Negative electrode sheet, battery and electric device
By adding 0.1% to 5% of inorganic porous materials to the negative electrode sheet of lithium-ion batteries, the problem of high carrier transmission impedance of the negative electrode sheet is solved, the rate performance and cycle life of the battery are improved, and the demand for high-rate applications is met. Reduced costs.
Patent Information
- Application Number
- PCT/CN2024/084308
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
The existing lithium-ion battery negative electrode sheet has high carrier transmission impedance, which restricts the rate performance of the battery. Modified negative electrode active materials are costly and have limited effects.
Add 0.1% to 5% of inorganic porous materials to the negative electrode sheet to improve ion conductivity, shorten carrier conduction paths, reduce polarization phenomena, and optimize pore structure.
It effectively improves the rate performance of the battery to meet the needs of high-rate applications, while reducing costs and ensuring conductivity and cycle life.
Smart Images

Figure CN2024084308_03102024_PF_FP_ABST
Abstract
Description
Negative electrode sheet, battery and electrical equipment
[0001] Priority information
[0002] This disclosure claims priority to and benefits of patent application No. 202310338119.9 filed with the State Intellectual Property Office of China on March 31, 2023, and incorporates the entire text of the patent application herein by reference. Technical Field
[0003] The present disclosure relates to the technical field of batteries, and in particular to a negative electrode sheet, a battery, and an electrical device. Background Art
[0004] Secondary batteries (e.g., lithium-ion batteries) are widely used in new energy vehicles, portable electronics, and large-scale energy storage devices due to their high operating voltage, high energy density, long cycle life, and low self-discharge. The performance of secondary batteries depends primarily on the physical and chemical properties of their positive and negative electrodes. The high transfer impedance and severe polarization of charge carriers (e.g., lithium ions) in the negative electrode limit the rate performance of secondary batteries (e.g., lithium-ion batteries).
[0005] In the prior art, the mobility of charge carriers (e.g., lithium ions) within the negative electrode sheet is increased by modifying the negative electrode active material, thereby improving the battery's rate performance. However, modified negative electrode active materials are expensive and only improve the diffusion of charge carriers (e.g., lithium ions) within the negative electrode active material, with little effect on the diffusion of charge carriers between the negative electrode active materials within the electrode sheet.
[0006] Therefore, it is necessary to provide a new negative electrode sheet to meet the application requirements of high rate performance of secondary batteries (such as lithium-ion batteries).
[0007] Public content
[0008] In view of this, the present disclosure provides a negative electrode sheet that can meet the high rate performance of a secondary battery.
[0009] A first aspect of the present disclosure provides a negative electrode sheet, comprising a current collector and a negative electrode active material layer coated on at least one side of the current collector; the negative electrode active material layer comprises a negative electrode active material, an inorganic porous material and a first binder; the inorganic porous material accounts for 0.1% to 5% of the total mass of the negative electrode active material layer.
[0010] The negative electrode sheet disclosed in the present invention contains 0.1% to 5% of inorganic porous material, which can effectively improve the ionic conductivity of the negative electrode sheet and enhance the rate performance of the negative electrode sheet and the corresponding battery. The pores in the inorganic porous material can absorb electrolyte. When the inorganic porous material is added to the negative electrode sheet, it can not only serve as a buffer pool for the electrolyte in the negative electrode sheet, but also improve the pore structure of the negative electrode sheet. During the battery charging and discharging process, the electrolyte penetrates from the pores of the inorganic porous material to the negative electrode active material, shortening the carrier (lithium ion) conduction path and reducing or alleviating the polarization phenomenon in the negative electrode sheet. If the content of the inorganic porous material in the negative electrode sheet is too high, it will affect the conductivity of the negative electrode sheet. If the content of the inorganic porous material in the negative electrode sheet is too low, the ionic conductivity of the negative electrode sheet will not be significantly improved. In this way, when the inorganic porous material in the present invention accounts for 0.1% to 5% of the total mass of the negative electrode active material layer, it can effectively improve the rate performance of the negative electrode sheet and the battery.
[0011] A second aspect of the present disclosure provides a battery, comprising a positive electrode sheet, an electrolyte, a diaphragm, and the negative electrode sheet provided in the first aspect.
[0012] Since the battery includes the negative electrode sheet provided by the first aspect of the present disclosure, the battery has a higher rate performance and meets more application requirements.
[0013] A third aspect of the present disclosure provides an electrical device, comprising the battery provided in the second aspect of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] FIG1 is a pore structure distribution curve of the inorganic porous material (mesoporous silica) disclosed in the present invention.
[0015] Detailed Description of the Invention
[0016] The present disclosure is further illustrated by the following examples and comparative examples. These examples are only used to illustrate the present disclosure and the present disclosure is not limited to the following examples. Any modification or equivalent replacement of the technical solution of the present disclosure without departing from the scope of the technical solution of the present disclosure shall be included in the scope of protection of the present disclosure.
[0017] An embodiment of the present disclosure provides a negative electrode sheet, which includes a current collector and a negative electrode active material layer coated on at least one side of the current collector; the negative electrode active material layer includes a negative electrode active material, an inorganic porous material and a first binder; the inorganic porous material accounts for 0.1% to 5% of the total mass of the negative electrode active material layer.
[0018] The negative electrode sheet disclosed in the present invention contains 0.1% to 5% of inorganic porous material, which can effectively improve the ionic conductivity of the negative electrode sheet and enhance the rate performance of the negative electrode sheet and the corresponding battery. The pores in the inorganic porous material can absorb electrolyte. When added to the negative electrode sheet, it can not only serve as a buffer pool for the electrolyte in the negative electrode sheet, but also improve the pore structure of the negative electrode sheet. During the charge and discharge process of the battery, the electrolyte penetrates from the pores of the inorganic porous material to the negative electrode active material, shortening the carrier (lithium ion) conduction path, reducing or alleviating the polarization phenomenon in the negative electrode sheet, and enhancing the rate performance of the negative electrode sheet and the battery. In addition, the inorganic porous material has stable chemical properties and will not destroy the electrochemical reaction system of the battery.
[0019] Inorganic porous materials have relatively poor electrical conductivity and energy storage properties (e.g., converting chemical energy into electrical energy during the storage and release of lithium ions). Excessive (greater than 5%) content of inorganic porous materials in the negative electrode sheet can affect the negative electrode's conductivity and indirectly reduce the content of the negative electrode active material, thereby affecting the negative electrode's energy density. However, low (less than 0.1%) content of inorganic porous materials has little impact on battery rate performance. Therefore, the content of inorganic porous materials in the negative electrode sheet is crucial to the present disclosure.
[0020] In some embodiments of the present disclosure, the inorganic porous material accounts for 0.2% to 3% of the total mass of the negative electrode active material layer.
[0021] When the inorganic porous material accounts for 0.2% to 3% of the total mass of the negative electrode active material layer, the uniformity of the dispersion of the inorganic porous material in the negative electrode sheet can be ensured, thereby achieving the effect of a uniform electrode pore structure, further shortening the electrolyte diffusion path, reducing the lithium ion transfer impedance, and improving the electrode polarization.
[0022] The inorganic porous material content in the negative electrode sheet can be measured using a thermogravimetric method. The method involves scraping the first solid material from the current collector after removing charge carriers (e.g., lithium ions), washing it with dilute hydrochloric acid, and drying it at 120°C for 2 hours. A certain mass (m1) of the first solid material is placed in the sample tray of a TA TGA 2050 thermogravimetric analyzer and pyrolyzed at 800°C in an air atmosphere. The residual mass is m2. The percentage of inorganic porous material is calculated as (mass of the residual mass (m2) / first solid material (m1)) * 100%.
[0023] In the present disclosure, the negative electrode active material layer can be applied to one side of the current collector. The negative electrode active material layer can also be applied to both sides of the current collector. When the negative electrode active material layer is applied to both sides of the current collector, the thickness, surface density, component content, etc. of the negative electrode active material layers on the two sides of the current collector can be independently designed according to application requirements and can be the same or different.
[0024] In the present disclosure, the negative electrode active material may be a carbon-based material.
[0025] The carbon-based material can be one or a combination of artificial graphite, natural graphite, soft carbon, hard carbon, mesophase carbon microbeads, and carbon fibers.
[0026] In the present disclosure, the current collector may be any one of copper foil, carbon-coated copper foil, polymer-coated copper foil, carbon cloth, carbon nanotube film or carbon paper.
[0027] In the present disclosure, the current collector may also be any one of aluminum foil, carbon-coated aluminum foil, and polymer-coated aluminum foil (for example, for the negative electrode current collector of a sodium ion battery).
[0028] In the present disclosure, the binder includes one or a combination of several of styrene butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyethylene acrylic acid (PEAA), sodium alginate, carboxymethyl chitosan, polyacrylonitrile (PAN) and polyvinyl alcohol (PVA).
[0029] In some embodiments of the present disclosure, the porosity of the negative electrode sheet is 20% to 60%.
[0030] In the present disclosure, the negative electrode sheet contains an inorganic porous material. It can be understood that the pores of the negative electrode sheet include the pores of the inorganic porous material itself, the gaps formed by the disordered stacking of the inorganic porous material and the negative electrode active material, and the gaps formed by the disordered stacking of the negative electrode active materials. The porosity of the negative electrode sheet is in the range of 20% to 60%, the carrier (lithium ion) shuttle efficiency in the negative electrode sheet is good, and the negative electrode sheet and the battery have a high rate performance; at the same time, the negative electrode sheet has a high liquid storage capacity, which can provide more sufficient electrolyte during the battery cycle and increase the cycle life of the battery. Exemplarily, the porosity of the negative electrode sheet can be 20%, 30%, 40%, 50% or 60%, etc.
[0031] In the present disclosure, the porosity of the negative electrode sheet is further preferably 30% to 50%. When the porosity of the negative electrode sheet is within this range, the mechanical properties of the negative electrode sheet can be further improved, thereby further enhancing the cycle stability of the battery.
[0032] The porosity of the negative electrode sheet is determined by cutting the negative electrode sheet into sheets of a certain area, drying the sheets in a vacuum drying oven at 120°C for 12 hours, removing them from the oven, and cooling them in a desiccator before testing. The thickness of the sample is first measured with a micrometer (excluding the thickness of the current collector foil). The apparent volume (V1) of the sample is calculated based on the sample surface area and thickness. The true volume (V2) of the sample is then measured using a true density meter (excluding the volume of the current collector foil). The following equation is used to determine the porosity of the negative electrode sheet: (true volume (V2) / apparent volume (V1)) * 100%.
[0033] In some embodiments of the present disclosure, the liquid absorption rate of the negative electrode sheet is 2 to 8 mg / min.
[0034] It can be understood that the inorganic porous material filled in the negative electrode sheet changes the pore structure in the negative electrode sheet, making the liquid absorption rate of the negative electrode sheet 2 to 8 mg / min, and the corresponding battery has a higher rate performance.
[0035] The liquid absorption rate of the negative electrode sheet refers to the amount of electrolyte absorbed by the negative electrode sheet per unit time; the method for determining the liquid absorption rate of the negative electrode sheet is as follows: the negative electrode sheet is cut into a film of a certain area, the film is dried in a vacuum drying oven at 120°C for 12 hours, taken out and placed in a desiccator for cooling before testing. A 2cm×5cm negative electrode sheet is fixed on the stage of the SDC-2000S contact angle tester, and a certain mass of electrolyte (m) is vertically dripped on the negative electrode sheet through a syringe. The time (t) taken for the electrolyte to be completely absorbed is recorded by a camera. The liquid absorption rate of the negative electrode sheet = the mass of the electrolyte dripped (m) / the time (t) taken for the electrolyte to be completely absorbed. The test is repeated 5 times at different positions of the electrode sheet and the average value is taken. The electrolyte used in the present disclosure is: ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate are mixed in a volume ratio of 1:1:1 to prepare an electrolyte containing 1M LiPF6; the test temperature is 25°C. Note: The test results may vary slightly depending on the type of electrolyte and test environment.
[0036] In some embodiments of the present disclosure, the dielectric constant of the inorganic porous material is ε, 0<ε≤50.
[0037] In the present disclosure, the dielectric constant of the inorganic porous material in the negative electrode sheet is within the above range, which can stabilize the contact interface between the negative electrode sheet and the electrolyte, reduce or alleviate its side reactions with the electrolyte, thereby improving the coulombic efficiency of the battery and further increasing the cycle life of the battery.
[0038] In the present disclosure, the dielectric constant ε of the inorganic porous material is further preferably 0 < ε ≤ 10. That is, the lower the dielectric constant of the inorganic porous material, the better the performance, provided that the application requirements are met. For example, the dielectric constant of the inorganic porous material can be, but is not limited to, 0.5, 1, 1.56, 3, 3.6, 6, 6.5, 8.8, or 10.
[0039] The dielectric constant of the inorganic porous material is determined by using an Agilent Technologies E8362B vector network tester to test the dielectric constant of the sample in the frequency range of 8.2-12.4 GHz. The powder to be tested (mass M1) and paraffin wax (mass M2) are heated and evenly mixed in a ratio of M1:M2=1:4, and then poured into a standard copper flange. After curing in air, a rectangular sample of 22.86 mm (length) × 10.16 mm (width) × 2.52 mm thick is obtained for testing. The real part of the dielectric constant in the test result is the dielectric constant ε of the first inorganic porous material.
[0040] In some embodiments of the present disclosure, the inorganic porous material includes at least one of: porous oxide of Si, porous nitride of Si, porous fluoride of Si, porous oxide of Ti, porous nitride of Ti, porous fluoride of Ti, porous oxide of Zn, porous nitride of Zn, porous fluoride of Zn, porous oxide of Mg, porous nitride of Mg, porous fluoride of Mg, porous oxide of Zr, porous nitride of Zr, porous fluoride of Zr, porous oxide of Ca, porous nitride of Ca, porous fluoride of Ca, porous oxide of Zn, porous nitride of Zn, porous fluoride of Zn, porous oxide of Ba, porous nitride of Ba, and porous fluoride of Ba.
[0041] In some embodiments of the present disclosure, the inorganic porous material is further preferably at least one of porous silica, porous titanium oxide, porous alumina or porous boehmite. The above-mentioned inorganic porous materials have relatively better dielectric properties, and are filled between the negative electrode active materials to help reduce the side reactions at the interface of the negative electrode sheet; they have a certain mechanical strength, and can effectively alleviate the uneven pore structure in the negative electrode sheet caused by the expansion and contraction of the negative electrode active materials during the charge and discharge process of the battery; they have stable chemical properties and will not destroy the electrochemical reaction system inside the battery; they have good thermal insulation properties, which can increase the safety performance of the battery; they are relatively low in price to meet the application needs of industrial grade; in addition, the preparation process of the above-mentioned inorganic porous materials is relatively mature, and their pore structure and interfacial activity can be adjusted as needed. Therefore, the above-mentioned inorganic porous materials are filled between the negative electrode active materials, which can effectively improve the specific capacity, rate performance, cycle life and safety performance of the battery.
[0042] In some embodiments of the present disclosure, the inorganic porous material comprises mesopores, and the volume of the mesopores accounts for 10% to 95% of the total pore volume of the inorganic porous material.
[0043] Internationally, pores are generally divided into three categories according to their size: micropores, mesopores (also known as mesopores), and macropores. Among them, pores with a diameter less than 2nm are micropores, pores with a diameter in the range of 2 to 50nm are mesopores, and pores with a diameter greater than 50nm are macropores. The mesopores of inorganic porous materials have a high electrolyte adsorption capacity and can be used as a buffer pool for the electrolyte in the negative electrode sheet, providing a continuous supply of carriers during the battery cycle and increasing the cycle life of the battery. In addition, during the charge and discharge process of the battery, the pore structure in the negative electrode sheet changes dynamically, which affects the diffusion of the electrolyte and the transport of carriers, resulting in uneven ion flux. By adding inorganic porous materials with a mesopore content of 10% to 95% to the negative electrode sheet, the flux during the negative electrode change process can be uniform, the distance for the carriers to diffuse to the negative electrode active material layer can be shortened, and the battery's rate performance can be improved.
[0044] The volume of the mesopores accounts for 10% to 95% of the total pore volume of the inorganic porous material, and the cycle life and rate performance of the negative electrode sheet and the corresponding battery are good.
[0045] The mesopore volume of the inorganic porous material is obtained based on the ratio of the pore volume of mesopores (pore diameter of 2 to 50 nm) to the total cumulative pore volume in the BET test results of the inorganic porous material.
[0046] In some specific embodiments of the present disclosure, the volume of the mesopores accounts for 40% to 95% of the total pore volume of the inorganic porous material. Thus, when the mesopore volume of the inorganic porous material of the present disclosure is within the above range, the cycle life and rate performance of the battery are better.
[0047] In some embodiments of the present disclosure, the inorganic porous material further comprises macropores, with the volume of the macropores constituting 5% to 40% of the total pore volume of the inorganic porous material. The macropores within the inorganic porous material provide pathways for electrolyte transport. Electrolyte ions stored in the mesopores diffuse through the macropores to the surface of the negative electrode active material, shortening the carrier diffusion path within the negative electrode sheet and further improving the battery's rate performance.
[0048] The macropore volume of the inorganic porous material is obtained based on the ratio of the pore volume of macropores (pore diameter > 50 nm) to the total cumulative pore volume in the BET test results of the inorganic porous material.
[0049] In some embodiments of the present disclosure, the average particle size of the inorganic porous material is 10 to 1000 nm.
[0050] The inorganic porous material disclosed herein has an average particle size in the range of 10 to 1000 nm, which can meet the use requirements of negative electrode active materials with different particle size ranges, achieve better filling effects, and thus facilitate the absorption and diffusion of the electrolyte. For example, the particle size of the inorganic porous material can be 10 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 600 nm, 800 nm, 900 nm, or 1000 nm.
[0051] In the present disclosure, the average particle size of the inorganic porous material is further preferably 200 to 1000 nm. If the average particle size of the inorganic porous material is too small, the surface energy is too large, affecting its dispersibility in the negative electrode sheet; if the average particle size of the inorganic porous material is too large, it will affect its contact effect with the negative electrode active material.
[0052] The average particle size of the inorganic porous material is determined by ultrasonically dispersing the inorganic porous material in anhydrous ethanol for 5 minutes and then measuring it using a laser particle size analyzer. D50 is the average particle size of the inorganic porous material, which is the particle size corresponding to less than 50% of the total volume on the particle size distribution curve.
[0053] In some embodiments of the present disclosure, the negative electrode active material layer further includes a conductive agent.
[0054] In the present disclosure, the negative electrode sheet contains both an inorganic porous material and a conductive agent, and the synergistic effect of the two can further improve the electrochemical performance of the battery.
[0055] In some embodiments of the present disclosure, the conductive agent accounts for 0.1% to 5% of the total content of the active material layer.
[0056] Understandably, the conductive agent in the negative electrode sheet, placed between the negative electrode active materials, can serve a certain purpose in terms of liquid storage and conductivity. However, its exposed conductive interface can also increase electrolyte side reactions. Therefore, maintaining the conductive agent content within the above range can ensure the conductivity and liquid storage capacity of the negative electrode sheet, while also suppressing side reactions in the electrode sheet, thereby ensuring battery rate performance and cycle life.
[0057] In some specific embodiments of the present disclosure, the conductive agent accounts for 0.1% to 2% of the total content of the active material layer.
[0058] When the content of the conductive agent is within the range of 0.1% to 2%, the synergistic effect between the inorganic porous material and the conductive agent is stronger, and the overall performance of the battery is better.
[0059] In the present disclosure, the conductive agent may be one or a combination of conductive carbon black, carbon nanotubes, graphene, and carbon fibers. The conductive carbon black material may be one or a combination of acetylene black, furnace black, channel black, thermal black, lamp black, and Ketjen black; the carbon nanotubes may be one or a combination of carbon nanotubes of varying diameters (1 to 100 nm) and lengths (0.05 to 100 μm); and the graphene may be one or a combination of graphenes of varying numbers of layers (1 to 1000 layers).
[0060] Accordingly, embodiments of the present disclosure further provide a battery comprising a positive electrode sheet, an electrolyte, a diaphragm, and the negative electrode sheet provided in the first aspect. Because the battery comprises the negative electrode sheet provided in the first aspect of the present disclosure, the battery has high specific capacity, rate capability, and cycle life, meeting a wider range of application requirements.
[0061] In the present disclosure, the battery may be a lithium-ion battery or a sodium-ion battery.
[0062] In the present disclosure, a positive electrode sheet includes a current collector and a positive electrode active material layer coated on at least one side of the current collector; the active material layer includes a positive electrode active material, a conductive agent, and a binder.
[0063] In the present disclosure, the positive electrode active material layer can be coated on one side of the current collector; it can also be coated on both sides of the current collector. When the positive electrode active material layer is coated on both sides of the current collector, the thickness, surface density, component content, etc. of the positive electrode active material layers respectively located on the two sides of the current collector can be independently designed according to application requirements and can be the same or different.
[0064] In the present disclosure, the positive electrode current collector may be any one of aluminum foil, carbon-coated aluminum foil, polymer-coated aluminum foil, carbon cloth, carbon nanotube film or carbon paper.
[0065] In the present disclosure, the separator may be one of polyethylene, polypropylene, and polyvinylidene fluoride, or a composite membrane of several thereof.
[0066] In the present disclosure, the positive electrode active material can be one or a combination of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and olivine-structured lithium-containing phosphate. The above positive electrode active materials are suitable for lithium-ion batteries.
[0067] In the present disclosure, the positive electrode active material may also be one or a combination of transition metal oxides, polyanionic compounds, organic polymers, Prussian blue / white materials, etc. The above positive electrode active materials are suitable for sodium ion batteries.
[0068] In the present disclosure, the electrolyte is an organic solvent in which carriers are dissolved. The present disclosure does not limit the electrolyte, and the electrolyte can be prepared according to actual conditions.
[0069] The embodiments of the present disclosure further provide an electric device. The electric device uses the battery provided in the embodiments of the present disclosure, and the electric device can have higher market competitiveness.
[0070] In some embodiments of the present disclosure, the above-mentioned electrical devices include but are not limited to mobile phones, laptops, tablets, smart watches and other wearable electronic devices, electronic cigarettes, as well as new energy vehicles, electric bicycles, energy storage base stations, etc.
[0071] The technical solution of the present disclosure is further illustrated below with multiple embodiments.
[0072] Example 1
[0073] The negative electrode active material (artificial graphite), conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), and inorganic porous material (porous silica) were mixed in a ratio of 96:0.9:1:2:0.1. The powder was then stirred with deionized water using a homogenizer to form a negative electrode slurry, which was then evenly coated onto copper foil. The silica had a dielectric constant of 1.6, an average particle size of 500 nm, a mesopore volume of 80%, and a macropore volume of 15%. Figure 1 shows the pore structure distribution curve of the porous silica provided in the present embodiment, which shows that the porous silica contains both mesopores and macropores.
[0074] The positive electrode active material lithium iron phosphate (LiFePO4), the conductive agent (CNT), and the second binder (PVDF) were mixed in a ratio of 97:1:2, and then the powder and NMP were stirred into a positive electrode slurry using a homogenizer and evenly coated on an aluminum foil.
[0075] Ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 1:1:1 to prepare an electrolyte containing 1M LiPF6.
[0076] A polypropylene separator was selected to prepare a 2.0Ah laminated battery.
[0077] Example 2
[0078] The only difference from Example 1 is that the mixing ratio of the negative electrode active material (artificial graphite), the conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and the inorganic porous material (porous silica) is 95:1.8:1:2:0.2.
[0079] Example 3
[0080] The only difference from Example 1 is that the mixing ratio of the negative electrode active material (artificial graphite), the conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and the inorganic porous material (porous silica) is 93.75:3:1:2:0.25.
[0081] Example 4
[0082] The only difference from Example 1 is that the mass ratio of the negative electrode active material (artificial graphite), conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and inorganic porous material (porous silica) is 96:0.5:1:2:0.5.
[0083] Example 5
[0084] The only difference from Example 1 is that the mass ratio of the negative electrode active material (artificial graphite), conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and inorganic porous material (porous silica) is: 96:0.25:2:1:0.75.
[0085] Example 6
[0086] The only difference from Example 1 is that the mass ratio of the negative electrode active material (artificial graphite), conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and inorganic porous material (porous silica) is 95:0.5:1:2:1.5.
[0087] Example 7
[0088] The only difference from Example 1 is that the mixing ratio of the negative electrode active material (artificial graphite), the conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and the inorganic porous material (porous silica) is 95:0.2:1:2:1.8.
[0089] Example 8
[0090] The only difference from Example 1 is that the mixing ratio of the negative electrode active material (artificial graphite), the conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and the inorganic porous material (porous silica) is 96:0:1:2:1.
[0091] Example 9
[0092] The only difference from Example 1 is that the mixing ratio of the negative electrode active material (artificial graphite), the conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and the inorganic porous material (porous silica) is 95:0:1:2:2.
[0093] Example 10
[0094] The only difference from Example 1 is that the mixing ratio of the negative electrode active material (artificial graphite), the conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and the inorganic porous material (porous silica) is 94:0:1:2:3.
[0095] Example 11
[0096] The only difference from Example 1 is that the mixing ratio of the negative electrode active material (artificial graphite), the conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and the inorganic porous material (porous silica) is 93:0:1:2:4.
[0097] Example 12
[0098] The only difference from Example 1 is that the mixing ratio of the negative electrode active material (artificial graphite), the conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and the inorganic porous material (porous silica) is 92:0:1:2:5.
[0099] Example 13
[0100] The only difference from Example 12 is that the inorganic porous material is porous alumina with a dielectric constant of 6.5, an average particle size of 400 nm, a mesopore volume of 76%, and a macropore volume of 20%.
[0101] Example 14
[0102] The only difference from Example 12 is that the inorganic porous material is porous boehmite, with a dielectric constant of 10; an average particle size of 800 nm; a mesopore volume of 60%; and a macropore volume of 18%.
[0103] Example 15
[0104] The only difference from Example 12 is that the inorganic porous material is porous titanium oxide, with a dielectric constant of 48, an average particle size of 1000 nm, a mesopore volume of 92%, and a macropore volume of 5%.
[0105] Example 16
[0106] The only difference from Example 15 is that the inorganic porous material is porous titanium oxide, whose dielectric constant is 48; the average particle size is 1000 nm; the mesopore volume is 42%; and the macropore volume is 21%.
[0107] Example 17
[0108] The only difference from Example 15 is that the inorganic porous material is porous titanium oxide, whose dielectric constant is 48; the average particle size is 1000 nm; the mesopore volume is 25%; and the macropore volume is 26%.
[0109] In order to highlight the beneficial effects of the embodiments of the present disclosure, the following comparative examples are provided.
[0110] Comparative Example 1
[0111] The only difference from Example 1 is that the mass ratio of the negative electrode active material (artificial graphite), conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and inorganic porous material (porous silica) is 91.99:5:1:2:0.01.
[0112] Comparative Example 2
[0113] The only difference from Example 1 is that the mass ratio of the negative electrode active material (artificial graphite), the conductive agent (conductive carbon black), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and the inorganic porous material (porous silica) is 90:0:1:2:7.
[0114] The parameters of the inorganic porous material content, conductive agent content, porosity and liquid absorption rate in the negative electrode sheet of the present invention are shown in Table 1; the battery performance test results are shown in Table 2.
[0115] Table 1
[0116] Electrochemical performance test
[0117] The batteries prepared above (including the comparative example batteries) were tested at room temperature using a Blue Power CT3002A battery testing system. The test results are summarized in Table 2.
[0118] Battery discharge capacity test: Perform a 0.1C / 0.1C cycle test on the battery at 25°C with a voltage range of 2.0V-3.8V (charge at 0.1C to a voltage of 3.8V, stand for 30 minutes, and then discharge at a discharge rate of 0.1C to a voltage of 2.0V, which is one cycle). Repeat the test 3 times and record the battery's third discharge capacity as the battery's discharge capacity.
[0119] First charge and discharge test:
[0120] The battery was subjected to a 0.1C / 0.1C cycle test at 25°C with a voltage range of 2.0V-3.8V (charge at 0.1C to a voltage of 3.8V, stand for 10 min, and then discharge at a discharge rate of 0.1C to a voltage of 2.0V, i.e., 1 cycle). The first charge specific capacity and the first discharge specific capacity of the battery were recorded, and the first charge and discharge efficiency of the battery was calculated based on this; battery first discharge efficiency (%) = (first charge specific capacity / first discharge specific capacity) * 100%.
[0121] Discharge ratio test:
[0122] The battery was charged at 0.1C to a voltage of 3.8V at 25°C, left for 30 minutes, and then discharged at a discharge rate of 3C to a voltage of 2.0V. This cycle was repeated three times. The discharge efficiency of the battery was calculated using the third charge and discharge data to evaluate the battery's rate performance; battery discharge rate (%) = (third discharge specific capacity (3C) / third charge specific capacity (0.1C)) * 100%.
[0123] Charge ratio test:
[0124] The battery was charged at 3C to a voltage of 3.8V at 25°C, left for 30 min, and then discharged at a discharge rate of 0.1C to a voltage of 2.0V. This cycle was repeated three times. The charge and discharge data of the third cycle were used to calculate the battery charging efficiency; battery charge rate (%) = (third discharge specific capacity (0.1C) / third charge specific capacity (3C)) * 100%.
[0125] Cycle life test: At 25°C, charge the battery at 1C to a voltage of 3.8V, let it rest for 10 minutes, then discharge at a discharge rate of 1C to a voltage of 2.0V. Repeat this cycle 1000 times, and record the capacity retention rate. Capacity retention rate after 1000 cycles (%) = discharge specific capacity after 1000 cycles / discharge specific capacity after the third cycle * 100%.
[0126] Table 2
[0127] As can be seen from the data in Table 1-2, compared with Comparative Example 1 and Comparative Example 2, the negative electrode sheet provided by the embodiment of the present disclosure contains an appropriate mass percentage of inorganic porous material, and the inorganic porous material partially replaces or completely replaces the conductive agent and is filled in the middle of the negative electrode active material. The porosity and liquid absorption rate of the negative electrode sheet are regulated, which can significantly improve the rate performance (discharge ratio and charge ratio) of the battery. In Comparative Example 1, a very small amount of inorganic porous material is added to the negative electrode sheet, the electrode sheet porosity and liquid absorption amount are low, and the electrolyte diffusion circuitous path is long, resulting in high lithium ion transfer impedance and poor battery rate performance. It can be seen that by adding inorganic porous material to the negative electrode sheet, changing the pore structure in the negative electrode sheet, increasing the porosity and liquid absorption rate of the negative electrode sheet, it is of great benefit to promoting the adsorption and migration of the electrolyte.
[0128] The above is an exemplary embodiment of the present disclosure. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made thereto without departing from the principles of the present disclosure. These improvements and modifications are also considered to be within the scope of protection of the present disclosure.
Claims
1. A negative electrode sheet, wherein: The negative electrode sheet comprises a current collector and a negative electrode active material layer coated on at least one side of the current collector; the negative electrode active material layer comprises a negative electrode active material, an inorganic porous material and a first binder; the inorganic porous material accounts for 0.1% to 5% of the total mass of the negative electrode active material layer.
2. The negative electrode sheet according to claim 1, wherein: The inorganic porous material accounts for 0.2% to 3% of the total mass of the negative electrode active material layer.
3. The negative electrode sheet according to claim 1 or 2, wherein: The porosity of the negative electrode sheet is 20% to 60%.
4. The negative electrode sheet according to any one of claims 1 to 3, wherein: The liquid absorption rate of the negative electrode sheet is 2 to 8 mg / min.
5. The negative electrode sheet according to any one of claims 1 to 4, wherein: The dielectric constant of the inorganic porous material is ε, 0<ε≤50; or, 0<ε≤10.
6. The negative electrode sheet according to any one of claims 1 to 5, wherein: The inorganic porous material contains mesopores, and the volume of the mesopores accounts for 10% to 95% of the total pore volume of the inorganic porous material.
7. The negative electrode sheet according to any one of claims 1 to 6, wherein: The average particle size of the inorganic porous material is 10 to 1000 nm.
8. The negative electrode sheet according to any one of claims 1 to 7, wherein: The inorganic porous material includes at least one of porous silica, porous titanium oxide, porous aluminum oxide or porous boehmite.
9. The negative electrode sheet according to any one of claims 1 to 8, wherein: The negative electrode active material is a carbon-based material.
10. The negative electrode sheet according to any one of claims 1 to 9, wherein: The negative electrode active material layer further includes a conductive agent.
11. The negative electrode sheet according to claim 10, wherein: The conductive agent accounts for 0.1% to 5% of the total mass of the negative electrode active material layer; 12. The negative electrode sheet according to claim 11, wherein: The conductive agent accounts for 0.1% to 2% of the total mass of the negative electrode active material layer.
13. A battery, wherein: The invention comprises a positive electrode sheet, an electrolyte, a diaphragm and a negative electrode sheet as claimed in any one of claims 1 to 12.
14. An electrical device, wherein: The electric device comprises the battery as claimed in claim 13.
Citation Information
Patent Citations
Negative plate, battery and electric equipment
CN118738363A
Preparation method of high-capacity sodium ion battery
CN107039639A
Sodium-ion battery negative electrode slurry and method for preparing pole piece from sodium-ion battery negative electrode slurry
CN115188965A
Negative active material and negative plate and lithium ion battery using same
CN115732694A
Composite negative plate and preparation method thereof, and lithium ion battery and preparation method thereof
CN115863537A
Cited By
Secondary battery electrode, secondary battery and preparation method