Non-oriented electrical steel sheet and method of producing same
By controlling Co content and applying acid treatment to form an oxide layer, the method enhances non-oriented electrical steel sheets' magnetic properties, reducing iron loss without compromising flux density or productivity.
Patent Information
- Application Number
- KR1020247024352
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-02
- Filing Date
- 2023-01-23
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-01-23
AI Technical Summary
Existing non-oriented electrical steel sheets face challenges in achieving high magnetic flux density and low iron loss in the high-frequency range without adding alloying elements that lower flux density or through processes that reduce productivity.
Control the amount of Co in the steel to a predetermined range and apply an acid treatment after final annealing to control nitrogen in the surface layer, forming an oxide layer that reduces iron loss without affecting magnetic flux density or productivity.
The method achieves reduced iron loss in the high-frequency range without decreasing magnetic flux density and maintains productivity by controlling nitrogen through acid treatment, eliminating the need for additional alloying elements and processes like skin pass rolling.
Smart Images

Figure 112024078452556-PCT00010_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a non-oriented electrical steel sheet and a method for manufacturing the same. Background Technology
[0002] Recently, due to environmental concerns such as global warming, there is a growing demand for energy conservation. Consequently, the automotive sector is seeing the development of hybrid electric vehicles (HEVs) that combine engines and motors, electric vehicles (EVs) driven solely by electric motors, and fuel cell vehicles (FCEVs). To enhance efficiency, the motors used in these vehicles are generally operated in the high-frequency range, which is advantageous for high-speed rotation. Non-oriented electrical steel is widely used as the iron core material for the drive motors of these HEVs and EVs, and to achieve high motor efficiency, there is a strong demand for non-oriented electrical steel to reduce iron loss in the high-frequency range.
[0003] The reduction of iron loss in non-oriented electrical steel sheets has conventionally been achieved primarily by adding alloying elements such as Si or Al to increase resistivity, or by reducing eddy current loss by thinning the sheet thickness. However, adding a large amount of alloying elements to reduce iron loss results in a decrease in saturation magnetic flux density. A decrease in magnetic flux density leads to an increase in copper loss in motors, which in turn leads to a decrease in motor efficiency. Furthermore, reducing the thickness of non-oriented electrical steel sheets requires thinning the thickness of the hot-rolled steel sheet or increasing the cold-rolling reduction ratio during the manufacturing process, which lowers productivity.
[0004] Therefore, it is believed that developing non-oriented electrical steel sheets that combine high magnetic flux density and low iron loss in the high-frequency range, while also offering excellent productivity, would significantly contribute to the high efficiency of electrical equipment.
[0005] As a method for achieving low iron loss in the high frequency range, for example, Patent Document 1 discloses a method of achieving low iron loss in the high frequency range by increasing the intrinsic resistance of steel by adding 1.5 to 20 mass% of Cr.
[0006] Meanwhile, stress relief annealing is sometimes performed on non-oriented electrical steel sheets. For example, when non-oriented electrical steel sheets are used for the stator core of a motor, etc., stress relief annealing is performed to release the deformation introduced during processing after processing into a core shape by punching, etc.
[0007] Therefore, for example, in Patent Document 2, a technique is proposed to improve magnetic properties after strain relief annealing by performing skin pass rolling after final annealing and then strain relief annealing. Prior art literature
[0008] Japanese Published Patent Application No. Hei 11-343544, Japanese Published Patent Application No. 2006-265720 The problem to be solved
[0009] However, since Cr is an element that lowers saturation magnetic flux density, the technology disclosed in Patent Document 1, which requires the addition of a large amount of Cr, cannot achieve both high magnetic flux density and low iron loss at high frequency.
[0010] In addition, in the technology proposed in Patent Document 2, additional skin pass rolling is required, which reduces productivity and leads to an increase in manufacturing costs.
[0011] The present invention is made in consideration of the above-mentioned facts and aims to provide a non-oriented electrical steel sheet with reduced iron loss in the high-frequency range without adding a large amount of alloying elements such as Cr that lower magnetic flux density, and without performing skin pass rolling that lowers productivity. means of solving the problem
[0012] To solve the above problem, the inventors focused on the influence of surface conditions on the magnetic properties of non-oriented electrical steel sheets and conducted repeated investigations. As a result, they discovered that by controlling the amount of Co contained in the steel to a predetermined range, and then applying an acid treatment to the steel sheet after final annealing and before strain relief annealing to control the amount of nitrogen in the surface layer to a predetermined range, iron loss can be reduced without causing a decrease in magnetic flux density.
[0013] The present invention is completed based on the above recognition, and its gist is as follows.
[0014] 1. In mass %,
[0015] C: 0.0050% or less,
[0016] Si: 2.0–6.5%,
[0017] Mn: 0.05∼2.0%,
[0018] P: 0.10% or less,
[0019] S: 0.0050% or less,
[0020] Al: 0.3~3.0%,
[0021] N: 0.0050% or less,
[0022] Co: 0.0005∼0.0050%,
[0023] Ti: 0.0030% or less,
[0024] Nb: 0.0030% or less and,
[0025] O: Contains 0.0050% or less, and
[0026] It has a composition in which the remainder consists of Fe and unavoidable impurities,
[0027] At least on one surface, in the range from the surface to a depth of 1 / 20 of the plate thickness, the amount of N present as AlN is 0.003 mass% or less, and
[0028] On the above surface, an oxide layer containing one or both of Fe, Al, and Si,
[0029] A non-oriented electrical steel sheet having an oxide film composed of one or both of Al oxide and Si oxide at the interface between the oxide layer and the steel substrate.
[0030] 2. A non-oriented electrical steel sheet described in 1, wherein the above component composition additionally contains, in mass%, one or more groups from A to F below.
[0031] Group A: Sn: 0.005–0.20% and, Sb: 0.005–0.20%, either or both
[0032] Group B: At least one selected from the group consisting of Ca, Mg, and REM, in a total of 0.0005–0.020%
[0033] Group C: At least one selected from the group consisting of Cu, Cr, and Ni, in total of 0.03 to 1.0%
[0034] Group D: One or both of Ge and Ga, total 0.0005–0.01%
[0035] Group E: Zn: 0.001∼0.05%
[0036] Group F: One or both of Mo and W, total 0.001–0.05%
[0037] 3. In mass %,
[0038] C: 0.0050% or less,
[0039] Si: 2.0–6.5%,
[0040] Mn: 0.05∼2.0%,
[0041] P: 0.10% or less,
[0042] S: 0.0050% or less,
[0043] Al: 0.3~3.0%,
[0044] N: 0.0050% or less,
[0045] Co: 0.0005∼0.0050%,
[0046] Ti: 0.0030% or less,
[0047] Nb: 0.0030% or less and,
[0048] O: Contains 0.0050% or less, and
[0049] A steel material having a composition in which the remainder consists of Fe and unavoidable impurities is subjected to one cold rolling or two or more cold rollings with intermediate annealing in between to produce a cold-rolled steel sheet, and
[0050] A method for manufacturing a non-oriented electrical steel sheet by performing finish annealing and deformation removal annealing on the above cold-rolled steel sheet,
[0051] The above deformation removal annealing is performed under conditions of a cracking temperature of 750℃ to 950℃ and a nitrogen content in the atmosphere of 50 volume% or more, and
[0052] A method for manufacturing a non-oriented electrical steel sheet, wherein, after the above-mentioned finishing annealing and before the above-mentioned deformation removal annealing, an acid treatment is performed on the surface of the steel sheet for 1 to 60 seconds using an acid containing at least one selected from the group consisting of hydrochloric acid, phosphoric acid, sulfuric acid, and nitric acid at a total concentration of 3 to 30 weight%.
[0053] 4. Prior to the above cold rolling, the steel material is hot-rolled to form a hot-rolled steel sheet, and
[0054] The above hot-rolled steel plate is subjected to hot-rolled plate annealing to become a hot-rolled annealed plate, and
[0055] A method for manufacturing a non-oriented electrical steel sheet as described in 3, wherein the hot-rolled annealed sheet is provided to the cold-rolled sheet.
[0056] 5. A method for manufacturing a non-oriented electrical steel sheet as described in 3 or 4, wherein the above component composition additionally contains, in mass%, one or more groups from A to F below.
[0057] Group A: Sn: 0.005–0.20% and, Sb: 0.005–0.20%, either or both
[0058] Group B: At least one selected from the group consisting of Ca, Mg, and REM, in a total of 0.0005–0.020%
[0059] Group C: At least one selected from the group consisting of Cu, Cr, and Ni, in total of 0.03 to 1.0%
[0060] Group D: One or both of Ge and Ga, total 0.0005–0.01%
[0061] Group E: Zn: 0.001∼0.05%
[0062] Group F: One or both of Mo and W, total 0.001–0.05% Effects of the invention
[0063] According to the present invention, it is possible to provide a non-oriented electrical steel sheet with reduced iron loss in the high-frequency range without causing a decrease in magnetic flux density or productivity. Specifically, since the present invention enables low iron loss at high frequencies by adding a small amount of Co and controlling the amount of nitrogen in the surface layer through acid treatment, there is no need to add large amounts of alloying elements such as Cr, which reduce magnetic flux density. Furthermore, excellent magnetic properties can be achieved without performing skin pass rolling, which causes a decrease in productivity. In addition, while skin pass rolling requires the installation of new skin pass rolling equipment, acid treatment can be performed using cleaning equipment already installed in a general steel sheet manufacturing line, thus not compromising productivity. Brief explanation of the drawing
[0064] Figure 1 shows the Co content and high-frequency iron loss (W 10 / 400 This is a graph showing the correlation with ). Figure 2 shows the surface nitriding amount and high-frequency iron loss (W 10 / 400 This is a graph showing the correlation with ). Figure 3 shows acid concentration and high-frequency iron loss (W 10 / 400 This is a graph showing the correlation with ). Figure 4 is a graph showing the correlation between acid concentration and surface nitrification amount. Figure 5 shows the acid treatment time and high-frequency iron loss (W 10 / 400 This is a graph showing the correlation with ). Figure 6 is a graph showing the correlation between acid treatment time and surface nitridation amount. Specific details for implementing the invention
[0065] (Form for carrying out the invention)
[0066] First, the experiment that served as the impetus for developing the present invention will be described. Furthermore, in this specification, "%" as a unit of content shall refer to "mass%" unless otherwise specified. Additionally, the unit of acid concentration shall be "weight%".
[0067] Experiment 1
[0068] Multiple non-oriented electrical steel sheets with different Co contents were produced in the following order, and the iron loss of the obtained non-oriented electrical steel sheets in the high-frequency range was evaluated.
[0069] A steel containing C: 0.0019%, Si: 3.1%, Mn: 0.8%, P: 0.01%, S: 0.0015%, Al: 0.9%, N: 0.0018%, Ti: 0.0010%, Nb: 0.0008%, and O: 0.0021%, with Co in the range of 0.0001 to 0.01%, and the remainder being Fe and unavoidable impurities, was melted in a vacuum furnace and cast to form a steel ingot. The above steel ingot was hot-rolled to form a hot-rolled steel sheet with a thickness of 2.0 mm, and the above hot-rolled steel sheet was subjected to hot-rolled annealing at 960°C × 30 sec to form a hot-rolled annealed sheet. After acid cleaning the above hot-rolled annealed plate, it was cold-rolled to obtain a cold-rolled steel plate with a final thickness of 0.25 mm.
[0070] The obtained cold-rolled steel sheet was subjected to finish annealing at 850°C for 10 seconds under an atmosphere of H2:N2 = 20:80 by volume%, followed by acid treatment. In the acid treatment, the steel sheet was immersed in 10% hydrochloric acid for 10 seconds. Subsequently, strain relief annealing was performed under conditions of 850°C for 2 hours and a nitrogen content in the atmosphere of 100 volume%, thereby obtaining a non-oriented electrical steel sheet.
[0071] A test specimen measuring 30 mm in width × 180 mm in length was cut from the rolling direction (L direction) and width direction (C direction) of the non-oriented electrical steel sheet obtained in the above sequence, and the high-frequency iron loss of the test specimen was evaluated. Specifically, the iron loss W in the (L+C) direction of the test specimen at a maximum magnetic flux density of 1.0 T and a frequency of 400 Hz is 10 / 400 ...was measured using the Epstein test. The Co content and the measured W 10 / 400 The correlation with is shown in Figure 1.
[0072] As can be seen from the results shown in Figure 1, iron loss is significantly reduced in the range of Co content from 0.0005% to 0.0050%.
[0073] To investigate the cause of the reduction in iron loss due to the addition of trace amounts of Co, the rolling direction cross-section of the non-oriented electrical steel sheet prepared in the above experiment was observed using a scanning electron microscope (SEM). As a result, in the non-oriented electrical steel sheet with a Co content outside the range of 0.0005 to 0.0050%, fine AlN precipitation was confirmed in the range from the surface of the steel sheet to a depth of 1 / 20 of the sheet thickness (hereinafter referred to as the surface layer). On the other hand, in the non-oriented electrical steel sheet with a Co content within the range of 0.0005 to 0.0050%, almost no AlN was precipitated in the surface layer.
[0074] Generally, in the manufacturing process of non-oriented electrical steel sheets, nitrogen in the atmosphere diffuses into the interior of the steel sheet during the final annealing, resulting in the formation of nitrides such as AlN in the surface layer (in this way, the surface layer where nitrides are precipitated is sometimes referred to as the nitride layer). However, from the above experimental results, it is thought that in non-oriented electrical steel sheets with a Co content in the range of 0.0005 to 0.0050%, the amount of nitride (AlN) in the surface layer is reduced for some reason, and as a result, iron loss is reduced.
[0075] Therefore, the concentration of N present as AlN (hereinafter referred to as "surface nitridation amount") in the range from the surface of this non-oriented electrical steel sheet to a depth of 1 / 20 of the sheet thickness was analyzed by electrolytic extraction. The measured value of the surface nitridation amount and W 10 / 400 The correlation with is shown in Figure 2.
[0076] As can be seen from the results shown in Figure 2, there is a strong correlation between the surface nitriding amount and iron loss, and in particular, iron loss is significantly reduced when the surface nitriding amount is 0.003% or less. In this regard, as previously mentioned, it can be confirmed that iron loss is reduced by reducing the amount of AlN. Furthermore, all steel sheets with a surface nitriding amount of 0.003% or less had a Co content within the range of 0.0005 to 0.0050%.
[0077] Furthermore, regarding the non-oriented electrical steel sheet in which iron loss reduction was confirmed, observation of the surface using a transmission electron microscope (TEM) revealed that an oxide layer containing one or both of Fe, Al, and Si was formed on the surface of the steel sheet, and an oxide film composed of one or both of Al oxide and Si oxide was formed at the interface between the oxide layer and the base steel. Additionally, further investigation revealed that an oxide layer is formed on the surface of the steel sheet by the acid treatment, and that an oxide film is formed at the interface between the oxide layer and the base steel during the subsequent strain relief annealing.
[0078] From the above experimental results, it is believed that nitridation during strain removal annealing is effectively suppressed by the oxide layer and the oxide film, and as a result, iron loss is reduced.
[0079] Experiment 2
[0080] Next, to evaluate the effect of acid treatment conditions on the magnetic properties of non-oriented electrical steel sheets, acid treatment was performed under various conditions, and the high-frequency iron loss of the obtained non-oriented electrical steel sheets was measured.
[0081] Specifically, first, a steel containing C: 0.0024%, Si: 3.6%, Mn: 0.5%, P: 0.01%, S: 0.0021%, Al: 1.0%, N: 0.0022%, Ti: 0.0011%, Nb: 0.0007%, O: 0.0020%, and Co: 0.0023%, with the remainder being Fe and unavoidable impurities, was melted in a vacuum furnace and cast to form a steel ingot. The steel ingot was hot-rolled to produce a hot-rolled steel sheet with a thickness of 1.8 mm, and the hot-rolled steel sheet was subjected to hot-rolled annealing at 980°C for 30 seconds to produce a hot-rolled annealed sheet. The hot-rolled annealed sheet was acid-cleaned and then cold-rolled to obtain a cold-rolled steel sheet with a final thickness of 0.20 mm.
[0082] The obtained cold-rolled steel sheet was subjected to finish annealing at 950°C for 10 seconds under an atmosphere of H2:N2 = 15:85 by volume% ratio, followed by acid treatment. The acid treatment was performed by immersing the steel sheet in hydrochloric acid for 10 seconds, with the concentration of the hydrochloric acid used varying within the range of 1 to 50%. Subsequently, strain relief annealing was performed under conditions of 800°C for 2 hours and a nitrogen content in the atmosphere of 100 volume%, thereby obtaining a non-oriented electrical steel sheet.
[0083] A test specimen with a width of 30 mm × a length of 180 mm is cut from the rolling direction (L direction) and the width direction (C direction) of the non-oriented electrical steel sheet obtained in the above sequence, and the high-frequency iron loss (W) of the test specimen 10 / 400 ) was evaluated. Specifically, the iron loss W in the (L+C) direction of the above test specimen at a maximum magnetic flux density of 1.0T and a frequency of 400Hz was evaluated. 10 / 400 It was measured using the Epstein test. In addition, the concentration of N present as AlN in the range from the surface of the non-oriented electrical steel sheet to a depth of 1 / 20 of the sheet thickness was measured by electrolytic extraction. The measurement results are shown in Figures 3 and 4.
[0084] Experiment 3
[0085] In addition, non-oriented electrical steel sheets were fabricated in the same procedure as Experiment 2 above, except that the concentration of hydrochloric acid in the acid treatment was set to 20% and the acid treatment time (immersion time) was varied within the range of 0.5 to 100 sec, and high-frequency iron loss (W 10 / 400 ) and surface nitriding amount were measured. The measurement results are shown in Figures 5 and 6.
[0086] As can be seen from the results shown in Figures 3 to 6, a significant reduction in high-frequency iron loss was confirmed when the acid concentration was in the range of 3 to 30% and the acid treatment time was in the range of 1 to 60 seconds. In contrast, when the acid concentration was less than 3% or the acid treatment time was less than 1 second, the iron loss remained high despite the acid treatment. This is thought to be because, when the acid concentration is low and the acid treatment time is short, the effect of the acid treatment becomes insufficient, and the nitride layer formed during the final annealing cannot be sufficiently removed. As a result, an oxide film is not formed during the strain relief annealing, and nitriding proceeds. Furthermore, when the acid concentration exceeds 30% or the acid treatment time exceeds 60 seconds, the iron loss also remained high. This is thought to be because a thick oxide layer is formed on the surface of the steel sheet during the acid treatment, and as a result, an oxide film is not formed during the strain relief annealing, and nitriding proceeds during the strain relief annealing.
[0087] The present invention is based on the above understanding. Below, embodiments for carrying out the present invention will be described in detail. Furthermore, the present invention is not limited to these embodiments.
[0088] [Ingredient Composition]
[0089] In the present invention, the reason for limiting the component composition of the non-oriented electrical steel sheet to the above range is explained.
[0090] C: 0.0050% or less
[0091] C is a harmful element that degrades iron loss through self-aging. That is, if the C content is excessive, C forms carbides and precipitates over time, increasing iron loss. Therefore, the C content is limited to 0.0050% or less. Preferably, it is 0.0040% or less. Meanwhile, although the lower limit of the C content is not particularly limited, from the perspective of suppressing decarburization costs in the refining process, it is desirable to have a C content of 0.0001% or more.
[0092] Si: 2.0–6.5%
[0093] Si is an element that increases the intrinsic resistance of steel and has the effect of reducing iron loss. In addition, Si also has the effect of increasing the strength of steel through solid solution strengthening. To obtain these effects, the Si content is set to 2.0% or more, preferably 2.5% or more. On the other hand, if the Si content exceeds 6.5%, slab cracks are prone to occur during manufacturing, and productivity decreases. Therefore, the Si content is set to 6.5% or less, preferably 6.0% or less.
[0094] Mn: 0.05∼2.0%
[0095] Mn, like Si, is an element that increases the intrinsic resistance of steel and has the effect of reducing iron loss. In addition, Mn has the effect of improving hot brittleness by forming sulfides. To obtain these effects, the Mn content is set to 0.05% or more, preferably 0.1% or more. On the other hand, if the Mn content exceeds 2.0%, slab cracking becomes more likely to occur during manufacturing, which lowers productivity. Therefore, the Mn content is set to 2.0% or less, preferably 1.5% or less.
[0096] P: 0.10% or less
[0097] Excessive addition of P leads to a deterioration in cold rolling performance. Therefore, the P content is set to 0.10% or less, preferably 0.05% or less. Meanwhile, the lower limit of the P content is not particularly limited and may be 0%. However, since P is an element that increases resistivity and has a significant effect in reducing eddy current losses, it may be added arbitrarily within the above range. From the perspective of reducing eddy current losses, it is preferable to have a P content of 0.001% or more, and more preferable to have a P content of 0.003% or more.
[0098] S: 0.0050% or less
[0099] Sulfur (S) becomes a sulfide and forms precipitates or inclusions, which degrades manufacturability (hot rolling properties) and the magnetic properties of non-oriented electrical steel sheets. Therefore, the S content is set to 0.0050% or less, preferably 0.0030% or less. Meanwhile, since a lower S content is preferable, the lower limit is not specifically limited and 0% is acceptable. However, since excessive reduction leads to an increase in manufacturing costs, it is preferable to set the S content to 0.0001% or more, and more preferable to set it to 0.0005% or more.
[0100] Al: 0.3~3.0%
[0101] Al, like Si, is an element that increases the intrinsic resistance of steel and has the effect of reducing iron loss. However, if the Al content exceeds 3.0%, the steel becomes embrittled, making it prone to slab cracking during manufacturing. Therefore, the Al content is set to 3.0% or less, preferably 2.0% or less, and more preferably 1.5% or less. On the other hand, if Al is less than 0.3%, fine nitrides are formed and precipitated, which actually increases iron loss. Therefore, the Al content is set to 0.3% or more, preferably 0.4% or more.
[0102] N: 0.0050% or less
[0103] N is a harmful element that forms nitrides and degrades magnetic properties. Therefore, the N content is set to 0.0050% or less, preferably 0.0040% or less. Meanwhile, since a lower N content is preferable, the lower limit is not specifically limited and 0% is acceptable. However, since excessive reduction leads to an increase in manufacturing costs, it is preferable to set the N content to 0.0005% or more, and more preferable to set it to 0.0010% or more.
[0104] Co: 0.0005∼0.0050%
[0105] As previously mentioned, Co is an element that has the effect of suppressing nitriding of the surface layer of the steel sheet during finish annealing. For this reason, the Co content is set to 0.0005% or more, preferably 0.001% or more. On the other hand, if the Co content exceeds 0.0050%, the outer oxide layer formed during finish annealing becomes thicker, and the formation of the oxide layer by acid treatment is inhibited. Therefore, the Co content is set to 0.0050% or less, preferably 0.0040% or less.
[0106] Ti: 0.0030% or less
[0107] Ti is a harmful element that forms and precipitates fine carbonitrides, thereby increasing iron loss. In particular, if the Ti content exceeds 0.0030%, the adverse effects of Ti become significant. Therefore, the Ti content is set to 0.0030% or less, preferably 0.0020% or less. Meanwhile, since a lower Ti content is preferable, the lower limit is not specifically restricted, and 0% is acceptable. However, since excessive reduction leads to an increase in manufacturing costs, it is preferable to set the Ti content to 0.0001% or more, and more preferable to set it to 0.0005% or more.
[0108] Nb: 0.0030% or less
[0109] Nb is a harmful element that forms and precipitates fine carbonitrides, thereby increasing iron loss. In particular, if the Nb content exceeds 0.0030%, the adverse effects of Nb become significant. Therefore, the Nb content is set to 0.0030% or less, preferably 0.0020% or less. Meanwhile, since a lower Nb content is preferable, the lower limit is not specifically restricted, and 0% is acceptable. However, since excessive reduction leads to an increase in manufacturing costs, it is preferable to set the Nb content to 0.0001% or more, and more preferable to set it to 0.0005% or more.
[0110] O: 0.0050% or less
[0111] O is a harmful element that forms oxides and degrades magnetic properties. Therefore, the O content is limited to 0.0050% or less. Preferably, it is 0.0040% or less. Meanwhile, since a lower O content is preferable, the lower limit is not specifically limited and 0% is acceptable. However, since excessive reduction leads to an increase in manufacturing costs, it is preferable to keep the O content at 0.0005% or more, and more preferable to keep it at 0.0010% or more.
[0112] A non-oriented electrical steel sheet in one embodiment of the present invention has a composition consisting of the above components, the remainder of Fe, and unavoidable impurities.
[0113] (Group A)
[0114] The above composition of components may optionally additionally include one or both of Sn and Sb in the following amounts.
[0115] Sn: 0.005∼0.20%
[0116] Sn is an element that improves magnetic flux density and iron loss by improving the recrystallization texture. When adding Sn, the Sn content is set to 0.005% or more to obtain the above effect. On the other hand, if the Sn content exceeds 0.20%, the effect becomes saturated. Therefore, the Sn content is set to 0.20% or less.
[0117] Sb: 0.005∼0.20%
[0118] Sb, like Sn, is an element that improves the recrystallization texture and has the effect of improving magnetic flux density and iron loss. When adding Sb, the Sb content is set to 0.005% or more to obtain the above effect. On the other hand, if the Sb content exceeds 0.20%, the effect becomes saturated. Therefore, the Sb content is set to 0.20% or less.
[0119] (Group B)
[0120] The above composition of components may optionally additionally include at least one selected from the group consisting of Ca, Mg, and REM (rare earth metals) in the following amounts.
[0121] Ca, Mg, REM: Total 0.0005–0.020%
[0122] Ca, Mg, and REM are components that form stable sulfides and have the effect of improving grain growth. When adding at least one selected from the group consisting of Ca, Mg, and REM, the total content of Ca, Mg, and REM is set to 0.0005% or more to obtain the above effect. On the other hand, if the total content exceeds 0.020%, the effect becomes saturated. Therefore, the total content is set to 0.020% or less.
[0123] (Group C)
[0124] The above component composition may optionally additionally include at least one selected from the group consisting of Cu, Cr, and Ni in the following amounts.
[0125] Cu, Cr, Ni: Total 0.03–1.0%
[0126] Cu, Cr, and Ni are elements that increase the intrinsic resistance of steel and have the effect of further reducing iron loss. When adding at least one of Cu, Cr, and Ni, the total content of Cu, Cr, and Ni is set to 0.03% or more to obtain the above effect. On the other hand, excessive addition lowers the magnetic flux density. Therefore, the total content is set to 1.0% or less.
[0127] (Group D)
[0128] The above component composition may optionally additionally include one or both of Ge and Ga in the following amounts.
[0129] Ge, Ga: Total 0.0005–0.01%
[0130] Ge and Ga are elements that have the effect of improving the texture. When adding one or both of Ge and Ga, the total content of Ge and Ga is set to 0.0005% or more, preferably 0.0020% or more, in order to obtain the above effect. On the other hand, if the above total content exceeds 0.01%, the above effect becomes saturated, and the alloy cost increases. Therefore, the above total content is set to 0.01% or less, preferably 0.0050% or less.
[0131] (Group E)
[0132] The above composition of components may optionally additionally include Zn in the following amounts.
[0133] Zn: 0.001∼0.05%
[0134] Zn is an element that has the effect of suppressing nitridation during final annealing. When adding Zn, the Zn content is set to 0.001% or more, preferably 0.002% or more. On the other hand, if the Zn content exceeds 0.05%, Zn forms sulfides, which actually increases iron loss. Therefore, the Zn content is set to 0.05% or less, preferably 0.01% or less.
[0135] (Group F)
[0136] The above composition of components may optionally additionally include one or both of Mo and W in the following amounts.
[0137] Mo, W: Total 0.001–0.05%
[0138] Mo and W are elements that have the effect of improving high-temperature strength, and by adding one or both of Mo and W, surface defects (scab) in non-oriented electrical steel sheets can be suppressed. Since the steel sheet of the present invention is a high-alloy steel and its surface is prone to oxidation, the incidence rate of scab caused by surface cracks is high. Therefore, by adding one or both of Mo and W, said cracks can be suppressed. When adding one or both of Mo and W, in order to sufficiently obtain the said effect, the total content of Mo and W is set to 0.001% or more, preferably 0.005% or more. On the other hand, if the said total content exceeds 0.05%, the said effect saturates, and the alloy cost increases. Therefore, the said total content is set to 0.05% or less, preferably 0.020% or less.
[0139] [Nitride]
[0140] Surface nitriding amount: 0.003% or less
[0141] As confirmed in the aforementioned experiments, there is a strong correlation between the surface nitriding amount and high-frequency iron loss, and iron loss decreases significantly when the surface nitriding amount is 0.003% or less. Therefore, in the present invention, the surface nitriding amount on at least one side of the non-oriented electrical steel sheet is set to 0.003% or less. Meanwhile, from the perspective of reducing high-frequency iron loss, the lower the surface nitriding amount, the better; thus, the lower limit of the surface nitriding amount is not particularly limited and may be 0%. However, from the perspective of manufacturing, the surface nitriding amount may be 0.0001% or more, or 0.0005% or more. Furthermore, "surface nitriding amount" here refers to the amount of N present as AlN in the range from the surface of the non-oriented electrical steel sheet to a depth of 1 / 20 of the sheet thickness. The above surface nitriding amount can be measured by electrolytic extraction analysis, and more specifically, by the method described in the example. In addition, it is desirable that the surface layer nitridation amount on both sides of the non-oriented electrical steel sheet satisfies the above conditions.
[0142] [Oxide layer]
[0143] The non-oriented electrical steel sheet of the present invention has an oxide layer containing one or both of Fe, Al, and Si on at least one surface. The oxide layer is formed by acid treatment after finish annealing and before strain relief annealing, as described below.
[0144] The oxide layer may be an Fe-Al oxide layer containing Fe and Al, an Fe-Si oxide layer containing Fe and Si, or an Fe-Si-Al oxide layer containing Fe, Si, and Al. The Fe concentration in the oxide layer is not particularly limited, but it is preferable that it be less than 100 mass% as a ratio to the total concentration of Al and Si. The Fe may be dissolved in the oxide, or may exist as a precipitate or an oxide. Additionally, the oxide layer may optionally contain other elements, for example, one or both of Co and Mn.
[0145] The thickness of the oxide layer is not particularly limited, but from the perspective of further suppressing nitriding during strain relief annealing, it is preferable to make the thickness of the oxide layer 50 nm or more. On the other hand, if the oxide layer is excessively thick, nitriding is promoted, and in addition, the stacking factor of the steel sheet decreases. Therefore, from the perspective of further suppressing nitriding and improving the stacking factor, it is preferable to make the thickness of the oxide layer 200 nm or less. The thickness of the oxide layer can be measured by scanning transmission electron microscopy-energy dispersive X-ray spectroscopy (STEM-EDS), and more specifically, by the method described in the example.
[0146] The oxide layer may be amorphous, crystalline, or a composite oxide of amorphous and crystalline phases. The ratio of the crystalline phase to the total of the amorphous and crystalline phases contained in the oxide layer is preferably 0% or more and 30% or less, and more preferably 0% or more and 10% or less. The ratio of the crystalline phase can be measured by observing the oxide layer with a scanning transmission electron microscope (STEM). Specifically, first, a STEM image is acquired at a magnification of approximately 2 million to 10 million times with a beam diameter that obtains a resolution of 1 nm or less. In the obtained STEM image, the region where a lattice pattern can be observed is designated as the crystalline phase, and the region where a maze pattern can be observed is designated as the amorphous phase, and the areas of both are calculated. From the result, the ratio of the area of the crystalline phase to the total area of the amorphous and crystalline phases is calculated, and the result expressed as a percentage is defined as the ratio of the crystalline phase.
[0147] [Oxide film]
[0148] The non-oriented electrical steel sheet of the present invention has an oxide film composed of one or both of Al oxide and Si oxide at the interface between the oxide layer and the base steel. In other words, the non-oriented electrical steel sheet of the present invention has an oxide film on the surface of the base steel and has the oxide layer on the surface of the oxide film.
[0149] The thickness of the oxide film is not particularly limited. However, as previously mentioned, a significant reduction in high-frequency iron loss was confirmed when the acid concentration was 3 to 30% and the acid treatment time was 1 to 60 seconds. In that case, the thickness of the oxide film was 10 to 40 nm. Therefore, it is desirable to make the thickness of the oxide film 10 nm or more and 40 nm or less.
[0150] The above oxide film may consist of a single film or may consist of multiple films. For example, the above oxide film may be an Al-rich oxide film, a Si-rich oxide film, or a multilayer film in which an Al-rich oxide film and a Si-rich oxide film are stacked. Among these, it is preferable that the oxide film be one in which an Al-rich oxide film and a Si-rich oxide film are alternately deposited.
[0151] Here, an Al-rich oxide film is defined as an oxide film in which the Al concentration is higher than the Si concentration. The above Al-rich oxide film may be a film substantially composed of Al oxide. Likewise, a Si-rich oxide film is defined as an oxide film in which the Si concentration is higher than the Al concentration. The above Si-rich oxide film may be a film substantially composed of Si oxide.
[0152] The coverage rate of the oxide film is not particularly limited, but it is preferable that it be 80% or more, and more preferable that it be 90% or more. Meanwhile, the upper limit of the coverage rate is not particularly limited, but 100% is acceptable. Here, the coverage rate is the coverage rate of the oxide film on the surface of the steel plate.
[0153] The structure of the above oxide film can be measured by observing the interface between the oxide layer and the base iron using STEM-EDS.
[0154] That is, the thickness and layer structure of the oxide film can be measured by observing the interface between the oxide layer and the base iron using STEM-EDS. Specifically, the EDS-line profile at the interface between the oxide layer and the base iron is acquired at intervals of 0.5 nm, and the thickness and layer structure of the oxide film can be determined from the elemental distribution of Al, Si, and O obtained.
[0155] In addition, the coverage rate of the oxide film can also be measured using STEM-EDS. Specifically, first, an elemental analysis map of the interface between the oxide layer and the base steel is obtained using STEM-EDS at a magnification of 100,000 times or more. The length of the oxide film covering the base steel is determined from the elemental distribution of Al, Si, and O in the obtained elemental analysis map. The coverage rate of the oxide film is calculated by dividing the obtained length of the oxide film by the length of the base steel. In other words, the coverage rate of the oxide film referred to here is a value expressed as a percentage of the ratio of the length of the oxide film to the length of the base steel, measured by STEM-EDS.
[0156] [Manufacturing Method]
[0157] Next, a method for manufacturing a non-oriented electrical steel sheet in one embodiment of the present invention will be described.
[0158] In one embodiment of the present invention, a steel material (slab) having the above-described composition can be manufactured by sequentially performing the following treatments (1) to (4).
[0159] (1) Cold rolling
[0160] (2) Finishing annealing
[0161] (3) Acid treatment
[0162] (4) Deformation removal annealing
[0163] In addition, in another embodiment of the present invention, hot rolling and hot-rolled sheet annealing may be performed prior to the cold rolling. In other words, in the other embodiment, a non-oriented electrical steel sheet can be manufactured by sequentially performing the following treatments (1) to (6) on a steel material (slab) having the above-mentioned composition.
[0164] (1) Hot rolling
[0165] (2) Hot-rolled plate annealing
[0166] (3) Cold rolling
[0167] (4) Finishing annealing
[0168] (5) Acid treatment
[0169] (6) Deformation removal annealing
[0170] [Steel Material]
[0171] As the above steel material, any steel material having the aforementioned compositional composition may be used. Typically, a steel slab may be used as the above steel material.
[0172] The method of manufacturing the above steel material is not particularly limited and can be manufactured by any method. For example, steel can be melted using a refining process using a converter, an electric furnace, a vacuum degassing device, etc., and then produced as a steel material by a continuous casting method or an ingot-blowing rolling method. In addition, a thin cast billet with a thickness of 100 mm or less produced by a direct casting method may be used as the above steel material.
[0173] [Hot Rolled]
[0174] When hot rolling is performed, the above steel material is hot-rolled to form a hot-rolled steel sheet. The conditions for the above hot rolling are not particularly limited and can be carried out under generally known conditions.
[0175] Typically, steel materials are rolled after being reheated by a heating furnace or the like, but cast steel materials may be provided directly to hot rolling without reheating.
[0176] If hot rolling is not performed, the steel material can be directly provided for cold rolling. When hot rolling is omitted, it is preferable to use a thin billet as the steel material.
[0177] [Hot-rolled plate annealing]
[0178] When hot rolling is performed, the obtained hot-rolled steel sheet is subjected to hot-rolled annealing to become a hot-rolled annealed sheet. The conditions for the hot-rolled annealing are not particularly limited. However, if the cracking temperature is below 800°C, the effect of hot-rolled annealing is small, and a sufficient improvement in magnetic properties may not be obtained. Therefore, it is preferable to set the cracking temperature during the hot-rolled annealing to 800°C or higher, and more preferable to set it to 850°C or higher. On the other hand, if the cracking temperature is higher than 1100°C, in addition to increased manufacturing costs, the grain size becomes coarsened, making it prone to brittle fracture (fracture) during subsequent cold rolling. Therefore, it is preferable to set the cracking temperature to 1100°C or lower, and more preferable to set it to 1000°C or lower.
[0179] In addition, regarding the annealing of the hot-rolled plate, it is preferable to make the cracking time 3 min or less, and more preferable to make it 1 min or less, from the perspective of securing productivity. Meanwhile, although the lower limit of the cracking time is not particularly limited, it is preferable to make it 1 sec or more, and more preferable to make it 5 sec or more.
[0180] [Cold Rolled]
[0181] Next, cold rolling is performed. If hot rolling and hot-rolled plate annealing have been performed, cold rolling is performed on the hot-rolled annealed plate to produce a cold-rolled steel sheet having a final plate thickness. On the other hand, if hot rolling and hot-rolled plate annealing have not been performed, cold rolling is performed directly on the steel material to produce a cold-rolled steel sheet having a final plate thickness. The above cold rolling may be performed only once or two or more times. If cold rolling is performed two or more times, intermediate annealing is performed between the cold rolling steps. The conditions for the above cold rolling are not particularly limited and can be performed under generally known conditions.
[0182] The final sheet thickness in the above cold rolling, that is, the thickness of the non-oriented electrical steel sheet finally obtained, is not particularly limited and can be any thickness. However, since iron loss increases if it is excessively thick, it is desirable to make the final sheet thickness 0.35 mm or less. On the other hand, if the non-oriented electrical steel sheet is excessively thin, it becomes difficult to handle during manufacturing processes such as cold rolling or annealing. Therefore, it is desirable to make the final sheet thickness 0.10 mm or more.
[0183] [Finishing Annealing]
[0184] Finish annealing is performed on the cold-rolled steel sheet obtained by the above cold rolling. The conditions for the finish annealing are not particularly limited and can be performed under generally known conditions. However, from the perspective of coarsening the crystal grain size to further reduce iron loss, it is preferable to set the cracking temperature during the finish annealing to 700 to 1200°C, and more preferable to set it to 800 to 1100°C. For the same reason, it is preferable to set the cracking time during the finish annealing to 1 to 120 sec, and more preferable to set it to 5 to 60 sec.
[0185] [Acid Treatment]
[0186] After the above-mentioned finishing annealing, an acid treatment is performed on the surface of the steel sheet prior to the subsequent strain relief annealing. In order to form a desired oxide film during strain relief annealing and suppress nitridation, the acid treatment must use an acid containing at least one selected from the group consisting of hydrochloric acid, phosphoric acid, sulfuric acid, and nitric acid at a total concentration of 3 to 30%. It is preferable that the total concentration of the acid be 5 to 25%. In addition, for the same reason, the acid treatment time is 1 to 60 sec, preferably 2 to 20 sec.
[0187] In addition, it is desirable to form an insulating film on the surface of the non-oriented electrical steel sheet after acid treatment. The formation of the insulating film can be carried out under generally known conditions. As for the insulating film, it is desirable to use an organic film containing resin to ensure good punchability. On the other hand, if weldability is important, it is desirable to use a semi-organic film or an inorganic film.
[0188] In addition, in the case of a motor stator core, etc., a steel sheet after finish annealing is processed into a core shape by punching or the like, laminated, fixed, and then manufactured by performing deformation relief annealing. Accordingly, the non-oriented electrical steel sheet of the present invention includes a core-shaped steel sheet in which a steel sheet after finish annealing is processed into a core shape by punching or the like, laminated, fixed, and then subjected to deformation relief annealing.
[0189] [Deformation Removal Annealing]
[0190] The above strain relief annealing is performed under conditions of a cracking temperature of 750°C to 950°C and a nitrogen content in the atmosphere of 50 volume% or more. This is because if the cracking temperature is below 750°C, the effect of improving iron loss by strain relief annealing is small, while if it exceeds 950°C, it becomes difficult to ensure insulation between laminated steel plates. The cracking time in the above strain relief annealing is not particularly limited, but it is preferable to be 0.1 to 10 hours. Furthermore, in the present invention, excellent iron loss characteristics can be obtained even when strain relief annealing is performed in an atmosphere mainly composed of relatively inexpensive nitrogen gas. Therefore, the upper limit of the nitrogen content in the above atmosphere is not limited and may be 100%.
[0191] In addition, by setting the heating rate in the above strain removal annealing to 50℃ / hr to 800℃ / hr, an oxide film having a structure in which a Si-rich oxide film and an Al-rich oxide film are alternately deposited can be formed.
[0192] Examples
[0193] To verify the effects of the present invention, a non-oriented electrical steel sheet was fabricated in the following order, and its magnetic properties were evaluated.
[0194] A steel slab having the compositional components shown in Tables 1 to 3 was heated at 1120°C for 30 minutes and then hot-rolled to produce a hot-rolled steel sheet with a thickness of 1.9 mm. Subsequently, the hot-rolled steel sheet was annealed under conditions of 970°C × 30 sec to produce a hot-rolled annealed sheet. After acid-cleaning the hot-rolled annealed sheet, it was cold-rolled to produce a cold-rolled steel sheet with the final thickness shown in Tables 4 to 6.
[0195] After that, the above cold-rolled steel sheet was subjected to finishing annealing at 820°C for 10 seconds in an atmosphere of H2:N2 = 20:80 in volume % ratio, and then acid treatment was performed under the conditions shown in Tables 4 to 6. After the acid treatment, further strain relief annealing was performed under the conditions shown in Tables 4 to 6 to produce a non-oriented electrical steel sheet.
[0196] In addition, manufacturing was discontinued for Comparative Example No. 14, which had an excessive amount of Mn, because slab cracks occurred during hot rolling. Similarly, manufacturing was discontinued for Comparative Example No. 15, which had an excessive amount of Al, and Comparative Example No. 18, which had an excessive amount of Si, because slab cracks occurred during hot rolling. Furthermore, manufacturing was discontinued for Comparative Example No. 21, which had an excessive amount of P, because cracks occurred during cold rolling.
[0197] (Surface nitrification amount)
[0198] Next, test specimens were taken from the obtained non-oriented electrical steel sheet and subjected to electrolytic extraction analysis to measure the amount of N present as AlN (surface nitridation amount) in the range from one surface of the non-oriented electrical steel sheet to a depth of 1 / 20 of the sheet thickness. The measurement results are shown in Tables 7 to 9.
[0199] (Thickness of the oxide layer)
[0200] In addition, an oxide layer containing Fe and one or both of Al and Si was formed on the surface of the obtained non-oriented electrical steel sheet. The thickness of the oxide layer was measured by scanning transmission electron microscopy-energy dispersive X-ray spectroscopy (STEM-EDS). Specifically, EDS-line profiles were acquired at intervals of 0.5 nm, and the thickness of the oxide layer was determined from the elemental distribution of Al, Si, and O obtained. The measurement results are shown in Tables 7 to 9.
[0201] (Oxide film)
[0202] In addition, the thickness and layer structure of the oxide film formed at the interface between the oxide layer and the base steel in the obtained non-oriented electrical steel sheet were measured using STEM-EDS. Specifically, EDS-line profiles at the interface were acquired at intervals of 0.5 nm, and the thickness and layer structure of the oxide film were determined from the elemental distribution of Al, Si, and O obtained.
[0203] In Tables 7 to 9, in the examples labeled "Si, Al," a film-shaped oxide film containing Si and Al exists, and said film-shaped oxide film had a structure in which a Si-rich oxide film and an Al-rich oxide film were alternately deposited. In addition, in the examples labeled "Al," a film-shaped oxide film containing Si and Al exists, and said film-shaped oxide film was composed only of an Al-rich oxide film.
[0204] In addition, the coverage rate of the oxide film was also measured using STEM-EDS. Specifically, first, an elemental analysis map of the interface between the oxide layer and the base steel was obtained using STEM-EDS at a magnification of 100,000x or higher. The length of the oxide film covering the steel sheet base steel was determined from the elemental distribution of Al, Si, and O in the obtained elemental analysis map. The coverage rate of the oxide film was calculated by dividing the obtained length of the oxide film by the length of the steel sheet base steel. The measurement results are shown in Tables 7 to 9.
[0205] (Iron Hand)
[0206] In addition, samples were taken from each of the obtained non-oriented electrical steel sheets, and test specimens measuring 30 mm in width × 180 mm in length were cut from the rolling direction (L direction) and the width direction (C direction), and the iron loss W in the (L + C) direction was measured by the Epstein test. 10 / 400 was measured. In addition, in this embodiment, the measured iron loss W 10 / 400 In this case, it was determined that the high-frequency iron loss is good when it is lower than the iron loss reference value (W / kg) obtained from the following (1).
[0207] Iron loss reference value (W / kg) = 21.8 × t + 7.5… (1)
[0208] Here, t: thickness of non-oriented electrical steel sheet (mm)
[0209] The measurement results are shown in Tables 7 to 9. From these results, it can be seen that all non-oriented electrical steel sheets satisfying the conditions of the present invention have reduced iron loss in the high-frequency range. According to the present invention, since the reduction of iron loss in the high-frequency range is achieved without adding a large amount of alloying elements that cause a decrease in magnetic flux density, the non-oriented electrical steel sheets of the present invention can be suitably used as materials for motor cores for hybrid electric vehicles, electric vehicles, high-speed generators, air conditioner compressors, vacuum cleaners, machine tools, etc.
[0210]
[0211]
[0212]
[0213]
[0214]
[0215]
[0216]
[0217]
[0218]
Claims
Claim 1 It has a compositional composition in mass% containing C: 0.0050% or less, Si: 2.0–6.5%, Mn: 0.05–2.0%, P: 0.10% or less, S: 0.0050% or less, Al: 0.3–3.0%, N: 0.0050% or less, Co: 0.0005–0.0050%, Ti: 0.0001–0.0030%, Nb: 0.0001–0.0030%, and O: 0.0050% or less, with the remainder being Fe and unavoidable impurities; on at least one surface, in a range from the surface to a depth of 1 / 20 of the plate thickness, the amount of N present as AlN is 0.003 mass% or less; on the surface, it has an oxide layer containing Fe and one or both of Al and Si; and the oxide layer and the steel A non-oriented electrical steel sheet having an oxide film composed of one or both of Al oxide and Si oxide at the interface with the substrate. Claim 2 A non-oriented electrical steel sheet according to claim 1, wherein the above component composition additionally contains, in mass%, one or more of the following groups A to F: Group A: Sn: 0.005 to 0.20% and Sb: 0.005 to 0.20% or both; Group B: at least one selected from the group consisting of Ca, Mg, and REM, in a total of 0.0005 to 0.020%; Group C: at least one selected from the group consisting of Cu, Cr, and Ni, in a total of 0.03 to 1.0%; Group D: at least one or both of Ge and Ga, in a total of 0.0005 to 0.01%; Group E: Zn: 0.001 to 0.05%; Group F: at least one or both of Mo and W, in a total of 0.001 to 0.05% Claim 3 A method for manufacturing a non-oriented electrical steel sheet by performing two or more cold rolling steps with intermediate annealing in between on a steel material having a composition in mass% containing C: 0.0050% or less, Si: 2.0–6.5%, Mn: 0.05–2.0%, P: 0.10% or less, S: 0.0050% or less, Al: 0.3–3.0%, N: 0.0050% or less, Co: 0.0005–0.0050%, Ti: 0.0001–0.0030%, Nb: 0.0001–0.0030%, and O: 0.0050% or less, with the remainder being Fe and unavoidable impurities, to produce a cold-rolled steel sheet, and performing finish annealing and strain relief annealing on the cold-rolled steel sheet, wherein the strain relief annealing is crack A method for manufacturing a non-oriented electrical steel sheet, wherein the process is carried out under conditions of a temperature of 750℃ to 950℃ and a nitrogen content of 50 volume% or more in the atmosphere, and after the finishing annealing and before the deformation removal annealing, an acid treatment is performed on the surface of the steel sheet for 1 to 60 sec using an acid containing at least one selected from the group consisting of hydrochloric acid, phosphoric acid, sulfuric acid, and nitric acid at a total concentration of 3 to 30 weight%, and the non-oriented electrical steel sheet has, on at least one surface, an amount of N present as AlN in a range from the surface to a depth of 1 / 20 of the sheet thickness is 0.003 mass% or less, and on the surface, an oxide layer containing Fe and one or both of Al and Si, and on the interface between the oxide layer and the base steel, an oxide film consisting of one or both of Al oxide and Si oxide. Claim 4 A method for manufacturing a non-oriented electrical steel sheet according to claim 3, wherein prior to the cold rolling, the steel material is hot-rolled to form a hot-rolled steel sheet, the hot-rolled steel sheet is annealed to form a hot-rolled annealed sheet, and the hot-rolled annealed sheet is provided to the cold rolling. Claim 5 A method for manufacturing a non-oriented electrical steel sheet according to claim 3 or 4, wherein the above component composition additionally contains, in mass%, one or more of the following groups A to F. Group A: Sn: 0.005 to 0.20% and Sb: 0.005 to 0.20% or both Group B: At least one selected from the group consisting of Ca, Mg, and REM, in a total of 0.0005 to 0.020% Group C: At least one selected from the group consisting of Cu, Cr, and Ni, in a total of 0.03 to 1.0% Group D: One or both of Ge and Ga, in a total of 0.0005 to 0.01% Group E: Zn: 0.001 to 0.05% Group F: One or both of Mo and W, in a total of 0.001 to 0.05%
Citation Information
Patent Citations
High-strength magnetic steel sheet and process for producing them
KR1020060063960A