Method and device for extracting and obtaining low-impurity lithium ions by electrochemical method
Mesoporous activated carbon materials absorb impurity cations in salt solution and combine with chemical deintercalation lithium ion screens to separate lithium ions, which solves the problem of impurity cation adsorption in the existing technology, improves the extraction efficiency and purity of lithium ions, simplifies the process and Enhanced electrode conductivity.
Patent Information
- Application Number
- PCT/CN2023/084367
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Existing capacitive deionization lithium extraction methods and existing patents have problems with impurity cation adsorption, resulting in insufficient lithium ion extraction efficiency.
Mesoporous activated carbon materials are used as the negative electrode to absorb impurity cations in salt solution, and combined with chemical deintercalation lithium ion screens to achieve the separation and enrichment of lithium ions. By adjusting the pore size and the composition of the adsorption layer, the impact of the adsorption of impurity cations on lithium ions is reduced. Influence.
The extraction efficiency and purity of lithium ions are improved, the amount of impurity cations embedded in the crystal lattice is reduced, the process is simplified and the electrode conductivity is enhanced.
Smart Images

Figure CN2023084367_03102024_PF_FP_ABST
Abstract
Description
A method and device for electrochemical extraction of low-impurity lithium ions Technical Field
[0001] The present application relates to the field of capacitive deionization technology, and in particular to a method and device for extracting low-impurity lithium ions using an electrochemical method. Background Art
[0002] Lithium-ion batteries are widely used in portable electronic devices and new energy electric vehicles. Market demand for lithium resources is rapidly growing, and there is an urgent need to develop lithium resources to provide high-quality, low-cost lithium raw materials for lithium-ion batteries. Lithium is naturally concentrated in deposits such as ores, salt lake brines, geothermal water, and seawater. Salt lake brines are particularly abundant and have relatively high lithium content. Efficient lithium extraction from salt lake brines has become a major research focus in the development and utilization of lithium resources.
[0003] In view of the characteristics of different types of brine, researchers have carried out research on a variety of lithium extraction processes. The main extraction methods at this stage include concentrated precipitation crystallization, adsorption, electrodialysis, extraction, membrane separation, electrolysis, calcination and leaching, etc. Among them, capacitive deionization (CDI) is an electrosorption desalination technology based on the electrochemical double-layer capacitance theory. The electrode material is mainly carbon material. When a certain voltage is applied to both ends of the porous electrode, the ions in the salt water will move toward the electrode with opposite charge under the action of the electric field and adsorb on the electrode surface. After the porous electrode is saturated with adsorption, the two ends of the electrode are short-circuited, and the anions and cations adsorbed on the porous electrode can be released back into the water body to achieve electrode regeneration. Existing patent CN102382984A discloses a method and device for separating magnesium and lithium from salt lake brine and enriching lithium. The method uses an electrodialysis device isolated by anion exchange membrane and an iron phosphate ion sieve to separate lithium from other ions, and obtain a lithium-rich solution at the same time.
[0004] However, the above-mentioned capacitor deionization method for extracting lithium and the technology disclosed in the existing patent CN102382984A both adsorb Mg while extracting lithium ions from the solution. 2+ or other impurity cations, the lithium extraction efficiency is not high enough. Therefore, it is urgent to find a lithium extraction method that reduces the adsorption of impurity cations and is efficient.
[0005] Summary of the Invention
[0006] The present application provides a method and apparatus for electrochemically extracting low-impurity lithium ions, which utilizes activated carbon to adsorb impurity cations, thereby reducing the probability of impurity cations entering a chemical deintercalation lithium ion sieve and improving the efficiency and purity of the chemical deintercalation lithium ion sieve in selectively extracting lithium.
[0007] In order to solve the above technical problems, one of the purposes of this application is to provide a device for extracting low-impurity lithium ions by electrochemical method, comprising a positive electrode current collector and a negative electrode current collector respectively connected to a power source;
[0008] The positive electrode current collector is an activated carbon electrode material;
[0009] The working surface of the negative electrode current collector is coated with a cation adsorption coating, which contains a mesoporous activated carbon material and a chemical deintercalation lithium ion sieve.
[0010] The inventors of this application have found in their research that during the operation of the chemical deintercalation lithium ion sieve, in addition to the adsorption of Li + In addition, it also accumulates Ca 2+ Mg 2+ , K + 、Na + These impurity cations gather on the surface of the chemical deintercalation lithium ion sieve, which will prevent the target cation Li + Close to chemical deintercalation lithium ion sieve, on the other hand, these impurity cations may enter the lattice structure of chemical deintercalation lithium ion sieve, making the product contain impurities; In capacitive deionization technology, mesoporous activated carbon electrode as cathode is more likely to adsorb high-valent cations and cations with small hydration radius, which is more sensitive to Ca 2+ Mg 2+ , K + 、Na + The adsorption capacity is greater than that of Li + The adsorption capacity of the lithium ion sieve is improved by using mesoporous activated carbon as the negative electrode to adsorb impurity cations in the salt solution and chemical deintercalation of lithium ions to adsorb Li + ions, realizing Li + Separation from other impurity cations, thereby improving lithium extraction efficiency and purity.
[0011] Furthermore, there is a gap between the working surfaces of the positive electrode current collector and the negative electrode current collector. The gap can be used for the flow of lithium ion solution and can connect the working surfaces of the positive electrode current collector and the negative electrode current collector.
[0012] Furthermore, the pore occupancy rate of the mesoporous activated carbon material with a pore diameter of 0.5 to 10 nm is 40% to 80%.
[0013] By adopting the above scheme, since the hydration radius of high-valent ions is smaller than that of low-valent ions, it is necessary to ensure that the pores of the activated carbon material are larger than the hydration radius of the high-valent ions, so that high- and low-valent ions can easily enter the activated carbon material. When the valence of the two ions is the same, the activated carbon material is more inclined to adsorb ions with a smaller hydration radius, such as sodium and potassium, which have a smaller hydration radius than lithium. The inventors of the present application selected a pore occupancy within this pore size range to meet the better adsorption effect on impurity cations while reducing the adsorption effect on lithium ions. A lower pore occupancy will lead to a decrease in the adsorption effect of mesoporous activated carbon on impurity anions and cations, affecting the lithium extraction efficiency and purity, while a higher pore occupancy will lead to excessively high preparation costs.
[0014] Furthermore, the raw materials for preparing the cationic adsorption coating include a mesoporous activated carbon material slurry and a chemical deintercalation lithium ion sieve slurry;
[0015] The mesoporous activated carbon material slurry contains mesoporous activated carbon material, a first binder, a first dispersant and a first conductive agent, and the chemical deintercalation lithium ion sieve slurry contains a chemical deintercalation lithium ion sieve, a second binder, a second dispersant and a second conductive agent.
[0016] Furthermore, the chemical deintercalation lithium ion sieve slurry and the mesoporous activated carbon material slurry are alternately coated in a width ratio of 1: (1 to 5) along the parallel direction of the working surface of the negative electrode current collector to form a cation adsorption coating; using this method, the impurity cations and lithium ions can be better separated, and the width ratio of the two can be controlled to avoid the adsorption area of the mesoporous activated carbon material being too large to affect the adsorption capacity of the chemical deintercalation lithium ion sieve for lithium, or the adsorption area being too small to affect the purity of the lithium extracted by the chemical deintercalation lithium ion sieve; alternatively, the chemical deintercalation lithium ion sieve slurry and the mesoporous activated carbon material slurry are mixed and coated on the working surface of the negative electrode current collector in a mass ratio of 1: (1 to 70) to form a cation adsorption coating. Using this method, the preparation method is relatively simple, and the mixed amount of the two can avoid the adsorption amount of the mesoporous activated carbon material being too large to affect the adsorption capacity of the chemical deintercalation lithium ion sieve for lithium, or the adsorption amount being too small to affect the purity of the lithium extracted by the chemical deintercalation lithium ion sieve, but the mixed coating makes the distance between the impurity cations and the lithium ions closer, resulting in limited improvement in separation quality.
[0017] Furthermore, the chemical deintercalation lithium ion sieve slurry and the mesoporous activated carbon material slurry are mixed in a mass ratio of 1: (10-15) and coated on the working surface of the negative electrode current collector to form a cation adsorption coating.
[0018] Furthermore, when the chemical deintercalation lithium ion sieve slurry and the mesoporous activated carbon material slurry are alternately coated in a width ratio of 1: (1 to 5) along a direction parallel to the working surface of the negative electrode current collector to form a cationic adsorption coating, the width ratio is in centimeters.
[0019] Furthermore, after the chemical deintercalation lithium ion sieve slurry and the mesoporous activated carbon material slurry are coated on the working surface of the negative electrode current collector, they are vacuum dried at a temperature of 100-140° C. for 550-700 minutes to form a cation adsorption coating.
[0020] Furthermore, at least one of the following is satisfied:
[0021] (a) The raw materials for preparing the mesoporous activated carbon slurry are in a mass ratio of: mesoporous activated carbon material: first conductive agent: first binder = (5-10):1:1;
[0022] (b) The raw materials for preparing the chemical deintercalation lithium ion sieve slurry are in a mass ratio of: chemical deintercalation lithium ion sieve: second conductive agent: second binder = (12-17): 1:1;
[0023] (c) the raw materials for preparing the mesoporous activated carbon slurry further include a first dispersant;
[0024] (d) The raw materials for preparing the chemical deintercalation lithium ion sieve slurry further include a second dispersant.
[0025] Furthermore, the first conductive aid and the second conductive aid are each independently selected from at least one of conductive carbon black, conductive graphite, carbon nanotubes and graphene.
[0026] Furthermore, the first dispersant and the second dispersant are each independently selected from at least one of N-methylpyrrolidone, ethanol, tetrachloroethane, toluene, xylene, anisole, dimethylformamide, dimethylacetamide, dibutyl phthalate and dimethyl sulfoxide.
[0027] Furthermore, the first binder and the second binder are each independently selected from at least one of polyvinylidene fluoride, polytetrafluoroethylene and polyimide.
[0028] Furthermore, the chemical deintercalation lithium ion screening is at least one of iron phosphate ion sieve, lithium manganate ion sieve, and lithium titanate ion sieve.
[0029] Furthermore, the amount of slurry applied to the negative electrode current collector working surface is 100 to 300 g / cm 2 .
[0030] Furthermore, the mesoporous activated carbon material is prepared by the following method: after mixing activated carbon and alkali metal, heating to 250-550°C under the protection of inert gas, keeping the temperature for 2-5 hours, continuing to heat to 750-950°C, and introducing activation gas water vapor and carbon dioxide, keeping the temperature for 1-2 hours to obtain activated activated carbon; impregnating the activated activated carbon with hydrochloric acid, introducing water vapor to make it boil, filtering while hot, washing to neutrality, and drying to obtain the mesoporous activated carbon material.
[0031] Furthermore, the mass ratio of the activated carbon to the alkali metal is 1:(1-2).
[0032] Furthermore, the alkali metal is sodium hydroxide and / or potassium hydroxide.
[0033] Furthermore, in the mesoporous activated carbon material preparation step, the activated activated carbon is impregnated with 5-10 wt% hydrochloric acid, 0.3-0.6 MPa steam is introduced to boil it, filtered while hot, washed to neutrality, and dried to obtain the mesoporous activated carbon material.
[0034] Furthermore, the volume ratio of water vapor to carbon dioxide in the activation gas is (1-4):2.
[0035] Furthermore, the chemical deintercalation lithium ion sieve is prepared by the following method: lithium iron phosphate is placed in a conductive solution, the positive divalent iron is oxidized to positive trivalent iron by adjusting the potential and the lithium ions enter the conductive solution, and the solid phase is filtered, washed and dried to obtain the iron phosphate ion sieve.
[0036] Furthermore, in the preparation step of the chemical deintercalation lithium ion sieve, the potential is adjusted to 1V to 1.2V.
[0037] Furthermore, in the step of preparing the chemical deintercalation lithium ion sieve, the conductive solution is a 25-30 g / L sodium chloride solution.
[0038] In order to solve the above technical problems, the second object of this application is to provide a method for electrochemically extracting low-impurity lithium ions, comprising the following steps:
[0039] A lithium ion-containing solution is circulated through the gap between the working surface of the positive electrode current collector and the working surface of the negative electrode current collector of the device, and a voltage is applied for the first time to cause lithium ions to be intercalated into the chemically deintercalated lithium ion sieve. After power is cut off, the cations adsorbed by the mesoporous activated carbon material are allowed to re-enter the lithium ion-containing solution to obtain a lithium ion intercalation sieve electrode;
[0040] The lithium ion sieve electrode is placed in an electrolyte solution, and voltage is applied for a second time to deintercalate the lithium ions in the lithium ion sieve electrode to obtain a solution enriched with lithium ions.
[0041] Furthermore, when the voltage is applied for the first time, the flow rate of the lithium ion solution between the two parallel electrode working surfaces of the device is 10 to 40 mL / min, and the cycle is repeated 3 to 5 times.
[0042] Furthermore, after power is turned off, the circulating flow is carried out for 2 to 5 minutes so that the cations adsorbed by the mesoporous activated carbon material re-enter the lithium ion-containing solution.
[0043] Furthermore, the lithium ion-containing solution is a chloride salt solution, which can be one of salt lake brine or its evaporated concentrate, seawater or its evaporated concentrate, and industrial waste brine containing LiCl.
[0044] Furthermore, the concentration of lithium ions in the lithium ion-containing solution is below 500 mg / L, and the concentration of impurity cations is above 1000 mg / L.
[0045] Furthermore, the first applied voltage is 0.5V to 2.1V; the second applied voltage is 0.5V to 1.5V.
[0046] Furthermore, the electrolyte solution is a 25-30 g / L sodium chloride solution.
[0047] Compared with the existing technology, this application has the following beneficial effects:
[0048] 1. This application uses mesoporous activated carbon material as the negative electrode to adsorb impurity cations in the salt solution. The cations in the brine are simultaneously adsorbed by the chemical deintercalation lithium ion sieve and the mesoporous activated carbon material. Due to the selectivity of the mesoporous activated carbon material, the impurity cations are enriched on the surface of the mesoporous activated carbon material and will not accumulate on the surface of the chemical deintercalation lithium ion sieve. At the same time, Li + Embedded in the lattice of the chemically deintercalated lithium ion sieve, preventing impurity cations from hindering the Li + Close to the chemical deintercalation lithium ion sieve, the lithium extraction efficiency of the chemical deintercalation lithium ion sieve can be improved, the content of impurity cations embedded in the lattice of the chemical deintercalation lithium ion sieve can be reduced, and the chemical deintercalation lithium ion sieve can be improved. + The adsorption efficiency and purity of the mesoporous activated carbon material are improved by making use of the easy adsorption and desorption characteristics of the mesoporous activated carbon material. After the power is turned off, the impurity cations adsorbed by the mesoporous activated carbon material are completely desorbed, thereby converting Li + and Mg 2+ The impurity cations are separated from each other.
[0049] 2. The mesoporous activated carbon material prepared in this application is not only easy to 2+ Mg 2+ , K + 、Na + The adsorption process is simple and easy to implement. When it is coated on the surface of the current collector at the same time as the chemical deintercalation lithium ion sieve, it can also greatly enhance the electrode conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] FIG1 is a schematic diagram of a lithium extraction device for obtaining low-impurity lithium ions by electrochemical extraction in Examples 1-2 of the present application;
[0051] Figure 2: Schematic diagram of a lithium extraction device for a method of electrochemically extracting low-impurity lithium ions in Examples 3-4 of the present application. DETAILED DESCRIPTION
[0052] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0053] Example 1
[0054] A method for obtaining low-impurity lithium ions by electrochemical extraction, comprising the following steps:
[0055] (1) Preparation of ferric phosphate ion sieve slurry:
[0056] a. Place the lithium iron phosphate cathode material (FePO4 / C) in a conductive solution, which is a 25g / L sodium chloride solution. Adjust the system potential to 1.2V to make the Fe in the lithium iron phosphate cathode material 2+ Oxidized to Fe 3+ , while making the Li in the lithium iron phosphate cathode material + Entering the solution, the solid phase is filtered, washed, and dried to obtain the iron phosphate ion sieve;
[0057] b. Mix the ferric phosphate ion sieve, the conductive agent and the adhesive in a mass ratio of 15:1:1, add the mixed powder into the dispersant and grind into a slurry. The conductive agent is acetylene black, the adhesive is polyvinylidene fluoride, and the dispersant is N-methylpyrrolidone.
[0058] (2) Preparation of mesoporous activated carbon material slurry:
[0059] a. Mix the activated carbon raw material with sodium hydroxide in a mass ratio of 1:2, heat under the protection of inert gas for 4 hours at a heating temperature of 450°C to obtain pretreated activated carbon, continue heating to 900°C, introduce activation gas water vapor and carbon dioxide in a volume ratio of 1:1, and heat for 1.5 hours to obtain activated activated carbon;
[0060] b. The activated carbon was impregnated with 8 wt % hydrochloric acid solution, and steam at 0.5 MPa was introduced to make it boiled. The mixture was filtered while hot, washed three times, and then washed with deionized water until neutral. The mesoporous activated carbon material was dried to obtain a pore size of 0.5 to 10 nm with an occupancy of 60%.
[0061] c. The mesoporous activated carbon material, the conductive agent and the adhesive are mixed evenly in a mass ratio of 8:1:1, and the mixed powder is added dropwise into the dispersant and ground into a slurry. The conductive agent is acetylene black, the adhesive is polyvinylidene fluoride, and the dispersant is N-methylpyrrolidone.
[0062] (3) Preparation of an electrode coated with mesoporous activated carbon and iron phosphate ion sieve: The iron phosphate ion sieve slurry obtained in step (1) and the mesoporous activated carbon material slurry obtained in step (2) were mixed uniformly in a ratio of 1:15 and coated on the working section surface of the negative electrode current collector at a coating amount of 200 g / cm 2 After vacuum drying at 125°C for 650 minutes, a negative electrode with a mesoporous activated carbon and iron phosphate ion sieve coating was obtained. The positive electrode current collector was a conventional activated carbon electrode material. After electrically connecting the positive electrode and the negative electrode to the battery, a lithium extraction device was obtained.
[0063] (4) Separation of lithium:
[0064] a. As shown in Figures 1 and 2, 1L of salt lake brine flows through the gap between the positive electrode current collector and the negative electrode current collector working surface of the lithium extraction device. The composition and content of the salt lake brine are shown in Table 1 below. The flow rate is 25mL / min, a voltage of 1.0V is applied, and the cycle is repeated 3 times to make the Li in the brine + embedded in the iron phosphate ion sieve, while the activated carbon part preferentially adsorbs Ca 2+ Mg 2+ , K + 、Na + , reducing Ca 2+ Mg 2+ The probability of impurity cations entering the ion sieve;
[0065] b. After power failure, the impurity cations adsorbed by activated carbon re-enter the brine, while Li + It is embedded in the ion sieve lattice and is not easy to desorb. After a circulation of 5 minutes, the impurity cations are separated and a lithium-intercalated ion sieve electrode is obtained to achieve lithium separation.
[0066] (5) Lithium extraction: Take out the lithium-embedded ion sieve electrode and place it in a Ca-free 2+ Mg 2+In the electrolyte salt solution, the electrolytic salt solution is a 25g / L sodium chloride solution, and a voltage of 1V is applied to deintercalate the lithium ions embedded in the ion sieve coating to obtain a solution enriched with lithium ions, thereby realizing the extraction of lithium.
[0067] Table 1 - Salt lake brine composition and content
[0068] In Example 1 of the present application, the salt lake brine was circulated three times on the lithium extraction device and tested. The iron phosphate ion sieve had a high affinity for Li + The adsorption capacity is 40.3 mg / g, accounting for 98% of the total adsorption capacity. 2+ The adsorption capacity of Mg is 0.12 mg / g. 2+ The adsorption capacity of activated carbon is 0.15 mg / g, the adsorption capacity of K+ is 0.25 mg / g, and the adsorption capacity of Na+ is 0.32 mg / g. Since the mesoporous activated carbon electrode as a cathode is more likely to adsorb high-valent cations and cations with small hydration radius, such as Ca 2+ Mg 2+ , K + 、Na + Adsorption capacity>Li + Therefore, the mesoporous activated carbon material at the cathode can be used to adsorb Ca in salt lake brine. 2+ Mg 2+ , K + 、Na + Impurity cations can effectively reduce the accumulation of these impurity cations on the surface of the iron phosphate ion sieve, on the one hand, reducing the impurity cations from blocking the target cations Li with the same electrical properties. + On the other hand, it reduces the chance of these impurity cations entering the lattice structure of the iron phosphate ion sieve, thereby improving the purity of the extracted lithium. At the same time, since the impurity cations adsorbed by the mesoporous activated carbon material are easy to detach after the power is turned off, the Li + It is difficult to detach from the lattice of the iron phosphate ion sieve, thus realizing Li + Separation from impurity cations.
[0069] Example 2
[0070] A method for obtaining low-impurity lithium ions by electrochemical extraction, wherein each step and the reagents and process parameters used in each step are the same as those in Example 1, except that in step (3), the iron phosphate ion sieve slurry obtained in step (1) and the mesoporous activated carbon material slurry obtained in step (2) are mixed uniformly in a ratio of 1:10 and coated on the working section surface of the negative electrode current collector in an amount of 200 g / cm 2 .
[0071] In Example 2 of the present application, the salt lake brine was circulated three times on the lithium extraction device and tested. The iron phosphate ion sieve had a high affinity for Li + The adsorption capacity is 39.8 mg / g, accounting for 97.3% of the total adsorption capacity. 2+ The adsorption capacity of Mg is 0.16 mg / g. 2+ The adsorption capacity of iodine is 0.21 mg / g, the adsorption capacity of K+ is 0.30 mg / g, and the adsorption capacity of Na+ is 0.42 mg / g.
[0072] Example 3
[0073] A method for obtaining low-impurity lithium ions by electrochemical extraction, wherein each step and the reagents and process parameters used in each step are the same as those in Example 1, except that in step (3), the iron phosphate ion sieve slurry obtained in step (1) and the mesoporous activated carbon material slurry obtained in step (2) are mixed uniformly in a ratio of 1:20 and coated on the working section surface of the negative electrode current collector in an amount of 200 g / cm 2 .
[0074] In Example 3 of the present application, the salt lake brine was circulated three times on the lithium extraction device and tested. The iron phosphate ion sieve had a high affinity for Li + The adsorption capacity is 36.6 mg / g, accounting for 98.4% of the total adsorption capacity. 2+ The adsorption capacity of Mg is 0.10 mg / g. 2+ The adsorption capacity of Mg2+ is 0.11 mg / g, the adsorption capacity of K+ is 0.19 mg / g, and the adsorption capacity of Na+ is 0.21 mg / g.
[0075] Example 4
[0076] A method for obtaining low-impurity lithium ions by electrochemical extraction, wherein each step and the reagents and process parameters used in each step are the same as those in Example 1, except that in step (3), the iron phosphate ion sieve slurry obtained in step (1) and the mesoporous activated carbon material slurry obtained in step (2) are mixed uniformly in a ratio of 1:4 and coated on the working section surface of the negative electrode current collector in an amount of 200 g / cm 2 .
[0077] In Example 4 of the present application, the salt lake brine was circulated three times on the lithium extraction device and tested. The iron phosphate ion sieve had a high affinity for Li + The adsorption capacity is 40.5 mg / g, accounting for 96.8% of the total adsorption capacity. 2+ The adsorption capacity of Mg is 0.28 mg / g. 2+ The adsorption capacity of iodine is 0.31 mg / g, the adsorption capacity of K+ is 0.34 mg / g, and the adsorption capacity of Na+ is 0.42 mg / g.
[0078] Example 5
[0079] A method for electrochemically extracting low-impurity lithium ions, wherein each step and the reagents and process parameters used in each step are the same as those in Example 1, except that in step (3), the iron phosphate ion sieve slurry obtained in step (1) and the mesoporous activated carbon material slurry obtained in step (2) are alternately and evenly coated in a width ratio of 1 cm:4 cm along the parallel direction of the negative electrode current collector working section, and the coating amount is 200 g / cm 2 .
[0080] In Example 5 of the present application, the salt lake brine was circulated three times on the lithium extraction device and tested. The iron phosphate ion sieve had a high affinity for Li + The adsorption capacity is 41.1 mg / g, accounting for 98.6% of the total adsorption capacity. 2+ The adsorption capacity of Mg is 0.13 mg / g. 2+ The adsorption capacity of iodine is 0.15 mg / g, the adsorption capacity of K+ is 0.13 mg / g, and the adsorption capacity of Na+ is 0.18 mg / g.
[0081] Example 6
[0082] A method for obtaining low-impurity lithium ions by electrochemical extraction, wherein each step and the reagents and process parameters used in each step are the same as those in Example 5, except that in step (3), the iron phosphate ion sieve slurry obtained in step (1) and the mesoporous activated carbon material slurry obtained in step (2) are alternately and evenly coated in a width ratio of 1 cm:7 cm along the parallel direction of the negative electrode current collector working section, and the coating amount is 200 g / cm 2 .
[0083] In Example 6 of the present application, after the salt lake brine circulates three times on the lithium extraction device, the iron phosphate ion sieve has a great influence on the Li + The adsorption capacity is 36.5 mg / g, accounting for 98.9% of the total adsorption capacity. 2+ The adsorption capacity of Mg is 0.10 mg / g. 2+ The adsorption capacity of iodine is 0.08 mg / g, the adsorption capacity of K+ is 0.10 mg / g, and the adsorption capacity of Na+ is 0.11 mg / g.
[0084] Example 7
[0085] A method for obtaining low-impurity lithium ions by electrochemical extraction, wherein each step and the reagents and process parameters used in each step are the same as those in Example 6, except that in step (3), the iron phosphate ion sieve slurry obtained in step (1) and the mesoporous activated carbon material slurry obtained in step (2) are alternately and evenly coated in a width ratio of 1:2 along the parallel direction of the negative electrode current collector working section, and the coating amount is 200g / cm 2 .
[0086] In Example 7 of this application, after the salt lake brine circulates three times on the lithium extraction device, the iron phosphate ion sieve is + The adsorption capacity is 41.7 mg / g, accounting for 97.6% of the total adsorption capacity. 2+ The adsorption capacity of Mg is 0.22 mg / g. 2+ The adsorption capacity of iodine is 0.31 mg / g, the adsorption capacity of K+ is 0.23 mg / g, and the adsorption capacity of Na+ is 0.28 mg / g.
[0087] Example 8
[0088] A method for electrochemically extracting low-impurity lithium ions, wherein each step and the reagents and process parameters used in each step are the same as those in Example 7, except that in step (3), the iron phosphate ion sieve slurry obtained in step (1) and the mesoporous activated carbon material slurry obtained in step (2) are alternately and evenly coated in a width ratio of 2:1 along the parallel direction of the negative electrode current collector working section, and the coating amount is 200g / cm 2 .
[0089] In Example 8 of the present application, the salt lake brine circulates three times on the lithium extraction device, and the iron phosphate ion sieve is used for Li + The adsorption capacity is 32.6 mg / g, accounting for 88% of the total adsorption capacity. 2+ The adsorption capacity of Mg is 0.68 mg / g. 2+ The adsorption capacity of 0.71 mg / g, the adsorption capacity of K+ is 1.47 mg / g, and the adsorption capacity of Na+ is 1.58 mg / g.
[0090] Comparative Example 1
[0091] A method for electrochemically extracting low-impurity lithium ions, wherein each step, the reagents used in each step, and the process parameters are the same as those in Example 1, except that, in step (3), the iron phosphate ion sieve slurry obtained in step (1) is evenly coated on the surface of the working section of the negative electrode current collector.
[0092] In the comparative example 1 of this application, the salt lake brine circulates 3 times in the lithium extraction device, and the iron phosphate ion sieve is used for Li + The adsorption capacity of Ca2+ The adsorption capacity of Mg is 0.75 mg / g. 2+ The adsorption capacity of the lithium ion extraction device is 0.81 mg / g, the adsorption capacity of K+ is 1.64 mg / g, and the adsorption capacity of Na+ is 1.72 mg / g. Compared with the embodiment, the lithium extraction device of comparative example 1 is not coated with mesoporous activated carbon material at the cathode, and cannot adsorb the impurity cations in the salt lake brine to reduce the content entering the lattice structure of the iron phosphate ion sieve, resulting in the adsorption of Li + The adsorption capacity of the ions was significantly reduced, and at the same time, a large amount of impurity cations such as Mg 2+ and Ca 2+ .
[0093] Comparative Example 2
[0094] A method for electrochemically extracting low-impurity lithium ions, wherein each step, the reagents used in each step, and the process parameters are the same as those in Example 1, except that, in step (2) c, an activated carbon material that has not been treated to form mesoporous material, a conductive agent, and a binder are uniformly mixed in a mass ratio of 8:1:1, and the mixed powder is added dropwise to a dispersant and ground into a slurry.
[0095] In the comparative example 2 of this application, the salt lake brine circulates 3 times on the lithium extraction device, and the iron phosphate ion sieve is + The adsorption capacity of Ca 2+ The adsorption capacity of Mg is 0.63 mg / g. 2+ The adsorption capacity is 0.62 mg / g. It can be seen that the use of mesoporous activated carbon materials helps to improve the adsorption of impurity cations such as Ca in salt lake brine. 2+ Mg 2+ , K + 、Na + The adsorption and desorption of the iron phosphate ion sieve can reduce the content of impurity cations embedded in the lithium ion sieve lattice and hinder the chance of Li+ approaching the lithium ion sieve, thereby increasing the iron phosphate ion sieve's + Extraction purity and content.
[0096] The specific embodiments described above further illustrate the objectives, technical solutions, and beneficial effects of this application. It should be understood that the above descriptions are merely specific embodiments of this application and are not intended to limit the scope of protection of this application. In particular, it should be noted that any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of this application by those skilled in the art should be included within the scope of protection of this application.
Claims
1. A device for electrochemically extracting low-impurity lithium ions, characterized in that: including a positive electrode current collector and a negative electrode current collector respectively connected to a power source; The positive electrode current collector is an activated carbon electrode material; The working surface of the negative electrode current collector is coated with a cation adsorption coating, which contains a mesoporous activated carbon material and a chemically deintercalated lithium ion sieve.
2. The device for electrochemically extracting low-impurity lithium ions according to claim 1, characterized in that: The pore occupancy rate of the mesoporous activated carbon material with a pore diameter of 0.5 to 10 nm is 40% to 80%.
3. The device for electrochemically extracting low-impurity lithium ions according to claim 1, characterized in that: The raw materials for preparing the cation adsorption coating include a mesoporous activated carbon material slurry and a chemical deintercalation lithium ion sieve slurry; The mesoporous activated carbon material slurry comprises a mesoporous activated carbon material, a first binder, a first dispersant and a first conductive agent; the chemical deintercalation lithium ion sieve slurry comprises a chemical deintercalation lithium ion sieve, a second binder, a second dispersant and a second conductive agent.
4. The device for electrochemically extracting low-impurity lithium ions as claimed in claim 3, characterized in that: The chemically deintercalated lithium ion sieve slurry and the mesoporous activated carbon material slurry are alternately coated in a direction parallel to the working surface of the negative electrode current collector at a width ratio of 1: (1-5) to form a cation adsorption coating; Alternatively, the chemically deintercalated lithium ion sieve slurry and the mesoporous activated carbon material slurry are mixed in a mass ratio of 1: (1-70) and coated on the working surface of the negative electrode current collector to form a cation adsorption coating.
5. A device for electrochemically extracting low-impurity lithium ions as claimed in claim 4, characterized in that: After the chemically deintercalated lithium ion sieve slurry and the mesoporous activated carbon material slurry are coated on the negative electrode current collector working surface, they are vacuum dried at a temperature of 100 to 140° C. for 550 to 700 minutes to form a cation adsorption coating.
6. A device for electrochemically extracting low-impurity lithium ions as claimed in claim 3 or 4, characterized in that: Satisfy at least one of the following: (a) In the raw materials for preparing the mesoporous activated carbon slurry, the mass ratio of each raw material is: mesoporous activated carbon material: first conductive agent: first binder = (5-10): 1:1; (b) In the raw materials for preparing the chemical deintercalation lithium ion sieve slurry, the mass ratio of each raw material is: chemical deintercalation lithium ion sieve: second conductive agent: second binder = (12-17): 1:1; (c) the raw materials for preparing the mesoporous activated carbon slurry further include a first dispersant; (d) The raw materials for preparing the chemical deintercalation lithium ion sieve slurry further include a second dispersant.
7. The device for electrochemically extracting low-impurity lithium ions as claimed in claim 6, characterized in that: The first conductive agent and the second conductive agent are each independently selected from at least one of conductive carbon black, conductive graphite, carbon nanotubes and graphene; The first binder and the second binder are each independently selected from at least one of polyvinylidene fluoride, polytetrafluoroethylene and polyimide; The first dispersant and the second dispersant are each independently selected from at least one of N-methylpyrrolidone, ethanol, tetrachloroethane, toluene, xylene, anisole, dimethylformamide, dimethylacetamide, dibutyl phthalate and dimethyl sulfoxide; The chemical deintercalation of lithium ions is screened by at least one of an iron phosphate ion screen, a lithium manganate ion screen, and a lithium titanate ion screen.
8. The device for electrochemically extracting low-impurity lithium ions as claimed in claim 3, characterized in that: The amount of slurry applied on the working surface of the negative electrode current collector is 100 to 300 g / cm 2 .
9. The device for electrochemically extracting low-impurity lithium ions as claimed in claim 1, characterized in that: The mesoporous activated carbon material is prepared by the following method: after mixing activated carbon and alkali metal, heating to 250-550°C under the protection of inert gas, keeping the temperature for 2-5 hours, continuing to heat to 750-950°C, and introducing activation gas water vapor and carbon dioxide, keeping the temperature for 1-2 hours, to obtain activated activated carbon; impregnating the activated activated carbon with hydrochloric acid, introducing water vapor to make it boil, filtering while hot, washing to neutrality, and drying to obtain the mesoporous activated carbon material.
10. The device for electrochemically extracting low-impurity lithium ions as claimed in claim 9, characterized in that: The mass ratio of the activated carbon to the alkali metal is 1:(1-2), and the alkali metal is sodium hydroxide and / or potassium hydroxide.
11. The device for electrochemically extracting low-impurity lithium ions according to claim 1, characterized in that: The chemical deintercalation lithium ion sieve is prepared by the following method: lithium iron phosphate is placed in a conductive solution, the positive divalent iron is oxidized to positive trivalent iron by adjusting the potential and the lithium ions enter the conductive solution, and the solid phase is filtered, washed and dried to obtain the iron phosphate ion sieve.
12. The device for electrochemically extracting low-impurity lithium ions according to claim 11, characterized in that: In the preparation step of the chemical deintercalation lithium ion sieve, the potential is adjusted to 1V to 1.2V, and the conductive solution is a 25 to 30 g / L sodium chloride solution.
13. A method for obtaining low-impurity lithium ions by electrochemical extraction using the device according to any one of claims 1 to 12, characterized in that: The following steps are involved: The lithium ion-containing solution is circulated through the gap between the working surface of the positive electrode current collector and the working surface of the negative electrode current collector of the device, and a voltage is applied for the first time to embed the lithium ions into the chemically deintercalated lithium ion sieve. After the power is turned off, the cations adsorbed by the mesoporous activated carbon material are circulated to re-enter the lithium ion-containing solution to obtain a lithium ion intercalation sieve electrode; The lithium ion embedded sieve electrode is placed in an electrolyte solution, and voltage is applied for a second time to de-embed the lithium ions in the lithium ion embedded sieve electrode to obtain a solution enriched with lithium ions.
14. The method for obtaining low-impurity lithium ions by electrochemical extraction as claimed in claim 13, characterized in that: The first applied voltage is 0.5V to 2.1V; the second applied voltage is 0.5V to 1.5V.
15. The method for obtaining low-impurity lithium ions by electrochemical extraction as claimed in claim 14, characterized in that: When the voltage is applied for the first time, the flow rate of the lithium ion solution between the gap between the two parallel electrode working surfaces of the device is 10 to 40 mL / min.
Citation Information
Patent Citations
Mesoporous activated carbon and preparation process thereof
CN101439857A
Green production method for separating and extracting lithium from salt lake brine
CN111592018A
Method for preparing lithium carbonate by electrochemically extracting lithium from chloride type lithium-containing saline water
CN112645362A
Method for inhibiting coexisting cation interference by electrochemical lithium extraction of brine
CN112795940A
Membrane electrode material, its preparation method and application in lithium extraction by adsorption-electrochemical coupling technology
US20210388465A1
Cited By
Cathode for electrodialysis device, preparation method of cathode, electrodialysis device and application of electrodialysis device
CN119409293A
Method for recycling low-concentration lithium resource by using lithium nickel manganese oxide material as capacitive deionization positive electrode
CN121872454A
Flowing electrode slurry, preparation method thereof and ammonium ion enrichment and recovery method
CN122301336A
A flow electrode slurry, a preparation method thereof and an ammonium ion enrichment recovery method
CN122301336B