Solar cell and manufacturing method therefor

By using a doped conductive layer containing oxygen and carbon elements in a crystalline silicon-based heterojunction cell to form a microcrystalline silicon layer with a high band gap, the problems of high cost and low photoelectric conversion efficiency are solved, and high-efficiency, low-power cost photoelectric conversion effect.

WO2024198703A1PCT designated stage expired Publication Date: 2024-10-03JA SOLAR TECH YANGZHOU

Patent Information

Application Number
PCT/CN2024/074933
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-01-31
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

At present, the preparation cost of crystalline silicon-based heterojunction cells is relatively high, which limits their large-scale market occupation, and the photoelectric conversion efficiency needs to be further improved to improve cost performance.

Method used

Using a doped conductive layer containing oxygen and carbon elements, by forming Si-O and Si-C chemical bonds, the bandgap width and doping element concentration of the conductive layer are adjusted, combined with microcrystalline silicon technology, to form a high bandgap width and low light The absorbent conductive layer improves battery efficiency.

Benefits of technology

It effectively reduces the light absorption rate of the conductive layer, improves the photoelectric conversion efficiency and cost performance of the battery, reduces the energy consumption of the preparation process, and reduces the cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024074933_03102024_PF_FP_ABST
    Figure CN2024074933_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a solar cell and a manufacturing method for same. At least some embodiments of the present disclosure provide a solar cell, comprising: a silicon substrate; a first passivation layer provided on a first side of the silicon substrate; and a first doped conductive layer provided on the first passivation layer, such that the first passivation layer is located between the silicon substrate and the first doped conductive layer. The first doped conductive layer contains an oxygen element and a carbon element, and contains a Si-O chemical bond and a Si-C chemical bond.
Need to check novelty before this filing date? Find Prior Art

Description

Solar cell and method for manufacturing the same

[0001] This application claims priority to Chinese patent application No. 202310322839.6, entitled “Solar cell unit and method for manufacturing the same,” filed on March 29, 2023. The contents of the Chinese patent application disclosure are hereby incorporated by reference in their entirety as a part of this application. Technical Field

[0002] The present disclosure relates to a solar cell unit and a method for manufacturing a solar cell unit. Background Art

[0003] A crystalline silicon heterojunction cell is a semiconductor device that converts sunlight into electrical output. Typically, a heterojunction cell is fabricated using an n-type silicon substrate. The cell comprises a silicon substrate, two passivation layers on either side of the silicon substrate, and a doped conductive layer on each of the passivation layers.

[0004] The preparation process is as follows: hydrogenated amorphous silicon layers are deposited on both sides of the textured silicon substrate, phosphorus- and boron-doped silicon layers are deposited on the surfaces of the hydrogenated amorphous silicon layers on both sides, a transparent conductive ITO layer is deposited on the surface of the doped silicon layer, and finally an electrode is formed on the ITO layer. Heterojunction batteries have many advantages: high battery efficiency, no attenuation, fewer process steps, low process energy consumption (temperature is below 300 degrees), etc. At this stage, the main factor limiting heterojunction batteries from occupying the market on a large scale is that the cost of their preparation is slightly higher than that of other photovoltaic cell products. Therefore, continuously improving the photoelectric conversion efficiency of heterojunction batteries and improving the cost-effectiveness of heterojunction batteries remain the development direction of heterojunction batteries.

[0005] Summary of the Invention

[0006] At least some embodiments of the present disclosure provide a solar cell unit comprising: a silicon substrate; a first passivation layer disposed on a first side of the silicon substrate; and a first doped conductive layer disposed on the first passivation layer such that the first passivation layer is located between the silicon substrate and the first doped conductive layer. The first doped conductive layer contains oxygen and carbon and includes Si-O and Si-C chemical bonds.

[0007] For example, in some embodiments, the total molar content of carbon and oxygen is 20-30%.

[0008] For example, in some embodiments, the first doped conductive layer contains silicon, oxygen, carbon, and hydrogen, and the molar content of carbon is 3-15%.

[0009] For example, in some embodiments, the carbon element exists by forming Si-C chemical bonds, CC chemical bonds, CO chemical bonds and CH chemical bonds, and the molar ratios of Si-C chemical bonds, CC chemical bonds, CO chemical bonds and CH chemical bonds in the total carbon content are 40-60%, 30-50%, 5-18% and 2-10%, respectively.

[0010] For example, in some embodiments, the first doped conductive layer contains silicon, oxygen, carbon, and hydrogen, and the molar content of oxygen is 10-30%.

[0011] For example, in some embodiments, oxygen elements exist by forming Si-O chemical bonds, CO chemical bonds, and PO chemical bonds, and the molar ratios of Si-O chemical bonds, CO chemical bonds, and PO chemical bonds in the total oxygen content are 70-90%, 6-18%, and 2-10%, respectively.

[0012] For example, in some embodiments, the bandgap of the first doped conductive layer is in the range of 1.9-2.4 eV.

[0013] For example, in some embodiments, the thickness of the first doped conductive layer is in the range of 6-14 nm.

[0014] For example, in some embodiments, in a direction toward the silicon substrate, the molar content of carbon in the first doped conductive layer gradually decreases, the molar content of oxygen in the first doped conductive layer gradually increases, and the molar content of doping elements in the first doped conductive layer gradually decreases.

[0015] For example, in some embodiments, the content of the doping element in the first doped conductive layer is between 2×10 18 -3×10 21 atoms per cubic centimeter.

[0016] For example, in some embodiments, at least a portion of the silicon component of the first doped conductive layer is crystallized.

[0017] For example, in some embodiments, the crystallinity of the first doped conductive layer is in the range of 40-70%.

[0018] For example, in some embodiments, the first doped conductive layer is a hydrogenated amorphous silicon layer with crystallized silicon embedded therein. Alternatively, the first doped conductive layer is a microcrystalline silicon layer that is only partially crystallized.

[0019] For example, in some embodiments, the crystallinity of the first doped conductive layer gradually decreases in a direction toward the silicon substrate.

[0020] For example, in some embodiments, the first doped conductive layer is an n-type conductive layer and contains silicon, oxygen, carbon, hydrogen, and phosphorus.

[0021] For example, in some embodiments, the silicon substrate is an n-type silicon substrate.

[0022] For example, in some embodiments, the first doped conductive layer is a p-type conductive layer and contains silicon, oxygen, carbon, hydrogen, and boron.

[0023] For example, in some embodiments, the solar cell unit further includes a second doped conductive layer disposed on the first doped conductive layer such that the first doped conductive layer is located between the first passivation layer and the second doped conductive layer.

[0024] For example, in some embodiments, the content of the doping element in the second doped conductive layer is 10 19 -10 21 atoms per cubic centimeter.

[0025] For example, in some embodiments, the solar cell unit further includes a second passivation layer disposed on the second side of the silicon substrate; and a third doped conductive layer disposed on the second passivation layer, such that the second passivation layer is located between the silicon substrate and the third doped conductive layer. At least the first side is a light-receiving side.

[0026] At least some embodiments of the present disclosure provide a method for manufacturing a solar cell, comprising: providing a silicon substrate; forming a first passivation layer on a first side of the silicon substrate; and forming a first doped conductive layer on the first passivation layer, such that the first passivation layer is located between the silicon substrate and the first doped conductive layer. During the formation of the first doped conductive layer, an oxygen-containing reaction gas and a carbon-containing reaction gas are used, such that the first doped conductive layer contains Si-O chemical bonds and Si-C chemical bonds.

[0027] For example, in some embodiments, the oxygen-containing reaction gas is selected from one or more of N2O, O2, CO2, and CO.

[0028] For example, in some embodiments, the carbon-containing reaction gas is selected from CH4, C2H6, C3H 10 and one or more of C2H4.

[0029] For example, in some embodiments, phosphine gas is used when forming the first doped conductive layer, so that the first doped conductive layer is doped with phosphorus element.

[0030] For example, in some embodiments, when forming the first doped conductive layer, PH3 gas and SiH4 gas are used, and the flow ratio of the PH3 gas to the SiH4 gas is 0.02-0.1.

[0031] For example, in some embodiments, the first doped conductive layer is formed by plasma enhanced chemical vapor deposition, wherein a radio frequency (RF) power source or a very high frequency (VHF) power source is used as a plasma excitation source, and the ion source energy density is 100-600 mW / cm 2 , the deposition pressure is in the range of 0.4-5 Torr, and the deposition temperature is in the range of 130-230°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] FIG1 shows a portion of the light-receiving side of a solar cell unit;

[0033] FIG2 shows a portion of the light-receiving side of another solar cell unit;

[0034] FIG3 shows the effect of using gases with different oxygen-to-silicon ratios and carbon-to-silicon ratios on the phosphorus content in the microcrystalline silicon doped conductive layer when forming the microcrystalline silicon doped conductive layer;

[0035] FIG4 shows a schematic diagram of a solar cell unit according to an embodiment of the present disclosure;

[0036] FIG5 shows the thickness and bandgap values ​​of four doped conductive layer samples formed using different reaction gases;

[0037] FIG6 shows the phosphorus doping concentrations in Samples 3 and 4 in FIG5 ;

[0038] 7 and 8 respectively show the results of X-ray photoelectron spectroscopy (XPS) analysis of carbon and silicon elements in the first doped conductive layer of the solar cell unit according to Example 1;

[0039] FIG. 9 shows a comparison of the performance of the solar cell units according to Comparative Example 1 and Example 2. FIG. DETAILED DESCRIPTION

[0040] Hereinafter, a solar cell unit and a method for manufacturing the same according to embodiments of the present disclosure will be described in detail with reference to the accompanying drawings.

[0041] Figure 1 shows a portion of the light-receiving side of a solar cell. This solar cell is a silicon-based heterojunction cell. As shown in Figure 1, the solar cell comprises a silicon substrate 101, an intrinsic hydrogenated amorphous silicon passivation layer 102 disposed on one surface of the silicon substrate 101, and an amorphous silicon doped conductive layer 103 deposited on the intrinsic hydrogenated amorphous silicon passivation layer 102. The inner intrinsic hydrogenated amorphous silicon passivation layer passivates the surface of the silicon substrate 101. The outer amorphous silicon doped conductive layer 103, through its own doping, bends the energy band, enabling the extraction and transmission of corresponding carriers. Because amorphous silicon has a band gap of approximately 1.6-1.7 eV and is a material with a direct band gap, the amorphous silicon layer strongly absorbs short-wavelength light. If the amorphous silicon doped conductive layer 103 is used on the light-receiving side of the heterojunction cell, current loss will obviously occur due to the absorption of light by the amorphous silicon doped conductive layer 103. Using wide bandgap materials on the light-receiving side of heterojunction cells to reduce light absorption is an effective way to improve cell conversion efficiency.

[0042] Figure 2 shows a portion of the light-receiving side of another solar cell. As shown in Figure 2, the solar cell comprises a silicon substrate 201, an intrinsic hydrogenated amorphous silicon passivation layer 202 disposed on a surface of the silicon substrate 201, and a microcrystalline silicon doped conductive layer 203 deposited on the intrinsic hydrogenated amorphous silicon passivation layer 202. During the conductive layer preparation process, at least a portion of the amorphous silicon doped conductive layer is crystallized to transform into the microcrystalline silicon doped conductive layer 203. This converts at least a portion of the direct bandgap material into an indirect bandgap material, reducing light absorption. Furthermore, the crystallized microcrystalline silicon doped conductive layer 203 also increases the concentration of dopant atoms. This technology is called silicon thin film microcrystallization technology. For example, when forming the doped conductive layer via plasma-enhanced chemical vapor deposition (PECVD), crystallization of the amorphous silicon doped conductive layer is achieved by increasing the H2 / SiH4 flow ratio, and the crystallization rate increases with increasing H2 / SiH4 flow ratio. However, the bandgap of the crystallized microcrystalline silicon doped conductive layer 203 is close to that of crystalline silicon, which also increases light absorption. Furthermore, when the microcrystalline silicon doped conductive layer 203 is deposited, oxygen elements are introduced into the microcrystalline silicon doped conductive layer 203 by introducing an oxygen-containing gas such as N2O, so that at least a portion of the silicon elements form Si-O chemical bonds, thereby increasing the band gap width of the microcrystalline silicon doped conductive layer 203.

[0043] Figure 3 shows the effect of using different oxygen-to-silicon ratio gases (O2 / SiH4) and carbon-to-silicon ratio gases (CH4 / SiH4) when forming the microcrystalline silicon doped conductive layer 203 on the phosphorus content in the microcrystalline silicon doped conductive layer 203. The oxygen-to-silicon ratio and carbon-to-silicon ratio of the gases can be roughly considered to be the oxygen-to-silicon ratio and carbon-to-silicon ratio in the microcrystalline silicon doped conductive layer 203. As shown in Figure 3, as the oxygen content in the microcrystalline silicon doped conductive layer 203 increases, the content of doping elements (such as phosphorus and boron) in the conductive layer gradually decreases. Excessive oxygen content is detrimental to the extraction and conduction of carriers by the microcrystalline conductive layer. Therefore, the oxygen content in the microcrystalline silicon doped conductive layer 203 cannot exceed a certain value. The oxygen content in the microcrystalline silicon doped conductive layer 203 controls the band gap width and impurity doping concentration of the conductive layer. On the one hand, a higher oxygen content is required to reduce light absorption in the conductive layer and increase the band gap width of the material. On the other hand, to improve the conductivity of the conductive layer and increase the content of doping impurities in the conductive layer, the oxygen content in the conductive layer needs to be reduced.

[0044] An embodiment of the present disclosure provides a solar cell unit comprising a microcrystalline silicon doped conductive layer. The microcrystalline silicon doped conductive layer is doped with doping elements so that the conductive layer has excellent conductive properties, and the conductive layer also includes oxygen and carbon elements so that the conductive layer has a higher band gap and a lower absorption rate of light. As shown in FIG3 , the carbon content in the conductive layer has little effect on the doping element content. By increasing the carbon element and adjusting the ratio of the carbon element to the oxygen element, the band gap can be increased and the absorption of light can be reduced while avoiding the reduction of the doping element concentration in the conductive layer due to too high an oxygen content.

[0045] FIG4 shows a schematic diagram of a solar cell according to an embodiment of the present disclosure. As shown in FIG4 , the solar cell includes a silicon substrate 301, a first passivation layer 302 disposed on a first side of the silicon substrate 301, a first doped conductive layer 303 disposed on the first passivation layer 302, a second doped conductive layer 304 disposed on the first doped conductive layer 303, a first transparent conductive layer 308 disposed on the second doped conductive layer 304, a first electrode 3091 disposed on the first transparent conductive layer 308, a second passivation layer 305 disposed on a second side of the silicon substrate 301, a third doped conductive layer 306 disposed on the second passivation layer 305, a second transparent conductive layer 307 disposed on the third doped conductive layer 306, and a second electrode 3092 disposed on the second transparent conductive layer 307. The first side is the light-receiving side of the solar cell.

[0046] The silicon substrate 301 is an n-type silicon substrate 301. The first passivation layer 302 and the second passivation layer 305 are intrinsic hydrogenated amorphous silicon layers. The first doped conductive layer 303 is a hydrogenated microcrystalline silicon doped conductive layer doped with phosphorus atoms and contains Si-O chemical bonds and Si-C chemical bonds. The second doped conductive layer 304 is a hydrogenated amorphous silicon doped conductive layer doped with phosphorus atoms and substantially does not contain Si-O chemical bonds and Si-C chemical bonds. The third doped conductive layer 306 is a hydrogenated amorphous silicon doped conductive layer doped with boron. The first transparent conductive layer 308 and the second transparent conductive layer 307 are ITO layers. The first electrode 3091 and the second electrode 3092 are silver electrodes.

[0047] In the first doped conductive layer 303, Si-Si chemical bonds, Si-O chemical bonds, and Si-C chemical bonds serve as the conductive layer network formers, hydrogen elements serve as network modifiers to passivate dangling bonds in the saturated conductive layer, and phosphorus atoms serve as doping elements to impart excellent conductivity to the conductive layer. This conductive layer has a wide bandgap (e.g., Eg = 1.9-2.4 eV) and good carrier conduction capability. For example, the thickness of the first doped conductive layer 303 is in the range of 6-14 nm.

[0048] Since the first doped conductive layer 303 contains Si-O chemical bonds and Si-C chemical bonds, the introduction of carbon elements avoids the reduction of the doping element concentration in the conductive layer due to too high oxygen content, thereby achieving a conductive layer with excellent conductive properties while having a higher band gap width and lower light absorption rate.

[0049] The total content of carbon and oxygen in the first doped conductive layer 303 can be in the range of 20-30%. The molar content of carbon can be in the range of 3-15%. The molar content of oxygen can be in the range of 10-30%. Increasing the total content of carbon and oxygen in the conductive layer can increase the band gap of the conductive layer and reduce the absorption of incident light. Maintaining the total content of carbon and oxygen in the conductive layer, increasing the carbon content in the conductive layer, and decreasing the oxygen content in the conductive layer can increase the phosphorus doping concentration in the conductive layer.

[0050] The carbon element may exist by forming Si-C chemical bonds, CC chemical bonds, CO chemical bonds and CH chemical bonds, and the molar proportions of these chemical bonds in the total carbon content may be in the ranges of 40-60%, 30-50%, 5-18% and 2-10%, respectively.

[0051] The oxygen element can exist by forming Si-O chemical bonds, CO chemical bonds and PO chemical bonds, and the molar proportions of these chemical bonds in the total oxygen content are 70-90%, 6-18% and 2-10% respectively.

[0052] The contents of carbon, oxygen, and silicon in the first doped conductive layer 303 may be gradually changed. For example, in the direction toward the silicon substrate 301, the molar content of carbon in the first doped conductive layer 303 may gradually decrease, the molar content of oxygen in the first doped conductive layer 303 may gradually increase, and the molar content of doping elements in the first doped conductive layer 303 may gradually decrease. For example, the content of phosphorus in the first doped conductive layer 303 may be between 2×10 18 - 3×10 21 atoms per cubic centimeter.

[0053] As used herein, a microcrystalline silicon doped conductive layer refers to a silicon conductive layer in which at least a portion of the silicon component is crystallized. For example, at least a portion of the silicon component of the first doped conductive layer 303 is crystallized, and its crystallization rate can be in the range of 40-70%. The crystallization rate of the first doped conductive layer 303 can gradually decrease toward the silicon substrate 301. In this embodiment, the first doped conductive layer 303 is a hydrogenated amorphous silicon layer having crystallized silicon embedded therein.

[0054] The second doped conductive layer 304 can be an amorphous conductive layer doped with high concentration of phosphorus. The second doped conductive layer 304 has good coverage on the first doped conductive layer 303, which can prevent the subsequent high temperature process from causing a decrease in the concentration of phosphorus atoms.

[0055] In addition, the present disclosure is not limited to this. The silicon substrate 301 can be a p-type silicon substrate 301. The first passivation and / or second passivation layer 305 can be other types of passivation layers. For example, the first passivation layer 302 and the second passivation layer 305 can be composed of a passivation stack, and an amorphous silicon layer and a hydrogenated silicon layer can be arranged in sequence in the direction away from the silicon substrate 301. The first doped conductive layer 303 can be a hydrogenated microcrystalline silicon doped conductive layer doped with boron atoms and containing Si-O chemical bonds and Si-C chemical bonds. In addition, the second doped conductive layer 304 can also be omitted. In addition, the third doped conductive layer 306 can be a hydrogenated microcrystalline silicon doped conductive layer similar to the first doped conductive layer 303 and contain Si-O chemical bonds and Si-C chemical bonds, which is particularly advantageous when the second side is also the light-receiving side of the solar cell unit.

[0056] The embodiments of the present disclosure provide a method for manufacturing a solar cell unit, which can be used to manufacture the solar cell unit described above. The method comprises the following steps:

[0057] Step S11 , providing a silicon substrate 301 .

[0058] In step S12 , a first passivation layer 302 and a second passivation layer 305 are formed on two opposite surfaces of the silicon substrate 301 .

[0059] In step S13 , a first doped conductive layer 303 is formed on the first passivation layer 302 on the first side of the silicon substrate 301 using an oxygen-containing reaction gas and a carbon-containing reaction gas, so that the first doped conductive layer contains Si—O chemical bonds and Si—C chemical bonds.

[0060] Step S14 , forming a second doped conductive layer 304 on the first doped conductive layer 303 of the silicon substrate 301 .

[0061] Step S15 , forming a third doped conductive layer 306 on the second passivation layer 305 on the second side of the silicon substrate 301 .

[0062] Step S16 , forming a transparent conductive layer on the first doped conductive layer 303 and the third doped conductive layer 306 , respectively.

[0063] Step S17 , forming electrodes, such as silver electrodes, on the transparent conductive layers on both sides respectively.

[0064] In step S13, the oxygen-containing reaction gas may be selected from the group consisting of N2O, O2, CO2 and CO, and the carbon-containing reaction gas may be selected from the group consisting of CH4, C2H6, C3H 10 and C2H4. Furthermore, phosphine gas may be used to dope the first doped conductive layer with phosphorus. More specifically, PH3 gas and SiH4 gas may be used, with a flow ratio of PH3 gas to SiH4 gas of 0.02-0.1, so that the formed hydrogenated amorphous silicon layer is at least partially crystallized.

[0065] In one example, the first doped conductive layer is formed using a PECVD process, wherein a radio frequency (RF) power source or a very high frequency (VHF) power source is used as a plasma excitation source, and the ion source energy density is 100-600 mW / cm 2 , the deposition pressure is in the range of 0.4-5 Torr, and the deposition temperature is in the range of 130-230°C.

[0066] Figure 5 shows the thickness and bandgap values ​​of four doped conductive layer samples formed using different reaction gases. Each sample was formed on a polished silicon substrate by a PECVD process. The reaction conditions of sample 1 were: deposition pressure (i.e., the pressure in the reaction chamber where the sample was located during deposition) was 133 Pa, the RF power was 2000 W, the reaction gases were SiH4, H2, and PH3, with flow rates of 2000 sccm, 2000 sccm, and 200 sccm, respectively, and the deposition time was 8 min. The reaction conditions of sample 2 were: deposition pressure was 153 Pa, the RF power was 4000 W, the reaction gases were SiH4, H2, and PH3, with flow rates of 1000 sccm, 50 SLM, and 100 sccm, respectively, and the deposition time was 15 min. The reaction conditions for Sample 3 were: deposition pressure of 163 Pa, RF power of 4500 W, reactant gases of SiH4, H2, PH3, and CO2, with flow rates of 1000 sccm, 50 SLM, 100 sccm, and 2000 sccm, respectively, and deposition time of 15 min. The reaction conditions for Sample 4 were: deposition pressure of 183 Pa, RF power of 5000 W, reactant gases of SiH4, H2, PH3, CH4, and CO2, with flow rates of 1000 sccm, 50 SLM, 100 sccm, 500 sccm, and 1000 sccm, respectively, and deposition time of 15 min.

[0067] It can be seen from FIG5 that samples 3 and 4 have wider band gaps.

[0068] FIG6 shows the phosphorus doping concentrations in Sample 3 and Sample 4 in FIG5. As shown in FIG6, at a doping depth of 0 to about 0.13 μm, the doping concentration of Sample 4 is about 1×10 20 atoms / cm3, the doping concentration of sample 3 is about 1×10 19 atoms / cm3, sample 4 has a higher concentration of phosphorus doping than sample 3.

[0069] The performances of the solar cell units according to Comparative Example 1, Comparative Example 2, and the three embodiments (Example 1, Example 2, and Example 3) of the present disclosure will be compared below.

[0070] The solar cell unit according to Comparative Example 1 was prepared by the following steps:

[0071] Step S21: providing a silicon substrate, which is a single crystal n-type silicon substrate with a bulk resistivity of 3.5 Ω·cm.

[0072] Step S22 , performing surface texturing on the silicon substrate, specifically, using a sodium hydroxide alkaline solution with a mass fraction of 5% to anisotropically etch the silicon substrate to obtain a textured silicon substrate surface with a reflectivity of no more than 12%.

[0073] Step S23: Form a first passivation layer and a second passivation layer on opposite surfaces of the silicon substrate. Specifically, a 10 nm thick hydrogenated amorphous silicon layer is formed on opposite surfaces of the silicon substrate using a PECVD process. The simulated open circuit voltage of the double-sided passivated silicon substrate reaches 750 mV.

[0074] Step S24: Form a phosphorus-doped hydrogenated amorphous silicon layer as a first doped conductive layer on the first passivation layer on the first side of the silicon substrate. Specifically, a PECVD process is used to deposit the phosphorus-doped hydrogenated amorphous silicon layer on the hydrogenated amorphous silicon layer on one side of the silicon substrate using a reaction gas composed of SiH₄, H₂, and PH₃. The phosphorus-doped hydrogenated amorphous silicon layer has a thickness of 15 nm.

[0075] In step S25, a boron-doped hydrogenated amorphous silicon layer is formed on the second passivation layer on the second side of the silicon substrate as a third doped conductive layer. Specifically, a PECVD process is used using a reaction gas composed of SiH₄, H₂, and B₂H₆ to deposit the boron-doped hydrogenated amorphous silicon layer on the surface of the hydrogenated amorphous silicon film on the other side of the silicon substrate. The boron-doped hydrogenated amorphous silicon layer has a thickness of 15 nm.

[0076] In step S26 , a PVD device is used to deposit an ITO transparent conductive film layer with a thickness of 80 nm on the phosphorus-doped hydrogenated amorphous silicon layer and the boron-doped hydrogenated amorphous silicon layer on both sides of the silicon substrate.

[0077] Step S27 , using low-temperature silver paste to form silver electrodes on the ITO transparent conductive film layer on both sides of the silicon substrate by printing and curing at 255° C.

[0078] The solar cell unit according to Comparative Example 2 was prepared similarly to the solar cell unit according to Comparative Example 1, with the only difference being step S24. During the preparation of the solar cell unit according to Comparative Example 2, in step S24, a phosphorus-doped hydrogenated microcrystalline silicon layer was deposited on the hydrogenated amorphous silicon layer on one side of the silicon substrate using a PECVD process using a reaction gas composed of SiH4, H2, and PH3, as a first doped conductive layer. In this step, the chamber pressure was set to 153 Pa, the RF power was set to 4000 W, and 1000 sccm SiH4, 50 SLM H2, and 100 sccm PH3 were introduced. The phosphorus-doped hydrogenated microcrystalline silicon layer had a thickness of 15 nm. A phosphorus-doped hydrogenated amorphous silicon layer was then deposited on the phosphorus-doped hydrogenated microcrystalline silicon layer using a PECVD process using a reaction gas composed of SiH4, H2, and PH3, as an additional second doped conductive layer. The phosphorus-doped hydrogenated amorphous silicon layer had a thickness of 3 nm.

[0079] The solar cell according to Example 1 was prepared similarly to the solar cell according to Comparative Example 1, differing only in step S24. During the preparation of the solar cell according to Example 1, in step S24, a phosphorus-doped hydrogenated microcrystalline carbon oxide layer was deposited as a first doped conductive layer on the first passivation layer on one side of the silicon substrate using a PECVD process using a reaction gas composed of SiH4, H2, CO2, CH4, and PH3. The thickness of this phosphorus-doped hydrogenated microcrystalline carbon oxide layer was 15 nm. A phosphorus-doped hydrogenated amorphous silicon layer was then deposited as an additional second doped conductive layer on this hydrogenated microcrystalline carbon oxide layer using a PECVD process using a reaction gas composed of SiH4, H2, and PH3. The thickness of this phosphorus-doped hydrogenated amorphous silicon layer was 3 nm.

[0080] Figures 7 and 8 show the results of X-ray photoelectron spectroscopy analysis of carbon and silicon in the first doped conductive layer of the solar cell according to Example 1. As shown in Figures 7 and 8 , the first doped conductive layer contains carbon, silicon, and oxygen, with the oxygen and a portion of the carbon forming Si-O and Si-C chemical bonds.

[0081] The solar cell according to Example 2 was prepared similarly to the solar cell according to Example 1, differing only in step S24. In step S24, a phosphorus-doped hydrogenated microcrystalline carbon oxide layer was deposited as a first doped conductive layer on the first passivation layer on one side of a silicon substrate using a PECVD process using a reaction gas composed of SiH4, H2, CO2, CH4, and PH3. The flow ratio of CH4 to SiH4 was gradually increased from 0.05 to 1.5, while the flow ratio of CO2 to SiH4 was gradually decreased from 1.5 to 0.5, from an inner position close to the silicon substrate to an outer position away from the silicon substrate. This formed a first doped conductive layer in which the total carbon and oxygen contents remained constant, but the carbon content gradually increased and the oxygen content gradually decreased in a direction away from the silicon substrate. The phosphorus-doped hydrogenated microcrystalline carbon oxide layer had a thickness of 15 nm. Then, a phosphorus-doped hydrogenated amorphous silicon layer is deposited on the hydrogenated microcrystalline carbon oxide silicon layer using a PECVD process using a reaction gas composed of SiH4, H2 and PH3 as an additional second doped conductive layer. The phosphorus-doped hydrogenated amorphous silicon layer has a thickness of 3 nm.

[0082] The solar cell according to Example 3 was prepared similarly to the solar cell according to Example 1, differing only in step S24. During the preparation of the solar cell according to Example 3, in step S24, a phosphorus-doped hydrogenated microcrystalline carbon oxide layer was deposited as a first doped conductive layer on the first passivation layer on one side of the silicon substrate using a PECVD process using a reaction gas composed of SiH4, H2, CO2, CH4, and PH3. The thickness of this phosphorus-doped hydrogenated microcrystalline carbon oxide layer was 15 nm. However, in the solar cell according to Example 3, a phosphorus-doped hydrogenated amorphous silicon layer was not deposited as an additional second doped conductive layer on this hydrogenated microcrystalline carbon oxide layer.

[0083] FIG. 9 shows a performance comparison of solar cell units according to Comparative Example 1, Comparative Example 2, Example 1, Example 2, and Example 3. FIG. As shown in FIG9 , when the open-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of the solar cell unit according to Comparative Example 1 are 100% respectively, the open-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of the solar cell unit according to Comparative Example 2 are 97.81%, 100.40%, 101.501%, and 99.67% respectively; the open-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of the solar cell unit according to Example 1 are 101.10%, 100.20%, 101.01%, and 102.64% respectively; the open-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of the solar cell unit according to Example 2 are 101.20%, 100.30%, 101.46%, and 102.98% respectively; and the open-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of the solar cell unit according to Example 3 are 101.30%, 100.30%, 100.76%, and 101.34% respectively. Compared to the solar cell unit of Comparative Example 1, the solar cell unit of Comparative Example 2 has a higher open circuit voltage and fill factor, but lower short circuit current and photoelectric conversion efficiency. In Comparative Example 2, since the first doped conductive layer is not doped with oxygen and carbon, the concentration of active phosphorus atoms in the first doped conductive layer is increased. Therefore, although the passivation performance and fill factor are improved, the band gap value of the phosphorus-doped microcrystalline silicon film layer is small, which has an absorption effect on light of a larger wavelength band, thereby reducing the short circuit current. For heterojunction cells with excellent passivation, the current plays a decisive role in the photoelectric conversion efficiency of the cell. As can be seen from Figure 9, it is difficult to improve the cell efficiency simply by microcrystallization. Therefore, it is necessary to further dope oxygen and carbon in the first doped conductive layer to increase the band gap value of the microcrystalline film layer. Compared to the solar cell unit according to Comparative Example 1, the solar cell units of Examples 1-3 have higher short circuit current, open circuit voltage, fill factor and photoelectric conversion efficiency. And compared to the solar cell unit according to Comparative Example 2, the solar cell units of Examples 1-3 have higher short circuit current and photoelectric conversion efficiency. Therefore, compared to a phosphorus-doped hydrogenated amorphous silicon layer or a phosphorus-doped hydrogenated microcrystalline silicon layer that does not contain Si-O and Si-C chemical bonds as the first doped conductive layer, a phosphorus-doped hydrogenated microcrystalline carbon oxide silicon layer that contains Si-O and Si-C chemical bonds as the first doped conductive layer is beneficial for improving the performance of the battery cell. Compared to the solar cell according to Example 1, the solar cell according to Example 2 has a higher short-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency. Therefore, a first doped conductive layer in which the carbon content gradually increases and the oxygen content gradually decreases in the direction away from the silicon substrate is beneficial for improving the performance of the battery cell.The solar cell according to Example 1 has a higher photoelectric conversion efficiency than the solar cell according to Example 3. Therefore, forming the second doped conductive layer is beneficial to improving the performance of the solar cell.

[0084] The scope of the present disclosure is not limited by the above-described embodiments but by the appended claims and their equivalents.

Claims

1. A solar cell unit, include: Silicon substrate; a first passivation layer disposed on a first side of the silicon substrate; as well as A first doped conductive layer is disposed on the first passivation layer, so that the first passivation layer is located between the silicon substrate and the first doped conductive layer, wherein: The first doped conductive layer contains oxygen and carbon, and includes Si—O chemical bonds and Si—C chemical bonds.

2. The solar cell unit according to claim 1, in, The total molar content of the carbon element and the oxygen element is 20-30%.

3. The solar cell unit according to claim 1 or 2, in, The first doped conductive layer contains silicon, oxygen, carbon and hydrogen, and the molar content of the carbon element is 3-15%.

4. The solar cell unit according to any one of claims 1 to 3, in, The carbon element exists by forming Si-C chemical bonds, CC chemical bonds, CO chemical bonds and CH chemical bonds, and the molar proportions of the Si-C chemical bonds, the CC chemical bonds, the CO chemical bonds and the CH chemical bonds in the total carbon content are 40-60%, 30-50%, 5-18% and 2-10% respectively.

5. The solar cell unit according to any one of claims 1 to 4, in, The first doped conductive layer contains silicon, oxygen, carbon and hydrogen, and the molar content of the oxygen is 10-30%.

6. The solar cell unit according to any one of claims 1 to 5, in, The oxygen element exists by forming Si-O chemical bonds, CO chemical bonds and PO chemical bonds, and the molar proportions of the Si-O chemical bonds, the CO chemical bonds and the PO chemical bonds in the total oxygen content are 70-90%, 6-18% and 2-10% respectively.

7. The solar cell unit according to any one of claims 1 to 6, in, The bandgap width of the first doped conductive layer is in the range of 1.9-2.4 eV.

8. The solar cell unit according to any one of claims 1 to 7, in, The thickness of the first doped conductive layer is in the range of 6-14 nm.

9. The solar cell unit according to any one of claims 1 to 8, in, In the direction toward the silicon substrate, the molar content of the carbon element of the first doped conductive layer gradually decreases, the molar content of the oxygen element of the first doped conductive layer gradually increases, and the molar content of the doping element of the first doped conductive layer gradually decreases.

10. The solar cell unit according to any one of claims 1 to 9, in, The content of the doping element in the first doped conductive layer is 2×10 18 -3×10 21 atoms per cubic centimeter.

11. The solar cell unit according to any one of claims 1 to 10, in, At least a portion of the silicon component of the first doped conductive layer is crystallized.

12. The solar cell unit according to claim 11, in, The crystallinity rate of the first doped conductive layer is in the range of 40-70%.

13. The solar cell unit according to claim 12, in, The first doped conductive layer is a hydrogenated amorphous silicon layer in which crystallized silicon is embedded.

14. The solar cell unit according to any one of claims 11 to 13, in, In a direction toward the silicon substrate, the crystallization rate of the first doped conductive layer gradually decreases.

15. The solar cell unit according to any one of claims 1 to 14, in, The first doped conductive layer is an n-type conductive layer and contains silicon, oxygen, carbon, hydrogen and phosphorus.

16. The solar cell unit according to claim 15, in, The silicon substrate is an n-type silicon substrate.

17. The solar cell unit according to any one of claims 1 to 5 and 7 to 14, in, The first doped conductive layer is a p-type conductive layer and contains silicon, oxygen, carbon, hydrogen and boron.

18. The solar cell unit according to any one of claims 1 to 17, further comprising The second doped conductive layer is disposed on the first doped conductive layer, so that the first doped conductive layer is located between the first passivation layer and the second doped conductive layer.

19. The solar cell unit according to claim 18, in, The content of the doping element in the second doped conductive layer is 10 19 -10 21 atoms per cubic centimeter.

20. The solar cell unit according to any one of claims 1 to 19, further comprising a second passivation layer disposed on a second side of the silicon substrate; and a third doped conductive layer, which is disposed on the second passivation layer, so that the second passivation layer is located between the silicon substrate and the third doped conductive layer, wherein At least the first side is a light receiving side.

21. A method for manufacturing a solar cell unit, include: providing a silicon substrate; forming a first passivation layer on a first side of the silicon substrate; as well as A first doped conductive layer is formed on the first passivation layer, so that the first passivation layer is located between the silicon substrate and the first doped conductive layer, wherein: When forming the first doped conductive layer, an oxygen-containing reaction gas and a carbon-containing reaction gas are used, so that the first doped conductive layer contains Si—O chemical bonds and Si—C chemical bonds.

22. The manufacturing method according to claim 21, in, The oxygen-containing reaction gas is selected from N 2 O, O 2 , CO 2 and CO.

23. The manufacturing method according to claim 21 or 22, in, The carbon-containing reaction gas is selected from CH 4 , C 2 H 6 , C 3 H 10 and C 2 H 4 One or more of .

24. The manufacturing method according to any one of claims 21 to 23, in, When forming the first doped conductive layer, phosphine gas is used so that the first doped conductive layer is doped with phosphorus element.

25. The manufacturing method according to any one of claims 21 to 24, in, When forming the first doped conductive layer, PH 3 Gas and SiH 4 Gas, the pH 3 Gas and the SiH 4 The gas flow ratio is 0.02-0.

1.

26. The manufacturing method according to any one of claims 21 to 25, in, The first doped conductive layer is formed by plasma enhanced chemical vapor deposition, wherein a radio frequency power source or a very high frequency power source is used as a plasma excitation source, and the ion source energy density is 100-600 mW / cm 2 , the deposition pressure is in the range of 0.4-5 Torr, and the deposition temperature is in the range of 130-230°C.

Citation Information

Patent Citations

  • Solar cell and method for manufacturing same

    CN116344653A

  • Solar cell

    CN102473776A

  • Heterojunction cell preparation method and heterojunction cell

    CN113363340A

  • Heterojunction solar cell and manufacturing method thereof

    CN114566561A

  • Silicon heterojunction solar cell and photovoltaic module with novel projecting pole

    CN205920977U

Cited By

  • TOPCon solar cell, preparation method thereof and photovoltaic module

    CN120344029A