Multicomponent blended cement

A multi-component cement blend of Type 3 Portland cement, blast furnace slag, and fly ash, enhanced with steelmaking dust, addresses the need for early and long-term strength while eliminating the need for activators, thus optimizing construction efficiency and environmental sustainability.

KR103047055B1Active Publication Date: 2026-11-11SAMPYO IND CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020240132334
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2026-11-11
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

Conventional ternary blended cements require a separate alkali stimulant to enhance initial reactivity, leading to increased construction costs due to extended formwork removal times, and they compromise on both early and long-term strength development.

Method used

A multi-component mixed cement comprising 45 to 55 parts of Type 3 rapid-strength Portland cement, 25 to 35 parts of blast furnace slag fine powder, and 15 to 25 parts of fly ash, with up to 8 wt% of steelmaking dust substitution, promoting early and long-term strength through the use of Type 3 cement's high alite content and steelmaking dust's latent hydraulic properties.

Benefits of technology

The cement achieves improved early strength development and long-term strength while reducing environmental impact by utilizing steelmaking dust, an industrial byproduct, without the need for additional activators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024106296284-PAT00001
    Figure 112024106296284-PAT00001
  • Figure 112024106296284-PAT00002
    Figure 112024106296284-PAT00002
  • Figure 112024106296284-PAT00004
    Figure 112024106296284-PAT00004
Patent Text Reader

Abstract

The present invention relates to a multi-component mixed cement composed of Type 3 rapid-strength Portland cement, blast furnace slag fine powder, and fly ash, and steelmaking dust to ensure long-term strength. The present invention provides a multi-component mixed cement based on a multi-component mixed cement comprising 45 to 55 parts by weight of Type 3 rapid-strength Portland cement; 25 to 35 parts by weight of blast furnace slag fine powder; and 15 to 25 parts by weight of fly ash, wherein an amount corresponding to 8 wt% or less (excluding 0 wt%) of the total weight of the multi-component mixed cement is substituted with steelmaking dust in the Type 3 rapid-strength Portland cement, and wherein the steelmaking dust contains 50 wt% or more of pure CaO that is not bonded within the mineral phase, under the condition that the steelmaking dust contains 2 to 3 wt% of SO3.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a multi-component mixed cement composed of a mixture of Type 3 high-strength Portland cement, blast furnace slag fine powder, and fly ash, and a mixture of steelmaking dust to ensure long-term strength. Background Technology

[0003] Mixed cement refers to cement made by mixing appropriate admixtures with Type 1 ordinary Portland cement (OPC). Depending on the main ingredient mixed, it is classified into blast furnace slag cement, fly ash cement, silica cement, etc., and is mainly used for the purpose of improving durability, water resistance, watertightness, and long-term strength, or for the purpose of easier construction.

[0004] In particular, a ternary mixed cement in which blast furnace slag fine powder (SP) and fly ash (FA) are mixed with OPC can reduce the amount of OPC used, increase the proportion of industrial by-products used as raw materials, and improve long-term strength through the latent hydraulic properties of SP and the pozzolanic reaction of FA.

[0005] However, the aforementioned ternary blended cement has a relatively low OPC content, resulting in lower initial reactivity and requiring a longer curing period; consequently, problems such as increased construction costs due to the extended formwork removal time arise at construction sites. Therefore, ternary blended cement is used in combination with an activator that promotes initial reactivity.

[0006] The present invention aims to improve both early strength development performance and long-term strength development performance by improving the raw material composition of a ternary mixed cement. Prior art literature

[0008] 1. Registered Patent 10-2349613 "Composition of a rapid-expansion hardening cement admixture, an on-site hydrated concrete mat using the same, and a method for constructing a concrete mat" 2. Published Patent 10-2024-0064306 "Composition of a rapid-strengthening admixture cement using silica and a fluidized concrete composition using the same" 3. Registered Patent 10-1849927 "Strength-enhancing agent composition for ternary admixture cement and ternary admixture cement containing the same"

[0009] 1. Yoon Jae-hong, Yoon Chi-hyun, Hirofumi Sugimoto, Akio Honjo, "A Study on the Resource Recovery of Fe-Clinker Generated During the Recycling Process of Electric Furnace Steelmaking Dust", Resource Recycling, 32(1), 171, pp.50-59 Feb, 2023. The problem to be solved

[0010] The purpose of the present invention is to provide a multi-component mixed cement that secures both early strength development performance and long-term strength development performance compared to conventional mixed cements, thereby eliminating the need to add a separate alkali stimulant to mortar or concrete compositions. means of solving the problem

[0012] To solve the aforementioned problem, the present invention provides a multi-component mixed cement comprising: 45 to 55 parts by weight of Type 3 rapid-strength Portland cement; 25 to 35 parts by weight of blast furnace slag fine powder; and 15 to 25 parts by weight of fly ash.

[0014] In addition, to improve long-term strength, an amount equivalent to 8 wt% or less (excluding 0 wt%) of the total weight of the multi-component mixed cement can be substituted with steelmaking dust in the above-mentioned Type 3 rapid-strength Portland cement.

[0015] The above steelmaking dust may be applied as containing 50 wt% or more of pure CaO that is not bonded within the mineral phase, and may contain 2 to 3 wt% of SO3. Effects of the invention

[0017] The multi-component mixed cement provided by the present invention is,

[0018] The early strength of mortar or concrete can be improved by applying Type 3 high-strength Portland cement, and the long-term strength of mortar or concrete can be improved by mixing steel dust.

[0019] In addition, the environmental burden can be reduced by utilizing steelmaking dust, an industrial byproduct, as a raw material for cement. Specific details for implementing the invention

[0021] The present invention is derived based on a ternary mixed cement in which Type 1 ordinary Portland cement (OPC), blast furnace slag fine powder (SP), and fly ash (FA) are mixed in a weight ratio of 5:3:2.

[0022] However, depending on the curing temperature of the concrete or mortar composition, the amount of binder, the water-to-binder ratio, the amount of aggregate, the fine aggregate ratio, the type and amount of additives, and whether or not admixtures are used, the mixing ratio of OPC, SP, and FA of the mixed cement provided by the present invention can be adjusted in the range of 4.5~5.5:2.5~3.5:1.5~2.5 by weight.

[0024] Mixed cement has the disadvantage that the early strength of concrete or mortar is lowered due to the mixing of SP and FA. Accordingly, the present invention aims to derive a mixed cement with improved early strength by applying Type 3 rapid-strength Portland cement (EPC) instead of OPC. This is because, compared to OPC, EPC has a high content of alite (C3S), which is effective for short-term strength development, and a high specific surface area (Blain), resulting in excellent early strength development performance.

[0025] Table 1 below shows the chemical composition and physical properties of OPC and EPC applied to the test of the present invention compared with KS standards.

[0026]

[0028] In the present invention, based on the raw material composition of a conventional ternary mixed cement using OPC, a multi-component mixed cement was specified in which 45 to 55 parts by weight of EPC, 25 to 35 parts by weight of SP, and 15 to 25 parts by weight of FA were mixed. However, while replacing OPC with EPC improved the early strength of concrete or mortar, a phenomenon occurred in which the 28-day strength (long-term strength) was somewhat lowered.

[0030] Accordingly, in this invention, a portion of the EPC is replaced with steelmaking dust (SMD), which is generated as a byproduct from steel mills, to enhance long-term strength.

[0032] The molten iron from which impurities have been removed in the blast furnace undergoes a preliminary treatment process (KR process) to remove silicon, phosphorus, sulfur, etc., a converter process corresponding to a decarbonization process, a ladle furnace (LF), and an RH vacuum degassing device, and then a secondary refining process to adjust the temperature and composition of the molten iron. The SMD is collected through a dry dust collector in each process of the converter steelmaking process (KR, converter, and secondary refining process).

[0033] The main components of these SMDs are CaO, Fe2O3, SO3, etc., and since limestone (CaO) is added to remove impurities during the steelmaking process, the SMDs contain a significant amount of unreacted CaO.

[0034] Table 2 below shows the XRF analysis results for SMD. It contains 2.71 wt% SO3, which affects the setting and hydration reaction rates, and is identified as having a ratio equivalent to Portland cement containing SO3 in the range of 2 to 3 wt%.

[0035] Meanwhile, the above SMD contains 50.49 wt% of CaO, which is a somewhat small amount compared to Portland cement, which contains 60 wt% or more of CaO. However, in Portland cement, CaO exists in a state bound within the mineral phase, such as in alite (3CaO·SiO2(C3S)), belite (2CaO·SiO2(C2S)), and tricalcium aluminate (3CaO·Al2O3(C3A)), whereas the CaO contained in the SMD exists in a pure CaO state rather than bound within the mineral phase, so a large amount of calcium hydroxide (Ca(OH)2) is generated during the hydration reaction.

[0036]

[0038] Ca(OH)2 cleaves the alumina silicate structure of SP, initiating hydration and consuming calcium ions. Additionally, a pozzolanic reaction proceeds in which Ca(OH)2 reacts with FA to form CSH (calcium silicate hydrate). Consequently, the CaO component of SMD stimulates the latent hydraulic properties of SP and promotes the pozzolanic reaction of FA, thereby improving long-term strength.

[0039] However, since the specific chemical composition of the SMD may vary depending on the dust collector (process in which it was collected), the date of collection, etc., and the content of CaO and SO3 may also vary, it is preferable to select one with a CaO content of 50 wt% or more and an SO3 content of 2 to 3 wt% and apply it to the present invention.

[0041] In each of the following tests, the compressive strength of the mortar at different ages was examined by increasing the amount of steel making dust (SMD) that replaced a portion of the EPC in a mixed cement with a weight ratio of 5:3:2 of EPC, SP, and FA.

[0043] Table 4 below shows the composition of the binder applied to each test example and the compressive strength test results for each test example at different ages. The curing temperature at the time of the test was set to 20℃.

[0045]

[0047] Test Example #2, which applied EPC, was found to have a significantly increased compressive strength at 1 day compared to Test Example #1, which applied OPC, and also improved compressive strengths at 3 and 7 days, but a phenomenon was observed where the compressive strength at 28 days was slightly lower. In other words, Test Example #2 is considered to have the most advantage in terms of securing early strength, but has a slight disadvantage in terms of developing long-term strength.

[0048] In Test Example #3, where an amount equivalent to 4 wt% of the total binder content (total amount of EPC, SP, FA) was substituted with SMD from EPC, the compressive strength at 1 and 3 days of age was slightly lower than that of Test Specimen #2, but the strength at 7 and 28 days of age was improved compared to Test Specimen #2. In addition, the compressive strength at all ages was higher than that of Test Specimen #1. It is determined that the raw material composition of Test Example #3 is the most appropriate in terms of improving both early and long-term strength compared to the ternary mixed cement using OPC.

[0049] In Test Example #4, where an amount equivalent to 8 wt% of the total binder was substituted from EPC to SMD, the compressive strength from age 1 to age 7 was slightly lower compared to Test Specimen #2, but the strength at age 28 was improved compared to Test Specimen #2. In this case as well, the compressive strength over all ages was higher than that of Test Specimen #1. Although the compressive strength of Test Specimen #4 is generally lower than that of Test Specimen #3, the raw material composition of Test Example #4 is judged to also exhibit an effective effect in terms of improving both early and long-term strength compared to the three-component mixed cement using OPC. Furthermore, the effectiveness of Test Example #4 can be emphasized in terms of reducing the environmental burden by using a large amount of SMD, an industrial byproduct.

[0050] In Test Example #5, where an amount equivalent to 12 wt% of the total binder was substituted from EPC to SMD, the compressive strength at all ages was lower than that of Test Specimen #2. Even when compared to Test Specimen #1, the compressive strength at 1 day of age increased slightly, but the increase was not significant, and the compressive strength after 3 days of age was actually lower than that of Test Specimen #1. Therefore, Test Example #5 is deemed inappropriate to present as an improved mixed cement.

[0051] From the above test results, it can be seen that when an amount equivalent to 8 wt% or less (excluding 0 wt%) of the total weight of the multi-component mixed cement is replaced with steelmaking dust in the above Type 3 rapid-strength Portland cement to improve the long-term strength of the multi-component mixed cement, both the early strength and long-term strength are improved compared to general 3-component mixed cement.

[0053] The present invention has been examined in detail above, along with specific test and analysis results. However, the present invention is not limited by the above embodiments and may be modified and varied within the scope without departing from the essence of the invention. Accordingly, the claims of the present invention include such modifications and variations.

Claims

Claim 1 A multi-component mixed cement based on a multi-component mixed cement comprising 45 to 55 parts by weight of Type 3 rapid-strength Portland cement; 25 to 35 parts by weight of blast furnace slag fine powder; and 15 to 25 parts by weight of fly ash, wherein an amount corresponding to 8 wt% or less (excluding 0 wt%) of the total weight of the multi-component mixed cement is substituted with steelmaking dust in the Type 3 rapid-strength Portland cement, and wherein the steelmaking dust contains 50 wt% or more of pure CaO that is not bonded within the mineral phase, under the condition that the steelmaking dust contains 2 to 3 wt% of SO3. Claim 2 delete Claim 3 delete Claim 4 delete

Citation Information

Patent Citations

  • Slag mixed cement having steel slag, mortar, and concrete

    KR1020220089454A

  • Cement composition using steel making dust

    KR1020240098515A