Secondary battery and electrical device
By setting up multi-region positive active material layers in the positive electrode sheet of lithium-ion batteries and regulating their quality and adhesion, combined with appropriate current collectors and conductive agents, the problem of structural phase change in lithium-ion batteries at high temperatures is solved. Improved high-temperature storage and rate performance of the battery.
Patent Information
- Application Number
- PCT/CN2023/085644
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium-ion batteries can easily cause structural phase changes of the positive active material in high-temperature environments, causing gas production and battery expansion, affecting storage performance.
By arranging different areas of positive active material layers in the positive electrode sheet, the mass and bonding force per unit area are controlled, the structural stability and conductivity of the positive electrode sheet are improved, and appropriate positive electrode current collector materials and conductive agents are selected to enhance the electrode assembly. high temperature performance.
It significantly improves the high-temperature storage performance and rate performance of the secondary battery, reduces the thickness expansion rate of the battery under high-temperature conditions, and extends the cycle life of the battery.
Smart Images

Figure CN2023085644_03102024_PF_FP_ABST
Abstract
Description
A secondary battery and an electrical device Technical Field
[0001] This application relates to the field of electrochemistry, and specifically relates to a secondary battery and an electrical device. Background Art
[0002] Secondary batteries, such as lithium-ion batteries, have advantages such as high energy density, low self-discharge, no memory effect, and long cycle life, and are therefore widely used in fields such as portable electronic devices, electric vehicles, drones, and large energy storage devices.
[0003] During the use of lithium-ion batteries, if they are in a high-temperature environment for a long time, it is easy to cause irreversible structural phase changes in the positive active materials therein, and then gas generation problems occur, resulting in the thickness expansion of lithium-ion batteries and affecting the high-temperature storage performance of lithium-ion batteries.
[0004] Summary of the Invention
[0005] The purpose of this application is to provide a secondary battery and an electrical device to improve the high-temperature storage performance of the secondary battery.
[0006] It should be noted that in the application content, lithium-ion batteries are used as examples of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries. The specific technical solutions are as follows:
[0007] In the first aspect of this application, a secondary battery is provided, which includes an electrode assembly. The electrode assembly includes a positive electrode tab. The positive electrode tab includes a positive electrode current collector and a positive electrode active material layer. The positive electrode active material layer includes positive electrode active materials. The positive electrode current collector includes a first region, a second region, and a third region. Positive electrode active material layers are provided on both sides of the first region, a positive electrode active material layer is provided on one side of the second region, and positive electrode active material layers are not provided on both sides of the third region. In this application, the mass per unit area of the first region is defined as Ma g / m 2 , the mass per unit area of the second region is defined as Mb g / m 2 , and the mass per unit area of the third region is defined as Mc g / m 2 , satisfying: Ma ≤ Mb < Mc, and Ma / Mc ≤ 99%, preferably, Ma / Mc ≤ 98.5%.
[0008] Beneficial effects of the embodiments of this application: By regulating the mass per unit area of the first region, the second region, and the third region of the positive electrode current collector within the above range, this application improves the degree of fragmentation of the positive electrode active material particles, improves the structural stability of the positive electrode tab, and further improves the high-temperature storage performance of the secondary battery.
[0009] In some embodiments of the present application, the thickness of the positive electrode active material layer located in the first region is Hc μm, and the mass per unit area of the positive electrode active material layer located in the first region is Md g / m 2 , satisfying: Ma / Mc ≤ -0.0892 × Md / Hc + 1.3652. Without being limited to any theory, regulating Ma, Mc, Md, and Hc to satisfy the above relationship can facilitate the production of a positive electrode with excellent structural stability, thereby improving the high-temperature storage performance of the secondary battery.
[0010] In some embodiments of the present application, the porosity of the positive electrode sheet is P, and the mass per unit area of the positive electrode active material layer located in the first region is Md g / m 2 , satisfying: P ≥ [Md / Hc × (-0.2429) + 1.2007] × 100%. Without being limited to any theory, by regulating the relationship between P, Md, and Hc to meet the above relationship, the rate performance of lithium-ion batteries can be improved, which is conducive to obtaining lithium-ion batteries with excellent rate performance and high-temperature storage performance.
[0011] In some embodiments of the present application, the electrode assembly further comprises a negative electrode sheet, which includes a negative electrode active material layer. The thickness of the negative electrode active material layer on a single surface is Ha μm, satisfying the following relationship: 0.2 ≤ Hc / Ha ≤ 4. Preferably, 0.5 ≤ Hc / Ha ≤ 1.5. By regulating Ha and Hc to satisfy this relationship, the lithium-ion battery can achieve good dynamic performance.
[0012] In some embodiments of the present application, the bonding force between the wet film of the positive electrode active material layer and the positive electrode current collector is FN / m, where F ≥ 1, preferably, F ≥ 2. By regulating the bonding force between the wet film of the positive electrode active material layer and the positive electrode current collector within the above range, the positive electrode active material layer and the positive electrode current collector can maintain appropriate bonding strength under high temperature conditions, thereby improving the high temperature storage performance of the secondary battery.
[0013] In some embodiments of the present application, the positive electrode current collector comprises at least one of aluminum foil, nickel foil, or aluminum-nickel alloy foil. Selecting such materials as the positive electrode current collector can provide the positive electrode current collector with good conductivity, meeting the performance requirements for conducting electrons, while also providing a certain degree of strength and weldability, ensuring sufficient strength during processing and facilitating welding of the electrode tabs thereto.
[0014] In some embodiments of the present application, the positive electrode active material includes at least one of lithium cobalt oxide, lithium manganate, lithium nickelate, lithium nickel cobalt manganate, lithium nickel cobalt aluminate, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, or lithium-rich manganese-based material. Selecting the above materials as the positive electrode active material can take into account the energy density and cycle performance of the secondary battery while improving the high-temperature storage performance of the secondary battery.
[0015] In some embodiments of the present application, the positive electrode active material layer further includes a binder, and the binder includes at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate salt, polyvinylpyrrolidone, polyamide, polyethylene ether, polymethyl methacrylate, polytetrafluoroethylene, polyhexafluoropropylene, polypropylene, polyethylene, polyetherimide, or a copolymer of an olefin hydrocarbon derivative. Selecting the above materials as the binder is beneficial to improving the bonding strength between the positive electrode active material layer and the positive electrode current collector, thereby improving the high-temperature storage performance of the secondary battery.
[0016] In some embodiments of the present application, the positive electrode active material layer further includes a conductive agent, and the conductive agent includes at least one of conductive carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes, nanofiber carbon, or graphene. By selecting the above materials as the conductive agent in the positive electrode active material layer, the conductivity between the positive electrode active material layer and the positive electrode current collector can be improved, which is beneficial to the improvement of the rate performance of the secondary battery.
[0017] The second aspect of the present application provides an electrical device, which includes the secondary battery described in any of the foregoing embodiments. Accordingly, the electrical device has good high-temperature storage performance.
[0018] The present application provides a secondary battery and an electrical device. The secondary battery includes an electrode assembly, and the electrode assembly includes a positive electrode tab, and the positive electrode tab includes a positive electrode current collector and a positive electrode active material layer. Among them, the unit area mass of the first region of the positive electrode current collector, that is, the region coated with the positive electrode active material on both sides, is Ma g / m 2 , the second region, that is, the region coated with the positive electrode active material on one side, is Mb g / m 2 , and the unit area mass of the third region, that is, the region not coated with the positive electrode active material, is Mc g / m 2 , satisfying Ma≤Mb<Mc, and Ma / Mc≤99%. By regulating the unit area mass of the first region, the second region, and the third region of the positive electrode current collector within the above range, the present application improves the degree of fragmentation of the positive electrode active material particles, improves the structural stability of the positive electrode tab, and improves the high-temperature storage performance of the secondary battery. Of course, implementing any product or method of the present application does not necessarily require all the advantages described above to be achieved simultaneously. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present application and the technical solutions of the prior art, the following briefly introduces the drawings required for use in the embodiments and the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.
[0020] FIG1 is a schematic structural diagram of an electrode assembly in some embodiments of the present application;
[0021] FIG2 is a schematic diagram of the cross-sectional structure of an electrode assembly along its thickness direction in some embodiments of the present application;
[0022] FIG3 is a top view of the positive electrode current collector along its thickness direction in some embodiments of the present application;
[0023] FIG4 is a schematic diagram of the cross-sectional structure of a positive electrode sheet along its thickness direction in some embodiments of the present application;
[0024] FIG5 is a schematic diagram showing the relationship between adhesion and travel in an adhesion test.
[0025] Reference numerals: 10 - electrode assembly, 20 - positive electrode sheet, 21 - positive electrode current collector, 22 - positive electrode active material layer, 30 - negative electrode sheet, 40 - separator, 211 - first region, 212 - second region, 213 - third region. DETAILED DESCRIPTION
[0026] To make the objectives, technical solutions, and advantages of this application more clearly understood, the present application is further described below with reference to the accompanying drawings and examples. It is apparent that the described examples are only a portion of the embodiments of this application, and not all of them. All other embodiments derived by persons of ordinary skill in the art based on the examples in this application are intended to fall within the scope of protection of this application.
[0027] It should be noted that in the specific implementation, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries. The specific technical solution is as follows:
[0028] In the first aspect of the present application, a secondary battery is provided, which includes an electrode assembly 10. As shown in FIG. 1, for the convenience of understanding, a three-dimensional rectangular coordinate system is established with the width direction of the electrode assembly 10 itself as the X direction, the length direction of the electrode assembly 10 itself as the Y direction, and the thickness direction of the electrode assembly 10 itself as the Z direction. As shown in FIG. 2, the electrode assembly 10 includes a positive electrode plate 20, a negative electrode plate 30, and a separator 40 disposed between the positive electrode plate 20 and the negative electrode plate 30. Among them, the positive electrode plate 20 includes a positive electrode current collector 21 and a positive electrode active material layer 22, and the positive electrode active material layer 22 includes positive electrode active materials. As shown in FIG. 3, the positive electrode current collector 21 includes a first region 211, a second region 212, and a third region 213. As shown in FIG. 4, along the X direction, the first region 211 is located in the middle of the positive electrode current collector, the third region 213 is located at the head and tail ends of the positive electrode current collector, and the second region 212 is located between the first region 211 and the third region 213. As shown in FIG. 4, positive electrode active material layers 22 are provided on both sides of the first region 211, a positive electrode active material layer 22 is provided on one side of the second region 212, and positive electrode active material layers 22 are not provided on both sides of the third region 213. The present application defines the mass per unit area of the first region 211 as Ma g / m 2 , the mass per unit area of the second region 212 as Mb g / m 2 , and the mass per unit area of the third region 213 as Mc g / m 2 , satisfying: Ma ≤ Mb < Mc, and Ma / Mc ≤ 99%, preferably, Ma / Mc ≤ 98.5%. The inventors have found through research that in a lithium-ion battery, such as a wound structure battery, the first region of the positive electrode current collector has a structure with positive electrode active material layers provided on both sides, the second region has a structure with a positive electrode active material layer provided on one side, and the third region is an empty foil area. The first region and the second region of the positive electrode current collector are more likely to undergo extension after being compressed compared to the third region, releasing a part of the extrusion stress suffered by the positive electrode active material particles during the cold pressing process of the electrode plate. By regulating the mass per unit area of the first region, the second region, and the third region of the positive electrode current collector within the above range, the present application improves the degree of fragmentation of the positive electrode active material particles, enhances the structural stability of the positive electrode plate, and further improves the high-temperature storage performance of the secondary battery.
[0029] In some embodiments of the present application, as shown in FIG. 4, the single-sided thickness of the positive electrode active material layer 22 located in the first region 211 is Hc μm, and the single-sided mass per unit area of the positive electrode active material layer 22 located in the first region 211 is Md g / m 2 , satisfying: Ma / Mc ≤ -0.0892 × Md / Hc + 1.3652. Without being limited to any theory, by regulating the relationship between Ma, Mc, Md, and Hc to satisfy the above relationship, it is beneficial to obtain a positive electrode plate with good structural stability and improve the high-temperature storage performance of the secondary battery.
[0030] In some embodiments of the present application, the porosity of the positive electrode sheet is P, and the mass per unit area of the positive electrode active material layer located in the first region is Md g / m 2 , satisfying: P ≥ [Md / Hc × (-0.2429) + 1.2007] × 100%. Without being limited to any theory, by regulating the relationship between P, Md, and Hc to meet the above relationship, the rate performance of lithium-ion batteries can be improved, which is conducive to obtaining lithium-ion batteries with excellent rate performance and high-temperature storage performance.
[0031] In some embodiments of the present application, the electrode assembly further comprises a negative electrode sheet, which includes a negative electrode active material layer. The thickness of the negative electrode active material layer on a single surface is Ha μm, satisfying the following relationship: 0.2 ≤ Hc / Ha ≤ 4, preferably, 0.5 ≤ Hc / Ha ≤ 1.5. By regulating Ha and Hc to satisfy the above relationship, the lithium-ion battery can achieve good dynamic performance.
[0032] In some embodiments of the present application, the bonding force between the wet film of the positive electrode active material layer and the positive electrode current collector is FN / m, F≥1, preferably, F≥2. By regulating the bonding force between the wet film of the positive electrode active material layer and the positive electrode current collector within the above range, the positive electrode active material layer and the positive electrode current collector can maintain appropriate bonding strength under high temperature conditions, thereby improving the high temperature storage performance of the secondary battery. The present application does not particularly limit the method for adjusting the bonding force between the wet film of the positive electrode active material layer and the positive electrode current collector, as long as the purpose of the invention of the present application can be achieved. For example, the bonding force between the wet film of the positive electrode active material layer and the positive electrode current collector can be adjusted by adjusting the binder content.
[0033] In some embodiments of the present application, the positive electrode current collector comprises at least one of aluminum foil, nickel foil, or aluminum-nickel alloy foil. Selecting such materials as the positive electrode current collector can provide the positive electrode current collector with good conductivity, meeting the performance requirements for conducting electrons, while also providing a certain degree of strength and weldability, ensuring sufficient strength during processing and facilitating welding of the electrode tabs thereto.
[0034] In some embodiments of the present application, the positive electrode active material includes at least one of lithium cobaltate, lithium manganate, lithium nickelate, lithium nickel cobalt manganate, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, or a lithium-rich manganese-based material. In the present application, the positive electrode active material may also contain non-metallic elements, such as fluorine, phosphorus, boron, chlorine, silicon, sulfur, and other elements, which can further improve the stability of the positive electrode active material. The selection of the above materials as the positive electrode active material can take into account the energy density and cycle performance of the secondary battery while improving the high-temperature storage performance of the secondary battery.
[0035] In some embodiments of the present application, the positive electrode active material layer further includes a binder, and the binder includes at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinyl pyrrolidone, polyamide, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, polyhexafluoropropylene, polypropylene, polyethylene, polyetherimide, or a copolymer of a propylene derivative. Selecting the above materials as the binder is beneficial for improving the bond strength between the positive electrode active material layer and the positive electrode current collector, thereby improving the high-temperature storage performance of the secondary battery.
[0036] In some embodiments of the present application, the positive electrode active material layer further includes a conductive agent, wherein the conductive agent includes at least one of conductive carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes, carbon nanofibers, or graphene. By selecting any of the above materials as the conductive agent in the positive electrode active material layer, the conductivity between the positive electrode active material layer and the positive electrode current collector can be improved, which is beneficial for improving the rate performance of the secondary battery.
[0037] The present application does not particularly limit the mass ratio of the positive electrode active material, conductive agent, and binder in the positive electrode active material layer. Those skilled in the art may select the mass ratio according to actual needs, as long as the purpose of the present application can be achieved. For example, the mass ratio of the positive electrode active material, conductive agent, and binder in the positive electrode active material layer is (97.5-97.9):(0.9-1.7):(1.0-2.0).
[0038] The present application has no particular limitation on the preparation method of the positive electrode current collector, and any preparation method known in the art may be used as long as the purpose of the present application can be achieved.
[0039] The negative electrode sheet of the present application includes a negative electrode current collector and a negative electrode active material layer arranged on at least one surface of the negative electrode current collector. The above-mentioned "negative electrode active material layer arranged on at least one surface of the negative electrode current collector" means that the negative electrode active material layer can be arranged on one surface of the negative electrode current collector along the thickness direction of itself, or can be arranged on two surfaces of the negative electrode current collector along the thickness direction of itself. It should be noted that the "surface" here can be the entire area of the negative electrode current collector, or it can be a partial area of the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved. This application has no special restrictions on the negative electrode current collector, as long as the purpose of this application can be achieved. For example, the negative electrode current collector can include copper foil, copper alloy foil, nickel foil, titanium foil, foam nickel or foam copper, etc. The negative electrode active material layer includes negative electrode active material. This application has no special restrictions on the type of negative electrode active material, as long as the purpose of this application can be achieved. For example, the negative electrode active material may include at least one of natural graphite, artificial graphite, soft carbon, hard carbon, mesophase carbon microbeads, tin-based materials, silicon-based materials, lithium titanate, transition metal nitrides or natural flake graphite. Optionally, the negative electrode active material layer further includes at least one of a conductive agent, a thickener, and a binder. The present application does not particularly limit the types of conductive agents, thickeners, and binders in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the negative electrode binder may include, but is not limited to, at least one of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene 1,1-difluoride, polyethylene, polypropylene, polyacrylic acid, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, or nylon.
[0040] Optionally, the negative electrode sheet may further include a conductive layer, which is located between the negative electrode current collector and the negative electrode material layer. The present application does not particularly limit the composition of the conductive layer, and it may be any conductive layer commonly used in the art. The conductive layer may include, but is not limited to, the aforementioned negative electrode conductive agent and the aforementioned negative electrode binder.
[0041] The secondary battery of the present application also includes a diaphragm. The present application does not particularly limit the diaphragm, and those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. For example, the material of the diaphragm may include but is not limited to polyethylene (PE), polypropylene (PP)-based polyolefin (PO), polyester, (such as polyethylene terephthalate (PET)), cellulose, polyimide (PI), polyamide, (PA), spandex or aramid at least one; the type of diaphragm may include but is not limited to woven membrane, non-woven membrane (non-woven fabric), microporous membrane, composite membrane, diaphragm paper, rolled membrane or spinning membrane at least one. For example, the diaphragm may include a substrate layer and a surface treatment layer. The substrate layer may be a non-woven fabric, a membrane or a composite membrane with a porous structure, and the material of the substrate layer may include at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer can be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. For example, the inorganic layer includes inorganic particles and a binder, and the inorganic particles are not particularly limited, and for example, can be selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The binder is not particularly limited, and for example, can be selected from at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. The polymer layer includes a polymer, and the polymer material includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride or poly(vinylidene fluoride-hexafluoropropylene).
[0042] The secondary battery of the present application also includes an electrolyte. The present application has no particular restrictions on the electrolyte. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. For example, at least one of ethylene carbonate (also known as ethylene carbonate, abbreviated as EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl propionate (EP), propyl propionate (PP), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), vinylene carbonate (VC) or fluoroethylene carbonate (FEC) is mixed in a certain mass ratio to obtain a non-aqueous organic solvent, and then a lithium salt is added to dissolve and mix evenly. The present application has no particular restrictions on the above-mentioned "mass ratio", as long as the purpose of the present application can be achieved. The present application has no restrictions on the type of lithium salt, as long as the purpose of the present application can be achieved. For example, the lithium salt may include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, lithium bis(oxalatoborate) (LiBOB), or lithium difluoroborate. The present application does not particularly limit the concentration of the lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. For example, the concentration of the lithium salt is 1.0 mol / L to 2.0 mol / L.
[0043] The secondary battery of the present application also includes a housing. The present application does not particularly limit the housing, and those skilled in the art can select it according to actual needs, as long as it can achieve the purpose of the present application. For example, the housing may include an aluminum-plastic film.
[0044] The secondary battery of the present application is not particularly limited and may include a device that generates an electrochemical reaction. For example, the secondary battery may include but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery (lithium ion battery), a sodium ion secondary battery, a lithium polymer secondary battery, and a lithium ion polymer secondary battery.
[0045] This application does not particularly limit the preparation method of the positive electrode sheet. Any preparation method known in the art can be used as long as the purpose of this application can be achieved. For example, the preparation method of the positive electrode sheet includes but is not limited to the following steps: dispersing the active material, conductive agent, and binder in N-methylpyrrolidone (NMP) solvent to form a uniform positive electrode slurry, coating the positive electrode slurry on the positive electrode current collector, drying, cold pressing, cutting, slitting, and drying again to obtain the positive electrode sheet.
[0046] The present application has no particular restrictions on the method of regulating Ma, Mb, and Mc, as long as the purpose of the invention of the present application can be achieved. For example, the adjustment of Ma, Mb, and Mc can be achieved by adjusting at least one of the cold pressing process, the surface roughness of the active material, the elongation of the current collector, or the tensile strength of the current collector. In the process of preparing the positive electrode sheet, an aluminum foil with higher extensibility is selected, or a small pressure multiple step-by-step cold pressing method is used to press the positive electrode sheet to the target thickness, thereby reducing the degree of crushing of the positive electrode active material particles and improving the structural stability of the positive electrode sheet. Exemplarily, the positive electrode sheet can be cold pressed in the following manner: in the first step, the cold pressing pressure is 20 tons, in the second step, the cold pressing pressure is 30 tons, and in the third step, the cold pressing pressure is 30 tons. The elongation of the aluminum foil of the present application along the rolling line direction is 2%-5%.
[0047] The present application does not particularly limit the method for adjusting the porosity P of the positive electrode sheet, as long as the purpose of the present invention can be achieved. For example, the porosity of the positive electrode sheet generally decreases with increasing cold pressing pressure, and its porosity can be adjusted by adjusting the cold pressing pressure of the positive electrode sheet. The present application does not particularly limit the method for adjusting the single-sided unit area mass Md of the positive electrode active material layer in the first region, as long as the purpose of the present invention can be achieved. For example, it can be adjusted through a cold pressing process.
[0048] This application does not particularly limit the preparation method of the secondary battery; any preparation method known in the art may be used, as long as the objectives of this application are achieved. For example, the preparation method of the secondary battery includes, but is not limited to, the following steps: stacking the positive electrode sheet, the separator, and the negative electrode sheet in sequence, and performing winding and folding operations as needed to obtain a wound electrode assembly; placing the electrode assembly in a packaging bag; injecting an electrolyte into the packaging bag and sealing it to obtain an electrochemical device.
[0049] A second aspect of the present application provides an electrical device comprising the secondary battery described in any of the aforementioned embodiments.
[0050] The electrical devices of the present application are not particularly limited and may be any electrical devices known in the art. For example, the electrical devices may include, but are not limited to, laptop computers, pen-type computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, automobiles, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries, and lithium-ion capacitors.
[0051] Example
[0052] Hereinafter, the embodiments of the present application will be described in more detail with reference to Examples and Comparative Examples. Various tests and evaluations were performed according to the following methods.
[0053] Test methods and equipment:
[0054] Positive electrode current collector unit area weight test:
[0055] a) Under a temperature of (25±3)°C, remove the positive electrode sheet from the secondary battery and soak it in NMP solvent until the positive electrode active material layer falls off the positive electrode current collector;
[0056] b) Samples were taken from the first region a where positive electrode active material layers were provided on both sides of the positive electrode current collector, the second region b where positive electrode active material layers were provided on one side, and the third region c where positive electrode active material layers were not provided on both sides. The area of the positive electrode current collector samples taken from the three regions was ≥ 1 cm 2 , and denoted as s a 、s b 、s c ;
[0057] c) Weigh the weight of the current collector sample in each region on an electronic balance with an accuracy of 0.1 mg. a 、m b 、m c ;
[0058] d) The unit area weight of the positive electrode current collector in regions a, b, and c is Ma=m a / s a g / m 2 、Mb=m b / s b g / m 2 、Mc=m c / s c g / m 2 .
[0059] The thickness Hc of the positive electrode active material layer on the first region and the thickness Ha of the negative electrode active material layer on the first region are tested:
[0060] a) Remove the positive and negative electrodes from the secondary battery at a temperature of (25±3)°C.
[0061] b) Wipe the electrolyte on the surface of the electrode in a) with dust-free paper, cut the electrode using plasma, and measure the thickness of the upper coating at the first target position of the electrode under a scanning electron microscope. 1-上 , the thickness of the lower layer H 1-下 , the thickness of this point is H1=(H 1-上 +H 1-下) / 2, use the same method to test the thickness of n (n≥15) points H1, H2...H n , then (H1+H2+……+H n ) / n It is recorded as the positive electrode sheet thickness Hc or the negative electrode sheet thickness Ha.
[0062] The mass per unit area of the positive electrode active material layer located in the first region is measured as Md:
[0063] a) Remove the positive electrode from the secondary battery at a temperature of (25±3)°C.
[0064] b) Take the electrode in step a) and bake it at 60°C for 60 minutes;
[0065] c) Take the middle piece in b) and cut out at least n (n≥5) pieces with an area of ≥8cm 2 The double-sided coated electrodes are numbered 1 to n, and their weights are tested in sequence on an electronic balance with an accuracy of 0.1 mg, and are recorded as M 0-1 ~M 0-n ;
[0066] d) Take the electrode piece weighed in c) and soak it in NMP until the positive electrode active material layer falls off. Take the empty current collector and bake it at 60°C for 60 minutes. The weight of each current collector is measured on an electronic balance with an accuracy of 0.1 mg, and recorded as M. 1-1 ~M 1-n ;
[0067] e) Mass per unit area of a single surface Md = [(M 0-1 -M 1-1 )+……+(M 0-n -M 1-n )] / 2n.
[0068] Porosity P of the positive electrode sheet:
[0069] a) removing the positive electrode sheet coated with a double-sided positive electrode active material layer from the secondary battery;
[0070] b) Soak the electrode obtained in a) in DMC at (25±3)°C for 30 minutes, then remove and air-dry in a fume hood;
[0071] c) The porosity of the electrode obtained in b) is measured using mercury intrusion porosimetry, and is recorded as the porosity P of the positive electrode.
[0072] Test of adhesion F:
[0073] Positive electrode sheets removed from secondary batteries were placed in a (25±3)°C environment and allowed to stand for 60 minutes in a (10±5)% humidity environment. The sheets were then formed into strips measuring 30 mm x 120 mm in width x length. A portion of the sheet was attached to a steel plate along its length from one end using double-sided tape measuring 20 mm x 100 mm in width x length. The steel plate was then secured to the corresponding position in a high-speed rail tensile test machine. The sheet not attached to the steel plate was pulled up and clamped in a chuck using a connector or directly. When the tension in the chuck was greater than 0 kgf and less than 0.02 kgf, testing with the high-speed rail tensile test machine began. The average tensile force in the plateau region was measured and recorded as the adhesion force (F) between the wet film of the positive electrode active material layer and the positive current collector. As shown in Figure 5, the ratio of the standard deviation of the adhesion force data in this plateau region to the average value was required to be no more than 10%.
[0074] Secondary battery storage 85 ℃ 24h thickness expansion rate test:
[0075] a) Place the secondary battery in a 25°C environment for 2 hours, and use a micrometer to measure the thickness of the Al-Tab (aluminum tab) at three different locations, and take the average value as H. 前 ;
[0076] b) Place the secondary battery in a) in an 85°C environment for 24 hours, and use a micrometer to measure the thickness of the Al-Tab at three different locations, and take the average value as H. 后 ;
[0077] c) Secondary battery thickness expansion rate (H) 后 -H 前 ) / H 后 ×100%.
[0078] Secondary battery 3C charging capacity retention rate:
[0079] a) Discharge the secondary battery at 25°C and 0.5C rate to 3V;
[0080] b) Fully charge the secondary battery in a) at a rate of 0.2C to the design voltage, then charge it at the design voltage with a constant voltage until the cutoff current reaches 0.05C, let it rest for 5 minutes, and then discharge it at a current of 1.0C to 3.0V. The discharge capacity is recorded as C0;
[0081] c) Fully charge the secondary battery in b) at a rate of 3C to the design voltage, then charge it at the design voltage with a constant voltage until the cutoff current reaches 0.05C, let it rest for 5 minutes, and then discharge it at a current of 1.0C to 3.0V. The discharge capacity is recorded as C1;
[0082] d) The 3C charge capacity retention rate of the secondary battery is C1 / C0×100%.
[0083] Example 1-1
[0084] <Preparation of positive electrode sheet>
[0085] Lithium cobalt oxide, polyvinylidene fluoride, and conductive carbon black (SP) were mixed in a mass ratio of 97:1.5:1.5, and N-methylpyrrolidone (NMP) was added as a solvent to form a slurry with a solid content of 70 wt%, which was then stirred evenly. The slurry was evenly coated on one surface of a 10 μm thick positive electrode current collector aluminum foil (elongation 3.0%), leaving the ends of the positive electrode current collector uncoated. The cathode was then dried at 90°C to produce a positive electrode sheet with a positive electrode active material layer thickness of 40 μm. The slurry was then coated on the other surface of the positive electrode sheet, with the slurry coating length on this surface being shorter than that on the other surface along the length of the current collector. This resulted in the positive electrode sheet comprising a bare foil area, a single-sided coated area, and a double-sided coated area. The double-sided coated area of the positive electrode sheet was located in the first area, the single-sided coated area was located in the second area, and the bare foil area was located in the third area. The sheet was then cold-pressed and cut to produce the positive electrode sheet. The cold pressing process parameters are three low-pressure cold pressing cycles: the first cold pressing cycle is at 20 tons and a roll gap of -100 μm; the second cold pressing cycle is at 30 tons and a roll gap of -100 μm; and the third cold pressing cycle is at 30 tons and a roll gap of -100 μm. The resulting positive electrode sheet has a porosity of 15%.
[0086] <Preparation of negative electrode sheet>
[0087] Artificial graphite, styrene-butadiene rubber (SBR), and sodium carboxymethyl cellulose (CMC) were mixed in a mass ratio of 97.4:1.9:0.7, and deionized water was added to form a slurry with a solid content of 70 wt%. The mixture was then stirred evenly. The slurry was evenly coated on one surface of an 8 μm thick negative electrode current collector copper foil and dried at 85°C to produce a negative electrode sheet with a 40 μm thick negative electrode active material layer. The above steps were then repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet coated on both sides with negative electrode material. The resulting negative electrode sheet was then cold pressed, slit, and cut into negative electrode sheets.
[0088] <Preparation of Electrolyte>
[0089] EC, DEC, PC, PP and VC were mixed in a mass ratio of 20:30:20:28:2 to obtain a non-aqueous organic solvent. Then, lithium salt LiPF6 and the non-aqueous organic solvent were prepared in a mass ratio of 8:92 to obtain an electrolyte.
[0090] <Preparation of Separator>
[0091] A porous polyethylene film with a thickness of 7 μm was used.
[0092] <Preparation of lithium-ion batteries>
[0093] The positive electrode sheet, separator, and negative electrode sheet prepared above are stacked in order, with the separator positioned between the positive and negative electrode sheets to act as a separator, and then wound to form an electrode assembly. The electrode assembly is then placed in an aluminum-plastic film packaging bag, dried, and then injected with electrolyte. The lithium-ion battery is then produced through vacuum packaging, resting, formation, degassing, and trimming.
[0094] Example 1-2 to Example 1-6
[0095] Except that in the <Preparation of Positive Electrode Sheet>, Ma and Mb are adjusted as shown in Table 1 by adjusting the cold pressing process, current collector elongation and current collector tensile strength, the rest is the same as Example 1-1.
[0096] Example 2-1 to Example 2-3
[0097] Except that Hc is adjusted as shown in Table 2 in <Preparation of Positive Electrode Sheet>, and Ma is adjusted by adjusting the cold pressing process, current collector elongation, and current collector tensile strength, the rest is the same as Example 1-1.
[0098] Example 3-1 to Example 3-4
[0099] Except that in <Preparation of Positive Electrode Sheet>, Ma is adjusted as shown in Table 3 by adjusting the cold pressing process, collector elongation and collector tensile strength, and the porosity P of the positive electrode sheet is adjusted as shown in Table 3 by adjusting the cold pressing pressure, the rest is the same as Example 1-1.
[0100] Example 4-1 to Example 4-4
[0101] Except that in the preparation of the positive electrode sheet, the binder content was adjusted to adjust F as shown in Table 4, the rest was the same as in Example 1-6.
[0102] Comparative Example 1
[0103] Except that in the <Preparation of Positive Electrode Sheet>, Ma is adjusted as shown in Table 1 by adjusting the cold pressing process, current collector elongation and current collector tensile strength, the rest is the same as Example 1-1.
[0104] Comparative Example 2
[0105] Except that Hc is adjusted as shown in Table 2 in <Preparation of Positive Electrode Sheet> and Ma is adjusted by adjusting the cold pressing process, current collector elongation and current collector tensile strength, the rest is the same as Example 1-1.
[0106] Comparative Example 3
[0107] Except in the preparation of the positive electrode sheet, by adjusting the cold pressing process, the elongation rate of the current collector, and the tensile strength of the current collector to adjust Ma as shown in Table 3, and by adjusting the cold pressing pressure to adjust the porosity P of the positive electrode sheet as shown in Table 3, the rest is the same as in Example 1-1.
[0108] Table 1
[0109] As can be seen from Examples 1-1 to 1-5 and Comparative Example 1 in Table 1, by controlling the mass per unit area Ma, Mb, Mc of the first region, the second region, and the third region of the positive current collector to satisfy: Ma ≤ Mb < Mc, and Ma / Mc ≤ 99%, the thickness expansion rate of the secondary battery after storage at 85°C for 24 h is significantly reduced, indicating that the solution of the present application can effectively improve the structural stability of the positive electrode sheet, thereby improving the high-temperature storage performance of the secondary battery.
[0110] Table 2
[0111] As can be seen from Examples 1-1, Examples 2-1 to 2-3 and Comparative Example 2 in Table 2, on the basis of satisfying Ma ≤ Mb < Mc and Ma / Mc ≤ 99%, by controlling Ma / Mc ≤ -0.0892 × Md / Hc + 1.3652, the thickness expansion rate of the secondary battery after storage at 85°C for 24 h is further reduced, indicating that the solution of the present application can effectively improve the structural stability of the positive electrode sheet, thereby improving the high-temperature storage performance of the secondary battery.
[0112] Table 3
[0113] As can be seen from Examples 1-1, Examples 3-1 to 3-4 and Comparative Example 3 in Table 3, on the basis of satisfying Ma ≤ Mb < Mc and Ma / Mc ≤ 99%, by controlling P ≥ [Md / Hc × (-0.2429) + 1.2007] × 100%, the 3C charge capacity retention rate of the secondary battery is significantly improved, and the thickness expansion rate of the secondary battery after storage at 85°C for 24 h is relatively low. It shows that the solution of the present application can improve the rate performance of the lithium-ion battery while improving the high-temperature storage performance of the secondary battery, which is beneficial to obtaining a lithium-ion battery with excellent rate performance and high-temperature storage performance.
[0114] Table 4
[0115] As can be seen from Examples 1-6, Examples 4-1 to Examples 4-4 in Table 4, the thickness of the positive electrode active material layer, the thickness of the negative electrode active material layer, and the adhesion force F between the wet film of the positive electrode active material layer and the positive electrode current collector usually also affect the performance of the secondary battery. On the basis of satisfying Ma ≤ Mb < Mc and Ma / Mc ≤ 99%, by adjusting the above parameters within the scope of this application, it is beneficial to obtain a secondary battery with excellent high-temperature storage performance.
[0116] The above are only the preferred embodiments of this application and are not intended to limit this application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of this application shall be included within the scope of protection of this application.
Claims
1. A secondary battery, comprising an electrode assembly, the electrode assembly comprising a positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer comprising a positive electrode active material, the positive electrode current collector comprising a first region, a second region and a third region, the positive electrode active material layer being disposed on both sides of the first region, the positive electrode active material layer being disposed on one side of the second region, and the positive electrode active material layer being not disposed on both sides of the third region, in, The mass per unit area of the first region is Mag / m 2 , the mass per unit area of the second region is Mb g / m 2 The mass per unit area of the third region is Mc g / m 2 , satisfying: Ma≤Mb<Mc, and Ma / Mc≤99%.
2. The secondary battery according to claim 1, wherein The thickness of the positive electrode active material layer on the first region is Hc μm, and the mass per unit area of the positive electrode active material layer on the first region is Md g / m 2 , satisfying: Ma / Mc≤-0.0892×Md / Hc+1.3652.
3. The secondary battery according to claim 1, wherein The porosity of the positive electrode sheet is P, and the mass per unit area of the positive electrode active material layer located in the first region is Md g / m 2 , satisfying: P≥[Md / Hc×(-0.2429)+1.2007]×100%.
4. The secondary battery according to claim 2, wherein The electrode assembly further includes a negative electrode sheet, the negative electrode sheet includes a negative electrode active material layer, the single-side thickness of the negative electrode active material layer is Ha μm, and satisfies: 0.2≤Hc / Ha≤4.
5. The secondary battery according to claim 1, wherein The bonding force between the wet film of the positive electrode active material layer and the positive electrode current collector is FN / m, where F≥1.
6. The secondary battery according to claim 1 or 2, wherein: The secondary battery satisfies at least one of the following characteristics: 1)Ma / Mc≤98.5%; 2)0.5≤Hc / Ha≤1.
5.
7. The secondary battery according to claim 1, wherein The positive electrode current collector includes at least one of aluminum foil, nickel foil or aluminum-nickel alloy foil.
8. The secondary battery according to claim 1, wherein The positive electrode active material includes at least one of lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate or lithium-rich manganese-based materials.
9. The secondary battery according to claim 1, wherein The positive electrode active material layer also includes a binder, which includes at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinyl pyrrolidone, polyamide, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, polyhexafluoropropylene, polypropylene, polyethylene, polyetherimide or a copolymer of propylene olefin derivatives.
10. The secondary battery according to claim 1, wherein The positive electrode active material layer also includes a conductive agent, which includes at least one of conductive carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes, nanocarbon fibers or graphene.
11. An electric device comprising the secondary battery according to any one of claims 1 to 10.
Citation Information
Patent Citations
Surface-textured metal foil electrode plates for lithium-ion batteries and their manufacturing method
CN102299341A
An electrochemical device and an electronic device comprising the same
CN109244475A
Positive plate, preparation method and lithium ion battery comprising positive plate
CN111554878A
Positive plate and lithium ion battery
CN115548255A
Battery
CN214956957U