Photosensitive resin composition, photosensitive resin film, multilayer printed circuit board and semiconductor package, and method for manufacturing multilayer printed circuit board.
Patent Information
- Application Number
- TW110125072
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-17
- Filing Date
- 2021-07-08
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-07-07
AI Technical Summary
Conventional photosensitive resin compositions used in multilayer printed wiring boards face challenges in achieving high resolution via holes, improved bonding strength with copper plating, and enhanced electrical insulation reliability, particularly in the context of miniaturization and increased density of semiconductor packaging substrates, where laser processing is inefficient and time-consuming, and thermosetting resin compositions lack the necessary characteristics for interlayer insulating layers.
A photosensitive resin composition comprising a photopolymerizable compound with ethylenically unsaturated groups, a photopolymerization initiator, and an inorganic filler surface-treated with a specific coupling agent, which includes a photopolymerizable compound with an acidic substituent and an alicyclic skeleton, and optionally a thermosetting resin, to enhance resolution, adhesion, and electrical insulation.
The proposed resin composition enables high-resolution via holes, improved bonding strength with copper plating, and enhanced electrical insulation reliability, facilitating efficient manufacturing of multilayer printed wiring boards with smaller via holes and improved manufacturing efficiency.
Smart Images

Figure TWG2TB001919874_001 
Figure TWG2TB001919874_002
Abstract
Description
Technical Field
[0001] This disclosure relates to a photosensitive resin composition, a photosensitive resin film, a multilayer printed circuit board and semiconductor packaging, and a method for manufacturing a multilayer printed circuit board. Prior Technology
[0002] In recent years, the miniaturization and high performance of electronic devices have led to the high-density development of multilayer printed circuit boards (PCBs) through the increase in the number of circuit layers and the miniaturization of wiring. In particular, the high-density development of semiconductor packaging substrates such as ball grid arrays (BGAs) and chip-size packages (CSPs) for mounting semiconductor chips has been significant. In addition to the miniaturization of wiring, there is also a requirement for thinner insulating films and further miniaturization of the diameter of vias (also known as "via holes") used for interlayer connections. Furthermore, along with the thinning of insulating films in PCBs, excellent electrical insulation reliability between layers is also required [especially electrical insulation reliability after moisture absorption (high accelerated stress test (HAST) resistance)].
[0003] As a method for manufacturing printed circuit boards, one example is a multilayer printed circuit board manufacturing method that utilizes a build-up method (for example, see Patent Document 1) formed by sequentially depositing interlayer insulating layers and conductor circuit layers. In multilayer printed circuit boards, with the miniaturization of circuits, the semi-additive process of forming circuits by plating has become mainstream. In the previous semi-additive process, for example, (1) a thermosetting resin film is laminated on the conductor circuit, and the thermosetting resin film is hardened by heating to form an "interlayer insulating layer". (2) Next, vias for interlayer connection are formed by laser processing, and desmearing and roughening treatment is performed by alkaline permanganate treatment, etc. (3) Then, electroless copper plating is performed on the substrate, a pattern is formed using a resist, and then electrolytic copper plating is performed to form a copper circuit layer. (4) Subsequently, resist stripping is performed, and electroless flash etching is performed to form a copper circuit (for example, see Patent Document 2).
[0004] As mentioned above, laser processing has become the mainstream method for forming vias in interlayer insulation layers formed by curing thermosetting resin films. However, the miniaturization of vias using laser irradiation with a laser processing machine has reached its limit. Furthermore, in the formation of vias using a laser processing machine, each via needs to be formed individually. When multiple vias are required for high-density applications, the formation of vias takes a long time, resulting in poor manufacturing efficiency.
[0005] In this situation, as a method to form multiple vias at once, the following method is proposed: using a photosensitive resin composition and photolithography to form multiple small-diameter vias at once, wherein the photosensitive resin composition contains (A) an acid-modified vinyl-containing epoxy resin, (B) a photopolymerizable compound, (C) a photopolymerization initiator, (D) an inorganic filler and (E) a silane compound, and the content of the (D) inorganic filler is 10% to 80% by mass (for example, see Patent Document 3). [Existing Technical Documents] [Patent Literature]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 7-304931 [Patent Document 2] Japanese Patent Application Publication No. 2019-66793 [Patent Document 3] Japanese Patent Application Publication No. 2017-116652 Summary of the Invention
[0007] [The problem that the invention aims to solve] Patent Document 2 describes an alkaline-developable photosensitive resin composition exhibiting excellent resistance to adhesive residue removal. This composition contains an alkaline-soluble resin with intramolecular carboxyl and vinyl unsaturated groups, a photopolymerization initiator, and a cyanate ester compound. However, in addition to further miniaturization of wiring, there is also progress in thinning insulating films and reducing the diameter of vias used for interlayer bonding. Therefore, in addition to the increasing demands for improved adhesion strength to copper plating and electrical insulation reliability, the demand for improved resistance to adhesive residue removal is also increasing. In these aspects, the photosensitive resin composition of Patent Document 2 has room for further improvement. Patent Document 3 addresses the issue of reducing the adhesion strength to copper plating caused by using a photosensitive resin composition instead of the previous thermosetting resin composition as the interlayer insulation layer or surface protective layer. Furthermore, it addresses the issues of via resolution and the tightness of the silicon material with the substrate and wafer components, and resolves these issues. However, as mentioned above, the requirements for improving the adhesion strength to copper plating and the reliability of electrical insulation are increasing, and in these aspects, the photosensitive resin composition of Patent Document 3 has room for further improvement. Furthermore, although the use of photosensitive resin compositions, which were previously used as solder resist materials, as interlayer insulating materials is also considered, the interlayer insulating layer requires properties that are not necessary for the solder resist (e.g., reliability of interlayer electrical insulation, adhesion strength to copper plating, high heat resistance to withstand repeated heating, high dimensional accuracy of via shape, etc.). Therefore, it is difficult to predict whether it can withstand the practical use based on the function of the interlayer insulating layer, and it cannot be easily switched.
[0008] Therefore, the purpose of this disclosure is to provide a photosensitive resin composition with excellent via resolution, adhesion strength to copper plating, electrical insulation reliability, and resistance to desmearing; a photosensitive resin composition for forming photovias; and a photosensitive resin composition for interlayer insulating layers. Furthermore, this disclosure provides a photosensitive resin film comprising the aforementioned photosensitive resin composition and a photosensitive resin film for interlayer insulating layers, a multilayer printed circuit board and a semiconductor package, and a method for manufacturing the aforementioned multilayer printed circuit board. [Methods for solving problems]
[0009] Through repeated efforts, the inventors have discovered that the stated purpose can be achieved through this disclosure. This disclosure includes the following embodiments [1] to
[19] .
[0010] [1] A photosensitive resin composition comprising (A) a photopolymerizable compound having an ethylene unsaturated group, (B) a photopolymerization initiator and (F) an inorganic filler, wherein the photosensitive resin composition, The photopolymerizable compound (A) having an vinyl unsaturated group includes (A1) a photopolymerizable compound having an vinyl unsaturated group, an acidic substituent, and an alicyclic skeleton. The inorganic filler (F) comprises an inorganic filler surface-treated with a coupling agent that does not have at least one functional group selected from the group consisting of amine and (meth)acrylic groups. [2] The photosensitive resin composition as described in [1], wherein the coupling agent has an alkoxy group. [3] The photosensitive resin composition as described in [1] or [2], wherein the average particle size of the inorganic filler (F) is 0.01 μm to 5 μm. [4] The photosensitive resin composition as described in any of [1] to [3], wherein the content of the inorganic filler (F) is 5% to 80% by mass based on the total amount of solids. [5] The photosensitive resin composition as described in any one of [1] to [4], wherein the (A) photopolymerizable compound having an ethylene unsaturated group further comprises at least one selected from the group consisting of (Ai) a monofunctional vinyl monomer having one polymerizable ethylene unsaturated group, (Aii) a difunctional vinyl monomer having two polymerizable ethylene unsaturated groups and (Aiii) a polyfunctional vinyl monomer having at least three polymerizable ethylene unsaturated groups. [6] The photosensitive resin composition described in any one of [1] to [5], wherein in the photopolymerizable compound having an ethylene unsaturated group, an acidic substituent and an alicyclic skeleton, the alicyclic skeleton is an alicyclic skeleton with 5 to 20 carbon atoms forming the ring. [7] The photosensitive resin composition as described in any one of [1] to [5], wherein in the photopolymerizable compound having an ethylene unsaturated group, an acidic substituent and an alicyclic skeleton in (A1), the alicyclic skeleton comprises two or more rings. [8] The photosensitive resin composition described in any of [1] to [7] further contains (C) a thermosetting resin. [9] The photosensitive resin composition described in any of [1] to [8] further contains (D) an elastomer.
[10] The photosensitive resin composition as described in [9], wherein the (D) elastomer comprises at least one selected from the group consisting of styrene elastomers, olefin elastomers, polyester elastomers, carbamate elastomers, polyamide elastomers, acrylic elastomers and silicone elastomers.
[11] The photosensitive resin composition described in any of [1] to
[10] , wherein (A) the content of the photopolymerizable compound having an ethylene unsaturated group is 0.1% to 60% by mass based on the total solid content of the photosensitive resin composition.
[12] A photosensitive resin composition for forming photosensitive vias, comprising the photosensitive resin composition described in any one of [1] to
[11] .
[13] A photosensitive resin composition for an interlayer insulating layer, comprising the photosensitive resin composition described in any one of [1] to
[11] .
[14] A photosensitive resin film comprising a photosensitive resin composition as described in any one of [1] to
[11] .
[15] A photosensitive resin film for an interlayer insulating layer, comprising a photosensitive resin composition as described in any one of [1] to
[11] .
[16] A multilayer printed wiring board comprising an interlayer insulating layer formed using a photosensitive resin composition as described in any one of [1] to
[11] .
[17] A multilayer printed wiring board comprising an interlayer insulating layer formed using a photosensitive resin film as described in
[14] .
[18] A semiconductor package having: a multilayer printed wiring board as described in
[16] or
[17] ; and a semiconductor element.
[19] A method for manufacturing a multilayer printed circuit board, comprising the following (1) to (4). (1): The photosensitive resin film as described in
[14] is laminated onto one or both sides of the circuit board. (2): An interlayer insulating layer with vias is formed by exposing and developing the laminated photosensitive resin film in (1). (3): Roughen the vias and the interlayer insulation layer. (4): A circuit pattern is formed on the interlayer insulating layer. [The effects of the invention]
[0011] According to this disclosure, a photosensitive resin composition with excellent via resolution, adhesion strength to copper plating, electrical insulation reliability, and resistance to desmearing can be provided; a photosensitive resin composition for forming photosensitive vias and a photosensitive resin composition for interlayer insulating layers can also be provided. Furthermore, a photosensitive resin film comprising the aforementioned photosensitive resin composition and a photosensitive resin film for interlayer insulating layers can be provided; a multilayer printed circuit board and a semiconductor package containing an interlayer insulating layer formed using the aforementioned photosensitive resin composition or the aforementioned photosensitive resin film can also be provided. Furthermore, a method can be provided for efficiently manufacturing multilayer printed circuit boards (PCBs) with high-resolution vias, high adhesion strength between interlayer insulating layers and copper plating, and excellent electrical insulation reliability. The vias in the multilayer PCBs obtained by the manufacturing method disclosed herein can be fabricated to have a diameter smaller than that of vias formed by laser processing. Simple Explanation of the Diagram
[0012] Figure 1 is a schematic diagram showing one aspect of the manufacturing steps of the multilayer printed circuit board of this embodiment. Implementation
[0013] Within the numerical range described in this specification, the upper or lower limit of the numerical range can also be replaced by the values shown in the embodiments. Furthermore, the lower and upper limits of the numerical range can be arbitrarily combined with the lower or upper limits of other numerical ranges. In the description of the numerical range "AA~BB", the values AA and BB at both ends are included within the numerical range as the lower and upper limits, respectively. In this specification, for example, "10 or more" refers to a value of 10 or more, and the same applies to cases where the value differs. Similarly, for example, "10 or less" refers to a value of 10 or less, and the same applies to cases where the value differs. Furthermore, in this specification, the content of each component in the photosensitive resin composition, in the presence of multiple substances equivalent to each component, refers to the total content of the multiple substances present in the photosensitive resin composition unless otherwise specified. In this specification, "ring-forming carbon number" refers to the number of carbon atoms required to form the ring, excluding the number of carbon atoms of substituents present in the ring. For example, the ring-forming carbon number of the cyclohexane skeleton and the methylcyclohexane skeleton is 6. The expression "(meth)acrylic acid XX" refers to one or both of acrylic acid XX and its corresponding methacrylic acid XX. Additionally, "(meth)acrylyl" refers to one or both of acrylyl and methacrylyl. Furthermore, any combination of the items described in this specification is also included in this embodiment.
[0014] [Photosensitive resin composition, photosensitive resin composition for forming photosensitive vias, and photosensitive resin composition for interlayer insulating layers] The photosensitive resin composition of this embodiment (hereinafter sometimes simply referred to as this embodiment) is a photosensitive resin composition containing (A) a photopolymerizable compound having an vinyl unsaturated group, (B) a photopolymerization initiator and (F) an inorganic filler. In the photosensitive resin composition, the (A) photopolymerizable compound having an vinyl unsaturated group includes (A1) a photopolymerizable compound having an vinyl unsaturated group, an acid substituent and an alicyclic skeleton. The (F) inorganic filler includes an inorganic filler that has been surface-treated with a coupling agent that does not have at least one functional group selected from the group consisting of amine and (meth)acrylic groups. Furthermore, in this specification, the components are sometimes referred to as component (A), component (B), component (F), component (A1), etc., and other components are sometimes abbreviated in the same way. In this specification, "resin component" refers to components (A) and (B), etc., and also includes other components that may be included as needed (e.g., components (C), (D), (E), and (H), etc.), but excludes inorganic compounds such as inorganic fillers (F) and pigments (G). In addition, "solid component" refers to the non-volatile components in the photosensitive resin composition, excluding volatile substances such as water and solvents, and indicates the components that do not volatilize and remain when the resin composition is dried. It also includes components that are liquid, syrupy, or waxy at room temperature around 25°C.
[0015] The photosensitive resin composition of this embodiment is suitable for via formation using photolithography (also known as photosensitive via formation), therefore, this disclosure also provides a photosensitive resin composition for photosensitive via formation. Furthermore, the photosensitive resin composition of this embodiment exhibits excellent via resolution, adhesion strength to copper plating, electrical insulation reliability, and resistance to desmearing, and is effectively used as an interlayer insulating layer in multilayer printed circuit boards. Therefore, this disclosure also provides a photosensitive resin composition for interlayer insulating layers. In this specification, the term "photosensitive resin composition" also includes photosensitive resin compositions for forming photosensitive vias and photosensitive resin compositions for interlayer insulating layers. Furthermore, the photosensitive resin composition of this embodiment can be effectively used as a negative photosensitive resin composition. The following is a detailed description of the components that may be contained in the photosensitive resin composition of this embodiment.
[0016] <(A) Photopolymerizable compounds with vinyl unsaturated groups> From the viewpoint of adhesion strength to copper plating, the photosensitive resin composition of this embodiment includes a photopolymerizable compound having an vinyl unsaturated group as component (A). Examples of vinyl unsaturated groups in component (A) include: vinyl, allyl, propargyl, butenyl, ethynyl, phenylethynyl, maleimino, nadicimino, (meth)acrylyl, etc. (meth)acrylyl is preferred as the vinyl unsaturated group. In this embodiment, component (A) includes "(A1) a photopolymerizable compound having an ethylene unsaturated group, an acidic substituent, and an alicyclic skeleton" as described later. By including component (A1) in component (A), it becomes a photosensitive resin composition with excellent via resolution, adhesion strength to copper plating, electrical insulation reliability, and resistance to descaling. The following is a detailed description starting with component (A1).
[0017] ((A1) Photopolymerizable compounds that also possess vinyl unsaturated groups, acidic substituents, and alicyclic skeletons) The vinyl unsaturated group present in component (A1) can be the same as the vinyl unsaturated group, preferably selected from at least one group consisting of vinyl, allyl, propargyl, butenyl, ethynyl, phenylethynyl, maleimino, nadicimino and (meth)acrylyl, more preferably vinyl, allyl, (meth)acrylyl, and even more preferably (meth)acrylyl. The acidic substituents present in component (A1) are preferably selected from at least one of the group consisting of carboxyl, sulfonic acid, phenolic hydroxyl, etc., and more preferably carboxyl.
[0018] From the viewpoints of via resolution, adhesion strength to copper plating, electrical insulation reliability, and resistance to descaling, the cycloaliphatic skeleton of component (A1) is preferably a cycloaliphatic skeleton with 5 to 20 carbon atoms, more preferably a cycloaliphatic skeleton with 5 to 18 carbon atoms, even more preferably a cycloaliphatic skeleton with 6 to 18 carbon atoms, particularly preferably a cycloaliphatic skeleton with 8 to 14 carbon atoms, and most preferably a cycloaliphatic skeleton with 8 to 12 carbon atoms. Furthermore, from the viewpoints of via resolution, adhesion strength to copper plating, electrical insulation reliability, and resistance to descaling, the alicyclic skeleton preferably contains two or more rings, more preferably two to four rings, and even more preferably three rings. Examples of alicyclic skeletons with one ring include cyclohexane and cyclohexene skeletons. Examples of alicyclic skeletons with two or more rings include norbornene, decahydronaphthalene, bicycloundecane, and saturated dicyclopentadiene skeletons. From the viewpoints of via resolution, adhesion strength to copper plating, electrical insulation reliability, and resistance to descaling, the alicyclic skeleton is preferably a saturated dicyclopentadiene skeleton, and more preferably an alicyclic skeleton (saturated dicyclopentadiene skeleton) represented by the following general formula (a). [Chemistry 1] (In general formula (a), R A1 represents an alkyl group with 1 to 12 carbon atoms, which can be substituted at any position in the alicyclic skeleton; m1 is an integer from 0 to 6; * represents the bonding site with other structures)
[0019] In general formula (a), examples of alkyl groups having 1 to 12 carbon atoms represented by RA1 include: methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tributyl, n-pentyl, etc. Preferably, the alkyl group is an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and even more preferably methyl. m1 is an integer from 0 to 6, preferably an integer from 0 to 2, and even more preferably 0. When m1 is an integer from 2 to 6, multiple Ra1 atoms can be the same or different. Furthermore, multiple Ra1 atoms can be substituted on the same carbon atom as much as possible, or they can be substituted on different carbon atoms. *For bonding sites with other structures, any carbon atom on the alicyclic framework can be used for bonding, preferably using carbon atom represented by 1 or 2 in the following general formula (a') to carbon atom represented by any one of 3 to 5 respectively. [Chemistry 2] (In general formula (a'), RA1, m1 and * are the same as in general formula (a))
[0020] Examples of the (A1) component include "(A1-1) acid-modified epoxy derivatives containing vinyl unsaturated groups and alicyclic skeletons" and "(A1-2) acid-modified phenolic varnishes or cresol varnishes resins containing vinyl unsaturated groups and alicyclic skeletons". • The “(A1-1) acid-modified epoxy derivative containing ethylene unsaturated groups and an alicyclic skeleton” is obtained by reacting a compound obtained by modifying an epoxy resin containing an alicyclic skeleton (a1) with an organic acid containing ethylene unsaturated groups (a2) [hereinafter, sometimes referred to as component (A')] with a polyacid anhydride containing saturated or unsaturated groups (a3); • The “(A1-2) acid-modified phenolic varnish or cresol varnish resin containing ethylene unsaturated groups and alicyclic skeleton” is formed by reacting modified phenolic varnish type epoxy resin with (a2) an organic acid containing ethylene unsaturated groups and (a4) a polyacid anhydride containing alicyclic skeleton and saturated or unsaturated groups. The modified phenolic varnish type epoxy resin is formed by addition polymerization of phenolic varnish resin or cresol varnish resin with at least one selected from the group consisting of ethylene oxide and propylene oxide. From the viewpoint that the (A1) component can be alkaline developed and has excellent resolution of vias, adhesion strength to copper plating, electrical insulation reliability and resistance to descaling, it is preferred to be "(A1-1) acid-modified epoxy derivative containing ethylene unsaturated groups and alicyclic skeleton". The "(A1-1) acid-modified epoxy derivative containing ethylene unsaturated groups and alicyclic skeleton" is obtained by reacting the compound [(A') component] obtained by modifying the epoxy resin containing the alicyclic skeleton of (a1) with an organic acid containing ethylene unsaturated groups of (a2) with a polybasic acid anhydride containing saturated or unsaturated groups of (a3). First, the raw materials that can be used in the manufacture of "(A1-1) acid-modified epoxy derivatives containing ethylene unsaturated groups and alicyclic skeletons" are described in detail.
[0021] -(a1) Epoxy resins containing alicyclic skeletons- The epoxy resin containing the alicyclic skeleton in (a1) is preferably an epoxy resin having two or more epoxy groups. Epoxy resins are classified into glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, etc. Among these, glycidyl ether type epoxy resins are preferred.
[0022] In this embodiment, an epoxy resin having at least an alicyclic backbone is used as the epoxy resin. The alicyclic backbone can be described as being the same as that of component (A1), and the preferred embodiment is also the same. The epoxy resin containing the alicyclic skeleton (a1) is preferably the epoxy resin represented by the following general formula (a1-1). Alternatively, the epoxy resin having the structural unit represented by the following general formula (a1-2) is also preferred. [Chemistry 3] (In general formula (a1-1), RA1 represents an alkyl group having 1 to 12 carbon atoms, which can be substituted at any position in the alicyclic skeleton; RA2 represents an alkyl group having 1 to 12 carbon atoms; m1 is an integer from 0 to 6, m2 is an integer from 0 to 3; n is 0 to 10) [Chemistry 4] (In general formula (a1-2), R A1 represents an alkyl group with 1 to 12 carbon atoms, which can be substituted at any position in the alicyclic skeleton; m1 is an integer from 0 to 6)
[0023] In general formulas (a1-1) and (a1-2), RA1 is the same as RA1 in general formula (a), and the better state is also the same. Examples of alkyl groups having 1 to 12 carbon atoms, represented by RA2 in general formula (a1-1), include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tributyl, n-pentyl, etc. Preferably, the alkyl group has 1 to 6 carbon atoms, more preferably 1 to 3 carbon atoms, and even more preferably methyl. The m1 in general formula (a1-1) and general formula (a1-2) is the same as the m1 in general formula (a), and the better state is also the same. In the general formula (a1-1), m2 is an integer from 0 to 3, preferably 0 or 1, and even more preferably 0. In general formula (a1-1), n represents the number of structural units within the parentheses, ranging from 0 to 10. Typically, epoxy resin is a mixture of structural units with varying numbers within the parentheses; therefore, in this case, n is represented by the average value of the mixture. Preferably, n is 2 to 10.
[0024] As an epoxy resin containing an alicyclic skeleton (a1), commercially available products can also be used. Examples of commercially available products include: XD-1000 (manufactured by Nippon Kayaku Co., Ltd., trade name), EPICLON HP-7200L, EPICLON HP-7200, EPICLON HP-7200HH, EPICLON HP-7200HHH (manufactured by DIC Co., Ltd., trade name, "EPICLON" is a registered trademark), etc.
[0025] As (a1) epoxy resin, epoxy resins other than those having an alicyclic skeleton (hereinafter, sometimes referred to as other epoxy resins) may be used. Examples of other epoxy resins include: bisphenol-based epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, and bisphenol S type epoxy resin; bisphenol-based phenolic varnish-type epoxy resins such as bisphenol A phenolic varnish-type epoxy resin and bisphenol F phenolic varnish-type epoxy resin; and phenolic varnish-type epoxy resins other than those described in the bisphenol-based phenolic varnish-type epoxy resins, such as phenolic varnish-type epoxy resin, cresol phenolic varnish-type epoxy resin, and biphenyl phenolic varnish-type epoxy resin. Epoxy resins; phenolic aralkyl type epoxy resins; biphenyl aralkyl type epoxy resins; stilbene type epoxy resins; naphthalene type epoxy resins, naphthol phenolic varnish type epoxy resins, naphthol type epoxy resins, naphthol aralkyl type epoxy resins, naphthyl ether type epoxy resins, and other naphthalene-containing skeleton epoxy resins; biphenyl type epoxy resins; xylylene type epoxy resins; dihydroanthracene type epoxy resins; aliphatic chain epoxy resins; rubber-modified epoxy resins, etc.
[0026] -(a2) Organic acids containing ethylene unsaturated groups- There are no particular limitations on the organic acid containing the vinyl unsaturated group in (a2), but it is preferably a monocarboxylic acid containing the vinyl unsaturated group. The vinyl unsaturated group is as described in the description of the vinyl unsaturated group in component (A1). Examples of monocarboxylic acids containing an ethylene unsaturated group include: acrylic acid; acrylic acid dimers, methacrylic acid, β-furfurylic acid, β-styrylic acid, cinnamic acid, crotonic acid, α-cyanocinonic acid, and other acrylic acid derivatives; half-ester compounds that are the reaction products of hydroxyl-containing acrylates and diacid anhydrides; and half-ester compounds that are the reaction products of monoglycidyl ethers or monoglycidyl esters containing ethylene unsaturated groups and diacid anhydrides. Among these, acrylic acid is preferred. (a2) Components may be used alone or in combination with two or more.
[0027] The half-ester compound can be obtained, for example, by reacting a hydroxyl-containing acrylate, a monoglycidyl ether containing an vinyl unsaturated group, or a monoglycidyl ether containing an vinyl unsaturated group with a dicarboxylic anhydride in an equal molar ratio.
[0028] Examples of hydroxyl-containing acrylates, vinyl unsaturated monoglycidyl ethers, and vinyl unsaturated monoglycidyl esters used in the synthesis of the half-ester compound, as an example of component (a2), include: hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol pentaacrylate, dipentaerythritol pentamethacrylate, glycidyl acrylate, glycidyl methacrylate, etc.
[0029] The diacid anhydride used in the synthesis of the half-ester compound may contain either a saturated group or an unsaturated group. Examples of diacid anhydrides include: succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, itaconic anhydride, etc.
[0030] While there are no particular limitations, in the reaction between component (a1) and component (a2), component (a2) is preferably reacted at a ratio of 0.6 to 1.05 equivalents relative to the epoxy group equivalent of component (a1), and may also be reacted at a ratio of 0.8 to 1.0 equivalents. By reacting at this ratio, there is a tendency to improve photopolymerization, i.e., increase photosensitivity, and improve the resolution of the pores.
[0031] The (a1) component and the (a2) component are soluble in organic solvents to react. Examples of organic solvents include: ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ether compounds such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha.
[0032] Furthermore, in order to promote the reaction between component (a1) and component (a2), a catalyst is preferably used. Examples of such catalysts include: amine catalysts such as triethylamine and benzylmethylamine; quaternary ammonium salt catalysts such as methyltriethylammonium chloride, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide, and benzyltrimethylammonium iodide; and phosphine catalysts such as triphenylphosphine. Among these, phosphine catalysts are preferred, and triphenylphosphine is even more preferred. Relative to a total of 100 parts by mass of component (a1) and component (a2), the amount of catalyst used is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 2 parts by mass. At such amounts, there is a tendency to promote the reaction between component (a1) and component (a2).
[0033] In addition, to prevent polymerization during the reaction, it is preferable to use polymerization inhibitors. Examples of polymerization inhibitors include hydroquinone, methyl hydroquinone, hydroquinone monomethyl ether, catechol, and gallol. In the case of using a polymerization inhibitor, from the viewpoint of improving the storage stability of the composition, the amount of polymerization inhibitor used is preferably 0.01 to 1 part by mass, more preferably 0.02 to 0.8 parts by mass, and even more preferably 0.05 to 0.5 parts by mass, relative to a total of 100 parts by mass of the (a1) and (a2) components.
[0034] From a productive point of view, the reaction temperature of component (a1) and component (a2) is preferably 60°C to 150°C, more preferably 70°C to 120°C, and even more preferably 80°C to 110°C.
[0035] As described above, it is presumed that component (A'), formed by reacting component (a1) with component (a2), is a compound having hydroxyl groups formed by the ring-opening addition reaction of the epoxy group of component (a1) with the carboxyl group of component (a2).
[0036] -(a3) Polyacid Anhydrides- The component (a3) may contain either saturated or unsaturated groups. Examples of components (a3) include: succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, itaconic anhydride, etc. Among these, tetrahydrophthalic anhydride is preferred from the viewpoint of pore resolution.
[0037] It is speculated that by reacting the obtained (A') component with the (a3) component containing saturated or unsaturated groups, the hydroxyl groups of (A') component (including the hydroxyl groups originally present in the (a1) component) and the anhydride groups of the (a3) component are semi-esterified to form "(A1-1) acid-modified epoxy derivative containing ethylene unsaturated groups and alicyclic skeleton".
[0038] In the reaction between component (A') and component (a3), for example, relative to 1 equivalent of the hydroxyl group in component (A'), component (a3) reacts by 0.1 equivalent to 1.0 equivalent, thereby adjusting the acid value of the epoxy derivative containing ethylene unsaturated groups and alicyclic skeleton modified by (A1-1). (A1-1) The acid value of the acid-modified epoxy derivative containing vinyl unsaturated groups and an alicyclic skeleton is preferably 20 mgKOH / g to 150 mgKOH / g, more preferably 30 mgKOH / g to 120 mgKOH / g, and even more preferably 40 mgKOH / g to 100 mgKOH / g. If the acid value is above 20 mgKOH / g, the photosensitive resin composition tends to have excellent solubility in dilute alkaline solutions; if it is below 150 mgKOH / g, the electrical properties of the hardened film tend to be improved.
[0039] From a productive point of view, the reaction temperature of component (A') and component (a3) is preferably 50°C to 150°C, more preferably 60°C to 120°C, and even more preferably 70°C to 100°C.
[0040] Based on the above, there are no particular limitations on the photopolymerizable compound (A1) which has an ethylene unsaturated group, an acidic substituent and an alicyclic skeleton, but it is preferably represented by the following general formula (A-1). [Chemistry 5] (In general formula (A-1), RA1 represents an alkyl group having 1 to 12 carbon atoms, which can be substituted at any position in the alicyclic skeleton; RA2 represents an alkyl group having 1 to 12 carbon atoms; RA3 is an organogroup having an ethylene unsaturated group, an organogroup having an ethylene unsaturated group and an acidic substituent, or a glycidyl group, at least one RA3 being an organogroup having an ethylene unsaturated group and an acidic substituent; m1 is an integer from 0 to 6, m2 is an integer from 0 to 3; n is 0 to 10)
[0041] In the general formula (A-1), RA1, RA2, m1, m2 and n are the same as those in the general formula (a1-1), and preferably also the same. RA3 is defined as described above, but is defined as follows: it corresponds to the site formed by the reaction of the glycidyl group in the general formula (a1-1) with components (a2) and (a3), while also considering that a portion of the glycidyl group remains unreacted. Specifically, "organic group having an ethylene unsaturated group" as one option of RA3 is a group derived from component (a2), and "organic group having an ethylene unsaturated group and an acidic substituent" as another option of RA3 is a group derived from components (a2) and (a3). That is, if components (a2) and (a3) react with all glycidyl groups in the general formula (a1-1), then RA3 becomes an "organic group having an ethylene unsaturated group and an acidic substituent". However, only the part of the glycidyl group that reacts with component (a2) becomes an "organic group having an ethylene unsaturated group", and the part of the glycidyl group that does not react with either component (a2) or component (a3) becomes a "glycidyl group".
[0042] Secondly, a brief description is given of the raw materials that can be used in the manufacture of the "(A1-2) acid-modified phenolic varnish or cresol varnish resin containing ethylene unsaturated groups and alicyclic skeleton". One of the raw materials is a modified phenolic varnish-type epoxy resin obtained by addition polymerization of phenolic varnish resin or cresol varnish resin with at least one selected from the group consisting of ethylene oxide and propylene oxide. In this addition polymerization, a catalyst is preferably used. Examples of catalysts include: metallic sodium, sodium methoxide, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium phenolate, and various Lewis acids. There are no particular limitations on the weight average molecular weight of phenolic varnish resin and cresol varnish resin, but it is preferably 500 to 30,000, and more preferably 1,000 to 10,000, respectively. Furthermore, in this specification, the weight average molecular weight (and number average molecular weight) are values obtained by gel permeation chromatography (GPC) using tetrahydrofuran as the solvent and converted using standard polystyrene; more specifically, they are values determined according to the methods described below. There are no particular restrictions on the reaction temperature in the addition polymerization, which can be carried out in the range of 60℃ to 230℃. Regarding the addition polymerization, any known method can be used or applied, and there are no limitations on the method itself. Modified phenolic varnish-type epoxy resin can be obtained by the addition polymerization.
[0043] As for the "(a2) organic acid containing an ethylene unsaturated group" that reacts with the modified phenolic varnish-type epoxy resin obtained therein, it can be described in the same way as the description of the organic acid containing an ethylene unsaturated group in (a2). Furthermore, the alicyclic skeleton contained in the "(a4) polycyclic anhydride containing an alicyclic skeleton and saturated or unsaturated groups" that reacts with the obtained modified phenolic varnish-type epoxy resin is preferably an alicyclic skeleton with 5 to 20 carbon atoms, more preferably an alicyclic skeleton with 5 to 15 carbon atoms, even more preferably an alicyclic skeleton with 5 to 10 carbon atoms, and particularly preferably an alicyclic skeleton with 5 to 8 carbon atoms. This alicyclic skeleton may be a single ring or may contain two or more rings, but is preferably a single ring. As this alicyclic skeleton, a cyclohexane skeleton, a cyclohexene skeleton, etc., is preferred, and a cyclohexene skeleton is even more preferred. Examples of "(a4) polycyclic anhydrides containing an alicyclic skeleton and saturated or unsaturated groups" include: tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, etc. Among these, tetrahydrophthalic anhydride and phthalic anhydride are preferred, and tetrahydrophthalic anhydride is even more preferred. There are no particular restrictions on the conditions for reacting the modified phenolic varnish-type epoxy resin with (a2) an organic acid containing an ethylene unsaturated group and (a4) a polycyclic anhydride containing an alicyclic skeleton and either a saturated or unsaturated group. For example, methods such as reacting the modified phenolic varnish-type epoxy resin with component (a2) in the presence of a catalyst at 20°C to 100°C, and then reacting it with component (a4) at 20°C to 100°C, can be cited as needed.
[0044] ((A1) Molecular weight of photopolymerizable compounds that also possess ethylene unsaturated groups, acidic substituents, and alicyclic skeletons) The weight-average molecular weight (Mw) of component (A1) is preferably 1,000 to 30,000, more preferably 2,000 to 25,000, and even more preferably 3,000 to 18,000. Within this range, the adhesion strength, heat resistance, and electrical insulation reliability with copper plating are improved. Particularly, the weight-average molecular weight (Mw) of the acid-modified epoxy derivative containing ethylene unsaturated groups and an alicyclic skeleton of (A1-1) is within the aforementioned range. Here, the weight-average molecular weight (and number-average molecular weight) is a value determined by gel permeation chromatography (GPC) (manufactured by Tosoh Corporation) using a standard curve of standard polystyrene, and more specifically, a value determined according to the method described below. <Methods for determining weight-average molecular weight and number-average molecular weight> The weight-average molecular weight and number-average molecular weight were determined using the GPC measuring apparatus and conditions described below. The values converted from the standard curve of standard polystyrene were used as the weight-average molecular weight or number-average molecular weight. In addition, in the preparation of the standard curve, a set of 5 samples ("PStQuick MP-H" and "PStQuick B", manufactured by Tosoh Corporation) was used as the standard polystyrene. (GPC measuring device) GPC device: High-speed GPC device "HCL-8320GPC", detector is differential refractometer or ultraviolet (UV), manufactured by Tosoh Corporation. Tube String: TSKgel SuperMultipore HZ-H (tube length: 15 cm, tube inner diameter: 4.6 mm), manufactured by Tosoh Corporation. (Measurement conditions) Solvent: Tetrahydrofuran (THF) Measurement temperature: 40℃ Flow rate: 0.35 mL / min Sample concentration: 10 mg / THF 5 mL Injection volume: 20 μL
[0045] ((A2-1) Acid-modified epoxy derivatives containing vinyl unsaturated groups without an alicyclic skeleton) As a photopolymerizable compound having an ethylene unsaturated group (A), it may also be a form that includes "(A2-1) an acid-modified epoxy derivative containing an ethylene unsaturated group without an alicyclic skeleton". The "(A2-1) an acid-modified epoxy derivative containing an ethylene unsaturated group without an alicyclic skeleton" is obtained by reacting a compound obtained by modifying an epoxy resin (a21) (wherein, an epoxy resin without an alicyclic skeleton) with an organic acid containing an ethylene unsaturated group (a22) with a polyacid anhydride containing a saturated or unsaturated group (a23).
[0046] As for the epoxy resin mentioned in (a21), if it is an epoxy resin without an alicyclic skeleton, there are no other particular limitations, and examples include: glycidyl ether type epoxy resin, glycidyl amine type epoxy resin, glycidyl ester type epoxy resin, etc. Among these, glycidyl ether type epoxy resin is preferred. In addition, the epoxy resin (a21) is also classified into various epoxy resins according to the different main skeletons, and among the various types of epoxy resins, they are further classified as follows. Specifically, these include bisphenol-based epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, and bisphenol S type epoxy resin; bisphenol-based phenolic varnish epoxy resins such as bisphenol A phenolic varnish epoxy resin and bisphenol F phenolic varnish epoxy resin; phenolic varnish epoxy resins other than the aforementioned bisphenol-based phenolic varnish epoxy resins, such as phenolic varnish epoxy resin, cresol phenolic varnish epoxy resin, and biphenyl phenolic varnish epoxy resin; phenolic aralkyl type epoxy resin; stilbene type epoxy resin; naphthalene-type epoxy resin, naphthol phenolic varnish epoxy resin, naphthol type epoxy resin, naphthol aralkyl type epoxy resin, and naphthyl ether type epoxy resin containing a naphthalene skeleton; biphenyl type epoxy resin; biphenyl aralkyl type epoxy resin; xylylene type epoxy resin; dihydroanthracene type epoxy resin; aliphatic chain epoxy resin; and rubber-modified epoxy resin. Among these, bisphenol-based phenolic varnish-type epoxy resin is preferred, and more preferably bisphenol F phenolic varnish-type epoxy resin.
[0047] As for the organic acid containing an ethylene unsaturated group (a22) and the polybasic acid anhydride containing a saturated or unsaturated group (a23), they can be described in the same manner as the descriptions of the organic acid containing an ethylene unsaturated group (a2) and the polybasic acid anhydride containing a saturated or unsaturated group (a3), and the preferred forms are also the same. Furthermore, as a method for reacting the compound obtained by modifying component (a21) using component (a22) with component (a23), the method of reacting the compound obtained by modifying component (a1) using component (a2) with component (a3) can be referred to.
[0048] As an acid-modified epoxy derivative containing an ethylene unsaturated group without an alicyclic skeleton (A2-1), commercially available products can also be used. Examples of commercially available products include: CCR-1218H, CCR-1159H, CCR-1222H, PCR-1050, TCR-1335H, ZAR-1035, ZAR-2001H, UXE-3024, ZFR-1185, ZCR-1569H, ZXR-1807, ZCR-6000, ZCR-8000 (manufactured by Nippon Kayaku Co., Ltd., trade names), UE-9000, UE-EXP-2810PM, UE-EXP-3045 (manufactured by DIC Co., Ltd., trade names), etc.
[0049] When component (A) contains both component (A1) (or component (A1-1)) and component (A2-1), from the viewpoint of balancing via resolution, copper plating adhesion strength, electrical insulation reliability, and resistance to descaling, the content ratio of component (A1) (or component (A1-1)) to component (A2-1) [((A1) or (A1-1)) / (A2-1)] by mass is preferably 20 / 80 to 99 / 1, more preferably 50 / 50 to 99 / 1, further preferably 60 / 40 to 99 / 1, particularly preferably 60 / 40 to 85 / 15, and most preferably 65 / 35 to 80 / 20.
[0050] ((A2-2)Styrene-maleic acid resin) As a photopolymerizable compound having an ethylene unsaturated group (A), it can also be used in combination with styrene-maleic anhydride copolymers such as (meth)acrylate hydroxyethyl ester modified resins, forming "(A2-2) styrene-maleic acid resins". This (A2-2) component does not contain an alicyclic skeleton. The (A2-2) component can be used alone or in combination with two or more.
[0051] ((A2-3) Epoxy polyurethane resin) Additionally, as a photopolymerizable compound having an ethylene unsaturated group (A), it can also be used in conjunction with "(A2-3) epoxy polyurethane resin," which is obtained by reacting a compound (e.g., component (A')) obtained by modifying the epoxy resin (a21) with an organic acid containing an ethylene unsaturated group (a22) with an isocyanate compound. Component (A2-3) does not contain an alicyclic skeleton. Component (A2-3) can be used alone or in combination with two or more.
[0052] (other than the ingredient mentioned in (A)) From the viewpoint of improving chemical resistance after curing (exposure) and increasing the difference in developer resistance between the exposed and unexposed areas, the photopolymerizable compound (A) having an vinyl unsaturated group is preferably in the following form: Specifically, the photopolymerizable compound (A) having an vinyl unsaturated group preferably comprises at least one selected from the group consisting of (Ai) a monofunctional vinyl monomer having one polymerizable vinyl unsaturated group, (Aii) a difunctional vinyl monomer having two polymerizable vinyl unsaturated groups, and (Aiii) a polyfunctional vinyl monomer having at least three polymerizable vinyl unsaturated groups, and more preferably, a form comprising the (Aiii) component. Components (Ai) to (Aiii) are preferably those with a molecular weight of 1,000 or less. In this embodiment, components (Ai) to (Aiii) do not comprise component (A).
[0053] ((Ai) monofunctional vinyl monomer) Examples of monofunctional vinyl monomers having a polymerizable vinyl unsaturated group include (meth)acrylic acid and alkyl (meth)acrylates. Examples of such alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and hydroxyethyl (meth)acrylate. The (Ai) component may be used alone or in combination with two or more components.
[0054] ((Aii) difunctional vinyl monomer) Examples of difunctional vinyl monomers having two polymerizable vinyl unsaturated groups include: polyethylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, polypropylene glycol di(meth)acrylate, 2,2-bis(4-(meth)acryloxypolyethoxypolypropoxyphenyl)propane, bisphenol A diglycidyl ether di(meth)acrylate, etc. The (Aii) component can be used alone or in combination with two or more components.
[0055] ((Aiii) Multifunctional vinyl monomers) Examples of polyfunctional vinyl monomers having at least three polymerizable vinyl unsaturated groups include: trimethylolpropane tri(meth)acrylate and other (meth)acrylate compounds having a backbone derived from trimethylolpropane; tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate and other (meth)acrylate compounds having a backbone derived from tetramethylolmethane; pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate and other (meth)acrylate compounds having a backbone derived from pentaerythritol; dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate and other (meth)acrylate compounds having a backbone derived from dipentaerythritol; di-trimethylolpropane tetra(meth)acrylate and other (meth)acrylate compounds having a backbone derived from dimethylolpropane; and (meth)acrylate compounds having a backbone derived from diglycerol. Of these, from the viewpoint of improving chemical resistance after curing (exposure) and increasing the difference in developer resistance between the exposed and unexposed areas, a (meth)acrylate compound having a backbone derived from dipentaerythritol is preferred, and a dipentaerythritol penta(meth)acrylate is even more preferred. Component (Aiii) may be used alone or in combination with two or more. Here, the so-called "(meth)acrylate compound having a skeleton derived from XXX" (where XXX is the name of the compound) refers to the esterification of XXX and (meth)acrylic acid, which also contains compounds modified by alkyloxy groups.
[0056] (A) Content of component (A) There are no particular restrictions on the content (total content) of the components. From the viewpoint of heat resistance, electrical properties and chemical resistance, based on the total solid content of the photosensitive resin composition, it is preferably 0.1% to 60% by mass, more preferably 0.1% to 55% by mass, even more preferably 1% to 50% by mass, particularly preferably 5% to 45% by mass, most preferably 15% to 45% by mass, and can be 30% to 45% by mass.
[0057] There are no particular limitations on component (A), but from the viewpoint of photosensitivity, it is preferable to use both component (A1) and component (Aiii). In this case, the content ratio of component (A1) to component (Aiii) [(A1) / (Aiii)] (mass ratio) is preferably 2 to 20, more preferably 2 to 15, further preferably 2.5 to 10, and particularly preferably 3 to 6. In addition, from the viewpoints of via resolution, adhesion strength to copper plating, electrical insulation reliability and resistance to descaling, the content ratio of component (A1) relative to the total amount of component (A) is preferably 20% to 95% by mass, more preferably 40% to 95% by mass, even more preferably 65% to 95% by mass, particularly preferably 70% to 95% by mass, and may be 80% to 95% by mass, or may be 80% to 90% by mass.
[0058] <(B) Photopolymerization initiators> As for component (B) used in this embodiment, there are no particular restrictions on whether it is a component (A) that can polymerize, and it can be appropriately selected from commonly used photopolymerization initiators. As component (B), examples include: benzoin, benzoin methyl ether, benzoin isopropyl ether, and other benzoin-based compounds; acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexylphenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinylphenyl)-1-butanone, 2-methyl-1-[4-( [Methylthiophenyl]-2-morpholino-1-propanone, N,N-dimethylaminoacetophenone and other acetophenone compounds; anthraquinone compounds such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-pentylanthraquinone, 2-aminoanthraquinone and other anthraquinone compounds; thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone and other thioxanthone compounds. Compounds; ketal compounds such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzophenone compounds such as methyl benzophenone, 4,4'-dichlorobenzophenone, 4,4'-bis(diethylamino)benzophenone, Michleck's ketone, and 4-benzoyl-4'-methyl diphenyl sulfide; acridine compounds such as 9-phenyl acridine and 1,7-bis(9,9'-acridyl)heptane; 2,4,6- Trimethylbenzyldiphenylphosphine oxide and other acetophosphine oxide compounds; oxime ester compounds such as 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzyl oxime), 1-[9-ethyl-6-(2-methylbenzyl)-9H-carbazole-3-yl]acetophenone-1-(O-acetyl oxime), and 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime]. Among these, acetophenone compounds and thioxanthone compounds are preferred, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone and 2,4-diethylthioxanthone are even more preferred. Acetophenone compounds have the advantages of being non-volatile and not easily becoming escaped gases, while thioxanthone compounds have the advantage of being photocurable in the visible light region. (B) Components may be used alone or in combination with two or more. When two or more are used in combination, it is preferable to use acetophenone-based compounds and thioxanthone-based compounds in combination, and even more preferably to use 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone and 2,4-diethylthioxanthone in combination.
[0059] ((B) Content of component) The content of component (B) is not particularly limited, but based on the total solid content of the photosensitive resin composition, it is preferably 0.1% to 15% by mass, more preferably 0.15% to 5% by mass, even more preferably 0.15% to 1.5% by mass, and particularly preferably 0.20% to 1.2% by mass. If the content of component (B) is 0.1% by mass or more, there is a tendency to reduce the possibility of the exposed portion dissolving during development in the interlayer insulating layer formed using the photosensitive resin composition; if it is 15% by mass or less, there is a tendency to improve heat resistance.
[0060] <(B') Photopolymerization initiator> The photosensitive resin composition of this embodiment may also contain the aforementioned component (B) and the photopolymerization initiator (B'). Examples of photopolymerization initiators (B') include: ethyl N,N-dimethylaminobenzoate, isoamyl N,N-dimethylaminobenzoate, pentyl-4-dimethylaminobenzoate, triethylamine, triethanolamine, and other tertiary amines. Component (B') may be used alone or in combination with two or more. When the photosensitive resin composition of this embodiment contains component (B'), the content of component (B') is preferably 0.01% to 20% by mass, more preferably 0.2% to 5% by mass, and even more preferably 0.3% to 2% by mass, based on the total amount of resin components in the photosensitive resin composition. Furthermore, the photosensitive resin composition of this embodiment may also be free of component (B').
[0061] <(C) Thermosetting Resins> The photosensitive resin composition of this embodiment may further contain a thermosetting resin as component (C), preferably. In this respect, component (C) does not contain anything equivalent to component (A), meaning that component (C) does not have vinyl unsaturated groups. The vinyl unsaturated groups described here can be explained in the same way as the vinyl unsaturated groups present in component (A). Furthermore, a substance having epoxy groups (such as epoxy-modified polybutadiene) may be included in component (C) while satisfying the condition of not having vinyl unsaturated groups. The photosensitive resin composition of this embodiment contains (C) thermosetting resin, which tends to improve not only the adhesion strength and insulation reliability with copper plating, but also the heat resistance. Examples of thermosetting resins include: epoxy resins, phenolic resins, unsaturated amide resins, cyanate ester resins, isocyanate ester resins, benzoxazine resins, oxetine resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, melamine resins, etc. However, these are not particularly limited to these, and known thermosetting resins may be used. Among these, epoxy resins are preferred. (C) Components may be used alone or in combination with two or more.
[0062] As an epoxy resin, it is preferable to have an epoxy resin having two or more epoxy groups. Epoxy resins are classified into glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, etc. Among these, glycidyl ether type epoxy resins are preferred.
[0063] Furthermore, epoxy resins are also classified into various types based on their main skeleton, and these epoxy resins are further classified as follows: Specifically, they are classified as follows: Bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, etc.; Bisphenol A phenolic varnish type epoxy resin, bisphenol F phenolic varnish type epoxy resin, etc.; Phenolic varnish type epoxy resin other than the aforementioned bisphenol phenolic varnish type epoxy resins, such as phenolic varnish type epoxy resin, cresol phenolic varnish type epoxy resin, biphenyl phenolic varnish type epoxy resin; Phenolic aralkyl type epoxy resin; Stilbene type epoxy resin; Naphthalene type epoxy resin; Epoxy resins containing naphthalene skeletons, including lipopolymer, naphthol phenolic varnish type epoxy resin, naphthol type epoxy resin, naphthol aralkyl type epoxy resin, and naphthyl ether type epoxy resin; biphenyl type epoxy resin; biphenyl aralkyl type epoxy resin; xylylene type epoxy resin; dihydroanthracene type epoxy resin; dicyclopentadiene type epoxy resin; alicyclic epoxy resin; heterocyclic epoxy resin; spirocyclic epoxy resin; cyclohexanediol type epoxy resin; trimethylol type epoxy resin; aliphatic chain epoxy resin; and rubber-modified epoxy resin, etc. (C) Components may be used alone or in combination with two or more.
[0064] Among these, particularly from the viewpoints of heat resistance, electrical insulation reliability, and adhesion strength to copper plating, bisphenol-based epoxy resins, naphthol-type epoxy resins, naphthyl ether-type epoxy resins, and cresol-phenolic varnish-type epoxy resins are preferred; more preferably, bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and biphenyl-type epoxy resins are preferred; even more preferably, bisphenol F-type epoxy resins and biphenyl-type epoxy resins are preferred; and especially preferably, biphenyl-type epoxy resins are preferred. These can also use commercially available products, such as: bisphenol A type epoxy resin ("jER828EL", "YL980" manufactured by Mitsubishi Chemical Corporation), bisphenol F type epoxy resin ("jER806H", "YL983U" manufactured by Mitsubishi Chemical Corporation), naphthalene type epoxy resin ("HP4032D", "HP4710" manufactured by DIC Corporation), naphthalene-containing skeleton type multifunctional epoxy resin ("NC7000" manufactured by Nippon Chemical Co., Ltd.), and naphthol type epoxy resin (Nippon Steel Chemical & Materials Co., Ltd.). Epoxy resins with biphenyl structures include "ESN-475V" manufactured by Nippon Chemical & Material Co., Ltd., "NC3000H" and "NC3500" manufactured by Nippon Chemical Co., Ltd., "YX4000HK" and "YL6121" manufactured by Mitsubishi Chemical Co., Ltd., anthracene-type epoxy resin ("YX8800" manufactured by Mitsubishi Chemical Co., Ltd.), glycerol-type epoxy resin ("ZX1542" manufactured by Nippon Chemical & Material Co., Ltd.), naphthyl ether-type epoxy resin ("EXA7311-G4" manufactured by DIC Co., Ltd.), and cresol phenolic varnish-type epoxy resin ("EPICLON N-680" manufactured by DIC Co., Ltd.).
[0065] In addition to the examples described above, epoxy-modified polybutadiene may also be used as component (C) of the epoxy resin. In particular, from the viewpoint of processability during the manufacture of printed circuit boards, it is preferable to use both an aromatic epoxy resin that is solid at room temperature and an epoxy resin that is liquid at room temperature as component (C). From this viewpoint, it is preferable to use the epoxy resin (aromatic epoxy resin that is solid at room temperature) and epoxy-modified polybutadiene (epoxy resin that is liquid at room temperature) as exemplified as the preferred combination. In this case, the content ratio of the two used (aromatic epoxy resin that is solid at room temperature / epoxy resin that is liquid at room temperature) by mass is preferably 95 / 5 to 60 / 40, more preferably 95 / 5 to 70 / 30, and even more preferably 95 / 5 to 80 / 20.
[0066] The epoxy-modified polybutadiene preferably has hydroxyl groups at the ends of the molecule, more preferably has hydroxyl groups at both ends of the molecule, and even more preferably has hydroxyl groups only at both ends of the molecule. In addition, there is no particular limitation on the number of hydroxyl groups in the epoxy-modified polybutadiene if it has more than one, preferably 1 to 5, more preferably 1 or 2, and even more preferably 2. From the viewpoint of adhesion strength, heat resistance, coefficient of thermal expansion and flexibility of copper plating, the epoxy-modified polybutadiene is preferably the epoxy-modified polybutadiene represented by the following general formula (C-1).
[0067] [Chemistry 6] (In the formula (C-1), a, b, and c represent the ratios of the structural units within the brackets, where a is 0.05~0.40, b is 0.02~0.30, and c is 0.30~0.80. Furthermore, a+b+c=1.00 and (a+c)>b are satisfied; y represents the number of structural units within the square brackets, which is an integer from 10 to 250.)
[0068] In the general formula (C-1), the bonding order of the structural units within the square brackets is different. That is, the structural units shown on the left, the structural units shown in the center, and the structural units shown on the right can be interleaved. When each is represented by (a), (b), and (c), there are various bonding sequences such as -[(a)-(b)-(c)]-[(a)-(b)-(c)-]-, -[(a)-(c)-(b)]-[(a)-(c)-(b)-]-, -[(b)-(a)-(c)]-[(b)-(a)-(c)-]-, -[(a)-(b)-(c)]-[(c)-(b)-(a)-]-, -[(a)-(b)-(a)]-[(c)-(b)-(c)-]-, -[(c)-(b)-(c)]-[(b)-(a)-(a)-]-. From the viewpoints of adhesion strength, heat resistance, coefficient of thermal expansion, and flexibility of copper plating, a is preferably 0.10~0.30, b is preferably 0.10~0.30, and c is preferably 0.40~0.80. Furthermore, from the same viewpoints, y is preferably an integer from 30 to 180.
[0069] In the general formula (C-1), commercially available epoxidized polybutadiene products with a=0.20, b=0.20, c=0.60, and y=10~250 integers can be listed as "Epolead (registered trademark) PB3600" (manufactured by Daicel Co., Ltd.).
[0070] (C) Content of component When the photosensitive resin composition of this embodiment contains component (C), its content is not particularly limited. Based on the total solid content of the photosensitive resin composition, it is preferably 5% to 70% by mass, more preferably 5% to 40% by mass, further preferably 7% to 30% by mass, and most preferably 10% to 30% by mass. If the content of component (C) is 5% by mass or more, there is a tendency to obtain sufficient cross-linking of the photosensitive resin composition, and to improve the adhesion strength and electrical insulation reliability with copper plating. On the other hand, if it is 70% by mass or less, there is a tendency to improve the resolution of perforations.
[0071] <(D) Elastomers> The photosensitive resin composition of this embodiment may contain an elastomer as component (D), or it may not, but it is preferable to contain an elastomer. By containing component (D), it tends to become a photosensitive resin composition with excellent through-hole resolution, adhesion strength to copper plating, and electrical insulation reliability. In addition, component (D) also has the effect of suppressing the reduction in flexibility and adhesion strength to copper plating caused by the strain (internal stress) inside the hardened material due to the hardening shrinkage of component (A). As component (D), it is preferably an elastomer that is liquid at 25°C. (D) Components may be used alone or in combination with two or more.
[0072] Examples of elastomers include styrene-based elastomers, olefin-based elastomers, polyester-based elastomers, urethane-based elastomers, polyamide-based elastomers, acrylic elastomers, and silicone-based elastomers, with at least one selected from these being preferred. These elastomers contain hard segment components and soft segment components; the former tends to contribute to heat resistance and strength, while the latter tends to contribute to flexibility and toughness. As component (D), in the examples described, from the viewpoint of compatibility, solubility, and adhesion strength to copper plating, it is preferably selected from at least one group consisting of olefin elastomers, polyester elastomers, and urethane elastomers, and more preferably from polyester elastomers. Furthermore, component (D) is further preferably selected from at least one group consisting of olefin elastomers, polyester elastomers, and urethane elastomers, and particularly preferably from polyester elastomers.
[0073] (Styrene-based elastomers) Examples of styrene-based elastomers include: styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, styrene-ethylene-butene-styrene block copolymers, and styrene-ethylene-propylene-styrene block copolymers. A single styrene-based elastomer may be used, or two or more may be used in combination. As components constituting styrene-based elastomers, examples include: styrene; styrene derivatives such as α-methylstyrene, 3-methylstyrene, 4-propylstyrene, and 4-cyclohexylstyrene. As a styrene-based elastomer, it is preferred to have a number average molecular weight of 1,000 to 50,000, and more preferably 3,000 to 20,000. In this specification, the number average molecular weight is a value obtained by gel permeation chromatography (GPC) using tetrahydrofuran as the solvent and converted using standard polystyrene. As a styrene-based elastomer, commercially available products can be used.
[0074] (Olefin-based elastomers) The olefin-based elastomer is, for example, a polymer or copolymer of α-olefins with 2 to 20 carbon atoms, such as ethylene, propylene, 1-butene, 1-hexene, and 4-methyl-pentene. Furthermore, the olefin-based elastomer may have hydroxyl groups at the molecular ends, preferably. One olefin-based elastomer may be used alone, or two or more may be used in combination. Examples of olefin-based elastomers include polyethylene, polybutadiene, hydroxyl-containing polybutadiene, hydroxyl-containing polyisopropylene, ethylene-propylene rubber (EPR), and ethylene-propylene-diene monomer (EPDM). Additionally, copolymers of the aforementioned α-olefins with 2 to 20 carbon atoms with non-conjugated dienes of 2 to 20 carbon atoms, such as dicyclopentadiene, 1,4-hexadiene, cyclooctadiene, methylene norbornene, ethylidene norbornene, butadiene, and isoprene, can also be listed. Furthermore, carboxyl-modified nitrile-butadiene rubber (NBR), formed by copolymerizing butadiene-acrylonitrile copolymer with methacrylic acid, can also be listed. As an olefin-based elastomer, it is preferably of a number average molecular weight of 1,000 to 8,000, and more preferably of 1,500 to 6,500. As an olefin-based elastomer, commercially available products can be used.
[0075] (Polyester-based elastomers) Examples of polyester elastomers include those obtained by polycondensation of dicarboxylic acids or their derivatives and diol compounds or their derivatives. A single polyester elastomer may be used, or two or more may be used in combination. Examples of dicarboxylic acids include: aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid; aromatic dicarboxylic acids in which the hydrogen atoms of the aromatic ring are substituted with methyl, ethyl, phenyl, or other methyl groups; aliphatic dicarboxylic acids with 2 to 20 carbon atoms such as adipic acid, sebacic acid, and dodecanedicarboxylic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid. From the viewpoint of adhesion to the substrate, dimer acids derived from natural sources are preferred as dicarboxylic acids. A single dicarboxylic acid may be used, or two or more may be used in combination. Examples of derivatives of the dicarboxylic acid include anhydrous forms of the dicarboxylic acid.
[0076] Examples of such diol compounds include: aliphatic diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, and 1,10-decanediol; alicyclic diols such as 1,4-cyclohexanediol; and aromatic diols represented by the following general formula (D-1). A single diol compound may be used alone, or two or more may be used in combination.
[0077] [Chemistry 7] (In general formula (D-1), XD1 represents an alkyl group with 1 to 10 carbon atoms, an alkylene group with 2 to 10 carbon atoms, an alkylene group with 4 to 8 carbon atoms, -O-, -S-, -SO2-; RD1 and RD2 independently represent halogen atoms or alkyl groups with 1 to 12 carbon atoms; p and q are independent integers from 0 to 4, and r is 0 or 1)
[0078] In general formula (D-1), examples of alkyl groups having 1 to 10 carbon atoms, represented by X D1, include methylene, 1,2-dimethylene, 1,3-trimethylene, 1,4-tetramethylene, and 1,5-pentamethylene. From the viewpoints of via resolution, adhesion strength to copper plating, and electrical insulation reliability, an alkyl group having 1 to 3 carbon atoms is preferred, and methylene is more preferred. Examples of alkylene groups with 2 to 10 carbon atoms, as represented by X D1, include: ethylene, propylene, isopropylene, butylene, isobutylene, pentylene, isopentylene, etc. From the viewpoints of via resolution, adhesion strength to copper plating, and electrical insulation reliability, isopropylene is preferred as the alkylene group. Examples of cycloalkyl groups with 4 to 8 carbon atoms represented by X D1 include: cyclopentyl, cyclohexyl, cyclooctyl, etc. As X D1, the preferred form described above is an alkylene group having 1 to 10 carbon atoms, an alkylene group having 2 to 10 carbon atoms, and more preferably a methylene or isopropylene group.
[0079] In general formula (D-1), the halogen atoms represented by RD1 and RD2 can be listed as: fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, etc. Examples of alkyl groups having 1 to 12 carbon atoms, represented by RD1 and RD2, include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tributyl, n-pentyl, etc. Preferably, the alkyl group is an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and even more preferably methyl. p and q are independent integers from 0 to 4, preferably 0 or 1 respectively. r can be 0 or 1, either of which is acceptable. When r is 0, it becomes the structure represented by the following general formula (D-1'). [Chemistry 8] (In general formula (D-1'), R, D1, and p are the same as in general formula (D-1), and the better state is also the same.)
[0080] Examples of aromatic diols represented by the general formula (D-1) include: bisphenol A, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-3-methylphenyl)propane, resorcinol, etc.
[0081] Furthermore, as a polyester elastomer, a multi-block copolymer in which an aromatic polyester (e.g., polybutylene terephthalate) portion is used as the hard segment component and an aliphatic polyester (e.g., polybutylene glycol) portion is used as the soft segment component can also be used, and such a multi-block copolymer is preferred. As such a multi-block copolymer, there are various grades of commercially available products depending on the type, ratio, and molecular weight of the hard and soft segments. Specifically, examples include: "Hytrel" (registered trademark) (manufactured by Toray-DuPont Co., Ltd.), "Pelprene" (registered trademark) (manufactured by Toyobo Co., Ltd.), "Espel" (registered trademark) and "Teslac" (registered trademark) (manufactured by Showa Denko Materials Co., Ltd.), etc.
[0082] As a polyester elastomer, it is preferred to have a number average molecular weight of 900 to 30,000, more preferably 1,000 to 25,000, and even more preferably 5,000 to 20,000.
[0083] (Carbamate-based elastomers) Examples of urethane-based elastomers include, for example, hard segments comprising short-chain diols and diisocyanates, and soft segments comprising high-molecular-weight (long-chain) diols and diisocyanates. A single urethane-based elastomer may be used, or two or more may be used in combination. Examples of high molecular weight (long-chain) diols include: polypropylene glycol, polytetramethylene oxide, poly(1,4-butenyl adipate), poly(ethylene-1,4-butenyl adipate), polycaprolactone, poly(1,6-hexene carbonate), and poly(1,6-hexene-neoprene adipate). The preferred average molecular weight of these high molecular weight (long-chain) diols is 500–10,000. Examples of short-chain diols include ethylene glycol, propylene glycol, 1,4-butanediol, and bisphenol A. The preferred average molecular weight for short-chain diols is 48–500. As a carbamate-based elastomer, it is preferred to have a number average molecular weight of 1,000 to 25,000, more preferably 1,500 to 20,000, and even more preferably 2,000 to 15,000. As a carbamate-based elastomer, commercially available products can be used.
[0084] (Polyamide elastomer) Polyamide elastomers are broadly classified into two types: polyether block amide type, which uses polyamide in the hard chain segment and polyether in the soft chain segment; and polyether ester block amide type, which uses polyamide in the hard chain segment and polyester in the soft chain segment. Specific examples of the polyamide-based elastomers include block copolymers with polyamide as the hard segment component and polybutadiene, butadiene-acrylonitrile copolymer, styrene-butadiene copolymer, polyisoprene, ethylene-propylene copolymer, polyether, polyester, polybutadiene, polycarbonate, polyacrylate, polymethacrylate, polyurethane, silicone rubber, etc., as the soft segment component. A single polyamide-based elastomer may be used, or two or more may be used in combination. As a polyamide-based elastomer, it is preferred to have a number average molecular weight of 1,000 to 50,000, and more preferably 2,000 to 30,000. As a polyamide-based elastomer, commercially available products can be used.
[0085] (Acrylic elastomer) Examples of acrylic elastomers include polymers of monomers primarily composed of acrylates. Preferred acrylates include ethyl acrylate, butyl acrylate, methoxyethyl acrylate, and ethoxyethyl acrylate. Furthermore, crosslinking monomers can be copolymers of glycidyl methacrylate, allyl glycidyl ether, etc., and further, copolymers of acrylonitrile, ethylene, etc. Specifically, examples include acrylonitrile-butyl acrylate copolymers, acrylonitrile-butyl acrylate-ethyl acrylate copolymers, and acrylonitrile-butyl acrylate-glycidyl methacrylate copolymers. One type of acrylic elastomer can be used alone, or two or more types can be used in combination. As an acrylic elastomer, it is preferred to have a number average molecular weight of 1,000 to 50,000, and more preferably 2,000 to 30,000. As an acrylic elastomer, commercially available products can be used.
[0086] (Silicone-based elastomers) The silicone-based elastomers are elastomers with organic polysiloxanes as the main component, such as polydimethylsiloxane elastomers, polymethylphenylsiloxane elastomers, and polydiphenylsiloxane elastomers. Silicone-based elastomers can be used alone or in combination with two or more types. As a silicone-based elastomer, it is preferred to have a number average molecular weight of 1,000 to 50,000, and more preferably 2,000 to 30,000. As a silicone-based elastomer, commercially available products can be used.
[0087] (Other elastomers) Additionally, component (D) may also be a state comprising at least one selected from the group consisting of polyphenylene ether resin, phenoxy resin, polycarbonate resin, polyamide-imide resin, polyamide resin, xylene resin, polyphenylene sulfide resin, polyether-imide resin, polyether ether ketone resin, tetrafluoroethylene resin, polyacrylonitrile resin, maleic anhydride modified polybutadiene, phenol modified polybutadiene, and carboxyl modified polyacrylonitrile.
[0088] (Content of component (D)) When the photosensitive resin composition of this embodiment contains component (D), based on the total solid content of the photosensitive resin composition, the content of component (D) is preferably 0.5% to 20% by mass, more preferably 0.5% to 15% by mass, even more preferably 0.5% to 10% by mass, particularly preferably 1.0% to 6% by mass, and most preferably 1.0% to 4.0% by mass. If the content of component (D) is 0.5% by mass or more, the improvement in adhesion strength with copper plating tends to be sufficient, and the electrical insulation reliability is further improved. If the content of component (D) is 20% by mass or less, the resolution of the perforation, the adhesion strength with copper plating, and the electrical insulation reliability all tend to be sufficient.
[0089] <(E) Thermal polymerization initiator> The photosensitive resin composition of this embodiment may contain a thermal polymerization initiator as component (E), or it may not. There are no particular limitations on hydroperoxides used as thermal polymerization initiators. Examples include: diisopropylbenzene hydroperoxide "Percumyl P" (trade name, manufactured by Nippon Oil Co., Ltd., hereinafter the same), isopropylbenzene hydroperoxide "Percumyl H", and tributyl hydroperoxide "Perbutyl H"; α,α-bis(tributylperoxide-m-isopropyl)benzene "Perbutyl P", dicumyl peroxide "Percumyl D", 2,5-dimethyl-2,5-bis(tributylperoxide)hexane "Perhexa 25B", and tributylcumyl peroxide "Perbutyl P". Dialkyl peroxides such as yl)C, di-tert-butyl peroxide "Perbutyl D", 2,5-dimethyl-2,5-bis(tert-butyl peroxide)hexyn-3 "Perhexyne 25B", and tert-butyl peroxide-2-ethylhexanoate "Perbutyl O"; ketone peroxides; peroxy ketals such as n-butyl 4,4-di-(tert-butyl peroxide)valerate "Perhexa V"; diacyl peroxides; peroxydicarbonates; peroxide esters and other organic peroxides; azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-cyclopropylpropionitrile), and 2,2'-azobis(2,4-dimethylvaleronitrile). From the viewpoint that it does not hinder photopolymerization and improves the physical properties and characteristics of the photosensitive resin composition, dialkyl peroxide is preferred, and 2,5-dimethyl-2,5-bis(tert-butylperoxide)hexyne-3 is more preferred. A single thermal polymerization initiator can be used alone, or two or more can be used together.
[0090] (Content of component (E)) When the photosensitive resin composition of this embodiment contains component (E), its content is not particularly limited. Based on the total amount of resin component in the photosensitive resin composition, it is preferably 0.01% to 5% by mass, more preferably 0.02% to 3% by mass, and even more preferably 0.03% to 2% by mass. If it is 0.01% by mass or more, there is a tendency for sufficient thermosetting, and if it is 5% by mass or less, there is a tendency for the photosensitive properties and heat resistance to become better.
[0091] <(F) Inorganic filler> The photosensitive resin composition of this embodiment contains an inorganic filler as component (F). The inorganic filler (F) in the photosensitive resin composition of this embodiment comprises an inorganic filler (hereinafter referred to as (F1) inorganic filler) that has been surface-treated with a coupling agent that does not have at least one functional group selected from the group consisting of amino groups and (meth)acrylic groups. Here, regarding "a coupling agent that does not have at least one functional group selected from the group consisting of amino groups and (meth)acrylic groups," a coupling agent having an amino group is not equivalent to this, nor is a coupling agent having a (meth)acrylic group, and of course, a coupling agent having both amino groups and (meth)acrylic groups is also not equivalent to this. When the coupling agent used in the surface treatment of the inorganic filler has an amino group or a (meth)acrylic group as a functional group, the adhesion strength with copper plating is particularly reduced. From the viewpoint of balancing via resolution, adhesion strength to copper plating, electrical insulation reliability, and resistance to descaling, the coupling agent preferably has an alkoxy group, and more preferably has at least one group selected from the group consisting of methoxy and ethoxy groups. Examples of alkoxy groups include methoxy, ethoxy, propoxy, and butoxy. The alkoxy group can be an alkoxy group itself.
[0092] Furthermore, in addition to the inorganic filler (F1), the photosensitive resin composition of this embodiment may also include at least one inorganic filler selected from the group consisting of: an inorganic filler surface-treated with a coupling agent having at least one functional group selected from the group consisting of amine and (meth)acrylic groups (hereinafter referred to as (F2) inorganic filler); and an untreated inorganic filler (hereinafter referred to as (F3) inorganic filler). From the viewpoint of the effect brought about by the inorganic filler (F1), the content of the inorganic filler (F1) relative to the total amount of the inorganic filler (F) is preferably 50% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, and particularly preferably 90% by mass or more (all including 100% by mass).
[0093] By including inorganic fillers, low thermal expansion can be achieved, reducing the possibility of warping. Previously used thermosetting resin compositions, serving as interlayer insulation layers in multilayer printed circuit boards, achieved low thermal expansion by including inorganic fillers. However, when photosensitive resin compositions contain inorganic fillers, the fillers become a cause of light scattering and hinder development, making it difficult to achieve low thermal expansion by including them in large quantities. As described above, photosensitive resin compositions present unique challenges compared to those containing inorganic fillers, but the photosensitive resin composition of this embodiment tends to maintain high via resolution even when containing inorganic fillers. Therefore, the photosensitive resin composition of this embodiment can simultaneously achieve low thermal expansion and high via resolution. Furthermore, in the photosensitive resin composition of this embodiment, by including the inorganic filler (F1) in component (F), there is a tendency to obtain a high level of adhesion strength to copper plating, and it is also easier to obtain a high level of crack resistance.
[0094] The coupling agent used in the surface treatment of the inorganic filler (F1) is provided that it does not have at least one functional group selected from the group consisting of amino and (meth)acrylic groups, but examples include silane coupling agents, titanium coupling agents, zirconium coupling agents, aluminum coupling agents, etc. Among these, silane coupling agents are preferred from the viewpoint of insulation. Commercially available products can be used as such coupling agents. Examples of commercially available products include: Shin-Etsu Silicone (registered trademark) series manufactured by Shin-Etsu Chemical Industry Co., Ltd., such as KBM-13, KBM-22, KBE-13, KBE-22, KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402, KBM-1403, KBE-1003, and KBM-303; and Orgatix (registered trademark) series manufactured by Matsumoto Fine Chemical Co., Ltd., such as ZA-45, ZA-65, TA-8, TA-21, and AL-3001. The inorganic filler treated with the coupling agent can be incorporated into the photosensitive resin composition of this embodiment. Alternatively, it can be configured such that the untreated inorganic filler and the coupling agent are separately incorporated into the photosensitive resin composition of this embodiment (so-called integral blending), with the inorganic filler treated with the coupling agent in the photosensitive resin composition. From the viewpoint of avoiding a decrease in crack resistance caused by residual coupling agent, it is preferable to use inorganic filler treated with the coupling agent.
[0095] (Surface treatment methods for inorganic fillers) Furthermore, there are no particular limitations on the method of treating inorganic fillers with coupling agents, and known methods can be used. For example, it can be carried out as follows: dissolve the coupling agent in a solvent (e.g., a mixed solvent of alcohol such as methanol and water, etc.) as needed to prepare a coupling agent solution. For 100 parts by weight of the untreated inorganic filler, mix the coupling agent solution, preferably in a ratio of 500 to 10,000 parts by weight (more preferably 1,000 to 7,000 parts by weight, and even more preferably 1,500 to 5,000 parts by weight), using a mixer. Then, heat treat at a preferably 80°C to 130°C for 1 to 10 hours, and then cool to room temperature. There are no particular limitations on the type of mixer mentioned, and examples include: Henschel mixers, mixing oscillators, drum mixers, V-type mixers, double cone mixers, belt mixers, Nota mixers, and super mixers. Among these, a Henschel mixer is preferred from the viewpoint of fully surface-treating the inorganic filler.
[0096] Examples of components (F) and (F1) include: silicon dioxide (SiO2), aluminum oxide (Al2O3), titanium dioxide (TiO2), tantalum oxide (Ta2O5), zirconium oxide (ZrO2), silicon nitride (Si3N4), barium titanate (BaO‧TiO2), barium carbonate (BaCO3), magnesium carbonate (MgCO3), aluminum hydroxide (Al(OH)3), magnesium hydroxide (Mg(OH)2), lead titanate (PbO‧TiO2), lead-zirconate-titanate (PZT), lead lanthanum zirconate titanate (PLZT), gallium oxide (Ga2O3), spinel (MgO‧Al2O3), mullite (3Al2O3‧2SiO2), cordierite (2MgO‧2Al2O3 / 5SiO2). 2) Talc (3MgO‧4SiO 2‧H 2O), aluminum titanate (TiO 2‧Al 2O 3), yttrium-containing zirconium oxide (Y 2O 3‧ZrO 2), barium silicate (BaO‧8SiO 2), boron nitride (BN), calcium carbonate (CaCO 3), barium sulfate (BaSO 4), calcium sulfate (CaSO 4), zinc oxide (ZnO), magnesium titanate (MgO‧TiO 2), hydrotalcite, mica, calcined kaolin, carbon, etc. (F) Components can be used alone or in combination of two or more. From the viewpoint of heat resistance and low thermal expansion, components (F) and (F1) preferably contain silicon dioxide, and more preferably silicon dioxide. That is, components (F) and (F1) preferably contain silicon dioxide that has been surface-treated with the coupling agent.
[0097] From the viewpoint of pore resolution, the average particle size of components (F) and (F1) is preferably 0.01 μm to 5 μm, more preferably 0.1 μm to 3 μm, even more preferably 0.1 μm to 2 μm, and particularly preferably 0.1 μm to 1 μm. Here, the average particle size of components (F) and (F1) is the volume average particle size of the inorganic filler dispersed in the photosensitive resin composition, and is assumed to be a value obtained by measurement as described below. First, the photosensitive resin composition is diluted (or dissolved) to 1,000 times using methyl ethyl ketone, and then the particles dispersed in the solvent are measured using a submicron particle analyzer (Beckman-Coulter, Inc., trade name: N5) according to international standard ISO 13321, with a refractive index of 1.38. The particle size at 50% (volume basis) of the cumulative value in the particle size distribution is taken as the average particle size (volume average particle size). In addition, all (F) components contained in the photosensitive resin film and interlayer insulating layer disposed on the carrier film can be diluted or dissolved to 1,000 times (volume ratio) using solvents such as methyl ethyl ketone as described above, and then measured using the submicron particle analyzer.
[0098] (Content of component (F)) The content of component (F) in the photosensitive resin composition of this embodiment is not particularly limited. Based on the total solid content of the photosensitive resin composition, it is preferably 5% to 80% by mass, more preferably 10% to 60% by mass, and even more preferably 15% to 50% by mass. Alternatively, based on the total solid content of the photosensitive resin composition, the content of component (F) can be 20% to 45% by mass, or 10% to 30% by mass. If the content of component (F) is within the aforementioned range, in addition to the effects brought about by component (F), mechanical strength and heat resistance can be further improved.
[0099] <(G) Pigment> In order to adjust photosensitivity, the photosensitive resin composition of this embodiment may contain pigment as component (G) depending on the desired color, or it may not contain pigment. As for component (G), any suitable coloring agent that produces the desired color can be selected and used. Examples of suitable coloring agents include: phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, carbon black, and naphthalene black.
[0100] (Content of component (G)) When the photosensitive resin composition of this embodiment contains component (G), from the viewpoint of adjusting photosensitivity, the content of component (G) is preferably 0.01% to 5% by mass, more preferably 0.03% to 3% by mass, and even more preferably 0.05% to 2% by mass, based on the total amount of solid components in the photosensitive resin composition.
[0101] <(H) Hardener or hardening accelerator> From the viewpoint of further improving properties such as heat resistance, adhesion strength to copper plating, and chemical resistance, the photosensitive resin composition of this embodiment may also contain a curing agent or a curing accelerator. In particular, when the aforementioned thermosetting resin (C) contains epoxy resin, it is preferable to use an epoxy resin curing agent as the curing agent. As a component (H), examples include: active ester-based curing agents; imidazole derivatives such as 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole; guanidines such as acetylguanidine and benzoguanidine; polyamines such as diaminodiphenylmethane, m-phenylenediamine, m-xylenediamine, diaminodiphenylamine, dicyandiamine, urea, urea derivatives, melamine, and polyhydrazine; organic acid salts and / or epoxy adducts of these; organic acid salts and epoxy adducts of the imidazole derivatives, guanidine compounds, and polyamine compounds; amine complexes of boron trifluoride; ethyldiamino-triazine, 2,4-diamino-triazine, and 2,4-diamino-6-xylene-triazine. Triazine derivatives; tertiary amines such as trimethylamine, N,N-dimethyloctylamine, N-benzyldimethylamine, pyridine, N-methylmorpholine, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), tetramethylguanidine, and m-aminophenol; polyphenols such as polyvinylphenol, polyvinylphenol bromide, phenolic varnish, and alkylphenolic varnish; organophosphorus salts such as tributylphosphine, triphenylphosphine, and tri-2-cyanoethylphosphine; phosphonium salts such as tri-n-butyl(2,5-dihydroxyphenyl)phosphonium bromide and hexadecyltributylphosphonium chloride; quaternary ammonium salts such as benzyltrimethylammonium chloride and phenyltributylammonium chloride; polyacid anhydrides; diphenylmonofluoroborate, triphenylsilane hexafluoroantimonate, and 2,4,6-triphenylthiopyranium hexafluorophosphate. Of these, from the viewpoint of further improving heat resistance, adhesion strength to copper plating, and chemical resistance, polyamine is preferred, and melamine is even more preferred. When the photosensitive resin composition of this embodiment contains the (H) component, the content of the (H) component is preferably 0.01% to 20% by mass, more preferably 0.02% to 10% by mass, and even more preferably 0.03% to 3% by mass, based on the total amount of resin components in the photosensitive resin composition.
[0102] <Diluent> A diluent may be used as needed in the photosensitive resin composition of this embodiment. Organic solvents may be used as diluents. Examples of organic solvents include: ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ether compounds such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, naphtha, hydrogenated naphtha, and solvent oil. One diluent may be used alone, or two or more may be used in combination. Ketones and esters are preferred as diluents, and esters are more preferred.
[0103] (Diluent content) The amount of diluent can be adjusted appropriately so that the concentration of the total solid components in the photosensitive resin composition is preferably 40% to 90% by mass, more preferably 45% to 80% by mass, and even more preferably 45% to 70% by mass. By adjusting the amount of diluent used in this way, the coatability of the photosensitive resin composition is improved, and more intricate patterns can be formed.
[0104] <Other Ingredients> The photosensitive resin composition of this embodiment may, as needed, contain polymerization inhibitors such as hydroquinone, methyl hydroquinone, hydroquinone monomethyl ether, catechol, and galloquinone; tackifiers such as bentonite and montmorillonite; foaming agents such as silicone-based foaming agents, fluorinated foaming agents, and vinyl resin-based foaming agents; and various commonly used additives such as silane coupling agents. Furthermore, it may also contain flame retardants such as brominated epoxy compounds, acid-modified brominated epoxy compounds, antimony compounds, and phosphorus-based phosphate compounds, aromatic condensed phosphate esters, and halogenated condensed phosphate esters; and thermoplastic resins such as polyester polyurethane resins.
[0105] The photosensitive resin composition of this embodiment can be obtained by mixing and blending the various components using a roller mill, bead mill, or the like. Here, the photosensitive resin composition of this embodiment can be used in liquid form or in film form. When the photosensitive resin composition is used in liquid form, the coating method of the photosensitive resin composition in this embodiment is not particularly limited, and various coating methods can be listed, such as printing, spin coating, spray coating, jet dispensing, inkjet coating, and dip coating. From the viewpoint of making it easier to form a photosensitive layer, any suitable method can be selected from printing and spin coating. Furthermore, when the photosensitive resin composition is used in a film-like state, for example, it can be used in the form of a photosensitive resin film as described later. In this case, the photosensitive resin film can be deposited onto a carrier film using a laminator or the like to form a photosensitive layer of the desired thickness. Moreover, when used in a film-like state, the manufacturing efficiency of multilayer printed circuit boards is increased, which is therefore preferable.
[0106] [Photosensitive resin film, photosensitive resin film for interlayer insulating layer] The photosensitive resin film of this embodiment is a photosensitive layer that subsequently becomes an interlayer insulating layer, and includes the photosensitive resin composition of this embodiment. The photosensitive resin film of this embodiment may also be a form in which a photosensitive resin film is disposed on a carrier film. There is no particular limitation on the thickness of the photosensitive resin film (photosensitive layer) (the thickness after drying). From the viewpoint of making multilayer printed circuit boards thinner, it is preferably 1 μm to 100 μm, more preferably 1 μm to 50 μm, and even more preferably 5 μm to 40 μm.
[0107] The photosensitive resin film of this embodiment can be obtained, for example, by coating the photosensitive resin composition of this embodiment onto a carrier film using a known coating apparatus such as a corner-cutting wheel coater, a rod coater, a coincidence coater, a roller coater, a gravure coater, or a die coater, and then drying it to form a photosensitive layer that becomes an interlayer insulating layer. Examples of suitable carrier films include: polyester films such as polyethylene terephthalate (PET) films and polybutylene terephthalate (PET) films; and polyolefin films such as polypropylene (PP) films and polyethylene (PE) films. The thickness of the carrier film can be appropriately selected within the range of 5 μm to 100 μm, preferably 5 μm to 60 μm, and even more preferably 15 μm to 45 μm.
[0108] Furthermore, in this embodiment, a protective film can also be provided on the side of the photosensitive layer opposite to the side in contact with the carrier film. For example, a polymer film such as polyethylene or polypropylene can be used as the protective film. Alternatively, the same polymer film as the carrier film can be used, or a different polymer film can be used.
[0109] In the drying of the coating film formed by coating a photosensitive resin composition, a hot air dryer, a far-infrared dryer, or a near-infrared dryer can be used. The drying temperature is preferably 60°C to 150°C, more preferably 70°C to 120°C, and even more preferably 80°C to 100°C. The drying time is preferably 1 minute to 60 minutes, more preferably 2 minutes to 30 minutes, and even more preferably 5 minutes to 20 minutes. From the viewpoint of preventing the diffusion of diluent during the manufacturing process of the multilayer printed circuit board, the residual diluent content in the dried photosensitive resin film is preferably 3% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less.
[0110] The photosensitive resin film of this embodiment exhibits excellent via resolution, adhesion strength to copper plating, electrical insulation reliability, and resistance to adhesive residue removal, making it suitable as an interlayer insulating layer for multilayer printed circuit boards. In other words, this disclosure also provides a photosensitive resin film for interlayer insulating layers. Furthermore, the photosensitive resin film for interlayer insulating layers can also be referred to as an interlayer insulating photosensitive film.
[0111] Multilayer printed circuit boards and their manufacturing methods This disclosure also provides a multilayer printed circuit board containing an interlayer insulating layer formed from a photosensitive resin composition or photosensitive resin film using the present embodiment. Here, the phrase "containing an interlayer insulating layer" includes cases where the interlayer insulating layer is directly present; and cases where the interlayer insulating layer is present after various processing such as via formation, roughening treatment, and wiring formation. Regarding the multilayer printed circuit board of this embodiment, as long as it includes the step of forming an interlayer insulating layer using the photosensitive resin composition of this embodiment, its manufacturing method is not particularly limited. For example, it can be easily manufactured by the manufacturing method of the multilayer printed circuit board of this embodiment described below.
[0112] Hereinafter, an example of a preferred embodiment of a method for manufacturing a multilayer printed circuit board will be described, with reference to FIG1, of a method for manufacturing a multilayer printed circuit board using a photosensitive resin film (photosensitive resin film for interlayer insulation layer) of this embodiment. The multilayer printed circuit board 100A can be manufactured, for example, by manufacturing methods including (1) to (4) below. (1): The photosensitive resin film of this embodiment is laminated onto one or both sides of the circuit board (hereinafter referred to as "lamination step (1)"). (2): By exposing and developing the photosensitive resin film laminated in step (1), an interlayer insulating layer with vias is formed (hereinafter referred to as "photosensitive via formation step (2)"). (3): The through hole and the interlayer insulating layer are roughened (hereinafter referred to as "roughening step (3)"). (4): A circuit pattern is formed on the interlayer insulating layer (hereinafter referred to as "circuit pattern forming step (4)"). Here, as described above, for convenience, the specified operation is sometimes referred to as "Step XX", but Step XX is not limited to the specific state described in this specification.
[0113] (Lamination step (1)) The lamination step (1) is as follows: using a vacuum laminator, the photosensitive resin film (photosensitive resin film for interlayer insulation) of this embodiment is laminated onto one or both sides of the circuit board (substrate 101 having circuit pattern 102). Examples of vacuum laminators include: vacuum applicators manufactured by Nichigo-Morton Co., Ltd., vacuum pressure laminators manufactured by Meiki Manufacturing Co., Ltd., roller dry coating machines manufactured by Hitachi, Ltd., and vacuum laminators manufactured by Showa Denko Materials & Electronics Co., Ltd.
[0114] When a protective film is provided on the photosensitive resin film, after the protective film is peeled off or removed, the photosensitive resin film can be pressed onto the circuit board while being pressed and heated, thereby performing lamination. The lamination process can be performed, for example, by preheating the photosensitive resin film and the circuit board as needed, and then under reduced pressure conditions of 70°C to 130°C, 0.1 MPa to 1.0 MPa, and 20 mmHg (26.7 hPa) or less, but is not particularly limited to these conditions. Furthermore, the lamination method can be batch lamination or continuous lamination using rollers. Finally, the photosensitive resin film (hereinafter sometimes referred to as the photosensitive layer) laminated on the circuit board is cooled to near room temperature to form an interlayer insulating layer 103. The carrier film can be peeled off here, or it can be peeled off after exposure as described later.
[0115] (Step 2 of forming a photosensitive aperture) In the photosensitive via formation step (2), at least a portion of the photosensitive resin film laminated on the circuit board is exposed, and then developed. The portion exposed to photochemical rays by exposure is photocured, thereby forming a pattern. There are no particular limitations on the exposure method. For example, a method of irradiating photochemical rays in an image-like manner using a negative or positive mask pattern called an artwork (mask exposure method) can be used. Alternatively, a direct drawing exposure method such as Laser Direct Imaging (LDI) exposure method or Digital Light Processing (DLP) exposure method can be used to irradiate photochemical rays in an image-like manner. As the source of photochemical rays, known light sources can be used. Specifically, examples include: gas lasers such as carbon arc lamps, mercury vapor arc lamps, high-pressure mercury lamps, xenon lamps, and argon lasers; solid lasers such as yttrium aluminum garnet (YAG) lasers; and semiconductor lasers that effectively emit ultraviolet or visible light. The exposure dose can be appropriately selected based on the light source used and the thickness of the photosensitive layer. For example, when irradiating with ultraviolet light from a high-pressure mercury lamp, with a photosensitive layer thickness of 1 μm to 100 μm, a dose of approximately 10 mJ / cm² to 1,000 mJ / cm² is generally preferred, and more preferably 15 mJ / cm² to 500 mJ / cm².
[0116] During development, an interlayer insulating layer containing the photocured material is formed on the substrate by removing the uncured portion of the photosensitive layer from the substrate. If a carrier film is present on the photosensitive layer, the carrier film is removed, and then the unexposed areas are removed (developed). There are wet development and dry development methods, either of which can be used, but wet development is widely used. In this embodiment, wet development is employed. In wet development, a developer solution compatible with the photosensitive resin composition is used, and development is performed using a known development method. Examples of development methods include immersion, coating, spraying, brushing, slapping, scrubbing, and agitation immersion. Of these, spraying is preferred from the viewpoint of improving aperture resolution, and high-pressure spraying is particularly preferred. Development can be performed using only one method, or two or more methods can be combined. The structure of the developer can be appropriately selected based on the structure of the photosensitive resin composition. Examples of developers include: alkaline aqueous solutions, aqueous developers, and organic solvent-based developers. Among these, an alkaline aqueous solution is preferred.
[0117] In the photosensitive via formation step (2), after exposure and development, post-UV curing with an exposure amount of about 0.2 J / cm 2~10 J / cm 2 (preferably 0.5 J / cm 2~5 J / cm 2) and post-thermal curing at a temperature of about 60℃~250℃ (preferably 120℃~200℃) can be performed as needed to further harden the interlayer insulating layer. In addition, it is preferred to perform it in this way. An interlayer insulating layer with vias 104 can be formed in the manner described above. The shape of the via is not particularly limited; examples include quadrilaterals and inverted trapezoids (with the upper side longer than the lower side) when described in terms of cross-sectional shape, and circles and quadrilaterals when described in terms of shape viewed from the front (from the direction where the bottom of the via is visible). In the via formation using photolithography in this embodiment, vias with an inverted trapezoidal cross-sectional shape (upper side longer than the lower side) can be formed. In this case, the uniformity of copper plating on the via wall surface is higher, which is therefore preferable.
[0118] The via size (diameter) formed by this step can be set to 60 μm or less, and further, it can be set to less than 40 μm or 30 μm or less, which can achieve a smaller diameter compared with the via size formed by laser processing. There is no particular limitation on the lower limit of the via size (diameter) formed by this step, which can be 15 μm or more, or 20 μm or more. The size (diameter) of the via formed by this step is not necessarily limited to less than 60 μm. For example, it can be less than 200 μm, or it can be arbitrarily selected within the range of 15 μm to 300 μm.
[0119] (Roughening process step (3)) In the roughening process step (3), the surface of the via and the interlayer insulation layer is roughened using a roughening solution. Furthermore, if smear is generated in the photosensitive via formation step (2), the roughening solution can also be used to remove the smear. The roughening process and the removal of smear can be performed simultaneously. Examples of roughening solutions include: chromium / sulfuric acid roughening solution, alkaline permanganate roughening solution (e.g., sodium permanganate roughening solution), sodium fluoride / chromium / sulfuric acid roughening solution, etc. The roughening process creates uneven anchors on the surfaces of vias and interlayer insulation layers.
[0120] (Circuit pattern formation step (4)) The circuit pattern forming step (4) is a step of forming a circuit pattern on the interlayer insulating layer after the roughening process step (3). From the perspective of forming fine wiring, circuit pattern formation is better implemented through a semi-additive process. The circuit pattern formation and via connection are performed simultaneously through the semi-additive process. In the semi-additive process, firstly, an electroless copper plating process is performed on the via bottom, via wall, and the entire surface of the interlayer insulating layer after the roughening treatment step (3) using a palladium catalyst, etc., to form a seed layer 105. This seed layer is used to form the power supply layer for electrolytic copper plating, and preferably has a thickness of about 0.1 μm to 2.0 μm. If the thickness of the seed layer is 0.1 μm or more, there is a tendency to suppress the decrease in connection reliability during electrolytic copper plating; if it is 2.0 μm or less, there is a tendency to avoid increasing the etching amount when flash etching the seed layer between the wirings, and to suppress the damage to the wirings caused by etching.
[0121] The electroless copper plating process is carried out by reacting copper ions with a reducing agent to deposit metallic copper on the surface of vias and interlayer insulating layers. The electroless electroplating process and the electroplating process can be known methods and are not particularly limited. The catalyst in the electroless electroplating step is preferably a palladium-tin mixed catalyst, and the primary particle size of this catalyst is preferably less than 10 nm. Furthermore, the plating composition in the electroless electroplating step preferably contains hypophosphoric acid as a reducing agent. Commercially available products can be used as electroless copper plating solutions. Examples of commercially available products include: "MSK-DK" manufactured by Atotech Japan Co., Ltd., and the "Thru-cup (registered trademark) PEA ver.4" series manufactured by Uemura Kogyo Co., Ltd.
[0122] After performing the electroless copper plating process, a dry film resist is hot-pressed onto the electroless copper plating using a roller laminator. The thickness of the dry film resist must be greater than the wiring height after copper plating; from this perspective, a dry film resist with a thickness of 5 μm to 30 μm is preferred. For example, the "Photek" series (registered trademark) manufactured by Showa Denko Materials Co., Ltd. can be used as a dry film resist. After hot lamination of the dry film resist, the dry film resist is exposed, for example, via a mask with a desired wiring pattern. Exposure can be performed using the same apparatus and light source used when forming vias in the photosensitive resin film. After exposure, the carrier film on the dry film resist is peeled off, and development is performed using an alkaline aqueous solution to remove unexposed areas, forming the resist pattern 106. Then, if necessary, a process such as using plasma can be performed to remove developing residues from the dry film resist. After development, copper is electroplated to form the copper circuit layer 107 and fill the vias.
[0123] After copper electroplating, the dry film resist is stripped using an alkaline aqueous solution or an amine-based stripping agent. Following the stripping of the dry film resist, the seed layer between the wirings is removed (flash etching). Flash etching is performed using acidic solutions such as sulfuric acid and hydrogen peroxide, as well as oxidizing solutions. Specifically, examples include "SAC" manufactured by JCU Corporation and "CPE-800" manufactured by Mitsubishi Gas Chemical Corporation. After flash etching, palladium and other substances adhering to the wirings are removed as needed. Palladium removal is preferably performed using acidic solutions such as nitric acid or hydrochloric acid.
[0124] After the dry film resist is peeled off or after the flash etching step, a post-baking process is preferably performed. During the post-baking process, unreacted thermosetting components are fully thermoset, thereby improving electrical insulation reliability, curing characteristics, and adhesion strength to copper plating. The thermosetting conditions vary depending on the type of resin composition, but a curing temperature of 150°C to 240°C and a curing time of 15 minutes to 100 minutes are preferred. The post-baking process completes one step of manufacturing a printed circuit board using the photosensitive via method, but the process is repeated to manufacture the substrate depending on the required number of interlayer insulating layers. Then, a solder resist layer 108 is preferably formed on the outermost layer.
[0125] The above describes a method for manufacturing a multilayer printed circuit board using the photosensitive resin composition of this embodiment to form vias. The photosensitive resin composition of this embodiment exhibits excellent pattern resolution, and is therefore suitable for forming cavities for housing, such as chips or passive components. The cavity can be preferably formed, for example, by means of the following: In the description of the multilayer printed circuit board, the pattern drawn during pattern formation by exposing the photosensitive resin film is set as a pattern capable of forming the desired cavity. Furthermore, the photosensitive resin composition of this embodiment can also be effectively used as a surface protective film for solder resists, etc.
[0126] [Semiconductor Packaging] This disclosure also provides a semiconductor package having the multilayer printed circuit board and semiconductor components of this embodiment. The semiconductor package of this embodiment can be manufactured by mounting semiconductor components such as semiconductor chips and memory chips at predetermined locations on the multilayer printed circuit board of this embodiment, and sealing the semiconductor components using a sealing resin or the like. [Example]
[0127] The present embodiment will be described in more detail below by way of examples, but the present embodiment is not limited to these examples. Furthermore, the properties of the photosensitive resin compositions obtained in Examples 1 to 6 and Comparative Examples 1 to 3 were evaluated by the methods shown below.
[0128] [1. Evaluation of the resolution of vias (pattern 1)] (1-1) Evaluation of the fabrication of laminates The surface of the copper foil of a printed wiring board substrate (manufactured by Showa Denko Materials Co., Ltd., trade name "MCL-E-679"), which is made by depositing 12 μm thick copper foil on a glass epoxy material, is treated with a roughening treatment solution (manufactured by MEC Co., Ltd., trade name "CZ-8100"), then washed with water, and then dried to obtain a roughened printed wiring board substrate. Next, the protective film was peeled off from the "photosensitive resin film with a carrier film and a protective film bonded" manufactured in the various embodiments and comparative examples. The exposed photosensitive resin film was placed in contact with the copper foil of the roughened printed circuit board substrate, and then lamination was performed using a vacuum laminator (manufactured by Meiki Seisakusho Co., Ltd., trade name "MVLP-500"). Furthermore, the lamination conditions were set as follows: hot plate temperature 70°C, vacuum time 20 seconds, lamination pressing time 30 seconds, air pressure 4 kPa or less, and pressing pressure 0.4 MPa. After lamination, the film was left at room temperature for more than 1 hour to obtain an evaluation laminate in which a photosensitive resin film and a carrier film are sequentially deposited on the copper foil surface of the printed circuit board substrate. (1-2) Sensitivity Measurement of Photosensitive Resin Films After peeling off and removing the carrier film of the evaluation laminate obtained in (1-1), a 41-segment step tablet was configured, and exposure was performed using a direct imaging exposure apparatus "DXP-3512" (manufactured by ORC Manufacturing Co., Ltd.) with an ultra-high pressure mercury lamp as the light source. The exposure pattern used a grid pattern of dots (the ratio of the diameter of the dots to the distance between the centers of the dots = 1:2). The diameter (ϕ) of the dots was varied in 5-μm intervals within the range of 30 μm to 100 μm. After exposure, the sample was left at room temperature for 30 minutes, and then the unexposed areas of the photosensitive resin composition were developed by spraying with a 1% sodium carbonate aqueous solution at 30°C for 60 seconds. After development, the exposure energy with a gloss retention stage number of 8.0 on a 41-stage exposure table was taken as the sensitivity of the photosensitive resin film (unit: mJ / cm²). Using the pattern exposed at this sensitivity, the resolution of the vias set in the photosensitive resin film was evaluated according to the following evaluation criteria. (1-3) Evaluation of the analytical performance of vias In the evaluation of via resolution, exposure is performed using the exposure energy of the photosensitive resin film with a sensitivity of 8.0 (i.e., the number of stages) as measured in (1-2), followed by spray development. The via pattern is then observed using an optical microscope, and the evaluation is based on the following criteria. The "opening" state refers to the condition of the copper foil of the printed circuit board substrate that can be confirmed when observing the via portion of the dot pattern using an optical microscope. A "A" rating indicates good characteristics. A: The ϕ60 μm via portion of the dot pattern is open. B: The ϕ60 μm via portion of the dot pattern is not open. C: It was not light-cured.
[0129] [2. Evaluation of adhesion strength (peel strength) to copper plating] The protective film is peeled off from the "photosensitive resin film with carrier film and protective film bonded" manufactured in the various embodiments and comparative examples. At the same time, a vacuum laminator (manufactured by Meiki Manufacturing Co., Ltd., trade name "MVLP-500") with a thickness of 1.0 mm is used to laminate a copper-clad laminate substrate with a pressing pressure of 0.4 MPa, a pressing hot plate temperature of 80°C, a vacuum time of 25 seconds, a lamination pressing time of 25 seconds, and an air pressure of less than 4 kPa to obtain a laminate. The obtained laminate was fully exposed using a parallel light exposure machine (manufactured by ORC Corporation, trade name "EXM-1201") with an ultra-high pressure mercury lamp as the light source at 500 mJ / cm². Next, it was exposed using an ultraviolet exposure device at an exposure dose of 2,000 mJ / cm² and heated at 170°C for 1 hour to obtain an evaluation laminate with a hardened material (hardened film) formed on the copper-clad laminate substrate.
[0130] Next, firstly, an aqueous solution of diethylene glycol monobutyl ether (200 ml / L) and sodium hydroxide (5 g / L) was prepared as a swelling solution, heated to 70°C, and then the evaluation laminate was impregnated for 10 minutes. Secondly, an aqueous solution of potassium permanganate (60 g / L) and sodium hydroxide (40 g / L) was prepared as a roughening solution, heated to 70°C, and then the evaluation laminate was impregnated for 15 minutes. Next, an aqueous solution of a neutralizing solution (tin chloride (SnCl₂): 30 g / L, hydrogen chloride: 300 ml / L) was prepared, heated to 40°C, and then the evaluation laminate was impregnated for 5 minutes to reduce the potassium permanganate. The surface of the hardened evaluation laminate was then treated to remove adhesive residue as described above. Next, the surface of the hardened evaluation laminate after degumming treatment was treated with an alkaline cleaner, "Cleaner Securiganth 902" (manufactured by Atotech Japan Co., Ltd., trade name), at 60°C for 5 minutes to degrease and clean. After cleaning, the hardened laminate was treated with a pre-dip Neoganth B (manufactured by Atotech Japan Co., Ltd., trade name) at 23°C for 1 minute. Then, the hardened laminate was treated with an activator, "Activator Neoganth 834" (manufactured by Atotech Japan Co., Ltd., trade name), at 35°C for 5 minutes, and then treated with a reducing agent, "Reducer Neoganth WA" (manufactured by Atotech Japan Co., Ltd., trade name), at 30°C for 5 minutes. The evaluation laminate obtained in the manner described was placed in a chemical copper solution ("Basic Printganth MSK-DK", "Copper Printganth MSK", and "Stabilizer Printganth MSK" (all manufactured by Atotech Japan Co., Ltd., trade names)) and electroless plating was performed until the plating thickness reached approximately 0.5 μm. After this electroless plating, an annealing treatment was performed at 120°C for 30 minutes to remove residual hydrogen. Then, copper sulfate electroplating was performed, followed by an annealing treatment at 180°C for 60 minutes to form a conductor layer with a thickness of 25 μm.
[0131] For the evaluation laminate in which the conductor layer is formed as described above, the vertical peel strength is measured at 23°C according to Japanese Industrial Standards (JIS) C6481 (1996), and the evaluation is carried out according to the following evaluation criteria. A: The adhesion strength with copper plating is above 0.40 kN / m. B: The adhesion strength with copper plating is above 0.30 kN / m but less than 0.40 kN / m. C: The adhesion strength with copper plating is less than 0.30 kN / m.
[0132] [3. Evaluation of HAST resistance (electrical insulation reliability after moisture absorption)] In the section [2. Evaluation of adhesion strength (peel strength) with copper plating], a conductor layer with a thickness of 35 μm is formed instead of a conductor layer with a thickness of 25 μm. Otherwise, the same operation is performed to obtain a laminate with a conductor layer. Next, a circular electrode with a diameter (ϕ) of 6 mm is formed by etching the conductor layer of the laminate. Then, a photosensitive solder resist film "FZ-2700GA" (manufactured by Showa Denko Materials Co., Ltd., trade name) is placed on the electrode and the hardened film. An interlayer insulating layer is formed using a vacuum laminator (manufactured by Meiki Seisakusho Co., Ltd., trade name "MVLP-500") with a pressing pressure of 0.4 MPa, a hot plate temperature of 80°C, a vacuum time of 25 seconds, a lamination pressing time of 40 seconds, and a pressure below 4 kPa, thus obtaining an evaluation laminate. Furthermore, the thickness of the interlayer insulating layer is 25 μm.
[0133] The evaluation laminate obtained as described above was fully exposed using a parallel light exposure machine (manufactured by ORC Corporation, trade name "EXM-1201") with an ultra-high pressure mercury lamp as the light source at 500 mJ / cm². Next, it was exposed using an ultraviolet exposure device at an exposure dose of 2,000 mJ / cm², and heated at 160°C for 1 hour to obtain a hardened film. Subsequently, wiring was performed with the circular electrode as the positive electrode and the copper foil on the side of the copper-clad laminate substrate where the circular electrode is formed as the negative electrode. The substrate was then exposed to a pressure cooker (model name "Unsaturated Type Ultra-Accelerated Life Test Apparatus PC-422RP", manufactured by Hirayama Manufacturing Co., Ltd.) at 135°C, 85%, and 5.5 V for 200 hours. The resistance between the electrodes was measured and evaluated according to the following evaluation criteria. A: The resistance value after 200 hours is above 10×10 7Ω. B: The resistance value after 200 hours is greater than 10×10 6Ω but less than 10×10 7Ω. C: The resistance value after 200 hours is less than 10 × 10 6 Ω.
[0134] [4. Evaluation of resistance to adhesive residue removal] The protective film of the "photosensitive resin film with carrier film and protective film bonded together" manufactured in the examples and comparative examples is peeled off, and the film is laminated on a copper-clad laminate substrate with a thickness of 1.0 mm using a vacuum laminator (manufactured by Meiki Manufacturing Co., Ltd., trade name "MVLP-500") with a pressing pressure of 0.4 MPa, a pressing hot plate temperature of 80°C, a vacuum time of 25 seconds, a lamination pressing time of 25 seconds, and an air pressure of less than 4 kPa to obtain a laminate. The obtained laminate was fully exposed using a parallel light exposure machine (manufactured by ORC Corporation, trade name "EXM-1201") with an ultra-high pressure mercury lamp as the light source at 500 mJ / cm². Next, it was exposed using an ultraviolet exposure device at an exposure dose of 2,000 mJ / cm² and heated at 170°C for 1 hour to obtain an evaluation laminate with a hardened material (hardened film) formed on the copper-clad laminate substrate.
[0135] Next, for the obtained evaluation laminate, an aqueous solution of diethylene glycol monobutyl ether (200 ml / L) and sodium hydroxide (5 g / L) was prepared as a swelling solution, heated to 70°C, and then the evaluation laminate was impregnated for 10 minutes. Next, an aqueous solution of potassium permanganate (60 g / L) and sodium hydroxide (40 g / L) was prepared as a roughening solution, heated to 70°C, and then the evaluation laminate was impregnated for 15 minutes. Then, an aqueous solution of a neutralizing solution (tin chloride (SnCl₂): 30 g / L, hydrogen chloride: 300 ml / L) was prepared, heated to 40°C, and then the evaluation laminate was impregnated for 5 minutes to reduce the potassium permanganate. The descaling process was performed as described above. Regarding resistance to degumming residue, the weight reduction after degumming residue treatment (g / m²) relative to the dry weight before degumming residue treatment was calculated and evaluated according to the following evaluation criteria. A: The quality reduction rate is less than 1.0%. B: Quality reduction rate of 1.0% or more but less than 3.0% C: Quality reduction rate of 3.0% or more
[0136] <Synthetic Example 1> Synthesis of acid-modified epoxy derivative 1 [(A1) component and (A1-1) component] containing vinyl unsaturated groups and an alicyclic skeleton Dicyclopentadiene-type epoxy resin ("XD-1000" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 252 g / eq, softening point 74.2℃, equivalent to component (a1), expressed by the general formula (a1-1); alicyclic skeleton ring-forming carbon number: 10) 350 parts by mass, acrylic acid (equivalent to component (a2)) 70 parts by mass, methyl hydroquinone 0.5 parts by mass, carbitol acetate 120 parts by mass, heated to 90℃ and stirred to react and dissolve the mixture. Next, the obtained solution was cooled to 60°C, 2 parts by mass of triphenylphosphine were added, and the mixture was heated to 100°C to carry out the reaction until the acid value of the solution reached 1 mgKOH / g. 98 parts by mass of tetrahydrophthalic anhydride (equivalent to component (a3)) and 85 parts by mass of carbitol acetate were added to the reacted solution, and the mixture was heated to 80°C and then reacted for 6 hours. Then, the mixture was cooled to room temperature to obtain an acid-modified dicyclopentadiene-type epoxy acrylate with a solid content of 73% by mass (equivalent to component (A1) and component (A1-1); hereinafter referred to as "acid-modified epoxy derivative 1 containing vinyl unsaturated groups and alicyclic skeleton").
[0137] <Synthetic Example 2> Synthesis of acid-modified epoxy derivative 2 [(A1) component and (A1-1) component] containing vinyl unsaturated groups and alicyclic skeleton In Synthesis Example 1, the dicyclopentadiene-type epoxy resin was changed to "EPICLON (registered trademark) HP-7200" (manufactured by DIC Corporation, epoxy equivalent 254 g / eq~264 g / eq, softening point 56℃~66℃, equivalent to component (a1), represented by the general formula (a1-1); number of ring-forming carbons of the alicyclic skeleton: 10). Otherwise, the same operation was performed to obtain an acid-modified dicyclopentadiene-type epoxy acrylate with a solid content of 74% by mass (equivalent to component (A1) and component (A1-1); hereinafter referred to as "acid-modified epoxy derivative 2 containing vinyl unsaturated groups and alicyclic skeleton").
[0138] <Synthetic Example 3> (A2-1) Synthesis of acid-modified epoxide derivatives containing vinyl unsaturated groups without alicyclic skeletons Add 350 parts by weight of bisphenol F phenolic varnish-type epoxy resin ("EXA-7376" manufactured by DIC Co., Ltd., equivalent to component (a21)), 70 parts by weight of acrylic acid (equivalent to component (a22)), 0.5 parts by weight of methyl hydroquinone, and 120 parts by weight of carbitol acetate, heat to 90°C, and then stir to react and dissolve the mixture. Next, the obtained solution was cooled to 60°C, 2 parts by mass of triphenylphosphine were added, and the mixture was heated to 100°C. The reaction was then carried out until the acid value of the solution reached 1 mgKOH / g. 98 parts by mass of tetrahydrophthalic anhydride (equivalent to component (a23)) and 85 parts by mass of carbitol acetate were added to the reacted solution, and the mixture was heated to 80°C. The reaction was then carried out for 6 hours. Then, cooling to room temperature yields an acid-modified bisphenol F epoxy acrylate with a solid content of 73% by mass (equivalent to component (A2-1); hereinafter referred to as "acid-modified epoxy derivative 3 containing vinyl unsaturated groups").
[0139] <Manufacturing Example 1> Manufacturing of Inorganic Filler 1 Five kg of calcined silica particles "KE-S50" (manufactured by Nippon Shokubai Co., Ltd., trade name) were added to a 20 L capacity Henschel mixer including a heating jacket. Furthermore, the Henschel mixer has a container for the mixture to be placed in and a rotating shaft with stirring blades attached to the bottom of the container. As a device for scraping off adhering material from the container walls, a rotating shaft with plate-shaped blades attached, positioned along the walls, is also installed on top of the container. During the stirring and calcination of silica particles, a solution was prepared by dropwise addition of 166.7 g of "KBM-13" (methyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.), which serves as a silane coupling agent, dissolved in 208.3 g of methanol and 41.7 g of deionized water. The mixture of calcined silica particles and the silane coupling agent was then heated to 100°C at a rate of 20°C / hour and held at 100°C for 5 hours for heat treatment. After cooling, an inorganic filler 1 treated with a "methoxyl-containing coupling agent" was obtained.
[0140] Manufacturing Examples 2-7: Manufacturing of Inorganic Filler 2-7 In Manufacturing Example 1, instead of "KBM-13" (methyltrimethoxysilane, manufactured by Shin-Etsu Chemical Industry Co., Ltd.), "KBM-22" (dimethyldimethoxysilane), "KBE-13" (methyltriethoxysilane), "KBE-22" (dimethyldiethoxysilane), "KBM-403" (3-glycidoxypropyltrimethoxysilane), "KBM-502" (3-methacryloxypropylmethyldimethoxysilane), or "KBE-903" (3-aminopropyltrimethoxysilane) were used. (Silane) [all manufactured by Shin-Etsu Chemical Industry Co., Ltd.], except for the above, the same operation was performed to manufacture inorganic filler 2 treated with a "coupling agent having a methoxy group", inorganic filler 3 and inorganic filler 4 treated with a "coupling agent having an ethoxy group", inorganic filler 5 treated with a "coupling agent having a glycidyl group", inorganic filler 6 (for comparison) treated with a "coupling agent having a methacrylic and methoxy group", and inorganic filler 7 (for comparison) treated with a "coupling agent having an amino and methoxy group". These are designated as Manufacturing Examples 2 to 7 in sequence.
[0141] <Examples 1-6, Comparative Examples 1-3> (Preparation of photosensitive resin composition) The composition was prepared according to the formulation and dosage shown in Table 1, and then kneaded using a three-roll mill to prepare the photosensitive resin composition. In each example, carbitol acetate was appropriately added to adjust the concentration, resulting in a photosensitive resin composition with a solid content of 60% by mass. (Preparation of photosensitive resin film) A 25 μm thick polyethylene terephthalate film (G2-25, manufactured by Teijin Co., Ltd., trade name) was used as a carrier film. The photosensitive resin composition prepared in each example was coated onto the carrier film, and dried at 100°C for 10 minutes using a hot air convection dryer to form a photosensitive resin film (i.e., a photosensitive layer). The thickness of the dried photosensitive resin film was 25 μm. Subsequently, a biaxially extended polypropylene film (MA-411, manufactured by Oji F-Tex Co., Ltd., trade name) is bonded to the surface of the photosensitive resin film on the side opposite to the side in contact with the carrier film, thereby producing a photosensitive resin film with a carrier film and a protective film bonded together. The prepared photosensitive resin film was used to perform various evaluations according to the method described above. The results are shown in Table 1.
[0142] [Table 1] unit Example Comparative example 1 2 3 4 5 6 1 2 3 Photosensitive resin composition (A) (A1-1) Acid-modified epoxy derivatives containing ethylene unsaturated groups and alicyclic skeletons 1 Quality 36 36 36 36 36 36 36 Acid-modified epoxy derivatives containing ethylene unsaturated groups and alicyclic skeletons 2 Quality 36 (A2-1) Acid-modified epoxy derivatives containing vinyl unsaturated groups without alicyclic skeleton 3 Quality 36 (Aiii) Dipentaerythritol pentaacrylate Quality 7.4 7.4 7.4 7.4 7.4 7.4 7.4 7.4 7.4 (B) Photopolymerization initiator 1 Quality 0.25 0.25 0.25 0.25 0.25 0.25 0.25 0.25 0.25 Photopolymerization initiator 2 Quality 0.04 0.04 0.04 0.04 0.04 0.04 0.04 0.04 0.04 (C) Biphenyl type epoxy resin Quality 12.8 12.8 12.8 12.8 12.8 12.8 12.8 12.8 12.8 Epoxy-modified polybutadiene Quality 1.8 1.8 1.8 1.8 1.8 1.8 1.8 1.8 1.8 (D) Polyester elastomers Quality 2.3 2.3 2.3 2.3 2.3 2.3 2.3 2.3 2.3 (F) (F1) Inorganic filler 1 Quality 39.7 39.7 39.7 Inorganic filler 2 Quality 39.7 Inorganic filler 3 Quality 39.7 Inorganic filler 4 Quality 39.7 Inorganic filler 5 Quality 39.7 (F2) Inorganic filler 6 Quality 39.7 Inorganic filler 7 Quality 39.7 Evaluation results (1) Resolution of vias (Pattern 1) - A A A A A A A A A (2) Adhesion strength to copper plating (peel strength) - A A A A A A B B A (3) Electrical insulation reliability (HAST resistance) - A A A A A A A A A (4) Resistance to glue residue removal - A A A A A A A A C
[0143] The components listed in Table 1 are as follows. (A)Ingredients: • Acid-modified epoxy derivative 1 containing ethylene unsaturated groups and an alicyclic skeleton [(A1) component and (A1-1) component]: the one obtained in Synthesis Example 1. • Acid-modified epoxy derivative 2 containing ethylene unsaturated groups and an alicyclic skeleton [(A1) component and (A1-1) component]: the one obtained in Synthesis Example 2. • Acid-modified epoxy derivative 3 containing ethylene unsaturated groups [(A2-1) component]: The one obtained in Synthesis Example 3 was used. • Dipentaerythritol pentaacrylate [(Aiii) component] (B) Ingredients: • Photopolymerization initiator 1: 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, acetophenone series compounds • Photopolymerization initiator 2: 2,4-Diethylthioxanthone, thioxanthone-based compounds (C) Ingredients: • Biphenyl-type epoxy resin: "YX-4000" (manufactured by Mitsubishi Chemical Corporation, trade name) • Epoxy-modified polybutadiene: "EPOLEAD (registered trademark) PB3600" (manufactured by Daicel Co., Ltd., trade name) (D) Ingredients: • Polyester-based elastomer: "Espel (registered trademark) 1108" (manufactured by Showa Denko Materials Co., Ltd., trade name) (F)Ingredients: • Inorganic filler 1: Silicon dioxide with an average primary particle diameter of 500 nm obtained in Manufacturing Example 1 • Inorganic filler 2: Silicon dioxide with an average primary particle diameter of 500 nm obtained in manufacturing example 2 • Inorganic filler 3: Silicon dioxide with an average primary particle diameter of 500 nm obtained in manufacturing example 3 • Inorganic filler 4: Silicon dioxide with an average primary particle diameter of 500 nm obtained in manufacturing example 4 • Inorganic filler 5: Silicon dioxide with an average primary particle diameter of 500 nm obtained in manufacturing example 5 • Inorganic filler 6 (for comparison): Silicon dioxide with an average primary particle diameter of 500 nm obtained in manufacturing example 6 • Inorganic filler 7 (for comparison): Silicon dioxide with an average primary particle diameter of 500 nm obtained in manufacturing example 7
[0144] According to Table 1, in Examples 1 to 6, compared to the Comparative Example, the via resolution, adhesion strength to copper plating, electrical insulation reliability, and resistance to descaling were all superior. The correct mechanism for obtaining this result is unclear, but it is speculated that it is influenced by the different intermolecular forces between (A1) photopolymers, which together possess ethylene unsaturated groups, acidic substituents, and alicyclic skeletons, and various inorganic fillers. On the other hand, in Comparative Example 1, which used inorganic filler 6 treated with a coupling agent containing methacrylic and methoxy groups, and in Comparative Example 2, which used inorganic filler 7 treated with a coupling agent containing amino and methoxy groups, the following results were observed: although the resolution of the vias, the reliability of electrical insulation, and the resistance to descaling were good, the adhesion strength to copper plating was reduced. Moreover, in Comparative Example 3, which contained (A2-1) but not (A1) in component (A), although the resolution of the vias, the adhesion strength to copper plating, and the reliability of electrical insulation were good, the resistance to descaling was significantly reduced.
[0145] 100A: Multilayer Printed Wiring Board 101:Substrate 102: Circuit Pattern 103: Interlayer insulation layer 104: Via (Through Hole) 105: Seed Crystal Layer 106: Resist Pattern 107: Copper Circuit Layer 108: Solder resist layer
Claims
1. A photosensitive resin composition comprising (A) a photopolymerizable compound having an ethylene unsaturated group, (B) a photopolymerization initiator, (C) a thermosetting resin, and (F) an inorganic filler, wherein the photopolymerizable compound having an ethylene unsaturated group comprises (A1) a photopolymerizable compound having an ethylene unsaturated group, an acidic substituent, and an alicyclic skeleton, wherein the (A1) photopolymerizable compound having an ethylene unsaturated group, an acidic substituent, and an alicyclic skeleton is (A1-1) an acid-modified epoxy derivative containing an ethylene unsaturated group and an alicyclic skeleton, wherein the (A1-1) acid-modified epoxy derivative containing an ethylene unsaturated group and an alicyclic skeleton is obtained by reacting a compound obtained by modifying an epoxy resin containing an alicyclic skeleton with an organic acid containing an ethylene unsaturated group (a2) with a polyacid anhydride containing a saturated or unsaturated group (a3). The inorganic filler (F) comprises an inorganic filler surface-treated with a coupling agent that does not have amine or (meth)acrylic groups, and the coupling agent has an alkoxy group. Based on the total solid content of the photosensitive resin composition, the content of the photopolymerizable compound (A) having an vinyl unsaturated group is 0.1% to 60% by mass, the content of the photopolymerization initiator (B) is 0.1% to 15% by mass, the content of the thermosetting resin (C) is 5% to 70% by mass, and the content of the inorganic filler (F) is 5% to 80% by mass.
2. The photosensitive resin composition as claimed in claim 1, wherein, The average particle size of the inorganic filler (F) is 0.01 μm to 5 μm.
3. The photosensitive resin composition as claimed in claim 1, wherein, The photopolymerizable compound having an vinyl unsaturated group (A) further comprises at least one selected from the group consisting of (Ai) a monofunctional vinyl monomer having one polymerizable vinyl unsaturated group, (Aii) a difunctional vinyl monomer having two polymerizable vinyl unsaturated groups, and (Aiii) a polyfunctional vinyl monomer having at least three polymerizable vinyl unsaturated groups.
4. The photosensitive resin composition as claimed in claim 1, wherein, In the photopolymerizable compound (A1) having an ethylene unsaturated group, an acidic substituent, and an alicyclic skeleton, the alicyclic skeleton is an alicyclic skeleton with 5 to 20 carbon atoms forming the ring.
5. The photosensitive resin composition as claimed in claim 1, wherein, In the photopolymerizable compound (A1) having an ethylene unsaturated group, an acidic substituent, and an alicyclic skeleton, the alicyclic skeleton comprises two or more rings.
6. The photosensitive resin composition as claimed in claim 1, further comprising (D) an elastomer.
7. The photosensitive resin composition as claimed in claim 6, wherein, The (D) elastomer comprises at least one selected from the group consisting of styrene-based elastomers, olefin-based elastomers, polyester-based elastomers, carbamate-based elastomers, polyamide-based elastomers, acrylic elastomers, and silicone-based elastomers.
8. The photosensitive resin composition as claimed in claim 1, wherein, The alicyclic skeletons are all cyclohexane skeletons, cyclohexene skeletons, norbornene skeletons, decahydronaphthalene skeletons, bicycloundecane skeletons, or saturated dicyclopentadiene skeletons.
9. A photosensitive resin composition for forming photosensitive vias, comprising the photosensitive resin composition as described in any one of claims 1 to 8.
10. A photosensitive resin composition for an interlayer insulating layer, comprising the photosensitive resin composition as described in any one of claims 1 to 8.
11. A photosensitive resin film comprising the photosensitive resin composition as described in any one of claims 1 to 8.
12. A photosensitive resin film for an interlayer insulating layer, comprising a photosensitive resin composition as described in any one of claims 1 to 8.
13. A multilayer printed wiring board comprising an interlayer insulating layer formed using a photosensitive resin composition as described in any one of claims 1 to 8.
14. A multilayer printed wiring board comprising an interlayer insulating layer formed using a photosensitive resin film as described in claim 11.
15. A semiconductor package comprising: a multilayer printed wiring board as described in claim 13 or 14; and a semiconductor element.
16. A method for manufacturing a multilayer printed wiring board, comprising the following (1) to (4): (1): laminating a photosensitive resin film as described in claim 11 onto one or both sides of a circuit board; (2): forming an interlayer insulating layer having vias by exposing and developing the photosensitive resin film laminated in (1); (3): roughening the vias and the interlayer insulating layer; (4): forming a circuit pattern on the interlayer insulating layer.
Citation Information
Patent Citations
Photosensitive resin composition
JP2013041114A
Curable resin composition, dry film, cured product, printed circuit board, and electronic component
TW202026354A