Positive electrode active material for nonaqueous electrolyte secondary batteries

JPWO2023188766A5Pending Publication Date: 2024-12-09
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024511312
Authority / Receiving Office
JP · JP
Patent Type
Applications
Filing Date
2024-06-17
Publication Date
2024-12-09

AI Technical Summary

Technical Problem

Current non-aqueous electrolyte secondary batteries face challenges in achieving high discharge voltage, with existing positive electrode active materials not meeting the desired voltage thresholds efficiently.

Method used

A positive electrode active material with a crystal structure belonging to the Fm-3m space group, composed of a complex oxide with the formula Li_x TM_tm M_y O_2-f F_f, where TM is a transition metal and M is a non-transition metal, is developed, which exhibits one or more peaks in the dV/dq-SOC curve within the 40% to 70% SOC range, enhancing discharge voltage performance.

Benefits of technology

The material achieves a high discharge voltage and capacity, with discharge capacities exceeding 100mAh/g and 200mAh/g under specific conditions, demonstrating improved performance compared to comparative examples.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A positive electrode active material for nonaqueous electrolyte secondary batteries according to the present invention is a composite oxide which is represented by general formula LixTMtmMyO2-fFf and has a crystal structure that belongs to the space group Fm-3m; and in the general formula, TM represents a transition metal, M represents a non-transition metal, and if Q = 2 × tm × (1 - (1 - f / 2)5), Q ≥ 1 is satisfied. With respect to a dV / dq-SOC curve showing the relationship between the state of charge SOC and dV / dq of a half cell that contains this composite oxide, the dV / dq-SOC curve being obtained by charging the half cell with a charging current of 0.1 C at 25°C to an end voltage within the range of 4.7 V to 4.95 V, there is one or more peaks within the SOC range from 40% to 70%.
Need to check novelty before this filing date? Find Prior Art

Description

Cathode active material for non-aqueous electrolyte secondary batteries

[0001] The present disclosure relates to a technique for a positive electrode active material for a non-aqueous electrolyte secondary battery.

[0002] BACKGROUND ART As a secondary battery with high output and high energy density, for example, a non-aqueous electrolyte secondary battery that includes a positive electrode, a negative electrode, and a non-aqueous electrolyte and performs charging and discharging by transferring lithium ions or the like between the positive electrode and the negative electrode has been widely used.

[0003] For example, Patent Document 1 discloses a composite oxide having a crystal structure belonging to the space group Fm-3m, containing lithium and molybdenum, and substantially not containing chromium, as a positive electrode active material for use in a non-aqueous electrolyte secondary battery.

[0004] JP 2017-202954 A

[0005] An object of the present disclosure is to provide a positive electrode active material for a non-aqueous electrolyte secondary battery having a high discharge voltage.

[0006] The positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure has a crystal structure belonging to the space group Fm-3m and has the general formula: Li x TM tm M y O 2-f F f In the general formula, TM is a transition metal, M is a non-transition metal, and Q=2×tm×{1−(1−f / 2) 5and when the composite oxide is made into a half-cell by the following method, the half-cell is charged at 25°C with a charging current of 0.1 C to an end voltage range of 4.7 to 4.95 V, and the dV / dq-SOC curve, which is the relationship between dV / dq, which is the ratio of a change in voltage V of the half-cell to a change in battery capacity q of the half-cell, and dq, and the state of charge SOC of the half-cell, has one or more peaks in the range of SOC 40% or more and 70% or less. (Method: The composite oxide, acetylene black, and polyvinylidene fluoride were mixed in a mass ratio of 7:2:1, and dispersed using N-methyl-2-pyrrolidone to prepare a slurry for the positive electrode composite layer. This slurry for the positive electrode composite layer was applied to aluminum foil, dried, and then rolled to a film thickness of 20 to 50 μm. The mixture was then punched out to a size of 20 mm × 20 mm to obtain a positive electrode. An electrode assembly, in which a separator was interposed between this positive electrode and a metallic lithium foil (thickness: 0.3 mm) serving as a negative electrode, was housed in an exterior case of aluminum laminate film, and LiPF was dissolved in a mixed solvent of fluoroethylene carbonate and methyl propionate (volume ratio: 1:3). 6 A non-aqueous electrolyte prepared by dissolving the above in an amount of 1 mol / L is poured into the outer casing and sealed to form a half-cell.

[0007] According to one aspect of the present disclosure, a positive electrode active material for a non-aqueous electrolyte secondary battery having a high discharge voltage can be provided.

[0008] FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment. FIG. 2 is a diagram showing X-ray diffraction results for Example 1. FIG. 3 is a diagram showing X-ray diffraction results for Example 6. FIG. 4 is a diagram showing X-ray diffraction results for Example 13. FIG. 5 is a diagram showing X-ray diffraction results for Example 14. FIG. 6 is a diagram showing X-ray diffraction results for Example 15. FIG. 7 is a diagram showing X-ray diffraction results for Example 17. FIG. 8 is a diagram showing X-ray diffraction results for Comparative Example 1. FIG. 9 is a diagram showing X-ray diffraction results for Comparative Example 2. FIG. 10 is a diagram showing X-ray diffraction results for Comparative Example 3. FIG. 11 is a diagram showing X-ray diffraction results for Comparative Example 4. The graphs show dV / dq-SOC curves for half-cells of Examples 1 and 2 and Comparative Examples 1 and 2. The graphs show dV / dq-SOC curves for half-cells of Examples 4, 5, 6, and 8. The graphs show dV / dq-SOC curves for half-cells of Examples 10, 13, and 14. The graphs show dV / dq-SOC curves for half-cells of Examples 15, 16, and 17.

[0009] An example of a nonaqueous electrolyte secondary battery using the positive electrode active material for a nonaqueous electrolyte secondary battery according to the present disclosure will be described below.

[0010] FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment. The nonaqueous electrolyte secondary battery 10 shown in FIG. 1 includes a wound electrode assembly 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, a nonaqueous electrolyte, insulating plates 18 and 19 disposed above and below the electrode assembly 14, respectively, and a battery case 15 for accommodating the above components. The battery case 15 is composed of a case body 16 and a sealing member 17 that closes the opening of the case body 16. Note that, instead of the wound electrode assembly 14, other electrode bodies may be used, such as a laminated electrode assembly formed by alternately stacking positive and negative electrodes with separators interposed therebetween. Examples of the battery case 15 include a cylindrical, prismatic, coin-shaped, or button-shaped metal case, and a resin case formed by laminating a resin sheet (a laminated battery).

[0011] The non-aqueous electrolyte includes, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms of these solvents are substituted with halogen atoms such as fluorine. The electrolyte salt may include, for example, LiPF 6 The non-aqueous electrolyte is not limited to a liquid electrolyte, but may be a solid electrolyte using a gel polymer or the like.

[0012] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has, for example, a protruding portion 22, which is a portion of the side surface that protrudes inward and supports the sealing body 17. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.

[0013] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked in this order from the electrode body 14 side. Each component constituting the sealing body 17 has, for example, a disk or ring shape, and all components except for the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the nonaqueous electrolyte secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 deforms and ruptures, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 ruptures, and gas is discharged from the opening of the cap 27.

[0014] 1 , a positive electrode lead 20 attached to the positive electrode 11 passes through a through-hole in the insulating plate 18 and extends toward the sealing body 17, and a negative electrode lead 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom of the case body 16. The positive electrode lead 20 is connected by welding or the like to the underside of a filter 23, which is the bottom plate of the sealing body 17, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected by welding or the like to the inner bottom surface of the case body 16, and the case body 16 serves as the negative electrode terminal.

[0015] The positive electrode 11, the negative electrode 12, and the separator 13 will be described in detail below.

[0016] <Positive Electrode> The positive electrode 11 includes a positive electrode current collector and a positive electrode composite layer disposed on the positive electrode current collector. The positive electrode current collector may be a foil of a metal such as aluminum that is stable within the potential range of the positive electrode, or a film having such a metal disposed on its surface. The thickness of the positive electrode current collector is preferably, for example, in the range of 1 μm to 20 μm.

[0017] The positive electrode mixture layer preferably contains a positive electrode active material and further contains a binder, a conductive material, etc. The thickness of the positive electrode mixture layer is preferably in the range of, for example, 10 μm to 300 μm.

[0018] The positive electrode 11 is obtained, for example, by applying a slurry for a positive electrode composite layer containing a positive electrode active material, a binder, a conductive material, etc. onto a positive electrode current collector and drying the slurry to form a positive electrode composite layer on the positive electrode current collector, and then rolling the positive electrode composite layer.

[0019] The positive electrode active material contains a composite oxide having a crystal structure belonging to the space group Fm-3m.

[0020] A crystalline structure belonging to the space group Fm-3m refers to a structure having peaks attributable to the space group Fm-3m in a diffraction pattern obtained by X-ray diffraction (XRD) measurement. The "-3" in the space group "Fm-3m" represents a symmetric element of the three-fold reversal axis, and should be expressed as a bar "-" above the "3." The X-ray diffraction pattern of the complex oxide can be measured by powder X-ray diffraction measurement using an X-ray diffractometer (Rigaku's "MiniFlex II"), using a CuKα radiation source, a tube voltage of 40 kV, and a tube current of 15 mA. The diffracted X-rays pass through a 30 μm-thick Kβ filter and are detected by a high-speed one-dimensional detector (D / teX Ultra 2). The sampling width is 0.02°, the scan speed is 10° / min, the divergence slit width is 0.625°, the receiving slit width is 13 mm (OPEN), and the scattering slit width is 8 mm. The crystal structure of the complex oxide can be identified by Rietveld analysis using the "RIETAN-FP" program (F. Izumi and K. Momma, Solid State Phenom., 130, 15-20 (2007)) based on the obtained X-ray diffraction pattern. The X-ray diffraction apparatus is not limited to the above apparatus, and the X-ray source is not limited to the above conditions. The X-ray diffraction measurement conditions are not limited to the above conditions. The method for analyzing the obtained X-ray diffraction pattern is not limited to the above method.

[0021] The composite oxide having a crystal structure belonging to the space group Fm-3m has the general formula: Li x TM tm M y O 2-f F f In the general formula, TM is a transition metal, M is a non-transition metal, and Q=2×tm×{1−(1−f / 2) 5}, Q≧1 is satisfied. Here, Q represents the number of oxygen atoms bonded to the transition metal bonded to fluorine. Furthermore, when a half-cell using this composite oxide as a positive electrode active material is charged at 25°C with a charging current of 0.1 C to an end voltage range of 4.7 to 4.95 V, the dV / dq-SOC curve, which is the relationship between dV / dq, which is the ratio of the change in half-cell voltage V (dV) to the change in battery capacity q (dq), of the half-cell, and the state of charge (SOC) of the half-cell, has one or more peaks in the range of SOC 40% to 70%. By using such a composite oxide, a high discharge voltage can be obtained. The conditions for preparing a half-cell using the composite oxide as a positive electrode active material will be described in the examples.

[0022] In the dV / dq-SOC curve of a half cell using a composite oxide as a positive electrode active material, there is no limit to the number of peaks as long as there is at least one peak in the range of SOC 40% to 70%. There may be only one peak. It is also preferable that there be no peak in the range of SOC less than 40%.

[0023] (dV / dq-SOC Curve) After starting charging of the half-cell under the above conditions, the battery voltage V and current value I of the half-cell are measured at predetermined time intervals, and the SOC (charge rate) is calculated based on the battery voltage V. Furthermore, the amount of change dq in the battery capacity (charge capacity) q of the half-cell and the amount of change dV in the battery voltage V are calculated from the measured values ​​of the battery voltage V and current value I at this time, and dV / dq is calculated based on these calculation results. Once the SOC and dV / dq of the half-cell are calculated at predetermined time intervals, a dV / dq-SOC curve showing the relationship between SOC and dV / dq can be obtained based on these calculation results. Specifically, the dV / dQ-SOC curve can be obtained by graphing these values ​​calculated at predetermined time intervals, with the SOC value on the horizontal axis and the dV / dq value on the vertical axis.

[0024] The composition of the composite oxide affects whether or not the dV / dq-SOC curve has one or more peaks in the range of SOC 40% or more and 70% or less. In order to have one or more peaks in the dV / dq-SOC curve in the range of SOC 40% or more and 70% or less, it is preferable to control tm and f in the above general formula within the range of Q≧1, for example. Furthermore, in the general formula, x, tm, y, and f preferably satisfy 1.75≦x+tm+y≦2, 0<f≦0.7, and also preferably satisfy 1.0<x≦1.4, 0.4≦tm<1.0, 0≦y≦0.2, 0.25≦f≦0.6. Note that the above crystal structure may have vacancies in which Li atoms, TM atoms, and M atoms are not arranged. Here, "having vacancies" means that in the positive electrode active material taken out immediately after production or after disassembling a discharged secondary battery, vacancies that are not filled with Li atoms, TM atoms, or M atoms exist in the composite oxide. The molar ratio of the vacancies is preferably 0.05 or more and 0.25 or less.

[0025] In a half-cell using the composite oxide of this embodiment, the half-cell is charged at a constant current of 0.1 C at 25° C. to an end voltage in the range of 4.7 to 4.95 V, and then charged at a constant voltage of 0.05 C at the end voltage, and then discharged at a discharge current of 0.1 C to an end voltage of 3.0 to 3.5 V. The discharge capacity is 100 mAh / g or more. The discharge capacity is the capacity per unit mass of the positive electrode active material.

[0026] Furthermore, in a half-cell using the composite oxide of this embodiment, the half-cell is charged at a constant current of 0.1 C at 25° C. to an end voltage in the range of 4.7 to 4.95 V, and then charged at a constant voltage of 0.05 C at the end voltage, and then discharged at a discharge current of 0.1 C to an end voltage of 2.5 to 3.0 V. The discharge capacity is 200 mAh / g or more.

[0027] The composite oxide preferably contains Mn as a transition metal (TM) in that a high discharge voltage can be obtained, and in the general formula, the molar ratio of Mn, tm_Mn, in tm, is preferably 0.6<tm_Mn<0.8.

[0028] The composite oxide preferably contains Mn and a transition metal other than Mn, such as Ni, Co, Fe, Ti, Y, Zr, Nb, Mo, Sc, W, V, Gd, Ce, Ta, and Ag, in order to obtain a high discharge voltage.

[0029] Examples of the non-transition metal (M) contained in the composite oxide include Al, Mg, Sb, Bi, Ca, Sr, Mg, K, Ga, Sn, and Zn.

[0030] The composition of the composite oxide can be confirmed by, for example, inductively coupled plasma emission spectroscopy, X-ray photoelectron spectroscopy, and Rietveld analysis of parameters obtained by powder X-ray diffraction.

[0031] The method for producing the composite oxide is not particularly limited and may be a known method for synthesizing positive electrode active materials. For example, the composite oxide can be obtained by treating a lithium source, an additive element source, a fluorine source, etc., by a mechanochemical method. The mechanochemical method (also referred to as mechanochemical treatment) refers to a synthesis method utilizing a mechanochemical reaction. A mechanochemical reaction refers to a chemical reaction such as a crystallization reaction, a solid solution reaction, or a phase transition reaction that utilizes high energy generated locally due to mechanical energy such as friction or compression during the crushing process of a solid substance. Examples of equipment used in the mechanochemical method include grinding and dispersing machines such as ball mills, bead mills, vibration mills, turbo mills, mechanofusion machines, and disk mills. Among these, a ball mill is preferred. The mechanochemical treatment may be performed in an inert gas atmosphere such as argon gas, or in an oxygen-containing atmosphere.

[0032] Examples of the lithium source include lithium carbonate and lithium hydroxide. Examples of the additive element source include a transition metal-containing compound and a non-transition metal-containing compound, such as a transition metal-containing oxide or hydroxide, a non-transition metal-containing oxide or hydroxide, or a transition metal and non-transition metal-containing composite oxide or hydroxide. Examples of the fluorine source include fluorides such as lithium fluoride, molybdenum fluoride, and magnesium fluoride. Lithium fluoride may be used as the lithium source, a transition metal fluoride such as molybdenum fluoride may be used as the transition metal-containing compound that is the additive element source, or a non-transition metal fluoride such as magnesium fluoride may be used as the non-transition metal-containing compound that is the additive element source.

[0033] The composite oxide obtained by the mechanochemical treatment may be heat-treated. The heating temperature is not particularly limited, but is, for example, in the range of 500°C to 1000°C. The heating time is also not particularly limited, but is, for example, 1 hour to 20 hours. Heating may be performed in an inert gas atmosphere such as argon gas, or in an oxygen-containing atmosphere.

[0034] The positive electrode active material may be composed of only the above-mentioned composite oxide, or may contain other active materials in addition to the above-mentioned composite oxide. x MO y (M represents at least one transition metal) 2 Li having a type crystal structure x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Ni α Co (1-α) O 2 , Li x Ni α Mn β Co (1-α-β) O 2 Li having a spinel-type crystal structure, such as x Mn 2 O 4 , Li x Ni α Mn (2-α) O4 etc.), Li w M' x (XO y ) z (M' represents at least one transition metal, and X represents, for example, P, Si, B, V, etc.) 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO 4 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 MnSiO 4 , Li 2 CoPO 4 F, etc.)

[0035] It has a crystal structure belonging to the space group Fm-3m and has the general formula: Li x TM tm M y O 2-f F f In the general formula, TM is a transition metal, M is a non-transition metal, and Q=2×tm×{1−(1−f / 2) 5}, the content of the composite oxide that satisfies Q≧1 and has one or more peaks in the SOC range of 40% or more and 70% or less in the dV / dq-SOC curve is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, relative to the total mass of the positive electrode active material.

[0036] Examples of the conductive material contained in the positive electrode mixture layer include carbon powders such as carbon black, acetylene black, ketjen black, and graphite. These may be used alone or in combination of two or more.

[0037] Examples of binders that can be used in the positive electrode mixture layer include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), PAN, polyimide-based resins, acrylic-based resins, polyolefin-based resins, styrene-butadiene rubber (SBR), CMC or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc.), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.

[0038] <Negative Electrode> The negative electrode 12 includes a negative electrode current collector such as a metal foil and a negative electrode composite layer formed on the negative electrode current collector. The negative electrode current collector can be a foil of a metal such as copper that is stable in the potential range of the negative electrode, or a film with such a metal disposed on the surface layer. The negative electrode composite layer includes, for example, a negative electrode active material, a binder, etc.

[0039] The negative electrode active material contained in the negative electrode mixture layer is not particularly limited as long as it is a material capable of absorbing and releasing lithium ions, and examples thereof include carbon materials, elements capable of forming an alloy with lithium, or compounds containing such elements. Examples of carbon materials that can be used include graphites such as natural graphite, non-graphitizable carbon, and artificial graphite, and cokes. Examples of elements capable of forming an alloy with lithium or compounds containing such elements include silicon, tin, and silicon oxide or tin oxide formed by bonding these with oxygen. In addition to the above, materials such as lithium titanate that have a higher charge / discharge potential relative to metallic lithium than carbon materials can also be used. Examples of binders contained in the negative electrode mixture layer include those similar to those used in the positive electrode.

[0040] <Separator> The separator 13 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include olefin-based resins such as polyethylene and polypropylene, and cellulose. The separator 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin-based resin, or the separator 13 may have an aramid resin or the like applied to its surface.

[0041] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.

[0042] Example 1 Preparation of Positive Electrode Active Material Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), gallium oxide (Ga 2 O 3 ), niobium oxide (Nb 2 O 5 ), cerium oxide (CeO 2 ) was used as the starting source of the composite oxide, and the Li:Mn:Ga:Nb:Ce:F molar ratio was weighed and mixed to be 1.126:0.695:0.048:0.038:0.005:0.431. The mixed powder was placed in a planetary ball mill (Fritsch Premium-Line P7, rotation speed: 600 rpm, container: zirconia 45 mL pot, ball: zirconia φ3 mm ball) and treated in an Ar atmosphere at room temperature for 35 hours (35 cycles of 1 hour operation followed by a 10 minute break). In this way, Li 1.126 Mn 0.695 Ga 0.048 Nb 0.038 Ce 0.005 O 1.569 F 0.431 A composite oxide represented by the formula:

[0043] The obtained composite oxide was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 2. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m. The conditions for the powder X-ray diffraction measurement were as described above (the same conditions were used for the other examples and comparative examples).

[0044] The obtained composite oxide was used as a positive electrode active material to prepare a half cell in the following manner.

[0045] [Preparation of Positive Electrode] 70 parts by mass of the composite oxide, 20 parts by mass of acetylene black, and 10 parts by mass of polyvinylidene fluoride were mixed, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a slurry for the positive electrode composite layer. Next, the slurry for the positive electrode composite layer was applied to an aluminum foil with a thickness of 15 μm, dried, and then rolled to a film thickness in the range of 20 to 50 μm. After that, the aluminum foil was die-cut into a size of 20 mm × 20 mm, and a positive electrode having a positive electrode composite layer formed on both sides thereof was obtained.

[0046] [Preparation of Non-Aqueous Electrolyte] A mixed solvent of fluoroethylene carbonate (FEC) and methyl propionate (FMP) in a volume ratio of 1:3 was dissolved in lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1 mol / liter to prepare a non-aqueous electrolyte.

[0047] [Preparation of Test Cell] Electrode leads were attached to the metal lithium foils (0.3 mm thick) used as the positive and negative electrodes. An electrode assembly was then prepared by interposing a separator between the positive and negative electrodes. This electrode assembly was then housed in an exterior case made of aluminum laminate film, and the nonaqueous electrolyte was poured into the exterior case, after which the exterior case was sealed. This was used as a half-cell (nonaqueous electrolyte secondary battery) of Comparative Example 1.

[0048] Example 2: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), magnesium oxide (MgO), gadolinium oxide (Gd 2 O 3 ), niobium oxide (Nb 2 O 5 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Gd:Nb:F was 1.139:0.678:0.024:0.025:0.048:0.436. 1.139 Mn 0.678 Mg 0.024 Gd 0.025 Nb 0.048 O1.564 F 0.436 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement to analyze its crystal structure, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0049] And Li 1.139 Mn 0.678 Mg 0.024 Gd 0.025 Nb 0.048 O 1.564 F 0.436 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0050] Example 3: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), gallium oxide (Ga 2 O 3 ), niobium oxide (Nb 2 O 5 ), cerium oxide (CeO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Ga:Nb:Ce:F was 1.2:0.58:0.05:0.01:0.01:0.6. 1.2 Mn 0.58 Ga 0.05 Nb 0.01 Ce 0.01 O 1.4 F 0.6 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 3. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0051] And Li 1.2 Mn 0.58 Ga 0.05 Nb 0.01 Ce 0.01 O 1.4 F 0.6 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0052] Example 4: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), magnesium oxide (MgO), niobium oxide (Nb 2 O 5 ), cerium oxide (CeO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Nb:Ce:F was 1.217:0.696:0.015:0.01:0.005:0.596. The same procedure as in Example 1 was carried out to obtain Li, 1.217 Mn 0.696 Mg 0.015 Nb 0.01 Ce 0.005 O 1.404 F 0.596 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement to analyze its crystal structure, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0053] And Li 1.217 Mn 0.696 Mg 0.015 Nb 0.01 Ce 0.005 O 1.404 F 0.596 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0054] Example 5: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), magnesium oxide (MgO), gallium oxide (Ga 2 O 3 ), cerium oxide (CeO 2) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Ga:Ce:F was 1.15:0.745:0.025:0.025:0.005:0.4. 1.15 Mn 0.745 Mg 0.025 Ga 0.025 Ce 0.005 O 1.6 F 0.4 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement to analyze its crystal structure, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0055] And Li 1.15 Mn 0.745 Mg 0.025 Ga 0.025 Ce 0.005 O 1.6 F 0.4 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0056] Example 6: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), magnesium oxide (MgO), gadolinium oxide (Gd 2 O 3 ), cerium oxide (CeO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Gd:Ce:F was 1.225:0.705:0.005:0.01:0.005:0.6. 1.225 Mn 0.705 Mg 0.005 Gd 0.01 Ce 0.005 O 1.4 F 0.6 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 4. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0057] And Li 1.225 Mn 0.705 Mg 0.005 Gd 0.01 Ce 0.005 O 1.4 F 0.6 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0058] Example 7: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), magnesium oxide (MgO), gallium oxide (Ga 2 O 3 ), niobium oxide (Nb 2 O 5 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Ga:Nb:F was 1.225:0.7:0.01:0.01:0.005:0.6. 1.225 Mn 0.7 Mg 0.01 Ga 0.01 Nb 0.005 O 1.4 F 0.6 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement to analyze its crystal structure, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0059] And Li 1.225 Mn 0.7 Mg 0.01 Ga 0.01 Nb 0.005 O 1.4 F 0.6 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0060] Example 8: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li2 O 2 ), magnesium oxide (MgO), niobium oxide (Nb 2 O 5 ), cerium oxide (CeO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Nb:Ce:F was 1.143:0.765:0.02:0.01:0.005:0.447. 1.143 Mn 0.765 Mg 0.02 Nb 0.01 Ce 0.005 O 1.553 F 0.447 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement to analyze its crystal structure, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0061] And Li 1.143 Mn 0.765 Mg 0.02 Nb 0.01 Ce 0.005 O 1.553 F 0.447 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0062] Example 9: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), gadolinium oxide (Gd 2 O 3 ), niobium oxide (Nb 2 O 5 ), cerium oxide (CeO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Gd:Nb:Ce:F was 1.168:0.755:0.005:0.01:0.005:0.447. 1.168 Mn 0.755 Gd 0.005 Nb 0.01 Ce 0.005 O1.553 F 0.447 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement to analyze its crystal structure, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0063] And Li 1.168 Mn 0.755 Gd 0.005 Nb 0.01 Ce 0.005 O 1.553 F 0.447 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0064] Example 10: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), gallium oxide (Ga 2 O 3 ), niobium oxide (Nb 2 O 5 ), cerium oxide (CeO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Ga:Nb:Ce:F was 1.175:0.76:0.005:0.005:0.005:0.45. 1.175 Mn 0.76 Ga 0.005 Nb 0.005 Ce 0.005 O 1.55 F 0.45 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement to analyze its crystal structure, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0065] And Li 1.175 Mn 0.76 Ga 0.005 Nb 0.005 Ce 0.005 O 1.55 F 0.45 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0066] Example 11: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), gallium oxide (Ga 2 O 3 ), niobium oxide (Nb 2 O 5 ), cerium oxide (CeO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Ga:Nb:Ce:F was 1.2:0.685:0.005:0.005:0.005:0.5 was weighed out. The same procedure as in Example 1 was carried out to obtain Li, 1.2 Mn 0.685 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement to analyze its crystal structure, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0067] And Li 1.2 Mn 0.685 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0068] Example 12: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), magnesium oxide (MgO), gallium oxide (Ga 2 O 3 ), cerium oxide (CeO 2) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Ga:Ce:F was 1.175:0.7:0.025:0.025:0.025:0.45. The same procedure as in Example 1 was carried out to obtain Li, 1.175 Mn 0.7 Mg 0.025 Ga 0.025 Ce 0.025 O 1.55 F 0.45 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement to analyze its crystal structure, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0069] And Li 1.175 Mn 0.7 Mg 0.025 Ga 0.025 Ce 0.025 O 1.55 F 0.45 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0070] Example 13: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), magnesium oxide (MgO), gadolinium oxide (Gd 2 O 3 ), niobium oxide (Nb 2 O 5 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Gd:Nb:F was 1.143:0.775:0.01:0.005:0.01:0.447. 1.143 Mn 0.775 Mg 0.01 Gd 0.005 Nb 0.01 O 1.553 F 0.447The composite oxide thus obtained was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 5. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0071] And Li 1.143 Mn 0.775 Mg 0.01 Gd 0.005 Nb 0.01 O 1.553 F 0.447 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0072] Example 14: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), gallium oxide (Ga 2 O 3 ), niobium oxide (Nb 2 O 5 ), cerium oxide (CeO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Ga:Nb:Ce:F was 1.213:0.703:0.01:0.01:0.005:0.545. 1.213 Mn 0.703 Ga 0.01 Nb 0.01 Ce 0.005 O 1.455 F 0.545 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 6. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0073] And Li 1.213 Mn 0.703 Ga 0.01 Nb 0.01 Ce 0.005 O 1.455 F 0.545 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0074] Example 15: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), potassium superoxide (KO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:K:F was 1.075:0.7:0.025:0.7. 1.075 Mn 0.7 K 0.025 O 1.3 F 0.7 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 7. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0075] And Li 1.075 Mn 0.7 K 0.025 O 1.3 F 0.7 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0076] Example 16: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), silver oxide (Ag 2 The same procedure as in Example 1 was carried out to obtain Li, Mn, Ag, and F, except that the starting material for the composite oxide was Li, Mn, Ag, and F, and the molar ratio of Li:Mn:Ag:F was 1.15:0.725:0.025:0.65. 1.15 Mn 0.725 Ag 0.025 O 1.35 F 0.65 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement to analyze its crystal structure, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0077] And Li 1.15 Mn 0.725 Ag 0.025 O 1.35 F 0.65 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0078] Example 17: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), silver oxide (Ag 2 The same procedure as in Example 1 was carried out to obtain Li, Mn, Ag, and F, except that the starting material for the composite oxide was Li, Mn, Ag, and F, and the molar ratio of Li, Mn, Ag, and F was 1.1:0.75:0.1:0.5. 1.1 Mn 0.75 Ag 0.1 O 1.5 F 0.5 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 8. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0079] And Li 1.1 Mn 0.75 Ag 0.1 O 1.5 F 0.5 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0080] Comparative Example 1: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), magnesium oxide (MgO), gadolinium oxide (Gd 2 O 3 ), niobium oxide (Nb 2 O 5) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Gd:Nb:F was 1.192:0.73:0.005:0.005:0.01:0.298. 1.192 Mn 0.73 Mg 0.005 Gd 0.005 Nb 0.01 O 1.702 F 0.298 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 9. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0081] And Li 1.192 Mn 0.73 Mg 0.005 Gd 0.005 Nb 0.01 O 1.702 F 0.298 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0082] Comparative Example 2: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), magnesium oxide (MgO), cerium oxide (CeO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Ce:F was 1.225:0.625:0.025:0.025:0.5 was weighed out. The same procedure as in Example 1 was carried out to obtain Li, 1.225 Mn 0.625 Mg 0.025 Ce 0.025 O 1.5 F 0.5 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 10. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0083] And Li 1.225 Mn 0.625Mg 0.025 Ce 0.025 O 1.5 F 0.5 A half cell was fabricated in the same manner as in Example 1 using a composite oxide represented by the formula:

[0084] Comparative Example 3: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), gallium oxide (Ga 2 O 3 ), niobium oxide (Nb 2 O 5 ), cerium oxide (CeO 2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Ga:Nb:Ce:F was 1.25:0.485:0.005:0.005:0.005:0.5 was weighed out. The same procedure as in Example 1 was carried out to obtain Li, 1.25 Mn 0.485 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 The composite oxide thus obtained was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 11. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0085] And Li 1.25 Mn 0.485 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0086] Comparative Example 4: Lithium fluoride (LiF), lithium manganese oxide (LiMnO 2 ), manganese(III) oxide (Mn 2 O 3 ), lithium peroxide (Li 2 O 2 ), magnesium oxide (MgO), cerium oxide (CeO2 ) was used as a starting source of the composite oxide, and the molar ratio of Li:Mn:Mg:Ce:F was 1.25:0.45:0.025:0.025:0.5. The same procedure as in Example 1 was carried out to obtain Li, 1.25 Mn 0.45 Mg 0.025 Ce 0.025 O 1.5 F 0.5 A composite oxide represented by the formula (1) was obtained. The obtained composite oxide was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 12. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m.

[0087] And Li 1.25 Mn 0.45 Mg 0.025 Ce 0.025 O 1.5 F 0.5 A test cell was prepared in the same manner as in Example 1 using a composite oxide represented by the formula:

[0088] [dV / dq-SOC curve] The half-cells of each example and comparative example were charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.95 V. During this charging, the SOC and dV / dq of the half-cell were calculated at predetermined time intervals to obtain dV / dq-SOC curves. The results are shown in Figures 13 to 16.

[0089] 13, the dV / dq-SOC curves of the half-cells of Examples 1 and 2 had one peak in the range of SOC 40% or more and 70% or less, while the dV / dq-SOC curves of the half-cells of Comparative Examples 1 and 2 had one peak in the range of SOC 10% or more and less than 40%.

[0090] As shown in FIG. 14, in the half-cells of Examples 4, 5, 6 and 8, the dV / dq-SOC curves had two peaks in the range of SOC 40% or more and 70% or less.

[0091] As shown in FIG. 15, in the half-cells of Examples 10, 13 and 14, the dV / dq-SOC curves had two peaks in the range of SOC 40% or more and 70% or less.

[0092] As shown in FIG. 16, in the half-cells of Examples 15, 16 and 17, the dV / dq-SOC curves had one peak in the range of SOC 40% or more and 70% or less.

[0093] It was confirmed that the dV / dq-SOC curves of the half-cells of Examples 3, 7, 9, 11, and 12 had one or more peaks in the range of SOC 40% or more and 70% or less. It was also confirmed that the dV / dq-SOC curves of the half-cells of Comparative Examples 3 and 4 had one peak in the range of SOC 10% or more and less than 40%.

[0094] [Charge / Discharge Test 1] The half-cells of each Example and Comparative Example were charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.95 V, and then charged at a constant voltage until the current value reached 0.05 C at 4.95 V. Thereafter, constant current discharge was performed at a constant current of 0.1 C until the end voltage (battery voltage) reached 2.5 V. The discharge voltage was calculated by dividing the total amount of power consumed during discharge by the total current.

[0095] Table 1 shows the composition of the composite oxides of each example and each comparative example, x TM tm M y O 2-f F f tm, f, Q (= 2 × tm × {1-(1-f / 2)} 5}) and the discharge voltage results are summarized.

[0096]

[0097] All of Examples 1 to 17 showed higher discharge voltages than Comparative Examples 1 to 4. From these results, it was found that the lithium ion batteries had a crystal structure belonging to the space group Fm-3m and had the general formula: Li x TM tm M y O 2-f F f In the general formula, TM is a transition metal, M is a non-transition metal, and Q=2×tm×{1−(1−f / 2) 5}, it can be said that a high discharge voltage can be obtained by using a composite oxide that satisfies Q≧1 and gives one or more peaks in the range of SOC 40% or more and 70% or less in the dV / dq-SOC curve, which is the relationship between dV / dq and SOC of a half cell.

[0098] Example 18 The half-cell of Example 1 was charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. During this charging, the SOC and dV / dq of the half-cell were calculated at predetermined time intervals to obtain a dV / dq-SOC curve.

[0099] Example 19 The half-cell of Example 2 was charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. During this charging, the SOC and dV / dq of the half-cell were calculated at predetermined time intervals to obtain a dV / dq-SOC curve.

[0100] Example 20 The half-cell of Example 7 was charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. During this charging, the SOC and dV / dq of the half-cell were calculated at predetermined time intervals to obtain a dV / dq-SOC curve.

[0101] Example 21 The half-cell of Example 9 was charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. During this charging, the SOC and dV / dq of the half-cell were calculated at predetermined time intervals to obtain a dV / dq-SOC curve.

[0102] Example 22 The half-cell of Example 11 was charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. During this charging, the SOC and dV / dq of the half-cell were calculated at predetermined time intervals to obtain a dV / dq-SOC curve.

[0103] Example 23 The half-cell of Example 16 was charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. During this charging, the SOC and dV / dq of the half-cell were calculated at predetermined time intervals to obtain a dV / dq-SOC curve.

[0104] Comparative Example 5 The half-cell of Comparative Example 2 was charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. During this charging, the SOC and dV / dq of the half-cell were calculated at predetermined time intervals to obtain a dV / dq-SOC curve.

[0105] Comparative Example 6 The half-cell of Comparative Example 3 was charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. During this charging, the SOC and dV / dq of the half-cell were calculated at predetermined time intervals to obtain a dV / dq-SOC curve.

[0106] When the dV / dq-SOC curves of Examples 18 to 23 and Comparative Examples 5 and 6 were examined, the dV / dq-SOC curves of the half-cells of Examples 18 to 23 had one or more peaks in the range of SOC 40% or more and 70% or less. On the other hand, the dV / dq-SOC curves of the half-cells of Comparative Examples 5 and 6 had one or more peaks in the range of SOC 10% or more and less than 40%.

[0107] [Charge / Discharge Test 2] The half-cells of Examples 18 to 23 and Comparative Examples 5 and 6 were charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. Thereafter, they were discharged at a constant current of 0.1 C until the end voltage (battery voltage) reached 3.0 V. The discharge capacity D1 (mAh / g) after the constant current discharge was determined.

[0108] [Charge / Discharge Test 3] The half-cells of Examples 18 to 23 and Comparative Examples 5 and 6 were charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. Thereafter, they were discharged at a constant current of 0.1 C until the end voltage (battery voltage) reached 2.5 V. The discharge capacity D2 (mAh / g) after the constant current discharge was determined.

[0109] [Charge / Discharge Test 4] The half-cells of Examples 18 to 23 and Comparative Examples 5 and 6 were charged at a constant current of 0.1 C in a temperature environment of 25° C. until the end voltage (battery voltage) reached 4.7 V. Thereafter, they were discharged at a constant current of 0.1 C until the end voltage (battery voltage) reached 1.5 V. The total amount of power during discharge was divided by the total current to obtain the discharge voltage V2.

[0110] Table 2 shows the compositions of the composite oxides of Examples 18 to 23 and Comparative Examples 5 and 6, and the compositions (Li x TM tm M y O 2-f F f tm, f, Q (= 2 × tm × {1-(1-f / 2)} 5}), and the results of the discharge capacity D1, the discharge capacity D2 and the discharge voltage V2 are summarized.

[0111]

[0112] All of Examples 18 to 23 exhibited higher discharge voltages than Comparative Examples 5 and 6. Furthermore, the discharge capacities D1 of Examples 18 to 23 exceeded 100 mAh / g, and the discharge capacities D2 exceeded 200 mAh / g, demonstrating not only high discharge voltages but also high discharge capacities. These results indicate that the lithium ion batteries have a crystal structure belonging to the space group Fm-3m and have the general formula: Li x TM tm M y O 2-f F f In the general formula, TM is a transition metal, M is a non-transition metal, and Q=2×tm×{1−(1−f / 2) 5}, it can be said that a high discharge voltage can be obtained by using a composite oxide that satisfies Q≧1 and gives one or more peaks in the range of SOC 40% or more and 70% or less in the dV / dq-SOC curve, which is the relationship between dV / dq and SOC of a half cell.

[0113] 10 Non-aqueous electrolyte secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 15 Battery case, 16 Case body, 17 Sealing body, 18, 19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Protruding portion, 23 Filter, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket.

Claims

1. It has a crystal structure belonging to the space group Fm-3m and has the general formula: Li x T.M. tm M y O 2-f F f In the general formula, TM is a transition metal, M is a non-transition metal, and Q=2×tm×{1−(1−f / 2) 5}, Q≧1 is satisfied, When the composite oxide is made into a half-cell by the following method, the half-cell is charged at 25° C. with a charging current of 0.1 C to an end voltage range of 4.7 to 4.95 V, and a dV / dq-SOC curve showing the relationship between dV / dq, which is a ratio of a change in voltage V of the half-cell to a change in battery capacity q of the half-cell, and dq, and the charging rate SOC of the half-cell, has one or more peaks in a range of SOC 40% or more and 70% or less. (Method: The composite oxide, acetylene black, and polyvinylidene fluoride are mixed in a mass ratio of 7:2:1, and dispersed using N-methyl-2-pyrrolidone to prepare a slurry for the positive electrode composite layer. This slurry for the positive electrode composite layer is applied to an aluminum foil, dried, and then rolled to a film thickness in the range of 20 to 50 μm. The mixture is then punched out to a size of 20 mm × 20 mm to obtain a positive electrode. The electrode assembly, in which a separator is interposed between this positive electrode and a metallic lithium foil (thickness 0.3 mm) as a negative electrode, is housed in an exterior body of an aluminum laminate film, and LiPF is dissolved in a mixed solvent (volume ratio 1:3) of fluoroethylene carbonate and methyl propionate. 6 A non-aqueous electrolyte having a concentration of 1 mol / L is poured into the exterior body and sealed to prepare a half cell.

2. 2. The positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, wherein the half-cell is charged at a constant current of 0.1 C at 25° C. to a cut-off voltage in the range of 4.7 to 4.95 V, and then charged at a constant voltage of 0.05 C at the cut-off voltage, and then discharged at a discharge current of 0.1 C to a cut-off voltage of 3.0 to 3.5 V, and the discharge capacity is 100 mAh / g or more.

3. The positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, wherein the half-cell is charged at a constant current of 0.1 C at 25° C. to a cut-off voltage in the range of 4.7 to 4.95 V, and then charged at a constant voltage of 0.05 C at the cut-off voltage, and then discharged at a discharge current of 0.1 C to a cut-off voltage of 2.5 to 3.0 V, and the discharge capacity is 200 mAh / g or more.

4. 3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein in the general formula, x, tm, y, and f satisfy 1.75≦x+tm+y≦2 and 0<f≦0.

7.

5. 3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein in the general formula, x, tm, y, and f satisfy 1.0<x≦1.4, 0.4≦tm<1.0, 0≦y≦0.2, and 0.25≦f≦0.

6.

6. The composite oxide contains Mn as the transition metal (TM), 3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein in the general formula, a molar ratio tm_Mn of Mn in tm satisfies 0.6<tm_Mn<0.

8.