Secondary battery and use thereof

By adding a conductive agent to the negative electrode sheet of the lithium-ion battery and adjusting its distribution, combined with appropriate graphite and silicon-based material content, the problem of poor conductivity of silicon-based materials is solved, and the energy density and dynamic performance of the battery are improved. Achieved more stable battery performance.

WO2024198585A1PCT designated stage expired Publication Date: 2024-10-03SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/142770
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2023-12-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Silicon-based materials in lithium-ion batteries have poor electrical conductivity, which affects the rate performance and cycle stability of the battery, resulting in poor energy density and dynamic performance.

Method used

Add a conductive agent to the negative electrode plate, and adjust the relationship between the aspect ratio of the conductive agent particles and the content of graphite and silicon-based materials to build a stable conductive network and improve the conductive performance. Through the density distribution of the conductive agent and the density of the binder, Select and optimize the conductive performance and stability of the negative electrode piece.

Benefits of technology

It significantly improves the energy density, rate performance and cycle performance of the battery, reduces the internal resistance and side reactions of the pole pieces, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023142770-FTAPPB-I100001
    Figure PCTCN2023142770-FTAPPB-I100001
  • Figure PCTCN2023142770-FTAPPB-I100002
    Figure PCTCN2023142770-FTAPPB-I100002
  • Figure PCTCN2023142770-FTAPPB-I100003
    Figure PCTCN2023142770-FTAPPB-I100003
Patent Text Reader

Abstract

A secondary battery and a use thereof. The secondary battery comprises a negative electrode sheet; the negative electrode sheet comprises a current collecting layer and a negative electrode active layer provided on at least one surface of the current collecting layer; the negative electrode active layer comprises a negative electrode active material and a conductive agent; the surface density of the surface of the conductive agent close to the current collecting layer is greater than the surface density of the surface away from the current collecting layer; the aspect ratio of the conductive agent is a; the negative electrode active material comprises graphite and SiOx, wherein 0<x≤2; in the negative electrode active material, the mass fraction of SiOx is b%, and the mass fraction of graphite is c%, wherein a, b and c satisfy: a:(c-7b)≥10. The negative electrode sheet in the secondary battery has good conductivity, and the secondary battery has good electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

A secondary battery and its application

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application is based on the Chinese patent application with application number 202310336795.2 and application date of March 27, 2023, and claims the priority of the Chinese patent application. The entire content of the Chinese patent application is hereby introduced into this application as a reference. Technical Field

[0003] The present application belongs to the field of battery technology, and specifically relates to a secondary battery and its application. Background Art

[0004] Secondary batteries, particularly lithium-ion batteries, are characterized by their long cycle life, lack of memory effect, and environmental friendliness, leading to rapid development and widespread application in consumer electronics and electric vehicles. Simultaneously, the demand for higher energy density in lithium-ion batteries is increasing. Currently, the focus of research on anode materials is on silicon-based materials with high theoretical specific capacities, which are more than ten times higher than those of traditional anode materials such as graphite. However, the electrical conductivity of silicon-based materials is inferior to that of traditional graphite, hindering electron transport and lithium ion diffusion in the silicon bulk phase. This, in turn, affects the kinetic performance of the silicon anode, impacting the battery's rate capability and cycling stability.

[0005] Summary of the Invention

[0006] The present application aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present application proposes a secondary battery, wherein the negative electrode sheet in the secondary battery has good electrical conductivity and good electrochemical performance.

[0007] The present application also provides an electrical device comprising the secondary battery.

[0008] In a first aspect of the present application, a secondary battery is provided, which includes a negative electrode plate, the negative electrode plate including a current collecting layer and a negative electrode active layer provided on at least one side of the current collecting layer, the negative electrode active layer including a negative electrode active material and a conductive agent, the surface density of the conductive agent close to the current collecting layer is greater than the surface density of the conductive agent away from the current collecting layer, the aspect ratio of the conductive agent is a, the negative electrode active material includes graphite and SiO x , 0<x≤2, the SiO in the negative electrode active material x The mass fraction of is b%, the mass fraction of graphite is c%, wherein a, b, and c satisfy the following: a:(c-7b)≥10.

[0009] Graphite has stable performance, low price and easy to obtain, but the energy density of graphite is low, so it is necessary to compound silicon-based materials (SiO x ), effectively improving the energy density of the negative electrode, thereby overcoming the problem of low energy density of the graphite negative electrode. However, due to the poor conductivity of silicon-based materials, the conductivity of the electrode sheet is affected, and thus the electrochemical performance of the battery is affected. Therefore, the present application adds a conductive agent to the negative electrode sheet and adjusts the aspect ratio of the conductive agent particles, the relationship with the graphite content and the silicon-based material content, that is, a: (c-7b) ≥ 10, where a represents the aspect ratio of the conductive agent, b represents SiO x The mass fraction of graphite, c represents the mass fraction of graphite. The aspect ratio represents the ratio of the longest diameter through the interior of the particle to the longest diameter perpendicular to it. Based on the above relationship, the conductive agent can be more fully wrapped around the graphite surface and SiO x The surface of the negative electrode sheet ensures that the conductive agent and the negative electrode active material are in full contact, building a stable conductive network, thereby optimizing the conductive performance of the negative electrode sheet, ensuring the conduction effect of electrons in the negative electrode active material, reducing the internal resistance of the negative electrode sheet, reducing battery polarization, and improving the rate performance and cycle performance of the battery. Based on the negative electrode sheet setting of this application, it is possible to improve the energy density of the battery while ensuring the stability of the negative electrode sheet, and also ensure that the rate performance and cycle performance of the battery are improved.

[0010] In addition, in this embodiment, the surface density of the conductive agent close to the current collecting layer is greater than the surface density of the surface away from the current collecting layer. That is, in the negative electrode plate, the mass concentration of the conductive agent in the lower layer of the negative electrode plate is greater than the mass concentration in the upper layer. This is conducive to increasing the rate at which electrons flow into the current collecting layer, thereby improving the overall conductivity of the negative electrode plate, reducing the battery DCR, and improving the battery rate performance. In some embodiments, the surface density of the conductive agent close to the current collecting layer is 0.01 to 0.5 mg / 1540 mm 2 The surface density of the conductive agent away from the current collecting layer is 0.01~0.35mg / 1540mm 2 In some embodiments, the ratio of the surface density of the conductive agent on the side close to the current collecting layer to the surface density on the side away from the current collecting layer is 1:(1-3). Within the above range, the conductivity of the negative electrode sheet is further optimized, and the battery dynamics performance is further improved.

[0011] In some embodiments, the value of a:(c-7b) is less than 750. When the value of a:(c-7b) is less than 750, it can prevent the internal chemical reaction rate of the battery from being too fast, thereby preventing the battery performance from deteriorating.

[0012] In some embodiments, the surface density of the negative electrode active material on the side close to the current collecting layer is greater than the surface density on the side away from the current collecting layer, thereby effectively reducing the consumption of negative electrode active lithium and reducing the contact surface area between the negative electrode active material and the electrolyte, thereby reducing battery side reactions, reducing gas production, and improving the cycle performance and rate performance of the battery. In some embodiments, the surface density of the negative electrode active material on the side close to the current collecting layer is 50 to 200 mg / 1540 mm 2 The surface density of the negative electrode active material away from the current collecting layer is 30 to 145 mg / 1540 mm 2 .

[0013] In some embodiments of the present application, the conductive agent includes at least one of single-walled carbon nanotubes, carbon black, and vapor-phase carbon fibers, and the aspect ratio a of the conductive agent is (1000-10000):1. Among the above conductive agents, single-walled carbon nanotubes have excellent conductivity, flexibility, and structural stability, and when the aspect ratio a of the single-walled carbon nanotubes is within the above range, they can be more fully wrapped around the SiO x Surface and SiO x Full contact, SiO x A stable conductive network is built on the surface. On the one hand, it greatly improves the SiO x On the other hand, due to the flexibility of single-walled carbon nanotubes, silicon-based materials (SiO x ) provides a restraining and buffering effect during the charge and discharge cycle, thereby inhibiting the SiO x The volume expansion during the charge and discharge cycle causes the pole piece to rebound, pulverize, and even peel off from the current collector. In addition, carbon black and vapor-phase carbon fiber have excellent conductivity and buffering capacity, and are widely available. Within the above-mentioned aspect ratio range, they also have similar effects to single-walled carbon nanotubes. In some embodiments, the conductive agent is a mixture of single-walled carbon nanotubes and carbon black, and the mass ratio of single-walled carbon nanotubes to carbon black in the mixture is (0.1 to 0.5):1.

[0014] In some embodiments, 88≤c≤95, 5≤b≤12. That is, based on the mass of the negative electrode active material, the mass fraction of the graphite is 88% to 95%, and the SiO x Accounting for 5% to 12%.

[0015] This application uses SiO x Mixing with graphite as negative electrode active material can not only improve energy density, but also reduce the volume expansion of silicon-based materials during charging and discharging. x The synergistic effect of the graphite content (mass fraction in the negative electrode active material) and the aspect ratio of the conductive agent significantly improves the conductivity, stability and energy density of the negative electrode sheet.

[0016] In some embodiments of the present application, the graphite includes at least one of artificial graphite or natural graphite.

[0017] In some embodiments, the diameter of the single-walled carbon nanotubes is 0.5 to 100 nm. When the diameter of the single-walled carbon nanotubes is within the above range, the conductivity of the negative electrode plate can be further improved, the electron transmission efficiency can be increased, and the electrochemical performance of the battery can be improved.

[0018] In some embodiments, the specific surface area of ​​the conductive agent is 600 to 1500 m 2 When the specific surface area of ​​the conductive agent is within the above range, it is beneficial to the battery performance.

[0019] Through the above-mentioned embodiment, single-walled carbon nanotubes have excellent conductivity, flexibility and structural stability. The present application uses single-walled carbon nanotubes with high aspect ratio and specific surface area as conductive agents, which further promotes the full winding of single-walled carbon nanotubes in SiO x The surface is in full contact with the SiO x A stable conductive network is constructed on the surface, which greatly improves the SiO x The conductivity of the single-walled carbon nanotubes ensures electronic conduction, improves lithium ion transmission, reduces the internal resistance of the electrode and reduces polarization, and improves the rate performance and cycle performance of the battery. The optimal aspect ratio and specific surface area are more conducive to the dispersion effect of single-walled carbon nanotubes, and it is not easy to have SiO x The situation where they are entangled and reunited with each other.

[0020] In some embodiments of the present application, the negative electrode plate further includes a binder, and the binder includes a polyacrylic acid material and a polystyrene material. In the negative electrode active layer, the mass content of the polyacrylic acid material is greater than that of the polystyrene material. On the one hand, the active material, the conductive agent and other materials need to be connected to form a whole by using a binder. On the other hand, the active material and the current collector also need to be bonded by a binder. In the silicon-carbon material negative electrode, due to the SiO x The volume expansion is large, and conventional polystyrene adhesives (such as styrene-butadiene rubber) have limited bonding or restraining capabilities, resulting in poor bonding effects and poor mechanical properties of the electrode, especially when SiO xWhen the content is high, the phenomenon of powdering and demolding of the pole piece is obvious, and a large amount of polystyrene binder needs to be added to form adhesion. The addition of a large amount of polystyrene binder reduces the proportion of active substances and cannot achieve the purpose of improving energy density. When polyacrylic acid materials are used as silicon-carbon material negative electrode binders, although the mechanical properties of the pole piece are improved, a series of processing difficulties are brought about, such as low solid content of the slurry, poor coating appearance, low coating drying efficiency, and polyacrylic acid material binders generally have a glass transition temperature higher than room temperature, and are in a brittle and hard glass state at room temperature. This makes the use of polyacrylic acid material binders more brittle when preparing pole pieces and coating and drying to form films, and the coating parameter window is narrow. The membrane is easy to crack, which seriously affects the production rate and efficiency and does not meet the actual production. Based on the above reasons, the present application uses a mixture of polyacrylic acid materials and polystyrene materials as the binder for the negative pole piece of the present application. The advantages of the two types of binders can be combined to complement each other and reduce the overall amount of binder, which can not only improve the bonding strength, but also inhibit SiO x Expansion performance, and can achieve the purpose of meeting processing performance, the negative electrode plate is not easy to pulverize and demold, and the bonding effect is good. Specifically, on the one hand, the present application adds polyacrylic acid materials to make the negative electrode plate have good bonding strength, inhibit the expansion of the silicon-carbon negative electrode material during the charge and discharge process, so that it has sufficient bonding and cohesive strength. On the other hand, by adding polystyrene materials (such as SBR), the plate has a certain flexibility, improves processing performance, and makes the negative electrode plate have both high bonding force and good flexibility, thereby obtaining a high energy density negative electrode plate. In some embodiments, the mass content of the polyacrylic acid material is greater than that of the polystyrene material, which can be more conducive to improving the adhesion of the negative electrode plate and is beneficial to the cycle performance of the battery.

[0021] In some embodiments of the present application, the mass ratio of the polyacrylic acid material to the polystyrene material is (1.5-3):1. When the mass ratio of the polyacrylic acid material to the polystyrene material is within the above range, the bonding strength of the negative electrode sheet can be further improved, and the cycle performance of the battery can be further optimized.

[0022] In some embodiments of the present application, the polyacrylic acid material includes at least one of polyacrylic acid, polyacrylamide, polyacrylonitrile, polyacrylic acid salt or polyacrylic ester.

[0023] Since polyacrylic acid binders contain a large number of polar functional groups such as carboxyl groups, they can react with SiO x It can form strong hydrogen bonds to form a coating on its surface, binding and buffering SiO x The volume expansion gives the electrode excellent mechanical properties, thereby improving the cycle performance of the negative electrode.

[0024] In some embodiments of the present application, the polyacrylate includes at least one of lithium polyacrylate or sodium polyacrylate.

[0025] In some embodiments of the present application, the polyacrylate includes at least one of polyacrylate or polymethacrylate.

[0026] In some embodiments of the present application, the polystyrene-based material includes at least one of styrene-butadiene rubber or styrene-acrylate.

[0027] In some embodiments of the present application, the mass percentage of the binder in the negative electrode active layer is 2% to 6%. Using the above composite binder can reduce the binder content in the negative electrode sheet while ensuring high bonding performance, which is beneficial for improving battery energy density.

[0028] In some embodiments of the present application, the compaction density of the negative electrode active layer is 1.5 g / cm 3 ~1.8g / cm 3 , preferably 1.6 / cm 3 ~1.8g / cm 3 When the compaction density of the negative electrode active layer is within the above range, the energy density of the battery can be effectively improved, while also improving the cycle performance and rate performance of the battery.

[0029] In some embodiments, the peeling force of the negative electrode sheet is 26 to 36 N / m. The peeling force of the negative electrode sheet is the force required to peel off the negative electrode active material layer and the current collector layer. Under the action of the binder, the peeling force of the negative electrode sheet can be improved, thereby effectively improving the stability of the negative electrode sheet and improving the cycle performance of the battery.

[0030] In a second aspect of the present application, a method for preparing the above-mentioned secondary battery is proposed, comprising the following steps: winding a negative electrode sheet, a diaphragm, and a positive electrode sheet and assembling them into a shell, injecting an electrolyte, and obtaining a secondary battery, wherein the negative electrode sheet comprises a negative electrode active material and a conductive agent, the aspect ratio of the conductive agent is a, and the negative electrode active material comprises graphite and SiO x , 0<x≤2, the SiO in the negative electrode active material x The mass fraction of is b%, the mass fraction of graphite is c%, wherein a, b, and c satisfy the following: a:(c-7b)≥10.

[0031] In some embodiments of the present application, the negative electrode plate includes a current collecting layer and a negative electrode active layer arranged on at least one side of the current collecting layer, the negative electrode active layer includes the negative electrode active material and a conductive agent, and the surface density of the conductive agent close to the current collecting layer is greater than the surface density of the conductive agent away from the current collecting layer.

[0032] In some embodiments of the present application, the secondary battery includes at least one of a lithium ion battery or a sodium ion battery.

[0033] In a third aspect of the present application, an electric device is provided. The electric device includes the secondary battery described above, and the secondary battery is used as a power source for the electric device. DETAILED DESCRIPTION

[0034] The following will clearly and completely describe the concept of this application and the technical effects produced in conjunction with the embodiments, so as to fully understand the purpose, features and effects of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments of this application, other embodiments obtained by those skilled in the art without paying creative work are within the scope of protection of this application. In the description of this application, greater than, less than, exceed, etc. are understood to exclude the number itself, and above, below, within, etc. are understood to include the number itself.

[0035] The experimental methods in the following examples, for which specific conditions are not specified, are generally performed in accordance with conventional conditions in the art or conditions recommended by the manufacturers; the raw materials and reagents used, unless otherwise specified, are all commercially available from conventional markets.

[0036] Example 1

[0037] A secondary battery preparation process is provided, comprising the following steps:

[0038] (1) Preparation of negative electrode sheet:

[0039] The negative electrode active material with a mass ratio of 95.5:1.1:2:1:0.4 (the mass fractions of graphite and SiO in the negative electrode active material are 90% and 10% respectively), single-walled carbon nanotubes (with an aspect ratio of 1000 and a specific surface area of ​​600m 2 / g), polyacrylic acid, SBR and sodium carboxymethyl cellulose, put into deionized water, stir and mix evenly to obtain a negative electrode slurry, and use a double-layer coater to coat the prepared negative electrode slurry on a single side of a copper foil (the lower layer is defined as the layer close to the copper foil, and the upper layer is defined as the layer away from the copper foil). The flow parameters of the feed pump of the extrusion die of the double-layer coater are adjusted to obtain upper and lower slurry layers with different coating surface densities. After baking and drying, rolling, slitting and cutting, a negative electrode sheet is obtained. In the negative electrode sheet, the surface density of the single-walled nanotubes close to the copper foil is 0.4 mg / 1540 mm 2 The surface density of single-walled nanotubes away from the copper foil is 0.3 mg / 1540 mm 2 The surface density of the negative electrode active material close to the copper foil is 180 mg / 1540 mm 2The surface density of the negative electrode active material away from the current collecting layer is 135mg / 1540mm 2 .

[0040] (2) Preparation of positive electrode: LiNi with a mass ratio of 97:1.5:1:0.5 0.8 Co 0.1 Mn 0.1 O2, PVDF5130, carbon black and carbon nanotubes are placed in N-methylpyrrolidone and mixed evenly to obtain a positive electrode slurry, which is then coated on both sides of an aluminum foil, and then baked, dried, rolled, slit and cut into pieces to obtain a positive electrode sheet.

[0041] (3) The positive electrode sheet, negative electrode sheet, and separator were wound to form a core, which was then encapsulated with aluminum-plastic film and baked under vacuum for 48 hours to remove moisture. The core was then filled with electrolyte and subjected to formation and volume separation to produce a soft-pack secondary battery. The resulting secondary battery had the parameters shown in Table 1.

[0042] Among them, the diaphragm adopts PP diaphragm;

[0043] The electrolyte was prepared as follows: ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed in a mass ratio of EC:PC:DEC = 2.5:3:5, and then LiPF6 was slowly added until the concentration of LiPF6 was 1 mol / L. Finally, 5% of the total weight of the electrolyte was added with fluoroethylene carbonate (FEC) and 0.5% of vinylene carbonate (VC).

[0044] Example 2

[0045] This embodiment prepares a secondary battery, which is different from the embodiment 1 only in that single-walled carbon nanotubes with an aspect ratio of 1500 are selected in step 1.

[0046] Example 3

[0047] This embodiment prepares a secondary battery, which is different from the embodiment 1 only in that single-walled carbon nanotubes with an aspect ratio of 3000 are selected in step 1.

[0048] Example 4

[0049] This embodiment prepares a secondary battery, which is different from the embodiment 1 only in that single-walled carbon nanotubes with an aspect ratio of 5000 are selected in step 1.

[0050] Example 5

[0051] This embodiment prepares a secondary battery, which is different from the embodiment 1 only in that single-walled carbon nanotubes with an aspect ratio of 10,000 are selected in step 1.

[0052] Example 6

[0053] This embodiment prepares a secondary battery, which differs from the embodiment 1 only in that: in step 1, the mass fraction b of SiO in the negative electrode active material is 5%, the mass fraction c of graphite is 95%, and the compacted density of the active material layer is 1.6 g / cm 3 .

[0054] Example 7

[0055] This embodiment prepares a secondary battery, which differs from the embodiment 3 only in that: in step 1, the mass fraction b of SiO in the negative electrode active material is 12%, the mass fraction c of graphite is 88%, and the compacted density of the active material layer is 1.8 g / cm 3 .

[0056] Example 8

[0057] This embodiment prepares a secondary battery, which is different from the embodiment 4 only in that: in step 1, the specific surface area of ​​the single-walled carbon nanotube is 900m 2 / g.

[0058] Example 9

[0059] This embodiment prepares a secondary battery which is different from the embodiment 4 only in that: in step 1, the specific surface area of ​​the single-walled carbon nanotube is 1100m 2 / g.

[0060] Example 10

[0061] This embodiment prepares a secondary battery, which differs from the embodiment 4 only in that: in step 1, the content of polyacrylic acid is adjusted to 1.7%, the specific surface area of ​​the single-walled carbon nanotube is 1200m 2 / g.

[0062] Example 11

[0063] This embodiment prepares a secondary battery which is different from the embodiment 4 only in that: in step 1, the content of polyacrylic acid is adjusted to 2.8%, the specific surface area of ​​the single-walled carbon nanotube is 1300m 2 / g.

[0064] Example 12

[0065] This embodiment prepares a secondary battery, which differs from the embodiment 4 only in that: polyacrylic acid is replaced by polymethacrylate, the content is 3.0%, and the specific surface area of ​​the single-walled carbon nanotube is 1450m 2 / g.

[0066] Example 13

[0067] This embodiment prepared a secondary battery, which differed from the embodiment 4 only in that: in step 1, the mass fraction b of SiO in the negative electrode active material was 5%, the mass fraction c of graphite was 95%, SBR was replaced by styrene-acrylic acid, and the content of polyacrylic acid was adjusted to 1.5%.

[0068] Examples 14 to 17

[0069] Examples 14 to 17 respectively prepare a secondary battery, which differs from Example 1 only in that the content of single-walled carbon nanotubes is adjusted to obtain negative electrode sheets with different conductive agent contents.

[0070] Comparative Example 1

[0071] In this comparative example, a negative electrode secondary battery was prepared, which differed from Example 1 only in that in step 1, the mass fraction b of SiO in the negative electrode active material was 3%, the mass fraction c of graphite was 97%, and the aspect ratio of the single-walled carbon nanotube was 700.

[0072] Comparative Example 2

[0073] In this comparative example, a negative electrode secondary battery was prepared, which differed from Example 1 only in that the negative electrode slurry was coated on only one side with a single layer.

[0074] Various parameters of the negative electrode sheets of the secondary batteries in the above embodiments and comparative examples are shown in Table 1. In the above embodiments, the aspect ratio of the conductive agent in the negative electrode sheet can be controlled by mechanical grinding, chemical etching, photolithography, or controlling the reaction time to control the length of the single-walled carbon nanotubes to achieve the aspect ratio, and the aspect ratio can be obtained by using a transmission electron microscope; the specific surface area can be controlled by adjusting different catalyst types, and the specific surface area value can be obtained by testing with a specific surface area tester.

[0075] Table 2

[0076] According to the data of the above-mentioned embodiment and comparative example, if the aspect ratio of the conductive agent particles, the relationship between the graphite content and the silicon-based material content satisfies: a:(c-7b)≥10, the secondary battery has excellent cycle performance and can reduce the DC resistance of the secondary battery, which is beneficial to the battery rate performance. In addition, according to the comparison of the data of Example 1 and Comparative Examples 1-2, it can be seen that if the surface density of the conductive agent on the side close to the current collecting layer is greater than the surface density on the side away from the current collecting layer, the battery DCR can be reduced, which is beneficial to the battery dynamic performance.

[0077] The embodiments of the present application have been described in detail above, but the present application is not limited to the above embodiments. Various modifications can be made within the scope of knowledge possessed by ordinary technicians in the relevant technical field without departing from the purpose of the present application. In addition, the embodiments of the present application and the features of the embodiments can be combined with each other unless there is a conflict.

Claims

1. A secondary battery, comprising a negative electrode sheet, the negative electrode sheet comprising a current collecting layer and a negative electrode active layer disposed on at least one side of the current collecting layer, the negative electrode active layer comprising a negative electrode active material and a conductive agent, the surface density of the conductive agent close to the current collecting layer is greater than the surface density of the conductive agent away from the current collecting layer, the aspect ratio of the conductive agent is a, the negative electrode active material comprises graphite and SiO x , 0<x≤2, the negative electrode active material SiO x The mass fraction of is b%, the mass fraction of graphite is c%, wherein a, b, and c satisfy the following: a:(c-7b)≥10.

2. The secondary battery according to claim 1, wherein a:(c-7b)<750.

3. The secondary battery according to claim 1, wherein The surface density of the negative electrode active material on a side close to the current collecting layer is greater than that on a side away from the current collecting layer.

4. The secondary battery according to claim 1, wherein 88≤c≤95, 5≤b≤12.

5. The secondary battery according to claim 1, wherein The conductive agent includes at least one of single-walled carbon nanotubes, carbon black, and vapor-phase carbon fibers, and the aspect ratio a of the conductive agent is (1000-10000):

1.

6. The secondary battery according to claim 5, wherein The diameter of the single-walled carbon nanotube is 0.5-100 nm.

7. The secondary battery according to claim 5, wherein The specific surface area of ​​the conductive agent is 600 to 1500 m 2 / g.

8. The secondary battery according to claim 1, wherein The negative electrode plate further includes a binder, which includes a polyacrylic acid material and a polystyrene material. In the negative electrode active layer, the mass content of the polyacrylic acid material is greater than that of the polystyrene material.

9. The secondary battery according to claim 8, wherein The polyacrylic acid material includes at least one of polyacrylic acid, polyacrylamide, polyacrylonitrile, polyacrylic acid salt or polyacrylic ester.

10. The secondary battery according to claim 8, wherein The polystyrene-based material includes at least one of styrene-butadiene rubber and styrene-acrylate.

11. The secondary battery according to claim 8, wherein The mass ratio of the polyacrylic acid material to the polystyrene material is (1.5-3):

1.

12. The secondary battery according to claim 1, wherein The compaction density of the negative electrode active material layer is 1.5 g / cm 3 ~1.8g / cm 3 .

13. The secondary battery according to claim 8, wherein Based on the mass of the negative electrode active layer, the mass percentage of the binder is 2% to 6%.

14. The secondary battery according to any one of claims 1 to 13, wherein The peeling force of the negative electrode sheet is 26 to 36 N / m. 15 . An electric device, comprising the secondary battery according to claim 1 , wherein the secondary battery is used as a power source of the electric device.

Citation Information

Patent Citations

  • Negative electrode material and preparation method thereof, negative electrode plate and lithium ion battery

    CN107946561A

  • Negative electrode material, negative electrode slurry, negative electrode plate and lithium ion battery

    CN111725509A

  • Silicon-based composite material for negative active material, negative plate and lithium ion battery

    CN112002883A

  • Secondary battery and application thereof

    CN116417658A

  • Negative electrode for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery using the same

    US20210384497A1

Cited By

  • Sodium-ion battery with wide temperature range and long service life as well as preparation method and application of sodium-ion battery

    CN120878944A

  • Negative pole piece and sodium ion battery

    CN121097017A

  • Secondary battery and electric device

    WO2026218905A1