Secondary battery
Patent Information
- Application Number
- JP2022521980
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2022-03-28
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2042-03-28
AI Technical Summary
Metal-air batteries face issues with product solid precipitation, safety concerns due to dendrites, and limited practicality when using aqueous electrolytes, and existing solutions with glass ceramic or polymer coatings do not adequately address these problems, particularly in terms of flexibility and separation efficiency.
A secondary battery design incorporating a non-aqueous electrolyte and an aqueous electrolyte with a separator that has high air permeability, ionic conductivity, and a polymer film with specific contact angles and meltdown temperature, using aromatic polyamides or polyimides to separate the electrolytes effectively.
The solution enhances battery capacity and cycle characteristics by preventing electrolyte mixing and ensuring safety through effective separation and ion conductivity, while maintaining structural integrity and flexibility.
Abstract
Description
secondary battery
[0001] The present invention relates to a secondary battery.
[0002] In recent years, the miniaturization of portable electronic devices has progressed rapidly, and their power sources are also required to have higher energy densities. Toward lighter and more energy-efficient batteries, active research has been conducted on metal Li anodes, all-solid-state batteries, and air batteries. In particular, the evolution of the cathode into an air cathode that uses air as an energy source will enable a dramatic weight reduction compared to current oxide batteries, and therefore will have a higher capacity than the currently widely used lithium secondary batteries, making them promising as next-generation power sources. Known examples of air batteries include metal-air batteries, such as lithium-air batteries, magnesium-air batteries, and zinc-air batteries.
[0003] For practical use, metal-air batteries face many challenges in the design of the positive electrode, negative electrode, separator, electrolyte, etc. A problem has arisen in that solids produced by the electrode reaction at the positive electrode (hereinafter referred to as "solid products") accumulate at the air electrode, clogging the air electrode and blocking contact between the electrolyte and air, which impedes charging and discharging.
[0004] As a technique for solving the problem of precipitation of the solid product, the use of an aqueous electrolyte as the electrolyte of a metal-air battery has been proposed. In the case of a metal-air battery using an aqueous electrolyte, a metal hydroxide is generated as the solid product, and since the solid product is water-soluble, the solid product can be dissolved in the aqueous electrolyte, thereby suppressing precipitation of the solid product.
[0005] However, metal-air batteries using aqueous electrolytes have the problem that if the saturated solubility of the salt in the aqueous electrolyte is exceeded, a solid product precipitates, causing the battery to become inactive. In addition, when metallic lithium is used in the negative electrode, practical use is difficult from a safety standpoint.
[0006] Furthermore, the negative electrode also faces the problem of reduced safety and reduced lifespan due to dendrites in various metal negative electrodes.
[0007] Therefore, it is important to solve the above problems of air batteries by using two different types of electrolytes in combination.
[0008] As an approach to using two different types of electrolytes in combination, Patent Document 1 proposes improving battery characteristics by placing an aqueous electrolyte solution on the positive electrode side and an ion-conductive glass ceramic on the negative electrode side. Patent Document 2 proposes providing a polymer-containing electrolyte coating layer on the surface of a lithium ion-conductive solid electrolyte to protect the negative electrode and improve characteristics.
[0009] JP 2010-192313 A JP 2017-191766 A
[0010] However, Patent Document 1 uses glass ceramic, which has high strength but poor flexibility and insufficient separation of the aqueous electrolyte when subjected to impact, and Patent Document 2 does not use or cannot use an aqueous electrolyte, and therefore is not considered to contribute to solving the fundamental problems of air electrodes.
[0011] Therefore, in view of the above problems, an object of the present invention is to provide a secondary battery using a nonaqueous electrolyte solution and an aqueous electrolyte solution, which has a high battery capacity and excellent cycle characteristics by using a separator that can separate the nonaqueous electrolyte solution and the aqueous electrolyte solution.
[0012] In order to solve the above problems, the secondary battery of the present invention has the following configuration: (1) A secondary battery including a positive electrode, a negative electrode, a non-aqueous electrolyte, an aqueous electrolyte, and a separator, wherein the positive electrode is an air electrode, the negative electrode is composed of a negative electrode current collector and a negative electrode mixture layer formed thereon, the negative electrode mixture layer containing one or more components selected from the group consisting of metallic lithium, magnesium, zinc, and aluminum, and the separator has an air permeability of more than 10,000 seconds and an ionic conductivity of 1×10 -5A secondary battery, wherein the polymer film has a water contact angle of 90° or more and a viscosity of 1000 S / cm or more. (2) The secondary battery according to (1), wherein the rate of change in the contact angle of the polymer film after 1 hour from the time when water is dropped onto the polymer film relative to the contact angle after 10 seconds from the time when water is dropped onto the polymer film is less than 10%. (3) The secondary battery according to (1) or (2), wherein the contact angle of the polymer film measured using dimethyl carbonate is 90° or more. (4) The secondary battery according to any one of (1) to (3), wherein the rate of change in the contact angle of the polymer film after 1 hour from the time when dimethyl carbonate is dropped onto the polymer film relative to the contact angle after 10 seconds from the time when dimethyl carbonate is dropped onto the polymer film is less than 10%. (5) The secondary battery according to any one of (1) to (4), wherein the meltdown temperature of the polymer film is 300° C. or more. (6) The secondary battery according to any one of (1) to (5), wherein the polymer constituting the polymer film includes aromatic polyamide, aromatic polyimide, or aromatic polyamideimide.
[0013] According to the present invention, a secondary battery having a high battery capacity and excellent cycle characteristics can be provided.
[0014] A secondary battery according to an embodiment of the present invention will be described in detail below. The secondary battery according to the embodiment of the present invention is a secondary battery including a positive electrode, a negative electrode, a non-aqueous electrolyte, an aqueous electrolyte, and a separator, in which the positive electrode is an air electrode, the negative electrode is composed of a negative electrode current collector and a negative electrode mixture layer formed thereon, the negative electrode mixture layer containing one or more components selected from the group consisting of metallic lithium, magnesium, zinc, and aluminum, and the separator has an air permeability of more than 10,000 seconds and an ionic conductivity of 1×10 -5 The secondary battery is a polymer film having a conductivity of 100 S / cm or more and a water contact angle of 90° or more.
[0015] [Positive Electrode] In an embodiment of the present invention, the electrode used as the positive electrode is an air electrode that uses air as an energy source. The air electrode may be, for example, a porous carbon sheet carrying an oxygen reduction catalyst such as platinum, or a sheet of highly catalytically active carbon, such as graphene or carbon nanotubes. Examples of the porous carbon sheet include carbon paper, carbon black, and acetylene black sheets.
[0016] The negative electrode includes a negative electrode current collector and a negative electrode mixture layer formed on the negative electrode current collector. The negative electrode current collector may be made of, for example, copper, nickel, or stainless steel.
[0017] In an embodiment of the present invention, the negative electrode active material contained in the negative electrode mixture layer contains one or more components selected from the group consisting of metallic lithium, magnesium, zinc, and aluminum. Among these, metallic lithium is preferably used from the viewpoints of the operating voltage of the battery and the theoretical capacity of the negative electrode active material.
[0018] The negative electrode is produced, for example, as follows: In the case of metallic lithium, lithium nanoparticles can be produced on a negative electrode current collector by gas deposition, and then spray-depositing the nanoparticles together with He gas.
[0019] [Electrolyte] The electrolyte used in the embodiment of the present invention is a non-aqueous electrolyte solution or an aqueous electrolyte solution. The non-aqueous electrolyte solution is composed of an organic solvent and a solute.
[0020] As the organic solvent for the non-aqueous electrolyte, cyclic esters, chain esters, cyclic ethers, chain ethers, amides, etc. are used, and specific examples thereof include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), γ-butyrolactone (γBL), 2-methyl-γ-butyrolactone, acetyl-γ-butyrolactone, γ-valerolactone, 1,2-dimethoxyethane (DME), 1,2-ethoxyethane, diethyl ether, ethylene glycol dialkyl ether, diethylene glycol dialkyl ether, triethylene glycol dialkyl ether, tetraethylene glycol dialkyl ether, dipropyl carbonate, methyl butyl carbonate, methyl Organic solvents such as methyl propyl carbonate, ethyl butyl carbonate, ethyl propyl carbonate, butyl propyl carbonate, alkyl propionate, dialkyl malonate, alkyl acetate, tetrahydrofuran (THF), alkyl tetrahydrofuran, dialkyl alkyl tetrahydrofuran, alkoxy tetrahydrofuran, dialkoxy tetrahydrofuran, 1,3-dioxolane, alkyl-1,3-dioxolane, 1,4-dioxolane, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, methyl propionate, ethyl propionate, phosphate triester, and N-methyl-2-pyrrolidone, as well as derivatives and mixtures thereof, are preferably used.
[0021] As the solute contained in the non-aqueous electrolyte, alkali metal halides, particularly lithium halides, perchlorates, thiocyanates, boron fluorides, phosphorus fluorides, arsenic fluorides, aluminum fluorides, trifluoromethyl sulfates, etc. are preferably used. For example, lithium perchlorate (LiClO 4 ), lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium arsenic hexafluoride (LiAsF6 ), lithium trifluoromethasulfonate (LiCF 3 SO 3 ), lithium bistrifluoromethylsulfonylimide [LiN(CF 3 SO 2 ) 2 However, lithium hexafluorophosphate is preferred from the viewpoint of oxidation resistance and reduction resistance.
[0022] The amount of solute dissolved in the organic solvent is preferably 0.5 to 3.0 mol / L, and more preferably 0.8 to 1.5 mol / L.
[0023] The non-aqueous electrolyte may contain additives, if necessary, such as vinylene carbonate, fluoroethylene carbonate, ethylene sulfite, 1,4-butane sultone, propane sultone, 2,4-difluoroanisole, biphenyl, cyclohexylbenzene, and the like, and one or more of these may be used.
[0024] Aqueous electrolytes include acidic electrolytes and alkaline electrolytes. Acidic electrolytes include, for example, hydrochloric acid, sulfuric acid, and hydrofluoric acid. Alkaline electrolytes include, for example, potassium hydroxide aqueous solution, calcium hydroxide aqueous solution, sodium hydroxide aqueous solution, and lithium hydroxide.
[0025] In addition, in view of the safety, life characteristics and stable operation of the battery, it is preferable that the electrolyte in the secondary battery of the present invention is an aqueous electrolyte on the positive electrode side and a non-aqueous electrolyte on the negative electrode side.
[0026] [Separator] The separator has an air permeability of more than 10,000 seconds and an ionic conductivity of 1×10 -5 The polymer film has a viscosity of 1000 S / cm or more and a water contact angle of 90° or more.
[0027] In a battery using two types of electrolytes, a non-aqueous electrolyte and an aqueous electrolyte, the separator must have an air permeability of more than 10,000 seconds because the electrolytes must be separated. Note that when the air permeability is more than 10,000 seconds, the separator can be considered to have a non-porous structure in which there are substantially no continuous pores.
[0028] Since the separator must not swell with the electrolyte and must not allow the aqueous electrolyte to pass through, it is important that the separator be a polymer film with a water contact angle of 90° or more. If the water contact angle is less than 90%, the aqueous electrolyte may pass through the separator and mix with the nonaqueous electrolyte, which may result in a deterioration in battery characteristics. Furthermore, from the viewpoint of enabling separation of the electrolyte during battery use and battery characteristics, the rate of change in the contact angle of the separator 1 hour after dropping water relative to the contact angle 10 seconds after dropping water is preferably less than 10%, more preferably less than 7%.
[0029] In addition, since the separator must not swell in a non-aqueous electrolyte and must not allow the non-aqueous electrolyte to pass through, it is preferable that the separator be a polymer film having a contact angle of 90° or more when measured with dimethyl carbonate. From the viewpoint of enabling separation of the electrolyte during battery use and battery characteristics, the rate of change in the contact angle of the separator 1 hour after dropping dimethyl carbonate relative to the contact angle 10 seconds after dropping dimethyl carbonate is preferably less than 10%, more preferably less than 7%.
[0030] Since the separator has a non-porous structure, it cannot be impregnated with an electrolyte and does not swell with the electrolyte. Therefore, it is important from the viewpoint of battery performance that the polymer membrane has ionic conductivity. The ionic conductivity, which is an index of the ionic conductivity of the separator, is 1 × 10 -5 It is important that the ionic conductivity is 1×10 S / cm or more. -5 If the electrical conductivity is less than S / cm, the resistance is high and the battery characteristics may be deteriorated.
[0031] From the viewpoint of battery safety, the meltdown temperature of the separator is preferably 300°C or higher, and more preferably 350°C or higher.
[0032] The polymer membrane that achieves the above separator will now be described in detail.
[0033] As the polymer constituting the polymer membrane serving as the separator, a polymer having an aromatic ring on the main chain is suitable, as it combines heat resistance, strength, and flexibility. Examples of such polymers include aromatic polyamide (aramid), aromatic polyimide, aromatic polyamideimide, aromatic polyetherketone, aromatic polyetheretherketone, aromatic polyarylate, aromatic polysulfone, aromatic polyethersulfone, aromatic polyetherimide, and aromatic polycarbonate. Blends of multiple polymers may also be used. Among these, aromatic polyamide, aromatic polyimide, or aromatic polyamideimide preferably accounts for 30 to 100% by mass, based on the total mass of the membrane as 100%, because they have excellent heat resistance and tend to maintain high strength when thinned. More preferably, the content is 50 to 100% by mass.
[0034] As a polymer that can be suitably used in the present invention, it is preferable that the polymer constituting the film contains a polymer having a structure represented by any one of the following chemical formulas (I) to (III), and examples of the aromatic polyamide include those having a repeating unit represented by the following chemical formula (I), the aromatic polyimide includes those having a repeating unit represented by the following chemical formula (II), and the aromatic polyamideimide includes those having a repeating unit represented by the following chemical formula (III): Chemical Formula (I):
[0035]
[0036] Chemical formula (II):
[0037]
[0038] Chemical formula (III):
[0039]
[0040] Here, Ar in chemical formulas (I) to (III) 1 and / or Ar 2 are aromatic groups, and each may be a single group or a multi-component copolymer with multiple groups. The bonds constituting the main chain on the aromatic ring may be either meta-oriented or para-oriented. Furthermore, some of the hydrogen atoms on the aromatic ring may be substituted with any group.
[0041] In the present invention, one method for achieving both separation of the electrolyte solution, heat resistance, and excellent ion conductivity is to transport ions by hopping by controlling the polarity of the polymer.
[0042] In the present invention, when an aromatic polyamide, aromatic polyimide, or aromatic polyamideimide is used, the carbonyl group in the structure generally serves as a site with high affinity for lithium ions. Therefore, in order for lithium ions to move through the polymer film, a site with lower affinity for lithium ions than the carbonyl group is required, and therefore it is preferable to have an ether bond or a thioether bond in the main chain or side chain (in the main chain or on the side chain). More preferably, it has an ether bond in the main chain, or at least one of a carboxylic acid group, a carboxylate group, a sulfonic acid group, a sulfonate group, an alkoxy group, and a cyanate group as a substituent on the aromatic ring. Even more preferably, Ar in chemical formulas (I) to (III) 1 and Ar 2 The total of all groups represented by the formulas (IV) to (VI) preferably accounts for 25 to 100 mol % of at least one group selected from the groups represented by the formulas (IV) to (VI), and more preferably the proportion is 50 to 100 mol %.
[0043]
[0044] (The double broken lines in chemical formulas (IV) to (VI) represent one or two bonds.) Here, some of the hydrogen atoms on the aromatic rings of chemical formulas (IV) to (VI) may be substituted with any group, such as a halogen group such as fluorine, bromine, or chlorine; a nitro group; a cyano group; an alkyl group such as methyl, ethyl, or propyl; an alkoxy group such as methoxy, ethoxy, or propoxy; or a carboxylic acid group.
[0045] It is also preferable to add a lithium salt to facilitate ion conduction in the polymer film, and it is even more preferable to add a lithium salt with a large anion radius and high dissociation rate of lithium ions to further improve ion conductivity. Here, the lithium salt to be added can be the same as the solute contained in the electrolyte. Among them, lithium perchlorate (LiClO 4 ), lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium arsenic hexafluoride (LiAsF 6 ), lithium trifluoromethasulfonate (LiCF 3 SO 3 ), lithium bistrifluoromethylsulfonylimide [LiN(CF 3 SO 2 ) 2 From the viewpoint of anion radius and dissociation property of lithium ions, lithium trifluoromethasulfonate (LiCF 3 SO 3 ), lithium bistrifluoromethylsulfonylimide [LiN(CF 3 SO 2 ) 2 ] is preferably added. More preferably, lithium bistrifluoromethylsulfonylimide [LiN(CF 3 SO 2 ) 2 The addition of ] is preferred.
[0046] Next, a method for producing the polymer membrane that serves as the separator will be described below.
[0047] [Polymer synthesis] First, methods for obtaining polymers that can be used in the polymer film of the present invention will be described using aromatic polyamides and aromatic polyimides as examples. Of course, the polymers that can be used in the present invention and the polymerization methods thereof are not limited to these.
[0048] Various methods are available for obtaining aromatic polyamides, but for example, when low-temperature solution polymerization is used using acid dichlorides and diamines as raw materials, they are synthesized in aprotic organic polar solvents such as N-methylpyrrolidone, N,N-dimethylacetamide, dimethylformamide, dimethyl sulfoxide, etc. In the case of solution polymerization, in order to obtain a polymer with a high molecular weight, it is preferable that the water content of the solvent used in polymerization is 500 ppm or less (by mass, the same applies hereinafter), and more preferably 200 ppm or less.
[0049] When aromatic polyimide or its precursor polyamic acid is polymerized using, for example, tetracarboxylic anhydride and aromatic diamine as raw materials, it can be synthesized by solution polymerization in an aprotic organic polar solvent such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, dimethylformamide, dimethyl sulfoxide, etc. Using equal amounts of the raw materials tetracarboxylic anhydride and aromatic diamine can result in the production of an ultra-high molecular weight polymer, so it is preferable to adjust the molar ratio of one to 90.0 to 99.5 mol % of the other.
[0050] The logarithmic viscosity (ηinh) of aromatic polyamides and aromatic polyimides, or their precursor polyamic acids, is preferably 0.5 to 6.0 dl / g, more preferably 3.0 to 6.0 dl / g. If the logarithmic viscosity is less than 0.5 dl / g, the interchain bonding strength due to entanglement of polymer molecular chains is reduced, which may result in reduced mechanical properties such as toughness and strength, or an increased thermal shrinkage rate. If the logarithmic viscosity exceeds 6.0 dl / g, ion permeability may be reduced.
[0051] [Preparation of Membrane-Forming Raw Materials] Next, the membrane-forming stock solution (hereinafter, sometimes simply referred to as membrane-forming stock solution) used in the process for producing the polymer membrane of the present invention will be described.
[0052] The polymer solution after polymerization may be used as it is for the membrane forming solution, or the polymer may be isolated and then redissolved in the above-mentioned aprotic organic polar solvent or an inorganic solvent such as sulfuric acid.
[0053] The concentration of the polymer in the film-forming solution is preferably 3 to 30% by mass, more preferably 5 to 20% by mass. The above-mentioned lithium salt is preferably added to the film-forming solution from the viewpoint of improving ionic conductivity. The amount of lithium salt added is preferably such that the molar ratio of lithium in the lithium salt to oxygen in the polymer is 0.1 or more, more preferably 0.2 or more.
[0054] [Polymer Film Formation] Next, a method for forming the polymer film of the present invention will be described. The film-forming solution prepared as described above can be used to form a film by a so-called solution film-forming method. Solution film-forming methods include a dry-wet method, a dry method, and a wet method, and any method may be used to form a film, but the dry-wet method will be described here as an example. The polymer film of the present invention may be formed directly on a porous substrate or an electrode to form a laminated composite, but here, a method for forming the polymer film as a single film will be described.
[0055] When forming a film using a dry / wet method, the film-forming solution is extruded from a die onto a support such as a drum, endless belt, or film to form a film, which is then dried until it becomes self-supporting. Drying conditions can be, for example, 60 to 220°C and 60 minutes or less. However, when using a polyamic acid polymer to obtain a film made of aromatic polyamic acid without imidization, the drying temperature is preferably 60 to 150°C, more preferably 60 to 120°C. After completing the dry process, the film is peeled from the support and introduced into a wet process, where it is subjected to desalting, desolvation, etc., followed by stretching, drying, and heat treatment. The stretching ratio is preferably in the range of 0.8 to 8.0 in areal ratio (area ratio is defined as the area of the film after stretching divided by the area of the film before stretching; a ratio of 1 or less means relaxation), more preferably 1.0 to 5.0. The heat treatment is carried out at a temperature of 80°C to 500°C, preferably 150°C to 400°C, for a period of several seconds to several tens of minutes. However, when a polyamic acid polymer is used and a film made of polyamic acid is to be obtained without imidization, the heat treatment temperature is preferably 80 to 150°C, and more preferably 80 to 120°C under reduced pressure.
[0056] [Secondary Battery] Examples of the form of the air battery of this embodiment include a coin battery, a laminate battery, etc. In a method for producing an air battery, for example, in the case of a laminate battery or a coin battery, a laminate is produced by stacking a positive electrode sheet, a separator, a negative electrode sheet, and a separator of a predetermined size in this order, and the produced wound body or laminate is filled into each battery case. After welding the lead bodies of the positive electrode and the negative electrode, an electrolyte is poured into the battery case, and the opening of the battery case is sealed to complete the battery.
[0057] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. The measurement methods used in these examples are as follows. [Measurement Method] (1) Separator Meltdown Temperature A separator measuring 50 mm x 50 mm was cut out, and the sample was sandwiched between two stainless steel plates with a 12 mm through-hole in the center, which was then sandwiched between heating block plates with a 12 mm through-hole in the center on both sides. A tungsten carbide ball with a diameter of 9.5 mm was placed in the through-hole, and the heating block was heated at a rate of 5°C / min, and the temperature at which the ball dropped was measured. The test was performed five times, and the average value was taken as the meltdown temperature (°C).
[0058] (2) Air Permeability of Separator: Measured using an Oken type air permeability resistance meter (manufactured by Asahi Seiko Co., Ltd., EGO-1T) in accordance with JIS P8117 (1998).
[0059] The air permeability measurement limit is 10,000 seconds, and the separator has a substantially non-porous structure.
[0060] (3) Ionic conductivity (unit: S / cm) The polymer membrane was immersed in an electrolyte (1 M LiTFSI ethylene carbonate (EC) / diethyl carbonate (DEC) = 1 / 1, manufactured by Mitsui Chemicals, Inc.) for 24 hours, then placed on a SUS304 electrode so as to cover the electrode portion, and the electrolyte was dripped onto the electrode. The electrode was then sandwiched between another SUS electrode to produce an electrode / polymer membrane / electrode laminate. The laminate was fixed with a silicon plate to prevent it from shifting, and an evaluation cell was produced.
[0061] The AC impedance of the prepared cell was measured at 25°C using an electrochemical tester (manufactured by Biologic, model number: SP-150) under conditions of an amplitude of 10 mV and a frequency of 1 MHz to 10 mHz. The resistance value was read from a graph plotted on a complex plane and substituted into the following formula to calculate the ionic conductivity. Five measurements were taken, and the calculated average value was used as the ionic conductivity.
[0062] σ=d1 / AR σ: ionic conductivity (S / cm) d1: thickness of polymer film (cm) (before immersion in electrolyte) A: area of electrode (cm 2 ) R: Resistance value (Ω) (4) Water contact angle of separator and its rate of change First, the separator is left to stand for 24 hours in an atmosphere of room temperature 23°C and relative humidity 65%. Then, in the same atmosphere, water is dropped onto the separator and the contact angle after 10 seconds is measured at five points using a contact angle meter DropMaster DM-501 manufactured by Kyowa Interface Science Co., Ltd. The average value of the three measured values excluding the maximum and minimum values of the five measured values was taken as the water contact angle.
[0063] The contact angle was measured in the same manner one hour after the dropping, and the rate of change from the contact angle 10 seconds after the dropping was evaluated using the following formula.
[0064] (Formula) (1 - (Contact angle after 1 hour of dropping) / (Contact angle after 10 seconds of dropping)) × 100 (5) Contact angle of separator measured using dimethyl carbonate and its rate of change First, the separator is left to stand for 24 hours in an atmosphere at room temperature of 23°C and a relative humidity of 65%. Then, in the same atmosphere, the contact angle of the separator 10 seconds after dropping dimethyl carbonate is measured at five points using a contact angle meter DropMaster DM-501 manufactured by Kyowa Interface Science Co., Ltd. The average value of the three measured values excluding the maximum and minimum values of the five measured values was taken as the contact angle measured using dimethyl carbonate.
[0065] The contact angle after 1 hour of dropping was measured in the same manner, and the rate of change from the contact angle after 10 seconds of dropping was evaluated using the following formula: (Formula) (Contact angle after 1 hour of dropping) / (Contact angle after 10 seconds of dropping)×100−100 (6) Logarithmic viscosity of polymer (unit: dl / g) A polymer was dissolved at a concentration of 0.5 g / dl in N-methylpyrrolidone (NMP) containing 2.5 wt % lithium bromide (LiBr), and the flow time was measured at 30°C using an Ubbelohde viscometer. The flow time of a blank LiBr 2.5 wt % / NMP solution in which no polymer was dissolved was also measured in the same manner, and the viscosity η (dl / g) was calculated using the following formula:
[0066] η=[ln(t / t0)] / 0.5, t0: flow-down time (S) of blank, t: flow-down time (S) of sample (7) Charge-Discharge Cycle Characteristics The charge-discharge cycle characteristics of the secondary batteries prepared in each of the Examples and Comparative Examples were tested according to the following procedure, and the discharge capacity retention rate was calculated.
[0067] <1st to 30th Cycles> One cycle consisted of charge and discharge. The charge conditions were a constant current charge of 0.1 C and 5 V, and a constant current discharge of 0.1 C and 2.8 V. The charge and discharge cycles were repeated 150 times at 25°C. <Calculation of Discharge Capacity Retention Rate> The discharge capacity retention rate was calculated by (discharge capacity at the 30th cycle) / (discharge capacity at the 1st cycle) × 100. Five secondary batteries prepared in each Example and Comparative Example were tested, and the results with the highest and lowest discharge capacity retention rates were removed. The average of the three measurement results was used as the discharge capacity retention rate. A discharge capacity retention rate of less than 60% was rated C (fail), 60% to less than 70% was rated B (passible), 70% to less than 75% was rated A (good), and 75% or greater was rated S (excellent). Furthermore, batteries that could not operate were rated "-."
[0068] (Example 1) A separator and a secondary battery were fabricated as follows. Table 1 shows the physical properties of the separator and the characteristics of the secondary battery. [Positive electrode] An air electrode in which 20% of a platinum catalyst was supported on carbon paper was used. [Negative electrode] A commercially available metallic lithium foil (manufactured by Honjo Metals Co., Ltd.) was used. [Electrolyte] A non-aqueous electrolyte was prepared as follows. 1.0 mol of lithium hexafluorophosphate (LiPF) was added to 1 L of a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1. 6 ) was dissolved to prepare a mixed solution, and 2 parts by mass of vinylene carbonate (VC) was further added to 100 parts by mass of the mixed solution to prepare a non-aqueous electrolyte solution.
[0069] The aqueous electrolyte was prepared as follows. A mixture was prepared by dissolving 1 mol% potassium hydroxide (KOH) in pure water. [Separator] 4,4'-diaminodiphenyl ether (diamine) was dissolved in dehydrated N-methyl-2-pyrrolidone under a nitrogen stream and cooled to below 30°C. While maintaining the system at below 30°C under a nitrogen stream, 2-chloroterephthaloyl chloride equivalent to 99 mol% of the total amount of diamine was added over 30 min. After the entire amount was added, the mixture was stirred for approximately 2 h to polymerize an aromatic polyamide. The resulting polymerization solution was neutralized with 97 mol% lithium carbonate and 6 mol% diethanolamine, based on the total amount of acid chloride, to obtain polymer solution A. The inherent viscosity η of the resulting polymer was 2.5 dl / g.
[0070] The resulting polymer solution was treated with lithium bistrifluoromethylsulfonylimide [LiN(CF)], a lithium salt. 3 SO 2 ) 2] was added so that the molar ratio of lithium in the lithium salt to oxygen in the polymer was 0.2, and the mixture was stirred and degassed using a mixer (THINKY Corporation, model number: AR-250) to obtain a uniform, transparent solution. The obtained uniform mixed solution of polymer and lithium salt was applied in the form of a film onto a glass plate as a support, and dried at a hot air temperature of 60°C until the polymer film became self-supporting, after which the polymer film was peeled off from the support. Next, the mixture was introduced into a water bath at 25°C to extract the solvent, neutralized salt, etc. Subsequently, the water on the surface of the obtained hydrated polymer film was wiped off, and then the film was subjected to a heat treatment for 1 minute in a tenter chamber at a temperature of 180°C to obtain a polymer film with a thickness of 5 μm. [Battery Assembly] In a dry atmosphere, the positive electrode and the negative electrode were placed in a two-compartment cell (SB-100B manufactured by EC Frontier Co., Ltd.) together with the separator, and an aqueous electrolyte was poured into the positive electrode side, and a non-aqueous electrolyte was poured into the negative electrode side, to fabricate a secondary battery with a battery capacity of 3 mAh. Note that oxygen was supplied to the air electrode by attaching a simple oxygen tank and supplying oxygen to the aqueous electrolyte.
[0071] Example 2 A secondary battery was fabricated in the same manner as in Example 1, except that the aqueous electrolyte solution was changed to 1 mol % hydrochloric acid.
[0072] (Example 3) In the preparation of the separator, lithium bistrifluoromethylsulfonylimide [LiN(CF 3 SO 2 ) 2 A secondary battery was fabricated in the same manner as in Example 1, except that the molar ratio of lithium in the lithium salt to oxygen in the polymer was 0.1.
[0073] Example 4 In the preparation of a separator, 4,4'-diaminodiphenyl ether (diamine) was dissolved in dehydrated N-methyl-2-pyrrolidone under a nitrogen stream and cooled to below 30°C. To this solution, 2-chloroterephthaloyl chloride (99.5 mol % of the total amount of diamine) was added over 30 min while maintaining the system at 30°C or below under a nitrogen stream. After the entire amount was added, the mixture was stirred for approximately 2 h to polymerize an aromatic polyamide. The resulting polymerization solution was neutralized with 97 mol % lithium carbonate and 6 mol % diethanolamine (based on the total amount of acid chloride) to obtain polymer solution B. The inherent viscosity η of the resulting polymer was 3.5 dL / g. A secondary battery was prepared in the same manner as in Example 1, except for using the resulting polymer solution B.
[0074] (Example 5) In the preparation of the separator, lithium trifluoromethasulfonate (LiCF 3 SO 3 A secondary battery was fabricated in the same manner as in Example 1, except that the temperature was changed to 100°C.
[0075] Example 6 A non-aqueous electrolyte solution was prepared by dissolving 1.0 mol of lithium hexafluorophosphate (LiPF 6 A secondary battery was fabricated in the same manner as in Example 1 except that 2 parts by mass of vinylene carbonate (VC) was further added to 100 parts by mass of the mixed solution.
[0076] Comparative Example 1 A secondary battery was fabricated in the same manner as in Example 1, except that both the positive electrode electrolyte and the negative electrode electrolyte were changed to non-aqueous electrolytes.
[0077] Comparative Example 2 A secondary battery was fabricated in the same manner as in Example 1, except that both the positive electrode electrolyte and the negative electrode electrolyte were changed to aqueous electrolytes. However, metallic lithium reacted with the aqueous electrolyte, and the battery was not viable.
[0078] (Comparative Example 3) The separator was a cellulose nonwoven fabric (thickness 40 μm, density 0.40 g / cm 3A secondary battery was fabricated in the same manner as in Example 1, except that the nonwoven fabric was made of 100% by mass of lyocell fiber, which is a regenerated cellulose fiber, using a Fourdrinier paper machine.
[0079] Comparative Example 4 A secondary battery was fabricated in the same manner as in Example 3, except that in the preparation of the separator, a polymer solution containing no lithium salt was used alone.
[0080]
[0081] As can be seen from Table 1, Examples 1, 2, 3, 4, and 5 contained a nonaqueous electrolyte solution and an aqueous electrolyte solution, and the water contact angle in the separator physical properties was 90° or more, which fell within the range of the present invention, and the secondary batteries exhibited good cycle characteristics.
[0082] On the other hand, in Comparative Examples 1, 2, 3, and 4, the water contact angle in the separator properties was less than 90°, which was outside the range of the present invention, or the electrolyte solution had only one type of solvent composition, and the cycle characteristics of the secondary battery were insufficient.
Claims
1. A secondary battery including a positive electrode, a negative electrode, a non-aqueous electrolyte, an aqueous electrolyte, and a separator, the positive electrode being an air electrode, the negative electrode being composed of a negative electrode current collector and a negative electrode mixture layer formed thereon, the negative electrode mixture layer containing one or more components selected from the group consisting of metallic lithium, magnesium, zinc, and aluminum, the separator having an air permeability of more than 10,000 seconds and an ionic conductivity of 1×10 -5 4. A secondary battery comprising a polymer film having a water contact angle of 90° or more, the contact angle of the polymer film being measured using dimethyl carbonate being 90° or more.
2. 2. The secondary battery according to claim 1, wherein a rate of change in contact angle of the polymer film after one hour from the application of water to the contact angle after 10 seconds from the application of water is less than 10%.
3. 3. The secondary battery according to claim 1, wherein the rate of change in the contact angle of the polymer film one hour after dimethyl carbonate is dropped relative to the contact angle 10 seconds after dimethyl carbonate is dropped is less than 10%.
4. 4. The secondary battery according to claim 1, wherein the polymer film has a meltdown temperature of 300° C. or higher.
5. 5. The secondary battery according to claim 1, wherein the polymer constituting the polymer film contains an aromatic polyamide, an aromatic polyimide or an aromatic polyamideimide.