Dental glass composition

JPWO2023171682A5Active Publication Date: 2024-11-13KURARAY NORITAKE DENTAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024506352
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-07
Filing Date
2023-03-07
Publication Date
2024-11-13
Estimated Expiration
2043-03-07

AI Technical Summary

Technical Problem

Conventional porcelain stains for dental prostheses face issues with viscosity changes over time, leading to application difficulties, bleeding, and the need for multiple fixation firings, which complicates the manufacturing process and can result in bubbles and interfacial peeling.

Method used

A dental glass composition comprising a glass powder and a hydrophilic organic compound that is solid at 25°C, with no water or propylene glycol, allowing direct application and bonding without fixation firing, while suppressing bubble generation and interfacial peeling.

Benefits of technology

The dental glass composition ensures excellent fixability and color layering without fixation firing, preventing bleeding and peeling, and simplifies the manufacturing process by allowing a single firing step, while maintaining desired color tones and aesthetics.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a dental glass composition which exhibits excellent fixability to dental prostheses and does not require firing for fixation, and which is capable of suppressing the generation of excessive air bubbles and the occurrence of interfacial debonding at the interface between a base material and a dental ceramic material in cases where firing for fixation is not carried out, while making it possible to build up and fire a dental ceramic material thereon. The present invention relates to a dental glass composition which contains a glass powder (A) and a binder, wherein the binder contains a hydrophilic organic compound (B) that is in a solid state at 25°C, while substantially containing no water and no propylene glycol.
Need to check novelty before this filing date? Find Prior Art

Description

Dental glass composition

[0001] The present invention relates to a dental glass composition used for coloring and adjusting the color tone of dental prostheses. More specifically, the present invention relates to a dental glass composition suitable for use in, for example, crowns, inlays, bridges, implant superstructures, dentures, and artificial teeth, which are made using ceramic raw materials, and in particular to a dental glass composition suitable as a color-adjusting composition for ceramic crown porcelain (hereinafter sometimes referred to as "porcelain stain").

[0002] Dental prostheses (e.g., veneers, crowns, dentures, etc.) that restore aesthetics close to those of natural teeth include ceramic dental prostheses such as metal ceramic dental prostheses and all-ceramic dental prostheses, which use dental porcelain that expresses the color tone of ivory or enamel on various materials such as metal, zirconium oxide (zirconia), aluminum oxide (alumina), feldspar glass, and disilicate glass.

[0003] In manufacturing ceramic dental prostheses, there is a technique for imitating the color tone of individual natural teeth by expressing the white bands, dentin, cervical and approximal surface coloration, hairlines, enamel cracks, etc. of natural teeth in the dental prosthesis. In this case, for example, porcelain stain is applied to the dental prosthesis, which makes the ceramic dental prosthesis more likely to blend in with the color tone of the natural teeth surrounding the tooth to which the dental prosthesis is applied.

[0004] When using a porcelain stain, a porcelain stain of an appropriately selected color tone is dispensed onto a glass mixing board or stain palette. Porcelain stains are generally provided in the form of powder or paste. When the porcelain stain is in powder form, an appropriate amount of the powder must be dispensed onto a glass mixing board or stain palette, and then water or a special liquid must be added to impart applicability to the powder, adjusting the powder-liquid ratio and other factors to form a paste. Even when the porcelain stain is in the form of a paste, the paste properties can change over time, such as during storage or after an appropriate amount of the paste has been dispensed onto a glass mixing board or stain palette, resulting in application problems such as increased viscosity, making it difficult to apply during use, and causing bleeding during application. Therefore, there is a demand for a porcelain stain that is easy to use and has excellent application properties.

[0005] Common techniques for coloring ceramic dental prostheses to mimic natural teeth include the "internal staining method," in which a porcelain stain is sandwiched between enamel-representing porcelain and dentin-representing porcelain, and the "surface staining method," in which a porcelain stain is applied to the outermost surface of the enamel-representing porcelain.

[0006] In these methods, in order to fuse the inorganic pigment components contained in the porcelain stain to the dental prosthesis and, in the case of the internal staining method, to prevent any influence on subsequent porcelain build-up using a different porcelain, it is essential to apply the porcelain stain to the dental prosthesis and then perform firing (hereinafter sometimes referred to as "fixing firing") using a dental laboratory porcelain firing furnace according to a firing schedule optimal for each porcelain stain. Since multiple firings are required to manufacture a dental prosthesis, there is a demand for porcelain stains that can shorten the manufacturing process.

[0007] As a color-adjusting composition for ceramic dental crown porcelain, for example, Patent Document 1 discloses a powder or paste-like porcelain stain containing a specific aluminosilicate glass. Also, Patent Document 2 discloses a paste that does not require firing before applying a body porcelain layer, by brushing a coating material consisting of an opaque porcelain powder and an aqueous colloidal dispersion of a urethane polymer onto a dental coping and air-drying it for 20 minutes before applying the body porcelain layer.

[0008] JP 2009-207743 A JP 59-196807 A

[0009] However, in Patent Document 1, it is necessary to apply the porcelain stain in a paste state, and the paste must be prepared by mixing powder and liquid (e.g., water) each time it is used, and it has been found that it is not easy to adjust the viscosity; if the viscosity is too high, it is difficult to apply, and if the paste viscosity is too low, it will bleed during application. Furthermore, even when the paste-like porcelain stain described in Patent Document 1 is used, there is a problem that the viscosity increases over time, changing the paste properties and making it difficult to apply.

[0010] Furthermore, in Patent Document 1, when applying multiple coats of paint, both the internal staining method and the surface staining method require firing each time, and the internal staining method requires firing to fix the porcelain stain before building up the porcelain on the surface, which poses the problem of requiring many steps.If the fixing firing is not performed, it has been found that problems such as the porcelain stain being unintentionally mixed with the porcelain to be built up subsequently, or the color of the porcelain stain bleeding out of the built-up porcelain before or during firing because the porcelain stain is not fixed, occur.

[0011] Furthermore, in Patent Document 2, the urethane polymer contained therein cannot be completely burned under the firing conditions of the porcelain, resulting in carbonization and the generation of bubbles, and the technique of Patent Document 2 makes it difficult to achieve uniform application. The generation of bubbles, in particular, is problematic because it adversely affects the firing of the porcelain to the coping (frame / substrate / base material). Furthermore, Patent Document 2 requires air drying for 20 minutes, which is longer than the time generally required for this process (5 to 8 minutes), and is therefore unrealistic from the standpoint of the time required for the process.

[0012] Therefore, an object of the present invention is to provide a dental glass composition that has excellent adhesion to dental prostheses, allows coloring to be layered without the need for a fixing firing, and, even when a fixing firing is not performed, can suppress the occurrence of significant bubbles and interfacial peeling at the interface between the substrate and dental porcelain, and allows dental porcelain to be built up and fired thereon.

[0013] As a result of extensive research into solving the above problems, the present inventors have discovered that a dental glass composition containing a glass component and a hydrophilic organic compound that is solid at 25°C, and substantially free of water and propylene glycol, can be applied directly to a dental prosthesis without preparing a paste, and that a dental prosthesis having a desired color tone can be obtained without performing the fixing and firing step that is essential for the internal stain method, and that the generation of bubbles can be suppressed.Further research led to the completion of the present invention.

[0014] The present invention encompasses the following inventions. [1] A dental glass composition comprising a glass powder (A) and a binder, wherein the binder contains a hydrophilic organic compound (B) that is solid at 25°C, and wherein the composition is substantially free of water and propylene glycol. [2] The dental glass composition according to [1], wherein the average particle size of the glass powder (A) is 0.05 μm to 50 μm. [3] The dental glass composition according to [1] or [2], wherein the melting point of the hydrophilic organic compound (B) is 35°C or higher. [4] The dental glass composition according to any one of [1] to [3], wherein the hydrophilic organic compound (B) is a water-soluble polymer. [5] The dental glass composition according to any one of [1] to [4], wherein the content of the hydrophilic organic compound (B) is 1 to 50 mass%. [6] The dental glass composition according to any one of [1] to [5], wherein the binder further contains an unsaturated fatty acid component (C) that is liquid at 25°C. [7] The dental glass composition according to [6], wherein the content of the unsaturated fatty acid component (C) is 0.5 to 30% by mass. [8] The dental glass composition according to any one of [1] to [7], wherein the binder further comprises a wax component (D) that is solid at 25°C. [9] The dental glass composition according to any one of [1] to [8], wherein the contents of water and propylene glycol are less than 1000 ppm by mass.

[10] The dental glass composition according to any one of [1] to [9], which is solid at 25°C.

[11] The dental glass composition according to any one of [1] to

[10] , which is a porcelain stain.

[12] A method for manufacturing a dental prosthesis, comprising the steps of applying the dental glass composition according to any one of [1] to

[11] to a substrate of a dental prosthesis having a ceramic surface, and firing the substrate after building up dental porcelain, without firing the substrate after applying the dental glass composition and before building up dental porcelain.

[13] The method for manufacturing a dental prosthesis according to

[12] , wherein the firing temperature in the firing step after building up the dental porcelain is 700 to 1100°C.

[0015] According to the present invention, a dental glass composition can be provided that has excellent adhesion to dental prostheses, allows for coloring to be layered without the need for a fixing or firing step, and, even when a fixing or firing step is not performed, prevents significant bubble formation and interfacial peeling at the interface between the substrate and the dental porcelain, allowing for the deposition and firing of dental porcelain thereon. Furthermore, the dental glass composition of the present invention has excellent adhesion without the need for a fixing or firing step, even when multiple coatings are performed, prevents mixing with the subsequently deposited dental porcelain, and prevents the color of the dental glass composition from bleeding out before or during firing of the deposited dental porcelain. Furthermore, since the dental glass composition of the present invention does not require a fixing or firing step, the manufacturing process can be shortened, which is industrially advantageous. Furthermore, the dental glass composition of the present invention has excellent color development properties, allowing for layered coloring and adjustment of a desired color tone.

[0016] Furthermore, the dental glass composition of the present invention suppresses changes over time in the glass composition itself, provides excellent operability, enables thin film application to dental prostheses, and, due to its lack of fluidity, allows application without bleeding. Furthermore, the dental glass composition of the present invention can be used alone for dental prostheses. It is also possible to impart a gradation from the cervical region to the incisal edge using a brush or a sponge such as an eye color tip, or to blend using a finger, allowing for easy production of dental prostheses with the desired color tone. Furthermore, subsequent porcelain build-up can be performed without performing a fixing firing, and the generation of bubbles can be suppressed, thereby shortening the manufacturing process for dental prostheses.

[0017] 1 is a photograph of a test piece used in the evaluation of fixation and color development according to Example 1. FIG. 2 is a photograph of a test piece used in the evaluation of fixation and color development according to Comparative Example 5. FIG. 3 is a fractured surface and an optical microscope photograph of the fractured surface when dental porcelain is built up on a substrate and fired using the internal stain method (with fixation and firing), which is a conventional technology, as a control. FIG. 4 is an optical microscope photograph of the fractured surface used in the evaluation of the interface condition according to Example 1. FIG. 5 is an optical microscope photograph of the fractured surface used in the evaluation of the interface condition according to Comparative Example 2.

[0018] The dental glass composition of the present invention comprises a glass powder (A) and a binder, the binder containing a hydrophilic organic compound (B) that is solid at 25°C, and is substantially free of water and propylene glycol.

[0019] <Glass Powder (A)> First, the glass powder (A) contained in the glass composition of the present invention will be described. The glass powder (A) used in the present invention is not particularly limited as long as it exhibits the effects of the present invention, and any dental glass powder that can be bonded to a substrate (such as a core or frame that is a material for a dental prosthesis) can be used.

[0020] Examples of the glass powder (A) include potassium aluminosilicate glass (amorphous type potassium aluminosilicate glass (4SiO 2 ・Al 2 O 3 ・K 2 O), leucite crystal type potassium aluminosilicate glass), fluoroapatite glass, lithium silicate glass, etc. The components constituting the glass powder (A) include SiO 2 , Al 2 O 3 , B 2 O 3 , Li 2 O, Na 2 O.K. 2 O, CaO, MgO, Sb 2 O 3 The components are selected in appropriate ratios depending on the substrate to be applied.

[0021] The glass powder (A) contains TiO 2 , SrO, BaO, ZnO, CeO 2 , ZrO 2 , P 2 O 5 The glass powder (A) may be used singly or in combination of two or more kinds.

[0022] The coefficient of linear thermal expansion of the glass powder (A) used in the present invention is preferably close to the coefficient of linear thermal expansion of the substrate to which it is applied. For example, the coefficient of linear thermal expansion in the range of 25°C to 500°C is 6.0 x 10-6 K -1 ~14.0 x 10 -6 K -1 The linear thermal expansion coefficient can be measured by a known method and apparatus. For example, the linear thermal expansion coefficient can be measured by heating a sample from room temperature to 500°C using a thermal analyzer (trade name "TMA120", manufactured by Seiko Instruments Inc., heating rate 5°C / min).

[0023] The raw materials for the glass powder (A) used in the present invention can be widely used, commonly known ceramic raw materials. The reason why a wide range of ceramic raw materials can be used without any limitations on the glass composition when the glass powder (A) is a glass powder is that the dental glass composition of the present invention combines powdered glass with a binder containing a hydrophilic organic compound (B), resulting in excellent fixability and adhesion at the interface between the substrate and the dental porcelain as a whole, and the fixability and adhesion at the interface are not affected by the glass composition (presence or absence of specific oxides). Therefore, any ceramic raw material capable of developing a desired color tone can be used as the glass powder (A). There are no particular limitations on the glass powder (A) as long as it is a raw material that can be converted into the above components by itself and / or by heating in air. The glass composition to be obtained is calculated in advance, and the blending ratio of each raw material is determined and mixed.

[0024] The method for mixing the raw materials of the glass is not particularly limited, and known methods and devices can be used. It is preferable that the raw materials of the glass powder (A) are uniformly dispersed by mixing.

[0025] The raw materials thus mixed are melted at 1200°C or higher, the melt is cooled, and the resulting material is pulverized to produce glass powder. The method for melting the raw materials is not particularly limited, and known methods and devices can be used. The method for melting the raw materials is not particularly limited as long as all of the mixed raw materials are melted to form a uniform amorphous material and sublimation of the components does not occur.

[0026] The method for cooling the melt is not particularly limited, and known methods and devices can be used. The melt can be cooled by, for example, quenching in water. The glass gobs thus obtained are dried and pulverized to obtain glass powder (A). The method for pulverizing the glass gobs is not particularly limited, and known methods and devices can be used. Furthermore, the method for classifying the glass gobs to the desired pulverized particle size is not particularly limited, and known methods and devices can be used.

[0027] The glass powder (A) used in the present invention may contain a colorant. The colorant may be amorphous or crystalline. The form of the colorant is not particularly limited, and may be a powder. In some embodiments, the colorant may contain a crystalline powder. Examples of colorants include pigments and fluorescent agents. A single colorant may be used alone, or two or more colorants may be used in combination. The reason why the colorant contained in the glass powder (A) can be widely used without being particularly limited in terms of crystal system or type is that the dental glass composition of the present invention combines powdered glass with a binder containing a hydrophilic organic compound (B), thereby providing the composition as a whole with excellent fixability and adhesion at the interface between the substrate and dental porcelain, and the fixability and adhesion at the interface do not change depending on the type of colorant (presence or absence of a specific oxide).

[0028] The pigment is preferably an inorganic pigment. Examples of inorganic pigments include oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, Tb, and Er, and preferably contain an oxide of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Pr, Tb, and Er. Examples of the oxides include praseodymium oxide, vanadium oxide, iron oxide, nickel oxide, chromium oxide, manganese oxide, cerium oxide, tin oxide, zirconium oxide, zinc oxide, and titanium oxide.

[0029] Furthermore, composite pigments can also be used as inorganic pigments. Examples of the composite pigments include (Zr, V)O 2, Fe(Fe,Cr) 2 O 4 , (Ni, Co, Fe) (Fe, Cr) 2 O 4 ZrSiO 4 , (Co,Zn)Al 2 O 4 (Zr, V)O 2 It is preferred that the compound contains:

[0030] Examples of fluorescent agents include Y 2 SiO 5 : Ce, Y 2 SiO 5 :Tb, (Y, Gd, Eu)BO 3 , Y 2 O 3 :Eu, YAG:Ce, ZnGa 2 O 4 :Zn, BaMgAl 10 O 17 : Eu, etc.

[0031] When the glass powder (A) contains a colorant, the glass powder (A) may be obtained by simply mixing a raw material glass powder containing no colorant with the colorant, or by mixing a raw material glass powder containing no colorant with the colorant, heating and fusing the mixture at 600 to 1200°C, and then pulverizing the mixture to obtain the glass powder (A).

[0032] Considering the need to balance the finest possible particle size to approximate the color tone of natural teeth with a somewhat coarse particle size for achieving color development, the average particle size of the glass powder (A) used in the present invention is preferably 0.05 to 50 μm, more preferably 0.08 to 35 μm, even more preferably 0.1 to 20 μm, particularly preferably 0.1 to 10 μm, and most preferably 0.1 to 5 μm. When the average particle size is 50 μm or less, the dental glass composition can be sufficiently adhered to the frame, does not fall off during porcelain build-up, and color particles are not visible to the naked eye, resulting in excellent aesthetics. Furthermore, when the average particle size is 0.05 μm or more, the composition is not burned out during firing, and sufficient color development can be achieved.

[0033] The average particle size of the glass powder (A) can be determined by a laser diffraction scattering method. The laser diffraction scattering method can be performed by volumetric measurement using, for example, a laser diffraction particle size distribution analyzer (SALD-2300, manufactured by Shimadzu Corporation). The average particle size of the glass powder (A) is the median diameter (d 50 ) means

[0034] In the dental glass composition of the present invention, the content of the glass powder (A) is preferably at a level that allows it to be kneaded with the hydrophilic organic compound (B). The content of the glass powder (A) is preferably 25% by mass or more based on the total amount of the dental glass composition. From the viewpoint of superior color development and adhesion to dental prostheses, the content is more preferably 35% by mass or more, even more preferably 45% by mass or more, and particularly preferably 55% by mass or more. The content of the glass powder (A) is not particularly limited, but is preferably 97% by mass or less, more preferably 95% by mass or less, even more preferably 93% by mass or less, and particularly preferably 91% by mass or less. In an embodiment in which the binder contains a wax component (D) in addition to the hydrophilic organic compound (B), the content of the glass powder (A) is preferably 25% by mass or more based on the total amount of the dental glass composition. From the viewpoint of superior color development and adhesion to dental prostheses, the content is more preferably 35% by mass or more, even more preferably 45% by mass or more, and particularly preferably 55% by mass or more. In the embodiment, the content of the glass powder (A) is not particularly limited, but is preferably 95% by mass or less, more preferably 93% by mass or less, even more preferably 89% by mass or less, and particularly preferably 85% by mass or less.

[0035] In the dental glass composition of the present invention, commercially available dental porcelain may be used as the glass powder (A). The commercially available dental porcelain is not particularly limited as long as it is a dental stain porcelain. Examples of commercially available dental stain porcelain include various surface stains and internal stains such as Cerabian (registered trademark) ZR Internal Stain / External Stain and Cerabian (registered trademark) ZR Press LF Internal Stain / External Stain (manufactured by Kuraray Noritake Dental Co., Ltd.).

[0036] <Hydrophilic Organic Compound (B) Solid at 25°C> Next, the hydrophilic organic compound (B) solid at 25°C (hereinafter also referred to simply as "hydrophilic organic compound (B)") contained in the dental glass composition of the present invention will be described. The binder of the dental glass composition of the present invention contains a hydrophilic organic compound (B). The binder refers to a substance capable of bonding a substrate and a dental porcelain. The hydrophilic organic compound (B) is contained to disperse the glass powder (A) and solidify the dental glass composition at 25°C. Furthermore, the inclusion of the hydrophilic organic compound (B) increases adhesion and fixation to the substrate, allowing coloring to be applied without the need for a fixation firing, and suppressing the generation of bubbles at the interface between the substrate and the dental porcelain when the dental porcelain is built up and fired thereon. The hydrophilic organic compound (B) may be used alone or in combination of two or more.

[0037] The hydrophilic organic compound (B) used in the present invention preferably contains a compound that is solid at 25°C and melts upon heating, in order to disperse the glass powder (A) and solidify the dental glass composition at 25°C. In this specification, "solid at 25°C" includes not only compounds that are solid at 25°C but also semi-solid compounds such as ointments. The dental glass composition solidified at 25°C may be semi-solid such as ointments. The heating temperature for melting the hydrophilic organic compound (B) can be changed depending on the type of hydrophilic organic compound (B) and is not particularly limited, and may be 50°C or higher, 80°C or higher, 100°C or higher, or 150°C or higher.

[0038] In a preferred embodiment, a dental glass composition is provided that includes a glass powder (A) and a binder, the binder containing a hydrophilic organic compound (B), the hydrophilic organic compound (B) being solid at 25°C and melting upon heating. By using a compound that is solid at 25°C and melts upon heating, the glass composition does not undergo changes in properties over time, such as an increase in viscosity, and no fixing or firing is required, eliminating the need for repeated fixing or firing. This is advantageous over conventional techniques. Therefore, the dental glass composition of the present invention allows for easy overlaying of coloring, allowing for the deposition of porcelain (e.g., dental porcelain for surface staining) on ​​top of the coloring. Furthermore, the dental glass composition of the present invention can be applied in the form of a thin film.

[0039] The hydrophilic organic compound (B) refers to an organic compound having a solubility in water of 1% by mass or more at 25°C, preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and particularly preferably 30% by mass or more. Having a solubility in water of 1% by mass or more at 25°C improves adhesion and fixation to the substrate, allowing coloring to be layered without the need for a fixation firing, and suppressing the generation of bubbles when a dental porcelain is built up and fired thereon. From the above-mentioned viewpoints, the hydrophilic organic compound (B) is not particularly limited and can be widely used, as long as it is solid at 25°C, can be melted by heating to a specific melting point, and is hydrophilic, as it can provide excellent dispersibility of the glass powder (A), excellent adhesion and fixation to the substrate, and suppress the generation of bubbles.

[0040] The melting point of the hydrophilic organic compound (B) is preferably 35°C or higher, more preferably 40°C or higher, even more preferably 45°C or higher, and particularly preferably 50°C or higher, from the viewpoints of achieving storage stability in a solid state at room temperature and good adhesion to dental prostheses. If the melting point is lower than 35°C, the solid cannot be maintained, and there is a risk that the dental glass composition will flow out from the drawing surface when recoating or when building up a surface porcelain. Furthermore, the melting point of the hydrophilic organic compound (B) is preferably 120°C or lower, more preferably 105°C or lower, even more preferably 95°C or lower, and particularly preferably 85°C or lower. If the melting point is higher than 120°C, there is a risk that adhesion to dental prostheses will not be achieved and coloring will be insufficient.

[0041] The hydrophilic organic compound (B) is preferably a water-soluble polymer, and known compounds can be used. Examples of the water-soluble polymer include cationic water-soluble polymers, anionic water-soluble polymers, amphoteric water-soluble polymers, and nonionic water-soluble polymers.

[0042] Examples of the cationic water-soluble polymer include water-soluble polymers containing at least one selected from the group consisting of polyethyleneimine, polyallylamine, polyvinylamine, dimethylaminoethyldextran, and an imidazole group.

[0043] Examples of anionic water-soluble polymers include polysaccharides such as xanthan gum, guar gum, carrageenan, tamarind seed gum, gum arabic, locust bean gum, pectin, sodium starch glycolate, sodium starch phosphate, alginates (such as sodium alginate), propylene glycol alginate, propylene glycol alginate ester, hyaluronic acid, chondroitin sulfate, dermatan sulfate, keratan sulfate, and heparan sulfate, as well as salts thereof, as well as polyacrylic acid, polyacrylates (such as sodium polyacrylate and ammonium polyacrylate), carboxyvinyl polymers, and polymaleic acid.

[0044] Examples of the amphoteric water-soluble polymer include proteins such as gelatin, collagen, casein, and gluten, amino acids, and derivatives thereof.

[0045] Examples of nonionic water-soluble polymers include lower alkyl cellulose ether compounds such as methyl cellulose, ethyl cellulose, carboxy cellulose, carboxymethyl cellulose, sodium carboxymethyl cellulose, calcium carboxymethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose; vinyl compounds such as polyvinylpyrrolidone and polyvinyl alcohol; polysaccharides and derivatives thereof such as pullulan and starch; polyacrylamides such as polyglucosyloxyethyl methacrylate; and polyalkylene glycol compounds such as polyethylene oxide, polyethylene glycol, polypropylene glycol, and block copolymers of polyethylene glycol and polypropylene glycol. In this specification, polyethylene glycol refers to a polymer having a weight-average molecular weight (Mw) of 20,000 or less. Polyethylene oxide refers to a polymer having a weight-average molecular weight (Mw) of more than 20,000, preferably 50,000 or more.

[0046] As the hydrophilic organic compound (B), a nonionic water-soluble polymer is more preferred, a polyalkylene glycol compound is even more preferred, and polyethylene glycol (PEG) is particularly preferred, because excellent color development can be achieved by improving the stability of the glass powder (A). PEG is also referred to as "macrogol" in this specification.

[0047] The weight average molecular weight (Mw) of the water-soluble polymer of the hydrophilic organic compound (B) is not particularly limited, but may be, for example, 20,000 or less. The weight average molecular weight (Mw) of the water-soluble polymer of the hydrophilic organic compound (B) is preferably 700 or more, more preferably 750 or more, even more preferably 850 or more, and particularly preferably 900 or more. The weight average molecular weight (Mw) of the water-soluble polymer of the hydrophilic organic compound (B) may be, for example, 700 or more and 20,000 or less.

[0048] In other embodiments, the weight average molecular weight (Mw) of the water-soluble polymer of the hydrophilic organic compound (B) may be more than 20,000. The weight average molecular weight (Mw) of the water-soluble polymer of the hydrophilic organic compound (B) may be 2.5 million or less, 1.5 million or less, 1 million or less, 300,000 or less, or 200,000 or less.

[0049] The weight average molecular weight (Mw) in this specification means the weight average molecular weight calculated as polystyrene as determined by gel permeation chromatography (GPC), and can be measured by a known method.

[0050] In another embodiment, the number average molecular weight (Mn) of the water-soluble polymer of the hydrophilic organic compound (B) is preferably 400 or more, more preferably 500 or more, and even more preferably 550 or more. The number average molecular weight (Mn) of the water-soluble polymer of the hydrophilic organic compound (B) may be 40,000 or less, 20,000 or less, or 10,000 or less.

[0051] The number average molecular weight (Mn) in this specification means the number average molecular weight calculated based on the hydroxyl value measured in accordance with JIS K 1557-1:2007, and can be measured by a known method.

[0052] From the viewpoints of maintaining a stable solid state at room temperature and obtaining good fixation of a dental prosthesis, the content of the hydrophilic organic compound (B) used in the present invention is preferably 1 to 50 mass %, more preferably 3 to 45 mass %, even more preferably 5 to 40 mass %, and particularly preferably 7 to 35 mass %, based on the total amount of the dental glass composition. Furthermore, when the binder contains the hydrophilic organic compound (B) and the wax component (D), the content of the hydrophilic organic compound (B) is preferably 1 to 40 mass %, more preferably 2.5 to 35 mass %, even more preferably 4 to 30 mass %, and particularly preferably 6 to 25 mass %, based on the total amount of the dental glass composition.

[0053] The dental glass composition of the present invention is substantially free of water and propylene glycol. In this specification, unless a separate numerical value is specified, "substantially free of a certain component" means less than 10% by mass, preferably less than 1% by mass, more preferably less than 0.1% by mass (less than 1000 ppm by mass), even more preferably less than 100 ppm by mass, even more preferably 10 ppm by mass or less, particularly preferably 1 ppm by mass or less, even more particularly preferably 0.1 ppm by mass or less, and most preferably 0 ppm by mass. An example of the above embodiment is a dental glass composition in which the contents of water and propylene glycol are both less than 10% by mass.

[0054] The absence of water and propylene glycol allows the dental glass composition to have excellent stability in properties during long-term storage, and allows for easy overlay of coloring without bleeding, and allows for the deposition of porcelain thereon. Furthermore, in some cases, the generation of bubbles at the interface between the substrate and the dental porcelain during firing can be suppressed.

[0055] The dental glass composition of the present invention may, if necessary, contain other components that are liquid at 25°C (hereinafter also referred to as "other liquid components") in addition to the unsaturated fatty acid component (C) described below.

[0056] The other liquid components may be used singly or in combination of two or more. Examples of the other liquid components include organic solvents. Examples of the organic solvent include non-aromatic hydrocarbon solvents (e.g., alkanes such as pentane, hexane, heptane, octane, nonane, decane, dodecane, isododecane, and tridecane, cyclohexane, methylcyclohexane, decahydronaphthalene, and liquid paraffin); aromatic hydrocarbon solvents (e.g., benzene, toluene, xylene, diethylbenzene, mesitylene, tetralin, indene, naphthalene, and methylnaphthalene); halogenated hydrocarbon solvents (e.g., dichloromethane, dichloroethane, chloroform, chlorobenzene); alcohol solvents (e.g., monohydric alcohols such as ethanol, propanol, 1-butanol, 2-butanol, 1-heptanol, 2-heptanol, 3-heptanol, 1-hexanol, 2-hexanol, benzyl alcohol, 3-(benzyloxy)-1-propanol, 2-(benzyloxy)-1-butanol, 5-(benzyloxy)-1-pentanol, and oleyl alcohol; ethylene glycol, polyethylene glycol, polypropylene glycol, and glycerin polyhydric alcohols such as ethanol, methyl t-butyl ether, diisoamyl ether, ethylene glycol derivatives (e.g., monoglyme (ethylene glycol dimethyl ether), methyl cellosolve, diethyl cellosolve, diglyme, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, triglyme, tetraglyme, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, ethylene glycol monobenzyl ether, ethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, poly(ethylene glycol) monomethyl ether), propylene glycol derivatives (e.g., 3-hexanol propylene glycol monopropyl ether, dipropylene glycol monoethyl ether, tripropylene glycol monomethyl ether), 1,1-dimethoxycyclohexane, phenetole, veratrole, dioxane, tetrahydrofuran);Ester solvents (e.g., ethyl acetate, butyl acetate, isopropyl acetate, 3-methoxy-3-methylbutyl acetate, dimethyl carbonate, diethyl malonate, ethylene carbonate, propylene carbonate, γ-butyrolactone, α-acetyl-γ-butyrolactone); ketone solvents (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, acetophenone, propiophenone, isophorone); sulfur-containing solvents (e.g., dimethyl sulfoxide, sulfolane, diphenyl sulfide); and nitrogen-containing solvents (e.g., N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone). amide solvents such as methylpyrrolidone, 1,3-dimethyl-2-imidazolidinone, N,N-dimethylacrylamide, N,N-dimethylacetoacetamide, N,N-diethylformamide, N,N-diethylacetamide, hexamethylphosphoramide, and methylpyrrolidone; amine solvents such as butylamine, hexylamine, octylamine, 3-methoxypropylamine, 2-methylbutylamine, and triethanolamine; nitrile solvents such as acetonitrile and benzonitrile; nitro solvents such as nitrobenzene and o-nitrotoluene; quinoline, tetrahydroquinoline, and dimethylimidazolidinone;

[0057] One embodiment includes a dental glass composition that is substantially free of water, ethylene glycol, propylene glycol, polyethylene glycol, polypropylene glycol, and glycerin. Another embodiment includes a dental glass composition that is substantially free of water and polyhydric alcohols. In this embodiment, the absence of the specific components described above allows the dental glass composition to have excellent stability in properties during long-term storage, and also allows for easy overlay of coloring without bleeding, allowing for porcelain buildup thereon. Furthermore, in some cases, the generation of bubbles at the interface between the substrate and the dental porcelain during firing can be suppressed.

[0058] Another embodiment includes a dental glass composition that is substantially free of water and alcohol compounds. In this embodiment, the absence of water and alcohol compounds allows the dental glass composition to have excellent property stability during long-term storage, and allows for easy overlay of coloring without bleeding, allowing for porcelain build-up thereon. Furthermore, the generation of bubbles at the interface between the substrate and the dental porcelain during firing can be suppressed. The alcohol compound content is preferably less than 10% by mass, more preferably 8% by mass or less, even more preferably 5% by mass or less, particularly preferably 3% by mass or less, and most preferably 1% by mass or less. In this embodiment, the alcohol compound content may be less than 0.1% by mass, less than 100 ppm by mass, 10 ppm by mass or less, 1 ppm by mass or less, 0.1 ppm by mass or less, or 0 ppm by mass.

[0059] Another embodiment includes a dental glass composition that is substantially free of amine compounds. By being substantially free of amine compounds, the dental glass composition can achieve excellent property stability during long-term storage, and can easily be overcolored without bleeding, allowing porcelain to be built up thereon. Furthermore, the generation of bubbles at the interface between the substrate and the dental porcelain during firing can be suppressed. The content of the amine compounds is preferably less than 10% by mass, more preferably 8% by mass or less, even more preferably 5% by mass or less, particularly preferably 3% by mass or less, and most preferably 1% by mass or less. In the above embodiment, the content of the amine compounds may be less than 0.1% by mass, less than 100 ppm by mass, 10 ppm by mass or less, 1 ppm by mass or less, 0.1 ppm by mass or less, or 0 ppm by mass.

[0060] In the embodiment that does not contain water, an alcohol compound, or an amine compound, the absence of water and a polyhydric alcohol allows the dental glass composition to have excellent stability in properties during long-term storage, and allows for easy overlay of coloring without bleeding, and allows for porcelain build-up thereon.Furthermore, in some cases, the generation of bubbles at the interface between the substrate and the dental porcelain during firing can be suppressed.

[0061] Furthermore, another embodiment includes a dental glass composition that is substantially free of any other component that is liquid at 25° C. other than the unsaturated fatty acid component (C). "Substantially free of a component" is as explained above. For example, the embodiment includes a dental glass composition in which the content of components that are liquid at 25° C. other than the unsaturated fatty acid component (C) is less than 1 mass %.

[0062] <Unsaturated Fatty Acid Component (C)> In the dental glass composition of the present invention, the binder preferably further contains an unsaturated fatty acid component (C). Examples of the unsaturated fatty acid component (C) include unsaturated fatty acids (C-1) and unsaturated fatty acid esters (C-2). As the unsaturated fatty acid component (C), one type may be used alone, or two or more types may be used in combination.

[0063] The unsaturated fatty acid component (C) is liquid at 25°C. By further containing the unsaturated fatty acid component (C) in the dental glass composition of the present invention, the smoothness of the composition can be increased, improving operability. In addition, the unsaturated fatty acid component (C) can suppress the hygroscopicity of the dental glass composition, thereby achieving excellent property stability during long-term storage. There are no particular limitations on the unsaturated fatty acid component (C), as long as it is possible to obtain desired effects, such as the ability to adjust the viscosity of the hydrophilic organic compound (B) in a molten state.

[0064] Known unsaturated fatty acids can be used as the unsaturated fatty acid (C-1), including monounsaturated fatty acids such as crotonic acid, myristoleic acid, palmitoleic acid, sapienic acid, elaidic acid, vaccenic acid, paulic acid, oleic acid, gadoleic acid, eicosenoic acid, erucic acid, and nervonic acid; and polyunsaturated fatty acids such as linoleic acid, conjugated linoleic acid, γ-linolenic acid, eicosadienoic acid, dihomo-γ-linolenic acid, arachidonic acid, α-linolenic acid, pinolenic acid, stearidonic acid, α-eleostearic acid, β-eleostearic acid, mead acid, adrenic acid, eicosatrienoic acid, eicosapentaenoic acid, docosapentaenoic acid, docosahexaenoic acid, tetracosapentaenoic acid, tetracosahexaenoic acid, bosseopentaenoic acid, osbondo acid, sardine acid, and herring acid. As the unsaturated fatty acid (C-1), from the viewpoint of suppressing the moisture absorption of the dental glass composition, unsaturated fatty acids having 8 to 30 carbon atoms are preferred, unsaturated fatty acids having 10 to 25 carbon atoms are more preferred, unsaturated fatty acids having 12 to 20 carbon atoms are even more preferred, and polyunsaturated fatty acids having 12 to 20 carbon atoms are particularly preferred. In this specification, "polyunsaturated" is not particularly limited as long as the degree of unsaturation (number of carbon-carbon double bonds) is 2 or more.

[0065] Examples of the unsaturated fatty acid ester (C-2) include esters of the above-mentioned unsaturated fatty acids and mixtures thereof. From the viewpoint of suppressing the moisture absorption of the dental glass composition, the unsaturated fatty acid ester (C-2) is preferably an unsaturated fatty acid ester having 8 to 30 carbon atoms, more preferably an unsaturated fatty acid ester having 10 to 25 carbon atoms, even more preferably an unsaturated fatty acid ester having 12 to 20 carbon atoms, and particularly preferably a polyunsaturated fatty acid ester having 12 to 20 carbon atoms.

[0066] The unsaturated fatty acid component (C) is compatible with or dissolves in the hydrophilic organic compound (B) in a molten state, thereby easily enhancing the dispersibility of the glass powder (A) and the hydrophilic organic compound (B). The inclusion of the unsaturated fatty acid component (C) allows for the adjustment of the viscosity of the hydrophilic organic compound (B) in a molten state, enhancing the dispersibility of the glass powder (A), allowing for uniform coloring with good operability, and providing superior lubricity during drawing. Furthermore, the inclusion of the unsaturated fatty acid component (C) enhances the dispersibility of the glass powder (A) and the hydrophilic organic compound (B), thereby further enhancing the fixability of the dental glass composition in combination with the components of the binder, including the hydrophilic organic compound (B), and also providing excellent color development. Among the unsaturated fatty acid components (C), the unsaturated fatty acid (C-1) is preferred due to its excellent effects described above.

[0067] The unsaturated fatty acid component (C) in the present invention must burn out sufficiently so as not to affect the color tone after firing when the dental glass composition is applied to a substrate, and then a dental porcelain is formed thereon, and then fired. Therefore, the boiling point of the unsaturated fatty acid component (C) is preferably 400°C or lower, more preferably 385°C or lower, and even more preferably 370°C or lower. Furthermore, if an unsaturated fatty acid component (C) with a boiling point of less than 100°C is used, it may volatilize and dry even at room temperature, making it difficult to maintain a stable solid state. Therefore, the boiling point of the unsaturated fatty acid component (C) is preferably 100 to 400°C, more preferably 100 to 385°C, and even more preferably 100 to 370°C.

[0068] When the binder contains an unsaturated fatty acid component (C), the content of the unsaturated fatty acid component (C) is preferably 0.5 to 30% by mass, more preferably 1.0 to 25% by mass, even more preferably 1.5 to 20% by mass, and particularly preferably 2.0 to 18% by mass, based on the total amount of the dental glass composition. When the content of the unsaturated fatty acid component (C) is within this range, it is easy to impart appropriate strength and heat resistance to dental prostheses, the smoothness and fixation of the dental glass composition during drawing are easily improved, and color development is also excellent. When the binder contains a wax component (D) in addition to the hydrophilic organic compound (B) and the unsaturated fatty acid component (C), the content of the unsaturated fatty acid component (C) is preferably 0.2 to 30% by mass, more preferably 0.5 to 25% by mass, even more preferably 1.0 to 20% by mass, and particularly preferably 1.5 to 18% by mass, based on the total amount of the dental glass composition.

[0069] Furthermore, when the binder of the present invention contains the unsaturated fatty acid component (C), whether the binder contains or does not contain the wax component (D) in addition to the hydrophilic organic compound (B), the content of the unsaturated fatty acid component (C) is preferably equal to or less than the content of the hydrophilic organic compound (B), and more preferably less than the content of the hydrophilic organic compound (B).

[0070] A preferred embodiment includes a dental glass composition in which the binder comprises a hydrophilic organic compound (B) that is solid at 25°C and an unsaturated fatty acid component (C) that is liquid at 25°C.

[0071] <Wax Component (D)> The dental glass composition of the present invention preferably further contains a wax component (D) that is a binder that is solid at 25°C. By including the wax component (D), the wax component (D) and other binders other than the wax component (D) work together to promote solidification of the dental glass composition at room temperature, and furthermore, the hygroscopicity of the dental glass composition can be suppressed, resulting in excellent property stability during long-term storage. The wax component (D) may be used alone or in combination of two or more types. The wax component (D) has a solubility in water at 25°C of less than 1% by mass.

[0072] The melting point of the wax component (D) used in the present invention is preferably 35 to 120°C, more preferably 40 to 110°C, and even more preferably 50 to 100°C, from the viewpoint of obtaining excellent property stability during long-term storage at room temperature and good adhesion of dental prostheses. If the melting point is 35°C or lower, the wax component (D) cannot maintain its solid state, and there is a risk that the dental glass composition will flow out from the drawing surface when recoating or when building up a surface porcelain. On the other hand, if the melting point is higher than 120°C, there is a risk that adhesion to dental prostheses will not be obtained and coloring will be insufficient.

[0073] The content of the wax component (D) is preferably 1 to 55% by mass, more preferably 3 to 50% by mass, even more preferably 5 to 45% by mass, and particularly preferably 7 to 35% by mass, based on the total amount of the dental glass composition of the present invention. When the content of the wax component is within this range, it is easy to obtain, in combination with other binders, a solid dental glass composition that is excellent in color development or colorability, has high moldability and strength, and has good adhesion and fixation to dental prostheses.

[0074] In one embodiment, the binder of the dental glass composition of the present invention preferably contains a wax component having a melting point of less than 75°C (hereinafter, sometimes referred to as "first wax (D-1)"). When the dental glass composition contains the first wax (D-1), the dental glass composition has better sliding properties during drawing. In particular, when the dental glass composition does not contain the unsaturated fatty acid component (C), the dental glass composition has better sliding properties during drawing when it contains the first wax (D-1).

[0075] The melting point of the first wax (D-1) is preferably 50° C. or higher and lower than 75° C., more preferably 55 to 73° C., and even more preferably 60 to 70° C. Preferred examples of the first wax (D-1) include white petrolatum (melting point: about 38 to 60° C.), stearic acid (melting point: about 69 to 70° C.), candelilla wax (melting point: about 68 to 72° C.), beeswax (melting point: about 63° C.), hydrogenated palm oil (melting point: about 59° C.), microcrystalline wax (melting point: about 67 to 70° C.), paraffin wax (melting point: about 47 to 69° C.), hydrogenated beef tallow oil (melting point: about 46° C.), and ketone wax (melting point: about 60 to less than 75° C.).

[0076] In one embodiment, the content of the first wax (D-1) is preferably 1 to 55 mass %, more preferably 1.5 to 50 mass %, even more preferably 5 to 45 mass %, and particularly preferably 7 to 35 mass %, based on the total amount of the dental glass composition. By having the content in this range, a dental glass composition having excellent property stability during long-term storage at room temperature and excellent smoothness during drawing can be obtained.

[0077] When the dental glass composition of the present invention contains the unsaturated fatty acid component (C) and / or the first wax (D-1), smoothness and sliding properties during drawing are improved, but the dental glass composition adhered to the dental prosthesis may be easily removed due to rubbing, etc. From the viewpoint of improving the fixation of the dental glass composition, it is preferable to contain a high-melting point wax (D-2) (hereinafter, sometimes referred to as "second wax (D-2)") together with the unsaturated fatty acid component (C) and / or the first wax (D-1).

[0078] In this specification, the second wax (D-2) has a melting point of 75 to 120°C. A melting point of 75°C or higher allows the wax to conform to the fine irregularities on the surface of the substrate when combined with the unsaturated fatty acid component (C) and / or the first wax (D-1), thereby improving the fixation of the dental glass composition. Examples of the second wax (D-2) include carnauba wax, hardened castor oil (melting point: about 80 to 90°C), polyolefin wax (melting point of 75°C or higher, such as low-molecular-weight polyethylene wax (melting point: about 100 to 120°C)), long-chain saturated fatty acids (behenic acid, etc.), saturated fatty acid amides (stearic acid amide (melting point: about 98 to 105°C)), and microcrystalline wax (melting point: about 75 to 98°C). Behenic acid and carnauba wax are preferred because they have a high melting point, can be solidified with a small amount, and do not leave a firing residue after combustion.

[0079] The content of the second wax (D-2) in the wax component (D) is preferably 3 to 55 mass%, more preferably 5 to 50 mass%, even more preferably 10 to 45 mass%, and particularly preferably 15 to 35 mass%. When the content of the second wax (D-2) is within this range, it is easy to achieve a balance between the smoothness of the dental glass composition when it is drawn and the fixation of the dental glass composition. In one embodiment, the content of the second wax (D-2) is preferably less than the content of the first wax (D-1).

[0080] Furthermore, in a dental glass composition containing the second wax (D-2), the content of the second wax (D-2) is preferably less than 15 mass %, more preferably less than 12 mass %, and even more preferably less than 10 mass %, of the total amount of the dental glass composition, in order to achieve better smoothness during drawing and better fixation of the dental glass composition.

[0081] The wax component (D) in the present invention is required to burn out sufficiently so as not to affect the color tone after firing when the dental glass composition is applied to a substrate, and then a dental porcelain is built up thereon, and then fired. Therefore, the boiling point of the wax component (D) is preferably 400°C or lower, more preferably 385°C or lower, and even more preferably 370°C or lower.

[0082] In one preferred embodiment, the binder includes a dental glass composition comprising a hydrophilic organic compound (B) that is solid at 25°C, an unsaturated fatty acid component (C) that is liquid at 25°C, and a wax component (D).

[0083] Another preferred embodiment includes a dental glass composition, wherein the binder comprises a hydrophilic organic compound (B) that is solid at 25° C., and a wax component (D).

[0084] Another preferred embodiment is a dental glass composition in which the binder consists solely of a hydrophilic organic compound (B) that is solid at 25°C.

[0085] Another preferred embodiment includes a dental glass composition in which the binder consists solely of a hydrophilic organic compound (B) that is solid at 25°C and an unsaturated fatty acid component (C) that is liquid at 25°C.

[0086] Another preferred embodiment is a dental glass composition in which the binder consists only of a hydrophilic organic compound (B) that is solid at 25°C and a wax component (D).

[0087] In one preferred embodiment, the binder is a dental glass composition consisting only of a hydrophilic organic compound (B) that is solid at 25°C, an unsaturated fatty acid component (C) that is liquid at 25°C, and a wax component (D).

[0088] In another preferred embodiment, the total content of the glass powder (A) and the binder is preferably 90% by mass or more, based on the total amount of the dental glass composition. From the viewpoint of superior color development and adhesion to dental prostheses, the total content is more preferably 95% by mass or more, even more preferably 97% by mass or more, and particularly preferably 98% by mass or more.

[0089] The dental glass composition of the present invention may contain, as needed, known additives used in dental glass compositions. Examples of such additives include resins (e.g., ethylene-vinyl acetate copolymers), binders, antioxidants, surfactants, preservatives, fungicides, and antibacterial agents. One type of additive may be used alone, or two or more types may be used in combination.

[0090] The dental glass composition of the present invention may optionally contain an adhesive resin (a known adhesive resin, for example, a petroleum resin such as rosin and / or a rosin-modified product). Examples of the rosin-modified product include esters such as rosin ester, hydrogenated rosin ester, and / or polymerized rosin ester.

[0091] The dental glass composition of the present invention can be produced by a known method using glass powder (A) and hydrophilic organic compound (B). Furthermore, when the dental glass composition contains unsaturated fatty acid component (C) and wax component (D), it can also be produced by a known method. The production method is not particularly limited, but the dental glass composition of the present invention can be obtained, for example, by adding glass powder (A) to hydrophilic organic compound (B), unsaturated fatty acid component (C), and wax component (D), kneading the mixture, and extruding the mixture.

[0092] In one embodiment, when the binder component (particularly the hydrophilic organic compound (B) and the wax component (D)) has a high melting point, the dental glass composition of the present invention can also be obtained by a method of manufacturing the dental glass composition, in which the glass powder (A) is added and mixed while the binder component is heated to melt, the mixture is poured into a mold, and solidified by cooling while blowing air, and then the mixture is removed from the mold. The dental glass composition of the present invention can be obtained by adding the glass powder (A) to the molten binder component, mixing, dispersing, and then cooling.

[0093] The components can be mixed while the components other than the glass powder (A) (preferably the binder component) are in a liquid state. Usually, a binder component having a melting point higher than room temperature is heated to a temperature equal to or higher than the melting point to form a liquid, and then mixed. The heating temperature for melting the binder component can be varied depending on the type of binder component, and is not particularly limited, and may be 50°C or higher, 80°C or higher, 100°C or higher, or 150°C or higher.

[0094] The order in which the components are mixed is not particularly limited, but it is preferable to add and disperse the glass powder (A) into the liquid hydrophilic organic compound (B). When the unsaturated fatty acid component (C) is included, the glass powder (A) may be dispersed in the hydrophilic organic compound (B) and then mixed with the unsaturated fatty acid component (C). However, it is preferable to premix the hydrophilic organic compound (B) and the unsaturated fatty acid component (C) and then add the glass powder (A). Alternatively, a portion of the hydrophilic organic compound (B) and a portion of the unsaturated fatty acid component (C) may be premixed, the glass powder (A) may be added, and further mixed, and then the hydrophilic organic compound (B) and the unsaturated fatty acid component (C) may be added. A solid dental glass composition can be obtained by cooling the mixture containing the components in a mold at a temperature lower than the melting point of the hydrophilic organic compound (B).

[0095] The dental glass composition of the present invention contains a glass powder (A) and a hydrophilic organic compound (B) that is solid at 25°C, and may further contain other components (optional components) as long as they do not impede the effects of the present invention, and are substantially free of solvents.

[0096] Such other components include colorants, pH adjusters, polymerization accelerators, polymerization initiators, etc. Examples of colorants include colorants that are decolorized during baking.

[0097] Coloring agents that are decolorized during baking include food dyes that dissolve in organic solvents. Examples of food dyes include organic dyes containing two or more aromatic groups, such as Yellow No. 4 (tartrazine), Yellow No. 5 (Sunset Yellow FCF), Red No. 2 (amaranth), Red No. 102 (New Coccine), Blue No. 1 (Brilliant Blue FCF), Blue No. 2 (indigo carmine), and Green No. 3 (Fast Green FCF); organic dyes containing a condensed aromatic group with a xanthene nucleus (xanthene dyes), such as Acid Red 289, Bromopyrogallol Red, Rhodamine B, Rhodamine 6G, Rhodamine 6GP, Rhodamine 3GO, Rhodamine 123, Eosin, Eosin B, Eosin Y, Fluorescein, and Fluorescein isothiocyanate; cochineal dye (carminic acid dye); and betalain dyes, such as beet red (main components: isobetanin and betanin), betanin, isobetanin, probetanin, and neobetanin.

[0098] In one embodiment, a dental glass composition is provided that contains a glass powder (A), a hydrophilic organic compound (B), and, optionally, an unsaturated fatty acid component (C), and is substantially free of colorants that decolorize upon firing. The term "substantially free of colorants that decolorize upon firing" refers to the content of colorants that decolorize upon firing being, for example, 1,000 ppm by mass or less, preferably 100 ppm by mass or less, more preferably 10 ppm by mass or less, even more preferably 1 ppm by mass or less, particularly preferably 0.1 ppm by mass or less, and most preferably 0 ppm by mass, relative to the mass of the dental glass composition. The content of other components is not particularly limited, but is preferably 15.0% by mass or less, more preferably 12.0% by mass or less.

[0099] The method for producing a dental prosthesis of the present invention includes a step of applying the dental glass composition to a substrate of a dental prosthesis having a ceramic surface, and a method for producing a dental prosthesis in which the substrate is not fired after applying the dental glass composition and before depositing dental porcelain, but is fired after depositing dental porcelain. The substrate is as described above. The substrate of a dental prosthesis having a ceramic surface refers to a substrate (core or frame, etc.) before depositing dental porcelain. The method for producing a dental prosthesis of the present invention includes a step of applying the dental glass composition to a substrate of a dental prosthesis having a ceramic surface, and a method for producing a dental prosthesis in which the substrate to which the dental glass composition has been applied is not fired, but is fired after depositing dental porcelain. The substrate is as described above. The substrate of a dental prosthesis having a ceramic surface refers to a substrate (core or frame, etc.) before depositing dental porcelain.

[0100] The substrate for the dental prosthesis is not particularly limited as long as it is used for dental purposes, and examples thereof include various ceramics (dental ceramics such as zirconium oxide (zirconia), aluminum oxide (alumina), feldspar glass, and lithium disilicate); and ceramics such as metal-ceramic dental prostheses and all-ceramic dental prostheses, which are formed by baking a single layer or multiple layers of dental porcelain that expresses the color tone of ivory or enamel onto a dental metal core or the above-mentioned ceramic core.

[0101] The substrate of the dental prosthesis may contain ceramics at least in part and have a ceramic surface, or may be entirely made of ceramics. A substrate of a dental prosthesis having a ceramic surface can be produced, for example, by processing a commercially available product (e.g., Katana (registered trademark) Zirconia STML (manufactured by Kuraray Noritake Dental Co., Ltd.)) into a dental prosthesis having a desired shape using a known method.

[0102] The method for applying the dental glass composition to the substrate of a dental prosthesis having a ceramic surface is not particularly limited, and known methods, devices and instruments can be used.

[0103] The dental glass composition of the present invention can be applied directly to a substrate of a dental prosthesis having a ceramic surface as a porcelain stain for internal staining and surface staining, followed by firing to color the substrate. Furthermore, when the substrate of a dental prosthesis having a ceramic surface is made of zirconia, which has become popular recently and is highly transparent, the glass composition of the present invention can be applied directly to the zirconia as a porcelain stain for internal staining, followed by firing to color the zirconia frame itself, for example, to resemble ivory. In this specification, "direct application" means application in its original state without going through a paste-forming process in which a special liquid (a liquid containing water, ethanol, etc.) is added.

[0104] In another aspect, the present invention provides use of a dental glass composition comprising a glass powder (A), a hydrophilic organic compound (B) that is solid at 25°C, an unsaturated fatty acid component (C), and a wax component (D), and which is substantially free of water and propylene glycol, as a "direct application" type porcelain stain.

[0105] The dental glass composition of the present invention may be solid at 25° C. Even if the dental glass composition of the present invention is solid at room temperature, it can be used as a porcelain stain for "direct application." In this specification, "room temperature" means a temperature within the range of 20° C.±15° C. as defined in JIS Z 8703-1983, and may be, for example, 25° C.

[0106] The dental glass composition of the present invention can easily imitate tooth features (hereinafter sometimes referred to as "characters") on a ceramic-surfaced dental prosthesis substrate. Specifically, the dental glass composition of the present invention can be used alone like drawing charcoal or crayons. Furthermore, by sharpening the tip of the composition into a pencil, fine details such as enamel cracks and hairlines can be easily imitated. Furthermore, the composition can be applied to a variety of techniques, such as applying it to a blush brush or a sponge-like eyeshadow tip and rubbing it onto a ceramic-surfaced dental prosthesis substrate, enabling color shading (gradation or shading). Examples of characters include the white band of natural teeth, staining or discoloration of the cervical or approximal surfaces, demineralization, enamel cracks, and hairlines where coloring components have penetrated.

[0107] With conventional porcelain stains, a fixing firing is performed after the porcelain stain is applied. Specifically, when using conventional porcelain stains, a fixing firing is always performed after the porcelain stain is applied and before the porcelain is built up on the surface to prevent the porcelain stain from bleeding or running out. In addition, to imitate the internal structure of natural teeth, such as dentin, the dental prosthesis is stained vertically from the incisal edge to the cervical area, and to express white bands, etc., the porcelain stain must be applied horizontally mesiodistally. Each time the staining direction is changed, a fixing firing is required to prevent the stains from mixing.

[0108] On the other hand, unlike conventional porcelain stains, the dental glass composition of the present invention is a solid with no fluidity, and therefore exhibits excellent adhesion to the dental glass composition, eliminating the need for a fixation firing after each recoat. Furthermore, even when dental porcelain is applied to the surface without a fixation firing after the dental glass composition of the present invention, the composition exhibits excellent adhesion to the final dental prosthesis, preventing bleeding and runoff. Furthermore, the subsequent firing of the applied dental porcelain prevents peeling, foaming, or blackening at the interface between the porcelain and the substrate, making it possible to omit the fixation firing step. Therefore, in the method for producing a dental prosthesis of the present invention, a dental prosthesis can be obtained by applying the dental glass composition to the substrate, building up the dental porcelain, and then performing a single firing, simplifying the production process and significantly improving production efficiency.

[0109] In the case of the internal staining method, after applying the dental glass composition of the present invention, dental porcelain is built up and fired, and then the outer shape is adjusted to match the natural tooth to represent the shape of a crown, and a glazing (self-glazing) process is carried out to melt only the surface layer of dental porcelain to obtain a gloss, thereby completing the dental prosthesis. Note that the dental glass composition of the present invention can also be used in the surface staining method, in which after adjusting the outer shape to the final shape, glazing is performed using a glaze glass with a low melting temperature to obtain a gloss and coloring at the same time.

[0110] The dental porcelain used in the method for producing a dental prosthesis of the present invention is not particularly limited, and any known dental porcelain can be used, including commercially available products such as Cerabian (registered trademark) ZR Internal Stain / External Stain and Cerabian (registered trademark) ZR Press LF Internal Stain / External Stain (manufactured by Kuraray Noritake Dental Co., Ltd.).

[0111] The firing temperature (maximum firing temperature) in the firing step after laying down the dental porcelain in the present invention can be appropriately changed depending on the type of dental porcelain, the form of use, etc., and is not particularly limited as long as it allows the colorant (e.g., inorganic pigment) to develop color, but is preferably 700°C or higher, more preferably 730°C or higher, and even more preferably 750°C or higher. The upper limit of the firing temperature is not particularly limited, but is preferably 1100°C or lower, more preferably 1050°C or lower, and even more preferably 1000°C or lower. The temperature rise rate during firing up to the maximum firing temperature can be appropriately changed depending on the type of porcelain, and is not particularly limited, but is preferably about 10 to 70°C / min, and more preferably about 20 to 60°C / min.

[0112] Examples of dental prostheses finally obtained using the glass composition of the present invention include metal ceramic dental prostheses and all-ceramic dental prostheses restored using an alumina core, zirconia core, or the like.

[0113] Specific examples of the dental prosthesis that can be finally obtained include copings, frameworks, denture bases, dentures, orthodontic products, and implant products.

[0114] Examples of dentures include crowns, bridges, inlays, onlays, and laminate veneers.

[0115] Orthodontic products include, for example, brackets.

[0116] Examples of dental implant products include implants, abutments, implant fixtures, implant bridges, implant bars, and implant superstructures in which a gum (gingival) portion is attached to a prosthesis.

[0117] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0118] Solid dental glass compositions of Examples 1 to 14 and Comparative Examples 1 to 9 were prepared as follows, and their properties were evaluated. The results are shown in Tables 1 and 2. For each component in Tables 1 and 2, "%" represents mass %. In Tables 1 and 2, "PEG-2000" and "PEG-1000" refer to polyethylene glycol with a weight-average molecular weight (Mw) of 2000 and polyethylene glycol with a weight-average molecular weight (Mw) of 1000, respectively. In Tables 1 and 2, "Macrogol Ointment" refers to a mixture of equal amounts of polyethylene glycol 400 (Mw: 400) and 4000 (Mw: 4000). In Tables 1 and 2, "room temperature" refers to evaluation at 25°C. The properties of the compositions were also evaluated at 25°C.

[0119] The weight average molecular weight was determined by gel permeation chromatography (GPC) and calculated in terms of polystyrene.

[0120] The solubility of PEG-2000 in water at 25°C was 50% by mass or more. The solubility of PEG-1000 in water at 25°C was 50% by mass or more. The solubility of macrogol ointment in water at 25°C was 50% by mass or more. The solubilities of stearic acid, white petrolatum, carnauba wax, and behenic acid in water at 25°C were all less than 1% by mass.

[0121] [Examples 1 to 14 and Comparative Examples 1 to 6 and 9] A hydrophilic organic compound (B), an unsaturated fatty acid component (C), and a wax component (D) were melted in a container on a hot stirrer at 120°C to the mass percentages shown in Tables 1 and 2, and then glass powder (A) (Cerabian® ZR Internal Stain, manufactured by Kuraray Noritake Dental Co., Ltd.) was added and mixed with a metal spatula until uniform. The resulting mixture was poured into a mold measuring 20.0 mm in length, 3.0 mm in width, and 3.0 mm in depth, and cooled to solidify, producing a solid dental glass composition. The glass powder (A) product was a potassium aluminosilicate glass containing a pigment and having a reddish-brown color.

[0122] The average particle diameter of the glass powder (A) was determined by a laser diffraction particle size distribution analyzer (SALD-2300, manufactured by Shimadzu Corporation) as the median diameter (d 50 ) was taken as the average particle size.

[0123] Comparative Examples 7 and 8 Each of the components shown in Table 2 was weighed on a glass plate so as to give the mass % shown in Table 2, and mixed as is with a spatula to obtain a paste composition.

[0124] [Preparation of Zirconia Sintered Body] Commercially available dental zirconia (Katana (registered trademark) Zirconia STML: manufactured by Kuraray Noritake Dental Co., Ltd.) was processed into a cylindrical shape with a diameter of approximately 18 mm, and fired in a firing furnace "Noritake Katana (registered trademark) F-1" manufactured by SK Medical Electronics Co., Ltd. at a maximum temperature of 1550°C for 2 hours, thereby obtaining a zirconia sintered body to be used as a substrate.

[0125] [Method for evaluating fixation property] A line was drawn on the surface of the zirconia sintered body of the base material prepared by the method described above using the dental glass composition of each Example and Comparative Example prepared by the method described above, and a dental porcelain (Cerabian (registered trademark) ZR Translucent Tx: manufactured by Kuraray Noritake Dental Co., Ltd.) mixed with purified water was built up on top of the line.

[0126] <Evaluation criteria> In the dental glass composition of all the obtained samples, if the shape of the drawn line was maintained, it was evaluated as "a", if even one of the drawn lines maintained its shape but the colors were mixed, it was evaluated as "b", and if even one of the lines flowed together with the porcelain and the shape of the line was not maintained, it was evaluated as "c" (n=3). In practical use, "a" and "b" were considered to be acceptable products.

[0127] [Method for evaluating color development] A line was drawn on the surface of the zirconia sintered body of the base material prepared by the method described above using the dental glass composition of each Example and Comparative Example prepared by the method described above, and a dental porcelain (Cerabian (registered trademark) ZR Translucent Tx: manufactured by Kuraray Noritake Dental Co., Ltd.) mixed with purified water was layered on top of the line, and fired by holding at 930°C for 1 minute.

[0128] <Evaluation criteria> In visual observation of all the obtained dental glass compositions, if the color of the drawn lines was clear, it was evaluated as "a", if even one line was unclear and whitish, it was evaluated as "b", and if even one line was bleeding or no color was observed, it was evaluated as "c" (n=3). In practical use, "a" and "b" were considered to be acceptable products.

[0129] A photograph of the test piece used to evaluate the fixability and color development of Example 1 is shown in Figure 1, and a photograph of the test piece used to evaluate the fixability and color development of Comparative Example 5 is shown in Figure 2. As shown in the photograph in Figure 2, in Comparative Example 5, the shape of the drawn line could not be maintained and the color was blurred. In contrast, in Figure 1, the shape of the drawn line was maintained and the color of the drawn line was clear.

[0130] [Method for Evaluating Interface Condition] The samples evaluated using the [Method for Evaluating Color Development] above were cut in a direction perpendicular to the drawn line and polished to a smooth cut surface. The polished cut surface was observed under an optical microscope (DIGITAL MICROSCOPE KH-7700: Hirox Co., Ltd.) at 1000x magnification to check for significant bubbles or peeling in the dental glass composition at the interface between the substrate and the dental porcelain. As a control, a cut surface of a sample in which dental porcelain was built up on a substrate using the conventional internal staining method (with fixation and firing) and fired was observed, and fine bubbles were observed. Figure 3 shows the results (photographs) of optical microscopic observations of the cut surface used for the evaluation method and the control cut surface. The presence of only fine bubbles, as shown in Figure 3, does not indicate peeling. Therefore, the interface was evaluated using the following evaluation criteria (n = 3).

[0131] <Evaluation criteria> If bubbles are found in all samples to the same extent as in the control, it is rated as: "a" If it is confirmed that there are more bubbles in even one sample than in the control, it is rated as: "b" If there are clearly more bubbles in even one sample than in the control, or if interfacial peeling is found in even one place, it is rated as: "c" If interfacial peeling is found in several places in even one sample, it is rated as: "d" In practical use, "a" and "b" were deemed to be acceptable products.

[0132] An optical microscope photograph of the fractured surface in the evaluation of the interface state in Example 1 is shown in Figure 4. Also, an optical microscope photograph of the fractured surface in the evaluation of the interface state in Comparative Example 2 is shown in Figure 5. In Figure 5, an air layer was formed between the substrate and the porcelain, and clear delamination was confirmed.

[0133] [Method for Evaluating Operability] A line was drawn on the surface of the zirconia sintered body prepared in the above [Preparation of Zirconia Sintered Body] using the dental glass composition prepared by the above method.

[0134] <Evaluation criteria> For all samples, if a line could be drawn and spread evenly, it was evaluated as "a", if even one line could be drawn but was not uniform in parts, it was evaluated as "b", and if even one surface of the zirconia sintered body was exposed, it was evaluated as "c" (n=3). In practical use, "a" and "b" were considered to be acceptable products.

[0135]

[0136]

[0137] In Comparative Examples 1 to 4, which did not contain the hydrophilic organic compound (B), the observation of the cut surface revealed the presence of peeling, cavities, or air bubbles at part of the interface between the base material (substrate) and the porcelain. It is presumed that the stain solidified only with the wax component was in a water-repellent state (non-wettable) with the porcelain for building up, and that an air layer remained at the interface between the base material and the porcelain upon firing the porcelain, resulting in the peeling, cavities, or air bubbles.

[0138] In Comparative Examples 5 to 9, which were in paste form, none of the compositions were able to set or develop color without firing for fixation, resulting in a loss of aesthetic appeal as a dental prosthesis. Paste compositions essentially require firing for fixation, and it is presumed that when porcelain was built up after the paste composition was applied, some of the paste composition mixed with the porcelain, causing the paste composition to shift from the original application location, thereby damaging the aesthetic appeal.

[0139] On the other hand, Examples 1 to 14, which are dental glass compositions containing the hydrophilic organic compound (B), exhibited good fixability and color development even without performing fixation baking. In particular, comparisons between Example 5 and Comparative Example 1 and between Example 12 and Comparative Example 3 confirmed that the present invention exhibits excellent effects.

[0140] Furthermore, it was also confirmed that the dental glass compositions of Examples 1 to 14 did not change over time, were easy to handle, and could be applied uniformly.

[0141] The glass composition of the present invention is preferably used as a dental glass composition because, by being solidified to have good fixability to dental prostheses, the glass composition itself undergoes almost no change over time, can be applied as a thin film to dental prostheses, and, because of its lack of fluidity, can be applied without bleeding, and dental prostheses having good operability and a desired color tone can be easily produced. Furthermore, with the increasing demand for ceramic dental crowns in particular and the increasing demand for individual aesthetics, it is expected that the frequency of use of dental glass compositions will increase, and therefore the dental glass composition of the present invention, which does not require a fixing or baking step, is useful.

Claims

1. A glass powder (A) and a binder, The binder comprises a hydrophilic organic compound (B) that is solid at 25° C., A dental glass composition that is substantially free of water and propylene glycol.

2. 2. The dental glass composition according to claim 1, wherein the average particle size of the glass powder (A) is 0.05 μm to 50 μm.

3. 2. The dental glass composition according to claim 1, wherein the hydrophilic organic compound (B) has a melting point of 35° C. or higher.

4. 2. The dental glass composition according to claim 1, wherein the hydrophilic organic compound (B) is a water-soluble polymer.

5. 2. The dental glass composition according to claim 1, wherein the content of the hydrophilic organic compound (B) is 1 to 50% by mass.

6. 2. The dental glass composition of claim 1, wherein the binder further comprises an unsaturated fatty acid component (C) that is liquid at 25°C.

7. 7. The dental glass composition according to claim 6, wherein the content of the unsaturated fatty acid component (C) is 0.5 to 30% by mass.

8. 2. The dental glass composition of claim 1, wherein the binder further comprises a wax component (D) that is solid at 25°C.

9. 2. The dental glass composition according to claim 1, wherein the water and propylene glycol content is less than 1000 ppm by weight.

10. 2. The dental glass composition of claim 1, which is solid at 25°C.

11. 10. The dental glass composition of claim 1 which is a porcelain stain.

12. 12. A method for producing a dental prosthesis, comprising the steps of: applying the dental glass composition according to any one of claims 1 to 11 to a substrate of a dental prosthesis having a ceramic surface; and firing the substrate after the application of the dental glass composition and before the deposition of dental porcelain, without firing the substrate.

13. The method for producing a dental prosthesis according to claim 12, wherein the firing temperature in the firing step after the deposition of the dental porcelain is 700 to 1100°C.