Manufacturing method of photoactive layer additive for perovskite solar cell, photoactive layer additive for perovskite solar cell manufactured thereby and perovskite solar cell comprising the same
The double heat treatment of sucrose to create a humin-rich photoactive layer additive addresses defects and instability in perovskite solar cells, enhancing crystal quality and efficiency while ensuring long-term stability.
Patent Information
- Application Number
- KR1020260035917
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2026-02-26
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2046-02-26
AI Technical Summary
Perovskite solar cells face issues such as defects during crystal growth, charge recombination, and instability due to environmental factors, leading to performance degradation and lack of long-term operational stability, with conventional additives causing non-uniformity and instability.
A method involving double heat treatment of sucrose to convert it into caramelized sucrose containing humin, which is used as a photoactive layer additive to stabilize crystal growth, reduce defects, and enhance charge transport.
Improves crystal quality, reduces defect density, and enhances charge carrier transport dynamics, resulting in higher photoelectric conversion efficiency and long-term stability of perovskite solar cells.
Smart Images

Figure R1020260035917_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a photoactive layer additive, and more specifically, to a photoactive layer additive for perovskite solar cells. Background Technology
[0002] Perovskite solar cells are attracting attention as next-generation solar cells due to their low-cost solution-process manufacturing capabilities, high light absorption coefficients, and excellent charge transport characteristics. Furthermore, with the recent rapid improvement in photoelectric conversion efficiency, their commercialization potential is also being discussed. However, perovskite solar cells are prone to various defects during the crystal growth process of the photoactive layer. Additionally, the presence of non-radiative recombination centers at grain boundaries, surfaces, and interfaces within the formed thin film promotes charge recombination, leading to an open-circuit voltage (V). oc Performance degradation, such as a decrease in ) and a decrease in fill factor (FF) and an increase in hysteresis, may occur. In addition, it has been pointed out that the chemical and structural stability of the photoactive layer may be degraded by external environments such as moisture, oxygen, heat, and continuous light irradiation, and that it is difficult to ensure long-term operational stability due to ion migration.
[0003] As a solution to these problems, techniques have been proposed to control the crystal growth behavior of perovskite thin films, reduce defects, and improve interfacial stability by introducing various additives into the precursor composition for forming the photoactive layer. For example, attempts have been made to increase grain size or reduce charge trap density and suppress non-radiative recombination by including halide salts, alkali metal ions, organic cations, compounds with Lewis base or Lewis acid properties, organic molecules with chelate structures, and polymer materials as photoactive layer additives to passivate under-coordinated ions at grain boundaries and surfaces. Additionally, methods have been proposed to introduce functional additives that can be adsorbed at the interface or control interfacial reactions to mitigate interfacial defects occurring at the interface between the photoactive layer and the electron transport layer or hole transport layer.
[0004] However, conventional photoactive layer additive technologies still have room for improvement in terms of additive chemical stability, process compatibility, and reproducibility. Some additives may impair thin film uniformity due to insufficient solubility or dispersibility with the precursor composition, or, depending on the amount added, may cause non-uniformity in crystal growth and an increase in residual impurities, thereby degrading device performance. Furthermore, certain organic additives may provide degradation pathways related to decomposition or moisture adsorption during prolonged operation, while polymeric additives may exhibit negative effects such as hindering charge transport or increasing interfacial resistance. Moreover, although natural product-based additives are being proposed due to their advantages in terms of eco-friendliness and cost, issues regarding the stable reproducibility of performance have been raised because the inherent characteristics of natural materials result in inconsistent molecular structures and compositions, or component variations depending on process conditions.
[0005] Therefore, there is a need to develop a new photoactive layer additive technology capable of effectively reducing defects in the photoactive layer of perovskite solar cells, stably controlling crystal growth and thin film morphology, while simultaneously suppressing charge recombination and improving long-term operational stability. Prior art literature
[0006] Republic of Korea Registered Patent Publication No. 10-2818781 The problem to be solved
[0007] The technical problem to be solved by the present invention is to provide a method for manufacturing a photoactive layer additive for a perovskite solar cell that can improve the efficiency of the perovskite solar cell by double heat treatment of sucrose so that at least a portion of the caramelized sucrose is converted into humin, a photoactive layer additive for a perovskite solar cell manufactured thereby, and a perovskite solar cell containing the same.
[0008] The technical problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned technical problems will be clearly understood by those skilled in the art to which the present invention belongs from the description below. means of solving the problem
[0009] To achieve the above technical objective, one embodiment of the present invention provides a method for preparing a photoactive layer additive for a perovskite solar cell, comprising the steps of: preparing purified sucrose; obtaining caramelized sucrose by performing a first heat treatment on the purified sucrose; and obtaining caramelized sucrose containing humin by performing a second heat treatment on the caramelized sucrose.
[0010] In the step of obtaining the caramelized sucrose, the first heat treatment may be characterized by being performed in a temperature range of 150 ℃ to 200 ℃.
[0011] In the step of obtaining caramelized sucrose containing the above humin, the second heat treatment may be characterized by being performed in a temperature range of 200 ℃ to 250 ℃.
[0012] In the step of obtaining caramelized sucrose containing the humin, the content of the humin may be characterized as being 0.00001% by weight to 0.01% by weight relative to the caramelized sucrose containing the humin.
[0013] To achieve the above technical objective, another embodiment of the present invention provides a photoactive layer additive for a perovskite solar cell prepared by the method for preparing a photoactive layer additive for a perovskite solar cell described above.
[0014] To achieve the above technical problem, another embodiment of the present invention provides a photoactive layer additive for a perovskite solar cell comprising caramelized sucrose containing humin.
[0015] The content of the above humin may be characterized as being 0.00001% to 0.01% by weight relative to the caramelized sucrose containing the above humin.
[0016] It may be characterized in that at least a portion of the sucrose containing hydroxyl groups is converted into the humin containing carbonyl groups.
[0017] To achieve the above technical objective, another embodiment of the present invention provides a perovskite solar cell comprising: a substrate; a lower electrode located on the substrate; an electron transport layer located on the lower electrode; a perovskite photoactive layer located on the electron transport layer and comprising the photoactive layer additive described above; a hole transport layer located on the photoactive layer; and an upper electrode located on the hole transport layer. Effects of the invention
[0018] The photoactive layer additive for a perovskite solar cell according to the present invention comprises caramelized sucrose in which at least a portion is converted into humin by double heat treatment of purified sucrose, thereby improving the crystal quality of the perovskite solar cell and reducing the defect density.
[0019] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the configuration of the invention described in the detailed description of the invention or the claims. Brief explanation of the drawing
[0020] FIG. 1 is a schematic diagram showing the method for manufacturing a photoactive layer additive for a perovskite solar cell according to the present invention. FIG. 2 is a flowchart schematically illustrating the method for manufacturing a photoactive layer additive for a perovskite solar cell according to the present invention. Figure 3 is a schematic diagram showing the structure of the perovskite solar cell of the present invention. Figure 4 is a graph showing the current density-voltage characteristics of the perovskite solar cell of the present invention. FIG. 5 is a graph showing the distribution of (a) photoelectric conversion efficiency (PCE), (b) short-circuit current density (Jsc), (c) open-circuit voltage (Voc), and (d) charge rate (FF) of the perovskite solar cell of the present invention. Figure 6 is a graph showing (a) the change in PCE over time under continuous light irradiation conditions and (b) the photoelectric conversion efficiency (PCE) of the perovskite solar cell of the present invention compared by year. Figure 7 is a graph showing (a) current-voltage characteristics and (b) output characteristics of the perovskite solar cell of the present invention. Figure 8 is a graph showing the FTIR spectrum of the photoactive layer of Comparative Example 1. Figure 9 is a graph showing the FTIR spectrum of the photoactive layer of Comparative Example 2. Figure 10 is a graph showing the FTIR spectrum of the photoactive layer of Preparation Example 2. Figure 11 is an AFM image of the photoactive layer of the perovskite solar cell of the present invention. Figure 12 is an SEM image of the photoactive layer of the perovskite solar cell of the present invention. Figure 13 is a graph showing the grain size distribution of the photoactive layer calculated from Figure 12. Figure 14 is an image showing the TEM image and FFT analysis results of the photoactive layer of the perovskite solar cell of the present invention. Figure 15 is a graph showing the XRD pattern analysis results of the photoactive layer of the perovskite solar cell of the present invention. Figure 16 is a graph showing the time-resolved photoluminescence (TRPL) measurement results of the photoactive layer of the perovskite solar cell of the present invention. Specific details for implementing the invention
[0021] The present invention will be described below with reference to the attached drawings. However, the present invention may be implemented in various different forms and is therefore not limited to the embodiments described herein. Furthermore, in order to clearly explain the present invention in the drawings, parts unrelated to the explanation have been omitted, and similar parts throughout the specification have been given similar reference numerals.
[0022] Throughout the specification, when it is stated that a part is "connected (connected, in contact, combined)" with another part, this includes not only cases where they are "directly connected," but also cases where they are "indirectly connected" with other members interposed between them. Furthermore, when it is stated that a part "includes" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but rather allows for the inclusion of additional components.
[0023] The terms used herein are merely for describing specific embodiments and are not intended to limit the invention. Singular expressions include plural expressions unless the context clearly indicates otherwise. In this specification, terms such as “comprising” or “having” are intended to indicate the presence of the features, numbers, steps, actions, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the existence or addition of one or more other features, numbers, steps, actions, components, parts, or combinations thereof.
[0024] Embodiments of the present invention will be described in detail below with reference to the attached drawings.
[0026] With reference to FIGS. 1 and 2, a method for manufacturing a photoactive layer additive for a perovskite solar cell according to one embodiment of the present invention will be described.
[0027] FIG. 1 is a schematic diagram showing the method for manufacturing a photoactive layer additive for a perovskite solar cell according to the present invention.
[0028] FIG. 2 is a flowchart schematically illustrating the method for manufacturing a photoactive layer additive for a perovskite solar cell according to the present invention.
[0029] Referring to FIGS. 1 and 2, a method for manufacturing a photoactive layer additive for a perovskite solar cell according to the present invention may include the step of preparing purified sucrose (S100); the step of obtaining caramelized sucrose by performing a first heat treatment on the purified sucrose (S200); and the step of obtaining caramelized sucrose containing humin by performing a second heat treatment on the caramelized sucrose (S300).
[0030] First, purified sucrose can be prepared (S100).
[0031] In one embodiment, the sucrose may be a sugar-based disaccharide that can be obtained from biomass-derived materials as a naturally abundant, cost-effective, and environmentally sustainable raw material.
[0032] The above sucrose can typically be extracted from sugarcane, but the source and extraction method of the sucrose are not limited thereto and may be applied in various forms, including sucrose obtained from other plant-derived raw materials such as sugar beet, or commercially available sucrose. Furthermore, the sucrose may be appropriately selected according to physical properties such as purity, moisture content, and powder or crystalline form, within a range that can achieve the purpose of the present invention.
[0033] The above sucrose may be characterized as being purified.
[0034] In one embodiment, the sucrose may be purified by heating in a temperature range of 120°C to 170°C, but the temperature range for purifying the sucrose is not limited to the above example.
[0035] By purifying the above sucrose, included impurities can be removed, and recrystallization can be performed together if necessary.
[0036] The purified sucrose above may include glucose and fructose, and more specifically, may include D-glucopyranose and D-fructofuranose.
[0037] Meanwhile, since the purified sucrose is prone to intermolecular aggregation due to hydrogen bonding caused by multiple hydroxyl groups within the molecule, when used as a photoactive layer additive, miscibility or dispersibility may be reduced within the precursor composition.
[0038] Secondly, the purified sucrose can be subjected to a first heat treatment to obtain caramelized sucrose (S200).
[0039] In the step (S200) of obtaining the caramelized sucrose, the first heat treatment may be performed in a temperature range of 150 ℃ to 200 ℃, preferably in a temperature range of 170 ℃ to 190 ℃, but the temperature range of the first heat treatment is not limited to the above example.
[0040] For example, the first heat treatment according to the present invention can be performed at 180°C.
[0041] If the temperature at which the first heat treatment is performed is less than 150 ℃, there may be a problem that caramelization does not occur, and if the temperature at which the first heat treatment is performed exceeds 200 ℃, there may be a problem that the caramel carbonizes.
[0042] In the step (S200) of obtaining the caramelized sucrose, the caramelized sucrose obtained through the first heat treatment may be characterized in that the hydroxyl groups and aromatics present in the purified sucrose are reduced by the dehydration reaction, and accordingly, the molecular structure may be partially rearranged.
[0043] The step of obtaining the caramelized sucrose (S200) can mitigate the excessive intermolecular hydrogen bonding tendency of the purified sucrose by caramelizing the purified sucrose through the first heat treatment.
[0044] Finally, the caramelized sucrose can be subjected to a second heat treatment to obtain caramelized sucrose containing humin (S300).
[0045] In the step (S300) of obtaining caramelized sucrose containing the humin, the second heat treatment may be performed in a temperature range of 200 ℃ to 250 ℃, preferably in a temperature range of 200 ℃ to 230 ℃, but the temperature range of the second heat treatment is not limited to the above example.
[0046] For example, the second heat treatment according to the present invention can be performed at a temperature of 220°C.
[0047] If the temperature at which the second heat treatment is performed is less than 200°C, sufficient humin may not be generated, and there may be a problem of aggregation due to hydrogen bonding, and if the temperature at which the second heat treatment is performed exceeds 250°C, there may be a problem of excessive carbonization.
[0048] In the step (S300) of obtaining caramelized sucrose containing the humin, additional dehydration and oligomerization reactions may proceed by performing a second heat treatment on the caramelized sucrose, and accordingly, at least a portion of the caramelized sucrose may be converted into humin.
[0049] The above humin may be a polymeric structure rich in carbonyl and carboxyl groups and depleted of hydroxyl groups.
[0050] The content of the humin may be 0.00001% to 0.01% by weight relative to the total weight of the perovskite precursor solution, preferably 0.00005% to 0.001% by weight, but the content of the humin is not limited to the above examples.
[0051] If the content of the above humin is less than 0.00001 wt% relative to the total weight of the perovskite precursor solution, Pb in the perovskite lattice 2+Insufficient carbonyl (C=O) functional groups may be supplied to adequately passivate defects, which can lead to charge recombination losses and a decrease in photoelectric conversion efficiency. Additionally, the formation of a protective film to block moisture penetration may be insufficient, resulting in reduced long-term stability.
[0052] If the content of the above humin exceeds 0.01 wt% relative to the total weight of the perovskite precursor solution, self-aggregation may occur due to intermolecular hydrogen bonding, and the self-aggregated humin may act as an impurity within the perovskite thin film to form trap sites that hinder charge transport, or it may hinder the crystallinity of the thin film, thereby causing a rapid decrease in the short-circuit current density (Jsc) and charge factor (FF).
[0053] When the photoactive layer additive containing the caramelized sucrose containing the humin is added to the photoactive layer of a perovskite solar cell due to the step (S300) of obtaining the caramelized sucrose containing the humin, the quality of the perovskite crystals of the photoactive layer can be improved, and the defect density can be reduced so that the charge carrier transport dynamics can be optimized.
[0055] A photoactive layer additive for a perovskite solar cell according to another embodiment of the present invention will be described.
[0056] A photoactive layer additive for a perovskite solar cell according to one embodiment of the present invention may be characterized by being manufactured by the method for manufacturing a photoactive layer additive for a perovskite solar cell described above, but the method for manufacturing the photoactive layer additive for a perovskite is not limited to the above examples.
[0057] The above photoactive layer additive for perovskite solar cells may include caramelized sucrose containing humin.
[0058] The above humin may be a polymeric structure rich in carbonyl and carboxyl groups and depleted of hydroxyl groups.
[0059] The content of the humin may be 0.00001 wt% to 0.01 wt% relative to the total weight of the perovskite precursor solution, preferably 0.00005 wt% to 0.001 wt%, but the content of the humin is not limited to the above examples.
[0060] If the content of the above humin is less than 0.00001 wt% relative to the total weight of the perovskite precursor solution, Pb in the perovskite lattice 2+ Insufficient carbonyl (C=O) functional groups may be supplied to adequately passivate defects, which can lead to charge recombination losses and a decrease in photoelectric conversion efficiency. Additionally, the formation of a protective film to block moisture penetration may be insufficient, resulting in reduced long-term stability.
[0061] If the content of the above humin exceeds 0.01 wt% relative to the total weight of the perovskite precursor solution, self-aggregation may occur due to intermolecular hydrogen bonding, and the self-aggregated humin may act as an impurity within the perovskite thin film to form trap sites that hinder charge transport, or it may hinder the crystallinity of the thin film, thereby causing a rapid decrease in the short-circuit current density (Jsc) and charge factor (FF).
[0062] The above-described photoactive layer additive for a perovskite solar cell comprises caramelized sucrose containing humin, which can act as a heterogeneous nucleation site during the growth of perovskite crystals within the photoactive layer or as a defect passivation layer at the crystal grain boundaries, thereby stabilizing the crystal growth of the perovskite and alleviating local stress concentrations, which can uniformly form the photoactive layer.
[0064] Referring to FIG. 3, a perovskite solar cell according to another embodiment of the present invention will be described.
[0065] Figure 3 is a schematic diagram showing the structure of the perovskite solar cell of the present invention.
[0066] Referring to FIG. 3, a perovskite solar cell according to one embodiment of the present invention may include a substrate; a lower electrode located on the substrate; an electron transport layer located on the lower electrode; a perovskite photoactive layer located on the electron transport layer and comprising the photoactive layer additive described above; a hole transport layer located on the photoactive layer; and an upper electrode located on the hole transport layer.
[0067] The above substrate is a transparent material and may include glass, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polypropylene (PP), polyimide (PI), triacetyl cellulose (TAC), etc., but the material of the substrate is not limited to the above examples.
[0068] For example, the substrate according to the present invention may be glass.
[0069] The lower electrode may be located on the substrate.
[0070] The lower electrode may include indium tin oxide (ITO), fluorine tin oxide (FTO), indium zinc oxide (IZO), indium zinc tin oxide (IZTO), aluminum zinc oxide (AZO), etc., but the material of the lower electrode is not limited to the above examples.
[0071] For example, the lower electrode according to the present invention may be fluorine oxide (FTO).
[0072] The electron transport layer may be located on the lower electrode.
[0073] The electron transport layer may include titanium dioxide (TiO2), tin dioxide (SnO2), zinc oxide (ZnO), tungsten trioxide (WO3), niobium pentoxide (Nb2O5), zirconium dioxide (ZrO2), PCBM (Phenyl-C61-butyric acid methyl ester), etc., but the material of the electron transport layer is not limited to the above examples.
[0074] For example, the electron transport layer according to the present invention may be tin dioxide (SnO2).
[0075] The above perovskite photoactive layer may have the charge transport layer located thereon.
[0076] The above photoactive layer may include formamidinium lead iodide (FAPbI-3), methylammonium lead iodide (MAPbI3), methylammonium lead bromide (MAPbBr3), formamidinium lead bromide (FAPbBr-3), etc., but the material of the above photoactive layer is not limited to the above examples.
[0077] For example, the photoactive layer according to the present invention may include formamidinium lead iodide (FAPbI-3) and methylammonium lead bromide (MAPbBr3).
[0078] The above photoactive layer may further include the above-described photoactive layer additive.
[0079] A detailed description of the components of the above-mentioned photoactive layer that overlap with the aforementioned photoactive layer additives will be omitted. However, even if a description of such components is omitted, it is not intended that such components are not included in any embodiment.
[0080] By including the photoactive layer additive, the crystal growth of perovskite within the photoactive layer can be stably controlled, and charge extraction efficiency and device reliability can be simultaneously improved.
[0081] The hole transport layer may be located on the photoactive layer.
[0082] The hole transport layer above is spiro-MeOTAD, polytriarylamine (PTAA), P3HT, PEDOT:PSS, nickel oxide (NiO₂ x ), copper iodide (CuI), copper thiocyanate (CuSCN), copper oxide (CuO x ), molybdenum oxide (MoO x The material may include vanadium pentoxide (V2O5), tungsten trioxide (WO3), graphene oxide, etc., but the material of the hole transport layer is not limited to the above examples.
[0083] For example, the hole transport layer according to the present invention may be a spiro-MeOTAD.
[0084] A surface modification layer may be further included between the photoactive layer and the hole transport layer.
[0085] The surface modification layer may include octylammonium iodide (OAI), phenylethylammonium iodide (PEAI), butylammonium iodide (BAI), formamidinium iodide (FAI), amino acids, etc., but the material of the surface modification layer is not limited to the above examples.
[0086] For example, the surface modification layer according to the present invention may be octylammonium iodide (OAI).
[0087] The above perovskite solar cell can improve the interfacial energy alignment between the photoactive layer and the hole transport layer and reduce the interfacial resistance by including the surface modification layer on the photoactive layer, and thereby improve the charge extraction efficiency of the perovskite solar cell.
[0088] The upper electrode may be located on the hole transport layer.
[0089] The upper electrode may include gold (Au), silver (Ag), aluminum (Al), copper (Cu), platinum (Pt), nickel (Ni), chromium (Cr), molybdenum (Mo), tungsten (W), titanium (Ti), palladium (Pd), carbon (C), indium tin oxide (ITO), fluorine tin oxide (FTO), aluminum zinc oxide (AZO), carbon nanotubes (CNT), etc.
[0090] For example, the upper electrode according to the present invention may be gold (Au).
[0091] The perovskite solar cell of the present invention can improve the crystal quality of the photoactive layer and improve charge extraction efficiency and reliability by including the photoactive layer additive.
[0093] The present invention will be explained in more detail below through manufacturing examples, comparative examples, and experimental examples. However, the present invention is not limited to the following manufacturing examples and experimental examples.
[0095] <Preparation Example 1> Preparation of a photoactive layer additive for a perovskite solar cell according to the present invention
[0096] Sucrose extracted from sugarcane was purified by heating at 160°C and then subjected to a first heat treatment on a hot plate at a temperature of 180°C to obtain caramelized sucrose. Subsequently, the caramelized sucrose was subjected to a second heat treatment on a hot plate at a temperature of 220°C to obtain caramelized sucrose containing a large amount of humin, which was utilized as an additive for the photoactive layer of a perovskite solar cell according to the present invention.
[0098] <Preparation Example 2> Preparation of the perovskite solar cell of the present invention
[0099] The fabrication of the perovskite solar cell of the present invention was carried out in a controlled dry room environment maintained at 25°C and 20% relative humidity. To prepare the perovskite precursor solution, 1202 mg of FAPbI3 was reacted with 35 mol% MACl, 0.8 mol% MAPbBr3, and a solvent mixture of DMF and DMSO in a 4:1 ratio. The resulting solution was filtered through a 0.2 μm polyvinylidene fluoride (PVDF) filter and then applied to an SnO2-coated substrate. Spin coating was performed at 7500 rpm for 50 seconds with a ramping time of 0.1 seconds. After 13 seconds of spin coating, 1 mL of diethyl ether was added as a reverse solvent, followed immediately by annealing on a hot plate at 150°C for 15 minutes. To deactivate the perovskite surface, an octylammonium iodide solution (4 mg / mL in IPA) was spin-coated onto the perovskite layer at 3000 rpm for 30 seconds. Subsequently, a hole transport layer was formed by adding various concentrations of tBP and Li-TFSI dopants to a Spiro-MeOTAD (Lumtech) solution and spin-coating it at 4000 rpm for 30 seconds. Finally, a perovskite solar cell was fabricated by depositing a 100 nm thick gold electrode via thermal evaporation under a high vacuum of 10⁻⁶ Torr.
[0101] <Comparative Example 1> Preparation of a perovskite solar cell not containing a photoactive layer additive
[0102] It was prepared under the same conditions as Preparation Example 2, except that the photoactive layer additive for perovskite solar cells was not added.
[0104] <Comparative Example 2> Preparation of a perovskite solar cell containing a photoactive layer additive containing caramelized sucrose
[0105] A photoactive layer additive containing caramelized sucrose, prepared under the same conditions as Preparation Example 1 but without performing a second heat treatment, was used instead of Preparation Example 1, and was prepared under the same conditions as Preparation Example 2.
[0107] <Experimental Example 1> Evaluation of device performance of the perovskite solar cell of the present invention
[0108] Figure 4 is a graph showing the current density-voltage characteristics of the perovskite solar cell of the present invention.
[0109] FIG. 5 is a graph showing the distribution of (a) photoelectric conversion efficiency (PCE), (b) short-circuit current density (Jsc), (c) open-circuit voltage (Voc), and (d) charge rate (FF) of the perovskite solar cell of the present invention.
[0110] Figure 7 is a graph showing (a) current-voltage characteristics and (b) output characteristics of the perovskite solar cell of the present invention.
[0111] Table 1 below shows the distribution of (a) photoelectric conversion efficiency (PCE), (b) short-circuit current density (Jsc), (c) open-circuit voltage (Voc), and (d) charge rate (FF) of the perovskite solar cell of the present invention according to FIG. 5.
[0112] Scan Direction J sc (mA / m 2 ) V oc (V) FF PCE (%) Hysteresis index Comparative Example 1 Reverse 25.88 1.16 0.82 24.66 0.04 Forward 25.86 1.16 0.79 23.61 Preparation Example 2 Reverse 25.96 1.17 0.83 25.26 0.01 Forward 25.90 1.17 0.83 25.12
[0113] Table 2 below shows the distribution of (a) photoelectric conversion efficiency (PCE), (b) short-circuit current density (Jsc), (c) open-circuit voltage (Voc), and (d) charge rate (FF) of the perovskite solar cell of the present invention according to FIG. 7.
[0114] V oc (V) I sc (mA) J sc (mA / cm 2 ) FF (%) I max (mA) V max (V) P max (mW) Eff. (%) Preparation Example 2 1.1702 2.0729 25.8156 82.98 1.9552 1.0296 2.0132 25.0678
[0115] Referring to Figures 4, 5, and 7 and Tables 1 and 2, the photoelectric conversion efficiency of Comparative Example 1 is 24.66%, whereas the photoelectric conversion efficiency of the perovskite solar cell of the present invention is 25.07% and 25.26%. It was confirmed that the photoelectric conversion efficiency was improved by improving the current density-voltage (JV) characteristics compared to Comparative Example 1, and it was also confirmed that the short-circuit current density (Jsc), open-circuit voltage (Voc), and charge factor (FF) showed a tendency to improve.
[0116] Through this, it was confirmed that the photoelectric conversion performance of the solar cell can be improved by applying the photoactive layer additive for a perovskite solar cell according to the present invention, which contains caramelized sucrose containing humin, to a perovskite solar cell, and it was also confirmed that the performance improvement effect is reproducible.
[0118] <Experimental Example 2> Evaluation of Long-term Operational Stability of the Perovskite Solar Cell of the Present Invention
[0119] Figure 6 is a graph showing (a) the change in PCE over time under continuous light irradiation conditions and (b) the photoelectric conversion efficiency (PCE) of the perovskite solar cell of the present invention compared by year.
[0120] Referring to FIG. 6a, it was confirmed that the perovskite solar cell of the present invention exhibits excellent operational stability, with a smaller decrease in photoelectric conversion efficiency (PCE) compared to Comparative Example 1 under conditions of continuous light irradiation for a long time. Through this, it was confirmed that the photoactive layer additive of the present invention can improve stability by suppressing degradation factors during long-term operation of the perovskite solar cell.
[0121] Referring to FIG. 6b, it was confirmed that the perovskite solar cell of the present invention can achieve a higher level of photoelectric conversion efficiency compared to conventional technology using natural product-based additives. Through this, it was confirmed that the present invention can provide technical advantages favorable for realizing high efficiency in the field of eco-friendly additive-based perovskite solar cells.
[0123] <Experimental Example 3> Chemical structure analysis of the photoactive layer additive of the present invention
[0124] Figure 8 is a graph showing the FTIR spectrum of a perovskite solar cell containing sucrose (S) and a photoactive layer additive containing sucrose.
[0125] Figure 9 is a graph showing the FTIR spectra of caramelized sucrose (C) and Comparative Example 2.
[0126] FIG. 10 is a graph showing the FTIR spectra of the photoactive layer additive (H) of the present invention and Preparation Example 2.
[0127] Referring to FIGS. 8 to 10, the photoactive layer additive of the present invention has approximately 3570 cm² attributable to free hydroxyl groups (OH) observed in conventional sucrose. -1 While the absorption peak in the vicinity is significantly reduced or disappears, at 1760–1770 cm⁻¹ -1 It was confirmed that a strong C=O (carbonyl or carboxyl group) absorption peak was newly observed in the vicinity.
[0128] Through this, it was confirmed that the photoactive layer additive of the present invention undergoes dehydration and polymerization reactions through the process of heat-treating sucrose at 220 °C or higher, resulting in a reduction of hydroxyl groups and conversion into a polymeric structure rich in carbonyl and carboxyl functional groups.
[0130] <Experimental Example 4> Analysis of the shape and crystallinity of the photoactive layer of the perovskite solar cell of the present invention
[0131] FIG. 11 is an AFM image of the photoactive layer of (a) Comparative Example 1, (b) Comparative Example 2, and (c) Preparation Example 2.
[0132] FIG. 12 is an SEM image of (a) a cross-section of a perovskite solar cell, (b) Comparative Example 1, (c) Comparative Example 2, and (d) Preparation Example 2 photoactive layers.
[0133] Figure 13 is a graph showing the grain size distribution of the photoactive layer calculated from Figure 12.
[0134] Figure 14 shows (a) FFT analysis results and (b) and (c) TEM images of the photoactive layer of the perovskite solar cell of the present invention.
[0135] FIG. 15 is a graph showing the results of XRD pattern analysis of the photoactive layer of the perovskite solar cell of the present invention. (a) is a graph comparing the XRD patterns of the photoactive layers of Comparative Example 1, Comparative Example 2 and Preparation Example 2; (b) is a graph comparing the FWHM of the (001) and (002) peaks of the photoactive layers of Comparative Example 1, Comparative Example 2 and Preparation Example 2; and (c) is a graph showing the XRD results with an enlarged α-phase (002) peak region of the photoactive layers of Comparative Example 1, Comparative Example 2 and Preparation Example 2.
[0136] Referring to Fig. 11, it was confirmed that the average surface roughness (Ra) of the photoactive layer of Example 2 was reduced (39.74 nm --> 36.70 nm) compared to Comparative Example 1, and the frequency of occurrence of voids and microcracks within the surface was significantly reduced.
[0137] Through this, it was confirmed that the photoactive layer additive of the present invention can induce the formation of a uniform thin film by stabilizing crystal growth within or at the boundaries of the crystal grains of the photoactive layer and alleviating local stress concentration, thereby simultaneously improving charge extraction efficiency and device reliability.
[0138] Referring to FIGS. 12 and 13, it was confirmed that the photoactive layer of Preparation Example 2 exhibited a significantly increased grain size compared to Comparative Example 1, and displayed a more distinct and dense microstructure with clearer grain boundaries. In addition, statistical analysis results also confirmed that the average grain size of the photoactive layer of Preparation Example 2 was 1.72 μm, compared to 1.16 μm for Comparative Example 1, indicating an increase in the average grain size.
[0139] Through this, it was confirmed that perovskite crystal growth can be controlled more stably by adding the photoactive layer additive of the present invention, and it was confirmed that the photoactive additive of the present invention can reduce nucleation density by preferentially interacting with PbI₂ in the perovskite precursor solution and induce a crystallization mechanism in which crystal growth proceeds centered around a small number of nuclei.
[0140] Referring to FIG. 14, it was confirmed that the photoactive layer additive of the present invention exists in a state of being uniformly dispersed inside or at the grain boundaries of the perovskite crystals, and that a structure coexisting with the perovskite crystals without separate phase separation was observed.
[0141] Through this, it was confirmed that the photoactive layer additive of the present invention can reduce defects by acting as a heterogeneous nucleation site during the crystal growth process of perovskite in the photoactive layer or by forming a defect passivation layer at the grain boundaries.
[0142] Referring to FIG. 15, in the photoactive layer of Preparation Example 2, the (001) and (002) diffraction peaks of the α-FAPbI3 phase were observed more distinctly, the full width at half maximum (FWHM) of the corresponding peaks was reduced, and the δ-FAPbI3 peak of the inactive phase ( It was confirmed that 11.7°) was not observed.
[0143] Through this, it was confirmed that the perovskite solar cell of the present invention, by including the photoactive layer additive of the present invention, can improve crystal orientation and lattice alignment during the crystal growth process of perovskite within the photoactive layer, and accordingly, increase the grain size within the photoactive layer and reduce lattice defects.
[0145] <Experimental Example 5> Analysis of charge recombination characteristics of the photoactive layer of the perovskite solar cell of the present invention
[0146] Figure 16 is a graph showing the time-resolved photoluminescence (TRPL) measurement results of the photoactive layer of the perovskite solar cell of the present invention.
[0147] Referring to Fig. 16, it was confirmed that the charge lifetime of the active layer of Comparative Example 1 was 0.712 μs for τ1 and 0.217 μs for τ2, whereas the charge lifetime of the active layer of Preparation Example 2 was 1.162 μs for τ1 and 0.291 μs for τ2, showing a significant increase.
[0148] Through this, it was confirmed that adding the photoactive layer additive of the present invention to the photoactive layer of a perovskite solar cell effectively suppresses non-radiative defect states, thereby reducing charge trap density; accordingly, the open-circuit voltage (V-) of the perovskite solar cell oc It was confirmed that high-efficiency, high-reliability perovskite solar cells can be realized by increasing ), reducing hysteresis, and improving long-term drivability.
[0150] Thus, it was confirmed that the photoactive layer additive for perovskite solar cells according to the present invention can simultaneously improve the photoelectric conversion performance and long-term operational stability of perovskite solar cells by effectively passivating defects in the photoactive layer, enhancing crystal growth and crystallinity, and suppressing non-radiative recombination.
[0152] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will understand that other specific forms can be easily modified without altering the technical spirit or essential features of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.
[0153] The scope of the present invention is defined by the claims set forth below, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of the present invention.
Claims
Claim 1 A method for preparing a photoactive layer additive for a perovskite solar cell, characterized by comprising the steps of: preparing purified sucrose; obtaining caramelized sucrose by performing a first heat treatment on the purified sucrose; and obtaining caramelized sucrose containing humin by performing a second heat treatment on the caramelized sucrose. Claim 2 A method for manufacturing a photoactive layer additive for a perovskite solar cell, characterized in that, in the step of obtaining the caramelized sucrose according to claim 1, the first heat treatment is performed in a temperature range of 150 ℃ to 200 ℃. Claim 3 A method for manufacturing a photoactive layer additive for a perovskite solar cell, characterized in that, in the step of obtaining caramelized sucrose containing the humin according to claim 1, the second heat treatment is performed in a temperature range of 200 ℃ to 250 ℃. Claim 4 A method for preparing a photoactive layer additive for a perovskite solar cell, characterized in that, in the step of obtaining caramelized sucrose containing the humin in claim 1, the content of the humin is 0.00001 weight% to 0.01 weight% relative to the caramelized sucrose containing the humin. Claim 5 A photoactive layer additive for a perovskite solar cell prepared by the method for preparing a photoactive layer additive for a perovskite solar cell according to claim 1. Claim 6 A photoactive layer additive for a perovskite solar cell characterized by containing caramelized sucrose containing humin. Claim 7 A photoactive layer additive for a perovskite solar cell, characterized in that, in claim 6, the content of the humin is 0.00001% to 0.01% by weight relative to caramelized sucrose containing the humin. Claim 8 A photoactive layer additive for a perovskite solar cell according to claim 6, characterized in that at least a portion of the sucrose containing hydroxyl groups is converted into the humin containing carbonyl groups. Claim 9 A perovskite solar cell characterized by comprising: a substrate; a lower electrode located on the substrate; an electron transport layer located on the lower electrode; a perovskite photoactive layer located on the electron transport layer and comprising a photoactive layer additive according to any one of claims 5 to 8; a hole transport layer located on the photoactive layer; and an upper electrode located on the hole transport layer.
Citation Information
Patent Citations
Composite comprising spinel type material and perovskite type material and Electrochemical Device having the same
KR101774154B1
Self-healable Perovskite Film, Method for Preparing Same and Electronic Element Using Same