Back-contact battery, manufacturing method therefor, and photovoltaic module

By arranging an insulating layer on the outer surface of the second semiconductor layer to span the side edges of the second semiconductor opening area, the problem of leakage in the back contact battery is solved, the battery efficiency and yield are improved, and the preparation process is simplified.

WO2024199002A1PCT designated stage expired Publication Date: 2024-10-03GOLD STONE (FUJIAN) ENERGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/082388
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current back-contact batteries are prone to leakage at the side edges of the second semiconductor opening area, resulting in reduced battery efficiency and yield, and complicated preparation processes.

Method used

An insulating layer is provided on the outer surface of the second semiconductor layer. The insulating layer spans the side edges of the second semiconductor opening area and extends at an appropriate proportion to avoid leakage and simplify the preparation process.

Benefits of technology

It effectively avoids leakage, improves the parallel resistance and conversion efficiency of the battery, improves the battery yield, and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082388_03102024_PF_FP_ABST
    Figure CN2024082388_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure belongs to the technical field of back-contact batteries, and in particular relates to a back-contact battery, a manufacturing method therefor, and a photovoltaic module. The back-contact battery comprises a silicon substrate provided with a front surface and a back surface, a first semiconductor layer which is disposed on the back surface and is provided with a second semiconductor opening region, and a second semiconductor layer. The back-contact battery also comprises a plurality of insulating layers arranged at intervals in the X-axis direction of the back surface. The insulating layers are arranged on the outer surface of the second semiconductor layer. Furthermore, in the X-axis direction, the insulating layers traverse a side edge of the second semiconductor opening region and the two ends of the insulating layers each extend. The traversing length W12 of the insulating layers on the second semiconductor opening region and the traversing length W11 of the insulating layers on the first semiconductor layer satisfy W12:W11=0.1-10:1. According to the back-contact battery disclosed by the present disclosure, the phenomenon of electrical leakage occurring at the side edge of the second semiconductor opening region can be effectively prevented at the same time, battery efficiency and battery yield are excellent, and the preparation process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Back contact battery, manufacturing method thereof, and photovoltaic module

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This disclosure claims priority to Chinese patent application number 2023103322311 filed with the Chinese Patent Office on March 31, 2023, entitled “A back-contact cell, its manufacturing method, and photovoltaic module,” the entire contents of which are incorporated by reference into this disclosure. Technical Field

[0003] The present disclosure belongs to the technical field of back-contact cells, and in particular relates to a back-contact cell, a manufacturing method thereof, and a photovoltaic module. Background Art

[0004] Currently, existing back-contact cells have either a conventional heterojunction passivation structure or a combined passivation structure. In the combined passivation structure, the first passivation layer of the first semiconductor layer is passivated using a tunneling oxide layer, while the second passivation layer of the second semiconductor layer is passivated using an intrinsic silicon layer. This structure offers superior cell performance compared to conventional heterojunction passivation. Furthermore, existing back-contact cells both have a second semiconductor opening region defined in the first semiconductor layer to accommodate a portion of the second semiconductor layer, and a first semiconductor opening region defined in the second semiconductor layer to expose a portion of the first semiconductor layer. These are configured to form two emitters when combined with metal electrodes.

[0005] However, a serious leakage short circuit phenomenon is prone to occur at the side edge of the second semiconductor opening area (i.e., the Z-axis contact interface between the first semiconductor layer and the second semiconductor layer), thereby reducing the parallel resistance of the battery and further reducing the battery efficiency and battery yield.

[0006] CN115588698A provides a back-contact solar cell, a method for manufacturing the same, and a photovoltaic module. The back-contact solar cell comprises: a silicon substrate; a first semiconductor layer, a second semiconductor layer, and a first insulating layer located on a first surface of the silicon substrate; a first portion of the second semiconductor layer alternating with the first semiconductor layer with a gap therebetween; a second portion of the second semiconductor layer being continuous with the first portion and extending in a second direction perpendicular to the first surface to a side of the first semiconductor layer away from the silicon substrate; and a first insulating layer located at least in the gap, with the first insulating layer being proximal to an end of the first conductive semiconductor layer. In addition to the second intrinsic semiconductor layer providing passivation and insulation between the first and second conductive semiconductor layers, the first insulating layer also provides excellent insulation reinforcement, reducing the probability of leakage between the different types of conductive semiconductor layers. This patent application proposes disposing the first insulating layer between the first and second semiconductor layers in the presence of a mask layer. Part of the first insulating layer's width directly contacts the silicon substrate, requiring both passivation and degradation, which impacts cell efficiency and yield. Furthermore, the manufacturing process is complex.

[0007] Therefore, the art urgently needs a back-contact battery that can effectively avoid leakage at the side edges of the second semiconductor opening region, has excellent battery efficiency and battery yield, and has a simple manufacturing process.

[0008] Summary of the Invention

[0009] The purpose of the present disclosure is to overcome the defects of the prior art that it is impossible to simultaneously take into account the effective avoidance of leakage phenomena at the side edges of the second semiconductor opening area, excellent battery efficiency and battery yield, and simple preparation process, and to provide a back-contact battery and its manufacturing method and photovoltaic module. The back-contact battery can simultaneously take into account the effective avoidance of leakage phenomena at the side edges of the second semiconductor opening area, excellent battery efficiency and battery yield, and simple preparation process.

[0010] In order to achieve the above-mentioned objectives, in a first aspect, the present disclosure provides a back-contact battery, comprising a silicon substrate having a front side and a back side, a first semiconductor layer having a second semiconductor opening region arranged on the back side, and a second semiconductor layer arranged on the outer surface of the first semiconductor layer and in the second semiconductor opening region, and also comprising a plurality of insulating layers arranged at intervals along the X-axis direction of the back side, wherein the insulating layer is arranged on the outer surface of the second semiconductor layer; and in the X-axis direction, the insulating layer spans the side edges of the second semiconductor opening region and extends at both ends respectively, and the span length W12 of the insulating layer on the second semiconductor opening region and the span length W11 of the insulating layer on the first semiconductor layer satisfy W12:W11=0.1-10:1.

[0011] In some optional embodiments, the length W1 of the insulating layer in the X-axis direction is 20-200 μm, and W12 is ≥10 μm.

[0012] In some optional embodiments, the material of the insulating layer includes at least one of silicon nitride, silicon oxynitride, and silicon oxide.

[0013] In some optional embodiments, the back-contact battery further includes: a conductive film layer, which is disposed on the outer surface of the insulating layer and has an isolation groove formed thereon, wherein the isolation groove is located on the outer surface of the insulating layer in the Z-axis direction.

[0014] In some optional embodiments, a width W3 of the isolation trench in the X-axis direction is 10-190 μm.

[0015] In some optional embodiments, a ratio of a length W1 of the insulating layer in the X-axis direction to a width W3 of the isolation trench is 0.3-10:1.

[0016] In some optional implementations, the isolation trench is located directly above a side edge of the second semiconductor opening region.

[0017] In some optional embodiments, the back-contact battery further includes an insulating protective layer covering the outer surface of the insulating layer, the insulating protective layer is located between the insulating layer and the conductive film layer, and the isolation groove is located on the outer surface of the insulating protective layer in the Z-axis direction.

[0018] In some optional embodiments, the thickness of the insulating protective layer is 5-30 μm.

[0019] In some optional embodiments, the material of the insulating protective layer includes at least one of epoxy resin, acrylic resin, and polyurethane resin.

[0020] In some optional embodiments, the first semiconductor layer includes a first passivation layer and a first conductive semiconductor film layer, the first passivation layer is a tunneling oxide layer or an intrinsic silicon layer; the second semiconductor layer includes a second passivation layer and a second conductive semiconductor film layer, the second passivation layer is an intrinsic silicon layer; one of the first conductive semiconductor film layer and the second conductive semiconductor film layer is N-type (optionally an N-type doped polycrystalline silicon layer), and the other is P-type (optionally a P-type doped amorphous silicon or microcrystalline silicon layer).

[0021] More optionally, the first passivation layer is a tunneling oxide layer, the first conductive semiconductor film layer is a doped polysilicon layer, and the second conductive semiconductor film layer is a doped amorphous silicon or microcrystalline silicon layer.

[0022] More optionally, the first conductive semiconductor film layer is N-type, and the second conductive semiconductor film layer is P-type.

[0023] In some optional embodiments, no mask layer is disposed between the first semiconductor layer and the second semiconductor layer.

[0024] In some optional embodiments, the front side of the silicon substrate is a textured surface, and the back side of the silicon substrate is a polished surface, or the second semiconductor opening area on the back side is a textured surface and the rest of the back side is a polished area.

[0025] In some optional embodiments, first semiconductor opening regions spaced apart along the X-axis direction are opened on the second semiconductor layer to expose the first semiconductor layer, the first semiconductor opening region is located between two adjacent second semiconductor opening regions, and the first semiconductor opening region accommodates part of the conductive film layer.

[0026] More optionally, in the X-axis direction, the length W4 of the first semiconductor opening region is 100-300 μm, the length W2 of the second semiconductor opening region is 300-700 μm, and the interval Wg between the first semiconductor opening region and the second semiconductor opening region is 50-400 μm.

[0027] More optionally, W12 / W2 is 1:3-55, and W11 / Wg is 1:1-10.

[0028] In some optional embodiments, the back contact battery further comprises:

[0029] Metal electrodes are respectively arranged on the outer surface of the first semiconductor opening region and the outer surface of the second semiconductor opening region;

[0030] a front passivation layer, which is disposed on the front side of the silicon substrate;

[0031] The front anti-reflection layer is arranged on the outer surface of the front passivation layer.

[0032] More optionally, the front passivation layer is a silicon dielectric passivation layer, and the front anti-reflection layer is a silicon dielectric anti-reflection layer.

[0033] In a second aspect, the present disclosure provides a method for manufacturing a back-contact battery, wherein the back-contact battery is the back-contact battery described in the first aspect, and the method for manufacturing the back-contact battery comprises the following steps:

[0034] S101, providing a silicon substrate on which a first semiconductor layer, a second semiconductor layer, and an insulating film are sequentially arranged along the Z-axis direction, wherein the first semiconductor layer is provided with second semiconductor openings spaced apart to accommodate a portion of the second semiconductor layer;

[0035] S102, applying protective ink on a portion of the outer surface of the insulating film on the back side obtained in S101, the protective ink covering the portion of the outer surface of the insulating film to be retained, the size of the protective ink being set accordingly according to the insulating layer to be formed;

[0036] S103 , on the back surface obtained in S102 , removing the portion of the insulating film not covered by the protective ink, so that the portion of the insulating film to be retained forms an insulating layer.

[0037] In some optional implementations, S103 further includes: after removing the portion of the insulating film not covered by the protective ink, further removing the protective ink.

[0038] In some other optional embodiments, the protective ink in S102 is an insulating protective layer, and the protective ink is not removed in S103.

[0039] In some optional embodiments, the manufacturing method further comprises:

[0040] S104, depositing a conductive film layer on the back surface obtained in S103;

[0041] S105 , forming an isolation groove on the conductive film layer on the back side obtained in S104 .

[0042] More optionally, the isolation grooves are formed by laser etching, printing, or inkjet printing with protective ink followed by corrosion.

[0043] In some optional implementations, S101 further includes forming a front passivation layer and a front anti-reflection layer on the front surface of the silicon substrate, and forming a first semiconductor opening region on the second semiconductor layer.

[0044] More optionally, the manufacturing method further comprises: S106, providing metal electrodes on the outer surface of the first semiconductor opening region and the outer surface of the second semiconductor opening region in the back surface obtained in S105, respectively.

[0045] In a third aspect, the present disclosure provides a photovoltaic module comprising the back-contact cell described in the first aspect. Beneficial effects:

[0046] The present invention provides an insulating layer on the outer surface of the second semiconductor layer, and in the X-axis direction, the insulating layer spans the side edges of the second semiconductor opening region and extends at the above-mentioned appropriate ratios at both ends. This can significantly improve leakage and avoid short circuits without the need for a mask layer, thereby improving the parallel resistance of the battery, and further improving the battery conversion efficiency and battery yield. Compared with CN115588698A, in which the first insulating layer is provided within the gap between the side edges of the second semiconductor opening region and a portion of its width directly contacts the silicon substrate, the insulating layer of the present invention is completely provided on the outer surface of the second semiconductor layer and spans the second semiconductor layer at an appropriate ratio. It is independent of the double semiconductor layer, does not have doping or crossover, does not weaken the passivation effect of the double semiconductor layer, does not need to consider passivation, and does not need to take into account both passivation and insulation effects. The insulation effect is better, and the passivation effect is better because a mask layer is not required. In addition, the preparation process is simplified.

[0047] Optionally, the name of the prior research patent application of the applicant of the present disclosure is a back-contact battery with a specific isolation groove arrangement and a preparation method thereof, wherein the isolation groove is located above the contact interface between the first semiconductor layer and the second semiconductor layer in the Z-axis direction and spans the textured surface and the polished surface. There is no mask layer protection between the isolation groove and the second semiconductor layer. If laser etching is used on the textured surface, the second semiconductor layer below will be severely damaged. Therefore, the battery reliability can only be guaranteed by mask etching. In this regard, in the optional scheme of the present disclosure, the isolation groove is located on the outer surface of the insulating layer in the Z-axis direction, and the insulating layer (or the insulating layer and the insulating protective layer) can be used as a mask layer for the preparation of the isolation groove, and the isolation groove can be entirely in the polishing area or on the outer surface of the insulating protective layer. It can be opened on the polishing area or on the insulating protective layer, and can be isolated by laser without damaging the second semiconductor layer. While the process is simple, it is more conducive to improving battery reliability. Moreover, the insulating layer of the present invention can be selected from at least one of silicon nitride, silicon oxynitride, and silicon oxide. Compared with the above-mentioned prior research patent application of the applicant of the present invention (the insulating layer printed or sprayed in the isolation groove is a polymer material), the waterproofness will be significantly improved, and thus the battery reliability will be better. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0049] FIG1 is a schematic diagram of a battery structure in which a front film layer, a first semiconductor layer, a second semiconductor layer, and an insulating film are formed on the back side in accordance with Embodiment 1 of the present disclosure;

[0050] FIG2 is a schematic diagram of the structure of forming a protective ink on the back of a silicon substrate in Example 1 of the present disclosure;

[0051] FIG3 is a schematic diagram of the structure of etching the outer insulating film of the protective ink in Example 1 of the present disclosure;

[0052] FIG4 is a schematic diagram of the structure of removing and cleaning the protective ink in Example 1 of the present disclosure;

[0053] FIG5 is a schematic structural diagram of a conductive film layer deposited on the back side of the embodiment 1 of the present disclosure;

[0054] FIG6 is a schematic structural diagram of an isolation trench formed directly above the insulating film on the back side of the first embodiment of the present disclosure;

[0055] FIG7 is a schematic structural diagram of a metal electrode formed on the back side of the first embodiment of the present disclosure.

[0056] FIG8 is a schematic structural diagram of a conductive film layer deposited on the back side of Example 3 of the present disclosure;

[0057] FIG9 is a schematic structural diagram of an isolation groove formed directly above the back insulating ink in Example 3 of the present disclosure;

[0058] FIG10 is a schematic diagram of the structure of a metal electrode formed on the back side of Example 3 of the present disclosure.

[0059] FIG11 is a schematic diagram of the battery structure of Comparative Example 1.

[0060] Explanation of the accompanying symbols: 1. Silicon substrate, 2. First passivation layer, 3. First conductive semiconductor film layer, 4. Second passivation layer, 5. Second conductive semiconductor film layer, 6. Insulating film, 7. Front film layer, 8. Protective ink, 9. Conductive film layer, 10. Metal electrode, 11. Mask layer; 101. Horizontal area of ​​the second semiconductor opening area, 102. Side edge of the second semiconductor opening area. DETAILED DESCRIPTION

[0061] In the description of the present disclosure, the direction close to the silicon substrate is considered to be inside, and the direction away from the silicon substrate is considered to be outside. The terms "first" and "second" are only configured for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present disclosure, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0062] In the present disclosure, unless otherwise expressly specified or limited, when a first feature is "above" or "below" a second feature, it may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Furthermore, when a first feature is "above," "above," or "above" a second feature, it may mean that the first feature is directly above or diagonally above the second feature, or simply means that the first feature is at a higher level than the second feature. When a first feature is "below," "below," or "below" a second feature, it may mean that the first feature is directly below or diagonally below the second feature, or simply means that the first feature is at a lower level than the second feature.

[0063] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. Among them, the terms "optional" and "optional" all mean that they may be included or not (or may be present or not).

[0064] In the first aspect, the present disclosure provides a back-contact battery, comprising a silicon substrate having a front side and a back side, a first semiconductor layer having a second semiconductor opening region arranged on the back side, and a second semiconductor layer arranged on the outer surface of the first semiconductor layer and in the second semiconductor opening region, and also comprising a plurality of insulating layers arranged at intervals along the X-axis direction of the back side, wherein the insulating layer is arranged on the outer surface of the second semiconductor layer; and in the X-axis direction, the insulating layer spans the side edge of the second semiconductor opening region and extends at both ends respectively, and the span length W12 of the insulating layer on the second semiconductor opening region and the span length W11 of the insulating layer on the first semiconductor layer satisfy W12:W11=0.1-10:1, specifically for example, it can be 0.1:1, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, and 1-5:1 is optional.

[0065] In the back-contact cell disclosed herein, the insulating layer having the aforementioned specific cross-length ratio significantly reduces leakage and prevents short circuits without requiring a mask layer, thereby increasing the cell's parallel resistance and, in turn, improving cell conversion efficiency and yield. Under the same conditions, if the ratio W12:W11 is too large or too small, the edge of the insulating layer will be too close to the side edge of the second semiconductor opening, resulting in poor insulation and affecting cell yield and conversion efficiency.

[0066] In some optional embodiments, a length W1 of the insulating layer in the X-axis direction is 20-200 μm.

[0067] More optionally, W12 ≥ 10 μm. In this option, the width of the insulating layer can exceed the side edge of the second semiconductor opening region by more than 10 μm, which is more conducive to improving leakage and avoiding short circuits, thereby improving the parallel resistance of the battery and the battery conversion efficiency.

[0068] In some optional embodiments, the insulating layer is made of at least one of silicon nitride, silicon oxynitride, and silicon oxide. In this optional solution, the insulating layer has better water resistance, which is more conducive to improving battery reliability, battery yield, and conversion efficiency.

[0069] In some optional embodiments, the back-contact battery further includes: a conductive film layer, which is disposed on the outer surface of the insulating layer and has an isolation groove formed thereon, wherein the isolation groove is located on the outer surface of the insulating layer in the Z-axis direction.

[0070] In some optional embodiments, the width W3 of the isolation trench in the X-axis direction is 10-190 μm, or optionally 50-190 μm. The isolation trench of the present disclosure primarily serves to insulate the conductive film layer on the surface of the first semiconductor layer from the second semiconductor layer. Within a suitable W3 range, this helps minimize short circuits to improve battery yield while also increasing the length of carrier transmission on the conductive film layer to improve battery efficiency.

[0071] Those skilled in the art can select the thickness of the insulating layer according to actual needs. For example, the thickness of the insulating layer can be 30-100 nm.

[0072] In some optional embodiments, a ratio of a length W1 of the insulating layer in the X-axis direction to a width W3 of the isolation trench is 0.3-10:1.

[0073] More optionally, the ratio of the length W1 of the insulating layer in the X-axis direction to the width W3 of the isolation trench is 1.1-10:1, more preferably 1.1-6:1. In this option, the width W1 is greater than the width of the isolation trench, and the isolation trench does not exceed the area of ​​W1. This allows the isolation trench W3 to be completely opened on the upper surface of the insulating layer. This provides insulation protection under the isolation trench, which helps improve battery reliability and avoids the phenomenon of the semiconductor layer behind the isolation trench being unprotected by the mask layer.

[0074] The isolation trench of the present disclosure only needs to be within the area of ​​W1. In some optional embodiments, the isolation trench is located directly above the side edge of the second semiconductor opening region, which is more conducive to improving battery reliability.

[0075] In some optional embodiments, the back-contact battery further includes an insulating protective layer covering the outer surface of the insulating layer, the insulating protective layer is located between the insulating layer and the conductive film layer, and the isolation groove is located on the outer surface of the insulating protective layer in the Z-axis direction.

[0076] Optionally in the present disclosure, the thickness of the insulating protective layer is 5-30 μm.

[0077] In some optional embodiments, the insulating protective layer is made of at least one of epoxy resin, acrylic resin, and polyurethane resin, which cannot be removed by washing with hot water or acid or alkali solutions.

[0078] The type of the conductive film layer disclosed in the present invention can be, for example, a transparent conductive film layer or a composite layer of a transparent conductive film and a metal film, wherein the transparent conductive film layer is an indium oxide-based film doped with tin, zinc, tungsten, titanium, etc., and the metal film is a film of one or more of gold, silver, copper, aluminum, nickel, and a nickel alloy; those skilled in the art can select according to their needs.

[0079] In some optional embodiments, the first semiconductor layer includes a first passivation layer and a first conductive semiconductor film layer, the first passivation layer is a tunneling oxide layer or an intrinsic silicon layer; the second semiconductor layer includes a second passivation layer and a second conductive semiconductor film layer, the second passivation layer is an intrinsic silicon layer; one of the first conductive semiconductor film layer and the second conductive semiconductor film layer is N-type and the other is P-type.

[0080] The first passivation layer is an intrinsic silicon layer, for example, an intrinsic amorphous silicon layer. In this case, the back contact cell of the present disclosure is a conventional heterojunction cell, and the first conductive semiconductor film layer and the second conductive semiconductor film layer can be doped amorphous silicon or microcrystalline silicon layers, respectively. In some specific embodiments of the conventional heterojunction cell structure, the thickness of the intrinsic silicon layer can be, for example, 5-10 nm. The thickness of the first conductive semiconductor film layer can be 10-15 nm, with a doping concentration of 8e18-8e20 cm-3, the thickness of the second passivation layer can be 5-15 nm, and the thickness of the second conductive semiconductor film layer can be 5-25 nm, with a doping concentration of 8e18-8e20 cm-3.

[0081] More optionally, the first passivation layer is a tunneling oxide layer, the first conductive semiconductor film layer is a doped polysilicon layer, and the second conductive semiconductor film layer is a doped amorphous silicon or microcrystalline silicon layer.

[0082] Those skilled in the art can select the thickness of the first passivation layer, the first conductive semiconductor film layer, the second conductive semiconductor film layer, and the second passivation layer, as well as the doping concentration of the first conductive semiconductor film layer and the second conductive semiconductor film layer according to actual needs. For example, the corresponding layer thicknesses and doping concentrations disclosed in the earlier patents of the applicant of the present disclosure or other conventional ranges can be adopted. In some specific embodiments of the combined passivation back contact cell, the first passivation layer has a thickness of 0.5-5 nm, the first conductive semiconductor film layer has a doping concentration of 8e18-8e20 cm-3 and a thickness of 100-200 nm, the second passivation layer has a thickness of 5-15 nm, and the second conductive semiconductor film layer has a thickness of 5-25 nm and a doping concentration of 8e18-8e20 cm-3.

[0083] More optionally, the first conductive semiconductor film layer is N-type, and the second conductive semiconductor film layer is P-type. In this optional solution, the bottom of the gap Wg between the first semiconductor opening region and the second semiconductor opening region is N-type semiconductor. Because N-type semiconductors have better passivation and conductivity than P-type semiconductors, they can improve the passivation effect of the battery and reduce electrical losses in carrier transmission, which is more conducive to improving the conversion efficiency of the battery.

[0084] In some optional embodiments, no mask layer is disposed between the first semiconductor layer and the second semiconductor layer.

[0085] In the present disclosure, those skilled in the art can select a structure such as polishing or texturing on the front and back sides of the silicon substrate, based on the light reflection conditions on the front or back sides and their impact on conversion efficiency or the impact of the preparation process. In some optional embodiments, the front side of the silicon substrate is a texturing surface, and the back side of the silicon substrate is a polishing surface, or the second semiconductor opening area on the back side is a texturing surface and the other areas on the back side are polishing areas, which is more conducive to significantly reducing light reflection while taking into account improving the conversion efficiency of the battery.

[0086] In some optional embodiments, first semiconductor opening regions spaced apart along the X-axis direction are opened on the second semiconductor layer to expose the first semiconductor layer, the first semiconductor opening region is located between two adjacent second semiconductor opening regions, and the first semiconductor opening region accommodates part of the conductive film layer.

[0087] More optionally, in the X-axis direction, the length W4 of the first semiconductor opening region is 100-300 μm, the length W2 of the second semiconductor opening region is 300-700 μm, and the interval Wg between the first semiconductor opening region and the second semiconductor opening region is 50-400 μm.

[0088] More optionally, W12 / W2 is 1:3-55, and W11 / Wg is 1:1-10.

[0089] More preferably, W12 / W2 is 1:3-35, more preferably 1:9-25, and W11 / Wg is 1:1-10, more preferably 1:1-5. Under this option, the insulating layer coverage area can extend beyond the side edges of the second semiconductor opening region by a certain appropriate safety distance, thereby facilitating both increasing the carrier transmission distance on the conductive film layer and appropriately reducing the carrier transmission distance on the semiconductor layer. Since the resistivity of the semiconductor layer is greater than that of the conductive film layer, carrier transmission losses can be significantly reduced. Furthermore, the isolation trench can be completely etched within the insulating layer coverage area, requiring relatively low alignment accuracy, facilitating efficient mass production and improving battery yield and conversion efficiency.

[0090] In some optional embodiments, the back-contact battery further includes: metal electrodes, which are respectively arranged on the outer surface of the first semiconductor opening region and the outer surface of the second semiconductor opening region.

[0091] In some optional embodiments, the back-contact cell further comprises: a front passivation layer disposed on the front side of the silicon substrate.

[0092] More optionally, the front passivation layer is a silicon dielectric passivation layer, which may be a tunneling silicon oxide layer and a polysilicon layer, or an intrinsic amorphous silicon layer and an N-type doped amorphous / microcrystalline silicon layer.

[0093] In some optional embodiments, the back-contact cell further comprises: a front anti-reflection layer, which is disposed on the outer surface of the front passivation layer.

[0094] More optionally, the front anti-reflection layer is a silicon dielectric anti-reflection layer. Those skilled in the art can use any conventional silicon dielectric anti-reflection layer in the prior art, which will not be described in detail here.

[0095] In a second aspect, the present disclosure provides a method for manufacturing a back-contact battery, wherein the back-contact battery is the back-contact battery described in the first aspect, and the method for manufacturing the back-contact battery comprises the following steps:

[0096] S101, providing a silicon substrate on which a first semiconductor layer, a second semiconductor layer, and an insulating film are sequentially arranged along the Z-axis direction, wherein the first semiconductor layer is provided with second semiconductor openings spaced apart to accommodate a portion of the second semiconductor layer;

[0097] S102, applying protective ink on a portion of the outer surface of the insulating film on the back side obtained in S101, the protective ink covering the portion of the outer surface of the insulating film to be retained, the size of the protective ink being set accordingly according to the insulating layer to be formed;

[0098] S103 , on the back surface obtained in S102 , removing the portion of the insulating film not covered by the protective ink, so that the portion of the insulating film to be retained forms an insulating layer.

[0099] In S103 , the portion of the insulating film not covered by the protective ink is removed. The insulating film may be removed by, for example, a corrosive solution, such as a solution containing HF (HF mass concentration may be, for example, 1 wt % to 10 wt %).

[0100] In some optional embodiments, S103 further includes removing the protective ink after removing the portion of the insulating film not covered by the protective ink. In this embodiment, the protective ink may be, for example, hot melt wax or other resin that can be cleaned with an alkaline solution. The protective ink may be removed using, for example, hot water or a weakly alkaline solution, as long as it can be completely removed.

[0101] In some other optional embodiments, the protective ink in S102 is an insulating protective layer, and the protective ink is not removed in S103.

[0102] In some optional embodiments, the manufacturing method further comprises:

[0103] S104, depositing a conductive film layer on the back surface obtained in S103;

[0104] S105 , forming an isolation groove on the conductive film layer on the back side obtained in S104 .

[0105] The method of depositing the conductive film layer in S104 may be, for example, physical vapor deposition (PVD) or activated plasma deposition (RPD).

[0106] More optionally, the isolation grooves are formed by laser etching, printing, or inkjet printing with protective ink followed by corrosion; laser etching is more optional, as the process is simpler.

[0107] In an optional solution disclosed herein, the isolation groove is located on the outer surface of the insulating layer in the Z-axis direction, the insulating layer (or the insulating layer and the insulating protective layer) can be used as a mask layer for preparing the isolation groove, and the isolation groove can be entirely on the polishing area or the outer surface of the insulating protective layer. It can be opened on the polishing area or the insulating protective layer, and laser isolation can be used without damaging the second semiconductor layer. The process is simple and is more conducive to improving battery reliability.

[0108] In some optional implementations, S101 further includes forming a front passivation layer and a front anti-reflection layer on the front surface of the silicon substrate, and forming a first semiconductor opening region on the second semiconductor layer.

[0109] More optionally, the manufacturing method further comprises: S106, providing metal electrodes on the outer surface of the first semiconductor opening region and the outer surface of the second semiconductor opening region in the back surface obtained in S105, respectively.

[0110] The metal electrodes can be formed by printing silver paste to form silver paste grid line electrodes, electroplating to form copper grid line electrodes, etc.

[0111] In a third aspect, the present disclosure provides a photovoltaic module comprising the back-contact cell described in the first aspect.

[0112] The following describes embodiments of the present disclosure in detail, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only configured to explain the present disclosure and are not to be construed as limiting the present disclosure.

[0113] Example 1

[0114] A back contact battery, the manufacturing method of which is as follows:

[0115] S101. As shown in FIG1 , a silicon substrate 1 is provided with a back surface on which a first semiconductor layer, a second semiconductor layer, and an insulating film 6 (silicon nitride) are formed. The first semiconductor layer comprises a first passivation layer 2 (a tunneling oxide layer with a thickness of 1.5 nm) and a first conductive semiconductor film layer 3 (an N-type polycrystalline layer with a doping concentration of 8e20 cm⁻³ and a thickness of 150 nm). The second semiconductor layer comprises a second passivation layer 4 (an intrinsic amorphous silicon layer with a thickness of 10 nm) and a second conductive semiconductor film layer 5 (a P-type doped amorphous silicon layer with a thickness of 20 nm and a doping concentration of 8e19 cm⁻³). A front surface of the silicon substrate forms a cell structure with a front film layer 7. The front film layer 7 comprises a silicon dielectric passivation layer and a silicon dielectric anti-reflection layer. A second semiconductor opening region is defined on the first conductive semiconductor film layer 3. The width W2 of the second semiconductor opening region is 500 μm. The silicon substrate surface where the horizontal region 101 of the second semiconductor opening region is located is polished. A first semiconductor opening region is opened on the second semiconductor layer to expose the first semiconductor layer. The length W4 of the first semiconductor opening region is 200 μm, and the interval Wg between the first semiconductor opening region and the second semiconductor opening region is 100 μm.

[0116] S102. As shown in FIG2 , a protective ink 8 (hot melt wax) is inkjet-printed on the outer surface of the back surface of the silicon substrate 1 directly above the side edge 102 of the second semiconductor opening region. The protective ink 8 extends across the side edge 102 of the second semiconductor opening region. The width W1 of the protective ink 8 is 100 μm. The length W12 of the protective ink 8 extending over the second semiconductor opening region is ≥ 10 μm, and the length W11 extending over the first semiconductor layer is ≥ 10 μm. Furthermore, W12:W11 = 1:1. W12 / W2 is 1:10, and W11 / Wg is 1:2.

[0117] S103, as shown in FIG3, a solution containing 5 wt% HF is used to etch away the insulating film 6 outside the protective ink 8 to form an insulating layer. As shown in FIG4, the protective ink 8 is removed and cleaned with hot water.

[0118] S104 , as shown in FIG5 , depositing a conductive film layer 9 on the back side of the silicon substrate 1 by physical vapor deposition (PVD) technology, wherein the conductive film layer 9 is a transparent conductive film layer, and the transparent conductive film layer is a tin-doped indium oxide-based thin film.

[0119] S105. As shown in FIG6 , an isolation trench is formed directly above the insulating film 6 on the back side of the silicon substrate 1. The width W3 of the isolation trench is 50 μm and the isolation trench is directly etched by laser. The ratio of W1 to the width of the isolation trench is 2:1.

[0120] S106 , as shown in FIG7 , forming a metal electrode 10 on the back side of the silicon substrate 1 .

[0121] The test results of the parallel resistance, battery yield and battery conversion efficiency of the back contact battery of this embodiment are shown in Table 1 below.

[0122] Example 2

[0123] The method of Example 1 was followed, except that the P / N types of the two semiconductor layers were different. Specifically, the first conductive semiconductor film layer 3 was a P-type polycrystalline silicon layer, and the second conductive semiconductor film layer 5 was an N-type doped amorphous silicon layer. Corresponding tests were conducted, and the results are shown in Table 1.

[0124] Example 3

[0125] The method of Example 1 is referred to, except that the protective ink 8 is an insulating ink and is not removed subsequently, as follows:

[0126] S102 , the printed protective ink 8 is an insulating ink (ie, an insulating protective layer), which is epoxy resin and cannot be removed by washing with hot water or acid or alkali solution. The thickness of the insulating ink is 10 μm.

[0127] S103, as shown in FIG3, the insulating film 6 outside the insulating ink is etched away by a solution containing HF.

[0128] S104 , as shown in FIG8 , depositing a conductive film layer 9 on the back side of the silicon substrate 1 by physical vapor deposition (PVD) technology.

[0129] S105 , as shown in FIG9 , forming an isolation groove directly above the insulating ink on the back side of the silicon substrate 1 .

[0130] S106 , as shown in FIG10 , forming a metal electrode 10 on the back side of the silicon substrate 1 .

[0131] The corresponding tests were carried out and the results are shown in Table 1.

[0132] Example 4

[0133] The method of Example 1 is referred to, except that W1 is 30 μm and W12:W11 remains unchanged; at this time, the adaptive calculated ratio of W1 to the width W3 of the isolation groove is 0.6:1, W12 / W2 is 1:33, and W11 / Wg is 1:6.7.

[0134] The corresponding tests were carried out and the results are shown in Table 1.

[0135] Example 5

[0136] The method of Example 1 was followed, except that W1 remained unchanged and W12:W11 was changed to 9:1; at this time, the adaptability calculated W12 / W2 was 1:5.6, and W11 / Wg was 1:10.

[0137] The corresponding tests were carried out and the results are shown in Table 1.

[0138] Example 6

[0139] The method of Example 1 was followed, except that W1 remained unchanged and W12:W11 was changed to 0.1:1; at this time, the adaptability calculated W12 / W2 was 1:55, and W11 / Wg was 1:1.1.

[0140] The corresponding tests were carried out and the results are shown in Table 1.

[0141] Example 7

[0142] The method of Example 1 is referred to, except that the width of the isolation trench is changed so that the ratio of the length W1 of the insulating layer in the X-axis direction to the width W3 of the isolation trench is 10:1;

[0143] The corresponding tests were carried out and the results are shown in Table 1.

[0144] Example 8

[0145] The method of Example 1 is referred to, except that a conventional heterojunction passivation structure is adopted. Specifically, the first passivation layer is an intrinsic amorphous silicon layer with a thickness of 10 nm, and the first conductive semiconductor layer is an N-type microcrystalline silicon layer with a thickness of 10 nm and the doping concentration is the same as in Example 1.

[0146] The corresponding tests were carried out and the results are shown in Table 1.

[0147] Comparative Example 1

[0148] The method of Example 1 is referred to, except that a combined passivation battery structure is adopted in which the insulating film 6 is not provided, as shown in FIG11 , but a mask layer 11 is further deposited in the gap Wg between the first semiconductor opening region and the second semiconductor opening region, the mask layer 11 is located between the first semiconductor layer and the second semiconductor layer, and the insulating groove is provided above the outer surface of the mask layer 11 and away from the side edge 102 of the second semiconductor opening region.

[0149] The corresponding tests were carried out and the results are shown in Table 1.

[0150] Comparative Example 2

[0151] The method of Example 1 is referred to, except that W1 remains unchanged and W12:W11 is changed to 20:1; at this time, the adaptability calculation W12 / W2 is 1:5.3, and W11 / Wg is 1:21.

[0152] The corresponding tests were carried out and the results are shown in Table 1.

[0153] Comparative Example 3

[0154] The method of Example 1 was followed, except that W1 remained unchanged and W12:W11 was changed to 0.05:1; at this time, the adaptability calculated W12 / W2 was 1:105, and W11 / Wg was 1:1.1.

[0155] The corresponding tests were carried out and the results are shown in Table 1.

[0156] Comparative Example 4

[0157] The method of Example 8 is referred to, except that a conventional heterojunction passivated battery structure without an insulating film 6 is adopted, and a mask layer 11 is further deposited in the gap Wg between the first semiconductor opening region and the second semiconductor opening region, the mask layer 11 is located between the first semiconductor layer and the second semiconductor layer, and the insulating groove is arranged above the outer surface of the mask layer 11 and away from the side edge 102 of the second semiconductor opening region.

[0158] The corresponding tests were carried out and the results are shown in Table 1.

[0159] Table 1

[0160] The above examples and comparative examples demonstrate that the embodiments of the present disclosure significantly improve leakage without requiring a mask layer, while also providing a passivation effect. This improves the parallel resistance of the battery, thereby increasing battery conversion efficiency and yield. Comparative Example 1, which utilizes a conventional structure, and Comparative Examples 2-4, which fall outside the scope of the present disclosure, fail to achieve the comprehensive benefits of the present disclosure.

[0161] Optionally, according to Example 1 and Example 2 of the present disclosure, the first semiconductor layer is an N-type semiconductor layer, and the second semiconductor layer is a P-type semiconductor layer, which is more conducive to improving the battery conversion efficiency. According to Example 1 and Example 3 of the present disclosure, removing the insulating ink on the upper surface of the insulating layer is more conducive to improving the battery production yield. According to Example 1 and Examples 4-7 of the present disclosure, providing an insulating layer of appropriate width and an isolation groove of appropriate width on both sides of the outer surface of the side edge of the second semiconductor opening area is more conducive to improving the parallel resistance of the battery, while improving the battery yield and conversion efficiency. According to Example 1 and Example 8 of the present disclosure, the use of a combined passivation structure is more conducive to improving the battery production yield and battery conversion efficiency compared to a conventional heterojunction structure.

[0162] The above describes in detail the optional embodiments of the present disclosure, but the present disclosure is not limited thereto. Within the technical concept of the present disclosure, various simple variations of the technical solution of the present disclosure can be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as the contents disclosed by the present disclosure and fall within the scope of protection of the present disclosure. Industrial Applicability

[0163] The back-contact battery disclosed in the present invention provides an insulating layer on the outer surface of the second semiconductor layer, and in the X-axis direction, the insulating layer spans the side edges of the second semiconductor opening area and extends at the above-mentioned appropriate proportions at both ends. This can greatly improve leakage and avoid short circuits without providing a mask layer, thereby increasing the parallel resistance of the battery, and further improving the battery conversion efficiency and battery yield.

Claims

1. A back contact battery, comprising a silicon substrate having a front side and a back side, a first semiconductor layer having a second semiconductor opening region disposed on the back side, and a second semiconductor layer disposed on an outer surface of the first semiconductor layer and within the second semiconductor opening region, characterized in that: It also includes a plurality of insulating layers arranged at intervals along the X-axis direction of the back side, and the insulating layers are arranged on the outer surface of the second semiconductor layer; and in the X-axis direction, the insulating layers span the side edges of the second semiconductor opening area and extend at both ends respectively, and the span length W12 of the insulating layer on the second semiconductor opening area and the span length W11 of the insulating layer on the first semiconductor layer satisfy W12:W11=0.1-10:

1.

2. The back contact cell according to claim 1, characterized in that: The length W1 of the insulating layer in the X-axis direction is 20-200 μm, and W12 ≥ 10 μm; and / or the material of the insulating layer includes at least one of silicon nitride, silicon oxynitride, and silicon oxide.

3. The back contact cell according to claim 1 or 2, characterized in that: The back contact battery further includes: a conductive film layer, which is arranged on the outer surface of the insulating layer and has an isolation groove formed thereon, wherein the isolation groove is located on the outer surface of the insulating layer in the Z-axis direction.

4. The back contact cell according to claim 3, characterized in that: The width W3 of the isolation groove in the X-axis direction is 10-190 μm, and the ratio of the length W1 of the insulating layer in the X-axis direction to the width W3 of the isolation groove is 0.3-10:1; And / or, the isolation trench is located directly above a side edge of the second semiconductor opening region.

5. The back contact cell according to claim 3 or 4, characterized in that: The back-contact battery also includes an insulating protective layer covering the outer surface of the insulating layer, the insulating protective layer is located between the insulating layer and the conductive film layer, and the isolation groove is located on the outer surface of the insulating protective layer in the Z-axis direction; wherein the thickness of the insulating protective layer is 5-30μm, and / or the material of the insulating protective layer includes at least one of epoxy resin, acrylic resin, and polyurethane resin.

6. The back contact battery according to any one of claims 3 to 5, characterized in that: The first semiconductor layer includes a first passivation layer and a first conductive semiconductor film layer, the first passivation layer is a tunneling oxide layer or an intrinsic silicon layer; the second semiconductor layer includes a second passivation layer and a second conductive semiconductor film layer, the second passivation layer is an intrinsic silicon layer; one of the first conductive semiconductor film layer and the second conductive semiconductor film layer is N-type and the other is P-type.

7. The back contact cell according to claim 6, characterized in that: The first passivation layer is a tunneling oxide layer, the first conductive semiconductor film layer is a doped polysilicon layer, and the second conductive semiconductor film layer is a doped amorphous silicon or microcrystalline silicon layer.

8. The back contact battery according to claim 7, characterized in that: The first conductive semiconductor film layer is of N type, and the second conductive semiconductor film layer is of P type.

9. The back contact cell according to any one of claims 1 to 8, characterized in that No mask layer is arranged between the first semiconductor layer and the second semiconductor layer; and / or, the front side of the silicon substrate is a textured surface, and the back side of the silicon substrate is a polished surface, or the second semiconductor opening area on the back side is a textured surface and other areas on the back side are polished areas.

10. The back contact battery according to claim 3, characterized in that: The second semiconductor layer is provided with first semiconductor opening regions spaced apart along the X-axis direction to expose the first semiconductor layer, the first semiconductor opening region is located between two adjacent second semiconductor opening regions, and the first semiconductor opening region contains a portion of the conductive film layer; wherein, In the X-axis direction, the length W4 of the first semiconductor opening region is 100-300 μm, the length W2 of the second semiconductor opening region is 300-700 μm, and the interval Wg between the first semiconductor opening region and the second semiconductor opening region is 50-400 μm; And / or, W12 / W2 is 1:3-55, and W11 / Wg is 1:1-10.

11. The back contact cell according to claim 10, characterized in that: The back contact battery further comprises: Metal electrodes are respectively arranged on the outer surface of the first semiconductor opening region and the outer surface of the second semiconductor opening region; A front passivation layer, which is disposed on the front side of the silicon substrate; The front anti-reflection layer is arranged on the outer surface of the front passivation layer.

12. A method for manufacturing a back contact battery, characterized in that: The back contact battery is the back contact battery according to any one of claims 1 to 11, and the method for manufacturing the back contact battery comprises the following steps: S101, providing a silicon substrate on the back side of which a first semiconductor layer, a second semiconductor layer, and an insulating film are sequentially arranged along the Z-axis direction, wherein the first semiconductor layer is provided with second semiconductor opening regions arranged at intervals to accommodate a portion of the second semiconductor layer; S102, providing a protective ink on a portion of the outer surface of the insulating film on the back side obtained in S101, the protective ink covering the outer surface of the portion of the insulating film to be retained, and the size of the protective ink being set accordingly according to the insulating layer to be formed; S103. On the back side obtained in S102, remove the portion of the insulating film not covered by the protective ink, so that the portion of the insulating film to be retained forms an insulating layer.

13. The manufacturing method according to claim 12, characterized in that: S103 further includes: after removing the portion of the insulating film not covered by the protective ink, removing the protective ink; Alternatively, the protective ink in S102 is an insulating protective layer, and the protective ink is not removed in S103.

14. The production method according to claim 12 or 13, characterized in that: The production method further comprises: S104, depositing a conductive film layer on the back surface obtained in S103; S105, forming an isolation groove on the conductive film layer on the back obtained in S104, wherein the isolation groove is formed by laser Etching, printing, or inkjet printing protective ink after corrosion; And / or, S101 also includes forming a front passivation layer and a front anti-reflection layer on the front side of the silicon substrate, and forming a first semiconductor opening area on the second semiconductor layer, and the manufacturing method also includes: S106, respectively arranging metal electrodes on the outer surface of the first semiconductor opening area and the outer surface of the second semiconductor opening area in the back side obtained in S105.

15. A photovoltaic module, characterized in that: Comprising a back contact cell as claimed in any one of claims 1-11.

Citation Information

Patent Citations

  • Back contact solar cell, preparation method thereof and photovoltaic module

    CN115588698A

  • Mask-layer-free joint passivation back contact battery and preparation method thereof

    CN115312633A

  • Tunneling type back contact heterojunction solar cell and manufacturing method thereof

    CN115763609A

  • Back contact battery, manufacturing method thereof and photovoltaic module

    CN116053331A

  • Back contact battery and manufacturing method thereof

    CN117174776A