Perovskite solar cell including organic ionic salt interlayer

Organic salts in interface layers improve interfacial stability and charge transport in perovskite solar cells, addressing stability issues and maintaining efficiency under sunlight exposure.

KR103044595B1Active Publication Date: 2026-11-06AGENCY FOR DEFENSE DEV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020250049439
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-04-16
Publication Date
2026-11-06
Estimated Expiration
2045-04-16

AI Technical Summary

Technical Problem

Inverted perovskite solar cells face issues with reduced stability due to defects at the heterojunction interfaces, leading to decreased charge transport capacity and performance degradation, especially under high temperatures and sunlight exposure.

Method used

Incorporating interface layers containing organic salts, such as amine group-containing and carboxylate group-containing organic halide salts, to enhance interfacial stability and suppress degradation between the perovskite thin film and charge transport layers.

Benefits of technology

Improves photoelectric conversion efficiency and photostability, maintaining 80% or more of initial efficiency after 500 hours of sunlight exposure, thereby enhancing the lifespan of perovskite solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025042978944-PAT00010_ABST
    Figure 112025042978944-PAT00010_ABST
Patent Text Reader

Abstract

The present disclosure relates to a perovskite solar cell comprising: a photoactive layer containing a perovskite compound; a first interface layer located on the photoactive layer and containing a first organic salt; an electron transport layer located on the first interface layer; a second interface layer located on the electron transport layer and containing a second organic salt; and a hole blocking layer located on the second interface layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to a perovskite solar cell comprising an interface layer containing an organic salt. Background Technology

[0002] Perovskite solar cells are solar cell devices that use organometal halides with a perovskite structure as light absorbers. They are attracting attention as next-generation solar cells to replace silicon solar cells due to their advantages, such as high photoelectric conversion efficiency, low manufacturing costs, and the possibility of low-temperature and low-cost solution processing.

[0003] Among them, research on inverted perovskite solar cells with pin structures is being conducted to overcome the limitations of regular perovskite solar cells with nip structures. Inverted perovskite solar cells have the advantage of enabling low-temperature solution processing and allowing for the fabrication of flexible devices using polymer and organic materials, but there is a problem of reduced stability resulting from low interlayer interaction at the heterojunction interface.

[0004] In polycrystalline perovskite thin films included in inverted structure perovskite solar cells, defects exist at the interfaces between crystals and on the surface of the thin film due to grain boundaries. These defects reduce the stability of the perovskite thin film and cause a decrease in the interfacial stability with the charge transport layer in contact with the perovskite thin film. As the number of defects increases, more recombination of electrons and holes occurs at the interface, which lowers charge transport capacity and causes a degradation in the performance of the solar cell.

[0005] Furthermore, when perovskite solar cells are exposed to high temperatures and sunlight, degradation occurs, severely reducing stability and resulting in a short service life; consequently, there are difficulties in the practical application of inverted-structure perovskite solar cells.

[0006] Accordingly, there is a need to develop perovskite solar cells that can not only improve photovoltaic conversion efficiency by enhancing interface stability between the perovskite thin film and the adjacent charge transport layer and suppressing degradation, but also minimize performance degradation through excellent photostability and mechanical stability even when exposed to sunlight for extended periods. The problem to be solved

[0007] The purpose of the present disclosure is to solve the problems of the prior art described above by providing a perovskite solar cell with improved photoelectric conversion efficiency through improved charge transport capability.

[0008] Another objective of the present disclosure is to provide a perovskite solar cell with improved photostability and mechanical stability by minimizing interface degradation between the charge transfer layer and the perovskite thin film. means of solving the problem

[0009] The present invention provides a perovskite solar cell, wherein the perovskite solar cell comprises: a photoactive layer containing a perovskite compound; a first interface layer located on the photoactive layer and containing a first organic salt; an electron transport layer located on the first interface layer; a second interface layer located on the electron transport layer and containing a second organic salt; and a hole blocking layer located on the second interface layer.

[0010] In the perovskite solar cell according to the present invention, the first organic salt and the second organic salt may each independently comprise an organic halide salt represented by the following chemical formula 1.

[0011] [Chemical Formula 1]

[0012]

[0013] (In the above Chemical Formula 1, R1 to R4 are each independently a substituted or unsubstituted hydroxyl group, C1-C10 alkyl group, C6-C30 aryl group, C1-C10 alkoxy group, carbamate group, ether group, amine group, nitrate group, thiol group, acetoxy group, phosphate group, carbonyl group, imide group, ester group, carboxyl group, cyano group, halogen group, nitro group, or sulfonyl group, and X is one or more halogen elements selected from the group comprising F, Cl, Br, and I)

[0014] In the perovskite solar cell according to the present invention, the first organic salt may comprise an amine group-containing organic halide salt represented by the following chemical formula 2.

[0015] [Chemical Formula 2]

[0016]

[0017] (In the above Chemical Formula 2, R1 and R3 are each independently a substituted or unsubstituted hydroxyl group, C1-C10 alkyl group, C6-C30 aryl group, C1-C10 alkoxy group, carbamate group, ether group, amine group, nitrate group, thiol group, acetoxy group, phosphate group, carbonyl group, imide group, ester group, carboxyl group, cyano group, halogen group, nitro group, or sulfonyl group, and X is one or more halogen elements selected from the group comprising F, Cl, Br, and I)

[0018] In the perovskite solar cell according to the present invention, the second organic salt may comprise a carboxylate group-containing organic halide salt represented by the following chemical formula 3.

[0019] [Chemical Formula 3]

[0020]

[0021] (In the above chemical formula 3, R1 and R3 are each independently a substituted or unsubstituted hydroxyl group, C1-C10 alkyl group, C6-C30 aryl group, C1-C10 alkoxy group, carbamate group, ether group, amine group, nitrate group, thiol group, acetoxy group, phosphate group, carbonyl group, imide group, ester group, carboxyl group, cyano group, halogen group, nitro group, or sulfonyl group, and X is one or more halogen elements selected from the group comprising F, Cl, Br, and I)

[0022] In the perovskite solar cell according to the present invention, the first organic salt may comprise Carbachol, and the second organic salt may comprise γ-butyrobetaine chloride.

[0023] In the perovskite solar cell according to the present invention, the organic halide salt can form a hydrogen bond with the electron transport layer.

[0024] In a perovskite solar cell according to the present invention,

[0025] In the perovskite solar cell according to the present invention, the perovskite compound may be represented by the following chemical formula 4 or 5.

[0026] [Chemical Formula 4]

[0027] ABX3

[0028] [Chemical Formula 5]

[0029] A2BX4

[0030] (In the above Chemical Formulas 4 and 5, A is a monovalent cation comprising an alkali metal; a C1-C24 alkyl group substituted with or unsubstituted with one or more of an amino group, a hydroxyl group, a cyano group, a halogen group, a nitro group, and a methoxy group; or a combination thereof; B is a divalent cation comprising one or more selected from the group comprising Pb, Sn, Ge, Cu, Ni, Co, Fe, Mn, Cr, Pd, Cd, and Yb; and X is one or more halogen anions selected from the group comprising F, Cl, Br, and I; a chalcogenide anion; or a combination thereof)

[0031] In the perovskite solar cell according to the present invention, the electron transport layer may contain one or more electron-conducting organic materials selected from the group comprising fullerene, PCBM ([6,6]-phenyl-C61-butyric acid methyl ester), C71-PCBM, C84-PCBM, and PC70BM ([6,6]-phenyl C70-butyric acid methyl ester).

[0032] In a perovskite solar cell according to the present invention, the hole blocking layer comprises Rhodamine, 1,4,5,8-naphthalene-tetracarboxylic dianhydride (NTCDA), Bathocuproine (BCP), Tris[3-(3-pyridyl)-methyl]borane (3TPYMB), LiF, Alq3 (tris(8-hydroxyquinoline) aluminum), Gaq3 (tris(8-hydroxyquinolinate) gallium), Inq3 (tris(8-hydroxyquinolinate) indium), Znq2 (Bis(8-hydroxyquinolates) zinc), Zn(BTZ)2 (Bis(2-(2-hydroxyphenyl)benzothiazolate) zinc (II)), BeBq2 (Bis(10-hydroxybenzo[h]quinolinato)beryllium) and derivatives thereof. It may contain one or more selected from the group.

[0033] A perovskite solar cell according to the present invention may further comprise: a hole transport layer located below the photoactive layer; a first electrode located below the hole transport layer; and a second electrode located on the hole blocking layer.

[0034] In a perovskite solar cell according to the present invention, the perovskite solar cell is 1 SUN (100 mW / cm²). 2 The photovoltaic conversion efficiency (PCE) when exposed for 500 hours with a light intensity of ) can be 80% or more of the initial photovoltaic conversion efficiency. Effects of the invention

[0035] A perovskite solar cell according to the present disclosure can improve solar cell performance, including photoelectric conversion efficiency, by introducing an interface layer containing an organic salt at the interface between a photoactive layer containing a perovskite compound and an electron transport layer, and at the interface between an electron transport layer and a hole blocking layer, thereby mitigating inter-layer interface defects and improving charge transport capability.

[0036] In addition, by suppressing interlayer interface degradation and improving photostability and mechanical stability, the decrease in photoelectric conversion efficiency when perovskite solar cells are exposed to sunlight for a long time can be minimized. Brief explanation of the drawing

[0037] FIG. 1 is a schematic diagram illustrating the structure of a perovskite solar cell according to one embodiment of the present disclosure. FIG. 2 is a schematic diagram illustrating a method for manufacturing a perovskite solar cell according to one embodiment of the present disclosure. FIG. 3 shows (a) Fourier transform infrared spectroscopic analysis spectra of PCBM, Carbachol, and a reaction product of PCBM and Carbachol (PCBM+Carbachol), (b) a cross-sectional Scanning Electron Microscope (SEM) image and (c) a surface Photoluminescence (PL) image of a perovskite solar cell according to Comparative Example 1, and (d) a cross-sectional Scanning Electron Microscope (SEM) image and (e) a surface Photoluminescence (PL) image of a perovskite solar cell according to Preparation Example 1. Figure 4 is the TRPL (Time-resolved Photoluminescence) analysis spectrum of perovskite solar cells according to Comparative Example 3 (Control), Preparation Example 3 (C), and Preparation Example 5 (A). Figure 5 is a graph showing the short-circuit current density (Jsc), open-circuit voltage (Voc), fill factor (FF), and photoelectric conversion efficiency (PCE) of perovskite solar cells according to Comparative Example 1 (Control) and Preparation Example 1 (C(IL 1)). Figure 6 is a current-voltage curve of a perovskite solar cell according to Preparation Example 4 (A(IL 1)). Figure 7 is a photoluminescence (PL) mapping image according to light exposure time of perovskite solar cells according to Comparative Example 2 (Control (wo IL)), Preparation Example 2 (C (IL 1)), and Example 2 (C(IL1) / G(IL2)). Figure 8 is the TRPL (Time-resolved Photoluminescence) analysis spectrum of perovskite solar cells according to Preparation Example 2 (IL1 C) and Example 2 (IL1 C + IL2 G). Figure 9 is a graph showing the short-circuit current density (Jsc), open-circuit voltage (Voc), fill factor (FF), and photoelectric conversion efficiency (PCE) of perovskite solar cells according to Preparation Example 6 (IL1 C) and Example 3 (IL1 C + IL2 G). FIG. 10 is a graph showing the change in photoelectric conversion efficiency according to light exposure time of perovskite solar cells according to Comparative Example 4 (Control(wo IL)), Preparation Example 6 (C(IL 1)), and Example 3 (C(IL1) / G(IL2)). Specific details for implementing the invention

[0038] The terms used in this specification have been selected to be as widely used as possible, taking into account the function of this disclosure; however, these terms may vary depending on the intent of those skilled in the relevant field, case law, the emergence of new technologies, etc. Unless otherwise defined, technical and scientific terms used may have the meaning commonly understood by those skilled in the art to which this invention pertains.

[0039] In this specification and the appended claims, terms such as “comprising” or “having” mean that the features or components described in the specification exist, and unless specifically limited, do not preclude the possibility that one or more other features or components may be added.

[0040] In this specification and the appended claims, when a part such as a film (layer), region, or component is described as being on or above another part, it includes not only cases where it is directly above in contact with the other part, but also cases where another film (layer), other region, or other component is interposed therein.

[0041] In this specification and the appended claims, terms such as "first," "second," etc. are used not in a limiting sense, but for the purpose of distinguishing one component from another.

[0042] Singular expressions used in this specification and the appended claims include plural expressions unless the context clearly indicates that they are singular. Additionally, plural expressions include singular expressions unless the context clearly indicates that they are plural.

[0043] Additionally, numerical ranges used herein include lower and upper limits and all values ​​within the range, increments logically derived from the form and width of the defined range, all of which are limited values, and all possible combinations of upper and lower limits of numerical ranges defined in different forms. Unless otherwise specifically defined in the specification of this disclosure, values ​​outside the numerical range that may occur due to experimental error or rounding of values ​​are also included in the defined numerical range.

[0044] Terms such as "approximately" used in this specification and the appended claims are used to encompass tolerances when tolerances exist.

[0045] Hereinafter, a perovskite solar cell comprising an interface layer containing an organic salt of the present disclosure will be described in detail.

[0046] The perovskite solar cell of the present disclosure comprises: a photoactive layer containing a perovskite compound; a first interface layer located on the photoactive layer and containing a first organic salt; an electron transport layer located on the first interface layer; a second interface layer located on the electron transport layer and containing a second organic salt; and a hole blocking layer located on the second interface layer.

[0047] A perovskite solar cell comprising a first interface layer containing a first organic salt and a second interface layer containing a second organic salt can improve surface defects of the electron transport layer through chemical interaction with the electron transport layer. As a result, interface defects between the electron transport layer and the photoactive layer, and between the electron transport layer and the hole blocking layer, can be suppressed, thereby improving electron transport capability.

[0048] In addition, photostability and thermal stability can be enhanced by preventing degradation of the interface between the photoactive layer and the electron transport layer and the interface between the electron transport layer and the hole blocking layer. In one embodiment, the perovskite solar cell is 1 SUN (100 mW / cm²). 2 When exposed for 500 hours with a light intensity of ), the photovoltaic conversion efficiency (PCE) is 80% or more, 81% or more, or 82% or more of the initial photovoltaic conversion efficiency, which can significantly improve long-term stability and lifespan characteristics.

[0049] The first interface layer and the second interface layer each have a clear boundary surface between the electron transport layer and the light absorption layer and between the electron transport layer and the hole blocking layer, and may not necessarily exist.

[0050] In an exemplary embodiment, the first interface layer may exist with a concentration gradient in which at least a portion of the first organic salt penetrates into the interface of the photoactive layer, so that the concentration of the first organic salt is highest in the first interface layer and decreases due to mutual diffusion as it moves away from the first interface layer toward the photoactive layer.

[0051] In another exemplary embodiment, the first organic salt may penetrate into the photoactive layer, so that the first interface layer in which the first organic salt is present is substantially non-existent, and the first organic salt may be present in a layer having a concentration gradient at a certain depth of the photoactive layer in the thickness direction.

[0052] In addition, at least a portion of the second organic salt has penetrated into the interface of the electron transport layer, so that the concentration of the second organic salt is highest in the second interface layer and exists with a concentration gradient in which the concentration decreases due to mutual diffusion as it moves away from the second interface layer toward the electron transport layer, or the second organic salt has penetrated into the electron transport layer so that the second interface layer in which the second organic salt exists does not substantially exist, and the second organic salt may exist with a concentration gradient at a certain depth of the electron transport layer in the thickness direction.

[0053] However, in all the embodiments exemplified, it does not mean that the organic salt contained in each interface layer penetrates into the entire volume of the photoactive layer and the electron transport layer, but rather that it penetrates into only a portion of the thickness in the thickness direction relative to the total volume of each layer of the photoactive layer and the electron transport layer, resulting in a concentration gradient due to interdiffusion.

[0054] In one example, the first organic salt and the second organic salt may each independently comprise an organic halide salt represented by the following chemical formula 1.

[0055] [Chemical Formula 1]

[0056]

[0057] (In the above chemical formula 1,

[0058] R1 to R4 are each independently a substituted or unsubstituted hydroxyl group, C1-C10 alkyl group, C6-C30 aryl group, C1-C10 alkoxy group, carbamate group, ether group, amine group, nitrate group, thiol group, acetoxy group, phosphate group, carbonyl group, imide group, ester group, carboxyl group, cyano group, halogen group, nitro group, or sulfonyl group, and

[0059] X is one or more halogen elements selected from the group including F, Cl, Br, and I)

[0060] The organic halide salt represented by Chemical Formula 1 above can form hydrogen bonds between the functional groups of the organic halide salt and the electron transport layer through chemical interaction with the electron transport layer. The electron transport layer and the organic halide salt can form a more uniform electron transport layer through hydrogen bonding, and the electron transport capacity can be improved and interfacial stability enhanced by effectively suppressing surface defects of the electron transport layer.

[0061] More specifically, the first organic salt may include an amine group-containing organic halide salt represented by the following chemical formula 2.

[0062] [Chemical Formula 2]

[0063]

[0064] (In the above chemical formula 2,

[0065] R1 and R3 are each independently a substituted or unsubstituted hydroxyl group, C1-C10 alkyl group, C6-C30 aryl group, C1-C10 alkoxy group, carbamate group, ether group, amine group, nitrate group, thiol group, acetoxy group, phosphate group, carbonyl group, imide group, ester group, carboxyl group, cyano group, halogen group, nitro group, or sulfonyl group, and

[0066] X is one or more halogen elements selected from the group including F, Cl, Br, and I)

[0067] When the organic halide salt included in the first organic salt contains an amine group, it is advantageous to form hydrogen bonds through easier chemical interaction with the electron transport layer by combining with the electron-conducting organic material described later.

[0068] In addition, the second organic salt may include a carboxyl group-containing organic halide salt represented by the following chemical formula 3.

[0069] [Chemical Formula 3]

[0070]

[0071] (In the above chemical formula 3,

[0072] R1 and R3 are each independently a substituted or unsubstituted hydroxyl group, C1-C10 alkyl group, C6-C30 aryl group, C1-C10 alkoxy group, carbamate group, ether group, amine group, nitrate group, thiol group, acetoxy group, phosphate group, carbonyl group, imide group, ester group, carboxyl group, cyano group, halogen group, nitro group, or sulfonyl group, and

[0073] X is one or more halogen elements selected from the group including F, Cl, Br, and I)

[0074] When the organic halide salt included in the second organic salt contains a carboxylate group, it is advantageous because it facilitates hydrogen bonding with the electron-conducting organic material and hole-blocking layer material described later.

[0075] In a preferred example, the first interface layer may include carbachol as an organic halide salt, and the second interface layer may include gamma-butyrobetaine chloride as an organic halide salt.

[0076] When the organic halide salts included in the first and second interface layers contain the above combination, the effect of mitigating interface defects between the photoactive layer and the electron transport layer and between the electron transport layer and the hole blocking layer, respectively, and minimizing surface defects of the photoactive layer, electron transport layer, and hole blocking layer can be further maximized. Accordingly, by suppressing non-radiative recombination and improving electron transport capacity, it can contribute to improving the photoelectric conversion efficiency of perovskite solar cells. Furthermore, since interface degradation is suppressed even when exposed to long-term light and high temperatures, long-term photostability and thermal stability are improved, thereby enhancing the lifespan characteristics of perovskite solar cells.

[0077] The electron transport layer may comprise one or more electron-conducting organic materials selected from the group comprising fullerenes and derivatives thereof; one or more electron-conducting inorganic materials selected from the group comprising SnO2, TiO2, ZrO, Al2O3, ZnO, WO3, Nb2O5, and TiSrO3; or a combination thereof, and preferably may comprise an electron-conducting organic material capable of suppressing surface and interface defects through hydrogen bonding with the first interface layer and the second interface layer.

[0078] The above electronically conductive organic material is fullerene (C 60 , C 70 , C 74 , C 76 , C 78 , C 82 , C 95 ), PCBM([6,6]-phenyl-C 61 butyric acid methyl ester), C 71 -PCBM, C 84 -PCBM and PC 70 BM([6,6]-phenyl C 70 It may include one or more selected from the group including -butyric acid methyl ester), and preferably PCBM ([6,6]-phenyl-C 61It may include butyric acid methyl ester.

[0079] The hole blocking layer comprises one or more selected from the group comprising Rhodamine, 1,4,5,8-naphthalene-tetracarboxylic dianhydride (NTCDA), Bathocuproine (BCP), Tris[3-(3-pyridyl)-methyl]borane (3TPYMB), LiF, Alq3 (tris(8-hydroxyquinoline) aluminum), Gaq3 (tris(8-hydroxyquinolinate) gallium), Inq3 (tris(8-hydroxyquinolinate) indium), Znq2 (Bis(8-hydroxyquinolates) zinc), Zn(BTZ)2 (Bis(2-(2-hydroxyphenyl)benzothiazolate) zinc (II)), BeBq2 (Bis(10-hydroxybenzo[h]quinolinato)beryllium) and derivatives thereof. It is preferable to include one or more selected from the group including Rhodamine and derivatives thereof, which can easily form hydrogen bonds with the second interface layer.

[0080] The perovskite compound included in the above photoactive layer refers to an organometal halide with a perovskite structure and can be represented by the following chemical formula 4 or 5.

[0081] [Chemical Formula 4]

[0082] ABX3

[0083] [Chemical Formula 5]

[0084] A2BX4

[0085] (In the above Chemical Formulas 4 and 5,

[0086] A is a monovalent cation comprising an alkali metal; a C1-C24 alkyl group substituted with or unsubstituted with one or more of an amino group, a hydroxyl group, a cyano group, a halogen group, a nitro group, and a methoxy group; or a combination thereof, and

[0087] B is a divalent cation comprising one or more selected from the group including Pb, Sn, Ge, Cu, Ni, Co, Fe, Mn, Cr, Pd, Cd, and Yb, and

[0088] X is one or more halogen anions selected from the group including F, Cl, Br, and I; chalcogenide anions; or a combination thereof)

[0089] More specifically, in the above Chemical Formulas 4 and 5, A may be a monovalent cation comprising an amidinium group ion, an organic ammonium ion, or a combination thereof, and more specifically, the amidinium group ion is formamidinium (formamidinium, NH2CH=NH2 + ) ion, acetamidinium (acetamidinium, NH2C(CH3)=NH2 + ) or Guamidinium (Guamidinium, NH2C(NH2)=NH2 + Examples include ) etc. If A contains both organic ammonium ions and amidinium-based ions, A is A' 1-x A'' x (A'' is the aforementioned monovalent organic ammonium ion, A' is the aforementioned amidinium-based ion, and x is 0 <x<1인 실수, 좋게는 0.05≤x≤의0.3인 실수)로 표시될 수 있으나, 본 개시가 이에 한정되는 것은 아니다.

[0090] In one example, it may further include a hole transport layer located below the photoactive layer; a first electrode located below the hole transport layer; and a second electrode located on the hole blocking layer.

[0091] That is, a perovskite solar cell according to one embodiment of the present disclosure may be an inverted structure perovskite solar cell (100) in which a first electrode (10), a hole transport layer (20), a photoactive layer (30), a first interface layer (40), an electron transport layer (50), a second interface layer (60), a hole blocking layer (70), and a second electrode (80) are sequentially stacked, as shown in FIG. 1.

[0092] The first electrode may be a conductive electrode that is ohmic-junctioned with a hole transport layer, and preferably may include a transparent conductive electrode. Specifically, the transparent conductive material may include fluorine-doped tin oxide (FTO), indium-doped tin oxide (ITO), ZnO, carbon nanotubes, graphene, or a combination thereof, but the present disclosure is not limited thereto. At this time, a transparent substrate (support) may be positioned below the first electrode. Examples of the transparent substrate may include glass, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyimide (PI), polycarbonate (PC), polypropylene (PP), triacetylcellulose (TAC), or polyethersulfone (PES) substrates, but the present invention is not limited to specific materials of the substrate.

[0093] The second electrode may be a conductive electrode that is ohmic-junctioned with an electron transport layer, and may be any material commonly used as an electrode material for the front electrode or the back electrode in a solar cell. As a non-limiting example, if the second electrode is an electrode material for the back electrode, the second electrode may be one or more selected from the group comprising gold (Au), silver (Ag), platinum (Pt), palladium (Pd), copper (Cu), aluminum (Al), carbon (C), cobalt sulfide, copper sulfide, nickel oxide, or combinations thereof. As a non-limiting example, if the second electrode is a transparent electrode, the second electrode may include fluorine-doped tin oxide (FTO), indium-doped tin oxide (ITO), ZnO, carbon nanotubes, graphene, or combinations thereof, but the present disclosure is not limited to specific materials of the second electrode.

[0094] The hole transport layer may include an organic hole transport material, an inorganic hole transport material, or a combination thereof.

[0095] In a non-limiting example, the hole transport layer may be a plurality of unit hole transport layers containing different hole transport materials stacked together; more specifically, the hole transport layer may consist of a first hole transport layer containing an inorganic hole transport material and a second hole transport layer containing an organic hole transport material stacked together. By having a structure in which unit hole transport layers containing different hole transport materials are stacked, hole mobility is improved and long-term operational stability can be secured without the need for a separate lithium additive.

[0096] In this case, the inorganic hole transport material is nickel oxide (NiO₂). x It may include one or more selected from ), CuSCN, CuCrO2, CuI, MoO, and V2O5.

[0097] Organic hole transporters include carbazole derivatives, polyarylalkane derivatives, phenylenediamine derivatives, arylamines, amino-substituted chalcone derivatives, styrylanthracene derivatives, fluorene derivatives, hydrazone derivatives, stilbene derivatives, silazane derivatives, aromatic tertiary amine compounds, styrylamine compounds, aromatic dimethylidine compounds, porphyrin compounds, phthalocyanine compounds, polythiophene derivatives, polypyrrole derivatives, polyparaphenylenevinylene derivatives, pentacene, coumarin 6 (3-(2-benzothiazolyl)-7-(diethylamino)coumarin), ZnPC (zinc phthalocyanine), CuPC (copper phthalocyanine), and TiOPC (titanium oxide phthalocyanine). Spiro-MeOTAD(2,2',7,7'-tetrakis(N,Np-dimethoxyphenylamino)-9,9'-spirobifluorene), F16CuPC(copper(II) 1,2,3,4,8,9,10,11,15,16,17,18,22,23,24,25-hexadecafluoro-29H,31H-phthalocyanine), SubPc (boron subphthalocyanine chloride) and N3(cis-di(thiocyanato)-bis(2,2'-bipyridyl-4,4'-dicarboxylic acid)-ruthenium(II), P3HT(poly[3-hexylthiophene]), MDMO-PPV(poly[2-methoxy-5-(3',7'-dimethyloctyloxyl)]-1,4-phenylene vinylene), MEH-PPV(poly[2-methoxy-5-(2''-ethylhexyloxy)-p-phenylene vinylene]), P3OT(poly(3-octyl thiophene)), POT(poly(octyl thiophene)), P3DT(poly(3-decyl thiophene)),P3DDT(poly(3-dodecyl thiophene), PPV(poly(p-phenylene vinylene)), TFB(poly(9,9'-dioctylfluorene-co-N-(4-butylphenyl)diphenyl amine), 폴리아닐린(Polyaniline), Spiro-MeOTAD([2,22′,7,77′-tetrkis (N,N-di-pmethoxyphenyl amine)-9,9,9′-spirobi fluorine]), PCPDTBT(Poly[2,1,3-benzothiadiazole-4,7-diyl[4,4-bis(2-ethylhexyl-4H-cyclopenta [2,1-b:3,4-b']dithiophene-2,6-diyl]], Si-PCPDTBT(poly[(4,4′-bis(2-ethylhexyl)dithieno[3,2-b:2′,3′-d]silole)-2,6-diyl-alt-(2,1,3-benzothiadiazole)-4,7-diyl]), PBDTTPD(poly((4,8-diethylhexyloxyl), PFDTBT(poly[2,7-(9-(2-ethylhexyl)-9-hexyl-fluorene)-alt-5,5-(4', 7, -di-2-thienyl-2',1', 3'-benzothiadiazole)]), PFO-DBT(poly[2,7-.9,9-(dioctyl-fluorene)-alt-5,5-(4',7'-di-2-.thienyl-2', 1', 3'-benzothiadiazole)]), PSiFDTBT(poly[(2,7-dioctylsilafluorene)-2,7-diyl-alt-(4,7-bis(2-thienyl)-2,1,3-benzothiadiazole)-5,5′-diyl]), PCDTBT(Poly [[9-(1-octylnonyl)-9H-carbazole-2,7-diyl] -2,5-thiophenediyl-2,1,3-benzothiadiazole-4,7-diyl-2,5-thiophenediyl]), PFB(poly(9,It may include one or more selected from 9′-dioctylfluorene-co-bis(N,N′-(4,butylphenyl))bis(N,N′-phenyl-1,4-phenylene)diamine), F8BT(poly(9,9′-dioctylfluorene-cobenzothiadiazole), PEDOT (poly(3,4-ethylenedioxythiophene)), PEDOT:PSS poly(3,4-ethylenedioxythiophene) poly(styrenesulfonate), PTAA (poly(triarylamine)), 2-PACz, MeO-2PACz, Br-2PACz, Me-4PACz, MeO-4PACz, and 6-PACz.

[0098] The present disclosure will be explained in more detail below through examples.

[0099] (Preparation Example 1)

[0100] A glass substrate coated with an ITO (Indium tin oxide) first electrode was washed with neutral soap, then sequentially immersed in acetone, deionized water, and isopropanol, sonicated for 20 minutes each, and washed by UV / Ozone treatment for 30 minutes.

[0101] A hole transport layer is formed by spin-coating an isopropanol anhydride solution containing 0.5 mg / ml of MeO-4PACz (Tokyo Chemical Industry) dispersed on a substrate at 4000 rpm for 20 seconds and annealing at 110°C for 10 minutes.

[0102] Next, a perovskite precursor solution was prepared by mixing a mixture of 160.0 mg of FAI dissolved in a 1.6 M concentration PbI2 solution (using a 4:1 volume ratio of DMF (Dimethylformamide) : DMSO (Dimethyl Sulfoxide) solvent), a mixture of 21.3 mg of MABr dissolved in a 1.6 M concentration PbBr2 solution (using a 4:1 volume ratio of DMF : DMSO solvent), and a solution of 124.8 mg of CsI dissolved in 300 μL of DMSO, each in a volume ratio of 730 : 110 : 42.

[0103] During spin coating of the perovskite precursor solution onto the hole transport layer at 6000 rpm for 30 seconds, 130 μl of ethyl acetate antisolvent was added 10 seconds before the spin was terminated to form an intermediate phase thin film. After the spin was terminated, the film was annealed at 100 °C for 20 minutes to form a photoactive layer containing a perovskite compound.

[0104] Subsequently, as shown in FIG. 2, 60 μL of an organic salt solution containing 0.55 mg / ml of Carbachol was dropped onto the photoactive layer, spin-coated at 6000 rpm for 20 seconds, and then annealed at 65 °C for 3 minutes to form a first interfacial layer. PC on the first interfacial layer 61 50 μL of chlorobenzene (CB) solution in which BM (1-Material) was dissolved at 20 mg / ml was added, and the electron transport layer was formed by spin-coating at 3000 rpm for 40 seconds and then annealing at 65 ℃ for 5 minutes.

[0105] 60 μL of an isopropanol anhydrous solution containing 0.5 mg / ml Rhodamine 101 (Sigma Aldrich) was deposited onto the electron transport layer and spin-coated at 6000 rpm for 30 seconds, followed by annealing at 65 °C for 3 minutes to form a hole blocking layer. On the hole blocking layer, 10 -6 A perovskite solar cell was fabricated by forming a second electrode by depositing gold (Au) to a thickness of 100 nm at a pressure of mbar and a deposition rate of 0.1 to 0.3 nm / s.

[0106] (Preparation Example 2)

[0107] A perovskite solar cell was prepared in the same manner as in Preparation Example 1, except that the first and second electrodes and the hole transport layer were not used.

[0108] (Preparation Example 3)

[0109] A perovskite solar cell was manufactured using the same method as in Example 2, except that a hole blocking layer was not used.

[0110] (Preparation Example 4)

[0111] A perovskite solar cell was prepared in the same manner as in Preparation Example 1, except that the first interface layer was formed using an isopropanol anhydride solution in which acetylcholine chloride was dissolved instead of carvacol.

[0112] (Preparation Example 5)

[0113] A perovskite solar cell was prepared in the same manner as in Preparation Example 3, except that the first interface layer was formed using an isopropanol anhydride solution in which acetylcholine chloride was dissolved instead of carvacol.

[0114] (Preparation Example 6)

[0115] NiO on the substrate x After depositing the thin film, NIO xA perovskite solar cell was prepared in the same manner as in Preparation Example 1, except that a hole transport layer was formed by forming a MeO-4PACz thin film on the thin film.

[0116] Specifically, to form a NiOx thin film, a substrate is immersed in a 0.1 M Ni(NO3)26H2O ultrapure water solution, then electrodeposited by applying a voltage of -0.8 V for 20 seconds, and then annealed at 300°C for 60 minutes to form a NiOx thin film.

[0117] (Example 1)

[0118] A perovskite solar cell was prepared in the same manner as in Preparation Example 1, except that 60 μL of an ionic salt solution containing 0.55 mg / ml of gamma-butyrobetaine chloride was dropped onto the electron transport layer, spin-coated at 6000 rpm for 20 seconds, and then annealed at 65 ℃ for 3 minutes to form a second interface layer.

[0119] (Example 2)

[0120] A perovskite solar cell was manufactured in the same manner as in Example 1, except that the first and second electrodes and the hole transport layer were not used.

[0121] (Example 3)

[0122] NiO on the substrate x After depositing the thin film, NIO x A perovskite solar cell was manufactured in the same manner as in Example 1, except that a hole transport layer was formed by forming a MeO-4PACz thin film on the thin film.

[0123] Specifically, to form a NiOx thin film, a substrate is immersed in a 0.1 M concentration Ni(NO3)26H2O ultrapure water solution, then electrodeposited by applying a voltage of -0.8 V for 20 seconds, and then annealed at 300°C for 60 minutes to form a NiOx thin film.

[0124] (Comparative Example 1)

[0125] A perovskite solar cell was manufactured in the same manner as in Example 1, except that the first interface layer and the second interface layer were not formed.

[0126] (Comparative Example 2)

[0127] A perovskite solar cell was manufactured using the same method as in Example 2, except that the first interface layer was not formed.

[0128] (Comparative Example 3)

[0129] A perovskite solar cell was manufactured using the same method as in Preparation Example 3, except that the first interface layer was not formed.

[0130] (Comparative Example 4)

[0131] A perovskite solar cell was manufactured in the same manner as in Example 3, except that the first interface layer and the second interface layer were not formed.

[0133] Physical Property Evaluation Methods

[0134] - Fourier Transform Infrared Spectroscopy (FT-IR) was performed using a Fourier Transform Infrared Spectrometer (Shimadzu, IRTracer-100).

[0135] - The cross-sectional structure of the perovskite solar cell was observed using a scanning electron microscope (JEOL, JSM-7600F).

[0136] - Photoluminescence (PL) spectroscopic image mapping analysis was performed using a microscope (Microscope Axio Imager, A2m, Zeiss) equipped with a CCD camera (Andor sCMOS Camera: Zyla 5.5) and an optical filter ((Chroma 19006 - AT - Texas Red Longpass (AT560 / 40x EX - AT600DC BS - AT610lp EM)).

[0137] - Time-Resolved Photoluminescence (TRPL) analysis was performed using a time-resolved photoluminescence spectrometer (Edinburgh Instruments, FLS-1000) by irradiating a pulsed diode laser with an excitation wavelength of 405 nm at a frequency of 5 MHz and measuring the 770 nm radiation wavelength range.

[0138] The electrical characteristics of the perovskite solar cells were measured using an artificial sun device (Oriel sol3A) and a source meter (Keithley, 2400 digital source meter) at a sweep speed of 100 mV / s. Calibration was performed under standard conditions of AM 1.5 G using a reference cell (KG-5 filtered Si cell). Additionally, unencapsulated perovskite solar cells were placed in a box filled with N2 gas and subjected to 1 SUN (100 mW / cm²) for 500 hours at a temperature of 25°C. 2 Long-term stability was evaluated by irradiating visible light with a light intensity of ).

[0139] FIG. 3 shows (a) Fourier transform infrared spectroscopic analysis spectra of PCBM, Carbachol, and a reaction product of PCBM and Carbachol (PCBM+Carbachol), (b) a cross-sectional Scanning Electron Microscope (SEM) image and (c) a surface Photoluminescence (PL) image of a perovskite solar cell according to Comparative Example 1, and (d) a cross-sectional Scanning Electron Microscope (SEM) image and (e) a surface Photoluminescence (PL) image of a perovskite solar cell according to Preparation Example 1.

[0140] Referring to Fig. 3(a), the reaction product of PCBM and carvacol is 1729±0.5 cm -1 and 1738±0.5 cm -1An FT-IR peak indicating the formation of hydrogen bonds was observed. This signal is not observed in the FT-IR spectra of PCBM and carvacol individually, suggesting that PCBM and carvacol are bonded through chemical interactions.

[0141] More specifically, referring to FIGS. 3(b) to FIGS. 3(e), the perovskite solar cell of Comparative Example 1, which does not include a first interface layer, had a PCBM electron transport layer thickness of 59±7 nm, and the electron transport layer was unevenly coated on the surface of the photoactive layer, so the surface of the photoactive layer was not completely covered by the electron transport layer and formed surface defects.

[0142] On the other hand, in the perovskite solar cell of Preparation Example 1, a first interface layer containing carvacol is located between the photoactive layer and the electron transport layer, and thus, the PCBM of the electron transport layer and the carvacol of the first interface layer formed hydrogen bonds through chemical interaction. Therefore, even though the electron transport layer was formed under the same conditions as Comparative Example 1, the thickness of the electron transport layer of Preparation Example 1 increased to 79 ± 11 nm, and the electron transport layer was uniformly coated, allowing for effective suppression of defects on the surface of the electron transport layer. In other words, it was confirmed that surface defects of the electron transport layer and interfacial stability can be improved by the formation of hydrogen bonds through chemical interaction between the PCBM of the electron transport layer and the carvacol of the first interface layer in contact with it.

[0143] Figure 4 shows the Time-resolved Photoluminescence (TRPL) analysis spectra of perovskite solar cells according to Comparative Example 3 (Control), Preparation Example 3 (C), and Preparation Example 5 (A). As shown in Figure 4, in the perovskite solar cell of Preparation Example 3, in which the first interface layer contains carvacol, the amine group (NH2) of carvacol was able to easily form hydrogen bonds with the PCBM of the electron transport layer. As a result, defects in the electron transport layer were improved, and as the interfacial stability with the photoactive layer was enhanced, the electron transport capacity was improved and non-radiative recombination was reduced. On the other hand, in the perovskite solar cell of Preparation Example 5, since the first interface layer contains acetylcholine chloride that does not contain amine groups, hydrogen bonds could not be formed with the electron transport layer, and consequently, the electron transport capacity was significantly reduced.

[0144] FIG. 5 shows the short-circuit current density (J) of a perovskite solar cell according to Comparative Example 1 (Control) and Preparation Example 1 (C(IL 1)). sc ), open-circuit voltage (V oc This is a graph measuring the fill factor (FF) and photoelectric conversion efficiency (PCE). As shown in FIG. 5, the perovskite solar cell of Preparation Example 1, comprising a first interface layer, passes the surface of the photoactive layer, mitigates surface defects in the electron transport layer, and enhances interface stability between the photoactive layer and the electron transport layer, thereby increasing the short-circuit current density (J sc ), open-circuit voltage (V oc Both the fill factor (FF) and the fill factor (FF) were improved compared to Comparative Example 1, and as a result, the photoelectric conversion efficiency was also improved.

[0145] Figure 6 is a current-voltage curve of a perovskite solar cell according to Preparation Example 4 (A(IL 1)). Referring to Figure 6, it was confirmed that when the first interface layer contains acetylcholine chloride, the output factors of the current-voltage curve decrease sharply, resulting in significantly lower solar cell performance.

[0146] Figure 7 is a photoluminescence (PL) mapping image according to light exposure time of perovskite solar cells according to Comparative Example 2 (Control (wo IL)), Preparation Example 2 (C (IL 1)), and Example 2 (C(IL1) / G(IL2)).

[0147] As shown in Fig. 7, the perovskite solar cell of Comparative Example 2, which does not include an interface layer, showed an increase in PL intensity as the PL quenching tendency decreased due to interface degradation between the photoactive layer and the electron transport layer as the exposure time to light increased. On the other hand, the perovskite solar cell of Manufacturing Example 2, which includes a first interface layer, showed almost no change in PL intensity even after 170h, and the perovskite solar cell of Example 2, which includes a first interface layer and a second interface layer, showed the least change in PL intensity after 620h, confirming that the excellent electron transport capacity of the perovskite solar cell can be maintained for a long time by introducing an interface layer.

[0148] FIG. 8 is the TRPL (Time-resolved Photoluminescence) analysis spectrum of perovskite solar cells according to Preparation Example 2 (IL1 C) and Example 2 (IL1 C + IL2 G), and FIG. 9 is the short-circuit current density (J) of perovskite solar cells according to Preparation Example 6 (IL1 C) and Example 3 (IL1 C + IL2 G). sc ), open-circuit voltage (V oc This is a graph showing the measured fill factor (FF) and photoelectric conversion efficiency (PCE).

[0149] As shown in FIGS. 8 and 9, the perovskite solar cell according to Example 3 includes a second interface layer between the electron transport layer and the hole blocking layer in addition to the first interface layer. Since the gamma-butyrobetaine chloride of the second interface layer mitigates interface defects and suppresses non-radiative recombination through interaction with the PCBM of the electron transport layer, it showed improved performance compared to the perovskite solar cell of Preparation Example 6.

[0150] FIG. 10 is a graph showing the change in photoelectric conversion efficiency according to the light exposure time of perovskite solar cells according to Comparative Example 4 (Control(wo IL)), Preparation Example 6 (C(IL 1)), and Example 3 (C(IL1) / G(IL2)). The perovskite solar cell of Comparative Example 4, which does not include an interface layer, not only had the lowest initial photoelectric conversion efficiency but also showed very low lifetime characteristics as the photoelectric conversion efficiency decreased rapidly after exposure to light. The perovskite solar cell of Preparation Example 6 operated stably for about 160 hours by introducing a first interface layer, but after 160 hours, the photoelectric conversion efficiency decreased rapidly and operated for only about 210 hours, showing low lifetime characteristics. On the other hand, the perovskite solar cell of Example 3, which includes a first interface layer and a second interface layer, not only had the highest initial photoelectric conversion efficiency of 21.37%, but also maintained a photoelectric conversion efficiency of 82.8% of the initial photoelectric conversion efficiency when exposed to light for 500 hours, exhibiting significantly improved photostability and lifespan characteristics.

[0151] As described above, the present invention has been explained by specific details, limited embodiments, and drawings; however, this is provided merely to aid in a more comprehensive understanding of the invention and is not limited to the above embodiments. Those skilled in the art can make various modifications and variations from this description.

[0152] Accordingly, the scope of the present invention is not limited to the described embodiments, and all things equivalent to or having equivalent variations to the claims set forth below, as well as the claims set forth below, shall be considered to fall within the scope of the concept of the present invention. Explanation of the symbols

[0153] 10: First electrode 20: Hole transport layer 30: Photoactive layer 40: First interface layer 50: Electron transport layer 60: Second interface layer 70: Hole blocking layer 80: Second electrode 100: Perovskite solar cell

Claims

Claim 1 A perovskite solar cell comprising: a photoactive layer containing a perovskite compound; a first interface layer located on the photoactive layer and containing a first organic salt; an electron transport layer located on the first interface layer; a second interface layer located on the electron transport layer and containing a second organic salt; and a hole blocking layer located on the second interface layer. Claim 2 A perovskite solar cell according to claim 1, wherein the first organic salt and the second organic salt each independently comprise an organic halide salt represented by the following chemical formula 1. [Chemical Formula 1] (In the above Chemical Formula 1, R1 to R4 are each independently a substituted or unsubstituted hydroxyl group, C1-C10 alkyl group, C6-C30 aryl group, C1-C10 alkoxy group, carbamate group, ether group, amine group, nitrate group, thiol group, acetoxy group, phosphate group, carbonyl group, imide group, ester group, carboxyl group, cyano group, halogen group, nitro group, or sulfonyl group, and X is one or more halogen elements selected from the group comprising F, Cl, Br, and I) Claim 3 A perovskite solar cell according to claim 2, wherein the first organic salt comprises an amine group-containing organic halide salt represented by the following chemical formula 2. [Chemical Formula 2] (In the above Chemical Formula 2, R1 and R3 are each independently a substituted or unsubstituted hydroxyl group, C1-C10 alkyl group, C6-C30 aryl group, C1-C10 alkoxy group, carbamate group, ether group, amine group, nitrate group, thiol group, acetoxy group, phosphate group, carbonyl group, imide group, ester group, carboxyl group, cyano group, halogen group, nitro group, or sulfonyl group, and X is one or more halogen elements selected from the group comprising F, Cl, Br, and I) Claim 4 A perovskite solar cell according to claim 2, wherein the second organic salt comprises a carboxylate group-containing organic halide salt represented by the following chemical formula 3. [Chemical Formula 3] (In the above chemical formula 3, R1 and R3 are each independently a substituted or unsubstituted hydroxyl group, C1-C10 alkyl group, C6-C30 aryl group, C1-C10 alkoxy group, carbamate group, ether group, amine group, nitrate group, thiol group, acetoxy group, phosphate group, carbonyl group, imide group, ester group, carboxyl group, cyano group, halogen group, nitro group, or sulfonyl group, and X is one or more halogen elements selected from the group comprising F, Cl, Br, and I) Claim 5 A perovskite solar cell according to claim 1, wherein the first organic salt comprises carbachol and the second organic salt comprises gamma-butyrobetaine chloride. Claim 6 A perovskite solar cell according to paragraph 2, wherein the organic halide salt forms a hydrogen bond with the electron transport layer. Claim 7 A perovskite solar cell according to claim 1, wherein the perovskite compound is represented by the following chemical formula 4 or 5. [Chemical Formula 4] ABX3 [Chemical Formula 5] A2BX4 (wherein in the above chemical formulas 4 and 5, A is a monovalent cation comprising an alkali metal; a C1-C24 alkyl group substituted or unsubstituted with one or more of an amino group, a hydroxyl group, a cyano group, a halogen group, a nitro group, and a methoxy group; or a combination thereof; B is a divalent cation comprising one or more selected from the group comprising Pb, Sn, Ge, Cu, Ni, Co, Fe, Mn, Cr, Pd, Cd, and Yb; and X is one or more halogen anions selected from the group comprising F, Cl, Br, and I; a chalcogenide anion; or a combination thereof) Claim 8 A perovskite solar cell according to claim 1, wherein the electron transport layer comprises one or more electron-conducting organic materials selected from the group comprising fullerene, PCBM ([6,6]-phenyl-C61-butyric acid methyl ester), C71-PCBM, C84-PCBM, and PC70BM ([6,6]-phenyl C70-butyric acid methyl ester). Claim 9 In claim 1, the hole blocking layer comprises one or more selected from the group comprising Rhodamine, 1,4,5,8-naphthalene-tetracarboxylic dianhydride (NTCDA), Bathocuproine (BCP), Tris[3-(3-pyridyl)-methyl]borane (3TPYMB), LiF, Alq3 (tris(8-hydroxyquinoline) aluminum), Gaq3 (tris(8-hydroxyquinolinate) gallium), Inq3 (tris(8-hydroxyquinolinate) indium), Znq2 (Bis(8-hydroxyquinolates) zinc), Zn(BTZ)2 (Bis(2-(2-hydroxyphenyl)benzothiazolate) zinc (II)), BeBq2 (Bis(10-hydroxybenzo[h]quinolinato)beryllium) and derivatives thereof. Perovskite solar cells. Claim 10 A perovskite solar cell according to claim 1, further comprising: a hole transport layer located below the photoactive layer; a first electrode located below the hole transport layer; and a second electrode located on the hole blocking layer. Claim 11 In claim 1, the perovskite solar cell is 1SUN (100 mW / cm²) 2 A perovskite solar cell having a photovoltaic conversion efficiency (PCE) of 80% or more of the initial photovoltaic conversion efficiency when exposed to a light intensity of ) for 500 hours.

Citation Information

Patent Citations

  • Perovskite composite bonded with molecular additive, method of manufacturing the same, and perovskite solar cell comprising the same

    KR101927793B1

  • A perovskite solar cell including an interfacial layer and the Fabrication Method Thereof

    KR1020240025334A

  • Perovskite solar cell enhanced α-phase stability and manufacturing method thereof

    KR1020240121631A