High-conductivity NANO carbon-coated current collector and preparation method therefor
By using highly conductive nano-coated carbon current collectors and branched modified polyurethane acrylate resins in lithium-ion batteries, the problems of reduced conductivity and insufficient adhesion of the conductive layer caused by the combination of traditional conductive agents and binders are solved, achieving High conductivity and improved uniformity.
Patent Information
- Application Number
- PCT/CN2023/141367
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-03
AI Technical Summary
In the manufacturing process of non-aqueous lithium-ion batteries, the traditional combination of conductive agents and binders leads to a decrease in the conductivity of the conductive layer and insufficient adhesion, which affects the rate performance of the current collector and the adhesion performance of the active material to the electrode piece.
Highly conductive nano-coated carbon current collectors are used to prepare conductive adhesives with branched structures, increase the amount of conductive carbon materials added, and use the spherical-like spatial structure of branched modified polyurethane acrylate resin to reduce the viscosity of the adhesive , improve conductivity and compatibility, while forming a dense cross-linked network to improve viscosity.
It significantly improves the conductivity and bonding performance of the current collector, avoids performance degradation caused by too much conductive carbon material, and improves the uniformity and conductivity of the conductive layer.
Smart Images

Figure PCTCN2023141367-FTAPPB-I100001
Abstract
Description
A high-conductivity nano-carbon-coated current collector and its preparation method Technical Field
[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a highly conductive nano-carbon-coated current collector and a preparation method thereof. Background Art
[0002] Currently, in the manufacturing process of non-aqueous secondary batteries, in order to improve the battery's rate performance and the adhesion of the active material to the electrode, a layer of conductive material is usually coated on the surface of the current collector. The manufacturing process of this layer is usually to add a conductive agent and a binder into water, stir and disperse them, and then coat them on the surface of the current collector. However, since the binder is traditional acrylic glue, which is an insulating material, as the amount of glue added increases, the conductivity of the conductive layer becomes weaker. Excessive addition of conductive material will cause poor compatibility, agglomeration, and decreased adhesion, affecting the normal use of the current collector.
[0003] Summary of the Invention
[0004] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0005] The purpose of this application is to provide a highly conductive nano-carbon-coated current collector and a preparation method thereof to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present application provides the following technical solutions: a highly conductive nano-carbon-coated current collector having the following characteristics: the highly conductive nano-carbon-coated current collector comprises a current collector and a highly conductive nano-carbon-coated layer coated on both sides of the current collector;
[0007] Wherein, the current collector is any one of copper foil, aluminum foil, and copper-aluminum alloy foil;
[0008] The highly conductive nano carbon coating layer is formed by coating and drying a conductive adhesive.
[0009] Optionally, the total thickness of the highly conductive nano-carbon-coated current collector is 3-20 μm; and the thickness of the current collector is 2-18 μm.
[0010] Optionally, the highly conductive nano-carbon coating layer has a thickness of 0.5-1 μm.
[0011] Optionally, the conductive adhesive comprises the following components, in parts by weight: 10-15 parts of methyl methacrylate, 5-8 parts of hydroxyethyl methacrylate, 3-5 parts of vinyl acetate, 8-12 parts of isobornyl methacrylate, 15-25 parts of branched modified polyurethane acrylate resin, 0.1-0.3 parts of initiator, 0.3-0.5 parts of emulsifier, 10-25 parts of conductive carbon material, 40-50 parts of water, 0.5-1 parts of defoaming agent, 0.5-1 parts of dispersant and 1-10 parts of isopropyl alcohol;
[0012] Wherein, the conductive carbon material is any one of conductive carbon black, CNT, graphene, and carbon nanofiber.
[0013] Optionally, the preparation method of the branched modified polyurethane acrylate resin comprises the following steps:
[0014] a. P-phenylene diisocyanate was dissolved in DMF, dibutyltin diisocyanate was added, mixed well, heated to 35-38 ° C, and after the temperature was constant, 1,3,5-cyclohexanetriol was added dropwise, nitrogen atmosphere was protected, and the reaction was kept warm for 1-2 hours. The temperature was raised to 75-80 ° C, the reaction was continued for 4-6 hours, and the temperature was lowered to 45-55 ° C. Bis-mercaptoethyl sulfide was added dropwise, and the reaction was stirred for 1-1.5 hours. Isophorone diisocyanate was continued to be added dropwise. After the reaction was allowed to proceed for 2-4 hours, pentaerythritol was added, the temperature was raised to 75-80 ° C, the reaction was continued for 3-6 hours, and the excess solvent was removed by rotary evaporation to obtain a branched polyurethane polyol;
[0015] b. Under nitrogen atmosphere, isophorone diisocyanate and p-hydroxyanisole were dissolved in DMF, heated to 45-50 ° C, a DMF solution of hydroxypropyl methacrylate was added dropwise. After the addition was completed, the reaction was continued for 2-3h. The branched polyurethane polyol obtained in step a was added, heated to 75-80 ° C, and the reaction was allowed to proceed for 4-8h. The excess solvent was evaporated in vacuo to obtain a branched modified polyurethane acrylate resin.
[0016] Optionally, in step a, the molar ratio of p-phenylene diisocyanate, dibutyltin diisocyanate, 1,3,5-cyclohexanetriol, bis-mercaptoethyl sulfide, isophorone diisocyanate, and pentaerythritol is (2.5-3.2): (0.01-0.03): 1: (2.5-3): (2.5-3): (2.2-3.2) in terms of molar ratio.
[0017] Optionally, in step b, the mass ratio of isophorone diisocyanate, p-hydroxyanisole, hydroxypropyl methacrylate, and branched polyurethane polyol is (1.8-2.1): (0.01-0.02): (1.1-1.4): (8-8.6) by mole.
[0018] Optionally, the initiator is azobisisobutyronitrile; the emulsifier is nonylphenol polyoxyethylene ether; the defoamer is an organosilicon defoamer; and the dispersant is sodium dodecylbenzenesulfonate.
[0019] A method for preparing a highly conductive nano-carbon-coated current collector comprises the following steps:
[0020] S1. Methyl methacrylate, hydroxyethyl methacrylate, vinyl acetate, isobornyl methacrylate and a branched modified polyurethane acrylate resin were mixed, an emulsifier and water were added, and the mixture was stirred to obtain an acrylic monomer emulsion;
[0021] S2. The initiator is dissolved in isopropanol to obtain an initiator dropwise solution. The acrylic monomer emulsion prepared in step S1 is heated to 85-95°C and the initiator dropwise solution is slowly added dropwise thereto. After the addition is completed, the reaction is kept warm for 2-4 hours and then cooled to 30-45°C. A dispersant, a defoaming agent and a conductive carbon material are added and stirred for 0.5-1 hour to obtain a conductive adhesive.
[0022] S3. Apply the conductive adhesive to both sides of the current collector, heat it to 105-120°C, and dry it for 2-4 minutes to obtain a highly conductive nano-carbon-coated current collector.
[0023] In order to enhance the conductivity of the highly conductive nano-carbon coating layer, the present application prepared a conductive adhesive and increased the amount of conductive carbon material added therein to ensure the conductive performance of the nano-conductive carbon coating layer. However, the addition of the conductive carbon material will reduce the viscosity and coating performance of the conductive adhesive and affect its overall uniformity. Therefore, to avoid this phenomenon, the present application further prepared a branched modified polyurethane acrylate resin with a branched structure;
[0024] The present application first uses 1,3,5-cyclohexanetriol as a core molecule, adds it dropwise to p-phenylene diisocyanate, reacts to form a three-arm compound with an isocyanate end group, and further mixes it with bismercaptoethyl sulfide, and controls the order of addition to control the end group of the reaction product to be an active mercapto group, and further reacts it with isophorone diisocyanate to generate an isocyanate end group reaction product again, and then mixes it again with pentaerythritol to finally form a branched polyurethane polyol with a terminal hydroxyl group;
[0025] On this basis, the present application further mixes isophorone diisocyanate with hydroxypropyl methacrylate, limits the order of addition and reaction conditions, prepares an acrylic monomer with a free isocyanate group, and then further mixes it with a branched polyurethane polyol with a branched structure to generate a branched modified polyurethane acrylate resin; the branched modified polyurethane acrylate resin has a spherical spatial structure, which can effectively reduce the viscosity of the adhesive, thereby improving the dispersibility of the conductive carbon material in the adhesive, and the end group of the modified polyurethane acrylate resin has a large number of active groups, which can form a denser cross-linked network, thereby improving the viscosity of the conductive adhesive.
[0026] Compared with the prior art, the beneficial effects achieved by the present application are: in order to improve the conductive properties of the current collector, the present application prepares a conductive adhesive with high conductivity; in order to enhance the conductive properties of the conductive adhesive, the present application first increases the amount of conductive carbon material added, and at the same time, in order to avoid the performance degradation caused by excessive conductive carbon material, the present application further prepares a branched modified polyurethane acrylate resin, and utilizes its spherical spatial structure to reduce the overall viscosity of the adhesive, improve its flow properties, and increase the compatibility and dispersion properties of the conductive carbon material in the system. In addition, the branched modified polyurethane acrylate resin also has a large number of acrylic groups, which can further improve the complexity of the cross-linked network, and can effectively improve the viscosity of the adhesive, while improving the conductivity and avoiding the degradation of the bonding performance.
[0027] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION
[0028] The following is a clear and complete description of the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0029] Example 1.
[0030] A method for preparing a highly conductive nano-carbon-coated current collector comprises the following steps:
[0031] S1. In parts by weight, 10 parts of methyl methacrylate, 5 parts of hydroxyethyl methacrylate, 3 parts of vinyl acetate, 8 parts of isobornyl methacrylate and 15 parts of branched modified polyurethane acrylate resin were mixed, 0.3 parts of nonylphenol polyoxyethylene ether emulsifier and 80 parts of water were added, and the mixture was stirred to obtain an acrylic monomer emulsion;
[0032] The preparation method of the branched modified polyurethane acrylate resin comprises the following steps:
[0033] a. In molar parts, 2.5 mol of p-phenylene diisocyanate was dissolved in DMF, 0.01 mol of dibutyltin disilicate was added, mixed well, heated to 35 ° C, and after constant temperature, 1 mol of 1,3,5-cyclohexanetriol was added dropwise under nitrogen atmosphere for 1 hour, heated to 75 ° C, and the reaction was continued for 4 hours, cooled to 45 ° C, 2.5 mol of bis-mercaptoethyl sulfide was added dropwise, stirred for 1 hour, and then 2.5 mol of isophorone diisocyanate was added dropwise. After 2 hours of reaction, 2.2 mol of pentaerythritol was added, heated to 75 ° C, and the reaction was continued for 3 hours. The excess solvent was removed by rotary evaporation to obtain a branched polyurethane polyol;
[0034] b. By mass, under a nitrogen atmosphere, 18 parts of isophorone diisocyanate and 0.1 parts of p-hydroxyanisole were dissolved in DMF, the temperature was raised to 45 ° C, 11 parts of hydroxypropyl methacrylate in a DMF solution were added dropwise, and after the addition was completed, the reaction was continued for 2h, 80 parts of the branched polyurethane polyol obtained in step a were added, the temperature was raised to 75 ° C, the reaction was allowed to proceed for 4h, and the excess solvent was evaporated in vacuo to obtain a branched modified polyurethane acrylate resin.
[0035] S2. By weight, 0.1 parts of azobisisobutyronitrile initiator were dissolved in 1 part of isopropanol to obtain an initiator dropwise solution. The acrylic monomer emulsion prepared in step S1 was heated to 85 ° C and the initiator dropwise solution was slowly added thereto. After the addition was completed, the reaction was kept warm for 2 hours, then cooled to 30 ° C, 0.5 parts of sodium dodecylbenzenesulfonate dispersant, 0.5 parts of silicone defoamer and 55 parts of conductive carbon black were added, and stirring was continued for 0.5-1 hour to obtain a conductive adhesive;
[0036] S3. Apply the conductive adhesive to both sides of the current collector, heat it to 105°C, and dry it for 2 minutes to obtain a highly conductive nano-carbon-coated current collector.
[0037] Example 2.
[0038] Compared with Example 1, this example increases the amount of branched modified polyurethane acrylate resin added in step S1;
[0039] A method for preparing a highly conductive nano-carbon-coated current collector comprises the following steps:
[0040] S1. In parts by weight, 10 parts of methyl methacrylate, 5 parts of hydroxyethyl methacrylate, 3 parts of vinyl acetate, 8 parts of isobornyl methacrylate and 25 parts of branched modified polyurethane acrylate resin were mixed, 0.3 parts of nonylphenol polyoxyethylene ether emulsifier and 80 parts of water were added, and the mixture was stirred to obtain an acrylic monomer emulsion;
[0041] The preparation method of the branched modified polyurethane acrylate resin comprises the following steps:
[0042] a. In molar parts, 2.5 mol of p-phenylene diisocyanate was dissolved in DMF, 0.01 mol of dibutyltin disilicate was added, mixed well, heated to 35 ° C, and after constant temperature, 1 mol of 1,3,5-cyclohexanetriol was added dropwise under nitrogen atmosphere for 1 hour, heated to 75 ° C, and the reaction was continued for 4 hours, cooled to 45 ° C, 2.5 mol of bis-mercaptoethyl sulfide was added dropwise, stirred for 1 hour, and then 2.5 mol of isophorone diisocyanate was added dropwise. After 2 hours of reaction, 2.2 mol of pentaerythritol was added, heated to 75 ° C, and the reaction was continued for 3 hours. The excess solvent was removed by rotary evaporation to obtain a branched polyurethane polyol;
[0043] b. By mass, under a nitrogen atmosphere, 18 parts of isophorone diisocyanate and 0.1 parts of p-hydroxyanisole were dissolved in DMF, the temperature was raised to 45 ° C, 11 parts of hydroxypropyl methacrylate in a DMF solution were added dropwise, and after the addition was completed, the reaction was continued for 2h, 80 parts of the branched polyurethane polyol obtained in step a were added, the temperature was raised to 75 ° C, the reaction was allowed to proceed for 4h, and the excess solvent was evaporated in vacuo to obtain a branched modified polyurethane acrylate resin.
[0044] S2. By weight, 0.1 parts of azobisisobutyronitrile initiator were dissolved in 1 part of isopropanol to obtain an initiator dropwise solution. The acrylic monomer emulsion prepared in step S1 was heated to 85 ° C and the initiator dropwise solution was slowly added thereto. After the addition was completed, the reaction was kept warm for 2 hours, then cooled to 30 ° C, 0.5 parts of sodium dodecylbenzenesulfonate dispersant, 0.5 parts of silicone defoamer and 55 parts of conductive carbon black were added, and stirring was continued for 0.5-1 hour to obtain a conductive adhesive;
[0045] S3. Apply the conductive adhesive to both sides of the current collector, heat it to 105°C, and dry it for 2 minutes to obtain a highly conductive nano-carbon-coated current collector.
[0046] Example 3.
[0047] Compared with Example 2, this example increases the amount of p-phenylenediisocyanate added in step a;
[0048] A method for preparing a highly conductive nano-carbon-coated current collector comprises the following steps:
[0049] S1. In parts by weight, 10 parts of methyl methacrylate, 5 parts of hydroxyethyl methacrylate, 3 parts of vinyl acetate, 8 parts of isobornyl methacrylate and 25 parts of branched modified polyurethane acrylate resin were mixed, 0.3 parts of nonylphenol polyoxyethylene ether emulsifier and 80 parts of water were added, and the mixture was stirred to obtain an acrylic monomer emulsion;
[0050] The preparation method of the branched modified polyurethane acrylate resin comprises the following steps:
[0051] a. In molar parts, 3.2 mol of p-phenylene diisocyanate was dissolved in DMF, 0.01 mol of dibutyltin silicate in February was added, mixed evenly, heated to 35 ° C, and after constant temperature, 1 mol of 1,3,5-cyclohexanetriol was added dropwise under nitrogen atmosphere for 1 hour, heated to 75 ° C, and the reaction was continued for 4 hours, cooled to 45 ° C, 2.5 mol of bis-mercaptoethyl sulfide was added dropwise, stirred for 1 hour, and then 2.5 mol of isophorone diisocyanate was added dropwise. After 2 hours of reaction, 2.2 mol of pentaerythritol was added, heated to 75 ° C, and the reaction was continued for 3 hours. The excess solvent was removed by rotary evaporation to obtain a branched polyurethane polyol;
[0052] b. By mass, under a nitrogen atmosphere, 18 parts of isophorone diisocyanate and 0.1 parts of p-hydroxyanisole were dissolved in DMF, the temperature was raised to 45 ° C, 11 parts of hydroxypropyl methacrylate in a DMF solution were added dropwise, and after the addition was completed, the reaction was continued for 2h, 80 parts of the branched polyurethane polyol obtained in step a were added, the temperature was raised to 75 ° C, the reaction was allowed to proceed for 4h, and the excess solvent was evaporated in vacuo to obtain a branched modified polyurethane acrylate resin.
[0053] S2. By weight, 0.1 parts of azobisisobutyronitrile initiator were dissolved in 1 part of isopropanol to obtain an initiator dropwise solution. The acrylic monomer emulsion prepared in step S1 was heated to 85 ° C and the initiator dropwise solution was slowly added thereto. After the addition was completed, the reaction was kept warm for 2 hours, then cooled to 30 ° C, 0.5 parts of sodium dodecylbenzenesulfonate dispersant, 0.5 parts of silicone defoamer and 55 parts of conductive carbon black were added, and stirring was continued for 0.5-1 hour to obtain a conductive adhesive;
[0054] S3. Apply the conductive adhesive to both sides of the current collector, heat it to 105°C, and dry it for 2 minutes to obtain a highly conductive nano-carbon-coated current collector.
[0055] Example 4.
[0056] Compared with Example 2, this example increases the amount of bis-mercaptoethyl sulfide added in step a;
[0057] A method for preparing a highly conductive nano-carbon-coated current collector comprises the following steps:
[0058] S1. In parts by weight, 10 parts of methyl methacrylate, 5 parts of hydroxyethyl methacrylate, 3 parts of vinyl acetate, 8 parts of isobornyl methacrylate and 25 parts of branched modified polyurethane acrylate resin were mixed, 0.3 parts of nonylphenol polyoxyethylene ether emulsifier and 80 parts of water were added, and the mixture was stirred to obtain an acrylic monomer emulsion;
[0059] The preparation method of the branched modified polyurethane acrylate resin comprises the following steps:
[0060] a. In molar parts, 2.5 mol of p-phenylene diisocyanate was dissolved in DMF, 0.01 mol of dibutyltin silicate in February was added, mixed evenly, heated to 35 ° C, and after constant temperature, 1 mol of 1,3,5-cyclohexanetriol was added dropwise under nitrogen atmosphere for 1 hour, heated to 75 ° C, and the reaction was continued for 4 hours, cooled to 45 ° C, 3 mol of bis-mercaptoethyl sulfide was added dropwise, stirred for 1 hour, and then 2.5 mol of isophorone diisocyanate was added dropwise. After 2 hours of reaction, 2.2 mol of pentaerythritol was added, heated to 75 ° C, and the reaction was continued for 3 hours. The excess solvent was removed by rotary evaporation to obtain a branched polyurethane polyol;
[0061] b. By mass, under a nitrogen atmosphere, 18 parts of isophorone diisocyanate and 0.1 parts of p-hydroxyanisole were dissolved in DMF, the temperature was raised to 45 ° C, 11 parts of hydroxypropyl methacrylate in a DMF solution were added dropwise, and after the addition was completed, the reaction was continued for 2h, 80 parts of the branched polyurethane polyol obtained in step a were added, the temperature was raised to 75 ° C, the reaction was allowed to proceed for 4h, and the excess solvent was evaporated in vacuo to obtain a branched modified polyurethane acrylate resin.
[0062] S2. By weight, 0.1 parts of azobisisobutyronitrile initiator were dissolved in 1 part of isopropanol to obtain an initiator dropwise solution. The acrylic monomer emulsion prepared in step S1 was heated to 85 ° C and the initiator dropwise solution was slowly added thereto. After the addition was completed, the reaction was kept warm for 2 hours, then cooled to 30 ° C, 0.5 parts of sodium dodecylbenzenesulfonate dispersant, 0.5 parts of silicone defoamer and 55 parts of conductive carbon black were added, and stirring was continued for 0.5-1 hour to obtain a conductive adhesive;
[0063] S3. Apply the conductive adhesive to both sides of the current collector, heat it to 105°C, and dry it for 2 minutes to obtain a highly conductive nano-carbon-coated current collector.
[0064] Example 5.
[0065] Compared with Example 2, this example increases the amount of pentaerythritol added in step a;
[0066] A method for preparing a highly conductive nano-carbon-coated current collector comprises the following steps:
[0067] S1. In parts by weight, 10 parts of methyl methacrylate, 5 parts of hydroxyethyl methacrylate, 3 parts of vinyl acetate, 8 parts of isobornyl methacrylate and 25 parts of branched modified polyurethane acrylate resin were mixed, 0.3 parts of nonylphenol polyoxyethylene ether emulsifier and 80 parts of water were added, and the mixture was stirred to obtain an acrylic monomer emulsion;
[0068] The preparation method of the branched modified polyurethane acrylate resin comprises the following steps:
[0069] a. In molar parts, 2.5 mol of p-phenylene diisocyanate was dissolved in DMF, 0.01 mol of dibutyltin silicate in February was added, mixed evenly, heated to 35 ° C, and after constant temperature, 1 mol of 1,3,5-cyclohexanetriol was added dropwise under nitrogen atmosphere for 1 hour, heated to 75 ° C, and the reaction was continued for 4 hours, cooled to 45 ° C, 2.5 mol of bis-mercaptoethyl sulfide was added dropwise, stirred for 1 hour, and then 2.5 mol of isophorone diisocyanate was added dropwise. After 2 hours of reaction, 3.2 mol of pentaerythritol was added, heated to 75 ° C, and the reaction was continued for 3 hours. The excess solvent was removed by rotary evaporation to obtain a branched polyurethane polyol;
[0070] b. By mass, under a nitrogen atmosphere, 18 parts of isophorone diisocyanate and 0.1 parts of p-hydroxyanisole were dissolved in DMF, the temperature was raised to 45 ° C, 11 parts of hydroxypropyl methacrylate in a DMF solution were added dropwise, and after the addition was completed, the reaction was continued for 2h, 80 parts of the branched polyurethane polyol obtained in step a were added, the temperature was raised to 75 ° C, the reaction was allowed to proceed for 4h, and the excess solvent was evaporated in vacuo to obtain a branched modified polyurethane acrylate resin.
[0071] S2. By weight, 0.1 parts of azobisisobutyronitrile initiator were dissolved in 1 part of isopropanol to obtain an initiator dropwise solution. The acrylic monomer emulsion prepared in step S1 was heated to 85 ° C and the initiator dropwise solution was slowly added thereto. After the addition was completed, the reaction was kept warm for 2 hours, then cooled to 30 ° C, 0.5 parts of sodium dodecylbenzenesulfonate dispersant, 0.5 parts of silicone defoamer and 55 parts of conductive carbon black were added, and stirring was continued for 0.5-1 hour to obtain a conductive adhesive;
[0072] S3. Apply the conductive adhesive to both sides of the current collector, heat it to 105°C, and dry it for 2 minutes to obtain a highly conductive nano-carbon-coated current collector.
[0073] Example 6.
[0074] A method for preparing a highly conductive nano-carbon-coated current collector comprises the following steps:
[0075] S1. In parts by weight, 15 parts of methyl methacrylate, 8 parts of hydroxyethyl methacrylate, 5 parts of vinyl acetate, 12 parts of isobornyl methacrylate and 25 parts of branched modified polyurethane acrylate resin were mixed, 0.5 parts of nonylphenol polyoxyethylene ether emulsifier and 100 parts of water were added, and the mixture was stirred to obtain an acrylic monomer emulsion;
[0076] The preparation method of the branched modified polyurethane acrylate resin comprises the following steps:
[0077] a. In molar parts, 3.2 mol of p-phenylene diisocyanate was dissolved in DMF, 0.03 mol of dibutyltin disilicate was added, mixed evenly, heated to 38 ° C, and after constant temperature, 1 mol of 1,3,5-cyclohexanetriol was added dropwise under nitrogen atmosphere for 2 hours, then heated to 80 ° C, the reaction was continued for 6 hours, cooled to 55 ° C, 3 mol of bis-mercaptoethyl sulfide was added dropwise, the reaction was stirred for 1.5 hours, and then 3 mol of isophorone diisocyanate was added dropwise. After 4 hours of reaction, 3.2 mol of pentaerythritol was added, the temperature was raised to 80 ° C, the reaction was continued for 6 hours, and the excess solvent was removed by rotary evaporation to obtain a branched polyurethane polyol;
[0078] b. By mass, under nitrogen atmosphere, 21 parts of isophorone diisocyanate and 0.2 parts of p-hydroxyanisole were dissolved in DMF, heated to 50 ° C, 14 parts of hydroxypropyl methacrylate in DMF solution were added dropwise. After the addition was completed, the reaction was continued for 3h, 86 parts of the branched polyurethane polyol obtained in step a were added, the temperature was raised to 80 ° C, the reaction was allowed to proceed for 8h, and the excess solvent was evaporated in vacuo to obtain a branched modified polyurethane acrylate resin.
[0079] S2. Dissolve 0.3 parts of azobisisobutyronitrile initiator in 20 parts of isopropanol by weight to obtain an initiator dropwise solution. Heat the acrylic monomer emulsion prepared in step S1 to 95°C and slowly add the initiator dropwise solution thereto. After the addition is completed, keep the mixture warm for 4 hours, cool it to 45°C, add 1 part of sodium dodecylbenzenesulfonate dispersant, 1 part of silicone defoamer and 75 parts of conductive carbon black, and continue stirring for 1 hour to obtain a conductive adhesive.
[0080] S3. Apply the conductive adhesive to both sides of the current collector, heat it to 110°C, and dry it for 4 minutes to obtain a highly conductive nano-carbon-coated current collector.
[0081] Comparative Example 1.
[0082] Compared with Example 1, this comparative example did not prepare branched polyurethane acrylate resin, and only used an equal amount of PVDF as a binder;
[0083] A method for preparing a highly conductive nano-carbon-coated current collector comprises the following steps:
[0084] S1. In parts by weight, 41 parts of PVDF were mixed with 80 parts of water, 0.5 parts of sodium dodecylbenzenesulfonate dispersant, 0.5 parts of silicone defoamer and 55 parts of conductive carbon black were added, and stirring was continued for 0.5-1h to obtain a conductive adhesive;
[0085] S3. Apply the conductive adhesive to both sides of the current collector, heat it to 105°C, and dry it for 2 minutes to obtain a highly conductive nano-carbon-coated current collector.
[0086] Detection:
[0087] The highly conductive nano-carbon-coated current collectors prepared in Examples 1-6 and Comparative Example 1 were prepared into lithium batteries, and the following tests were performed on them;
[0088] Rate performance 5C test: At a temperature of 25℃±5℃, the battery is charged at a constant current of 0.2C to the limit voltage, then switched to constant voltage charging until the cutoff current reaches 0.01C. Charging is then stopped. The battery is then discharged at a current of 5C to the cutoff voltage, and the discharge capacity is obtained. The capacity retention rate is calculated based on the discharge capacity and the initial capacity.
[0089] Cycling performance test: At a temperature of 25℃±5℃, charge the battery at a constant current of 1C to the limit voltage, then change to constant voltage charging until the cutoff current reaches 0.01C and stop charging; discharge at a current of 1C to the termination voltage, cycle continuously for 1000 times, and obtain the discharge capacity. The capacity retention rate is calculated based on the discharge capacity and the initial capacity.
[0090] High-temperature performance test: At a temperature of 25°C ± 5°C, charge the battery at a constant current of 0.2C to the limit voltage, then switch to constant voltage charging until the cutoff current reaches 0.01C and stop charging. Then, after placing the battery at a temperature of 60°C ± 2°C for 2 hours, discharge the battery at 1C to the cutoff voltage and calculate the capacity retention rate.
[0091] Low-temperature performance test: At a temperature of 25°C ± 5°C, charge the battery at a constant current of 0.2C to the limit voltage, then switch to constant voltage charging until the cutoff current reaches 0.01C and stop charging. Then, after placing the battery at a temperature of 60°C ± 2°C for 2 hours, discharge the battery at 1C to the cutoff voltage and calculate the capacity retention rate.
[0092] The test results are shown in the table below:
[0093] Finally, it should be noted that the above description is merely a preferred embodiment of the present application and is not intended to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art may still modify the technical solutions described in the aforementioned embodiments or substitute equivalents for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included within the scope of protection of the present application.
Claims
1. A highly conductive nano-carbon-coated current collector, comprising a current collector and a highly conductive nano-carbon-coated layer coated on both sides of the current collector; in, The current collector is any one of copper foil, aluminum foil, and copper-aluminum alloy foil; The highly conductive nano carbon coating layer is formed by coating and drying a conductive adhesive; The conductive adhesive comprises the following components by weight: 10-15 parts of methyl methacrylate, 5-8 parts of hydroxyethyl methacrylate, 3-5 parts of vinyl acetate, 8-12 parts of isobornyl methacrylate and 15-25 parts of branched modified polyurethane acrylate resin, 0.1-0.3 parts of initiator, 0.3-0.5 parts of emulsifier, 55-75 parts of conductive carbon material, 80-100 parts of water, 0.5-1 parts of defoamer, 0.5-1 parts of dispersant, and 1-20 parts of isopropanol; Wherein, the conductive carbon material is any one of conductive carbon black, CNT, graphene, and carbon nanofiber.
2. A highly conductive nano-carbon-coated current collector according to claim 1, in: The total thickness of the highly conductive nano-carbon-coated current collector is 3-20 μm; the thickness of the current collector is 2-18 μm.
3. A highly conductive nano-carbon-coated current collector according to claim 1 or 2, in: The thickness of the highly conductive nano carbon coating layer is 0.5-1 μm.
4. A highly conductive nano-carbon-coated current collector according to any one of claims 1 to 3, in: The initiator is azobisisobutyronitrile; the emulsifier is nonylphenol polyoxyethylene ether; the defoamer is an organosilicon defoamer; and the dispersant is sodium dodecylbenzene sulfonate.
5. A highly conductive nano-carbon-coated current collector according to any one of claims 1 to 4, in: The preparation method of the branched modified polyurethane acrylate resin comprises the following steps: a. Dissolve p-phenylene diisocyanate in DMF, add dibutyltin diisocyanate, mix well, heat to 35-38°C, add 1,3,5-cyclohexanetriol after the temperature is constant, protect with nitrogen atmosphere, keep warm for 1-2h, heat to 75-80°C, continue to react for 4-6h, cool to 45-55°C, add dithiothiocyanate ether, after stirring for 1-1.5 hours, continue to drop isophorone diisocyanate, after reacting for 2-4 hours, add pentaerythritol, raise the temperature to 75-80°C, continue to react for 3-6 hours, and remove excess solvent by rotary evaporation to obtain branched polyurethane polyol; b. Under nitrogen atmosphere, isophorone diisocyanate and p-hydroxyanisole are dissolved in DMF, the temperature is raised to 45-50 ° C, a DMF solution of hydroxypropyl methacrylate is added dropwise, and after the addition is completed, the reaction is continued for 2-3 hours, the branched polyurethane polyol obtained in step a is added, the temperature is raised to 75-80 ° C, the reaction is continued for 4-8 hours, and the excess solvent is evaporated in vacuo to obtain a branched modified polyurethane acrylate resin.
6. A highly conductive nano-carbon-coated current collector according to claim 5, in: In step a, the molar ratio of p-phenylene diisocyanate, dibutyltin diisocyanate, 1,3,5-cyclohexanetriol, bis-mercaptoethyl sulfide, isophorone diisocyanate and pentaerythritol is (2.5-3.2): (0.01-0.03): 1: (2.5-3): (2.5-3): (2.2-3.2) by mole.
7. A highly conductive nano-carbon-coated current collector according to claim 5 or 6, in: In step b, the mass ratio of isophorone diisocyanate, p-hydroxyanisole, hydroxypropyl methacrylate and branched polyurethane polyol is (1.8-2.1): (0.01-0.02): (1.1-1.4): (8-8.6) by mole.
8. A method for preparing a highly conductive nano-carbon-coated current collector, The following steps are involved: S1. Methyl methacrylate, hydroxyethyl methacrylate, vinyl acetate, isobornyl methacrylate and branched modified polyurethane acrylate resin were mixed, an emulsifier and water were added, and the mixture was stirred to obtain an acrylic monomer emulsion; S2. The initiator is dissolved in isopropanol to obtain an initiator drop solution, the acrylic monomer emulsion prepared in step S1 is heated to 85-95°C, and the initiator drop solution is slowly added thereto. After the addition is completed, the reaction is kept warm for 2-4 hours and then cooled to 30-45°C, a dispersant, a defoaming agent and a conductive carbon material are added, and stirring is continued for 0.5-1h to obtain a conductive adhesive; S3. Apply the conductive adhesive to both sides of the current collector, heat it to 105-120°C, dry it for 2-4 minutes, and then roll it up to obtain a highly conductive nano-carbon-coated current collector.
Citation Information
Patent Citations
Positive active material with topological structure and application thereof
CN107887573A
Organic silver complex ultraviolet-curing conductive silver paste
CN110010262A
Modified polyacrylate emulsion and coating composed of same
CN114276498A
High-power-density electrode plate and preparation method thereof
CN115172659A
High-conductivity nano carbon-coated current collector and preparation method thereof
CN116417620A
Cited By
High-power lead-acid battery electrolyte and preparation method thereof
CN119275381A
Release paper EB curing coating for automotive trim leather and preparation method of release paper EB curing coating
CN119754084A
Dispersing agent for conductive slurry and preparation method thereof
CN120865481A