Positive electrode and rechargeable lithium batteries including the same

A positive electrode with a lithium iron phosphate-based and lithium nickel-based composite oxide mixture addresses the issue of poor high-temperature performance in lithium secondary batteries by maintaining porosity and density, enhancing safety and capacity.

KR1020260163264APending Publication Date: 2026-11-16SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020250059339
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-07
Publication Date
2026-11-16

AI Technical Summary

Technical Problem

Lithium iron phosphate-based compounds in positive electrodes of lithium secondary batteries achieve high capacity but result in poor performance at high temperatures due to decreased porosity and pore size, compromising safety and stability.

Method used

A positive electrode design incorporating a mixture of lithium iron phosphate-based and lithium nickel-based composite oxides with a density of 2.5 g/cc and porosity of 22% or more, enhancing thermal stability and safety while maintaining high capacity.

Benefits of technology

The design ensures high safety and capacity retention at high temperatures, improving battery performance and lifespan characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PAT00001_ABST
    Figure PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode and a lithium secondary battery including the same, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material layer located on the positive electrode current collector, and the positive electrode active material layer comprises a first positive electrode active material containing a lithium iron phosphate-based compound and a second positive electrode active material containing a lithium nickel-based composite oxide, and the density of the positive electrode active material layer is 2.5 g / cc or more and the porosity is 22% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] This relates to a positive electrode and a lithium secondary battery containing the same. Background Technology

[0002] Lithium-ion batteries are widely used as power sources for mobile information terminals such as smartphones and laptops because they offer high combined energy density and portability. Recently, active research is being conducted on lithium-ion batteries with high safety and high capacity for use as power sources for hybrid or electric vehicles, or for power storage.

[0003] Recently, there has been a demand for lithium secondary batteries capable of securing rapid charging characteristics while ensuring high capacity and high safety, leading to the proposal of low-cost lithium iron phosphate-based compounds as cathode active materials. These lithium iron phosphate-based compounds possess a stable structure and excellent thermal stability.

[0004] Assuming that a lithium iron phosphate-based compound is used as the positive electrode active material, high capacity can be secured by increasing the density of the positive electrode active material layer. However, as the density of the positive electrode active material layer increases, the positive electrode active material becomes more densely located, and the porosity and pore size of the positive electrode decrease, which may result in poor battery performance at high temperatures.

[0005] Accordingly, in order to ensure high safety, a design for a cathode plate is required that uses a lithium iron phosphate-based compound as the cathode active material while ensuring performance at high capacity and high temperatures. The problem to be solved

[0006] One embodiment is intended to provide a positive electrode and a lithium secondary battery capable of securing high safety and high capacity while ensuring stable and excellent battery characteristics at high temperatures. means of solving the problem

[0007] In one embodiment, the positive current collector; and a positive active material layer located on the positive current collector, wherein the positive active material layer comprises a first positive active material containing a lithium iron phosphate-based compound and a second positive active material containing a lithium nickel-based composite oxide, and the density of the positive active material layer is 2.5 g / cc or more and the porosity is 22% or more.

[0008] In another embodiment, a lithium arch battery comprising the anode, cathode, and electrolyte is provided. Effects of the invention

[0009] The anode according to one embodiment can secure high safety and high capacity, while also ensuring stable and excellent battery characteristics even at high temperatures. Brief explanation of the drawing

[0010] FIG. 1 is a schematic perspective view showing a portion of a cylindrical lithium secondary battery cut off. Figure 2 is a cross-sectional view schematically illustrating a prismatic lithium secondary battery. Figures 3 and 4 are schematic exploded perspective views of a pouch-type lithium secondary battery. Specific details for implementing the invention

[0011] Specific embodiments are described below in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0012] The terms used herein are for describing exemplary embodiments only and are not intended to limit the invention. Singular expressions include plural expressions unless the context clearly indicates otherwise.

[0013] Here, "combinations of these" refers to mixtures of components, laminates, composites, copolymers, alloys, blends, reaction products, etc.

[0014] The terms "include," "equip," or "have" used herein are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should be understood as not excluding in advance the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0015] In the drawings, thicknesses have been enlarged to clearly represent various layers and regions, and the same reference numerals have been used for similar parts throughout the specification. When a part such as a layer, film, region, or plate is described as being "on" or "on" another part, this includes not only cases where it is "immediately on" another part, but also cases where there is another part in between. Conversely, when a part is described as being "immediately on" another part, it means that there is no other part in between.

[0016] In addition, the term "layer" here includes not only the shape formed on the entire surface when viewed in a plan view, but also the shape formed on some surfaces.

[0017] The average particle size can be measured by methods widely known to those skilled in the art, for example, by measuring with a particle size analyzer, or by using transmission electron microscope or scanning electron microscope images. Alternatively, the average particle size value can be obtained by measuring using dynamic light scattering, performing data analysis to count the number of particles for each particle size range, and then calculating from this. Unless otherwise defined, the average particle size is the diameter (D) of the particle at which the cumulative volume in the particle size distribution is 50 volume percent. 50 It may mean ). In addition, unless otherwise defined, the average particle size is obtained by measuring the size (diameter or length of the major axis) of approximately 20 randomly selected particles from scanning electron microscope images to obtain a particle size distribution, and the diameter (D) of the particle with a cumulative volume of 50% in the said particle size distribution. 50It may be that ) was taken as the average particle size.

[0018] Here, "or" is not interpreted in an exclusive sense; for example, "A or B" is interpreted to include A, B, A+B, etc.

[0019] The term "metal" is interpreted as a concept that includes ordinary metals, transition metals, and metalloids (semimetals).

[0020] anode

[0021] In one embodiment, a positive electrode is provided comprising: a positive current collector; and a positive active material layer located on the positive current collector, wherein the positive active material layer comprises a first positive active material containing a lithium iron phosphate-based compound and a second positive active material containing a lithium nickel-based composite oxide, and wherein the density of the positive active material layer is 2.5 g / cc or more and the porosity is 22% or more.

[0022] The above-mentioned cathode uses a mixture of a lithium iron phosphate-based compound and a lithium nickel-based composite oxide as the cathode active material, and by controlling the density and porosity within an appropriate range, it is possible to increase capacity while ensuring safety and improve lifespan and capacity retention rate at high temperatures.

[0023] positive active material layer

[0024] According to one embodiment, the positive active material layer is positioned on a positive current collector and comprises a positive active material, wherein the positive active material comprises a first positive active material containing a lithium iron phosphate-based compound and a second positive active material containing a lithium nickel-based composite oxide, and the density of the positive active material layer is 2.5 g / cc or more and the porosity is 22% or more.

[0025] (1st positive active material)

[0026] A first positive electrode active material according to one embodiment contains a lithium iron phosphate-based compound. The lithium iron phosphate-based compound can improve heat resistance and thermal stability, while also increasing capacity or output. Specifically, the lithium iron phosphate-based compound may be represented by the following chemical formula 1 or chemical formula 2.

[0027] [Chemical Formula 1]

[0028] Li a1 Fe (1-x1) M 1 x1 PO4

[0029] In Chemical Formula 1, 0.90≤a1≤1.5, 0≤x1≤0.4, and M 1 ... may be one or more of Al, B, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr. Here, 0.90 ≤ a1 ≤ 1.5 may be, for example, 0.90 ≤ a1 ≤ 1.2, or 0.95 ≤ a1 ≤ 1.1. Also, 0 ≤ x1 ≤ 0.4, 0 ≤ x1 ≤ 0.3, 0 ≤ x1 ≤ 0.2, 0 ≤ x1 ≤ 0.1, or 0 ≤ x1 ≤ 0.05.

[0030] [Chemical Formula 2]

[0031] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4

[0032] In Chemical Formula 2, 0.90≤a2≤1.5, 0.1≤x2≤0.9, 0≤y2≤0.9, 0.1≤x2+y2<1, and M 2... may be one or more of Al, B, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr. Here, 0.90 ≤ a2 ≤ 1.5 may be, for example, 0.90 ≤ a2 ≤ 1.2, or 0.95 ≤ a2 ≤ 1.1. Also, 0.1 ≤ x2 ≤ 0.9, 0.3 ≤ x2 ≤ 0.9, or 0.4 ≤ x2 ≤ 0.8, and 0 ≤ y2 ≤ 0.4, 0 ≤ y2 ≤ 0.3, 0 ≤ y2 ≤ 0.2, 0 ≤ y2 ≤ 0.1, or 0 ≤ y2 ≤ 0.05.

[0033] More specifically, the lithium iron phosphate-based compound is LiFePO4, LiMn 0.7 Fe 0.3 PO4, LiMn 0.6 Fe 0.4 PO4, LiMn 0.5 Fe 0.5 PO4, LiMn 0.4 Fe 0.6 PO4 and LiMn 0.3 Fe 0.7 It may contain one or more compounds of PO4.

[0034] The above lithium iron phosphate-based compound may further include one or more elements selected from Al, Mg, Mn, Ti, and V, in which case life characteristics may be improved. Additionally, the above lithium iron phosphate-based compound may further include one or more elements selected from Al, Mg, Ti, and V as a type of doping element, and one or more of the elements selected from Al, Mg, Ti, and V may be included in an amount of 0.1 mol% to 0.5 mol% based on 100 mol% of the total metal excluding lithium in the above lithium iron phosphate-based compound, in which case rate characteristics and life characteristics may be improved. As an example, the above lithium iron phosphate-based compound includes Ti as a doping element, and the content of Ti may satisfy 0.1 mol% to 0.5 mol% based on 100 mol% of the total metal excluding lithium. In this case, rate characteristics and life characteristics may be improved.

[0035] For example, M of the above chemical formula 1 1 and M of Chemical Formula 2 2 It may contain one or more elements among Al, Mg, Ti, and V, and in this case, the lifespan characteristics of the lithium iron phosphate-based cathode active material can be improved. For example, in Chemical Formula 1, 0.001≤x1≤0.005 or 0.001≤x1≤0.003 may be used, and in Chemical Formula 2, 0.001≤x2≤0.005 or 0.001≤x2≤0.003 may be used, and in this case, the lifespan characteristics of the lithium iron phosphate-based cathode active material can be improved.

[0036] In one embodiment, the first positive electrode active material containing the lithium iron phosphate-based compound may be in the form of a first particle, a second particle, or a mixture of the first particle and the second particle.

[0037] The first particle may be an assembly formed by the aggregation of multiple primary particles or a secondary particle. The first particle may have a spherical or elliptical shape as the primary particles are closely aggregated with each other. The average particle size (D) of the first particle 50 ) may be, for example, 6 μm to 25 μm, 7 μm to 20 μm, or 8 μm to 15 μm. The average particle size of the first particle may be larger than the average particle size of the second particle described later. The average particle size of the primary particles forming the assembly of the first particle may be, for example, 10 nm to 400 nm, 20 nm to 300 nm, or 50 nm to 200 nm. The average particle size of the first particle (D 50 ) may, for example, be obtained by randomly selecting about 30 first particles from electron microscope images of lithium transition metal phosphate, measuring their particle sizes, and taking the diameter of the particle with a cumulative volume of 50% of the particle size distribution as the average particle size. The average particle size of the first particles (D 50) may be the average particle size obtained by measuring the size of about 30 primary particles in an electron microscope image of the surface or cross-section of the first particle and taking the diameter of the particle with a cumulative volume of 50% of the particle size distribution as the average particle size.

[0038] The porosity of the first particle may be about 20% to about 50%. For example, the porosity may be the ratio of the area occupied by the voids within the particle using an image analysis program such as Image J in a scanning electron microscope image of a cross-section of the first particle.

[0039] The second particle may have a single particle form. The average particle size (D) of the second particle 50 ) may be 2 μm or less, for example, 0.1 μm to 2 μm, 0.5 μm to 2 μm, 0.5 μm to 1.5 μm, 0.6 μm to 1.2 μm, or 0.8 μm to 1.0 μm. The average particle size of the second particle may be smaller than the average particle size of the first particle, and may be equal to or larger than the average particle size of the primary particles of the first particle. The average particle size of the second particle (D 50 As an example, ) may be obtained by randomly selecting about 30 second particles from an electron microscope image of a lithium iron phosphate-based compound, measuring their particle sizes, and taking the diameter of the particle with a cumulative volume of 50% of the particle size distribution as the average particle size.

[0040] For example, the first positive electrode active material may include both the first particle and the second particle, and in this case, based on the total sum of the first particle and the second particle of 100 weight%, it may include 10 weight% to 90 weight% of the first particle and 10 weight% to 90 weight% of the second particle, and for example, it may include 40 weight% to 60 weight% of the first particle and 40 weight% to 60 weight% of the second particle. In this case, the energy density and lifespan characteristics of the battery can be improved.

[0041] The above lithium iron phosphate-based compound may further include a carbon coating layer located on the surface of the particles. The carbon coating layer can improve the electrical conductivity of the lithium iron phosphate-based compound and lower the resistance of the anode. The carbon coating layer may be formed using one or more raw materials selected from, for example, glucose, sucrose, lactose, starch, oligosaccharides, polyoligosaccharides, fructose, cellulose, polymers of furfuryl alcohol, block copolymers of ethylene and ethylene oxide, vinyl resins, cellulose resins, phenolic resins, pitch resins, and tar resins. Specifically, the carbon coating layer may be formed by placing the raw materials on the surface of the lithium iron phosphate-based compound particles and then performing a calcination process.

[0042] For example, the first positive active material may include a first particle in the form of a secondary particle, and the first positive active material may further include a carbon coating layer located on the surface of the secondary particle and / or on the surface of the primary particles constituting the secondary particle. Additionally, the first positive active material may include a second particle in the form of a single particle, and may further include a carbon coating layer located on the surface of the single particle.

[0043] (Second positive active material)

[0044] A second positive electrode active material according to one embodiment contains a lithium nickel-based composite oxide. By including the lithium nickel-based composite oxide, the positive electrode maintains the heat resistance and thermal stability characteristics of a lithium iron phosphate compound, while simultaneously increasing capacity and enabling operation at high voltage. Specifically, the lithium nickel-based composite oxide can be represented by the following chemical formula 3.

[0045] [Chemical Formula 3]

[0046] Li a3 Ni x3 M 3 y3 M 4 z3 O 2-b3 Xb3

[0047] In Chemical Formula 3, 0.9≤a3≤1.8, 0.3≤x3≤1, 0≤y3≤0.7, 0≤z3≤0.7, 0.9≤x3+y3+z3≤1.1, and 0≤b3≤0.1, and M 3 and M 4 Each is independently one or more of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more of F, P, and S.

[0048] In Chemical Formula 3, 0.6≤x3≤1, 0≤y3≤0.4, and 0≤z3≤0.4, or 0.8≤x3≤1, 0≤y3≤0.2, and 0≤z3≤0.2, or 0.9≤x3<1, 0 <y3≤0.1, 및 0≤z3≤0.1일 수 있다.

[0049] For example, the second positive electrode active material may be a high-nickel positive electrode active material in which, based on 100 mol% of the total metal excluding lithium in a lithium-nickel-based composite oxide, the nickel content is 80 mol% or more, 85 mol% or more, 90 mol% or more, 91 mol% or more, or 94 mol% or more and 99 mol% or less. The high-nickel positive electrode active material can achieve high capacity and can be applied to high-capacity, high-density lithium secondary batteries.

[0050] The second positive active material containing the above lithium nickel-based composite oxide has an average particle size (D 50 Large particles with a diameter of 10 µm to 25 µm, average particle size (D 50 It may include small particles having a size of 1 μm to 8 μm, or a combination thereof.

[0051] The above-mentioned allele may be in the form of a secondary particle formed by the aggregation of multiple primary particles, and the above-mentioned elementary particle may be in the form of a secondary particle, a single particle, or a combination thereof. The secondary particle and the single particle may be spherical, elliptical, polyhedron, or irregular shape, and the primary particle forming the secondary particle may be spherical, elliptical, plate-shaped, or a combination thereof.

[0052] Average particle size (D of the above alleles) 50 ) may be, for example, 10 μm to 25 μm, or 12 μm to 18 μm. The average particle size (D) of the above fine particles 50 ) can be, for example, 1 μm to 8 μm, or 2 μm to 6 μm. Here, the average particle size (D 50 ) may be obtained by measuring the size (diameter or length of the major axis) of about 20 randomly selected particles in scanning electron microscope images of positive electrode active materials to obtain a particle size distribution, and taking the diameter of the particle with a cumulative volume of 50% of the particle size distribution as the average particle size.

[0053] Based on a total sum of 100 weight% of the above-mentioned coarse particles and the above-mentioned small particles, the second positive active material may contain 40 weight% to 95 weight% of the coarse particles and 5 weight% to 60 weight% of the small particles, for example, may contain 60 weight% to 80 weight% of the coarse particles and 20 weight% to 40 weight% of the small particles.

[0054] The above positive active material layer may comprise 10% to 90% by weight of the first positive active material based on 100% by weight of the total of the first positive active material and the second positive active material, for example, 60% to 90% by weight, 70% to 90% by weight, or 80% to 90% by weight; and may comprise 10% to 90% by weight of the second positive active material based on 100% by weight of the total of the first positive active material and the second positive active material, for example, 10% to 40% by weight, 10% to 30% by weight, or 10% to 20% by weight. When the content of the first positive active material and the second positive active material falls within the above range, it is possible to increase capacity and enable operation at high voltage while ensuring safety.

[0055] The above positive active material layer may further include a binder and / or a conductive material.

[0056] The above binder serves to adhere the positive active material particles well to each other and also to adhere the positive active material well to the current collector. Representative examples of binders include, but are not limited to, polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylic resin, polyester resin, nylon, etc. The content of the above binder may be 0.1% to 5% by weight based on 100% by weight of the total positive active material layer.

[0057] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjenblack, carbon fiber, carbon nanofiber, carbon nanotube; metal-based materials in the form of metal powder or metal fibers containing copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof. The content of the above conductive material may be 0.1% to 5% by weight based on 100% by weight of the total positive electrode active material layer.

[0058] The above positive current collector is not particularly limited as long as it is conductive without causing chemical changes in the lithium secondary battery, and may be an aluminum foil with a thickness of 10 μm to 15 μm.

[0059] The above anode may be manufactured according to a conventional anode manufacturing method. For example, the above anode may be manufactured by mixing an anode active material and optionally a binder and / or a conductive material in a solvent to prepare an anode active material slurry, applying the anode active material slurry onto an anode current collector, and then drying and rolling.

[0060] The above solvent may be a solvent commonly used in the relevant technical field, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it has a viscosity that dissolves or disperses the anode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for anode manufacturing.

[0061] According to one embodiment, the cathode can secure excellent battery characteristics at high capacity and high temperature by designing the density of the cathode active material layer to be 2.5 g / cc or higher while achieving a porosity of 22% or higher in the cathode active material layer.

[0062] According to one embodiment, the density of the positive active material layer is 2.5 g / cc or higher. For example, the density of the positive active material layer may be 2.5 g / cc to 2.7 g / cc, 2.55 g / cc to 2.7 g / cc, or 2.55 g / cc to 2.65 g / cc. Within the above range, the capacity and energy composite density of the battery can be improved, and at the same time, rapid charging characteristics can be improved by satisfying the porosity and pore size of the positive electrode as described above. The density of the positive active material layer refers to the ratio of weight to volume of the positive active material layer in the rolled positive electrode. The density of the positive active material layer can be measured by measuring the thickness and weight of the positive active material layer excluding the positive current collector, and dividing the weight by the thickness.

[0063] In one embodiment, excellent battery characteristics at high capacity and high temperature can be secured by appropriately controlling not only the density but also the porosity of the positive active material layer. The porosity of the positive active material layer is 22% or more. For example, the porosity of the positive active material layer is 22% to 50%, 22% to 45%, or 22% to 40%, 22% to 30%, or 22% to 27%. Within this range, degradation in a high-temperature environment can be suppressed and battery performance can be stabilized. The porosity of the positive active material layer can be measured by mercury intrusion. The porosity of the positive can be adjusted to a range of 22% or more by appropriately controlling the particle size and physical properties of the positive active material, the formation conditions and drying conditions of the positive active material layer, and the rolling conditions of the positive.

[0064] The mercury intrusion method utilizes the unique property of mercury not to wet solids to intrude mercury into the pores of a sample by applying external pressure. Based on the amount of intrusion, the total pore volume, pore size and distribution, and pore surface area can be determined using a mercury porosimeter. Mercury only intrudes when external pressure is applied, and higher pressure is required as the pore size decreases. The measurement results can be expressed as a function of the cumulative volume of intruded mercury depending on the pressure or pore size. For example, if a sample is placed in the capillary tube of the meter, sealed, and vacuumed, then filled with mercury, and pressure is applied, the mercury intrudes into the pores of the sample, causing the mercury height in the capillary tube to decrease, and the pore volume or pore size can be calculated using the Washburn equation.

[0065] The interface resistance of the above anode is 0.025 Ωcm 2 It may be less than, for example, 0.02 Ωcm 2 to 0.025 Ωcm 2 , or 0.023 Ωcm 2 to 0.025 Ωcm 2 It can be. Here, the interface resistance of the anode may refer to the resistance at the anode surface, for example, the contact resistance between the anode current collector and the anode active material layer.

[0066] The interface resistance of the anode can be measured using a Multi-probe resistmeter (Hioki, RM2610). The resistance was measured by applying a constant current of 10 μA to 10 mA, for example, 100 μA, and a voltage of 5 V at 25°C through 46 probes in contact with the electrode surface, and by applying the inverse problem analysis method of the potential distribution by the finite volume method.

[0067] The anode according to one embodiment comprises the aforementioned first anode active material and second anode active material, simultaneously satisfying a density of 2.5 g / cc or more and a porosity of 22% or more, and further 0.025 Ωcm 2 The interface resistance below can be exhibited, thereby enabling significant improvements in high-temperature life characteristics and high-temperature storage characteristics while ensuring capacity characteristics and safety.

[0068] Since the density, porosity, pore size, and thickness of the active material layer may vary depending on the loading level, drying conditions, and rolling conditions of the anode active material layer, it is necessary to appropriately adjust the loading level, drying conditions, and rolling conditions of the anode active material layer.

[0069] The loading level of the positive active material layer per one area of ​​the positive current collector is not particularly limited, but, for example, 20 mg / cm² 2 to 50 mg / cm² 2 It may be. The loading level of the positive active material layer per one area of ​​the positive current collector is 25 mg / cm². 2 to 45 mg / cm² 2 , 30 mg / cm 2 to 40 mg / cm² 2 or 35 mg / cm² 2 to 40 mg / cm² 2 It could be.

[0070] The above drying can be performed at a temperature of 100 ℃ to 180 ℃. The above drying can be carried out under a constant temperature state or by sequentially increasing the temperature. When the above drying is carried out by sequentially increasing the temperature, the drying can be divided into 2 to 4 stages. In one embodiment, the drying can be carried out in 4 stages, and the drying temperature for each stage may be 138 ℃, 142 ℃, 145 ℃, and 150 ℃, but is not limited thereto.

[0071] The above rolling can be performed using a rolling roll at a temperature of 20°C to 25°C. The temperature of the rolling roll can be appropriately adjusted according to the purpose.

[0072] The thickness of the positive active material layer may be 145 μm to 200 μm. Specifically, the thickness of the positive active material layer may be 147 μm to 198 μm, 150 μm to 198 μm, or 155 μm to 195 μm.

[0073] The thickness of the positive active material layer refers to the thickness of the positive active material layer excluding the positive current collector, and can be measured through SEM images of the cross-section of the rolled positive. If the thickness of the positive active material layer satisfies the above range, the capacity and energy composite density can be improved, and at the same time, rapid charging characteristics can be improved by adjusting the pore size and porosity within the positive electrode as described above.

[0074] lithium secondary battery

[0075] In one embodiment, a lithium secondary battery comprising the aforementioned positive electrode, negative electrode, and electrolyte is provided. As an example, the lithium secondary battery may include a positive electrode, a negative electrode, a separator located between the positive electrode and the negative electrode, and an electrolyte.

[0076] FIGS. 1 to 4 are schematic diagrams illustrating lithium secondary batteries according to one embodiment, wherein FIG. 1 is a cylindrical battery, FIG. 2 is a prismatic battery, and FIGS. 3 and 4 are pouch-type batteries. Specifically, FIG. 1 is a schematic perspective view showing a portion of a cylindrical lithium secondary battery cut off, FIG. 2 is a cross-sectional view schematically illustrating a prismatic lithium secondary battery, and FIGS. 3 and 4 are schematic exploded perspective views of a pouch-type lithium secondary battery.

[0077] Referring to FIGS. 1 to 4, a lithium secondary battery (100) may include an electrode assembly (40) having a separator (30) interposed between a positive electrode (10) and a negative electrode (20), and a case (50) in which the electrode assembly (40) is housed. The positive electrode (10), the negative electrode (20), and the separator (30) may be impregnated with an electrolyte (not shown). As shown in FIG. 1, the lithium secondary battery (100) may include a sealing member (60) that seals the case (50). Also, in FIG. 2, the lithium secondary battery (100) may include a positive lead tab (11), a positive terminal (12), a negative lead tab (21), and a negative terminal (22). As shown in FIGS. 3 and 4, the lithium secondary battery (100) may include electrode tabs (70), namely a positive electrode tab (71) and a negative electrode tab (72), which serve as electrical pathways for inducing current formed in the electrode assembly (40) to the outside. The lithium secondary battery may be classified into cylindrical, prismatic, pouch, coin, etc., depending on its shape.

[0078] A lithium secondary battery according to one embodiment may be capable of being charged at high voltage or suitable for being operated at high voltage, and may be a battery with improved characteristics under high voltage conditions.

[0079] A lithium secondary battery according to one embodiment is designed to operate in a high voltage range, so charging can be performed in a voltage range of 4.0 V or higher with an upper charging limit voltage. By applying a positive electrode active material and a conductive material according to one embodiment, the lithium secondary battery can achieve high capacity and long lifespan characteristics even when charged at high voltage.

[0080] cathode

[0081] The cathode may include a current collector and a cathode active material layer located on the current collector, and the cathode active material layer may include a cathode active material and may further include a binder, a conductive material, or a combination thereof.

[0082] cathode active material

[0083] The negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.

[0084] A material capable of reversibly intercalating / deintercalating the above lithium ions may include a carbon-based negative electrode active material, for example, crystalline carbon, amorphous carbon, or a combination thereof. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.

[0085] As the above lithium metal alloy, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn may be used.

[0086] As a material capable of doping and undoping the above lithium, a Si-based negative electrode active material or a Sn-based negative electrode active material may be used. The above Si-based negative electrode active material may include silicon, silicon-carbon composites, and SiOx(0 <x≤2), Si-Q 합금(상기 Q는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소(Si를 제외함), 15족 원소, 16족 원소, 전이금속, 희토류 원소 및 이들의 조합에서 선택되는 원소이며, 예컨대 Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, 및 이들의 조합에서 선택됨), 또는 이들의 조합일 수 있다. 상기 Sn계 음극 활물질로는 Sn, SnO2, Sn 합금 또는 이들의 조합일 수 있다.

[0087] The above silicon-carbon composite may be a composite of silicon and amorphous carbon. The average particle size (D) of the silicon-carbon composite particles 50 The thickness may be, for example, 0.5 μm to 20 μm. According to one embodiment, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on the surface of the silicon particles. For example, it may include a secondary particle (core) assembled from silicon primary particles and an amorphous carbon coating layer (shell) located on the surface of the secondary particle. The amorphous carbon may also be located between the silicon primary particles, so that, for example, the silicon primary particles may be coated with amorphous carbon. The secondary particles may be dispersed in an amorphous carbon matrix.

[0088] The silicon-carbon composite may further include crystalline carbon. For example, the silicon-carbon composite may include a core comprising crystalline carbon and silicon particles and an amorphous carbon coating layer located on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. Examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.

[0089] When the silicon-carbon composite comprises silicon and amorphous carbon, the silicon content may be 10% to 50% by weight with respect to 100% by weight of the silicon-carbon composite, and the amorphous carbon content may be 50% to 90% by weight. Additionally, when the composite comprises silicon, amorphous carbon, and crystalline carbon, the silicon content may be 10% to 50% by weight with respect to 100% by weight of the silicon-carbon composite, the crystalline carbon content may be 10% to 70% by weight, and the amorphous carbon content may be 20% to 40% by weight.

[0090] In addition, the thickness of the amorphous carbon coating layer may be 5 nm to 100 nm. The average particle size (D) of the silicon particles (primary particles) 50 ) can be 10 nm to 1 µm, or 10 nm to 200 nm. The silicon particles may exist as silicon alone, in the form of a silicon alloy, or in an oxidized form. The oxidized form of silicon is SiO x (0 <x≤2)로 표시될 수 있다. 이때, 산화 정도를 나타내는 Si:O의 원자 함량 비율은 99:1 내지 33:67일 수 있다. 본 명세서에서, 별도의 정의가 없는 한, 평균 입경(D 50 ) refers to the diameter of the particle with a cumulative volume of 50 volume% in the particle size distribution.

[0091] The above Si-based negative electrode active material or Sn-based negative electrode active material may be used in combination with a carbon-based negative electrode active material. When the Si-based negative electrode active material or Sn-based negative electrode active material and the carbon-based negative electrode active material are mixed and used, the mixing ratio may be 1:99 to 90:10 by weight.

[0092] bookbinder

[0093] The above binder serves to effectively bond the negative electrode active material particles to each other and also to effectively bond the negative electrode active material to the current collector. As the binder, a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof may be used.

[0094] Examples of non-aqueous binders include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide imide, polyimide, or combinations thereof.

[0095] The water-based binder may be selected from styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylenepropylenediene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.

[0096] When a water-based binder is used as the cathode binder, a cellulose-based compound capable of imparting viscosity may be further included. As this cellulose-based compound, one or more types such as carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. Na, K, or Li may be used as the alkali metal.

[0097] The dry binder is a polymer material capable of fiberization, and may be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or a combination thereof.

[0098] Challenge

[0099] A conductive material is used to impart conductivity to an electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Specific examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjenblack, carbon fiber, carbon nanofiber, and carbon nanotube; metal-based materials in the form of metal powder or metal fibers including copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.

[0100] The content of the negative electrode active material may be 95% to 99.5% by weight with respect to 100% by weight of the negative electrode active material layer, and the content of the binder may be 0.5% to 5% by weight with respect to 100% by weight of the negative electrode active material layer. For example, the negative electrode active material layer may contain 90% to 99% by weight of the negative electrode active material, 0.5% to 5% by weight of the binder, and 0.5% to 5% by weight of the conductive material.

[0101] The whole house

[0102] The negative current collector may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or alloys thereof, and may be in the form of a foil, sheet, or foam. The thickness of the negative current collector may be, for example, 1 μm to 20 μm, 5 μm to 15 μm, or 7 μm to 10 μm.

[0103] electrolytes

[0104] The electrolyte for a lithium secondary battery may be, for example, an electrolyte solution, which may include a non-aqueous organic solvent and a lithium salt.

[0105] Non-aqueous organic solvents serve as a medium through which ions involved in the electrochemical reaction of a cell can move. Non-aqueous organic solvents may be carbonate-based, ester-based, ether-based, ketone-based, or alcohol-based solvents, aprotic solvents, or a combination thereof.

[0106] Carbonate-based solvents that may be used include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Ester-based solvents that may be used include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methylpropionate, ethylpropionate, decanolide, mevalonolactone, valerolactone, caprolactone, etc. As ether-based solvents, dibutyl ether, tetraglame, diglame, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc. may be used. Additionally, as ketone-based solvents, cyclohexanone, etc. may be used. As alcohol-based solvents, ethyl alcohol, isopropyl alcohol, etc. may be used, and as aprotic solvents, nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double bond, an aromatic ring, or an ether group); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane, 1,4-dioxolane; sulfolanes, etc. may be used.

[0107] Non-aqueous organic solvents may be used alone or in a mixture of two or more types, and when two or more types are mixed, the mixing ratio can be appropriately adjusted according to the desired battery performance, which is widely understood by those working in the field.

[0108] When using a carbonate-based solvent, a mixture of cyclic carbonates and chain carbonates can be used, and the cyclic carbonates and chain carbonates can be mixed in a volume ratio of 1:1 to 1:9.

[0109] The non-aqueous organic solvent may further include an aromatic hydrocarbon-based organic solvent. For example, a carbonate-based solvent and an aromatic hydrocarbon-based organic solvent may be mixed and used in a volume ratio of 1:1 to 30:1.

[0110] The electrolyte may further include vinyl ethyl carbonate, vinylene carbonate, or ethylene carbonate-based compounds to improve battery life.

[0111] Representative examples of the above ethylene carbonate compounds include fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, and cyanoethylene carbonate.

[0112] Lithium salts are substances that dissolve in organic solvents and act as a source of lithium ions within the battery, enabling the basic operation of rechargeable lithium batteries and facilitating the movement of lithium ions between the anode and cathode. Representative examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, and LiN(C x F 2x+1 SO2)(C y F 2y+1 It may include one or more selected from SO2)(x and y are integers from 1 to 20), lithium trifluoromethane sulfonate, lithium tetrafluoroethane sulfonate, lithium difluorobis(oxalate)phosphate (LiDFOB), and lithium bis(oxalate)borate (LiBOB).

[0113] It is preferable to use a lithium salt concentration within the range of 0.1M to 2.0M. When the lithium salt concentration falls within the above range, the electrolyte has appropriate ionic conductivity and viscosity, so it can exhibit excellent performance and lithium ions can move effectively.

[0114] separator

[0115] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or multilayer films of two or more layers thereof may be used, and of course, mixed multilayer films such as polyethylene / polypropylene two-layer separators, polyethylene / polypropylene / polyethylene three-layer separators, and polypropylene / polyethylene / polypropylene three-layer separators may be used.

[0116] The above separator may include a porous substrate and a coating layer comprising an organic material, an inorganic material, or a combination thereof located on one or both sides of the porous substrate.

[0117] The porous substrate may be a polymer membrane formed from any one of the following: polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyacetal; polyamide; polyimide; polycarbonate; polyetherketone; polyaryletherketone; polyetherimide; polyamideimide; polybenzimidazole; polyethersulfone; polyphenylene oxide; cyclic olefin copolymer; polyphenylene sulfide; polyethylene naphthalate; glass fiber; Teflon; and polytetrafluoroethylene, or a copolymer or mixture of two or more of these.

[0118] The porous substrate may have a thickness of about 1 μm to 40 μm, and may have a thickness of, for example, 1 μm to 30 μm, 1 μm to 20 μm, 5 μm to 15 μm, or 10 μm to 15 μm.

[0119] The above organic material may include a (meth)acrylic copolymer comprising a first structural unit derived from (meth)acrylamide, and a second structural unit comprising at least one of a structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamideidosulfonic acid or its salt.

[0120] The above inorganic materials are Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, It may include inorganic particles selected from SrTiO3, BaTiO3, Mg(OH)2, boehmite, and combinations thereof, but is not limited thereto. The average particle size (D) of the inorganic particles 50 ) can be 1 nm to 2000 nm, for example, 100 nm to 1000 nm, or 100 nm to 700 nm.

[0121] The above organic and inorganic materials may exist mixed in a single coating layer, or may exist in a stacked form with a coating layer containing organic materials and a coating layer containing inorganic materials.

[0122] The thickness of the coating layer may be 0.5 μm to 20 μm, for example, 1 μm to 10 μm, or 1 μm to 5 μm.

[0124] Examples and comparative examples of the present invention are described below. The following examples are merely illustrative of the present invention, and the present invention is not limited to the following examples.

[0125] Example 1

[0126] 1. Manufacture of the anode

[0127] (1st positive active material)

[0128] The iron phosphate precursor Fe1PO4·H2O, lithium carbonate, magnesium dioxide, and titanium dioxide were mixed in a molar ratio of 1:1.03:0.0025:0.004. The mixture, which was a slurry, was spray-dried and evaporated under conditions of a spray pressure of 0.5 MPa and a temperature of 230°C. The dried mixture was calcined at 750°C for 10 hours under a nitrogen atmosphere to obtain first particles in the form of secondary particles. The average particle size of the first particles was 10 μm. The size of the primary particles of the first particles was 50 nm to 200 nm.

[0129] The iron phosphate precursor Fe1PO4·H2O, lithium carbonate, magnesium dioxide, and titanium dioxide were mixed in a molar ratio of 1:1.03:0.0025:0.004. A wet ball milling process was performed on the mixture. The mixture was evaporatively dried on a furnace tray and then placed in a vacuum oven at 85°C for 4 hours. The dried mixture was calcined at 650°C for 10 hours under a nitrogen atmosphere. The calcined material was ground at a rotational speed of 8,000 rpm to obtain a second particle in the form of a single particle. The average particle size of the second particle was 0.9 μm. The primary particle size of the second particle was 200 nm to 300 nm.

[0130] A first positive active material was prepared by mixing the first particle and the second particle in a mass ratio of 50:50.

[0131] (Second positive active material)

[0132] Ni 0.85 Co 0.14 Al 0.01 (OH)2 and LiOH were mixed in a molar ratio of 1:1.05 and subjected to a first heat treatment at 845 °C for 8 hours in an oxygen atmosphere, so that the composition was Li 1.05 Ni 0.85 Co 0.14 Al 0.01 O2 and average particle size (D 50A second positive electrode active material was prepared containing a lithium nickel-cobalt-aluminum-based composite oxide in the form of secondary particles with a thickness of approximately 14 μm.

[0133] Finally, based on a total of 100 weight% of the first and second positive active materials manufactured above, a positive active material was prepared by mixing 85 weight% of the first positive active material and 15 weight% of the second positive active material.

[0134] After mixing 96.3 wt% of the manufactured final cathode active material, 2.2 wt% of a polyvinylidene fluoride binder, and 1.5 wt% of a carbon nanotube conductive material, N - A positive electrode active material layer slurry was prepared by dispersing in a methylpyrrolidone solvent.

[0135] The above slurry at 49.35 mg / cm² on a 12 µm thick Al foil 2 An anode was manufactured by coating at a loading level, drying in four stages sequentially at 138 ℃, 142 ℃, 145 ℃, and 150 ℃, and then rolling. Rolling was performed using rolling rolls at a temperature of approximately 25 ℃, with the rolling line pressure controlled to approximately 0.83 ton / cm.

[0136] After rolling, the density of the positive active material layer was approximately 2.58 g / cc, the thickness of the positive active material layer was 192 μm, the porosity of the positive active material layer was 22.48%, and the interfacial resistance of the positive was 0.025 Ωcm. 2 am.

[0137] At this time, the density of the positive active material layer refers to the ratio of the weight to the volume of the positive active material layer in the rolled positive electrode. The density of the positive active material layer can be measured by measuring the thickness and weight of the positive active material layer excluding the positive current collector, and dividing the weight by the thickness.

[0138] The porosity of the positive electrode active material layer can be measured using the mercury indentation method (Mercury Poremaster 60GT, Quantachrom). The interfacial resistance of the positive electrode can be measured using a multi-probe resistmeter (Hioki, RM2610). The resistance was measured by applying a constant current of 10 μA to 10 mA, for example, 100 μA, and a voltage of 5 V at 25°C through 46 probes in contact with the electrode surface, and by applying the inverse problem analysis method of the potential distribution by the finite volume method.

[0139] 2. Manufacture of lithium secondary batteries

[0140] A negative electrode active material layer slurry was prepared by mixing 97 wt% of graphite negative electrode active material, 0.5 wt% of particulate nanocarbon, 0.8 wt% of carboxymethyl cellulose, and 1.7 wt% of styrene butadiene rubber in a water solvent. A negative electrode was prepared by coating the negative electrode active material layer slurry onto a copper foil current collector, drying, and rolling.

[0141] A lithium secondary battery was manufactured by a conventional method using a polytetrafluoroethylene separator and an electrolyte in which 1M LiPF6 was dissolved in a solvent mixed with ethylene carbonate and dimethyl carbonate in a volume ratio of 3:7.

[0142] Comparative Example 1

[0143] A cathode and a lithium secondary battery were manufactured using substantially the same method as in Example 1, except that during cathode manufacturing, the density of the cathode active material layer was changed to 2.45 g / cc, the thickness of the cathode active material layer to 200 μm, and the porosity to 25.3%. At this time, the interfacial resistance of Comparative Example 1 was 0.03 Ωcm 2 am.

[0144] Comparative Example 2

[0145] A cathode and a lithium secondary battery were manufactured using substantially the same method as in Example 1, except that during cathode manufacturing, the density of the cathode active material layer was changed to 2.62 g / cc, the thickness of the cathode active material layer to 187 μm, and the porosity to 21.17%. At this time, the interfacial resistance of Comparative Example 2 was 0.024 Ωcm 2 am.

[0146] Comparative Example 3

[0147] A cathode and a lithium secondary battery were manufactured using substantially the same method as in Example 1, except that during cathode manufacturing, the density of the cathode active material layer was changed to 2.67 g / cc, the thickness of the cathode active material layer to 183 μm, and the porosity to 20%. At this time, the interfacial resistance of Comparative Example 3 was 0.02 Ωcm 2 am.

[0148] Evaluation Example 1: High-temperature life evaluation

[0149] The lithium secondary batteries prepared in Examples and Comparative Examples 1 to 3 were charged from 2.5V to an upper limit of 4.2V at 45°C under a constant current condition of 1.5C, rested for 10 minutes, and then discharged under a 0.5C condition until they reached 3.0V to perform initial charge-discharge. Subsequently, 120 charge-discharge cycles were repeated at 45°C in the range of 3.0V to 4.2V. The process was performed using a Constant Current-Constant Voltage (CCCV) method, and the cut-off condition was set to 0.2C.

[0150] The ratio of the discharge capacity at 120 cycles to the initial discharge capacity is calculated according to Equation 1 and expressed as the high-temperature capacity retention rate in Table 1 below, and the high-temperature capacity retention rate during 120 cycles is shown in Figure 1.

[0151] <Equation 1> = Capacity Retention Rate = 100 × (Discharge Capacity after 120 cycles) / (Initial Discharge Capacity)

[0152] 120-cycle capacity retention rate (%) Example 1 94.4 Comparative Example 1 92.2 Comparative Example 2 91.8 Comparative Example 3 86.0

[0153] Referring to Table 1, it can be seen that the lithium secondary battery according to Example 1 has an improved capacity retention rate at high temperatures compared to the lithium secondary batteries according to Comparative Examples 1 to 3. When the composite density and porosity satisfy the conditions according to one embodiment, the contact characteristics of the positive electrode plate are not degraded, and the occurrence of cracks during the rolling process can be prevented. In addition, side reactions are suppressed in a high-temperature environment, so the cycle capacity retention rate of Example 1 exhibits superior performance compared to Comparative Examples 1 to 3.

[0154] Evaluation Example 2: Evaluation of High-Temperature Storage Characteristics

[0155] The lithium secondary batteries prepared in Example 1 and Comparative Examples 1 to 3 are charged with a constant current at 25°C at a current rate of 0.3C until the voltage reaches 4.2V, and then cut off at a current rate of 0.05C while maintaining 4.2V in constant voltage mode. Subsequently, constant current discharge is performed at a current rate of 0.2C until the voltage reaches 2.5V. After repeating the above charging and discharging process one more time, the batteries are charged with a constant current at 25°C at a current rate of 0.3C until the voltage reaches 4.2V, and then cut off at a current rate of 0.05C while maintaining 4.2V in constant voltage mode. After storing the batteries at a high temperature of 60°C for 60 days, the capacity retention rate (%) is shown in Table 2 below. The capacity retention rate was calculated according to Equation 2 above and is expressed as the capacity retention rate in Table 2 below.

[0156] <Equation 2> = Capacity Retention Rate = 100 × (Discharge capacity after 60 days of storage at 60℃) / (Initial discharge capacity)

[0157] Capacity retention rate (%) after 60 days of storage Example 1 86.2 Comparative Example 1 80.4 Comparative Example 2 82.7 Comparative Example 3 71.8

[0158] Referring to Table 2, it can be seen that the lithium secondary battery according to Example 1 has an improved capacity retention rate after 60 days in a high-temperature environment compared to the lithium secondary batteries according to Comparative Examples 1 to 3. This indicates that the capacity retention rate is high even after 60 days of storage because the conductivity of the electrode in Example 1 is improved and the possibility of side reactions occurring at the electrode interface is reduced.

[0159] Although preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concepts defined in the following claims are also included within the scope of the present invention. Explanation of the symbols

[0160] 100: Lithium secondary battery 10: Anode 11: Positive lead tab 12: Positive terminal 20: Cathode 21: Cathode lead tab 22: Negative terminal 30: Separator 40: Electrode assembly 50: Case 60: Sealing member 70: Electrode tab 71: Positive tab 72: Negative tab

Claims

Claim 1 A positive current collector; and a positive active material layer located on the positive current collector, wherein the positive active material layer comprises a first positive active material containing a lithium iron phosphate-based compound and a second positive active material containing a lithium nickel-based composite oxide, and wherein the density of the positive active material layer is 2.5 g / cc or more and the porosity is 22% or more. Claim 2 In claim 1, the interface resistance of the anode is 0.025 Ωcm 2 The positive electrode below. Claim 3 In claim 1, the anode having a density of the anode active material layer of 2.55 g / cc or more and 2.7 g / cc or less. Claim 4 In claim 1, the anode having a porosity of the anode active material layer of 22% or more and 45% or less. Claim 5 In claim 1, the lithium iron phosphate-based compound is an anode represented by the following Chemical Formula 1 or Chemical Formula 2: [Chemical Formula 1]Li a1 Fe (1-x1) M 1 x1 In chemical formula 1 of PO4, 0.90≤a1≤1.5, 0≤x1≤0.4, and M 1 is one or more of the elements Al, B, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and [Chemical Formula 2]Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 In chemical formula 2 of PO4, 0.90≤a2≤1.5, 0.1≤x2≤0.9, 0≤y2≤0.9, 0.1≤x2+y2<1, and M 2 is one or more of the elements Al, B, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Si, Sr, Ti, V, W, Y, Zn, and Zr. Claim 6 In claim 1, the lithium iron phosphate-based compound is LiFePO4, LiMn 0.7 Fe 0.3 PO4, LiMn 0.6 Fe 0.4 PO4, LiMn 0.5 Fe 0.5 PO4, LiMn 0.4 Fe 0.6 PO4 and LiMn 0.3 Fe 0.7 An anode comprising one or more compounds of PO4. Claim 7 A cathode according to claim 1, wherein the lithium iron phosphate compound further comprises one or more elements selected from Al, Mg, Ti, and V, and wherein one or more elements selected from Al, Mg, Ti, and V are included in an amount of 0.1 mol% to 0.5 mol% based on 100 mol% of the total metals excluding lithium in the lithium iron phosphate compound. Claim 8 In claim 1, the first positive electrode active material containing the lithium iron phosphate-based compound comprises a first particle in the form of an assembly in which a plurality of primary particles are aggregated, a second particle in the form of a single particle, or a combination thereof, and the average particle size (D) of the first particle 50 ) is 6 μm to 25 μm, and the average particle size of the second particle (D 50 ) is an anode with a diameter of 0.1 μm to 2 μm. Claim 9 A cathode according to claim 1, wherein the nickel content is 80 mol% or more based on 100 mol% of the total metal excluding lithium in the lithium-nickel-based composite oxide. Claim 10 In claim 1, the lithium nickel-based composite oxide is an anode represented by the following chemical formula 3: [Chemical Formula 3]Li a3 Ni x3 M 3 y3 M 4 z3 O 2-b3 X b3 In Chemical Formula 3, 0.9≤a3≤1.8, 0.3≤x3≤1, 0≤y3≤0.7, 0≤z3≤0.7, 0.9≤x3+y3+z3≤1.1, and 0≤b3≤0.1, and M 3 and M 4 Each is independently one or more of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more of F, P, and S. Claim 11 In claim 1, the second positive active material containing the lithium nickel-based composite oxide has an average particle size (D 50 Large particles with a diameter of 10 µm to 25 µm, average particle size (D 50 An anode comprising a subatomic particle having a size of 1 μm to 8 μm, or a combination thereof, wherein the opposite is in the form of a secondary particle formed by the aggregation of a plurality of primary particles, and the subatomic particle is in the form of a secondary particle or a single particle. Claim 12 In claim 11, the second positive active material comprises 40% to 95% by weight of the alleles and 5% to 60% by weight of the sub-particles, based on a total sum of 100% by weight of the alleles and sub-particles. Claim 13 A positive electrode according to claim 1, wherein the thickness of the positive electrode active material layer is 145 μm to 200 μm. Claim 14 In claim 1, the positive electrode active material layer comprises, based on 100 weight% of the total positive electrode active material and the second positive electrode active material, 10 weight% to 90 weight% of the first positive electrode active material and 10 weight% to 90 weight% of the second positive electrode active material. Claim 15 In claim 1, the positive electrode active material layer comprises 60% to 90% by weight of the first positive electrode active material and 10% to 40% by weight of the second positive electrode active material, based on 100% by weight of the total of the first positive electrode active material and the second positive electrode active material. Claim 16 In claim 1, the positive electrode active material layer comprises 80% to 90% by weight of the first positive electrode active material and 10% to 20% by weight of the second positive electrode active material, based on 100% by weight of the total of the first positive electrode active material and the second positive electrode active material. Claim 17 In claim 1, the positive active material layer further comprises a binder and / or a conductive material. Claim 18 In claim 17, the content of the binder is 0.1% to 5% by weight based on 100% by weight of the positive electrode active material layer, and the content of the conductive material is 0.1% to 5% by weight based on 100% by weight of the positive electrode active material layer. Claim 19 A lithium secondary battery comprising a positive electrode, a negative electrode, and an electrolyte according to any one of claims 1 to 18. Claim 20 In claim 19, the negative electrode comprises a carbon-based negative electrode active material, lithium metal, an alloy of lithium metal, a silicon-based negative electrode active material, or a combination thereof, in a lithium secondary battery.