battery of CR2032 type (diameter 20 mm, height 3.2 mm) was fabricated.
[0633] The positive electrode prepared above and lithium metal as a counter electrode were used. Either a 23 μm-thick polyimide or a 25 μm-thick polypropylene was used as the separator. Four types of electrolytes (hereinafter, Electrolyte A, Electrolyte B, Electrolyte C, and Electrolyte D) were prepared. The secondary battery using Electrolyte A and the secondary battery using Electrolyte B used a 25 μm-thick polypropylene separator. The secondary battery using Electrolyte C and the secondary battery using Electrolyte D used a 23 μm-thick polyimide separator.
[0634] The coin positive electrode cans used in the secondary batteries using electrolyte A and electrolyte B were made of stainless steel. The coin positive electrode cans used in the secondary batteries using electrolyte C and electrolyte D were made of stainless steel covered with aluminum. The negative electrode cans were made of stainless steel.
[0635] An electrolyte A was prepared. As a solvent for the electrolyte A, a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC = 3:7 was used. As a lithium salt, lithium hexafluorophosphate (LiPF 6 The concentration of the lithium salt in the electrolyte was 1.00 mol / L. The water concentration in electrolyte A was 4.4 ppm.
[0636] Electrolyte B, which is a comparative example of electrolyte A, was prepared by adjusting the water concentration to approximately 1000 ppm. Electrolyte B used a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7 as the solvent, and lithium hexafluorophosphate (LiPF 6 The electrolyte solution was prepared using a lithium salt solution containing 1.00 mol / L of lithium salt. Water was then added in an amount equivalent to 1000 ppm of the total amount of electrolyte before the addition of water and the amount of water to be added.
[0637] Electrolyte C was prepared. EMI-FSA represented by structural formula (G11) was used as the solvent for electrolyte C. LiFSA (lithium bis(fluorosulfonyl)amide) was used as the lithium salt, and the concentration of the lithium salt in the electrolyte was 2.15 mol / L. The water concentration of electrolyte C was 25.6 ppm.
[0638]
[0639] Furthermore, an electrolyte D, which is a comparative example of electrolyte C, was used, in which the water concentration was adjusted to approximately 1000 ppm. EMI-FSA shown in structural formula (G11) was used as the solvent for electrolyte D, and LiFSA (lithium bis(fluorosulfonyl)amide) was used as the lithium salt, and the concentration of the lithium salt in the electrolyte was set to 2.15 mol / L, and water was added. The amount of water added was equivalent to 1000 ppm of the sum of the total amount of electrolyte before water addition and the amount of water to be added.
[0640] The water content of the electrolyte was measured using a Karl Fischer moisture meter MKC-610 (manufactured by Kyoto Electronics Manufacturing Co., Ltd.).
[0641] Through the above steps, a coin-type secondary battery was fabricated.
[0642] [Evaluation of Charge-Discharge Characteristics] The charge-discharge characteristics of the prepared coin-type secondary battery were evaluated. The battery was charged at 45° C. with CCCV (0.5 C, cut-off current 0.05 C, cut-off voltage 4.6 V) and discharged with CC (0.5 C, cut-off voltage 2.5 V).
[0643] 36A and 36B show the charge / discharge characteristics of secondary batteries. In Fig. 36A, the dashed line shows the charge / discharge characteristics of a secondary battery using electrolyte A, and the solid line shows the charge / discharge characteristics of a secondary battery using electrolyte B. In Fig. 36B, the dashed line shows the charge / discharge characteristics of a secondary battery using electrolyte C, and the solid line shows the charge / discharge characteristics of a secondary battery using electrolyte D.
[0644] As shown in Figure 36A, a voltage increase was observed in the early stage of charging, suggesting an increase in resistance, in the secondary battery using electrolyte B, which has a higher water content than electrolyte A. Furthermore, as shown in Figure 36B, the secondary battery using electrolyte D exhibited a region during charging where the voltage was slightly higher than that of the secondary battery using electrolyte C, but did not exhibit the significant voltage increase in the early stage of charging seen in the secondary battery using electrolyte B.
[0645] When the amount of water is large, there is a possibility that a reaction between the electrolyte and water may occur, inhibiting charging and discharging.
[0646] [Evaluation of Cycle Characteristics 1] Next, the cycle characteristics of the produced coin-type secondary battery were evaluated.
[0647] A cycle test was performed in an environment of 45°C. Charging was performed at CCCV (0.5C, cut-off current 0.05C, 4.6V), and discharging was performed at CC (0.5C, 2.5V). The capacity of the secondary battery was calculated based on the weight of the positive electrode active material. The C rate was calculated based on 1C being 200mA / g (per weight of positive electrode active material).
[0648] 37A and 37B show the cycle characteristics of the secondary batteries. In Fig. 37A, the dashed line shows the charge / discharge characteristics of the secondary battery using electrolyte A, and the solid line shows the charge / discharge characteristics of the secondary battery using electrolyte B. In Fig. 37B, the dashed line shows the charge / discharge characteristics of the secondary battery using electrolyte C, and the solid line shows the charge / discharge characteristics of the secondary battery using electrolyte D.
[0649] It is believed that when the water content is high, a reaction that inhibits charging and discharging occurs, resulting in a deterioration in performance. Furthermore, even when the water content is high, the ionic liquid showed better results than electrolyte A.
[0650] In this example, evaluation was performed using NMR. Measurements were performed using a nuclear magnetic resonance apparatus (AVANCEIII400 400 MHz, manufactured by Bruker Japan Co., Ltd.) and acetonitrile-d3 (CD3CN) as a solvent.
[0651] NMR analysis was carried out on the electrolytes A and B described in Example 1. FIG. 38 shows the NMR of the electrolyte A. 31 39A shows the P-NMR spectrum of electrolyte B. 31 39A shows a P-NMR spectrum, and FIG. 39B shows an enlarged view of a portion of FIG. 39A.
[0652] When the water content was high, a peak was observed around -20 ppm. 2 F 2 − It is assumed that this corresponds to H 2 O and LiPF 6 It is suggested that this is a product of the reaction with H 2 O and LiPF 6 It is thought that the reaction was suppressed.
[0653] 51: positive electrode active material particle, 52: recess, 53: barrier film, 54: hole, 55: crystal plane, 56: barrier film, 57: crack, 58: hole, 100: positive electrode active material, 130: laminate, 131: laminate, 300: secondary battery, 301: positive electrode can, 302: negative electrode can, 303: gasket, 304: positive electrode, 305: positive electrode current collector, 306: positive electrode active material layer, 307: negative electrode, 308: negative electrode current collector, 309: negative electrode active material layer, 310: separator, 312: washer, 313: ring-shaped insulator, 322: spacer, 400: negative electrode active material, 401: region, 401a: region, 401b: region, 402: Region, 500: Secondary battery, 501: Positive electrode current collector, 502: Positive electrode active material layer, 502a: Region, 503: Positive electrode, 504: Negative electrode current collector, 505: Negative electrode active material layer, 505a: Region, 506: Negative electrode, 507: Separator, 507a: Region, 507b: Region, 508: Electrolyte, 509: Outer body, 509a: Outer body, 509b: Outer body, 510: Positive electrode lead electrode, 511: Negative electrode lead electrode, 512: Laminate, 513: Resin layer, 514: Region, 515a: Electrolyte, 515b: Electrolyte, 515c: Electrolyte, 516: Inlet, 550: Laminate, 553: Acetylene bromide black, 554: graphene, 556: acetylene black, 557: graphene, 560: secondary battery, 561: positive electrode active material, 563: negative electrode active material, 570: manufacturing apparatus, 571: material input chamber, 572: transfer chamber, 573: treatment chamber, 580: transfer mechanism, 581: polymer film, 582: hole, 584: polymer film, 585: hole, 591: stage, 594: nozzle, 600: secondary battery, 601: positive electrode cap, 602: battery can, 603: positive electrode terminal, 604: positive electrode, 605: separator, 606: negative electrode, 607: negative electrode terminal, 608: insulating plate, 609: insulating plate, 610: Gasket (insulating packing), 611: PTC element, 613: safety valve mechanism, 614: conductive plate, 615: power storage system, 616: secondary battery, 620: control circuit, 621: wiring, 622: wiring, 623: wiring, 624: conductor, 625: insulator, 626: wiring, 627: wiring, 628: conductive plate, 701: commercial power source, 703: distribution board, 705: power storage controller, 706: display, 707: general load, 708: power storage system load, 709: router, 710: drop line attachment section, 711: measurement section, 712: prediction section, 713: planning section, 790: control device, 791: power storage device796: underfloor space, 799: building, 903: mixture, 904: mixture, 911a: terminal, 911b: terminal, 913: secondary battery, 930: housing, 930a: housing, 930b: housing, 931: negative electrode, 931a: negative electrode active material layer, 932: positive electrode, 932a: positive electrode active material layer, 933: separator, 950: wound body, 950a: wound body, 951: terminal, 952: terminal, 970: secondary battery, 971: housing, 972: laminate, 973a: positive electrode lead electrode, 973b: terminal, 973c: conductor, 974a: negative electrode lead electrode, 974b: terminal, 974c: conductor, 975a : Positive electrode, 975b: Positive electrode, 976: Separator, 977a: Negative electrode, 1301a: Battery, 1301b: Battery, 1302: Battery controller, 1303: Motor controller, 1304: Motor, 1305: Gear, 1306: DCDC circuit, 1307: Electric power steering, 1308: Heater, 1309: Defogger, 1310: DCDC circuit, 1311: Battery, 1312: Inverter, 1313: Audio, 1314: Power window, 1315: Lamps, 1316: Tire, 1317: Rear motor, 1320: Control circuit section, 1321 : control circuit unit, 1322: control circuit, 1324: switch unit, 1325: external terminal, 1326: external terminal, 1415: battery pack, 1421: wiring, 1422: wiring, 2001: automobile, 2002: transport vehicle, 2003: transport vehicle, 2004: aircraft, 2005: transport vehicle, 2100: electric bicycle, 2101: secondary battery, 2102: power storage device, 2103: display unit, 2104: control circuit, 2201: battery pack, 2202: battery pack, 2203: battery pack, 2204: battery pack, 2300: scooter, 2301: side mirror, 2302: power storage device, 2303: turn signal light, 2304: under-seat storage, 2603: vehicle, 2604: charging device, 2610: solar panel, 2611: wiring, 2612: power storage device, 2800: personal computer, 2801: housing, 2802: housing, 2803: display unit, 2804: keyboard, 2805: pointing device, 2806: secondary battery, 2807: secondary battery, 7100: portable display device, 7101: housing, 7102: display unit, 7103: operation button, 7104: secondary battery, 7200: portable information terminal, 7201: housing, 7202: display unit, 7203: band,7204: Buckle, 7205: Operation button, 7206: Input / output terminal, 7207: Icon, 7300: Display device, 7304: Display unit, 7400: Mobile phone, 7401: Housing, 7402: Display unit, 7403: Operation button, 7404: External connection port, 7405: Speaker, 7406: Microphone, 7407: Secondary battery, 7500: Electronic cigarette, 7501: Atomizer, 7502: Cartridge, 7504: Secondary battery, 7600: Tablet terminal, 7625: Switch, 7627: Switch, 7628: Operation switch, 7629: Fastener, 7630: Housing , 7630a: Housing, 7630b: Housing, 7631: Display unit, 7631a: Display unit, 7631b: Display unit, 7633: Solar cell, 7634: Charge / discharge control circuit, 7635: Power storage body, 7636: DCDC converter, 7637: Converter, 7640: Movable part, 8000: Display device, 8001: Housing, 8002: Display unit, 8003: Speaker unit, 8004: Secondary battery, 8100: Lighting device, 8101: Housing, 8102: Light source, 8103: Secondary battery, 8104: Ceiling, 8105: Side wall, 8106: Floor, 8107: Window, 8200: Indoor unit, 8201: Housing, 820 2: air outlet, 8203: secondary battery, 8204: outdoor unit, 8300: electric refrigerator-freezer, 8301: housing, 8302: refrigerator compartment door, 8303: freezer compartment door, 8304: secondary battery, 9000: eyeglass-type device, 9000a: frame, 9000b: display unit, 9001: headset-type device, 9001a: microphone unit, 9001b: flexible pipe, 9001c: earphone unit, 9002: device, 9002a: housing, 9002b: secondary battery, 9003: device, 9003a: housing, 9003b: secondary battery, 9005: wristwatch-type device, 9005a: Display unit, 9005b: belt unit, 9006: belt-type device, 9006a: belt unit, 9006b: wireless power supply receiving unit, 9300: cleaning robot, 9301: housing, 9302: display unit, 9303: camera, 9304: brush, 9305: operation button, 9306: secondary battery, 9310: dust, 9400: robot, 9401: illuminance sensor, 9402: microphone, 9403: upper camera, 9404: speaker, 9405: display unit, 9406: lower camera, 9407: obstacle sensor, 9408: movement mechanism, 9409: secondary battery, 9500: flying object,9501: Propeller, 9502: Camera, 9503: Secondary battery, 9504: Electronic component,
Claims
1. A positive electrode, a negative electrode, and an electrolyte, The secondary battery, wherein the moisture content of the electrolyte is less than 1000 ppm.
2. A positive electrode, a negative electrode, and an electrolyte, The water content of the electrolyte is less than 1000 ppm; The water content of the electrolyte is measured using a Karl Fischer moisture meter.
3. In claim 1 or 2, The secondary battery, wherein the electrolyte includes a lithium salt and a cyclic carbonate.
4. In claim 1 or 2, The secondary battery, wherein the electrolyte includes a lithium salt and an ionic liquid.
5. In claim 4, The ionic liquid is one or more cations selected from an imidazolium cation, a pyridinium cation, a quaternary ammonium cation, a tertiary sulfonium cation, and a quaternary phosphonium cation; one or more anions selected from a monovalent amide anion, a monovalent methide anion, a fluorosulfonate anion, a perfluoroalkylsulfonate anion, a tetrafluoroborate anion, a perfluoroalkylborate anion, a hexafluorophosphate anion, and a perfluoroalkylphosphate anion; A secondary battery having the above structure.
6. In any one of claims 1 to 5, A secondary battery in which no peak corresponding to P0 2 F 2 − is observed when 31 P-NMR spectrum analysis of the electrolyte is performed.
7. 7. An electronic device comprising: the secondary battery according to claim 1; a display unit; and a sensor.