Neutron Shield Artificial Light-weight Aggregate and Manufacturing method thereof

A cement-free binder using fly ash, calcium hydroxide, sodium carbonate, and boron compounds addresses the challenge of incorporating neutron shielding materials in lightweight aggregates, achieving high-strength and effective neutron shielding performance.

KR103044935B1Active Publication Date: 2026-11-06UNIST (ULSAN NAT INST OF SCI & TECH)
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020230133811
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-06
Publication Date
2026-11-06
Estimated Expiration
2043-10-06

AI Technical Summary

Technical Problem

Existing artificial lightweight aggregates face challenges in incorporating neutron shielding materials due to decomposition at high temperatures and reduced concrete strength when using boron compounds, and they require a cement-free binder that maintains neutron shielding performance.

Method used

A cement-free binder composed of fly ash, calcium hydroxide, sodium carbonate, and boron compounds, manufactured at low temperatures, which includes sucrose to form a neutron-shielding artificial lightweight aggregate.

Benefits of technology

The solution provides a high-strength, cement-free artificial lightweight aggregate that maintains neutron shielding performance and withstands neutron radiation without the issues of conventional methods, suitable for use in nuclear facilities and other concrete structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023110156430-PAT00002_ABST
    Figure 112023110156430-PAT00002_ABST
Patent Text Reader

Abstract

The present invention relates to artificial lightweight aggregates, and more specifically, to carbon-reducing artificial lightweight aggregates based on fly ash that can be manufactured even at low temperatures.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to artificial lightweight aggregates, and more specifically, to carbon-reducing artificial lightweight aggregates based on fly ash that can be manufactured even at low temperatures. Background Technology

[0002] Unlike fast neutrons, which are shielded by elastic collisions with water molecules, thermal neutrons require absorption shielding using materials such as boron, gadolinium, samarium, and cadmium, which have high neutron absorption cross-sections.

[0003] Among them, boron has been widely used for economic reasons, and research has been conducted on boron compounds such as B4C. However, there are difficulties in using them due to the problem of reduced concrete strength, the difficulty of incorporating large quantities at a price of nearly 1 million won per kg, and the difficulty in controlling particle size due to their characteristics.

[0004] For this reason, research has been conducted extensively on incorporating boric acid (1 kg, 2,960 won) or borax (1 kg, 2,640 won) into concrete to ensure economic efficiency and neutron shielding performance.

[0005] However, it has been widely reported that when these boron compounds are directly incorporated into ordinary Portland cement, they inhibit setting and reduce the development of compressive strength; consequently, direct incorporation into ordinary concrete is practically difficult.

[0006] Accordingly, there is a need to develop a new high-strength, cement-free binder that can contain neutron shielding materials without issues, unlike Portland cement.

[0007] When the crystalline structure of aggregates is exposed to neutron radiation, it becomes amorphous due to an increase in lattice constant and lattice defects, and the volume increases, resulting in severe expansive cracking of concrete. Consequently, since the aggregates used in concrete for nuclear facilities are all natural and crushed aggregates with high crystallinity, they are exposed to expansive fracture caused by neutron radiation; therefore, the use of amorphous aggregates is essential for concrete used for neutron shielding.

[0008] Existing artificial lightweight aggregate technologies use kilns for high-temperature firing at over 1,200 °C, so even if neutron shielding materials are included, they decompose and are lost during the manufacturing process. Therefore, it is virtually impossible to incorporate neutron shielding materials into existing artificial aggregates, and thus, they must be manufactured using an artificial lightweight aggregate technology that maintains neutron shielding materials by manufacturing and curing under low-temperature conditions. Prior art literature

[0009] Republic of Korea Registered Patent Publication No. 10-1938528 The problem to be solved

[0010] The objective of the present invention is to provide a construction material manufactured from coal ash (fly ash), a byproduct generated from thermal power plants, etc., without using forged plant cement.

[0011] In addition, the present invention provides an artificial lightweight aggregate that can be manufactured at low temperatures, does not use Portland cement, and can maintain a neutron shielding material.

[0012] The objectives of the present invention are not limited to those mentioned above, and other unmentioned objectives will be clearly understood from the description below. means of solving the problem

[0013] A neutron-shielding artificial lightweight aggregate according to one embodiment of the present invention comprises fly ash; calcium hydroxide (Ca(OH)2); sodium carbonate (Na2CO3), boron compounds and sucrose (C12 H 22 O 11 Includes ).

[0014] The above fly ash may consist of silicon dioxide (SiO2) and aluminum oxide (Al2O3) in greater than half of the content.

[0015] The above fly ash contains SiO2, Al2O3, CaO, and Fe2O3, and the fly ash may have a content distribution in the order of SiO2, Al2O3, CaO, and Fe2O3.

[0016] The above fly ash may be composed of SiO2, Al2O3, CaO, Fe2O3, MgO, TiO2, P2O5, K2O, Na2O, SO3, SrO, BaO, ZrO2, MnO, V2O5, ZnO, Cr2O3, CuO, NiO, Y2O3, and Ga2O3.

[0017] The above may comprise 55 to 69 wt% of fly ash, 20 wt% of calcium hydroxide, 10 wt% of sodium carbonate, and 1 to 5 wt% of boron compound, wherein the sucrose may be included in an amount of 0.6 parts by weight relative to a total of 100 parts by weight of the fly ash, calcium hydroxide, and sodium carbonate.

[0018] The above boron compound may be boric acid (H3BO3) or borax (Na2B4O7).

[0020] In addition, a method for manufacturing neutron-shielding artificial lightweight aggregate according to one embodiment of the present invention comprises fly ash; calcium hydroxide (Ca(OH)2); sodium carbonate (Na2CO3), a boron compound and sucrose (C 12 H 22 O 11The method includes the step of preparing 100 parts by weight of a mixture of ) mixed; the first pelletizing step of introducing 90 parts by weight of the mixture and 27 parts by weight of water onto a disk pelletizer; the second pelletizing step of adding 10 parts by weight of the mixture onto the disk pelletizer; and the third pelletizing step of adding 3 parts by weight of water onto the disk pelletizer.

[0021] The above fly ash may consist of silicon dioxide (SiO2) and aluminum oxide (Al2O3) in greater than half of the content.

[0022] The above fly ash contains SiO2, Al2O3, CaO, and Fe2O3, and the fly ash may have a content distribution in the order of SiO2, Al2O3, CaO, and Fe2O3.

[0023] The above fly ash may be composed of SiO2, Al2O3, CaO, Fe2O3, MgO, TiO2, P2O5, K2O, Na2O, SO3, SrO, BaO, ZrO2, MnO, V2O5, ZnO, Cr2O3, CuO, NiO, Y2O3, and Ga2O3.

[0024] The above mixture comprises 55 to 69 wt% of the fly ash, 20 wt% of the calcium hydroxide, 10 wt% of the sodium carbonate, and 1 to 5 wt% of the boron compound, and the sucrose may be included in an amount of 0.6 parts by weight per 100 parts by weight of the total of the fly ash, the calcium hydroxide, and the sodium carbonate.

[0025] The above boron compound may be boric acid (H3BO3) or borax (Na2B4O7). Effects of the invention

[0026] The present invention has the effect of providing a cement-free binder-based artificial aggregate that can be cured at low temperatures without using a rotary kiln, using coal ash (fly ash), a byproduct generated from thermal power plants, etc.

[0027] In addition, the present invention has the effect of providing a high-strength cement-free binder that does not cause problems even when containing neutron shielding material.

[0028] In addition, the present invention has the effect of providing an artificial lightweight aggregate that can maintain a barometer shielding material by manufacturing and curing under low-temperature conditions.

[0029] The technical effects of the present invention are not limited to those mentioned above, and other unmentioned technical effects will be clearly understood by those skilled in the art from the description below. Brief explanation of the drawing

[0030] Figure 1 illustrates the particle size analysis results of fly ash according to one embodiment of the present invention. Figure 2 illustrates the results of measuring the aggregate crushing rate and crushing load of artificial lightweight aggregate according to one embodiment of the present invention. Figure 3 illustrates the results of an analysis of the wear rate of artificial lightweight aggregate according to one embodiment of the present invention. Figure 4 illustrates the XRD analysis results of an artificial lightweight aggregate according to one embodiment of the present invention. Figure 5 illustrates the boron leaching test analysis results of artificial lightweight aggregate according to one embodiment of the present invention. Figure 6 illustrates the results of a compressive strength analysis of artificial lightweight aggregate according to one embodiment of the present invention. Figure 7 shows the results of the compressive strength analysis of Portland cement. FIG. 8 illustrates the results of a compressive strength analysis of concrete according to one embodiment of the present invention. Specific details for implementing the invention

[0031] The embodiments of the present invention are to be described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein. Additionally, throughout the specification, the same reference numerals denote the same components.

[0033] An artificial lightweight aggregate according to one embodiment of the present invention is based on fly ash, and by using fly ash, it can replace conventional Portland cement and provide a carbon-reducing artificial lightweight aggregate based on a cement-free binder. In addition, by simultaneously using a boron compound, it can provide an artificial lightweight aggregate for neutron shielding.

[0035] A neutron-shielding artificial lightweight aggregate according to one embodiment of the present invention comprises fly ash; calcium hydroxide (Ca(OH)2); sodium carbonate (Na2CO3), boron compounds and sucrose (C 12 H 22 O 11 Includes ).

[0036] The above fly ash may be composed of silicon dioxide (SiO2) and aluminum oxide (Al2O3) as the main materials, and more specifically, the above fly ash may be composed of silicon dioxide (SiO2) and aluminum oxide (Al2O3) accounting for more than half of the total fly ash content.

[0037] In addition, the fly ash may contain SiO2, Al2O3, CaO, and Fe2O3, wherein the fly ash may have a content distribution in the order of SiO2, Al2O3, CaO, and Fe2O3, and the fly ash may have a content in the order of SiO2, Al2O3, CaO, and Fe2O3.

[0038] More specifically, the fly ash may be composed of SiO2, Al2O3, CaO, Fe2O3, MgO, TiO2, P2O5, K2O, Na2O, SO3, SrO, BaO, ZrO2, MnO, V2O5, ZnO, Cr2O3, CuO, NiO, Y2O3, and Ga2O3, and as an example, the fly ash may have the composition of Table 1 below.

[0040] The above may comprise 55 to 69 wt% of fly ash, 20 wt% of calcium hydroxide, 10 wt% of sodium carbonate, and 1 to 5 wt% of boron compound, wherein the sucrose may be included in an amount of 0.6 parts by weight relative to a total of 100 parts by weight of the fly ash, calcium hydroxide, and sodium carbonate.

[0041] The above boron compound may be boric acid (H3BO3) or borax (Na2B4O7).

[0043] In addition, a method for manufacturing neutron-shielding artificial lightweight aggregate according to one embodiment of the present invention comprises fly ash; calcium hydroxide (Ca(OH)2); sodium carbonate (Na2CO3), a boron compound and sucrose (C 12 H 22 O 11 The method includes the step of preparing 100 parts by weight of a mixture of ) mixed; the first pelletizing step of introducing 90 parts by weight of the mixture and 27 parts by weight of water onto a disk pelletizer; the second pelletizing step of adding 10 parts by weight of the mixture onto the disk pelletizer; and the third pelletizing step of adding 3 parts by weight of water onto the disk pelletizer.

[0044] The above fly ash may consist of silicon dioxide (SiO2) and aluminum oxide (Al2O3) in greater than half of the content.

[0045] The above fly ash contains SiO2, Al2O3, CaO, and Fe2O3, and the fly ash may have a content distribution in the order of SiO2, Al2O3, CaO, and Fe2O3.

[0046] The above fly ash may be composed of SiO2, Al2O3, CaO, Fe2O3, MgO, TiO2, P2O5, K2O, Na2O, SO3, SrO, BaO, ZrO2, MnO, V2O5, ZnO, Cr2O3, CuO, NiO, Y2O3, and Ga2O3.

[0047] The above mixture comprises 55 to 69 wt% of the fly ash, 20 wt% of the calcium hydroxide, 10 wt% of the sodium carbonate, and 1 to 5 wt% of the boron compound, and the sucrose may be included in an amount of 0.6 parts by weight per 100 parts by weight of the total of the fly ash, the calcium hydroxide, and the sodium carbonate.

[0048] The above boron compound may be boric acid (H3BO3) or borax (Na2B4O7).

[0050] The above pelletizing step is a process of sphericalizing the mixture while rotating the disk pelletizer. The first pelletizing may be performed for 2 to 4 minutes, the second pelletizing may be performed for 5 to 8 minutes, and the third pelletizing may be performed for 5 to 8 minutes.

[0052] The present invention will be described in detail below through examples. The following examples are merely for understanding the present invention and are not intended to limit the invention.

[0054] Preparation Example 1. Preparation of Fly Ash

[0055] Fly ash (coal ash) having the composition of Table 1 below was prepared.

[0056] Fly ash Oxide Weight % SiO2 48.94 Al2O3 26.57 CaO 8.25 Fe2O3 7.22 MgO 1.58 TiO2 1.56 P2O5 1.45 K2O 1.30 Na2O 1.23 SO3 1.06 SrO 0.26 BaO 0.26 ZrO2 0.08 MnO 0.08 V2O5 0.05 ZnO 0.02 Cr2O3 0.02 CuO 0.02 NiO 0.02 Y2O3 0.01 Ga2O3 0.01 Sum 99.99

[0058] Experimental Example 1. Particle Size Analysis

[0059] Figure 1 shows the particle size analysis results of the fly ash from Preparation Example 1 above and Portland cement having the composition of Table 2 below. Figure 1 (a) shows the particle size analysis results of the fly ash from Preparation Example 1 above. Figure 1 (b) shows the particle size analysis results of Portland cement having the composition of Table 2 below.

[0060] Portland cement Oxide Weight % CaO 65.40 SiO2 17.15 Al2O3 4.33 MgO 3.64 SO3 3.55 Fe2O3 3.53 K2O 1.19 TiO2 0.34 P2O5 0.19 MnO 0.18 Na2O 0.16 ZnO 0.11 etc. 0.23 Total 100

[0062] Referring to Fig. 1, and looking at the density distribution and cumulative distribution, it can be seen that both fly ash (Preparation Example 1) and Portland cement have particle size distributions of similar trends.

[0064] Example. Manufacture of artificial lightweight aggregate

[0065] To a premixture prepared by mixing fly ash, Ca(OH)2, Na2CO3, and a boron compound (H3BO3 or Na2B4O7) from Preparation Example 1 having the composition of Table 3 below, 0.6 parts by weight of sucrose (sugar, C) per 100 parts by weight of the premixture. 12 H 22 O 11After preparing 1000 g of the mixture by adding ), 900 g of the mixture and 270 g of water are placed on a disc pelletizer (disk diameter: 400 mm, disc depth: 120 mm) at an inclination angle of 50° and a rotation speed of 46 rpm at room temperature (25 ℃), then rotated for 3 minutes (1st pelletizing), then 100 g of the mixture is added and rotated for 5 minutes (2nd pelletizing), then 30 g of water is added and rotated for 5 minutes (3rd pelletizing), and then cured at 90 ℃ for a total of 3 days.

[0066] division Fly ash (Preparation Example 1) (wt%) Ca(OH) 2 (wt%) Na 2 CO 3 (wt%) H 3 BO 3 (wt%) Na 2 B 4 O 7 (wt%) C 12 H 22 O 11 (Weight portion) Example 1 76.3 15.3 8.4 - - 0.6 Example 2 71.3 15.3 8.4 5 - 0.6 Example 3 71.3 15.3 8.4 - 5 0.6

[0068] Comparative Example 1. Preparation of general crushed stone aggregate

[0069] As a comparative example, commercially available general crushed stone aggregate was prepared. The prepared general crushed stone aggregate conformed to the ACI 211.1 standard, with a fineness modulus of 7.26, a surface-dry internal saturated specific gravity (SSD) of 2.68, a water absorption of 0.78%, and a unit weight of 1,601 kg / m³. 3 The maximum coarse aggregate size is 19 mm.

[0071] Experimental Example 2. Physical properties

[0072] For the general crushed stone aggregate of Comparative Example 1 and the artificial lightweight aggregates prepared in Examples 1, 2, and 3, the aggregate crushing value according to BS 812 part 110 and the 10 percent fines value according to BS 812 part 111 were measured and are shown in FIG. 2. In FIG. 2, "Crushed-agg" is the general crushed stone aggregate of Comparative Example 1, "CNF-agg" is the artificial lightweight aggregate prepared in Example 1, "CNF-HB-agg" is the artificial lightweight aggregate prepared in Example 2, and "CNF-BX-agg" is the artificial lightweight aggregate prepared in Example 3.

[0073] Referring to FIG. 2, it can be seen that the artificial lightweight aggregates produced in Examples 1, 2, and 3 have performance equivalent to that of general crushed stone aggregates.

[0075] The Los Angeles abrasion resistance test according to ASTM C 131 was performed on the general crushed stone aggregate of Comparative Example 1 and the artificial lightweight aggregates prepared in Examples 1, 23, and 3, and the results are shown in FIG. 3. In FIG. 3, "Crushed-agg" is the general crushed stone aggregate of the Comparative Example, "CNF-agg" is the artificial lightweight aggregate prepared in Example 1, "CNF-HB-agg" is the artificial lightweight aggregate prepared in Example 2, and "CNF-BX-agg" is the artificial lightweight aggregate prepared in Example 3.

[0076] Referring to Fig. 3, it can be seen that the artificial lightweight aggregates produced in Examples 1, 2, and 3 have an abrasion rate of 40% or less.

[0078] Various physical property values ​​were measured for the artificial lightweight aggregates prepared in Examples 2 and 3 above and summarized in Table 4 below.

[0079] division Example 2 Example 3 Dry specific gravity 1.446 1.491 Standard specific gravity 1.79 1.785 True specific gravity 2.206 2.112 Dry density (g / cm³) 3 ) 1.441 1.486 Loose bulk density (kg / cm³) 3 ) 671.705 726.454 Absorption rate (%) 23.829 19.75 Porosity (%) 53.541 51.26 Performance rate (%) 46.459 48.740

[0081] Referring to Table 4, it can be seen that the dry density (Ministry of Land, Infrastructure and Transport Concrete Standard Specification) and loose bulk density (ASTM C 330) satisfy their respective standards.

[0083] Experimental Example 3. XRD Analysis

[0084] XRD (X-ray Diffraction) analysis was performed on the general crushed stone aggregate of Comparative Example 1 and the artificial lightweight aggregates prepared in Examples 1, 2, and 3, respectively, and the analysis results are shown in Fig. 4. In Fig. 4, "Crushed-agg" is the general crushed stone aggregate of Comparative Example 1, "CNF-agg" is the artificial lightweight aggregate prepared in Example 1, "CNF-HB-agg" is the artificial lightweight aggregate prepared in Example 2, and "CNF-BX-agg" is the artificial lightweight aggregate prepared in Example 3.

[0085] Quantitative XRD analysis using Rietveld-RIR (reference-intensity-ratio) was performed to measure crystallinity, and 10 wt% of Corundum (NIST SRM 676a) was included as internal standard reference materials to normalize after rescaling based on the absolute amount of Corundum.

[0087] The results of the XRD quantitative analysis of the general crushed stone aggregate of Comparative Example 1, and the artificial lightweight aggregates prepared in Example 2 and Example 3 are summarized in Table 5 below.

[0088] Phase Reference Number Content (%) Comparative Example 1 Example 2 Example 3 Quartz 98-008-9277 26.7 11.7 11.9 Andesine 98-006-6240 45.9 Biotite 98-004-1304 10.1 Clinochlore 98-006-3193 5.2 Mullite 98-015-8098 18.1 18.1 Calcite 98-005-2151 27.4 30.1 Corundum 01-076-0144 12.1 42.8 39.9 Total sum 100 100 100 Crystalline 82.64 23.36 25.06 Amorphous 17.36 76.64 74.94

[0090] Referring to Figure 4 and Table 5, it can be seen that the artificial lightweight aggregates prepared in Examples 2 and 3 have an amorphous phase.

[0092] Experimental Example 4. Analysis of Heavy Metal Leaching (TCLP, Toxicity Characteristic Leaching Procedure) Test

[0093] The artificial lightweight aggregate (sample) prepared in Examples 2 and 3 above was subjected to a TCLP test under the conditions of Table 6 below, and the results are summarized in Table 7 below.

[0094] Test conditions TCLP method Sample pretreatment Grind to 9.5 mm or less Shaking device Magnetic stirring device Concussion time 18 hours (hr) pH of the solvent 4.93±0.05 Solvent: Sample Ratio (w:w) 20:1 High-value separation 0.6 to 0.8 µm membrane filter

[0096] element Standard value Detected heavy metal concentration (ppm) Example 2 Example 3 Arsenic(As) 5.0 0.001 0.001 Cadmium(Cd) 1.0 ND ND Chrmium(Cr) 5.0 ND ND Mercury(Hg) 0.2 0.001 0.001 Lead(Pb) 5.0 ND ND

[0098] Experimental Example 5. Boron Leaching Test Analysis

[0099] A boron leaching test was performed on the artificial lightweight aggregates (samples) prepared in Examples 2 and 3 above, and the results are summarized in Table 7 below and illustrated in Fig. 5. In Fig. 5, “CNF-HB-agg” is the artificial lightweight aggregate prepared in Example 2 above, and “CNF-BX-agg” is the artificial lightweight aggregate prepared in Example 3 above.

[0100] For the boron leaching test, 1.00 kg of the artificial lightweight aggregate prepared in Examples 2 and 3 above was prepared, and the weight ratio of water at 25°C to the artificial lightweight aggregate was set to 15 (water) : 1 (artificial lightweight aggregate). After immersion in water for 1 hour, 1 day, 1 week, and 1 month, the amount of boron leached was calculated using ICP-OES after each immersion period, and the results are shown in Fig. 5.

[0101] In Figure 5, the amount of boron leached after 1 month of immersion (Boron concentration at 1 month) and leaching ability were calculated and summarized in Table 8 below.

[0102] division Example 2 Example 3 Boron content in 1 kg of agg (mg) 6694.15 8227.79 Boron concentration at 1 month (mg / L) 3.81 2.87 Volume of leachate (L) 15.05 15.05 Total leached boron amount (mg) 57.32 43.18 Leachability(%) 0.86 0.52

[0104] Experimental Example 6. Analysis of Compressive Strength of Artificial Lightweight Aggregate

[0105] Figure 6 shows the results of the compressive strength analysis for the artificial lightweight aggregate produced in the above example according to curing time (curing date) of 1 day (1d), 3 days (3d) (curing time in the example), and 7 days (7d). In Figure 6, Example 1 is labeled "CNF", Example 2 is labeled "CNF-BX 5%", and Example 3 is labeled "CNF-BX 5%".

[0106] Referring to Fig. 6, it can be seen that the artificial aggregates of Example 2 and Example 3, in which the input amounts of boric acid (H3BO3) and borax (Na2B4O7) are 5 wt%, both develop a strength of 30 MPa or more after 3 days of curing (curing time in the examples), and it can be seen that both boric acid (H3BO3) and borax (Na2B4O7) can be incorporated up to 15 wt%.

[0108] Meanwhile, the compressive strength analysis results for Portland cement mixed with boron compounds according to the composition of Table 9 below, based on curing dates of 1 day (1d), 3 days (3d), and 7 days (7d), are shown in Fig. 7.

[0109] division Portland Cement (wt%) H 3 CO 3 (wt%) Na 2 B 4 O 7 (wt%) PC 100 - - PC-HB 5% 95 5 - PC-HX 5% 95 - 5

[0110] Referring to Figure 7, it can be seen that in the case of Portland cement, direct mixing of boron results in inhibition of setting time and a decrease in compressive strength due to the delay in setting time.

[0112] Application Example. Concrete Mix Design

[0113] In Examples 1, 2, and 3 above, concrete was mixed using artificial lightweight aggregates according to the mixing ratios in Table 10 below, and a standard concrete mix was used as a control group. The concrete was mixed to achieve a design strength of 40 MPa, a target slump of 100 ± 10 mm, and trapped air of 2 ± 1%. In particular, admixtures such as water reducers and air-entraining agents were not used for accurate neutron shielding experiments of the artificial aggregates.

[0114] Unit: kg / m² 3 water Portland Cement Coarse aggregate Fine aggregate (Fine aggregate) Crushed-agg Example 1 Example 2 Example 3 Control group (regular concrete) 183.92 459.79 1000.19 733.49 Application Example 1 183.92 459.79 581.55 715.89 Application Example 2 183.92 459.79 515.71 777.37 Application Example 3 183.92 459.79 539.37 736.84

[0115] In Table 10 above, Type 1 Portland cement was used. In Table 9 above, both the coarse aggregate (Comparative Example 1) and the fine aggregate conformed to the ACI 211.1 standard; as for the coarse aggregate, Comparative Example (Crushed-agg) had a fineness modulus of 7.26, a surface-dry internal saturated specific gravity (SSD) of 2.68, a water absorption of 0.78%, and a unit weight of 1,601 kg / m³. 3 The maximum coarse aggregate size is 19 mm. In Table 6 above, sand was used as the fine aggregate, and the sand has a fineness modulus of 2.80, a surface-dry internal saturated specific gravity (SSD) of 2.65, and a water absorption of 1.01%.

[0117] Experimental Example 7. Analysis of Concrete Compressive Strength

[0118] Compressive strength analysis was performed on the concrete of the control group and application examples mixed using the mix ratios of Table 10 above, and the results of the compressive strength analysis are shown in Fig. 8. In Fig. 8, the compressive strength of the concrete of the control group is indicated as "CA-con", the compressive strength of the concrete of application example 1 is indicated as "CNF-con", the compressive strength of the concrete of application example 2 is indicated as "CNF-HB-con", and the compressive strength of the concrete of application example 2 is indicated as "CNF-BX-con". The concrete compressive strength was measured according to ASTM C 39 using 100 x 200 mm cylinder specimens, which were prepared and used for compressive strength measurement after 7 and 28 days of curing.

[0119] Referring to FIG. 8, it can be seen that the concrete of Application Examples 1 to 3, in which the artificial lightweight aggregates prepared in Examples 1, 2, and 3 were used as coarse aggregates, satisfies both ACI 213 (17 MPa for 28-day compressive strength of concrete) and KS F 2527 (27 MPa for compressive strength of concrete).

[0121] Experimental Example 8. Analysis of Neutron Shielding Experiment Results

[0122] Rectangular specimens measuring 150 x 150 x 50 mm were prepared from the concrete manufactured in the above application example, and neutron shielding performance was measured after 28 days of curing. The neutron shielding performance is 241 Am-Be (neutron energy emission rate: 1.227 x 10⁻⁶ 7 s -1 ) was used as a neutron source, and the experiment was conducted after placing the source inside a high-purity graphite block to slow down fast neutrons into thermal neutrons. An SP9 3He proportional counter was used for thermal neutron detection, and the thermal neutron shielding rate was calculated using Equation 1 below.

[0123] [Equation 1]

[0124]

[0125] In the above Equation 1, S th Thermal neutron counting rate passing through the specimen(s -1 ) and, R air Thermal neutron counting rate at air without the specimen(s -1 )am.

[0126] The results of the neutron shielding performance analysis performed in this experimental example are summarized in Table 11 below. In Table 11, U R is the relative uncertainty (%).

[0127] Label Thermal Neutron Counting Rate, s -1 Shielding Efficiency, % (U R ) Air 78.59 - control group 15.77 79.93 (0.24) Application Example 2 2.68 96.59 (0.04) Application Example 3 0.54 99.31 (0.02)

[0128] Referring to Table 11, significantly high neutron shielding rates of 99.31% and 96.59% were confirmed, and consequently, it can be confirmed that cement-free amorphous artificial lightweight aggregates with neutron shielding performance can be provided. Through this, it is expected that artificial lightweight aggregates can be used not only in nuclear facilities but also in all concrete structures requiring neutron shielding performance.

[0130] Although preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concept of the present invention as defined in the following claims also fall within the scope of the present invention.

Claims

Claim 1 Fly ash; calcium hydroxide (Ca(OH)2); sodium carbonate (Na2CO3), boron compounds and sucrose (C 12 H 22 O 11 Neutron-shielding artificial lightweight aggregate comprising ), wherein the fly ash contains silicon dioxide (SiO2) and aluminum oxide (Al2O3) in greater than half of the content, and the boron compound is borax (Na2B4O7). Claim 2 A neutron-shielding artificial lightweight aggregate according to claim 1, wherein the fly ash comprises SiO2, Al2O3, CaO, and Fe2O3. Claim 3 In paragraph 2, the neutron-shielding artificial lightweight aggregate is such that the fly ash has a content distributed in the order of SiO2, Al2O3, CaO, and Fe2O3. Claim 4 A neutron-shielding artificial lightweight aggregate according to claim 1, wherein the fly ash is composed of SiO2, Al2O3, CaO, Fe2O3, MgO, TiO2, P2O5, K2O, Na2O, SO3, SrO, BaO, ZrO2, MnO, V2O5, ZnO, Cr2O3, CuO, NiO, Y2O3, and Ga2O3. Claim 5 A neutron-shielding artificial lightweight aggregate according to claim 1, comprising 55 to 69 wt% of fly ash, 20 wt% of calcium hydroxide, 10 wt% of sodium carbonate, and 1 to 5 wt% of a boron compound, wherein the sucrose is included in an amount of 0.6 parts by weight per 100 parts by weight of the total of fly ash, calcium hydroxide, and sodium carbonate. Claim 6 delete Claim 7 Fly ash; calcium hydroxide (Ca(OH)2); sodium carbonate (Na2CO3), boron compounds and sucrose (C 12 H 22 O 11 A method for manufacturing neutron-shielding artificial lightweight aggregate comprising: a step of preparing 100 parts by weight of a mixture of ) mixed; a first pelletizing step of introducing 90 parts by weight of the mixture and 27 parts by weight of water onto a disk pelletizer; a second pelletizing step of adding 10 parts by weight of the mixture onto the disk pelletizer; and a third pelletizing step of adding 3 parts by weight of water onto the disk pelletizer, wherein the fly ash comprises silicon dioxide (SiO2) and aluminum oxide (Al2O3) in a majority content, and the boron compound is borax (Na2B4O7). Claim 8 A method for manufacturing neutron-shielding artificial lightweight aggregate according to claim 7, wherein the fly ash comprises SiO2, Al2O3, CaO, and Fe2O3. Claim 9 A method for manufacturing neutron-shielding artificial lightweight aggregate according to claim 8, wherein the fly ash is distributed in the order of SiO2, Al2O3, CaO, and Fe2O3. Claim 10 A method for manufacturing neutron-shielding artificial lightweight aggregate according to claim 7, wherein the fly ash is composed of SiO2, Al2O3, CaO, Fe2O3, MgO, TiO2, P2O5, K2O, Na2O, SO3, SrO, BaO, ZrO2, MnO, V2O5, ZnO, Cr2O3, CuO, NiO, Y2O3, and Ga2O3. Claim 11 A method for manufacturing neutron-shielding artificial lightweight aggregate according to claim 7, wherein the mixture comprises 55 to 69 wt% of the fly ash, 20 wt% of the calcium hydroxide, 10 wt% of the sodium carbonate, and 1 to 5 wt% of the boron compound, and wherein the sucrose is included in an amount of 0.6 parts by weight per 100 parts by weight of the total of the fly ash, the calcium hydroxide, and the sodium carbonate. Claim 12 delete

Citation Information

Patent Citations

  • Radiation protective concrete and radiation protectivecasing

    KR1020010079675A

  • Cementless binder comprising initial setting time retarder and preparation method thereof

    KR1020160066467A