Method for recycling high-cod nickel-cobalt-lithium-magnesium wastewater and use thereof

High-COD nickel, cobalt, lithium and magnesium wastewater is treated through high-pressure CO2 air flotation oil removal and resin adsorption technology, combined with organophosphine chelating agents and ammonia precipitation, to prepare hexagonal magnesium hydroxide flame retardant, which solves the problems of magnesium loss and environmental pollution. It achieves efficient recovery and resource utilization of nickel, cobalt and lithium, reducing operating costs.

WO2024192575A1PCT designated stage expired Publication Date: 2024-09-26GUANGDONG BRUNP RECYCLING TECH CO LTD +1

Patent Information

Application Number
PCT/CN2023/082233
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-09-26

AI Technical Summary

Technical Problem

The existing technology has the problems of high loss of magnesium, environmental pollution and high operating costs when treating high COD wastewater containing nickel, cobalt, lithium and magnesium. In particular, the use of sodium sulfide can easily cause environmental pollution and damage workers' health, and its removal capacity is limited.

Method used

High-pressure CO2 flotation oil removal and resin adsorption technology are used to treat high COD nickel, cobalt, lithium and magnesium wastewater. Through the joint adsorption of hydrogen ion type and sodium ion type resin, combined with organic phosphine chelating agent and ammonia gas for precipitation, hexagonal hydroxide is prepared. Magnesium flame retardant, and precipitate and recover nickel and cobalt in the back-end concentrated solution to achieve efficient recovery and resource utilization of metals.

Benefits of technology

It achieves efficient recovery of nickel, cobalt and lithium metal, reduces the loss of magnesium, reduces the COD content, improves the purity and flame retardant properties of hexagonal magnesium hydroxide, reduces production costs, and improves process stability and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023082233_26092024_PF_FP
    Figure CN2023082233_26092024_PF_FP
Patent Text Reader

Abstract

A method for recycling high-COD nickel-cobalt-lithium-magnesium wastewater and the use thereof. The method comprises: carrying out an oil removal treatment on high-COD nickel-cobalt-lithium-magnesium wastewater; adsorbing Ni and Co ions in the liquid, which has been subjected to oil removal, with a hydrogen-ion-type resin; adsorbing Mg ions in the liquid, which has been subjected to primary adsorption, with a sodium-ion-type resin; then desorbing the adsorbed sodium-ion-type resin with an acid to obtain a magnesium salt desorption solution; and adding an organic phosphine chelating agent to the magnesium salt desorption solution, introducing ammonia thereto to carry out a magnesium precipitation reaction, and washing the precipitate with water and a dilute acid to obtain a hexagonal magnesium hydroxide solid. The COD-removed wastewater is subjected to the combined adsorption of two segments of resins of the hydrogen-ion-type resin and the sodium-ion-type resin, which contributes to subsequently obtaining a hexagonal magnesium hydroxide flame retardant solid with a higher purity; and the chelating agent can be grafted to the surface of the resulting hexagonal magnesium hydroxide solid to modify the hexagonal magnesium hydroxide solid, such that the thermal stability and the flame retardance of the modified hexagonal magnesium hydroxide solid can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Resource recovery method and application of high COD nickel-cobalt-lithium-magnesium wastewater Technical Field

[0001] The present invention belongs to the technical field of wastewater treatment and metal resource recycling, and specifically relates to a resource recovery method for high-COD nickel-cobalt-lithium-magnesium wastewater and its application. Background Art

[0002] With the rapid development of China's new energy industry, lithium-ion batteries have been widely used due to their high energy storage, rapid charge and discharge, long cycle life, and environmental friendliness. Positive and negative electrode materials are the core key materials in lithium-ion batteries. The lower limit of the energy density of lithium-ion batteries depends on the positive and negative electrode materials, and the positive and negative electrode materials account for 60% to 70% of the cost of lithium-ion batteries. Therefore, accelerating the research and development of positive and negative electrode materials and improving production processes will not only help improve the overall performance of lithium-ion batteries, but also have the potential to significantly reduce the currently high battery costs.

[0003] During the hydrometallurgical smelting of ternary cathode materials, the extraction, separation, and purification of nickel, cobalt, and manganese sulfates produces a large amount of high-COD nickel, cobalt, lithium, and magnesium wastewater. Due to the high economic value of nickel, cobalt, and lithium, this wastewater has a high recycling value. The current process involves degreasing with activated carbon, then removing the nickel, cobalt, and manganese metals with sodium sulfide. The resulting filter residue is then returned to the leaching process, where sodium hydroxide is added to the resulting sodium sulfate solution containing lithium and magnesium to produce magnesium hydroxide. After filter pressing, solid waste and liquid waste are generated. The wastewater is then evaporated and concentrated to produce sodium sulfate and lithium sulfate. This process relies on chemical precipitation to remove metals, resulting in significant lithium losses and limited removal capacity. This results in a high processing load for the back-end evaporation and concentration process, which increases operating costs. Therefore, the current method for treating magnesium-containing wastewater containing heavy metals, high salinity, and high COD uses sodium sulfide to remove nickel and cobalt, but some magnesium is precipitated and re-enters the system. Sodium sulfide is not only environmentally polluting but also harmful to the health of workers in the workplace. Sodium hydroxide is used to precipitate the magnesium, requiring a high dosage. Precipitation also presents the problem of high lithium losses. Therefore, there is an urgent need to develop a method for treating high COD nickel-cobalt-lithium-magnesium wastewater and realize resource utilization.

[0004] Summary of the Invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a resource recovery method and application for high-COD nickel-cobalt-lithium-magnesium wastewater. While treating high-COD nickel-cobalt-lithium-magnesium wastewater, a surface-modified hexagonal magnesium hydroxide flame retardant is prepared. Nickel and cobalt are then recovered by precipitation in the concentrated liquid at the back end, achieving efficient recovery and high-value utilization of metals in wastewater and waste residue.

[0006] According to one aspect of the present invention, a method for recycling high COD nickel-cobalt-lithium-magnesium wastewater is proposed, comprising the following steps:

[0007] S1: Deoiling high COD nickel-cobalt-lithium-magnesium wastewater to obtain deoiled liquid;

[0008] S2: using a hydrogen ion resin to adsorb Ni and Co ions in the deoiled liquid to obtain a primary adsorption liquid;

[0009] S3: adsorbing Mg ions in the primary adsorption liquid with a sodium ion resin to obtain a secondary adsorption liquid, and then desorbing the adsorbed sodium ion resin with an acid to obtain a magnesium salt desorption liquid;

[0010] S4: adding an organic phosphine chelating agent to the magnesium salt desorption solution, and introducing ammonia gas to carry out magnesium precipitation reaction, aging, and solid-liquid separation. The obtained precipitate is washed with water and dilute acid to obtain hexagonal magnesium hydroxide solid.

[0011] In some embodiments of the present invention, in step S1, the COD content in the high-COD nickel-cobalt-lithium-magnesium wastewater is 1000-1500 mg / L, the nickel metal content is 30-100 mg / L, the cobalt metal content is 15-100 mg / L, the lithium metal content is 0.5-10 g / L, and the magnesium metal content is 50-150 mg / L.

[0012] In some embodiments of the present invention, in step S1, the deoiling process is as follows: first, a high-pressure CO2 aqueous solution or a high-pressure CO2 liquid is introduced into the high-COD nickel-cobalt-lithium-magnesium wastewater for flotation deoiling, and then the wastewater after flotation deoiling is subjected to adsorption deoiling through a packed column to obtain the deoiled liquid. Furthermore, the high-pressure CO2 aqueous solution is a saturated CO2 pressurized aqueous solution with a pressurization pressure of 0.5-7Mpa, and the amount of the high-pressure CO2 aqueous solution is 8-12% of the volume of the high-COD nickel-cobalt-lithium-magnesium wastewater. Furthermore, the flotation deoiling time is 2-4h. Using a high-pressure CO2 aqueous solution for flotation deoiling can utilize the process characteristics of CO2 precipitating from the solution under reduced pressure to gasify or cause the micro-emulsified oil substances in the wastewater to agglomerate and float, and after the high-pressure carbon dioxide is treated with deoiling adsorption, it can be reused by an air compressor, thereby reducing the consumption of auxiliary materials in the production process. The present invention combines high-pressure CO2 aqueous solution for flotation oil removal and packed column adsorption oil removal, which can effectively reduce the COD content in wastewater, reduce the pollution of oil substances to the adsorption resin in subsequent work sections, and enhance process stability.

[0013] In some embodiments of the present invention, in step S1, the CO2 after the flotation oil removal is purified by air filtration and compressed at a pressure of 0.5-1 MPa and reused in the flotation oil removal process.

[0014] In some embodiments of the present invention, in step S1, the oil removal filler of the filling column is activated carbon or ethylene-acrylonitrile copolymer gel-type oil removal resin.

[0015] In some embodiments of the present invention, in step S1, the COD content in the high-COD nickel-cobalt-lithium-magnesium wastewater after oil removal is 50-200 mg / L.

[0016] In some embodiments of the present invention, in step S2, the hydrogen ion resin is a polystyrene molecular skeleton chelate resin.

[0017] In some embodiments of the present invention, in step S2, the adsorption conditions of the hydrogen ion resin are: the resin absorption tower is filled with a height-to-diameter ratio of (2-3):1, a flow rate of 4-5 BV / h, and the solution is controlled at a pH of 5-8.

[0018] In some embodiments of the present invention, step S2 further includes: desorbing and regenerating the adsorbed hydrogen ion resin with an acid to obtain a nickel-cobalt desorption solution. Furthermore, the acid used is sulfuric acid with a mass concentration of 10% to 20%, and the pH is maintained at >3 during the pickling process.

[0019] In some embodiments of the present invention, in step S3, the sodium ion resin is a styrene-divinylbenzene copolymer sulfonyl resin, a styrene-divinylbenzene cross-linked aminophosphonic acid chelate resin or a polystyrene copolymer type I quaternary amine functional resin.

[0020] In some embodiments of the present invention, in step S3, the adsorption conditions of the sodium ion resin are: the resin absorption tower is filled with a height-to-diameter ratio of (2-3): 1, a flow rate of 3-5 BV / h, and the solution is controlled at a pH of 7-9.

[0021] In some embodiments of the present invention, in step S3, desorption is performed using sulfuric acid with a mass concentration of 10%-20%, and the pickling flow rate is 2-4 BV / h.

[0022] In some embodiments of the present invention, in step S3, after desorption, the sodium ion resin is regenerated with a 20 wt % to 30 wt % sodium hydroxide solution at a flow rate of 2-5 BV / h for 1-2 hours.

[0023] In some embodiments of the present invention, step S3 further includes: performing MVR concentration on the secondary adsorption liquid to obtain sodium sulfate and a concentrated liquid, and subjecting the concentrated liquid to lithium precipitation with sodium carbonate to obtain crude lithium carbonate. The secondary adsorption liquid itself has a high salt content, and sodium sulfate can be obtained by concentrating it by evaporation to 1 / 5-1 / 3 of its original volume.

[0024] In some embodiments of the present invention, in step S4, the concentration of magnesium ions in the magnesium salt desorption solution is 0.5-2.5 mol / L.

[0025] In some embodiments of the present invention, in step S4, ammonia gas is introduced to maintain the pH of the solution at 10-12.

[0026] In some embodiments of the present invention, in step S4, the organic phosphine chelating agent is at least one of hexamethylenediaminetetramethylenephosphonic acid (HDTMPA), ethylenediaminetetramethylenephosphonic acid, hydroxyethylidene diphosphonic acid (HEDP), aminotrimethylenephosphonic acid, hexylphosphonic acid or dodecylphosphonic acid.

[0027] In some embodiments of the present invention, in step S4, the amount of the organic phosphine chelating agent added is 1 wt%-5 wt% of the theoretical yield of magnesium hydroxide.

[0028] In some embodiments of the present invention, in step S4, the temperature of the magnesium precipitation reaction is 40-80°C.

[0029] In some embodiments of the present invention, in step S4, the aging time is 2-6 hours.

[0030] In some embodiments of the present invention, in step S4, the mass concentration of the dilute acid is 1%-5%. Furthermore, the dilute acid is dilute hydrochloric acid.

[0031] In some embodiments of the present invention, step S4 further includes: evaporating and concentrating the filtrate after the solid-liquid separation, recycling the evaporated ammonia gas to the magnesium precipitation operation, adding alkali to the evaporated and concentrated solution to adjust the pH value for precipitation to obtain nickel-cobalt slag. Furthermore, the nickel-cobalt slag is acid-dissolved and then returned to the hydrogen ion resin in step S2 for adsorption, desorption to obtain a nickel-cobalt desorption solution, or returned to the front-end extraction process for purification to produce a refined nickel-cobalt solution.

[0032] The present invention also provides the use of the hexagonal magnesium hydroxide solid prepared by the resource recovery method in flame retardant materials.

[0033] According to a preferred embodiment of the present invention, there are at least the following beneficial effects:

[0034] 1. The wastewater after COD removal in the present invention is subjected to the combined adsorption of hydrogen ion resin and sodium ion resin in two stages, which can increase the content of Mg ions in the magnesium salt desorption solution and reduce the content of nickel, cobalt and manganese metals, which is conducive to the subsequent acquisition of a higher purity hexagonal magnesium hydroxide flame retardant solid. Moreover, the nickel cobalt salt solution obtained by desorption can be directly reused in the front-end extraction process for purification and production of refined nickel cobalt salt products. The best experimental process at present is to first adsorb nickel cobalt and then adsorb magnesium to achieve the separation of nickel cobalt and magnesium. Since the resins on the market that adsorb nickel cobalt have stronger selectivity, magnesium will only be carried over in small amounts due to the difference in nickel cobalt and magnesium concentrations, which does not affect the adsorption capacity of nickel cobalt. If magnesium in the wastewater is adsorbed first and then nickel cobalt is adsorbed, on the one hand, when magnesium is adsorbed, nickel cobalt will be adsorbed together, affecting the resin's adsorption effect on magnesium, and on the other hand, increasing the loss of nickel cobalt.

[0035] 2. The present invention uses a combined process of segmented adsorption of nickel, cobalt and magnesium with special selective resins to achieve short-range and efficient recovery of nickel, cobalt and lithium from wastewater. The two resins have low adsorption capacity for Li ions. After secondary adsorption, the lithium in the liquid can be concentrated to produce sodium sulfate as a by-product, and the concentrated mother liquor is precipitated to obtain crude lithium carbonate, with an overall recovery rate of up to 98%.

[0036] 3. Organic phosphine chelating agents can chelate with Ni, Co, Ca, and Fe metal ions in the magnesium salt desorption solution. Under the alkaline conditions of ammonia, they will basically not precipitate or be trapped in the magnesium hydroxide precipitate. The chelating agent has multiple phosphate groups, and its molecular chain can be preferentially adsorbed on the (001) and (101) crystal planes of the magnesium hydroxide crystal. The (001) and (101) crystal planes are the main exposed surfaces of the regular hexagonal flakes. Therefore, the chelating agent has the function of regulating the growth direction of the magnesium hydroxide crystal form, and can obtain a hexagonal crystal structure suitable for flame retardants. In addition, the chelating agent can also be grafted onto the surface of the generated hexagonal magnesium hydroxide solid to modify it. The modified hexagonal magnesium hydroxide solid has more carbon chains, and its thermal stability and flame retardant properties are improved. It can also improve the surface adhesion between magnesium hydroxide and the flame retardant matrix material and solve the problem of poor compatibility between the two, reaching the standard for adding to polymers for flame retardancy.

[0037] 4. The precipitate obtained after the magnesium precipitation reaction is washed with dilute acid to remove the complex impurity metal ions on the surface and at the same time make the phosphate groups grafted on the surface become P(OH). If it is not washed with dilute acid, it may become POM, which is not conducive to the flame retardancy of magnesium hydroxide. The use of low concentration dilute acid has less impact on the magnesium hydroxide solid. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:

[0039] FIG1 is a process flow chart of Example 1 of the present invention;

[0040] FIG2 is a schematic diagram of the principle of magnesium hydroxide surface modified with hexamethylenediaminetetramethylenephosphonic acid (HDTMPA) of the present invention;

[0041] FIG3 is an SEM image of hexagonal magnesium hydroxide surface-modified with different amounts of hexamethylenediaminetetramethylenephosphonic acid (HDTMPA) added (1%, 3%, 5%) according to the present invention;

[0042] FIG4 is a SEM image of magnesium hydroxide prepared by direct precipitation without using a chelating agent in Comparative Example 2 of the present invention;

[0043] Figure 5 shows the DSC curves of magnesium hydroxide before (a) and after (b) modification. DETAILED DESCRIPTION

[0044] The following will clearly and completely describe the concept and technical effects of the present invention in conjunction with the embodiments to fully understand the purpose, features and effects of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0045] Example 1

[0046] A resource recovery method for high COD nickel-cobalt-lithium-magnesium wastewater, referring to FIG1 , the specific process is as follows:

[0047] Step (1): After the high-COD nickel-cobalt-lithium-magnesium wastewater is allowed to stand, a 0.5 MPa CO2 aqueous solution is introduced to perform flotation deoiling operation for 4 hours, wherein the amount of the high-pressure CO2 aqueous solution is 10% of the volume of the high-COD nickel-cobalt-lithium-magnesium wastewater, and the high-COD nickel-cobalt-lithium-magnesium wastewater has a COD content of 1500 mg / L, a nickel metal content of 100 mg / L, a cobalt metal content of 35 mg / L, a lithium metal content of 10 g / L, and a magnesium metal content of 150 mg / L;

[0048] Step (2): The wastewater after flotation oil removal is again passed through an activated carbon column for adsorption oil removal, and the COD of the solution can be reduced to 150 mg / L;

[0049] Step (3): using a polystyrene molecular skeleton chelating resin (hydrogen ion resin D463 resin of Xi'an Lanxiao Technology Co., Ltd.) to adsorb Ni and Co metal ions in the wastewater obtained in step (2); the resin absorption tower is filled with a height-to-diameter ratio of 2:1, the flow rate is 4BV / h, the solution is controlled to have a pH of 5, and a primary adsorption liquid is obtained after the adsorption operation; using 10% sulfuric acid to desorb and regenerate the polystyrene molecular skeleton chelating resin, and the pH is maintained at 3 during the pickling process to obtain a nickel-cobalt sulfate desorption solution containing 2.4 g / L nickel, 0.9 g / L cobalt, and 0.1 g / L magnesium;

[0050] Step (4): passing the primary adsorption liquid obtained in step (3) into a styrene-divinylbenzene cross-linked aminophosphonic acid chelating resin (Xi'an Lanxiao Technology Co., Ltd. aminophosphonic acid chelating resin LSC-850) for Mg metal ion adsorption, wherein the operating conditions are a resin absorption tower filling height-to-diameter ratio of 3:1, a flow rate of 5BV / h, and a solution pH controlled at 9, to obtain a secondary adsorption liquid after the operation; the secondary adsorption liquid is subjected to MVR concentration and crystallization to obtain sodium sulfate, and the concentrated mother liquor is subjected to lithium precipitation operation using sodium carbonate to obtain crude lithium carbonate;

[0051] Step (5): Desorbing the saturated adsorption styrene-divinylbenzene copolymer sulfonyl resin in step (4) using 10% sulfuric acid at a flow rate of 2 BV / h to obtain a magnesium sulfate desorption solution; then regenerating the styrene-divinylbenzene copolymer sulfonyl resin using 20% ​​sodium hydroxide solution at a flow rate of 5 BV / h for 2 hours;

[0052] Step (6): adding a chelating agent HDTMPA and introducing ammonia to the magnesium salt desorption solution to carry out a magnesium precipitation reaction, wherein the concentration of the magnesium salt desorption solution is 0.5 mol / L, and ammonia is introduced to maintain the pH of the solution at 10. The amount of chelating agent added is 1% of the theoretical yield of magnesium hydroxide, the reaction temperature is 40°C, and the precipitation aging reaction time is 2h; after aging and filtering, washing with water and then washing with 1% dilute hydrochloric acid, and finally washing with water, and drying to obtain hexagonal magnesium hydroxide solid;

[0053] Step (7): filtering the magnesium precipitate in step (6) to obtain a filtrate, evaporating and concentrating it, and returning the evaporated ammonia to step (6); adding soda ash to the concentrated mother liquor to adjust the value and precipitate it to obtain nickel-cobalt slag; dissolving the nickel-cobalt slag with low acid to obtain an acid solution, returning it to step (3) to perform nickel-cobalt metal adsorption and desorption operations for recovery.

[0054] Example 2

[0055] A resource recovery method for high COD nickel-cobalt-lithium-magnesium wastewater, the specific process is as follows:

[0056] Step (1): After the high-COD nickel-cobalt-lithium-magnesium wastewater is allowed to stand, a 3MPa CO2 aqueous solution is introduced to perform flotation deoiling operation for 3 hours, wherein the amount of the high-pressure CO2 aqueous solution is 8% of the volume of the high-COD nickel-cobalt-lithium-magnesium wastewater, and the high-COD nickel-cobalt-lithium-magnesium wastewater has a COD content of 1300mg / L, a nickel metal content of 50mg / L, a cobalt metal content of 25mg / L, a lithium metal content of 5g / L, and a magnesium metal content of 100mg / L;

[0057] Step (2): The wastewater after flotation oil removal is again passed through an activated carbon column for adsorption oil removal, and the COD of the solution can be reduced to 100 mg / L;

[0058] Step (3): using a polystyrene molecular skeleton chelating resin to adsorb Ni and Co metal ions on the wastewater obtained in step (2); the resin absorption tower is filled with a height-to-diameter ratio of 2.5:1, the flow rate is 4.5 BV / h, the solution pH is controlled at 7, and a primary adsorption liquid is obtained after the adsorption operation; using 15% sulfuric acid to desorb and regenerate the polystyrene molecular skeleton chelating resin, and the pH is maintained at >3 during the pickling process to obtain a nickel-cobalt sulfate desorption solution containing 2.6 g / L nickel, 1.2 g / L cobalt, and 0.15 g / L magnesium;

[0059] Step (4): passing the primary adsorption liquid obtained in step (3) into a styrene-divinylbenzene copolymer sulfonyl resin to adsorb Mg metal ions. The operating conditions are as follows: the resin absorption tower is filled with a height-to-diameter ratio of 2.5:1, the flow rate is 4BV / h, and the solution is controlled to have a pH of 8. After the operation, a secondary adsorption liquid is obtained; the secondary adsorption liquid is subjected to MVR concentration and crystallization to obtain sodium sulfate, and the concentrated mother liquor is subjected to lithium precipitation operation using sodium carbonate to obtain crude lithium carbonate;

[0060] Step (5): Desorbing the saturated adsorption styrene-divinylbenzene copolymer sulfonyl resin in step (4) using 10% sulfuric acid at a flow rate of 2 BV / h to obtain a magnesium sulfate desorption solution; then regenerating the styrene-divinylbenzene copolymer sulfonyl resin using 20% ​​sodium hydroxide solution at a flow rate of 5 BV / h for 2 hours;

[0061] Step (6): adding a chelating agent HDTMPA and introducing ammonia to the magnesium salt desorption solution to carry out a magnesium precipitation reaction, wherein the concentration of the magnesium salt desorption solution is 1.5 mol / L, ammonia is introduced to maintain the pH of the solution at 11, the amount of the chelating agent added is 3% of the theoretical yield of magnesium hydroxide, the reaction temperature is 60°C, and the precipitation aging reaction time is 4h; after aging and filtering, washing with water and then washing with 3% dilute hydrochloric acid, and finally washing with water, and drying to obtain hexagonal magnesium hydroxide solid;

[0062] Step (7): filtering the magnesium precipitate in step (6) to obtain a filtrate, evaporating and concentrating it, and returning the evaporated ammonia to step (6); adding soda ash to the concentrated mother liquor to adjust the value and precipitate it to obtain nickel-cobalt slag; dissolving the nickel-cobalt slag with low acid to obtain an acid solution, returning it to step (3) to perform nickel-cobalt metal adsorption and desorption operations for recovery.

[0063] Example 3

[0064] A resource recovery method for high COD nickel-cobalt-lithium-magnesium wastewater, the specific process is as follows:

[0065] Step (1): After the high-COD nickel-cobalt-lithium-magnesium wastewater is allowed to stand, a 7MPa CO2 aqueous solution is introduced to perform flotation deoiling operation for 2 hours, wherein the amount of the high-pressure CO2 aqueous solution is 10% of the volume of the high-COD nickel-cobalt-lithium-magnesium wastewater, and the high-COD nickel-cobalt-lithium-magnesium wastewater has a COD content of 1000 mg / L, a nickel metal content of 30 mg / L, a cobalt metal content of 15 mg / L, a lithium metal content of 0.5 g / L, and a magnesium metal content of 50 mg / L;

[0066] Step (2): The wastewater after flotation oil removal is again passed through an activated carbon column for adsorption oil removal, and the COD of the solution can be reduced to 50 mg / L;

[0067] Step (3): using a polystyrene molecular skeleton chelating resin to adsorb Ni and Co metal ions on the wastewater obtained in step (2); the resin absorption tower is filled with a height-to-diameter ratio of 3:1, the flow rate is 5 BV / h, the solution is controlled to have a pH of 8, and a primary adsorption liquid is obtained after the adsorption operation; using 20% ​​sulfuric acid to desorb and regenerate the polystyrene molecular skeleton chelating resin, and the pH is maintained at >3 during the pickling process to obtain a nickel-cobalt sulfate desorption solution containing 2.8 g / L nickel, 1.3 g / L cobalt, and 0.25 g / L magnesium;

[0068] Step (4): passing the primary adsorption liquid obtained in step (3) into a styrene-divinylbenzene copolymer sulfonyl resin to adsorb Mg metal ions. The operating conditions are as follows: the resin absorption tower is filled with a height-to-diameter ratio of 2:1, the flow rate is 3BV / h, and the solution is controlled to have a pH of 7. After the operation, a secondary adsorption liquid is obtained; the secondary adsorption liquid is subjected to MVR concentration and crystallization to obtain sodium sulfate, and the concentrated mother liquor is subjected to lithium precipitation operation using sodium carbonate to obtain crude lithium carbonate;

[0069] Step (5): Desorbing the saturated adsorption styrene-divinylbenzene copolymer sulfonyl resin in step (4) using 10% sulfuric acid at a flow rate of 2 BV / h to obtain a magnesium sulfate desorption solution; then regenerating the styrene-divinylbenzene copolymer sulfonyl resin using 20% ​​sodium hydroxide solution at a flow rate of 5 BV / h for 2 hours;

[0070] Step (6): adding a chelating agent HDTMPA and introducing ammonia to the magnesium salt desorption solution to carry out a magnesium precipitation reaction, wherein the concentration of the magnesium salt desorption solution is 2.5 mol / L, and ammonia is introduced to maintain the solution pH at 12. The amount of chelating agent added is 5% of the theoretical yield of magnesium hydroxide, the reaction temperature is 80°C, and the precipitation aging reaction time is 6 hours; after aging and filtering, washing with water and then washing with 5% dilute hydrochloric acid, and finally washing with water, and drying to obtain hexagonal magnesium hydroxide solid;

[0071] Step (7): filtering the magnesium precipitate in step (6) to obtain a filtrate, evaporating and concentrating it, and returning the evaporated ammonia to step (6); adding soda ash to the concentrated mother liquor to adjust the value and precipitate it to obtain nickel-cobalt slag; dissolving the nickel-cobalt slag with low acid to obtain an acid solution, returning it to step (3) to perform nickel-cobalt metal adsorption and desorption operations for recovery.

[0072] Comparative Example 1

[0073] A resource recovery method for high COD nickel-cobalt-lithium-magnesium wastewater, which differs from Example 1 in that magnesium is adsorbed first and then nickel-cobalt is adsorbed. The specific process is as follows:

[0074] Steps (1) and (2) are the same as in Example 1;

[0075] Step (3): passing the wastewater obtained in step (2) into a styrene-divinylbenzene cross-linked aminophosphonic acid chelating resin to adsorb Mg metal ions. The operating conditions are as follows: a resin absorption tower with a height-to-diameter ratio of 3:1, a flow rate of 5 BV / h, and a solution pH controlled at 9. After the operation, a primary adsorption liquid is obtained;

[0076] Step (4): passing the primary adsorption liquid obtained in step (3) into a polystyrene molecular skeleton chelating resin to adsorb Ni and Co metal ions, the resin absorption tower is filled with a height-to-diameter ratio of 2:1, the flow rate is 4BV / h, and the solution is controlled to have a pH of 5, and a secondary adsorption liquid is obtained after the operation; using 10% sulfuric acid to desorb and regenerate the polystyrene molecular skeleton chelating resin, and the pH is maintained at >3 during the pickling process to obtain a nickel-cobalt sulfate desorption liquid containing 2.1 g / L nickel, 0.5 g / L cobalt, and 0.05 g / L magnesium;

[0077] Step (5): using 10% sulfuric acid at a flow rate of 2 BV / h to desorb the styrene-divinylbenzene cross-linked aminophosphonic acid chelating resin adsorbed saturated in step (3) to obtain a magnesium sulfate desorption solution; then using 20% ​​sodium hydroxide solution at a flow rate of 5 BV / h to regenerate the styrene-divinylbenzene copolymer sulfonyl resin for 2 hours;

[0078] Step (6): The secondary adsorption liquid obtained in step (4) is subjected to MVR concentration and crystallization to obtain sodium sulfate, and the concentrated mother liquor is subjected to lithium precipitation operation using sodium carbonate to obtain crude lithium carbonate.

[0079] Comparative Example 2

[0080] The difference between the styrene-divinylbenzene copolymer sulfonyl resin and Example 3 is that no chelating agent is added in the magnesium precipitation reaction. The specific process is as follows:

[0081] Steps (1) to (5) are the same as in Example 3;

[0082] Step (6): without adding a chelating agent, ammonia gas is directly introduced into the magnesium salt solution to precipitate magnesium, the concentration of the magnesium salt solution is 2.5 mol / L, ammonia gas is introduced to maintain the solution pH at 12, the reaction temperature is 80°C, and the precipitation aging reaction time is 6 hours; after aging and filtration, the solution is washed with water and dried to obtain hexagonal magnesium hydroxide solid.

[0083] The metal element compositions of the magnesium sulfate desorption solutions of Examples 1-3 and Comparative Example 1 were tested, and the results are shown in Table 1 below.

[0084] Table 1 Metal element composition of magnesium sulfate desorption solution

[0085] Note: Element content (wt%) refers to the ratio of each metal element to the total metal elements in the magnesium sulfate desorption solution.

[0086] As can be seen from Table 1, the Mg content in the magnesium sulfate desorption solution of Comparative Example 1 is significantly reduced, while the nickel and cobalt elements are increased. This is because the styrene-divinylbenzene copolymer sulfonyl resin has insufficient selectivity for magnesium. When adsorbing magnesium, some nickel and cobalt are adsorbed together, affecting the resin's adsorption effect on magnesium. In contrast, Example 1 first adsorbs nickel and cobalt, and then adsorbs magnesium. The polystyrene molecular skeleton chelate resin has a stronger selectivity for nickel and cobalt, and only a small amount of magnesium is entrained, which does not affect the adsorption capacity of nickel and cobalt.

[0087] The metal element composition, specific surface area (BET), and D50 of the magnesium hydroxide solids of Examples 1-3 and Comparative Example 2 were tested, and the results are shown in Table 2 below.

[0088] Table 2 Metal element composition, BET, D50 of magnesium hydroxide solid

[0089] As shown in Table 2, the impurity elements in the magnesium hydroxide solid obtained in Comparative Example 2 are obviously more than those in Example 3. This is because after Example 3 adds a chelating agent, the chelating agent can chelate with the Ni, Co, Ca, and Fe metal ions in the magnesium sulfate stripping solution, and can not be precipitated or be sandwiched in the magnesium hydroxide precipitation, thereby improving the purity of magnesium hydroxide. The specific surface area of ​​Comparative Example 2 is also obviously higher than that of Example 3, indicating that the magnesium hydroxide crystals generated without using a chelating agent have obvious defects, and the crystal form is incomplete.

[0090] The metal yields of Examples 1-3 and Comparative Examples 1-2 are shown in Table 3 below.

[0091] Table 3 Metal yields of Examples and Comparative Examples

[0092] The nickel-cobalt-magnesium recovery rate of comparative example 1 is significantly reduced. This is because the special selectivity of styrene-divinylbenzene cross-linked aminophosphonic acid chelate resin to magnesium is not strong enough. When adsorbing magnesium, part of nickel and cobalt can be adsorbed together, affecting the adsorption effect of resin on magnesium. While embodiment 1 first adsorbs nickel and cobalt, and then adsorbs magnesium. The special selectivity of polystyrene molecular skeleton chelate resin to nickel and cobalt is stronger, and magnesium only has a small amount of entrainment, which does not affect the adsorption capacity of nickel and cobalt. The nickel-cobalt-lithium-magnesium recovery rate of comparative example 2 is not much different from embodiment 3. This is because the chelating agent added in embodiment 3 does not affect the recovery rate of magnesium, and only has an impact on the hexagonal magnesium hydroxide crystal form. Adopting special selective resin segmented adsorption of nickel and cobalt and magnesium combined process can increase the nickel-cobalt-lithium-magnesium recovery rate.

[0093] Figure 3 shows SEM images of hexagonal magnesium hydroxide surface-modified with different amounts of hexamethylenediaminetetramethylenephosphonic acid (HDTMPA) (1%, 3%, and 5%). Figure 4 shows an SEM image of magnesium hydroxide prepared by direct precipitation without a chelating agent in Comparative Example 2. As can be seen from the figures, the hexagonal magnesium hydroxide prepared with 1%, 3%, and 5% HDTMPA additions differ significantly from that without the chelating agent. The crystals produced without the chelating agent exhibit varying morphologies, overlapping, and significant agglomeration, with obvious defects. With the addition of HDTMPA, the resulting crystals become more complete, more neatly arranged, and exhibit reduced agglomeration. With the addition of a smaller amount of HDTMPA (1%), the crystals still exhibit irregular, agglomerated flakes, due to insufficient chelating agent molecular chains. With the addition of a larger amount of HDTMPA (5%), the overly long molecular chains may cause the hexagonal flakes to entangle with each other during growth. Adding an appropriate amount of HDTMPA (3%) yields more successfully modified hexagonal magnesium hydroxide.

[0094] Figure 5 shows the DSC curves of magnesium hydroxide before (a) and after (b) modification, respectively, corresponding to Example 3 and Comparative Example 2. After the solid surface of hexagonal magnesium hydroxide is modified with HDTMPA, the carbon chain increases, the thermal stability and flame retardancy are improved, the heat absorption of the modified magnesium hydroxide increases, and the endothermic enthalpy increases. Due to the grafting of the chelating agent HDTMPA, the pyrolysis temperature increases.

[0095] While the embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to the embodiments described above. Various modifications may be made within the scope of knowledge possessed by a person skilled in the art without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof may be combined with one another unless there is a conflict.

Claims

1. A method for recycling high COD nickel-cobalt-lithium-magnesium wastewater, characterized in that: The following steps are involved: S1: Deoiling high COD nickel-cobalt-lithium-magnesium wastewater to obtain deoiled liquid; S2: using a hydrogen ion resin to adsorb Ni and Co ions in the deoiled liquid to obtain a primary adsorbed liquid; S3: adsorbing Mg ions in the liquid after the primary adsorption with a sodium ion resin to obtain a liquid after the secondary adsorption, and then desorbing the adsorbed sodium ion resin with an acid to obtain a magnesium salt desorption liquid; S4: adding an organic phosphine chelating agent to the magnesium salt desorption solution, and introducing ammonia gas to carry out magnesium precipitation reaction, and separating the solid and liquid after aging, and washing the obtained precipitate with water and dilute acid to obtain hexagonal magnesium hydroxide solid.

2. The resource recovery method according to claim 1, characterized in that: In step S1, the COD content of the high COD nickel-cobalt-lithium-magnesium wastewater is 1000-1500 mg / L, the nickel metal content is 30-100 mg / L, the cobalt metal content is 20-100 mg / L, the lithium metal content is 0.5-10 g / L, and the magnesium metal content is 50-150 mg / L.

3. The resource recovery method according to claim 1, characterized in that: In step S1, the oil removal process is: first, high-pressure CO2 aqueous solution or high-pressure CO2 liquid is introduced into the high-COD nickel-cobalt-lithium-magnesium wastewater for flotation oil removal, and then the wastewater after flotation oil removal is passed through a filling column for adsorption oil removal to obtain the deoiled liquid.

4. The resource recovery method according to claim 1, characterized in that: In step S2, the hydrogen ion type resin is a polystyrene molecular skeleton chelating resin.

5. The resource recovery method according to claim 1, characterized in that: In step S3, the sodium ion type resin is styrene-divinylbenzene copolymer sulfonyl resin, styrene-divinylbenzene cross-linked aminophosphonic acid chelating resin or polystyrene copolymer type I quaternary amine functional group resin.

6. The resource recovery method according to claim 1, characterized in that: Step S3 further includes: performing MVR concentration on the secondary adsorption liquid to obtain sodium sulphate and concentrated liquid, and using sodium carbonate to precipitate lithium from the concentrated liquid to obtain crude lithium carbonate.

7. The resource recovery method according to claim 1, characterized in that: In step S4, the organic phosphine chelating agent is at least one of hexamethylenediaminetetramethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, hydroxyethylidene diphosphonic acid, aminotrimethylenephosphonic acid, hexylphosphonic acid or dodecylphosphonic acid.

8. The resource recovery method according to claim 1, characterized in that: In step S4, the amount of the organic phosphine chelating agent added is 1wt%-5wt% of the theoretical output of magnesium hydroxide.

9. The resource recovery method according to claim 1, characterized in that: Step S4 also includes: evaporating and concentrating the filtrate after the solid-liquid separation, recycling the evaporated ammonia gas to the magnesium precipitation operation, adding alkali to the evaporated concentrated solution to adjust the pH value for precipitation, and obtaining nickel-cobalt slag.

10. Use of the hexagonal magnesium hydroxide solid obtained by the resource recovery method according to any one of claims 1 to 9 in flame retardant materials.

Citation Information

Patent Citations

  • Method for preparing magnesium hydrate through ammonia spray method

    CN103101936A

  • Cobalt and magnesium separation method in cobalt nickel wet metallurgy process

    CN108179272A

  • Modified magnesium hydroxide, surface modification method and application thereof

    CN110194852A

  • Method for recovering nickel and cobalt from laterite-nickel ore through resin adsorption method

    CN113249571A

  • Treatment method of nickel-cobalt smelting heavy metal wastewater

    CN113307438A

Cited By

  • Diammonium phosphate production process based on titanium chemical industry waste acid and wastewater

    CN122853335A

  • A Diammonium Phosphate Production Process Based on Waste Acid from Titanium Chemical Industry

    CN122853335B