Method for preparing solar cell and solar cell

By adopting a heterojunction bottom cell structure in a perovskite-silicon tandem solar cell and using evaporation and spin coating processes to form a perovskite light-absorbing layer, the low spectral utilization rate and low spectral utilization in perovskite-silicon tandem solar cells are solved. The problem of hindered interface charge transfer significantly improves the energy conversion efficiency of solar cells.

WO2024199030A1PCT designated stage expired Publication Date: 2024-10-03TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/082670
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing perovskite-silicon tandem solar cells have problems such as low spectral utilization and blocked interface charge transmission in industrial production and applications, resulting in low energy conversion efficiency.

Method used

Using a heterojunction bottom cell structure, the first cationic layer is formed by evaporation, and the second cationic layer is formed by spin coating. During the annealing process, the two react with the lead iodide skeleton layer to form a perovskite light-absorbing layer and improve the interface. Contact and charge transfer.

Benefits of technology

It improves the interface contact and charge transfer efficiency of the perovskite light-absorbing layer, significantly improves the energy conversion efficiency of solar cells, and promotes the industrial development of perovskite-silicon stacked cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082670_03102024_PF_FP_ABST
    Figure CN2024082670_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a method for preparing a solar cell and a solar cell. The method for preparing a solar cell comprises: forming a first cation layer (410) on the surface of the side of a hole passivation layer (320) away from a hole transport layer (310). By means of the first cation layer (410), the surfaces of both sides of a skeleton layer, where a perovskite layer is to be formed, in a perovskite-silicon tandem cell both can fully undergo cationic reactions, so that the possibility that the material of the skeleton layer still remains after annealing treatment is reduced, the interface impedance of the solar cell is reduced, and the device efficiency of the solar cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Method for preparing solar cell and solar cell

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on March 27, 2023, with application number 202310307721.6 and invention name “Method for preparing solar cells and solar cells”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of batteries, and in particular to a method for preparing a solar cell and a solar cell. Background Art

[0003] Photovoltaic technology is a technology that directly converts light energy into electrical energy and has become a research hotspot in the field of new energy. Among various solar cells, silicon-based solar cells have been commercialized due to their mature technology and good stability. Limited by the inherent characteristics of silicon materials, their photoelectric conversion efficiency has reached a bottleneck, and it is difficult to make a major breakthrough. Perovskite solar cells have excellent photoelectric properties such as adjustable band gap, low exciton binding energy, and high light absorption coefficient. The photoelectric conversion efficiency of single-junction cells has reached 25.7%. By connecting perovskite solar cells and heterojunction silicon (HJT) cells in series, the utilization rate of the spectrum can be improved. At present, there are still many problems to be solved in the industrial production and application of perovskite-silicon tandem cells.

[0004] Summary of the Invention

[0005] In one aspect of the present application, a method for preparing a solar cell is proposed, comprising: providing a heterojunction bottom cell, wherein a transparent composite layer, a hole transport layer, and a hole passivation layer are sequentially stacked on one side of the heterojunction bottom cell; forming a first cationic layer on the side of the hole passivation layer away from the hole transport layer; forming a skeleton layer on the side of the first cationic layer away from the hole passivation layer; forming a second cationic layer on the side of the skeleton layer away from the first cationic layer to obtain a preformed perovskite layer; annealing the preformed perovskite layer so that the first cationic layer, the second cationic layer, and the skeleton layer together form a perovskite light absorption layer; and sequentially forming a passivation layer, an electron transport layer, a buffer layer, and a second transparent electrode layer on the side of the perovskite light absorption layer away from the hole transport layer. Thus, the provision of the first cationic layer can effectively improve the interface contact and charge transfer within the solar cell, thereby improving the energy conversion efficiency of the solar cell.

[0006] According to an embodiment of the present application, forming a first cationic layer on a surface of the hole passivation layer away from the hole transport layer includes: forming the first cationic layer by a first evaporation process, wherein the first evaporation process satisfies at least one of the following conditions: the evaporation source of the first evaporation process includes at least one of formamidine vapor, formamidine bromide, formamidine iodide, methylamine chloride, methylamine bromide, and methylamine iodide; the evaporation rate of the first evaporation process is The vacuum degree of the first evaporation process is not greater than 10 -3 Pa. Thus, the first cationic layer can be formed by the first vapor deposition process.

[0007] According to an embodiment of the present application, the heterojunction bottom cell is disposed on a carrier, with the surface of the heterojunction bottom cell having the hole passivation layer facing the evaporation source. The carrier is reciprocated horizontally at a rate of 10 mm / s to 15 m / s. This facilitates the formation of a first cationic layer of uniform thickness.

[0008] According to an embodiment of the present application, the first evaporation process includes at least two evaporation sources, the distance between adjacent evaporation sources is fixed, the plane where the line connecting the adjacent evaporation sources lies is parallel to the plane where the carrier lies, and the distance between the plane where the line connecting the adjacent evaporation sources lies and the plane where the carrier lies is fixed. This helps to improve the formation effect of the perovskite light absorption layer.

[0009] According to an embodiment of the present application, forming a skeleton layer on the surface of the first cationic layer away from the hole passivation layer includes forming the skeleton layer using a second evaporation process, wherein the evaporation sources of the second evaporation process include a first evaporation source and a second evaporation source, and the second evaporation process meets at least one of the following conditions: the first evaporation source includes lead iodide; the second evaporation source includes at least one of cesium bromide, lead bromide, and lead chloride; and the ratio of the evaporation rate of the first evaporation source to the evaporation rate of the second evaporation source is 7-10. This helps to improve the reaction effect between the skeleton layer and the cationic layer.

[0010] According to an embodiment of the present application, forming a second cationic layer on a surface of the skeleton layer away from the first cationic layer includes: forming the second cationic layer by spin coating, wherein the spin coating liquid includes a cationic material and a solvent, wherein the cationic material includes: a first cationic material and a second cationic material; the spin coating satisfies at least one of the following conditions: the first cationic material includes at least one of formamidine iodide and formamidine bromide, and the second cationic material includes at least one of methylammonium bromide, methylammonium iodide, and methylammonium chloride; the solvent includes at least one of anhydrous ethanol and isopropanol; the concentration of the first cationic material in the spin coating liquid is 0.3 mol / L-0.6 mol / L; the concentration of the second cationic material is 0.15 mol / L-0.35 mol / L; the spin coating speed of the spin coating is 3000 rpm-6000 rpm, and the spin coating time is 20 s-40 s. This helps to improve the formation of the perovskite light absorption layer.

[0011] According to an embodiment of the present application, the annealing process satisfies at least one of the following conditions: a relative humidity of 5% to 40%; a temperature of 100°C to 150°C; and a duration of 15 to 30 minutes. This helps to improve the formation of the perovskite light-absorbing layer.

[0012] According to an embodiment of the present application, the conformal thickness of the first cationic layer is 5nm-20nm, and the conformal thickness of the skeleton layer is 300nm-400nm, thereby reducing the interface impedance between the perovskite light absorbing layer and the adjacent film layer.

[0013] According to an embodiment of the present application, the present invention further comprises: forming a back electrode on the surface of the heterojunction bottom cell away from the transparent composite layer; forming a positive electrode on the surface of the second transparent electrode layer away from the buffer layer; and forming an anti-reflection layer on the surface of the positive electrode away from the second transparent electrode layer. This helps to improve the energy conversion efficiency of the solar cell.

[0014] In another aspect of the present application, a solar cell is provided, wherein the solar cell is prepared by the aforementioned method. Therefore, the solar cell has all the features and advantages of the aforementioned method, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings; wherein:

[0016] FIG1 shows a schematic structural diagram of a solar cell according to an embodiment of the present application;

[0017] FIG2 shows a schematic diagram of a partial process for preparing a solar cell according to one embodiment of the present application;

[0018] FIG3 shows a schematic diagram of a partial structure of a solar cell in the related art;

[0019] FIG4 shows a schematic diagram of a partial process of preparing a solar cell according to another embodiment of the present application;

[0020] FIG5 shows a partial schematic diagram of a process for preparing a solar cell according to another embodiment of the present application;

[0021] FIG6 shows the voltage-current density curves of the solar cells in Example 1 and Comparative Example 1.

[0022] Explanation of the accompanying drawings: Lead iodide 10; heterojunction bottom cell 100; transparent composite layer 210; second transparent electrode layer 220; hole transport layer 310; hole passivation layer 320; perovskite light absorption layer 400; first cationic layer 410; skeleton layer 420; second cationic layer 430; passivation layer 500; electron transport layer 600; buffer layer 700; positive electrode 801; back electrode 802; anti-reflection layer 900. DETAILED DESCRIPTION

[0023] The following describes in detail embodiments of the present application. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application and are not to be construed as limiting the present application.

[0024] This application is based on the inventor's discovery and understanding of the following facts and problems:

[0025] A silicon heterojunction bottom cell refers to a cell that uses an n-type crystalline silicon wafer (C-Si) as the substrate light absorption area. After texturing and cleaning to obtain a texturized silicon wafer, an intrinsic amorphous silicon passivation layer (ia-Si:H) and a doped p-type amorphous silicon layer (pa-Si:H) are sequentially formed on the front side of the texturized silicon wafer (the surface close to the light incident side) through a deposition process; an intrinsic amorphous silicon passivation layer (ia-Si:H) and a doped n-type amorphous silicon layer (na-Si:H) are sequentially deposited on the back side of the texturized silicon wafer (the surface away from the light incident side), and a first transparent electrode layer is formed on the surface of the doped n-type amorphous silicon layer away from the intrinsic amorphous silicon layer. Specifically, a heterojunction bottom cell can be prepared according to the following method:

[0026] An n-type crystalline silicon wafer is provided. The n-type crystalline silicon wafer may have a resistivity of 1 Ω.cm-10 Ω.cm and a thickness of 50 μm-200 μm.

[0027] The n-type bulk silicon wafer 101 is sequentially polished, textured, and cleaned to form a textured silicon wafer. The textured silicon wafer serves as a light absorption layer of a silicon heterojunction bottom cell, and can convert photons into photogenerated carriers (electron-hole pairs).

[0028] Intrinsic amorphous silicon passivation layers are deposited on both sides of the textured silicon wafer, forming a first passivation layer on the front side of the textured silicon wafer and a second passivation layer on the back side. The first and second passivation layers primarily passivate the dangling bonds of the textured silicon wafer. The intrinsic amorphous silicon passivation layers can be fabricated using a plasma chemical vapor deposition (PECVD) process. Both the first and second passivation layers can be 5nm-10nm thick.

[0029] An n-type amorphous silicon layer is deposited on the first passivation layer to form a front field structure. The n-type amorphous silicon layer can be made using a PECVD process. The thickness of the n-type amorphous silicon layer can be 5nm-15nm.

[0030] A p-type amorphous silicon layer is deposited on the second passivation layer to form a back emitter. The p-type amorphous silicon layer can be made using a PECVD process. The thickness of the p-type amorphous silicon layer can be 5nm-15nm.

[0031] A first transparent electrode layer is formed on the p-type amorphous silicon layer to produce a silicon heterojunction bottom cell. This first transparent electrode layer primarily collects photogenerated carriers and transfers them to the rear metal electrode. Specifically, the material of the first transparent conductive layer can be at least one of indium tin oxide, tungsten-doped indium oxide, indium zinc oxide, and titanium-doped indium oxide. The first transparent electrode layer can be fabricated using a magnetron sputtering process. The thickness of the first transparent conductive layer can range from 70 nm to 120 nm.

[0032] For perovskite-silicon tandem cells, forming a perovskite top cell on the front of a silicon heterojunction bottom cell can achieve distributed absorption of the solar spectrum and achieve higher conversion efficiency. Methods for preparing perovskite top cells on the front of silicon heterojunction bottom cells include spin coating and vacuum deposition-spin coating. The inventors have discovered that spin coating is only suitable for depositing perovskite light-absorbing layers on polished or slightly textured silicon heterojunction bottom cells (texture size of 1μm-2μm). However, tandem cells prepared on polished or slightly textured silicon bottom cells suffer from partial light loss due to parasitic absorption, total internal reflection at the interface, and waveguide modes, thus affecting device efficiency. When the pyramid texture size exceeds 3μm, the perovskite light-absorbing layer prepared by spin coating has difficulty completely covering the pyramid apex, resulting in device short circuits or low energy conversion efficiency. The vacuum deposition-spin coating method has no specific requirements for the texture size of the textured silicon wafer used for heterojunction bottom cells and can completely cover even large-sized textures, achieving conformal growth.

[0033] Furthermore, the inventors discovered, referring to FIG3 , that when a perovskite light-absorbing layer is prepared using a vacuum deposition-spin coating method, the dense lead iodide skeleton layer formed by vacuum deposition makes it difficult for the cationic layer formed subsequently by spin coating to diffuse to the bottom, particularly to react with the skeleton layer at the base of the pyramid. Furthermore, as the thickness of the lead iodide skeleton layer increases, more lead iodide 10 remains at the base of the pyramid. Furthermore, due to the poor conductivity of lead iodide, the residual lead iodide 10 between the light-absorbing layer and the hole passivation layer 320′ in the finished solar cell significantly increases the interfacial resistance, thereby hindering interfacial charge transfer between the perovskite light-absorbing layer and adjacent film layers, resulting in low device energy conversion efficiency.

[0034] In one aspect of the present application, a method for preparing a solar cell is proposed, with reference to Figures 1 and 2, comprising: providing a heterojunction bottom cell 100, wherein the heterojunction bottom cell 100 has a surface on one side of an n-type amorphous silicon layer and further has a transparent composite layer 210, a hole transport layer 310, and a hole passivation layer 320 stacked in sequence; forming a first cation layer 410 on a surface on the side of the hole passivation layer 320 away from the hole transport layer; forming a bone cation layer 410 on a surface on the side of the first cation layer 410 away from the hole passivation layer 320; A skeleton layer 420 is provided; a second cationic layer 430 is formed on the surface of the skeleton layer 420 away from the first cationic layer 410 to obtain a preformed perovskite layer; the preformed perovskite layer is annealed to allow the first cationic layer 410, the second cationic layer 430 and the skeleton layer 420 to form a perovskite light absorption layer 400 together; a passivation layer 500, an electron transport layer 600, a buffer layer 700 and a second transparent electrode layer 220 are formed in sequence on the surface of the perovskite light absorption layer 400 away from the hole transport layer 320. In the present application, before depositing the skeleton layer 420, a first cationic layer 410 is pre-deposited on the surface of the hole passivation layer 320 away from the heterojunction bottom battery 100, and then a skeleton layer is formed by evaporation, and then a second cationic layer is formed by a spin coating process, and the above film layers are annealed. During the annealing process, the cationic material in the first cationic layer 410 pre-deposited at the bottom of the skeleton layer can fully react with the skeleton layer material located at the bottom of the skeleton layer 420 to form perovskite, and the second cationic layer 430 formed at the top of the skeleton layer 420 by the spin coating process can diffuse downward and react with most of the skeleton layer material located on the upper surface of the skeleton layer 420, thereby conformally growing on the surface of the heterojunction bottom battery to form a perovskite light absorption layer 400. The technical solution provided in this application can effectively solve the problem that the spin-coated cationic material cannot diffuse to the bottom of the skeleton layer for sufficient reaction due to the vacuum-deposited skeleton layer material being too dense, thereby resulting in excessive skeleton layer material remaining on the pyramid velvet surface and the bottom of the skeleton layer. This can effectively improve the interface contact and charge transfer of the perovskite light-absorbing layer, improve the energy conversion efficiency of the device, and promote the industrial development of perovskite-silicon stacked batteries.

[0035] It is understandable that in order to improve the energy conversion efficiency of solar cells, textured silicon wafers can be used to improve the light trapping effect. Therefore, when performing the film forming process on the heterojunction bottom cell, the conformal growth of the film should be achieved as much as possible, that is, the shape of the film formed on the heterojunction bottom cell should be consistent with or close to the velvet shape of the textured silicon wafer surface, so as to further improve the light trapping effect of the solar cell.

[0036] According to some embodiments of the present application, the method for forming the first cationic layer is not particularly limited. For example, forming the first cationic layer on the surface of the hole passivation layer away from the hole transport layer may include: forming the first cationic layer by a first evaporation process, wherein the first evaporation process may meet at least one of the following conditions: the evaporation source of the first evaporation process includes at least one of formamidine chloride, formamidine bromide, formamidine iodide, methylamine chloride, methylamine bromide and methylamine iodide; the evaporation rate of the first evaporation process is The vacuum degree of the first evaporation treatment is not greater than 10 -3 Pa. When the evaporation rate of the first evaporation process is less than When the evaporation rate is too slow, the first cationic layer formed is too dense and difficult to fully react with the skeleton layer; when the evaporation rate of the first evaporation treatment is greater than When the vacuum level during the first evaporation process is within the above range, the particles emitted by the evaporation source collide less with each other, resulting in a higher-quality first cation layer.

[0037] According to some embodiments of the present application, the size of the textured silicon wafer is not particularly limited. For example, the technical solution in the present application can be applied to a textured silicon wafer with a pyramid texture surface size of 3μm-8μm.

[0038] According to some embodiments of the present application, with reference to Figures 4 and 5 , during the first evaporation process, a heterojunction bottom cell can be placed on a carrier, with the surface of the heterojunction bottom cell having the hole clocking layer facing the evaporation source. The carrier can be moved back and forth horizontally during the evaporation process at a rate of 10 mm / s to 15 mm / s. By controlling the movement rate of the carrier, the uniformity of the film formation of the first cationic layer can be effectively improved, achieving conformal growth of the first cationic layer.

[0039] According to some embodiments of the present application, in order to further promote the reaction between the cationic material of the first cationic layer and the skeleton layer material, at least two or more evaporation sources can be used in the first evaporation treatment to perform the first evaporation treatment, referring to Figure 4, wherein the distance between adjacent evaporation sources should remain fixed, and the plane where the line connecting the adjacent evaporation sources is located can be parallel to the plane where the carrier is located, so that the nozzle of the evaporation source can be perpendicular to the carrier, thereby improving the evaporation efficiency, and the distance between the plane where the line connecting the adjacent evaporation sources is located and the plane where the carrier is located can also be kept fixed, thereby improving the uniformity of the evaporation, thereby obtaining a first cationic layer containing multiple cationic materials. According to some embodiments of the present application, the evaporation source of the first evaporation treatment can be formamidine iodide and methylammonium bromide, or the evaporation source of the first evaporation treatment can be formamidine bromide and methylammonium iodide.

[0040] According to some embodiments of the present application, the process for forming the skeleton layer is not particularly limited. For example, forming the skeleton layer on the surface of the first cationic layer away from the hole passivation layer may include: forming the skeleton layer using a second evaporation process, wherein the evaporation source of the second evaporation process includes a first evaporation source and a second evaporation source, and the second evaporation process meets at least one of the following conditions: the first evaporation source may include lead iodide; the second evaporation source may include at least one of cesium bromide, lead bromide, and lead chloride; and the ratio of the evaporation rate of the first evaporation source to the evaporation rate of the second evaporation source may be 7-10. By controlling the ratio of the evaporation rates, the content and / or ratio of the two substances in the skeleton layer can be controlled. According to some embodiments of the present application, when the first evaporation source is lead iodide, the second evaporation source may be lead bromide or lead chloride. Furthermore, when the second evaporation source is lead bromide or lead chloride, the second evaporation process may also include a third evaporation source, which may be cesium bromide.

[0041] According to some embodiments of the present application, the process of forming the second cationic layer is not particularly limited. For example, forming the second cationic layer on the surface of the skeleton layer away from the first cationic layer may include: forming the second cationic layer by spin coating, the spin coating liquid of the spin coating includes a cationic material and a solvent, wherein the cationic material may include: a first cationic material and a second cationic material; the spin coating satisfies at least one of the following conditions: the first cationic material may include at least one of formamidine iodide and formamidine bromide, and the second cationic material may include at least one of methylamine bromide, methylamine iodide and methylamine chloride; the solvent includes at least one of anhydrous ethanol and isopropanol; the concentration of the first cationic material in the spin coating liquid is 0.3 mol / L-0.6 mol / L; the concentration of the second cationic material is 0.15 mol / L-0.35 mol / L; the spin coating speed of the spin coating is 3000 rpm-6000 rpm, and the spin coating time is 20s-40s. According to some specific embodiments of the present application, when the first cationic material is formamidine iodide, the second cationic material can be methylammonium chloride and methylammonium bromide. At this time, the concentration of formamidine iodide in the spin-coating liquid can be 0.3 mol / L-0.6 mol / L, the concentration of methylammonium bromide in the spin-coating liquid can be 0.1 mol / L0.2 mol / L, and the concentration of methylammonium chloride in the spin-coating liquid can be 0.05 mol / L-0.15 mol / L; when the first cationic material is formamidine bromide, the second cationic material can be methylammonium chloride and methylammonium iodide.

[0042] According to some embodiments of the present application, an annealing process is performed to allow the cationic material in the deposited first cationic layer and the cationic material in the spin-coated second cationic layer to react with the evaporated skeleton layer to form a perovskite light-absorbing layer 400. The annealing process satisfies at least one of the following conditions: a relative humidity of 5%-40%; a temperature of 100°C-150°C; and an annealing time of 15-30 minutes. The annealing temperature and time can affect the film quality. When the annealing temperature is less than 100°C and / or the annealing time is less than 15 minutes, the perovskite phase transition temperature is not reached, or the reaction time is too short, resulting in a low perovskite yield. When the annealing temperature is greater than 150°C and / or the annealing time is greater than 30 minutes, the perovskite decomposes and loses its light-absorbing effect. According to some embodiments of the present application, annealing and crystallization can form a perovskite light-absorbing layer 400 with a wide bandgap (1.63 eV-1.70 eV).

[0043] According to some embodiments of the present application, conformal thickness refers to the average thickness of the film layer in a direction perpendicular to the surface to which the film layer is attached. In this application, the conformal thickness of the first cationic layer can be 5nm-20nm, and the conformal thickness of the skeleton layer can be 300nm-400nm, ultimately forming a perovskite light-absorbing layer with a thickness of 450nm-500nm.

[0044] According to some embodiments of the present application, it further includes: forming a back electrode on the surface of the heterojunction bottom cell away from the transparent composite layer; forming a positive electrode on the surface of the second transparent electrode layer away from the buffer layer; forming an anti-reflection layer on the surface of the positive electrode away from the second transparent electrode layer. In this way, a solar cell with lower interface impedance and higher energy conversion efficiency can be obtained. The positive electrode and the negative electrode are patterned metal electrodes, and the materials of the positive electrode and the negative electrode can independently include at least one of silver, copper, and aluminum. The thickness of the positive electrode and the negative electrode can be 150nm-300nm, and the evaporation rate of the materials of the positive electrode and the negative electrode can be

[0045] The present application is directed to the problem that the vacuum-deposited skeleton layer (such as lead iodide) in the vacuum deposition-spin coating method (two-step method) perovskite-silicon stacked cell technology is too dense. When the thickness of the deposited lead iodide reaches a certain value, the spin-coated cations are difficult to react completely with the lead iodide at the bottom of the skeleton layer. A technical solution for pre-depositing a cation layer is proposed to solve the problem that the bottom lead iodide in the related art is residual, hindering the interface charge transfer, and causing the device efficiency to be low. The present application has at least the following advantages compared with the related art: in the dense lead iodide skeleton layer in the related art, the lead iodide located near the side of the heterojunction bottom cell cannot effectively react with the spin-coated cation solution, and the residual unreacted lead iodide will significantly reduce the device efficiency due to the presence of poor conductivity. In the present application, the first cation layer is pre-deposited before the skeleton layer is formed, so that the surfaces on both sides of the skeleton layer can fully react with the cations, greatly reducing the possibility that the skeleton layer material still has residues after annealing, significantly reducing the interface impedance of the solar cell, and improving the device efficiency of the solar cell.

[0046] In another aspect of the present application, a solar cell is provided, which is prepared by the above method. Therefore, the solar cell has all the features and advantages of the above method, which will not be described in detail here.

[0047] According to some embodiments of the present application, the structure of the solar cell is not particularly limited. For example, the material of the transparent composite layer may include indium tin oxide (ITO) and / or indium zinc oxide (IZ0), and the thickness of the transparent composite layer may be 20nm-30nm; the material of the hole transport layer may include nickel oxide or Spiro-TTB, and the thickness of the hole transport layer may be 20nm-30nm; the material of the hole passivation layer may include 2PACz or 4PACz.

[0048] The present invention will be described below by way of specific examples. It should be noted that the following examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. Where specific techniques or conditions are not specified in the examples, they are determined according to the techniques or conditions described in the literature in this area or according to the product specifications. Reagents or instruments not specified by manufacturer are all commercially available conventional products.

[0049] Example 1:

[0050] S1: A patterned transparent composite layer of ITO with a thickness of 20 nm was prepared on one side of the heterojunction bottom cell using magnetron sputtering.

[0051] S2: A hole transport layer is prepared on one side of the transparent composite layer by magnetron sputtering. The material is nickel oxide with a thickness of 20 nm.

[0052] S3: A hole passivation layer was prepared on one side of the hole transport layer by spin coating. The material was 2PACz, the concentration of the spin coating solution was 0.8 mg / mL, the spin coating speed was 4000 rpm, the annealing temperature was 100°C, and the annealing time was 10 min.

[0053] S4-1: Referring to (a) in FIG4 , a first cationic layer is vacuum deposited on one surface of the hole passivation layer using a dual-source co-evaporation process. The evaporation sources are formamidine iodide and methylamine bromide. The evaporation rate is The thickness of the first cationic layer is 10 nm;

[0054] S4-2: Referring to (b) in Figure 4, a skeleton layer is prepared by evaporating lead iodide and cesium bromide on one surface of the first cationic layer using a dual-source co-evaporation process, and the evaporation rate ratio of lead iodide and cesium bromide is 7:1; the evaporation rate error during the evaporation process is less than 5%, and the thickness of the skeleton layer is 380nm.

[0055] S4-3: Referring to (e) in FIG4 , a second cationic layer was prepared on one surface of the skeleton layer by spin coating. The spin coating solution was a mixed solution of formamidine iodide, methylammonium chloride, and methylammonium bromide. The solvent was isopropyl alcohol. The concentration of formamidine iodide in the spin coating solution was 0.4 mol / L, the concentration of methylammonium bromide in the spin coating solution was 0.15 mol / L, and the concentration of methylammonium chloride in the spin coating solution was 0.1 mol / L. The spin coating speed was 5000 rpm, the spin coating time was 30 s, and the spin coating environment required a humidity of less than 10% and a temperature of 25° C.

[0056] S4-4: After the second cationic layer is prepared, annealing is performed at a relative humidity of 20% at a temperature of 120° C. for 20 minutes. During the annealing process, the cations in the first cationic layer and the cations in the second cationic layer react with the co-evaporated lead iodide and cesium bromide skeleton layer to crystallize to form a perovskite light-absorbing layer having a thickness of 450 nm.

[0057] S5: A passivation layer 500 is prepared on one side of the perovskite light absorbing layer by a vacuum deposition process; the passivation layer material is LiF, the thickness is 1 nm, and the evaporation rate is

[0058] S6: Evaporating an electron transport layer 600 on one side of the passivation layer; the electron transport layer material is C 60 , thickness is 18nm, evaporation rate

[0059] S7: A buffer layer 700 is formed on one surface of the electron transport layer by atomic layer deposition (ALD). The material is tin dioxide and the thickness is 20 nm.

[0060] S8: forming a second transparent electrode layer on one side of the buffer layer by magnetron sputtering, the material of which is ITO with a thickness of 100 nm;

[0061] S9-1: Evaporate the positive electrode on one side of the second transparent electrode. The material is silver with a thickness of 150nm and the evaporation rate is

[0062] S9-2: Evaporate the back electrode on the back of the heterojunction bottom cell. The material is silver with a thickness of 150nm and the evaporation rate is

[0063] S10: On the side of the positive electrode away from the heterojunction bottom cell, an anti-reflection layer is prepared by evaporation process. The material is LiF, the thickness is 100nm, and the evaporation rate is The refractive index n is approximately 1.4.

[0064] Example 2:

[0065] Example 2 is consistent with Example 1, except that, referring to (a) in FIG5 , the cationic material in the first cationic layer is formamidine bromide, the thickness is 10 nm, and the evaporation rate is The process flow is shown in FIG3 , and the rest is consistent with that of Example 1.

[0066] Example 3:

[0067] Example 2 is consistent with Example 1, except that the first cationic layer is prepared by a three-source co-evaporation process, the evaporation sources are formamidine iodide, methylammonium chloride and methylammonium bromide, the co-evaporation film thickness is 18nm, and the evaporation rate is

[0068] Comparative Example 1:

[0069] Comparative Example 1 is consistent with Example 1, except that the first cationic layer is not prepared.

[0070] Comparative Example 2:

[0071] Comparative Example 2 is consistent with Example 1, except that the first cationic layer is prepared by solution spin coating, the concentration of the cationic material in the spin coating solution is 0.2M, and the rotation speed is 5000 rpm.

[0072] Comparative Example 3:

[0073] Comparative Example 3 is consistent with Example 1, except that the first cationic layer is prepared by spraying, and the concentration of the cationic material in the spraying liquid is 0.2M.

[0074] The solar cells in Examples 1-3 and Comparative Examples 1-3 were tested as follows. Wavelabs solar simulators were used for testing. Before testing, the simulated sunlight intensity was calibrated using a standard silicon cell. Test conditions were: AM1.5, 1000 W / m 2 The test environment temperature was 25°C. The test scanning voltage range was (-0.2V)-(1.9V), with a step of 0.02V. The test results are shown in Table 1:

[0075] Open circuit voltage (V oc ) Test: V oc It is the potential difference generated by the accumulation of carriers at both ends of the device. In the JV curve, the intercept of the horizontal axis is V oc .

[0076] Short circuit current density (J sc ) Test: J sc It is the ratio of the current generated by the device to the effective area of ​​illumination. In the JV curve, the intercept of the ordinate is J sc .

[0077] Fill factor (FF) test: FF is the maximum power output point P of the device max With V oc and J sc The ratio of products.

[0078] Photovoltaic conversion efficiency (PCE) testing: PCE is a key parameter in battery performance, indicating the ratio of incident light energy converted to effective electrical energy. PCE is numerically equal to the product of open-circuit voltage, short-circuit current density, and fill factor: PCE = Voc × Jsc × FF.

[0079] The experimental results show that the cationic material in the first cationic layer pre-deposited at the bottom of the skeleton layer will fully react with the skeleton layer material at the bottom of the skeleton layer to form perovskite, and the second cationic layer formed by the spin coating process on the top of the skeleton layer will diffuse downward and react with most of the skeleton layer material on the upper surface of the skeleton layer, and then conformally grow on the surface of the heterojunction bottom battery to form a perovskite light-absorbing layer, thereby effectively solving the problem that when the vacuum-deposited skeleton layer material is too dense, the spin-coated cationic material cannot diffuse to the bottom of the skeleton layer for sufficient reaction, resulting in excessive residual skeleton layer material on the pyramid velvet and the bottom of the skeleton layer. This can effectively improve the interface contact and charge transfer of the perovskite light-absorbing layer, improve the energy conversion efficiency of the device, and promote the industrial development of perovskite-silicon stacked batteries.

[0080] Specifically, referring to Figure 6 , the device performance of Example 1 (Target) was significantly improved compared to that of Comparative Example 1 (Control), achieving an efficiency of 24.71%. The solar cell using spin coating or spray coating to form a pre-deposited cationic layer showed a slight improvement in performance compared to the solar cell without a pre-deposited cationic layer, but the effect was not significant.

[0081] In this application, all numerical values ​​disclosed herein are approximate, regardless of whether the word "about" or "approximately" is used. The numerical value of each number may vary by less than 10% or by a reasonable difference considered by a person skilled in the art, such as 1%, 2%, 3%, 4% or 5%.

[0082] In the description of this application, it should be understood that the terms "length", "width", "thickness", "up", "down", "front", "back", "left", "right", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on this application.

[0083] In the description of this application, "first feature" and "second feature" may include one or more of the features.

[0084] In the description of this application, “plurality” means two or more.

[0085] In the description of this application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for example, and may be any technical feature connected by "and / or" in this application.

[0086] Unless otherwise specified, all technical and scientific terms used in this application have the same meanings as commonly understood by those skilled in the art to which this application belongs. All patents and publications referred to in this application are incorporated herein by reference in their entirety. The terms "comprising" or "including" are open-ended expressions, meaning that they include the contents specified in this application but do not exclude contents elsewhere.

[0087] In the description of this specification, reference to the terms "one embodiment", "another embodiment", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and features of different embodiments or examples without contradiction.

Claims

1. A method for preparing a solar cell, comprising: A heterojunction bottom battery is provided, wherein a transparent composite hole transport layer and a hole passivation layer are sequentially stacked on one side surface of the heterojunction bottom battery; forming a first cationic layer on a surface of the hole passivation layer away from the hole transport layer; forming a skeleton layer on a surface of the first cation layer away from the hole passivation layer; forming a second cationic layer on a surface of the skeleton layer away from the first cationic layer to obtain a preformed perovskite layer; Annealing the preformed perovskite layer so that the first cation layer, the second cation layer and the skeleton layer together form a perovskite light absorption layer; A passivation layer, an electron transport layer buffer layer and a second transparent electrode layer are sequentially formed on a surface of the perovskite light absorbing layer away from the hole transport layer.

2. The method according to claim 1, wherein: The forming of the first cationic layer on the surface of the hole passivation layer away from the hole transport layer comprises: forming the first cationic layer by a first evaporation treatment, wherein the evaporation source of the first evaporation treatment comprises at least one of formamidine chloride, formamidine bromide, formamidine iodide, methylammonium chloride, methylammonium bromide and methylammonium iodide.

3. The method according to claim 2, wherein: The evaporation rate of the first evaporation process is 4. The method according to any one of claims 2 to 3, wherein: The vacuum degree of the first evaporation treatment is not greater than 10 -3 Pa.

5. The method according to any one of claims 2 to 4, wherein: The heterojunction bottom cell is arranged on a carrier, and a surface of one side of the heterojunction bottom cell having the hole passivation layer is arranged toward the evaporation source. The carrier reciprocates in a horizontal direction, and the reciprocating motion rate is 10 mm / s-15 m / s.

6. The method according to claim 5, wherein: The first evaporation process includes at least two evaporation sources, the distance between adjacent evaporation sources is fixed, the plane where the line connecting adjacent evaporation sources is located is parallel to the plane where the carrier is located, and the distance between the plane where the line connecting adjacent evaporation sources is located and the plane where the carrier is located is fixed.

7. The method according to any one of claims 1 to 6, wherein: The forming of the skeleton layer on the surface of the first cation layer away from the hole passivation layer comprises: forming the skeleton layer by a second evaporation process, wherein the evaporation source of the second evaporation process comprises a first evaporation source and a second evaporation source, and the first evaporation source comprises lead iodide.

8. The method according to claim 7, wherein: The second evaporation source includes at least one of cesium bromide, lead bromide and lead chloride.

9. The method according to any one of claims 7 to 8, wherein: The ratio of the evaporation rate of the first evaporation source to the evaporation rate of the second evaporation source is 7-10.

10. The method according to any one of claims 1 to 9, wherein: The forming of the second cationic layer on the surface of the skeleton layer away from the first cationic layer comprises: forming the second cationic layer by spin coating, wherein the spin coating liquid of the spin coating comprises a cationic material and a solvent, and the cationic material comprises: a first cationic material and a second cationic material; the first cationic material comprises at least one of formamidine iodide and formamidine bromide, and the second cationic material comprises at least one of methylammonium bromide, methylammonium iodide and methylammonium chloride.

11. The method according to claim 10, wherein: The solvent includes at least one of anhydrous ethanol and isopropanol.

12. The method according to any one of claims 10 to 11, wherein: The concentration of the first cationic material in the spin coating solution is 0.3 mol / L-0.6 mol / L.

13. The method according to any one of claims 10 to 12, wherein: The concentration of the second cationic material is 0.15 mol / L-0.35 mol / L.

14. The method according to any one of claims 10 to 13, wherein: The spin coating speed of the spin coating process is 3000rpm-6000rpm, and the spin coating time is 20s-40s.

15. The method according to any one of claims 1 to 14, wherein: The relative humidity of the annealing treatment is 5%-40%.

16. The method according to any one of claims 1 to 15, wherein: The annealing treatment is performed at a temperature of 100°C-150°C.

17. The method according to any one of claims 1 to 16, wherein: The annealing treatment time is 15min-30min.

18. The method according to any one of claims 1 to 17, wherein: The conformal thickness of the first cationic layer is 5nm-20nm, and the conformal thickness of the skeleton layer is 300nm-400nm.

19. The method according to any one of claims 1 to 18, wherein: Further including: Forming a back electrode on a surface of the heterojunction bottom cell away from the transparent composite layer; forming a positive electrode on a surface of the second transparent electrode layer away from the buffer layer; An anti-reflection layer is formed on a surface of the positive electrode at a side away from the second transparent electrode layer.

20. A solar cell, wherein the solar cell is prepared by the method according to any one of claims 1 to 19.

Citation Information

Patent Citations

  • High-efficiency perovskite solar cell and preparation method thereof

    CN111640870A

  • Laminated battery

    CN112086535A

  • Method for simultaneously improving open-circuit voltage and stability of full-suede perovskite / crystalline silicon laminated solar cell

    CN114267789A

  • Method for preparing solar cell and solar cell

    CN116344674A

  • Package sorting device

    KR102574268B1