Polypropylene film, laminate, packaging material, and packing body

JPWO2022138531A5Active Publication Date: 2024-11-29TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021576324
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-20
Filing Date
2021-12-20
Publication Date
2024-11-29
Estimated Expiration
2041-12-20

AI Technical Summary

Technical Problem

Conventional polypropylene films with aluminum vapor-deposited layers are opaque, making them unsuitable for applications requiring visibility, and their recyclability is compromised due to coloration, while transparent alternatives are fragile and prone to defects like pinholes and cracks, impairing gas barrier properties during processing and use.

Method used

A polypropylene film with a multi-layer structure comprising two incompatible layers, where one layer contains a thermoplastic resin like polymethylpentene, providing surface irregularities for slipperiness without anti-blocking agents or particles, and optimized surface roughness and skewness to enhance adhesion and homogeneity of vapor-deposited layers.

Benefits of technology

The film achieves structural stability during vapor deposition, maintaining excellent water vapor and oxygen barrier properties, ensuring effective packaging without compromising visibility or recyclability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention addresses the problem of providing a polypropylene film which is structurally stable to heat in deposition when used for packaging, and has appropriate slipperiness without using an antiblocking agent or particles, and thus has excellent water vapor barrier properties and oxygen barrier properties, in particular, when a transparent deposited layer is laminated. Moreover, the present invention provides a polypropylene film characterized by having at least two types of layers (A layer and B layer) containing a polypropylene-based resin as a main component, wherein the B layer contains a thermoplastic resin incompatible with a polypropylene-based resin, and when the skewnesses Ssk of the A layer and the B layer, as measured through three-dimensional non-contact surface shape measurement, are Ssk (A) and Ssk (B), respectively, the Ssk (B) is at least 5 and the Ssk (A) is less than 5.
Need to check novelty before this filing date? Find Prior Art

Description

Polypropylene films, laminates, packaging materials, and packaging bodies

[0001] The present invention relates to polypropylene films, laminates, wrapping materials, and packages that are particularly suitable for use in packaging applications.

[0002] Due to its excellent transparency, mechanical properties, electrical properties, etc., polypropylene films are used in a variety of applications, including packaging, tape, and electrical insulation applications such as cable wrapping and capacitors. Among these applications, when gas barrier properties are required for packaging, laminated films in which a thin film of aluminum (hereinafter sometimes referred to as "Al") is vapor-deposited onto a polypropylene film are widely used. However, films obtained by Al vapor deposition are opaque and therefore unsuitable for applications requiring visibility of the contents. Furthermore, while there has been an increase in the trend toward recycling packaging plastics in recent years, films containing an Al vapor-deposited layer have problems such as insufficient recyclability, such as difficulty in visually distinguishing them from Al foil laminate films and discoloration after recycling.

[0003] For the reasons described above, there is a trend to replace conventional Al vapor-deposited layers with transparent vapor-deposited layers of aluminum oxide (hereinafter sometimes referred to as AlOx), silicon oxide, or the like. The use of these transparent vapor-deposited layers can improve the transparency and recyclability of packaging materials. However, transparent vapor-deposited layers are generally thinner and more brittle than Al vapor-deposited layers, and therefore, there are problems such as the vapor-deposited layer peeling off during formation or in subsequent processes such as bag manufacturing, or defects such as pinholes and cracks occurring in the vapor-deposited layer, which can easily impair the water vapor barrier property and oxygen barrier property.

[0004] Furthermore, since appropriate transportability is required during vapor deposition processing and bag-making processing, anti-blocking agents or particles are sometimes added to the surface of the film to form irregularities on the film surface, thereby providing easy slippage. However, in processed films with vapor deposition layers, the protrusions formed by the anti-blocking agents or particles are hard. Therefore, when the film is transported as a rolled product, the opposing vapor deposition layer is easily scraped, causing defects and damage such as pinholes and cracks, which can easily impair the water vapor barrier property and oxygen barrier property.

[0005] As polypropylene films suitable for packaging applications, there have been proposals for films in which the molecular weight of the polypropylene resin is controlled to increase the degree of planar orientation of the polypropylene film, thereby increasing its rigidity (e.g., Patent Document 1), and for films in which a highly crystalline raw material is stretched at a high ratio in the longitudinal direction, or biaxially stretched and then further longitudinally stretched in the longitudinal direction to increase the degree of planar orientation and improve water vapor barrier properties (e.g., Patent Document 2). Furthermore, for packaging materials, there have been proposals for films in which particles are added to form irregularities on the film surface to provide easy slippage, in order to achieve appropriate vapor deposition processing and transportability during bag-making processing (e.g., Patent Document 3), and for laminated films in which particles are added to the film surface layer and the thickness of each layer is further controlled to provide easy slippage (e.g., Patent Document 4). On the other hand, there has been a proposal for a polypropylene film for adhesive release, in which a high-melting point resin different from the polypropylene resin is dispersed in the surface layer of the polypropylene film to provide easy slippage without adding particles (e.g., Patent Document 5).

[0006] Japanese Patent Application Laid-Open No. 2014-055283 Japanese Patent Application Laid-Open No. 2001-040111 Japanese Patent Application Laid-Open No. 2020-040361 International Publication No. 2018 / 181011 Pamphlet International Publication No. 2018 / 147334 Pamphlet

[0007] However, the polypropylene films described in Patent Documents 1 and 2 have a single-layer structure, making it impossible to control the surface irregularities on both sides of the film, resulting in insufficient control of fibril protrusion height. Therefore, particularly when a transparent vapor-deposited layer is laminated, there are problems with insufficient adhesion of the vapor-deposited layer and film uniformity, resulting in reduced water vapor barrier and oxygen barrier properties. The polypropylene films described in Patent Documents 3 and 4 contain particles in the heat-sealable layer, so that when vapor deposition is performed on the opposite surface, the vapor-deposited layer is damaged, resulting in defects such as scraping, pinholes, and cracks. Furthermore, the film described in Patent Document 5 has unevenness formed on both surfaces of the film by dispersing a high-melting-point resin different from the polypropylene resin in both surface layers of the polypropylene film. However, there are problems with insufficient control on both sides of the film and the lack of a technical concept for heat stabilization when forming a vapor-deposited layer on the surface, resulting in insufficient adhesion of the vapor-deposited film and film uniformity, resulting in reduced water vapor barrier and oxygen barrier properties.

[0008] Therefore, an object of the present invention is to provide a polypropylene film that, when used for packaging purposes, is structurally stable against the heat that occurs during vapor deposition, has appropriate slip properties without the use of antiblocking agents or particles, and thus has excellent water vapor barrier properties and oxygen barrier properties, particularly when a transparent vapor-deposited layer is laminated thereon.

[0009] The present inventors have conducted extensive research to solve the above problems and have come up with the following first polypropylene film of the present invention and second polypropylene film of the present invention.

[0010] The first polypropylene film of the present invention has at least two types of layers (layer A and layer B) containing a polypropylene-based resin as a main component, and layer B contains a resin that is incompatible with the polypropylene-based resin. When the skewness Ssk of layer A and layer B measured by three-dimensional non-contact surface profile measurement is Ssk(A) and Ssk(B), respectively, Ssk(B) is 5 or more and Ssk(A) is less than 5.

[0011] The second polypropylene film of the present invention has at least two layers (layer A and layer B) containing a polypropylene-based resin as a main component, and layer B contains a thermoplastic resin that is incompatible with the polypropylene-based resin, and when the skewness Ssk of layer A measured by three-dimensional non-contact surface profilometry is Ssk(A), and the surface roughnesses Sa of layer A and layer B are Sa(A) and Sa(B), respectively, Ssk(A) is less than 5, and Sa(A) and Sa(B) satisfy formula 1: Sa(B) / Sa(A)>1.1.

[0012] According to the present invention, it is possible to obtain a polypropylene film that is structurally stable against heat during vapor deposition and has appropriate slip properties without using an antiblocking agent or particles, and that has excellent water vapor barrier properties and oxygen barrier properties, particularly when a transparent vapor-deposited layer is laminated thereon.

[0013] The polypropylene film of the present invention will be described in detail below. In the present invention, the longitudinal direction refers to the direction in which the film runs during the production process of the polypropylene film, and refers to the winding direction of the roll when the polypropylene film is wound into a roll. Furthermore, the width direction refers to the direction perpendicular to the longitudinal direction within the plane of the film.

[0014] The first polypropylene film of the present invention has at least two types of layers (layer A and layer B) containing a polypropylene-based resin as a main component, and the layer B contains a resin that is incompatible with the polypropylene-based resin. When the skewness Ssk of the layer A and the layer B measured by three-dimensional non-contact surface profile measurement is Ssk(A) and Ssk(B), respectively, the Ssk(B) is 5 or more and the Ssk(A) is less than 5.

[0015] The second polypropylene film of the present invention has at least two layers (layer A and layer B) containing a polypropylene-based resin as a main component, and layer B contains a thermoplastic resin that is incompatible with the polypropylene-based resin, and is characterized in that, when the skewness Ssk of layer A measured by three-dimensional non-contact surface profilometry is Ssk(A), and the surface roughnesses Sa of layer A and layer B are Sa(A) and Sa(B), respectively, Ssk(A) is less than 5, and Sa(A) and Sa(B) satisfy formula 1: Sa(B) / Sa(A)>1.1.

[0016] Hereinafter, the first and second polypropylene films of the present invention may be collectively referred to as the present invention or the polypropylene film of the present invention. As described below, Ssk(A), Ssk(B), Sa(A), and Sa(B) are parameters relating to the surface shape and roughness, and therefore, both the A layer and the B layer are located on the outermost surface.

[0017] In the present invention, a polypropylene film refers to a sheet-like molded product containing 80% by mass or more but less than 100% by mass, preferably 80% by mass or more and 99.9% by mass or less, of a polypropylene-based resin when the total constituent components are taken as 100% by mass. A polypropylene-based resin refers to a resin in which 90% by mass or more and 100% by mass or less are propylene units when the total constituent units constituting the resin are taken as 100% by mass. A "layer containing a polypropylene-based resin as the main component" refers to a layer containing more than 50% by mass but not more than 100% by mass of a polypropylene-based resin when the total constituent components are taken as 100% by mass. Note that the "main component" below can be interpreted similarly. The term "having at least two types of layers (layer A and layer B) containing a polypropylene-based resin as the main component" refers to an embodiment in which a plurality of layers containing a polypropylene-based resin as the main component are present, and at least one of the layers has a different composition from the other layers.

[0018] One method for imparting lubricity to the surface of a polypropylene film is to add an antiblocking agent or particles. In this method, the antiblocking agent or particles form protrusions on the film surface, which can improve processability during vapor deposition and bag-making. However, when such a film is rolled into a laminate having a vapor-deposited layer on its surface, the protrusions formed by the antiblocking agent or particles are hard and can cause damage or defects in the vapor-deposited film, such as abrasion, pinholes, or cracks, in the opposing vapor-deposited layer, potentially compromising the water vapor barrier property and oxygen barrier property.

[0019] In addition to adding antiblocking agents or particles, a method of imparting lubricity is generally preferably a method utilizing crystal modification. More specifically, in the film production process, the molten resin composition is solidified on a casting (cooling) drum after melt extrusion at a high temperature of, for example, 60°C or higher to form β-crystal spherulites, and the thermally unstable β-crystals are transformed into α-crystals in the stretching process, thereby forming irregularities on the film surface. However, in the polypropylene film of the present invention, the film surface to be vapor-deposited is preferably smooth from the viewpoint of forming a uniform and homogeneous vapor-deposited film and obtaining excellent water vapor barrier property and oxygen barrier property, and therefore the casting temperature is preferably low. Furthermore, a polyolefin resin with low crystallinity and a low melting point may be used for the surface of the heat-sealable layer, and in this case, it may be difficult to apply the method utilizing the crystal modification described above.

[0020] Therefore, from the viewpoint of imparting easy slipperiness while taking the above points into consideration, it is important that the polypropylene film of the present invention has at least two types of layers (layer A and layer B) containing a polypropylene-based resin as the main component, and that layer B contains a thermoplastic resin that is incompatible with the polypropylene-based resin.

[0021] By blending a polypropylene-based resin with a thermoplastic resin that is incompatible with the polypropylene-based resin, it is possible to impart surface irregularities to the surface of the polypropylene film (layer B) by utilizing the domain structure. Furthermore, in the film production process, by setting the temperature at which the film is solidified on a cooling drum after melt extrusion to 10°C or higher and 40°C or lower, preferably 10°C or higher and 35°C or lower, more preferably 10°C or higher and 30°C or lower, and particularly preferably 10°C or higher and 25°C or lower, fine α-crystal spherulites or a mesophase structure are preferentially formed, thereby suppressing the formation of irregularities due to the β-crystals. Note that, hereinafter, "thermoplastic resin that is incompatible with the polypropylene-based resin" may be referred to as "incompatible resin."

[0022] As the immiscible resin, for example, a polymethylpentene resin can be preferably used. Here, in Layer B containing a polypropylene resin and an immiscible resin, by minimizing the size of the α-crystal spherulites or by forming all or part of the polypropylene resin component as a mesophase, it is possible to suppress interfacial peeling between the immiscible resin domain and the polypropylene resin during stretching. By suppressing interfacial peeling, it is possible to form surface protrusions without whitening the polypropylene film, and good processability can be obtained by reducing the occurrence of uneven deposition due to wrinkles during deposition processing and wrinkles during transport during bag making processing.

[0023] In Layer B constituting the polypropylene film of the present invention, the content of the incompatible resin is preferably 0.1% by mass or more and 10% by mass or less, based on 100% by mass of the entire layer. It is more preferably 0.5% by mass or more and 6% by mass or less, even more preferably 1% by mass or more and 4% by mass or less, and most preferably 1% by mass or more and 2% by mass or less. When the content of the incompatible resin in Layer B is 0.1% by mass or more, surface protrusions are efficiently formed on the surface of Layer B, improving the slipperiness of the surface of Layer B and reducing conveyance wrinkles during vapor deposition processing and bag making processing. On the other hand, when the content of the incompatible resin in Layer B is 10% by mass or less, excessive domain formation in Layer B is suppressed, and a decrease in transparency due to excessive voids occurring at the interface between resins during stretching is reduced. The content (mass %) of the immiscible resin in Layer A is not particularly limited, but from the viewpoint of making Ssk(A) smaller than Ssk(B), as described below, it is preferable to make it lower than the content (mass %) of the immiscible resin in Layer B, and an embodiment in which Layer A does not contain any immiscible resin may also be used.

[0024] In the polypropylene film of the present invention, it is particularly preferable to use a polymethylpentene resin as the incompatible resin because it has a relatively high affinity with the polypropylene resin and can reduce the domain size. The melting point of the polymethylpentene resin is preferably 185°C to 240°C, more preferably 220°C to 240°C, from the viewpoints of extrusion stability when blended with polypropylene and the ability to impart surface irregularities using a domain-island structure. Taking these characteristics into consideration, the polypropylene film of the present invention is preferably a polymer having 4-methylpentene-1 as the main structural unit (a structural unit comprising 80 mol% to 100 mol% of all structural units), and examples of such polymers that can be used include the "TPX" (registered trademark) MX series, "TPX" (registered trademark) DX series, and "TPX" (registered trademark) RT series sold by Mitsui Chemicals, Inc. as the "TPX" (registered trademark) series. Specifically, "TPX" (registered trademark) MX002, MX004, DX310, DX845, and RT31 are preferred from the viewpoint of having a relatively high affinity with polypropylene-based resins and being able to reduce the domain size.

[0025] In the first polypropylene film of the present invention, from the viewpoint of achieving both easy slippage and barrier properties, when the skewness Ssk of layer A and layer B measured by three-dimensional non-contact surface profilometry is Ssk(A) and Ssk(B), respectively, it is important that Ssk(B) is 5 or more and Ssk(A) is less than 5. From the same viewpoint, it is also important in the second polypropylene film of the present invention that Ssk(A) is less than 5.

[0026] Here, skewness Ssk (sometimes simply referred to as Ssk) is a parameter that indicates the degree of bias of the surface protrusion shape measured by three-dimensional non-contact surface shape measurement. This Ssk represents the cube mean of Z(x, y) on a reference plane that has been made dimensionless by the cube of the root-mean-square height Sq, and means skewness, and is an index that indicates the symmetry of the peaks and valleys centered on the average plane. If Ssk<0, it means that there is a downward bias with respect to the average line, that is, there are more valleys than peaks. On the other hand, if Ssk>0, it means that there is an upward bias with respect to the average line, that is, there are more peaks than valleys. And if Ssk=0, it means that there is no bias with respect to the average line.

[0027] Ssk (Ssk(A), Ssk(B), and Ssk(D) described below) can be measured using a known three-dimensional non-contact surface shape measuring device, and as the measuring device, for example, a scanning white light interference microscope VS1540 manufactured by Hitachi High-Tech Science Corporation can be used. Details of the measurement and analysis conditions when using this measuring device are shown in the Examples.

[0028] In the first polypropylene film of the present invention, by setting Ssk(B) to 5 or more, peaks are appropriately formed on the surface of Layer B, thereby improving the slipperiness between polypropylene films or between the polypropylene film and a transport roll. Furthermore, by setting Ssk(A) to less than 5, peaks are reduced and valleys are appropriately formed on the surface of Layer A, so that a layer containing more than 50% by mass and 100% by mass or less of metal and / or inorganic compounds applied by vapor deposition (Layer D, described below) is formed with few protruding convexes and a uniform height. This reduces defects such as pinholes and cracks in Layer D, enabling the film to exhibit high barrier performance.

[0029] Furthermore, in the second polypropylene film of the present invention, by making the Ssk(A) less than 5, it is possible to obtain the same effect as that obtained by making the Ssk(A) less than 5 in the first polypropylene film.

[0030] From the above viewpoints, in the first polypropylene film, Ssk(B) is preferably 7 or more, more preferably 10 or more. The upper limit is not particularly limited, but is set to 25 from the viewpoint of feasibility, and 20 is preferred from the viewpoint of obtaining appropriate handleability to reduce uneven deposition due to the influence of wrinkles during deposition processing and the occurrence of wrinkles during bag making. On the other hand, Ssk(A) is preferably 0 or less, more preferably -5 or less, from the viewpoint of suppressing the water vapor permeability and oxygen permeability of the laminate provided with the D layer and realizing sufficient barrier properties. The lower limit is not particularly limited, but is set to -20 from the viewpoint of feasibility.

[0031] For the same reason, in the second polypropylene film of the present invention, Ssk(A) is preferably 0 or less, more preferably −5 or less. The lower limit is not particularly limited, but is set to −20 from the viewpoint of feasibility.

[0032] In the first polypropylene film of the present invention, an example of a method for controlling the Ssk(B) within the above-mentioned range is to adjust the blending ratio of the polypropylene resin and the incompatible resin within a preferred range and then adjust the stretching conditions. Regarding the stretching conditions, a sequential biaxial stretching method can be used in which the longitudinal stretching ratio is 4.0 times or more, preferably 4.5 times or more. Furthermore, a longitudinal stretching temperature of 125°C or less, preferably 120°C or less, more preferably 115°C or less, and even more preferably 105°C or less can also be used. These stretching conditions can be used alone or in combination.

[0033] On the other hand, in the first and second polypropylene films of the present invention, methods for controlling Ssk(A) within the above-mentioned range include, for example, using a polypropylene-based resin with a high degree of crystallinity (more specifically, a polypropylene-based resin with a mesopentad fraction of 0.93 or more) or a polypropylene-based resin with a melting point of 151°C or higher (preferably 160°C or higher) as the raw material for Layer A, and then adjusting the film-forming and stretching conditions. Suitable film-forming conditions include placing the surface of Layer A of the molten sheet on the surface of a cooling drum during film formation, and setting the cooling and solidification temperature to 35°C or lower, preferably 30°C or lower. Suitable stretching conditions include sequential biaxial stretching with a longitudinal stretch ratio of 4.0 times or higher, preferably 4.5 times or higher, and a longitudinal stretching temperature of 125°C or lower, preferably 120°C or lower, more preferably 115°C or lower, and even more preferably 105°C or lower. These film-forming and stretching conditions can be used alone or in combination.

[0034] In the polypropylene film of the present invention, the fraction of propylene units in the resin components constituting Layer A is preferably 97.0 mol% or more and 100.0 mol% or less, and is equal to or greater than the fraction of propylene units in the resin components constituting the entire polypropylene film. Here, "the fraction of propylene units in the resin components constituting Layer A" refers to the fraction (mol%) of propylene units in Layer A when the constituent units of all resin components constituting Layer A are taken as 100 mol%. Furthermore, "the fraction of propylene units in the resin components constituting the entire polypropylene film" refers to the fraction (mol%) of propylene units in the polypropylene film when the constituent units of all resin components constituting the polypropylene film are taken as 100 mol%. The fraction of propylene units in the resin components can be calculated using known methods. 13 It can be measured by C-NMR.

[0035] By setting the fraction of propylene units in the A layer to 97.0 mol% or more, the movement and loosening of molecular chains on the surface are suppressed, resulting in a structure that is very stable against heat during vapor deposition. Therefore, when a laminate is formed by laminating a vapor deposition layer and a D layer (described later) thereon, the water vapor barrier property and oxygen barrier property thereof can be improved. From the above viewpoint, the lower limit of the fraction of propylene units in the A layer is preferably 99.0 mol%, more preferably 99.5 mol%. Note that a fraction of propylene units in the A layer of 99.5 mol% or more means that, although it may contain a small amount of impurities, the molecular chain of the polypropylene-based resin constituting the A layer is essentially composed only of polypropylene units, and such a polypropylene-based resin is also called a homopolypropylene resin.

[0036] The method for making the fraction of propylene units in layer A 97.0 mol% or more and 100.0 mol% or less or within the above-mentioned preferred range is not particularly limited, but an example is a method of using a polypropylene-based resin having a propylene unit fraction of 97.0 mol% or more and 100.0 mol% or less for layer A. In this case, the fraction of propylene units in layer A can be increased by increasing the fraction of propylene units in the polypropylene-based resin or by increasing the proportion of polypropylene-based resin in layer A.

[0037] In the polypropylene film of the present invention, the melting point of the polypropylene resin that is the main component of Layer A is preferably 151° C. or higher, more preferably 155° C. or higher, more preferably 160° C. or higher, even more preferably 162° C. or higher, particularly preferably 164° C. or higher, and most preferably 166° C. or higher. When the polypropylene resin that is the main component of Layer A has a melting point of 151° C. or higher, the crystallinity of Layer A is maintained at a high level, thereby reducing deformation of the polypropylene film due to heat during vapor deposition.

[0038] In the second polypropylene film of the present invention, from the viewpoint of achieving both easy slippage and barrier properties, it is important that when the surface roughnesses Sa of the A layer and the B layer are Sa(A) and Sa(B), respectively, Sa(A) and Sa(B) satisfy Formula 1. From the same viewpoint, in the first polypropylene film of the present invention, it is preferable that Sa(A) and Sa(B) satisfy Formula 2. Formula 1: Sa(B) / Sa(A)>1.1 Formula 2: Sa(B) / Sa(A)>1.0

[0039] Here, surface roughness Sa is a parameter representing the average absolute value of the height difference at each point relative to the average surface measured by three-dimensional non-contact surface profile measurement. It can be measured using, for example, a measuring instrument similar to Ssk. Sa(B) / Sa(A) > 1.1 (the second polypropylene film of the present invention) or Sa(B) / Sa(A) > 1.0 (the first polypropylene film of the present invention) indicates that the surface of Layer B is rougher than the surface of Layer A, and the surface of Layer A is smoother than the surface of Layer B. Having a rougher surface than the surface of Layer A improves the slipperiness when winding the polypropylene film. On the other hand, the surface of Layer A is sufficiently smooth, which allows for a uniform thickness of Layer D (described below) when laminating it, thereby suppressing defects such as pinholes and cracks in Layer D. This improves the water vapor barrier and oxygen barrier properties of the laminate including Layer D.

[0040] From the above viewpoints, the relationship of formula 1 in the polypropylene film of the present invention is preferably Sa(B) / Sa(A)>1.2, more preferably Sa(B) / Sa(A)>1.5, and even more preferably Sa(B) / Sa(A)>1.8. The upper limit of Sa(B) / Sa(A) in the polypropylene film of the present invention is preferably 4.0, more preferably 3.5, from the viewpoint of not impairing the balance between lubricity and barrier properties. When Sa(B) / Sa(A) is 4.0 or less, the B layer does not become too rough and the number of convex portions is reduced, thereby reducing defects such as pinholes and cracks caused by damage to the D layer by vapor deposition processing or the like, and maintaining the barrier performance of the laminate. In addition, as a method for adjusting Sa(B) / Sa(A) to a value greater than 1.0 or within the above-mentioned preferred range in the first polypropylene film of the present invention, and as a method for adjusting Sa(B) / Sa(A) to a value greater than 1.1 or within the above-mentioned preferred range in the second polypropylene film of the present invention, for example, a method similar to the method for adjusting Ssk(A) or Ssk(B) can be adopted.

[0041] From the viewpoint of being suitable for packaging applications, the polypropylene film of the present invention preferably has a thickness of more than 10 μm and not more than 60 μm. By making the thickness greater than 10 μm, the film can be made less susceptible to tearing due to sagging and tension during vapor deposition processing and transportation. From the above viewpoints, the lower limit of the thickness is more preferably 12 μm, even more preferably 14 μm, and particularly preferably 19 μm. On the other hand, by making the thickness 60 μm or less, handling properties can be improved and production costs can be reduced. From the above viewpoints, the upper limit of the thickness is more preferably 50 μm, and even more preferably 40 μm.

[0042] The thickness of the polypropylene film can be measured using a contact-type electronic micrometer in an atmosphere of 23°C and 65% RH. For example, an electronic micrometer (K-312A model) manufactured by Anritsu Corporation can be used as the contact-type electronic micrometer.

[0043] The method for adjusting the thickness to more than 10 μm and not more than 60 μm or within the above-mentioned preferred range is not particularly limited, and examples that can be used include adjusting the discharge rate during melt extrusion of the polypropylene-based resin composition, adjusting the rotation speed of the casting drum during cooling and solidifying of the molten sheet, adjusting the lip gap of the die that discharges the molten sheet, adjusting the longitudinal stretch ratio, adjusting the widthwise stretch ratio, etc. More specifically, the thickness can be reduced by reducing the discharge rate, increasing the rotation speed of the casting drum, narrowing the lip gap of the die, or increasing the longitudinal or widthwise stretch ratio.

[0044] Furthermore, the polypropylene film of the present invention preferably has a thickness of Layer A of 0.3 μm or more and 10 μm or less. By setting the thickness within this range, the surface of Layer A of the polypropylene film can be easily stretched even at low temperatures, making it easier to achieve high orientation and smoothness. Therefore, when Layer D formed by vapor deposition or the like is laminated onto the film to form a laminate, the thickness of the vapor-deposited film becomes uniform, improving the quality of the vapor-deposited film and improving the water vapor barrier property and oxygen barrier property of the laminate. From the above perspectives, the thickness of Layer A is more preferably 0.5 μm or more and 5.0 μm or less, and even more preferably 0.8 μm or more and 3.0 μm or less. The thickness of Layer A can also be adjusted by the same method as the method for adjusting the thickness to more than 10 μm but not more than 60 μm or within the above-mentioned preferred range.

[0045] The thickness of Layer A can be measured by preparing an ultrathin section using a microtome so that the longitudinal-thickness cross section of the polypropylene film is the observation surface, and then photographing the section using a transmission electron microscope. Note that the thickness of not only Layer A but also the thickness of each layer constituting the polypropylene film or the laminate can be measured in a similar manner.

[0046] The polypropylene film of the present invention preferably has a static friction coefficient (μs) of 0.3 to 1.0 when one surface of the film is superposed on the other surface, in order to provide adequate slipperiness to prevent uneven deposition due to wrinkles during vapor deposition and to prevent wrinkles during bag-making. A μs of 0.3 or more prevents excessive slipperiness of the film, reducing winding slippage during film formation, vapor deposition, and bag-making. A μs of 1.0 or less prevents a decrease in the film's slipperiness, improving handleability and reducing uneven deposition due to wrinkles during vapor deposition and wrinkles during bag-making. From the above perspectives, μs is more preferably 0.3 to 0.8, even more preferably 0.4 to 0.6. The static friction coefficient (μs) can be measured at 25°C and 65% RH in accordance with JIS K 7125 (1999). As a measuring device, for example, a slip tester manufactured by Toyo Seiki Co., Ltd. can be used (other measuring conditions are shown in the Examples).

[0047] As a method for controlling the static friction coefficient (μs) within the above range, for example, a method of adjusting the blending amount of the polypropylene resin and the incompatible resin within a preferred range and then adjusting the stretching conditions can be mentioned. Regarding the stretching conditions, a condition in which the longitudinal stretching ratio is 4.0 times or more, preferably 4.5 times or more, by the sequential biaxial stretching method can be adopted. In addition, a condition in which the longitudinal stretching temperature is 125 ° C or less, preferably 120 ° C or less, more preferably 115 ° C or less, and even more preferably 105 ° C or less can also be adopted. Note that these stretching conditions can be used alone or in combination.

[0048] The polypropylene film of the present invention preferably has a sum of the heat shrinkage rates in the longitudinal and width directions after heat treatment at 125°C for 10 minutes of 4.0% or less, more preferably 3.5% or less, even more preferably 3.0% or less, and most preferably 2.5% or less. There is no particular lower limit, but it is about -2.0%. When the sum of the heat shrinkage rates in the longitudinal and width directions of the film is 4.0% or less, in the case where a D layer is formed by vapor deposition or the like to form a laminate, defects such as pinholes and cracks due to damage to the D layer are reduced, and the oxygen barrier property and water vapor barrier property of the laminate are improved.

[0049] A method for controlling the sum of the longitudinal and transverse heat shrinkage rates after heat treatment at 125°C for 10 minutes to 4.0% or less or within the above-mentioned preferred range includes using a polypropylene raw material with a high mesopentad fraction and a low cold xylene solubles (CXS) content, and appropriately subjecting the film to heat setting and relaxation treatment after biaxial stretching. It is also effective to increase the ratio of the incompatible resin in Layer B within the above-mentioned preferred range.

[0050] In measuring the thermal shrinkage, if it is unclear from the appearance of the film which direction is the longitudinal direction and which is the width direction, a rectangular piece of film is sampled and the breaking strength (MPa) is determined using a tensile tester. The direction giving the maximum breaking strength is considered to be the width direction, and the direction perpendicular to this is considered to be the longitudinal direction. Specifically, the width direction and the longitudinal direction are determined using the following procedure. First, a rectangular sample measuring 20 mm or more (measurement direction) x 10 mm is arbitrarily obtained from the film, and the breaking strength (MPa) is measured using a tensile tester (e.g., Orientec's "Tensilon" (registered trademark) UCT-100) with a length measurement of 20 mm, a tensile speed of 300% / min, and a measurement environment of 23°C and 65% RH. Next, the same measurement is performed with the measurement direction rotated 15° to the right within the film plane, and this is repeated until 12 measurement directions are reached. Finally, the measured values ​​are compared, and the measurement direction in which the maximum breaking strength (MPa) is obtained is regarded as the width direction, and the direction perpendicular thereto is regarded as the length direction.

[0051] If the sample size is too small to measure the breaking strength with a tensile tester, the crystal orientation of the α-crystal (110) plane of the polypropylene film is measured using wide-angle X-rays as follows, and the longitudinal and width directions are estimated based on the following criteria: X-rays (CuKα rays) are incident perpendicularly to an arbitrarily selected film surface, and the crystal peak at 2θ = approximately 14° (α-crystal (110) plane) is scanned in the circumferential direction. The direction with the highest diffraction intensity in the obtained diffraction intensity distribution is defined as the width direction, and the direction perpendicular to this is defined as the longitudinal direction.

[0052] The polypropylene film of the present invention has excellent structural stability against heat during vapor deposition, and has good water vapor barrier property and oxygen barrier property, particularly when a transparent vapor-deposited layer is laminated thereon, and therefore can be suitably used for packaging purposes. The objects to be packaged with the polypropylene film of the present invention are not particularly limited, but include items that are susceptible to deterioration by water vapor or oxygen, such as food, medicines, and fresh flowers.

[0053] Furthermore, the polypropylene resin used as the main component of Layer A of the polypropylene film of the present invention preferably has a mesopentad fraction of 0.93 or more. The mesopentad fraction is more preferably 0.95 or more, even more preferably 0.96 or more, and particularly preferably 0.97 or more. The mesopentad fraction is an index indicating the stereoregularity of the crystalline phase of a polypropylene resin and is measured by nuclear magnetic resonance (NMR). In the polypropylene film of the present invention, by using a polypropylene resin having a mesopentad fraction of 0.93 or more as the main component of Layer A, the crystallinity of Layer A is increased, thereby improving the thermal stability of the polypropylene film (particularly Layer A). This suppresses deformation due to heat during vapor deposition when the polypropylene film is used for packaging applications, facilitating uniform lamination of Layer D, including the vapor-deposited film, and also suppressing defects such as pinholes and cracks in Layer D. This results in improved water vapor barrier properties and oxygen barrier properties for a laminate including Layer D. The upper limit of the mesopentad fraction of the polypropylene resin that is the main component of the layer A is not particularly limited.

[0054] The polypropylene resin used as the main component of Layer A of the polypropylene film of the present invention preferably has a polypropylene component dissolved in xylene (CXS, also referred to as cold xylene solubles) of less than 4.0% by mass when the polypropylene film is completely dissolved in xylene and then precipitated at room temperature. Here, the cold xylene solubles (CXS) are considered to be components that are difficult to crystallize due to low stereoregularity, low molecular weight, or the like. By reducing the CXS content to less than 4.0% by mass, the dimensional stability of the polypropylene film in high-temperature environments is improved. Therefore, when Layer D is formed by vapor deposition or the like to form a laminate, defects such as pinholes and cracks caused by damage to Layer D are reduced, improving the oxygen barrier property and water vapor barrier property of the laminate. From the above perspectives, the CXS content is preferably 2.0% by mass or less, more preferably 1.5% by mass or less. To achieve a CXS content of less than 4.0% by mass or within the above preferred range, methods such as increasing the catalytic activity when obtaining the polypropylene resin used and washing the obtained polypropylene resin with a solvent or propylene monomer itself can be used. Although the lower limit of CXS is not particularly limited, a practical value is 0.1% by mass. Maintaining a CXS content of 0.1% by mass or more reduces deterioration of stretchability during film formation and reduces the occurrence of film breakage. The CXS content can be determined by dissolving 0.5 g of a sample in 100 ml of xylene at 135°C, allowing it to cool, recrystallizing it in a thermostatic water bath at 20°C for 1 hour, filtering it, and quantitatively evaluating the polypropylene components dissolved in the filtrate using liquid chromatography.

[0055] The polypropylene-based resin used in the A layer of the polypropylene film of the present invention may be one type, or two or more types may be mixed. When the D layer is laminated by vapor deposition or the like, an adhesive polypropylene resin may be added from the viewpoint of obtaining interfacial adhesion between the D layer and the A layer. However, from the viewpoint of reducing deformation due to heat during vapor deposition when the polypropylene film is formed, the melting point of the polypropylene-based resin as the main component is preferably 151°C or higher, more preferably 155°C or higher, more preferably 160°C or higher, even more preferably 162°C or higher, particularly preferably 164°C or higher, and most preferably 166°C or higher. When the polypropylene-based resin as the main component of the A layer has a melting point of 160°C or higher, the crystallinity of the A layer is maintained at a high level, thereby reducing deformation of the polypropylene film due to heat during vapor deposition. In other words, when the D layer is laminated by vapor deposition or the like, defects such as pinholes and cracks in the D layer are reduced, and the water vapor barrier property and oxygen barrier property of the laminate including the D layer are improved.

[0056] Furthermore, the A layer of the polypropylene film of the present invention may optionally contain organic particles, inorganic particles, heat stabilizers, crystal nucleating agents, chlorine scavengers, slipping agents, antistatic agents, antiblocking agents, fillers, viscosity modifiers, color inhibitors, antioxidants, etc., as necessary. However, from the viewpoint of improving the uniformity of the vapor-deposited layer and suppressing defects such as pinholes when the D layer is laminated by vapor deposition or the like to form a laminate, the content of these components in the A layer is preferably as low as possible. Specifically, the content of these components is preferably 3% by mass or less, more preferably 1% by mass or less, of all components constituting the A layer.

[0057] The polypropylene resin used in the polypropylene film of the present invention for any of Layer A, Layer B, and Layer C (described below) preferably has a melt flow rate (MFR) measured at 230°C under a load of 21.18 N of 1 to 20 g / 10 min, more preferably 2 to 10 g / 10 min, and even more preferably 2 to 5 g / 10 min, from the viewpoint of film formability. In order to adjust the melt flow rate (MFR) measured under these conditions to the above value, a method for controlling the average molecular weight or molecular weight distribution is employed.

[0058] The layer structure of the polypropylene film of the present invention is not particularly limited as long as it has an A layer and a B layer, with the A layer being located on at least one outermost surface and the B layer being located on the outermost surface of the opposite surface. That is, the film may have a two-layer structure consisting of an A layer and a B layer, or may have another layer between the A layer and the B layer. As an embodiment having another layer between the A layer and the B layer, for example, it is preferable to have a layer (C layer) mainly composed of a polypropylene resin between the A layer and the B layer.

[0059] Such a configuration prevents the components contained in the C layer, which will be described later, from bleeding out onto the surface of the A layer on which the vapor-deposited layer is to be laminated, making it easier to laminate the vapor-deposited layer uniformly. The simplest example of such an embodiment is a three-type, three-layer configuration of the A layer / C layer / B layer, but other layers may be present between the A layer and the C layer or between the B layer and the C layer.

[0060] The composition of the C layer in the polypropylene film of the present invention is not particularly limited as long as it is primarily composed of a polypropylene resin. It may also contain a polypropylene resin with a long-chain branched structure, a petroleum resin, a crystal nucleating agent, etc. Furthermore, various additives, such as antioxidants, heat stabilizers, chlorine scavengers, slip agents, antistatic agents, fillers, viscosity modifiers, and color inhibitors, may also be included within the scope of the present invention. Among the above components, the C layer in the polypropylene film of the present invention preferably contains a petroleum resin. Here, the petroleum resin is a petroleum resin that does not have polar groups such as hydroxyl groups, carboxyl groups, halogen groups, sulfonic acid groups, or modified forms thereof. Specifically, it is a cyclopentadiene-based resin derived from petroleum-based unsaturated hydrocarbons or a resin derived primarily from higher olefin-based hydrocarbons.

[0061] The inclusion of a petroleum resin in the C layer improves uniform stretchability during film formation, allowing the longitudinal stretching temperature to be 120°C or lower. This facilitates improving the heat resistance of the polypropylene film and favorably controlling the static friction coefficient. Furthermore, the inclusion of a petroleum resin in the C layer reduces the void volume of the amorphous portion of the polypropylene resin, thereby improving the water vapor barrier properties of the polypropylene film. From the above perspectives, the amount of petroleum resin added in the C layer is preferably 2% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 15% by mass or less, and even more preferably 5% by mass or more and 10% by mass or less, when the total components of the C layer are taken as 100% by mass.

[0062] Furthermore, from the viewpoint of water vapor barrier properties and productivity, the softening point of the petroleum resin is preferably 90°C or higher and 140°C or lower, and more preferably 100°C or higher and 130°C or lower. By setting the softening point within this range, it becomes easier to improve not only the water vapor barrier properties of the polypropylene film but also the uniform stretchability during film formation. Specific examples of such petroleum resins include T-REZ HA125 (softening point 125°C) manufactured by JXTG Nippon Oil & Energy Corporation and "ALCON" (registered trademark) P125 (manufactured by Arakawa Chemical Industries, Ltd., softening point 125°C) manufactured by Arakawa Chemical Industries, Ltd.

[0063] The polypropylene film of the present invention has a structure in which Layer A is located on one outermost surface and Layer B is located on the other outermost surface, and in this case, Layer B may play a role as a heat seal. Heat sealing refers to the state (or the process) in which films are melted and pressure-bonded together through heat treatment when filling and packaging the contents and forming a bag, and heat sealability refers to the property of the film side that melts and pressure-bonds when heated.

[0064] In the polypropylene film of the present invention, it is preferable that Layer B is a layer having heat-sealing properties. Here, the layer having heat-sealing properties means a layer having a heat-sealing strength of 2 N / 25.4 mm or more measured by the method described below.

[0065] In order to impart low-temperature and high-speed heat-sealing properties, Layer B in the polypropylene film of the present invention preferably contains a polypropylene-based resin having lower crystallinity and a lower melting point than the polypropylene-based resin that is the main component of Layer A. Specifically, an ethylene-propylene random copolymer, an ethylene-propylene-butene random copolymer, a propylene-butene random copolymer, or the like can be preferably used.

[0066] The melting point of Layer B is preferably 100°C or higher but lower than 150°C, more preferably 110°C or higher but lower than 148°C, and even more preferably 120°C or higher but lower than 145°C, from the viewpoint of imparting low-temperature, high-speed sealing properties. The melting point of Layer B can be determined as the lowest peak temperature among the endothermic peaks due to melting when Layer B of the polypropylene film is analyzed by differential scanning calorimetry (DSC). It is important that Layer B of the polypropylene film of the present invention contain a resin that is incompatible with the polypropylene-based resin described above from the viewpoint of imparting appropriate slip properties without adding particles or lubricants. However, various additives, such as antioxidants, heat stabilizers, chlorine scavengers, antistatic agents, fillers, viscosity modifiers, and color inhibitors, may also be contained within a range that does not impair the object of the present invention.

[0067] The method for laminating the B layer is not particularly limited, but examples include a feedblock method or a multi-manifold method using melt coextrusion during film formation, as well as extrusion lamination and dry lamination. From the viewpoint of production efficiency and cost, a lamination method using melt coextrusion is preferred. The thickness of the B layer of the polypropylene film is not particularly limited, but the lower limit of the thickness of the B layer relative to 100% of the total thickness of the polypropylene film is preferably 0.5%, more preferably 1%. On the other hand, the upper limit of the thickness of the B layer relative to 100% of the total thickness of the polypropylene film is preferably 80%, more preferably 60%, even more preferably 40%, and particularly preferably 10%.

[0068] The polypropylene-based resin used in each of the A, B, and C layers of the polypropylene film of the present invention may contain a biomass-derived polypropylene-based resin. When the polypropylene film contains a biomass-derived polypropylene-based resin, the content thereof is preferably 5% by mass or more, more preferably 10% by mass or more, when the total polypropylene-based resin constituting each layer is taken as 100% by mass. The biomass content of the biomass-derived polypropylene is preferably 10% or more. When the polypropylene film of the present invention contains resin components other than the polypropylene-based resin, these components may be biomass-derived. The polypropylene film of the present invention may also contain polypropylene recycled by mechanical recycling or chemical recycling. This can also reduce the environmental impact.

[0069] The laminate of the present invention is characterized in that, when a layer containing more than 50 mass % and 100 mass % or less of a metal and / or inorganic compound in total is defined as Layer D, Layer D is in contact with Layer A of the polypropylene film of the present invention, and Layer D has a thickness of 50 nm or less.

[0070] The laminate of the present invention comprises the polypropylene film of the present invention and a layer (Layer D) containing a total of more than 50% by mass but not more than 100% by mass of a metal and / or inorganic compound. This configuration allows for high water vapor barrier properties and oxygen barrier properties. Here, the term "layer containing more than 50% by mass of an inorganic compound or metal" refers to a layer containing more than 50% by mass of a metal alone, a layer containing more than 50% by mass of an inorganic compound alone, or a layer containing both a metal and an inorganic compound in a total amount exceeding 50% by mass, where the total mass of all components constituting the layer is taken as 100% by mass. The inorganic compound or metal in Layer D is preferably, for example, aluminum, aluminum oxide, silicon oxide, cerium oxide, calcium oxide, diamond-like carbon, or a mixture thereof, from the viewpoints of improving adhesion to the polypropylene film, improving gas barrier properties when laminated to a polypropylene film, and reducing environmental impact.

[0071] The thickness of Layer D in the laminate of the present invention is 50 nm or less, preferably 40 nm or less, more preferably 30 nm or less, and even more preferably 20 nm or less, from the viewpoints of recyclability (reusing the laminate as a resin or film) and improving barrier properties by making the laminate less likely to crack. The lower limit is not particularly limited, but is set to 1 nm from the viewpoint of exhibiting barrier properties.

[0072] The method for forming the D layer on the polypropylene film of the present invention to form a laminate includes coating, vapor deposition, lamination, etc., but vapor deposition is preferred because it is independent of humidity and can exhibit excellent gas barrier properties even with a thin film. As the vapor deposition method, physical vapor deposition methods such as vacuum vapor deposition, EB vapor deposition, sputtering, and ion plating, and various chemical vapor deposition methods such as plasma CVD can be used, but vacuum vapor deposition is particularly preferred from the viewpoint of productivity.

[0073] The water vapor permeability of the laminate of the present invention is 2.0 g / m from the viewpoint of the preservation of the contents when used as a packaging material. 2 / day or less, more preferably 1.0 g / m 2 / day or less, more preferably 0.5 g / m 2 By setting the temperature in this range, deterioration of the contents due to moisture absorption or release can be reduced, particularly when used for food packaging.

[0074] In addition, the oxygen permeability of the laminate of the present invention is 40 cc / m from the viewpoint of the preservation of the contents when used as a packaging material. 2 / day or less, more preferably 30 cc / m 2 / day or less, more preferably 20cc / m 2 / day or less, most preferably 10cc / m 2 By setting the temperature in this range, deterioration of the contents due to oxidation can be reduced, particularly when the product is used for food packaging.

[0075] In the laminate of the present invention, when the skewness Ssk of the D layer measured with a three-dimensional non-contact surface roughness meter is defined as Ssk(D), it is preferable that Ssk(D) is less than 5. By setting Ssk(D) to less than 5, peaks are few and valleys are appropriately formed, and convexities protruding from the D layer formed by vapor deposition are reduced, resulting in a vapor-deposited layer formed with a uniform height. As a result, defects such as pinholes and cracks are reduced, and the laminate can exhibit high barrier performance. From the above viewpoints, Ssk(D) is preferably 0 or less, more preferably −5 or less, and even more preferably −6 or less. The lower limit is not particularly limited, but is set to −20 from the viewpoint of maintaining barrier properties.

[0076] Examples of methods for controlling Ssk(D) within the above range include using a polypropylene resin with a high degree of crystallinity as a raw material (more specifically, using a polypropylene resin with a mesopentad fraction of 0.93 or more), setting the cooling and solidifying temperature of the molten sheet during film formation to 30°C or less, setting the longitudinal stretching ratio to 4.0 times or more, preferably 4.5 times or more in a sequential biaxial stretching method, setting the longitudinal stretching temperature to 125°C or less, preferably 120°C or less, more preferably 115°C or less, and even more preferably 110°C or less, and setting the thickness of the metal layer when forming a D layer on the surface of a polypropylene film to 50 nm or less. These methods can be used alone or in combination.

[0077] <Packaging material, packaging body> The packaging material and packaging body of the present invention will be described below. The packaging material of the present invention is characterized by having at least one of the polypropylene film of the present invention and the laminate of the present invention. The packaging material of the present invention has excellent structural stability against heat during vapor deposition, and in particular, when a transparent vapor deposition layer is laminated, has good water vapor barrier property and oxygen barrier property, so that it can be suitably used for packaging items that are easily deteriorated by water vapor or oxygen.

[0078] The package of the present invention is characterized in that the contents are packaged in the packaging material of the present invention. The contents are not particularly limited, but since the packaging material of the present invention has excellent transparency, water vapor barrier properties, and oxygen barrier properties, it is preferable that the contents be visible from the outside and be easily deteriorated by water vapor or oxygen. The package of the present invention can be obtained by covering the contents with the packaging material of the present invention, and the form thereof is not particularly limited. For example, a package can be obtained by processing the packaging material of the present invention into a bag by heat sealing and placing the contents inside. Specific examples of such packages include snack foods and retort pouch foods.

[0079] <Production Method> The method for producing the polypropylene film of the present invention is described below. In producing the polypropylene film of the present invention, first, a molten polypropylene resin or a polypropylene resin composition is melt-extruded onto a support to form an unstretched polypropylene film. Next, this unstretched polypropylene film is stretched in the longitudinal direction and then in the width direction, thereby sequentially biaxially stretching it. Thereafter, a heat treatment and a relaxation treatment are performed to produce a biaxially oriented polypropylene film. The polypropylene film of the present invention and its production method are described in more detail below, but the polypropylene film of the present invention and its production method should not be construed as necessarily being limited thereto.

[0080] First, the polypropylene resin or polypropylene resin composition serving as the raw material for Layer A, Layer B, and Layer C is melt-extruded from separate single-screw extruders set at an extrusion temperature of 220°C to 280°C, preferably 230°C to 270°C, and passed through a filter to remove foreign matter. These molten resins are then joined in a feed block or the like to form the desired layer structure (e.g., Layer A / Layer C / Layer B, where Layer A is Layer A, Layer B is Layer B, and Layer C is Layer C). The resulting mixture is then extruded through a slit-shaped die at a temperature of 200°C to 260°C, more preferably 210°C to 240°C. During melt extrusion, the resin is sufficiently melted to prevent molecular chain scission due to shear caused by screw rotation, thereby stabilizing the film structure without relaxation even at high temperatures. Therefore, it is preferable to set the temperature before the filter high and after passing through the filter lower than before the filter, and further lower the die temperature immediately before discharge to achieve a multi-stage reduction in temperature.

[0081] Next, the molten resin sheet extruded from the slit die is cooled and solidified on a casting drum (cooling drum) whose surface temperature is controlled to 10°C to 40°C, preferably 10°C to 35°C, more preferably 10°C to 30°C, and most preferably 10°C to 25°C, to obtain an unstretched polypropylene film. Coextrusion lamination is preferably performed so that the drum surface side that the molten resin extruded from the die first comes into contact with is Layer A. By using this temperature range and configuration, the mesophase fraction of the surface layer of the unstretched polypropylene film, particularly on the drum surface side (Layer A side), can be increased, resulting in the unstretched polypropylene film having a mesophase structure. This makes it easier to control the skewness Ssk and surface roughness Sa of Layer A and Layer B within the desired ranges. This results in a smooth surface for Layer A of the resulting polypropylene film, improving the thickness uniformity and adhesion of Layer D, which is formed by vapor deposition or the like. The method for adhering the molten sheet to the casting drum may be any of electrostatic application, adhesion methods utilizing the surface tension of water, air knife, press roll, underwater casting, air chamber, etc., or a combination of several methods may be used, but the air knife method is preferred because it can improve the flatness of the film and easily control the skewness Ssk and surface roughness Sa. When using the air knife method, it is preferable to appropriately adjust the position of the air knife so that air flows downstream of the film production process to prevent vibration of the film.

[0082] The mesophase is an intermediate phase between crystals and amorphous phases, and is specifically formed when solidified from a molten state at an extremely rapid cooling rate. It is generally known that polypropylene resins crystallize and form spherulites when cooled and solidified. However, when unstretched polypropylene films containing such spherulites are stretched, differences in stretching stress occur within the spherulites and between the crystalline and amorphous regions between the spherulites, leading to localized stretching irregularities and thickness and structural irregularities. On the other hand, since the mesophase does not take a spherulite morphology, stretching irregularities are not observed and stretching uniformity is high. Therefore, when the film is formed, the thickness uniformity is high and the surface roughness is small and uniform. Furthermore, when an unstretched film contains a mesophase structure, the temperature for longitudinal stretching (longitudinal stretching) can be lower than that for unstretched propylene films that do not contain a mesophase.

[0083] In particular, in a laminated polypropylene film having an A layer containing a highly stereoregular polypropylene resin and a B layer containing a thermoplastic resin that is immiscible with the polypropylene resin, by making the A layer a mesophase, it is possible to improve the stretchability of the highly stereoregular polypropylene, which is difficult to stretch at low temperatures, and therefore, even when the longitudinal stretching temperature is set to a low temperature of, for example, 120°C or less, it is possible to improve film formability and smooth the surface of the A layer.

[0084] Next, the unstretched polypropylene film is biaxially stretched to obtain a biaxial orientation. First, the unstretched polypropylene film is preheated by passing it between rolls maintained at a lower limit of preferably 70°C, more preferably 80°C, and an upper limit of preferably 150°C, more preferably 130°C, and even more preferably 110°C. Subsequently, the unstretched polypropylene film is longitudinally stretched in an environment maintained at a lower limit of preferably 70°C, more preferably 80°C, and an upper limit of preferably 125°C or less, more preferably 120°C or less, even more preferably 115°C or less, and particularly preferably 105°C or less, at a stretching ratio of 2.0 to 15 times, preferably 4.0 to 10 times, more preferably 4.5 to 8.0 times, and even more preferably 4.5 to 6.0 times, and then cooled to room temperature to obtain a uniaxially oriented film.

[0085] Next, while holding both widthwise ends of the uniaxially oriented film with clips, the film is introduced into a tenter and stretched in the widthwise direction (transverse stretching). The temperature during this process (widthwise stretching temperature) is 150 to 175°C, preferably 155 to 170°C. The widthwise stretching ratio is preferably 8.5 to 20.0 times, more preferably 9.0 to 16.0 times, and even more preferably 10.0 to 12.0 times. A widthwise stretching ratio of 8.5 times or more imparts high orientation in the widthwise direction while maintaining high longitudinal orientation, thereby increasing in-plane molecular chain tension. Therefore, particularly when used for packaging applications, the film's structural stability against heat during vapor deposition is improved, and a uniform vapor deposition film is formed, resulting in excellent water vapor barrier properties and oxygen barrier properties. Furthermore, a widthwise stretching ratio of 20.0 times or less prevents film tearing during film formation and improves productivity.

[0086] In the production of the propylene film of the present invention, the areal stretching ratio is preferably 42.5 times or more and 100 times or less. The areal stretching ratio can be calculated by multiplying the longitudinal stretching ratio by the widthwise stretching ratio. The lower limit of the areal stretching ratio is more preferably 45.0 times, and even more preferably 53.0 times.

[0087] In the production of the polypropylene film of the present invention, it is preferable to subject the film to a heat treatment and relaxation treatment after transverse stretching. The heat treatment and relaxation treatment are carried out at a temperature of 140°C to 170°C, more preferably 152°C to 168°C, and even more preferably 154°C to 165°C, while applying a relaxation of 2% to 20% in the width direction while tenter clips tensely hold both widthwise end portions. Such heat treatment and relaxation treatment improve the structural stability of the film against heat and suppress the heat damage phenomenon that causes defects such as pinholes and cracks in the D layer when the D layer is formed by vapor deposition to form a laminate. As a result, the water vapor barrier property and oxygen barrier property of the laminate obtained from the polypropylene film can be improved.

[0088] In the relaxation treatment, from the viewpoint of enhancing the structural stability of the film against heat, the relaxation rate is preferably 2% or more and 20% or less, more preferably 4% or more and 18% or less, and even more preferably 6% or more and 15% or less. If the relaxation rate is less than 2%, the thermal dimensional stability of the film may be insufficient. Therefore, when the D layer is formed by vapor deposition to form a laminate, the film may deform, causing defects such as pinholes and cracks in the D layer, and the water vapor barrier property and oxygen barrier property of the laminate including the D layer may be impaired. On the other hand, if the relaxation rate exceeds 20%, the film may slacken too much inside the tenter, causing wrinkles in the film after film formation, which may lead to deterioration of mechanical properties and unevenness during vapor deposition.

[0089] After the heat treatment and relaxation treatment, the film is guided outside the tenter, the clips at both ends of the film width direction are released in a room temperature atmosphere, and the film edges are slit in a winding process. Thereafter, in order to improve the adhesion of the vapor-deposited layer to the surface to be vapor-deposited during use (usually the surface of layer A), corona discharge treatment or plasma treatment is preferably performed in air or in an atmospheric gas of oxygen, nitrogen, hydrogen, argon, carbon dioxide, silane gas, or a mixture thereof. Among these, nitrogen or a mixed gas containing nitrogen is particularly preferred. The polypropylene film of the present invention thus obtained can be wound into a roll to obtain the final product roll.

[0090] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments shown below. Each item was evaluated by the following methods.

[0091] <Methods for Measuring Characteristic Values ​​and Methods for Evaluating Effects> The methods for measuring characteristic values ​​and evaluating effects in the present invention are as follows.

[0092] (1) Thickness of Polypropylene Film The thickness of ten randomly selected points on the polypropylene film was measured in an atmosphere of 23°C and 65% RH using a contact-type electronic micrometer (K-312A model) manufactured by Anritsu Corporation. The arithmetic mean value of the thicknesses at the ten points was taken as the thickness (unit: μm) of the polypropylene film.

[0093] (2) Skewness Ssk(A), Ssk(B), and Ssk(D) Measurement of skewness Ssk was performed using a scanning white light interference microscope VS1540 manufactured by Hitachi High-Tech Science Corporation, a three-dimensional non-contact surface profile measuring instrument. Furthermore, for analysis, the accompanying analysis software was used to remove waviness components from the captured image using polynomial fourth-order approximation surface correction, followed by processing with a median (3 × 3) filter, followed by interpolation (processing in which height data for pixels for which height data could not be obtained is supplemented with height data calculated from surrounding pixels). Measurements were performed at five arbitrary locations on the film surface: side B (B layer surface), side A (A layer surface), and side D (D layer surface) in the case of a laminate having an inorganic compound layer or a metal layer laminated thereon, and the average value was calculated. The measurement conditions were as follows: <Measurement conditions> Manufacturer: Hitachi High-Tech Science Corporation Device name: Scanning white light interference microscope VS1540 Measurement conditions: Objective lens 10x Lens tube 1x Zoom lens 1x Wavelength filter 530 nm white Measurement mode: Wave Measurement software: VS-Measure Version 10.0.4.0 Analysis software: VS-Viewer Version 10.0.3.0 Measurement area: 0.561 x 0.561 mm 2 .

[0094] (3) Surface roughness Sa Sa(A) and Sa(B) were measured using the same equipment, measurement conditions, measurement mode, measurement software, analysis software, and measurement area as in (2) Skewness (Ssk). Measurements were taken at five arbitrary points on each of the A and B film surfaces, and the average value was calculated.

[0095] (4) Thickness of each layer of A, B, and C layers in polypropylene film, and D layer corresponding to an inorganic compound layer or metal layer. In the case of a laminate in which a film or an inorganic compound layer or a metal layer was laminated, the laminate was embedded in epoxy resin, and ultrathin sections were prepared using a microtome so that the longitudinal-thickness cross section of the film was the observation surface. Photographs of the cross section of the ultrathin section were taken at 20,000x magnification using a transmission electron microscope, and the thickness of each layer in the center of the film width direction was confirmed. The thickness units of the observed A, B, and C layers were "μm," and the thickness unit of the D layer was "nm."

[0096] (5) Static friction coefficient (μs) Measured at 25°C and 65% RH using a slip tester manufactured by Toyo Seiki Co., Ltd. in accordance with JIS K 7125 (1999). The measurement was performed with the film longitudinal direction aligned and with one surface of the film overlapping the other surface. The test was performed five times, and the average value of the obtained values ​​was calculated to be the static friction coefficient (μs) of the sample.

[0097] (6) Sum of Heat Shrinkage in the Longitudinal and Transverse Directions at 125°C for 10 Minutes The heat shrinkage of polypropylene film was measured in the longitudinal and transverse directions using the following method. A sample with the long side in the measurement direction was cut into a rectangle measuring 70 mm in length and 10 mm in width. Marks were made 10 mm from both ends so that the test length was 50 mm. The distance between the marks was measured using a Nikon V-16A universal projector to determine the test length (l0). Next, the test piece was sandwiched between paper and heated for 10 minutes in an oven maintained at 125°C under zero load. After removal, it was cooled at room temperature and the dimension (l1) was measured in the same manner. The heat shrinkage was calculated from the obtained l0 and l1 using the following formula, and the average of five samples was taken as the heat shrinkage in each direction, and the sum was calculated. Heat shrinkage = {(l0 - l1) / l0} x 100 (%).

[0098] (7) Melting Point of Polypropylene Resin Using a differential scanning calorimeter (EXSTAR DSC6220 manufactured by Seiko Instruments, Inc.), a 3 mg polypropylene resin sample was heated from 30°C to 260°C at a rate of 20°C / min in a nitrogen atmosphere. After holding at 260°C for 5 minutes, the sample was cooled to 30°C at a rate of 20°C / min. After holding at 30°C for 5 minutes, the sample was heated from 30°C to 260°C at a rate of 20°C / min. The peak temperature of the endothermic curve obtained during this temperature increase was taken as the melting point of the polypropylene resin. When multiple peak temperatures were observed, the highest temperature was taken as the melting point of the polypropylene resin.

[0099] (8) Heat Sealability A 12 μm-thick stretched PET film ("Lumirror" (registered trademark) Type S10, manufactured by Toray Industries, Inc.) was superimposed on the surface of Layer B of the polypropylene film and heat-sealed using a flat heat sealer under the following conditions to prepare a laminated product. A T-peel test was performed on the interface between the polypropylene film of the present invention and the stretched PET film using "Tensilon" (registered trademark) manufactured by Orientec Co., Ltd., to measure the heat seal strength. The laminated product for the peel test was sampled in a strip shape measuring 20 mm wide and 150 mm long, and the heat seal strength was measured at a pulling rate of 300 mm / min. This measurement was performed three times, and the average of the obtained values ​​was calculated, which was used as the heat seal strength (N / 25.4 mm). When a heat seal strength of 2 N / 25.4 mm or more was achieved, the heat sealability was judged to be acceptable (◯), and when it was less than 2 N / 25.4 mm, the heat sealability was judged to be unacceptable (×). <Heat Sealing Conditions> Press pressure: 0.4 N / mm 2 Pressing time: 1 sec. Heater temperature: 120°C.

[0100] (9) Adhesion of the Deposited Layer A film roll was set in a vacuum deposition device equipped with a film running device, and the film was -2After the pressure was reduced to a high vacuum of 100 Pa, the film was run through a cooled metal drum at 20°C, and aluminum metal was heated and evaporated to form a vapor-deposited thin film layer on Layer A. The thickness of the vapor-deposited film was controlled to be approximately 40 nm. After vapor deposition, the pressure inside the vacuum vapor deposition apparatus was returned to normal pressure, and the rolled film was rewound and aged at 40°C for two days to obtain a laminate with a vapor-deposited layer of Al (aluminum) laminated on the film. Next, Nichiban's "Cellotape" (registered trademark) was applied to the surface of the vapor-deposited layer of the resulting laminate with a rubber roller at a load of 2 kg and peeled at a peel angle of 180° and a peel speed of 3000 m / min using a peel tester. The surface of the laminate after peeling the cellophane tape was visually inspected, and the adhesion of the vapor-deposited layer was evaluated according to the following criteria: ○ or above was considered good adhesion, and △ was considered acceptable for practical use. (Evaluation Criteria) ⊚: No vapor-deposited layer peeled off at all. ○: Most of the vapor-deposited layer was not peeled off, but a small amount was peeled off. Δ: A small part of the vapor-deposited layer is not peeled off, but the majority is peeled off. ×: The entire vapor-deposited layer is peeled off.

[0101] (10) Water Vapor Permeability (Water Vapor Barrier Property) After Al Vapor Deposition or AlOx Vapor Deposition The laminate on which Al was vapor-deposited was obtained by the method described in (9). For the laminate on which AlOx was vapor-deposited, a film roll was set in a vacuum vapor deposition device equipped with a film running device, and a 1.00 × 10 -2 After the pressure was reduced to a high vacuum of 100 Pa, the film was run through a cooled metal drum at 20°C, and oxygen gas was introduced to reactively evaporate AlOx, forming a vapor-deposited layer on Layer A. Control was exercised to ensure that the vapor-deposited layer had a thickness of approximately 20 nm. After vapor deposition, the pressure inside the vacuum vapor deposition apparatus was returned to normal pressure, and the film was rewound and aged at 40°C for 2 days in the rolled state, yielding a laminate in which a vapor-deposited layer of AlOx was laminated on a polypropylene film.

[0102] The laminates on which Al vapor deposition or AlOx vapor deposition was performed were measured at a temperature of 40°C and a humidity of 90% RH using a water vapor transmission rate measuring device PERMATRAN-W3 / 30 manufactured by MOCON / Modern Controls. Measurements were performed five times for each sample, and the average of the obtained values ​​was calculated and used as the water vapor transmission rate of the film (unit: g / m 2 / day). From the obtained water vapor transmission rate, the water vapor barrier property of the laminate was judged according to the following criteria. ◯ or above was considered to be good water vapor barrier property, and △ was considered to be at a level that presents no problems in practical use. 2 / day or less. ○: 0.5g / m 2 / day and greater than 1.0 g / m 2 / day or less. △: 1.0g / m 2 / day and greater than 2.0 g / m 2 / day or less. ×: 2.0g / m 2 / day is greater.

[0103] (11) Oxygen permeability (oxygen barrier property) after Al vapor deposition or AlOx vapor deposition Laminates having an Al vapor deposition layer or an AlOx vapor deposition layer were obtained by the methods described in (9) and (10). The oxygen permeability of each laminate was measured at a temperature of 23°C and a humidity of 0% RH using an oxygen permeability measuring device Oxtran 2 / 20 manufactured by MOCON / Modern Controls. The measurement was performed five times for each sample, and the average value was calculated and used as the oxygen permeability of the film (unit: cc / m 2 / day). The oxygen barrier properties of the laminate were evaluated based on the obtained oxygen permeability according to the following criteria. ◯ or higher was considered to be good oxygen barrier properties, and △ was considered to be at a level that presents no practical problems. 2 / day or less. ○: 10cc / m 2 / day or more than 20cc / m 2 / day or less. △:20cc / m 2 / day and greater than 40cc / m 2 / day or less. ×: 40cc / m 2 / day is greater.

[0104] <Components used in producing polypropylene films in each example and comparative example> The following components were used in producing the polypropylene films in each example and comparative example. Note that MFR is a value measured at 230°C under a load of 21.18 N unless otherwise specified.

[0105] (Polypropylene-based resin for layer A) A1: Homopolypropylene resin ("F133A" manufactured by Prime Polymer Co., Ltd. (mesopentad fraction: 0.97, melting point: 167°C, MFR: 3.0g / 10min, CXS: 1.5% by mass, propylene unit fraction: 99.5 mol% or more)) A2: Homopolypropylene resin ("F113G" manufactured by Prime Polymer Co., Ltd. (mesopentad fraction: 0.94, melting point: 162°C, MFR: 2.9g / 10min, CXS: 3.8% by mass, propylene unit fraction: 99.5 mol% or more)) A3: Ethylene-propylene random copolymer ("WFW4M" manufactured by Japan Polypropylene Corporation (melting point: 135°C, MFR: 7.0g / 10min, metallocene-based, propylene content: 95.0%)) A4: Homopolypropylene resin (manufactured by Repsol (melting point: 153°C, MFR: 3.0 g / 10 min, CXS: 1.5 mass%, propylene unit fraction: 99.5 mol% or more)).

[0106] (Masterbatch for Layer A) AM1: A masterbatch prepared by kneading and extruding A2 (90 parts by mass), polymethylpentene resin 2 (10 parts by mass), and antioxidant (0.1 parts by mass) in an extruder set at 260°C, and then water-cooling the strands and chipping them.

[0107] (Polypropylene Resin for Layer B) B1: Ethylene-propylene random copolymer ("WFW5T" manufactured by Japan Polypropylene Corporation (melting point: 130°C, MFR: 3.5g / 10min, metallocene type)) B2: Homopolypropylene resin (same as A1).

[0108] (Masterbatch for Layer B) BM1: A masterbatch prepared by kneading and extruding B1 (90 parts by mass), polymethylpentene resin 1 (10 parts by mass), and antioxidant (0.1 parts by mass) using an extruder set at 260°C, followed by water-cooling and chipping the strands. BM2: A masterbatch prepared by kneading and extruding B1 (90 parts by mass), polymethylpentene resin 2 (10 parts by mass), and antioxidant (0.1 parts by mass) using an extruder set at 260°C, followed by water-cooling and chipping the strands. BM3: A masterbatch prepared by kneading and extruding B2 (90 parts by mass), polymethylpentene resin 1 (10 parts by mass), and antioxidant (0.1 parts by mass) using an extruder set at 260°C, followed by water-cooling and chipping the strands.

[0109] (Polypropylene Resin for Layer C) C1: Homopolypropylene resin ("HA3105" manufactured by Basell (melting point: 165°C, MFR: 3.0 g / 10 min, CXS: 2.5 mass%, propylene unit fraction: 99.5 mol% or more)) C2: Homopolypropylene resin ("FY6H" manufactured by Japan Polypropylene Corporation (mesopentad fraction: 0.92, melting point: 161°C, MFR: 3.3 g / 10 min, CXS: 4.1 mass%, propylene unit fraction: 99.5 mol% or more))).

[0110] (Masterbatch for Layer C) CM1: A masterbatch prepared by kneading and extruding C1 (70 parts by mass), petroleum resin 1 (30 parts by mass), and antioxidant (0.1 parts by mass) in an extruder set at 240°C, followed by water-cooling and chipping the strands. CM2: A masterbatch prepared by kneading and extruding C2 (70 parts by mass), petroleum resin 1 (30 parts by mass), and antioxidant (0.1 parts by mass) in an extruder set at 240°C, followed by water-cooling and chipping the strands.

[0111] (Resins other than polypropylene resins) Polymethylpentene resin 1: "TPX" (registered trademark) manufactured by Mitsui Chemicals, Inc. (DX845, melting point 232 ° C., MFR: 9 g / 10 min (measured at a temperature of 260 ° C.)) Polymethylpentene resin 2: "TPX" (registered trademark) manufactured by Mitsui Chemicals, Inc. (MX004, melting point 228 ° C., MFR: 25 g / 10 min (measured at a temperature of 260 ° C.)) Petroleum resin 1: T-REZ HA125 (manufactured by JXTG Energy Corporation).

[0112] (Additives, etc.) Antioxidant: "Irganox" (registered trademark) 1010 (manufactured by BASF Japan Ltd.) P1: Silica particles (SFP-20MHE (silane coupling surface treatment) manufactured by Denki Kagaku Kogyo Co., Ltd.) (average particle size: 0.3 μm).

[0113] Example 1: A1 was used as the raw material for Layer A. A mixture of B1 and BM1 at a mass ratio of 80:20 was used as the raw material for Layer B. A mixture of C1 and CM1 at a mass ratio of 75:25 was used as the raw material for Layer C. These raw materials were fed into separate single-screw extruders and melt-extruded at 260°C. After removing foreign matter with an 80 μm cutoff sintered filter, the extrusion rate was adjusted using a feed block to achieve a three-layer A / C / B laminate with a lamination ratio of 1 / 23 / 1. The molten laminated polymer was then extruded from a T-die. The extruded molten sheet was then placed on a casting drum maintained at 20°C, adhered with an air knife so that the Layer A side was in contact with the drum surface, and cooled and solidified to obtain an unstretched sheet. The unstretched sheet was then preheated stepwise to 105°C using a group of rolls, passed through rolls with different peripheral speeds, and stretched 5.2 times in the longitudinal direction to obtain a uniaxially oriented film. The obtained uniaxially oriented film was then introduced into a tenter, and while both ends of the film in the width direction were held with clips, it was stretched 10.5 times in the width direction at 165°C, and then heat-treated at 155°C while giving 10% relaxation in the width direction. Thereafter, the film was introduced to the outside of the tenter, and the clips at both ends of the film in the width direction were released. Next, a 25 W·min / m 2The corona discharge treatment was carried out in a mixed gas atmosphere of carbon dioxide and nitrogen gas, with the carbon dioxide concentration adjusted to 15% by volume, at a treatment intensity of 1000 psi. Finally, the biaxially oriented polypropylene film thus obtained, having a thickness of 25 μm, was wound into a roll. Furthermore, a laminate was obtained in which an Al vapor-deposited layer was provided as Layer D on the A side of the film of this example. The properties of the obtained biaxially oriented polypropylene film and laminate are shown in Table 1.

[0114] (Example 2) A biaxially oriented polypropylene film was produced in the same manner as in Example 1, and a laminate was obtained in which an AlOx vapor-deposited layer was provided as Layer D on the Layer A side of the biaxially oriented polypropylene film. The properties of the obtained biaxially oriented polypropylene film and laminate are shown in Table 1.

[0115] (Examples 3 to 10, Comparative Examples 2 to 4) Biaxially oriented polypropylene films and laminates were obtained in the same manner as in Example 2, except that the raw materials and film-forming conditions were changed as shown in Table 1. The properties of the obtained biaxially oriented polypropylene films and laminates are shown in Table 1.

[0116] (Comparative Example 1) A1 was used as the raw material for Layer A, and was fed into a single-screw extruder and melt-extruded at 250 ° C. After removing foreign matter with an 80 μm cut sintered filter, the molten polymer was extruded from a T-die. The extruded molten sheet was then placed on a casting drum maintained at 30 ° C., brought into close contact with an air knife, and cooled and solidified to obtain an unstretched sheet. Next, the unstretched sheet was preheated stepwise to 135 ° C. using a group of rolls, passed through rolls with different peripheral speeds, and stretched 4.5 times in the longitudinal direction to obtain a uniaxially oriented film. The resulting uniaxially oriented film was then introduced into a tenter, stretched 8.2 times in the width direction at 160 ° C. while holding both ends of the film width direction with clips, and then heat-treated at 168 ° C. while providing 6.7% relaxation in the width direction. The film was then introduced to the outside of the tenter, and the clips on both ends of the film width direction were released. Then, the film surface (the side contacting the casting drum: Layer A) was stretched at 25 W·min / m 2The biaxially oriented polypropylene film was then wound into a roll. The properties of the biaxially oriented polypropylene film and laminate are shown in Table 1.

[0117] Comparative Example 5: A mixture of A2 and AM1 at a mass ratio of 80:20 was used as the raw material for Layer A. A mixture of A2 and AM2, the same raw materials as those for Layer A, at a mass ratio of 80:20 was used as the raw material for Layer B. C1 was used as the raw material for Layer C. These raw materials were fed into separate single-screw extruders and melt-extruded at 260°C. After removing foreign matter with an 80 μm cutoff sintered filter, the extrusion rate was adjusted using a feed block to achieve a three-layer A / C / B laminate with a lamination ratio of 1 / 22 / 1, and the molten laminated polymer was extruded from a T-die. A biaxially oriented polypropylene film and laminate were obtained in the same manner as in Example 2, except that the film-forming conditions were changed as shown in Table 1. The properties of the obtained biaxially oriented polypropylene film and laminate are shown in Table 1.

[0118]

[0119] Since Comparative Example 1 had a single layer structure, the layer constituting the film was treated as Layer A. Comparative Examples 2 and 3 did not contain a thermoplastic resin that is incompatible with polypropylene-based resins, but the layer containing B1 as the main component was considered as Layer B. The fraction of propylene units in Layer A of Comparative Example 5 was calculated by regarding the fraction of propylene units in A2 as 100 mol %.

[0120] The polypropylene film of the present invention is structurally stable against heat during vapor deposition and has appropriate slip properties without the use of antiblocking agents or particles, and therefore has excellent water vapor barrier properties and oxygen barrier properties, particularly when a transparent vapor-deposited layer is laminated thereon, making it suitable for use in packaging applications.

Claims

1. The present invention relates to a polypropylene film having at least two types of layers (layer A and layer B) mainly composed of a polypropylene-based resin, the layer B containing a thermoplastic resin which is incompatible with the polypropylene-based resin, and a skewness Ssk of the layer A and the layer B measured by a three-dimensional non-contact surface shape measurement is Ssk(A) and Ssk(B), respectively, wherein the Ssk(B) is 5 or more and the Ssk(A) is less than 5; A laminate, characterized in that when a layer D contains more than 50 mass% and 100 mass% or less of a metal and / or inorganic compound in total, the layer D is in contact with the layer A of the polypropylene film, and the thickness of the layer D is 50 nm or less.

2. a polypropylene film having at least two types of layers (layer A, layer B) mainly composed of a polypropylene-based resin, the layer B containing a thermoplastic resin that is incompatible with the polypropylene-based resin, wherein when the skewness Ssk of the layer A measured by three-dimensional non-contact surface shape measurement is Ssk(A) and the surface roughness Sa of the layer A and the layer B are Sa(A) and Sa(B), respectively, the Ssk(A) is less than 5, and the Sa(A) and the Sa(B) satisfy formula 1; A laminate, characterized in that when a layer D contains more than 50 mass% and 100 mass% or less of a metal and / or inorganic compound in total, the layer D is in contact with the layer A of the polypropylene film, and the thickness of the layer D is 50 nm or less. Formula 1: Sa(B) / Sa(A)>1.1

3. 3. The laminate according to claim 1, wherein the fraction of propylene units in the resin component constituting the A layer is 97.0 mol% or more and 100.0 mol% or less, and is equal to or greater than the fraction of propylene units in the resin component constituting the entire polypropylene film.

4. The laminate according to any one of claims 1 to 3, wherein the polypropylene resin which is the main component of the layer A has a melting point of 151°C or higher.

5. The laminate according to claim 1, 3, or 4, wherein when the surface roughness Sa of the A layer and the B layer are Sa(A) and Sa(B), respectively, the Sa(A) and the Sa(B) satisfy formula 1. Formula 2: Sa(B) / Sa(A)>1.0

6. The laminate according to any one of claims 1 to 5, wherein the layer B is a layer having heat sealability.

7. The laminate according to any one of claims 1 to 6, further comprising a layer (layer C) mainly composed of a polypropylene-based resin between the layer A and the layer B.

8. The laminate of claim 7 , wherein the C layer comprises a petroleum resin.

9. The laminate according to any one of claims 1 to 8, which is used for packaging purposes.

10. The laminate according to any one of claims 1 to 9, wherein Ssk(D) is less than 5, where Ssk(D) is the skewness Ssk of the D layer measured by a three-dimensional non-contact surface roughness meter.

11. A packaging material comprising the laminate according to any one of claims 1 to 10.

12. A package comprising the packaging material according to claim 11 and contents packed therein.