Binder for battery, composition for preparing electrode sheet, and use thereof
By using a low-temperature thermal binder containing specific groups, the problems of binder side reactions and high-temperature rolling in the existing dry electrode process are solved, enabling efficient preparation of electrode pole pieces and improving battery performance.
Patent Information
- Application Number
- PCT/CN2024/085153
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-04-01
- Publication Date
- 2024-10-03
AI Technical Summary
In the existing dry electrode process, polytetrafluoroethylene (PTFE) binder can easily cause side reactions at high temperatures, affecting battery performance, and requires complex fiberization processing and high-temperature rolling, which increases equipment damage and production costs.
Use a low-temperature thermal binder containing alkylene, acrylate and isocyanate or urethane groups, mix it with the electrode material and calender it to form a film, directly bonding the current collector, eliminating the need for fiberization processing and high-temperature rollers Pressing process.
It achieves efficient preparation of electrode pole pieces under solvent-free conditions, improves battery performance and production efficiency, reduces costs and equipment damage, and is suitable for simplified dry processes for all-solid-state batteries.
Smart Images

Figure PCTCN2024085153-FTAPPB-I100001 
Figure PCTCN2024085153-FTAPPB-I100002 
Figure PCTCN2024085153-FTAPPB-I100003
Abstract
Description
Binder for battery, composition for preparing electrode sheet and application thereof Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a binder for batteries, a composition for preparing electrode plates, and applications thereof. Background Art
[0002] The battery industry is constantly pursuing new dry-process composite electrode processing technologies that enable high-load, solvent-free processing. Once successfully introduced into mass production, this technology will offer the following advantages: 1. It can further enhance the energy density of existing battery systems; 2. It can streamline the homogenization and electrode baking processes, reducing the electrode workshop floor space and lowering equipment and plant construction investment costs; since it does not require N-methylpyrrolidone (NMP) solvent, it saves raw material costs while also improving environmental safety and reducing environmental management and operating costs; 4. Dry-process electrodes can produce thicker electrodes with good flexibility and high safety, and are expected to be used in the development of solid-state battery technology.
[0003] Summary of the Invention
[0004] Dry-process electrodes have obvious advantages in the process of preparing sulfide all-solid-state batteries: high compaction, no solvent influence, and minimized binder usage. However, at the same time, they will also hinder the ionic conductivity of the solid electrolyte. Currently, conventional dry-process electrodes use polytetrafluoroethylene (PTFE) binder. The document "Overcoming binder limitations of sheet-type solid-state cathodes using a solvent-free dry-film approach" proposes to mix and shear the binder that needs to be fiberized with the active material, inorganic solid electrolyte, and conductive agent at high speed, and then roll it multiple times on a roller press, and then heat-compound it with the glue-coated current collector to produce a dry-process electrode sheet. This process does not use a large amount of organic solvents, reducing the solvent removal process; however, coating the glue layer on the current collector surface will affect the interface contact between the active material and the current collector, hinder electron transmission, and increase the internal resistance of the battery cell.
[0005] Chinese patent application CN1147158A proposes adding thermoplastic polymer additives to self-supporting electrodes, rolling the electrode powder into a dry film by horizontal and vertical rolling, and then rolling it into a roll; the dry film is bonded to both sides of the porous current collector by hot rolling (80-200°C), thus obtaining a dry electrode electrode assembly and porous current collector composite. However, the temperature of hot rolling is relatively high, and at high temperatures, side reactions between the solid electrolyte and the active material are prone to occur at the interface, which is detrimental to performance. In addition, in order to maintain surface cleanliness, the current large-scale production of hot rolling uses tungsten carbide coating. Hot rolling above 80°C will cause significant thermal expansion, which is harmful to the surface coating. Long-term high-temperature use will cause great damage to the equipment, and the use of polytetrafluoroethylene as a binder still requires the binder to be fiberized, and the process is relatively complicated.
[0006] In response to the above technical problems, the present application provides an adhesive for batteries, a composition for preparing electrode plates, and its application. The adhesive is a low-temperature thermal composite material that can be mixed with electrode materials and rolled into a film in the absence of solvent, and can adhere to current collectors to prepare electrode plates.
[0007] The specific technical solutions of this application are as follows:
[0008] The present application provides a binder for a dry-process electrode, wherein the binder comprises a unit containing an alkylene group, a unit containing an alkenoate group, and a unit containing an isocyanate or carbamate group.
[0009] In a preferred embodiment of the present application, based on the mass percentage in the binder, the units containing alkylene groups are 5-60%, the units containing alkenoate groups are 10-65%, and the units containing isocyanate or carbamate groups are 5-40%.
[0010] In a preferred embodiment of the present application, the binder is formed by polymerizing a first monomer, a second monomer and a third monomer, wherein the first monomer contains an alkylene group, the second monomer contains an alkene ester group and / or an alkene ester group containing a hydroxyl group, and the third monomer contains an isocyanate or a carbamate group.
[0011] In a preferred embodiment of the present application, the weight average molecular weight of the binder is 1000-200000 Da.
[0012] In a preferred embodiment of the present application, the unit containing isocyanate or urethane groups accounts for 10-30% by mass in the binder.
[0013] The present application provides a composition for preparing an electrode plate, which comprises the binder, active material, conductive agent and electrolyte mentioned above.
[0014] In a preferred embodiment of the present application, the binder is 0.1-10 parts by weight, preferably 2-5 parts;
[0015] The active material is 50-100 parts; the electrolyte is 0-50 parts; and the conductive agent is 0-10 parts.
[0016] The present application provides an electrode plate, which is obtained by coating the above-mentioned composition on a current collector.
[0017] The present application provides a method for preparing an electrode sheet, wherein the method comprises:
[0018] mixing the active material, the electrolyte, the conductive agent and the binder to obtain a mixture;
[0019] The mixture is coated on the surface of the current collector.
[0020] In a preferred embodiment of the present application, in parts by weight, the active material is 50-100 parts, the electrolyte is 0-50 parts, the conductive agent is 0-10 parts, and the binder is 0.1-10 parts.
[0021] In a preferred embodiment of the present application, the coating thickness is 1-1000 μm.
[0022] In a preferred embodiment of the present application, the mixture is coated on the surface of the current collector by one or more methods selected from hot roller pressing, hot flat pressing and hot isostatic pressing, preferably at a temperature of 25-80°C.
[0023] The present application provides a battery, which includes the electrode plate described above or the electrode plate prepared by the method described above.
[0024] The present application provides the use of the above-mentioned binder in the preparation of lithium-ion batteries.
[0025] Effects of the Invention
[0026] Polytetrafluoroethylene (PTFE) molecular chains are non-polar. In dry processes (i.e., processes without solvents), they do not adhere to aluminum or copper foil, requiring additional conductive adhesive to be applied to the current collector surface before the current collector is laminated to the PTFE-containing electrode sheet. The binder described in this application, however, contains highly electronegative cyano and / or amino groups, which strongly interact with cationic materials in the electrolyte. Therefore, it can be mixed with the electrode material and rolled into a film in the absence of solvent. Furthermore, it can directly bond the current collector to form the electrode sheet without the need for additional conductive adhesive.
[0027] Advantages of using the adhesive in this application:
[0028] 1. The use of the binder of the present application can eliminate the need for the binder fiberization process and the secondary composite process with the current collector, saving costs and energy consumption, and enabling the preparation of thick electrodes;
[0029] 2. The binder of this application can be applied to the dry process to prepare negative electrode plates. Traditional dry electrode binders, such as PTFE, have poor reduction resistance. The reaction between lithium and fluorine causes the C-F bond to break and is easily carbonized. The dry negative electrode battery prepared with this binder will cause the plate to shatter due to the decomposition of the binder, resulting in poor battery performance. Therefore, the use of the binder of this application solves the above problems and allows all-solid-state batteries to be prepared entirely through a simplified dry process.
[0030] 3. The binder of the present application has relatively high adhesion to the current collector, and the prepared electrode has high peel strength and high gram capacity, which helps to further improve the battery performance. DETAILED DESCRIPTION
[0031] The present application is described in detail below in conjunction with the described embodiments. Although specific embodiments of the present application are shown, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present application and to fully convey the scope of the present application to those skilled in the art.
[0032] It should be noted that certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that technicians may use different nouns to refer to the same component. This specification and claims do not use the difference in nouns as a way to distinguish components, but use the difference in the functions of the components as the criterion for distinction. As mentioned throughout the specification and claims, "including" or "comprising" are open-ended terms and should be interpreted as "including but not limited to". The subsequent description of the specification is a preferred embodiment of the present application, but the description is based on the general principles of the specification and is not intended to limit the scope of the present application. The scope of protection of this application shall be as defined by the attached claims.
[0033] The present application provides a binder for a battery, wherein the binder comprises units containing an alkylene group, units containing an alkenoate group, and units containing an isocyanate or carbamate group. In some embodiments, based on the mass percentage of the binder, the units containing an alkylene group are 5-60%, the units containing an alkenoate group are 10-65%, and the units containing an isocyanate or carbamate group are 5-40%.
[0034] For example, the unit containing an alkylene group may be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc., based on the mass percentage in the binder, and more preferably 20-50%;
[0035] The units containing alkenoate groups may be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, etc.;
[0036] The units containing isocyanate or urethane groups may be 5%, 20%, 25%, 30%, 35%, 40%, etc., more preferably 10-30%.
[0037] The present application controls the content of units containing acrylate groups in the adhesive within the above range, which can avoid the adhesive from exhibiting strong plasticity and strong oil resistance, and ensure a strong bonding effect; controlling the units containing isocyanate or carbamate groups within the above range can control the cross-linking degree of the adhesive, thereby ensuring the mechanical properties of the electrode.
[0038] In some embodiments, the unit containing isocyanate or urethane groups is further preferably 10-30% by mass percentage in the binder, which can reduce plasticity without affecting the bonding effect.
[0039] In some embodiments, the binder is formed by polymerizing a first monomer, a second monomer, and a third monomer, wherein the first monomer contains an alkylene group, the second monomer contains an alkenoate group, and the third monomer contains an isocyanate group or a urethane group.
[0040] In some embodiments, an initiator may be added before polymerization. In the present application, there is no limitation on the amount of the initiator, which may be conventionally selected as needed. For example, the amount of the initiator added is 0.01-1% based on the weight of the second monomer.
[0041] In the present application, there is no limitation on the initiator, which can be conventionally selected as needed. For example, the initiator can be di-tert-butyl peroxide, di-tert-butyl peroxide, tert-butyl 2-ethylhexyl peroxide, tert-butyl-2-ethylhexyl peroxide, or tert-butyl pivalate.
[0042] In some embodiments, the weight average molecular weight of the binder is 1,000-200,000 Da.
[0043] For example, the weight average molecular weight of the binder can be 1000 Da, 2000 Da, 3000 Da, 4000 Da, 10000 Da, 50000 Da, 100000 Da, 120000 Da, 150000 Da, 180000 Da, 200000 Da, etc.
[0044] The molecular weight of the adhesive described in this application is related to the amount of monomer containing diisocyanate added. The more the amount added, the higher the degree of crosslinking, the higher the molecular weight, and the greater the viscosity of the adhesive.
[0045] In the present application, there is no limitation on the first monomer, the second monomer and the third monomer, as long as they contain corresponding groups. For example, the first monomer only needs to contain an alkylene group, the second monomer only needs to contain an alkene ester group, and the third monomer only needs to contain an isocyanate group or a carbamate group.
[0046] For example, the first monomer may be selected from at least one of ethylene, propylene, butadiene, and pentene.
[0047] The second monomer can be selected from at least one of vinyl acetate, vinyl propylene, allyl acetate, allyl acrylate, vinyl butyrate, n-butenyl acetate, butenyl propionate, allyl butyrate, hydroxymethyl butenoate, hydroxypropyl acrylate, hydroxybutyl acrylate, 2-hydroxy-4-pentenoic acid, methyl 2-hydroxy-3-butenoate and 5-hydroxy-2-methyl-3-hexenoic acid.
[0048] The third monomer may be selected from one or more of methyl isocyanate, 1,4-cyclohexyl diisocyanate, 1,6-hexamethylene diisocyanate, toluene diisocyanate, xylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, lysine diisocyanate, trichloroacetyl isocyanate, chlorosulfonyl isocyanate, n-octyl isocyanate and hexamethylene diisocyanate.
[0049] In some embodiments, the binder comprises units containing an alkylene group, units containing an alkenoate group, and units containing isocyanate or carbamate groups. In some embodiments, based on the mass percentage shared in the binder, the units containing an alkylene group are 5-60%, the units containing an alkenoate group are 10-65%, and the units containing isocyanate or carbamate groups are 5-40%. In some embodiments, the binder is formed by polymerizing a first monomer, a second monomer, and a third monomer, wherein the first monomer contains an alkylene group, the second monomer contains an alkenoate group and / or an alkenoate group containing a hydroxyl group, and the third monomer contains an isocyanate or carbamate group. In some embodiments, the weight-average molecular weight of the binder is 1000-200,000 Da. In some embodiments, based on the mass percentage shared in the binder, the units containing isocyanate or carbamate groups are 10-30%.
[0050] The adhesive described in this application contains cyano or amino monomers with strong electronegativity, which have strong mutual forces with cationic materials in electrolyte materials such as lithium ions, and metal cations in sulfides and halides. It also has strong forces with metal ions on aluminum foil and copper foil, and can provide higher peel strength.
[0051] The present application provides a composition for preparing an electrode plate, which comprises the aforementioned binder, active material, conductive agent and electrolyte.
[0052] In the present application, there is no limitation on the active material, conductive agent and electrolyte, and active materials, conductive agents and electrolytes commonly used in the art can be used.
[0053] For example, in the present application, the active material can be a positive electrode active material or a negative electrode active material, for example, the positive electrode active material is selected from an oxide positive electrode active material and / or a sulfide positive electrode active material. For example, the oxide positive electrode active material is selected from lithium cobaltate LiCoO2, lithium manganate LiMnO2, lithium nickelate LiNiO2, lithium vanadate LiVO2, ternary nickel cobalt manganate LiNi 1 / 3 CO 1 / 3 Mn 1 / 3 O2, lithium manganese oxide LiMn2O4, lithium nickel manganese oxide Li (Ni 0.5 Mn 1.5 )O4, lithium iron silicate Li2FeSiO4 and lithium iron phosphate LiFePO4; the sulfide positive electrode active material is selected from one or more of ferrous sulfide FeS, iron sulfide Fe2S3, cobalt sulfide CoS, lithium sulfide Li2S and sulfur;
[0054] The negative electrode active material can be selected from but not limited to metal negative electrodes such as Li, Li alloy materials (Li-In, Li-Ag, Li-Sn negative electrodes, etc.), graphite, amorphous carbon negative electrodes, silicon-based negative electrodes such as Si, SiS2, SiO2, etc.
[0055] The conductive agent may be selected from one or more of Super P, low crystalline carbon, soft carbon, hard carbon, high crystalline carbon, natural graphite, pyrolytic carbon, mesophase pitch-based carbon fibers, and mesophase carbon microbeads.
[0056] The electrolyte may be an inorganic solid electrolyte, including one or more of a binary sulfide electrolyte, a sulfide electrolyte, an argyrodite-type sulfide electrolyte, an oxide electrolyte, and a halide electrolyte;
[0057] The binary sulfide electrolyte is selected from 80Li2S-20P2S5, Li7P3S 11 , Li6PS5Cl, 70Li2S-30P2S5;
[0058] The argyrodite-type sulfide electrolyte is selected from Li 5.5 PS 4.5 Cl 1.5 、Li7P2S8I、Li6PS5Cl、Li 6.6 P 0.4 Ge 0.6 S5I、Li 10 GeP2S 12 Li 11 Si2PS 12 Li9 .54 Si 1.74 P1 .44 S 11.7 Cl 0.3 、Li7P2S8Br 0.5 I 0.5 Li 3.25 Ge 0.25 P 0.75 One or more of S4;
[0059] The oxide electrolyte is selected from Li7La3M2O 12 (M=Zr,Sn,Hf),Li 0.3 La 0.57 TiO3、Li 1+x Al x M 1-x (PO4)3, M=Ti, Ge, Zr, Hf) and other oxide electrolytes or more.
[0060] The halide electrolyte is selected from LiInCl3, LiZrCl5, LiZrx Fe 1-x One or more halide electrolytes such as Cl5, LiScCl3, etc.
[0061] In some embodiments, the binder is present in an amount of 0.1-10 parts by weight, preferably 2-5 parts by weight; for example, the binder can be present in an amount of 0.1 parts, 0.5 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc. by weight;
[0062] The active material can be selected from positive electrode active material or negative electrode active material, specifically selected from oxide positive electrode, sulfur-containing positive electrode, graphite, silicon, silicon oxide, lithium titanate, etc., and the amount used is 50-100 parts; the active material can be 50 parts, 60 parts, 70 parts, 80 parts, 90 parts, 100 parts, etc.
[0063] The electrolyte dosage is 0-50 parts, and the electrolyte can be 0, 10, 20, 30, 40, 50 parts, etc.;
[0064] The conductive agent is 0-10 parts. The conductive agent can be 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, etc.
[0065] In the present application, the binder, active material, conductive agent and electrolyte can be mixed according to conventional methods in the art, for example, they can be mixed by grinding, ball milling, roller milling, stirring and the like.
[0066] In some embodiments, the composition for preparing an electrode plate comprises any one of the above-mentioned binders, active materials, conductive agents, and electrolytes. In some embodiments, the binder is present in an amount of 0.1-10 parts by weight, preferably 2-5 parts by weight.
[0067] The active material is 50-100 parts; the electrolyte is 0-50 parts; and the conductive agent is 0-10 parts.
[0068] The present application provides an electrode plate, which is obtained by directly coating the above-mentioned composition on a current collector.
[0069] The present application does not impose any restrictions on the coating method, and the coating can be carried out according to conventional methods in the art. For example, the composition can be evenly spread on the surface of the current collector to form a film, and then obtained by hot roller pressing, hot flat pressing, hot isostatic pressing, etc.
[0070] In the present application, there is no limitation on the thickness of the composition to be laid, and it can be laid according to the conventional thickness in the art. For example, the laying thickness can be 1-1000 μm, for example, the laying thickness can be 1 μm, 10 μm, 50 μm, 100 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1000 μm, etc.
[0071] In some embodiments, the temperature of hot roller pressing, hot flat pressing, hot isostatic pressing, etc. is 25-80°C, for example, the temperature can be 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, etc.
[0072] In the present application, the electrode plate mentioned above can be a positive electrode plate or a negative electrode plate.
[0073] The present application provides a method for preparing an electrode sheet, the method comprising:
[0074] An active material, an electrolyte, a conductive agent, and the binder described above are mixed to obtain a mixture; and the mixture is coated on the surface of a current collector. In some embodiments, the active material is 50-100 parts, the electrolyte is 0-50 parts, the conductive agent is 0-10 parts, and the binder is 0.1-10 parts by weight. In some embodiments, the coating thickness is 1-1000 μm. In some embodiments, the mixture is coated on the surface of the current collector by one or more methods selected from hot roller pressing, hot flat pressing, and hot isostatic pressing, preferably at a temperature of 25-80°C.
[0075] The present application provides a battery, which includes the electrode plate described above or the electrode plate prepared by the method described above.
[0076] The battery described in the present application has better reversible capacity performance due to the use of a binder containing a cyano group or an amino group with relatively strong electronegativity.
[0077] The present application provides the use of the above-mentioned binder in preparing a battery.
[0078] Example
[0079] This application provides general and / or specific descriptions of the materials and experimental methods used in the experiments. In the following examples, unless otherwise specified, % represents wt%, i.e., percentage by weight. All reagents or instruments used without manufacturer indication are commercially available conventional reagents.
[0080] Preparation Example 1 Preparation of binder
[0081] The first monomer, ethylene, is introduced into the second monomer (a mixed solution of 33.3 g of vinyl acetate and 3.7 g of hydroxyethyl acrylate) through a gas compressor, and polymerization is carried out with 0.38 g of benzoyl peroxide as an initiator and 212 g of ethanol as a dispersant at 80° C. for 2 hours. The mixture is cooled to room temperature, and 7.4 g of the third monomer (1,6-hexamethylene diisocyanate) is added in four batches. The reaction temperature is controlled to 75° C. and stirred for 2 hours and 1 hour. The residue is washed with deionized water and vacuum distilled to obtain a binder with a weight-average molecular weight of 15540 Da. The mass ratio of ethylene, vinyl acetate, hydroxyethyl acrylate and 1,6-hexamethylene diisocyanate is 4:(4.5:0.5):1.
[0082] Preparation Example 2 Preparation of binder
[0083] The first monomer, ethylene, is introduced into the second monomer (a mixture of 33.3 g of vinyl acetate and 11.1 g of hydroxyethyl acrylate) through a gas compressor, and polymerization is carried out using 0.21 g of benzoyl peroxide as an initiator and 202 g of ethanol as a dispersant. The polymerization is carried out at 80° C. for 2 hours, and the mixture is cooled to room temperature. 2.4 g of the third monomer (1,4-cyclohexane diisocyanate) is added, the reaction temperature is controlled to 30° C., and the mixture is stirred at room temperature for 30 minutes. The residue is washed with deionized water and vacuum distilled to obtain a binder with a weight-average molecular weight of 13820 Da, wherein the mass ratio of ethylene, vinyl acetate, hydroxyethyl acrylate, and 1,4-cyclohexane diisocyanate is 3:(4.5:1.5):1.
[0084] Preparation Example 3 Preparation of binder
[0085] The first monomer, ethylene, was introduced into a second monomer (a mixture of 33.3 g vinyl acetate and 3.7 g hydroxyethyl acrylate) via a gas compressor. Polymerization was carried out at 80°C for 2 hours using 0.12 g benzoyl peroxide as an initiator and 212 g ethanol as a dispersant. The mixture was cooled to room temperature, and 18.5 g of the third monomer (1,4-cyclohexane diisocyanate) was added. The reaction temperature was controlled at 30°C and stirred at room temperature for 30 minutes. The residue was washed with deionized water and vacuum distilled to obtain a binder with a weight-average molecular weight of 38,570 Da. The mass ratio of ethylene, vinyl acetate, hydroxypropyl acrylate, and 1,4-cyclohexane diisocyanate was 2.5:(4.5:0.5):2.5.
[0086] Preparation Example 4 Preparation of Binder
[0087] The first monomer, ethylene, was introduced into a second monomer (a mixture of 26.2g vinyl acetate and 5.24g hydroxyethyl acrylate) via a gas compressor. Polymerization was initiated with 0.55g benzoyl peroxide as an initiator and 198g ethanol as a dispersant. Polymerization was carried out at 80°C for 2 hours, followed by cooling to room temperature. Polymerization was then continued at 80°C for 2 hours, followed by cooling to room temperature. 5.24g of the third monomer, 1,4-cyclohexane diisocyanate, was added. The reaction temperature was controlled at 30°C and stirred at room temperature for 30 minutes. The residue was washed with deionized water and vacuum distilled to obtain a binder with a weight-average molecular weight of 9864 Da. The mass ratio of ethylene, vinyl acetate, hydroxyethyl acrylate, and 1,4-cyclohexane diisocyanate was 6:(2.5:0.5):1.
[0088] Preparation Example 5 Preparation of Binder
[0089] The first monomer, ethylene, is introduced into the second monomer (a mixture of 33.3 g of vinyl acetate and 6.66 g of hydroxyethyl acrylate) through a gas compressor, and polymerization is carried out with 0.21 g of benzoyl peroxide as an initiator, and 215 g of ethanol as a dispersant at 80° C. for 2 hours, cooled to room temperature, and polymerized with ethanol as a dispersant at 80° C. for 2 hours, cooled to room temperature, and 6.66 g of the third monomer (1,4-cyclohexane diisocyanate) is added. The reaction temperature is controlled to 30° C. and stirred at room temperature for 30 minutes. The residue is washed with deionized water and vacuum distilled to obtain a binder with a weight-average molecular weight of 14232 Da, wherein the mass ratio of ethylene, vinyl acetate, hydroxypropyl acrylate, and 1,4-cyclohexane diisocyanate is 3:(5:1):1.
[0090] Preparation Example 6 Preparation of Binder
[0091] The first monomer, ethylene, is introduced into the second monomer (a mixture of 33.3 g of vinyl acetate and 9.99 g of hydroxyethyl acrylate) through a gas compressor, and polymerization is carried out with 0.05 g of benzoyl peroxide as an initiator. 208 g of ethanol is used as a dispersant, and the polymerization is carried out at 80° C. for 2 hours. The mixture is cooled to room temperature. 19.98 g of the third monomer (1,4-cyclohexane diisocyanate) is added with ethanol as a dispersant, and the mixture is cooled to room temperature. The reaction temperature is controlled to 30° C. and stirred at room temperature for 30 minutes. The residue is washed with deionized water and vacuum distilled to obtain a binder with a weight-average molecular weight of 56214 Da, wherein the mass ratio of ethylene, vinyl acetate, hydroxypropyl acrylate, and 1,4-cyclohexane diisocyanate is 0.5:(5:1.5):3.
[0092] Preparation Example 7 Preparation of Binder
[0093] The first monomer, ethylene, is introduced into the second monomer (a mixture of 33.3 g of vinyl acetate and 5.55 g of hydroxyethyl acrylate) through a gas compressor, and polymerization is carried out with 0.48 g of benzoyl peroxide as an initiator, and 228 g of ethanol as a dispersant. The polymerization is carried out at 80° C. for 2 hours, cooled to room temperature, and ethanol as a dispersant. The polymerization is carried out at 80° C. for 2 hours, cooled to room temperature, and 16.65 g of the third monomer (1,4-cyclohexane diisocyanate) is added. The reaction temperature is controlled to 30° C. and stirred at room temperature for 30 minutes. The residue is washed with deionized water and vacuum distilled to obtain a binder with a weight-average molecular weight of 2854 Da, wherein the mass ratio of ethylene, vinyl acetate, hydroxypropyl acrylate, and 1,4-cyclohexane diisocyanate is 5:(3:0.5):1.5.
[0094] Preparation Example 8 Preparation of Binder
[0095] The first monomer, ethylene, is introduced into the second monomer (a mixture of 33.3 g of vinyl acetate and 11.1 g of hydroxyethyl acrylate) through a gas compressor, and polymerization is carried out with 0.24 g of benzoyl peroxide as an initiator, and 228 g of ethanol as a dispersant at 80° C. for 2 hours, cooled to room temperature, and polymerized with ethanol as a dispersant at 80° C. for 2 hours, cooled to room temperature, and 66.6 g of the third monomer (1,4-cyclohexane diisocyanate) is added. The reaction temperature is controlled to 30° C. and stirred at room temperature for 30 minutes. The residue is washed with deionized water and vacuum distilled to obtain a binder with a weight-average molecular weight of 16566 Da, wherein the mass ratio of ethylene, vinyl acetate, hydroxypropyl acrylate, and 1,4-cyclohexane diisocyanate is 2:(3:1):6.
[0096] Comparative Preparation Example 1 Preparation of Binder
[0097] The difference between Comparative Preparation Example 1 and Example 1 is that only the first monomer ethylene and the second monomer (a mixture of vinyl acetate and hydroxypropyl acrylate) are used to prepare the adhesive, whose weight-average molecular weight is 2340Da, wherein the mass ratio of ethylene to vinyl acetate and hydroxypropyl acrylate is 4:(5:1).
[0098] Preparation of comparative preparation example 2 binder
[0099] The difference between Comparative Preparation Example 2 and Example 2 is that only the second monomer (a mixture of vinyl acetate and hydroxyethyl acrylate) and the third monomer (1,4-cyclohexane diisocyanate) are used to prepare the adhesive, whose weight-average molecular weight is 4812 Da, wherein the mass ratio of vinyl acetate, hydroxyethyl acrylate and 1,4-cyclohexane diisocyanate is (4.5:0.5):1.
[0100] Comparative Preparation Example 3 Preparation of Binder
[0101] The difference between Preparation Example 3 and Example 1 is that the mass ratios of the first monomer ethylene, the second monomer (a mixture of vinyl acetate and hydroxyethyl acrylate) and the third monomer (1,6-hexamethylene diisocyanate) are different. The mass ratio of ethylene, vinyl acetate and hydroxyethyl acrylate to 1,6-hexamethylene diisocyanate is 8:(1:0.8):0.2, and the weight-average molecular weight is 1230 Da.
[0102] Comparative Preparation Example 4
[0103] The difference between Comparative Preparation Example 4 and Example 1 is that only the first monomer ethylene and the second monomer (1,6-hexamethylene diisocyanate) are used, and the mass ratio of the two is 4:1, and the two cannot undergo polymerization reaction.
[0104] Table 1 Selection and dosage relationship of each component in the preparation example
[0105] Prepare positive or negative electrode sheets using dry method:
[0106] Example 1 Preparation of positive electrode sheet
[0107] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 16 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 2 wt% of the binder of Preparation Example 1 were weighed and mixed on a stirring device to obtain a powder. The stirring device speed was 2000 r / min, the mixing time was 15 min, and the stirring temperature was 20°C.
[0108] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0109] Example 2 Preparation of positive electrode sheet
[0110] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 16 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 2 wt% of the binder of Preparation Example 2 were weighed and mixed on a stirring device at a speed of 2000 r / min, a mixing time of 15 min, and a stirring temperature of 20°C to obtain a powder.
[0111] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0112] Example 3 Preparation of negative electrode sheet
[0113] (1) Mixing process: Weigh 60 wt% Si, 35 wt% sulfide electrolyte Li6PS5Cl, 3 wt% acetylene black, and 2 wt% binder of Preparation Example 1. Mix them on a stirring device at a speed of 2000 rpm, a mixing time of 15 min, and a stirring temperature of 20°C to obtain a powder.
[0114] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers, and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C.
[0115] Example 4 Preparation of positive electrode sheet
[0116] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 16 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 2 wt% of the binder of Preparation Example 3 were weighed and mixed on a stirring device at a speed of 2000 r / min, a mixing time of 15 min, and a stirring temperature of 20°C to obtain a powder.
[0117] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0118] Example 5 Preparation of positive electrode sheet
[0119] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 16 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 2 wt% of the binder of Preparation Example 4 were weighed and mixed on a stirring device at a speed of 2000 r / min, a mixing time of 15 min, and a stirring temperature of 20°C to obtain a powder.
[0120] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0121] Example 6 Preparation of positive electrode sheet
[0122] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 13 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 5 wt% of the binder of Preparation Example 5 were weighed and mixed on a stirring device at a speed of 2000 r / min, a mixing time of 15 min, and a stirring temperature of 20°C to obtain a powder.
[0123] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0124] Example 7 Preparation of positive electrode sheet
[0125] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 17 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 1 wt% of the binder of Preparation Example 5 were weighed and mixed on a stirring device at a speed of 2000 r / min, a mixing time of 15 min, and a stirring temperature of 20°C to obtain a powder.
[0126] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0127] Example 8 Preparation of positive electrode sheet
[0128] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 16 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 2 wt% of the binder of Preparation Example 5 were weighed and mixed on a stirring device at a speed of 2000 r / min, a mixing time of 15 min, and a stirring temperature of 20°C to obtain a powder.
[0129] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0130] Example 9 Preparation of positive electrode sheet
[0131] (1) Mixing process: 96 wt% of nickel-cobalt-manganese ternary material (NCM811), 2 wt% of acetylene black and 2 wt% of the binder of Preparation Example 1 were weighed and mixed on a stirring device to obtain a powder. The stirring device speed was 2000 r / min, the mixing time was 15 min, and the stirring temperature was 20°C.
[0132] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0133] Example 10 Preparation of positive electrode sheet
[0134] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 16 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 2 wt% of the binder of Preparation Example 6 were weighed and mixed on a stirring device at a speed of 2000 r / min, a mixing time of 15 min, and a stirring temperature of 20°C to obtain a powder.
[0135] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0136] Example 11 Preparation of positive electrode sheet
[0137] (1) Mixing process: 80 wt% nickel-cobalt-manganese ternary material (NCM811), 16 wt% sulfide electrolyte Li6PS5Cl, 2 wt% acetylene black and 2 wt% binder of Preparation Example 7 are mixed on a stirring device to obtain a powder. The stirring device speed is 2000 r / min, the mixing time is 15 min, and the stirring temperature is 20°C.
[0138] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0139] Example 12 Preparation of positive electrode sheet
[0140] (1) Mixing process: 80 wt% nickel-cobalt-manganese ternary material (NCM811), 16 wt% sulfide electrolyte Li6PS5Cl, 2 wt% acetylene black and 2 wt% binder of Preparation Example 8 are mixed on a stirring device to obtain a powder. The stirring device speed is 2000 r / min, the mixing time is 15 min, and the stirring temperature is 20°C.
[0141] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, and rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C to obtain a positive electrode sheet.
[0142] Comparative Example 1 Preparation of positive electrode sheet
[0143] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 16 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 2 wt% of the binder of comparative preparation example 1 were weighed and mixed on a stirring device to obtain a powder. The stirring speed of the stirring device was 2000 r / min, the mixing time was 15 min, and the stirring temperature was 20°C.
[0144] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers, and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C.
[0145] Comparative Example 2 Preparation of positive electrode sheet
[0146] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 16 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 2 wt% of the binder of comparative preparation example 2 were weighed and mixed on a stirring device to obtain a powder. The stirring device speed was 2000 r / min, the mixing time was 15 min, and the stirring temperature was 20°C.
[0147] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers, and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C.
[0148] Comparative Example 3 Preparation of positive electrode sheet
[0149] (1) Mixing process: 80 wt% of nickel-cobalt-manganese ternary material (NCM811), 16 wt% of sulfide electrolyte Li6PS5Cl, 2 wt% of acetylene black and 2 wt% of the binder of comparative preparation example 3 were weighed and mixed on a stirring device to obtain a powder. The stirring device speed was 2000 r / min, the mixing time was 15 min, and the stirring temperature was 20°C.
[0150] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers, and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C.
[0151] Comparative Example 4 Preparation of positive electrode sheet
[0152] Since the raw materials in Comparative Preparation Example 4 did not react with each other and did not form a binder, the electrode could not be prepared.
[0153] In the preparation of the positive electrode sheet of Comparative Example 5, conventional binders and conventional dry electrode preparation methods were used.
[0154] (1) Mixing process: 80 wt% nickel-cobalt-manganese ternary material (NCM811), 16 wt% sulfide electrolyte Li6PS5Cl, 2 wt% acetylene black, and 2 wt% polytetrafluoroethylene were weighed and mixed on a stirring device to obtain a powder. The stirring speed of the stirring device was 2000 r / min, the mixing time was 15 min, and the stirring temperature was 20°C.
[0155] (2) Fiber process: The powder obtained in step (1) is subjected to secondary mixed fiber production using a jet milling device, with an air inlet pressure of 0.6 MPa, a crushing pressure of 0.8 MPa, compressed air, and a moisture content of ≤10 ppm;
[0156] (3) Laminating process: The powder in step (2) is rolled into a 150 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 120°C.
[0157] (4) Glue coating process: Apply a conductive glue with a solid content of 45% on the surface of the current collector to a thickness of 3 μm on both sides of the current collector, and dry at 80°C.
[0158] (5) Lamination process: Lamination of the dry-process positive electrode on both sides of the current collector obtained in step (4) is performed using a hot rolling process at a temperature of 120°C.
[0159] In the preparation of the negative electrode sheet of Comparative Example 6, conventional binders and conventional dry electrode preparation methods were used.
[0160] (1) Mixing process: 60 wt% Si, 35 wt% sulfide electrolyte Li6PS5Cl, 2 wt% polytetrafluoroethylene, and 3 wt% acetylene black were weighed and mixed on a stirring device to obtain a powder. The stirring device speed was 2000 r / min, the mixing time was 15 min, and the stirring temperature was 20°C.
[0161] (2) Fiber process: The powder obtained in step (1) is subjected to secondary mixed fiber production using a jet milling device, with an air inlet pressure of 0.6 MPa, a crushing pressure of 0.8 MPa, compressed air, and a moisture content of ≤10 ppm;
[0162] (3) Laminating process: The powder in step (2) is rolled into a 150 μm dry-process positive electrode through a horizontal roller and two vertical rollers and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 120°C.
[0163] (4) Glue coating process: Apply a conductive glue with a solid content of 45% on the surface of the current collector to a thickness of 3 μm on both sides of the current collector, and dry at 80°C.
[0164] (5) Lamination process: Lamination of the dry-process negative electrode on both sides of the current collector obtained in step (4) is performed using a hot rolling process at a temperature of 120°C.
[0165] Comparative Example 7: Preparation of positive electrode sheets using conventional binders and the dry electrode preparation method of this application.
[0166] (1) Mixing process: 80 wt% nickel-cobalt-manganese ternary material (NCM811), 16 wt% sulfide electrolyte Li6PS5Cl, 2 wt% acetylene black and 2 wt% polytetrafluoroethylene were weighed and mixed on a stirring device to obtain a powder. The stirring speed of the stirring device was 2000 r / min, the mixing time was 15 min, and the stirring temperature was 20°C.
[0167] (2) Lamination process: The powder in step (1) is evenly dispersed on the surface of the current collector, rolled into a 100 μm dry-process positive electrode through a horizontal roller and two vertical rollers, and rolled into a roll to obtain a dry-process positive electrode roll. The roller temperature is controlled at 60°C.
[0168] Table 2 Components and dosages in the examples
[0169] Battery Preparation Example
[0170] (1) Preparation of solid-state lithium-ion batteries:
[0171] The positive electrode sheets prepared in Examples 1-8, Examples 10-12, and Comparative Examples 1-3 and 5-7 were pressed in a Teflon mold with a diameter of 10 mm in the order of positive electrode | solid electrolyte layer | lithium metal, and the negative electrode sheets were pressed in the order of silicon electrode | solid electrolyte layer | metallic lithium. The solid electrolyte was 120 mg of Li6PS5Cl powder, the pressing pressure was 380 MPa, and the holding time was 5 min to obtain a solid-state lithium-ion battery.
[0172] (2) Preparation of liquid lithium-ion batteries:
[0173] The positive electrode sheet prepared in Example 9 was assembled in the order of positive electrode|electrolyte|lithium metal to obtain a liquid lithium-ion battery. The electrode liquid used was 10 wt% fluoroethylene carbonate dissolved with 1 M / L LiPF.
[0174] Test Example 1 Dry Electrode Peel Strength Test
[0175] The experiment was conducted at room temperature of 23°C ± 2°C and a dew point of -50°C. The pole pieces prepared in Examples 1-12 and Comparative Examples 1-3 and 5-7 were placed under these conditions for more than 2 hours. The adhesive tape was peeled off, the outer 3-5 layers were cut off, and the adhesive tape was evenly peeled off so that the adhesive tape was bonded to one end of the pole piece at an angle greater than 30°. A polyester film approximately 200 mm long and 40 mm wide was placed under the other end of the pole piece. The pole piece with the adhesive tape was then rolled back and forth three times at a speed of approximately 120 mm / s using the wheels of a rolling device under its own weight. The free end of the pole piece with the adhesive tape was folded 180° and the adhesive surface was peeled off by approximately 10 mm. The pole piece was clamped on the lower clamp and the free end of the pole piece with the adhesive tape was clamped on the upper clamp. The peeling surface was aligned with the force line of the testing machine. The testing machine continuously peeled at a descending speed of 300 ± 10 mm / min. The effective peeling adhesive surface length is about 100 mm, and an automatic technical device gives the peeling strength, the results of which are shown in Table 3.
[0176] Table 3
[0177] As can be seen from Table 3, the adhesives used in Examples 1 and 2 exhibit good bonding performance within the preferred range of the present application. The amount of the first monomer in the adhesive used in Example 1 is larger than that in the adhesive used in Example 2, so the adhesive used in Example 1 has better thermal processing performance. However, the above-mentioned difference in amount has little effect on the peelability, so the peel strengths of the two are similar.
[0178] In Example 3, the binder of Preparation Example 1 was applied to a silicon anode battery system. Compared to Example 1, which used NCM811 as the positive electrode material, the silicon particles were smaller, and the bonding effect was poorer at the same binder content. Similarly, in bonding a silicon anode (Comparative Example 6), the binder of this application exhibited better peel strength than conventional PTFE.
[0179] Example 4 uses the adhesive of Preparation Example 3, in which the content of the third monomer is relatively high, so that the adhesive has a higher degree of cross-linking, and therefore the adhesive of Preparation Example 3 has a high bonding effect.
[0180] Since Example 5 uses the adhesive of Preparation Example 4, the first monomer exceeds the preferred range, so the second monomer content is relatively small, and the cross-linking polymerization degree with the third monomer isocyanate is low, showing poor adhesive properties.
[0181] It can be seen from Examples 6-8 that different adhesive contents have different effects on the peel strength, and the more adhesive is used, the higher the peel strength.
[0182] In Example 9, the binder of Example 1 is applied to a liquid lithium-ion battery system, that is, without an inorganic solid electrolyte. Since the positive electrode active material particles are larger than the electrolyte particles, it exhibits stronger peel strength at the same binder content.
[0183] The electrode prepared by the adhesive used in Example 10 (preparation example 6) has a higher thermal melting point due to its lower ethylene content, and the electrode peel strength processed at 60°C is relatively low; the electrode prepared by the adhesive used in Example 11 has a higher first monomer content and lower second and third monomer contents, a low degree of polymerization, and relatively weak adhesion, so the electrode peel strength is lower than that of Example 1; Example 12 has a higher third monomer, but the third monomer is too high, while the first and second monomers are less, which is similar to the adhesive in Example 10, and the adhesive strength of the adhesive is deteriorated.
[0184] Since the binder of Comparative Example 1 contains only the first and second monomers, it exhibits strong thermoplasticity and its electrode peel strength is poor. Although the binder of Comparative Example 2 has relatively strong adhesion, it needs to be heated to above 200°C to adhere to the current collector. Compared with the binder processing temperature of the present application, it is higher and can easily lead to thermal degradation of the battery material. Comparative Example 3 is not within the scope of protection of the present application. The performance of the binder is poor due to the low content of the second monomer and the third monomer. Comparative Examples 5 and 6 are respectively prepared using traditional dry processes and use conventional PTFE adhesives. Compared with the present application, their peel strength is inferior to that of the present invention. Comparative Example 7 uses the dry process of the present application and a conventional PTFE adhesive to prepare the positive electrode. Because PTFE needs to be pre-fiberized and the adhesion between PTFE and the current collector is poor, the effect of simplifying the process flow cannot be achieved without using the binder of the present application.
[0185] Therefore, the peel strength of the positive electrode sheet is related to the binder content and the corresponding ratio of the synthetic binder monomer. The higher the binder content, the higher the peel strength. The higher the isocyanate content in the monomer, the stronger its electronegativity and the higher the bonding strength.
[0186] Test Example 2: Battery Performance Test
[0187] Battery charge and discharge settings: Examples 1-5 and 7-12 and Comparative Examples 1-2 and 5-7: 1. Rest step: 20 min, sampling interval 10 s, 2. Constant current charge 0.1C to 4.2V, rest 1 min, 3. Constant current discharge 0.1C to 2.7V, rest 1 min, repeat step 2, nominal specific capacity of the positive electrode 200 mAh / g;
[0188] Example 6 and Comparative Example 3: 1. Resting step: 20 min, sampling interval 10 s, 2. Constant current discharge 0.1C to 0.05V, rest 1 min, 3. Constant current charge 0.1C to 1.5V, rest 1 min, repeat step 2, nominal specific capacity of the negative electrode 3200 mAh / g;
[0189] Table 4
[0190] As can be seen from Table 4, the battery prepared using Example 1-2 exhibits good battery performance due to its relatively high peel strength and less adhesive addition.
[0191] By comparing the batteries prepared in Example 3 with those prepared in Comparative Example 6, it can be observed that the dry-process negative electrode battery prepared using the binder of the present application has better performance. The main reason is that PTFE has relatively poor reduction stability at low potentials, and PTFE is easily carbonized to form a loose structure with relatively poor peeling strength, forming a porous electrode sheet, which affects the performance of the battery.
[0192] The battery prepared using Example 4 has a strong adhesive property because the binder prepared in Example 3 has a high degree of cross-linking due to the large amount of third monomer. However, the binder has a mesh-like coating on the electrode, which hinders ion conduction and thus reduces battery performance.
[0193] The battery prepared in Example 5 has poor adhesion due to the small amount of second monomer and third monomer in the binder prepared in Example 4, which affects the capacity of the battery.
[0194] The batteries prepared in Examples 6-8 discussed the effect of binder content. A higher binder content would reduce ion conduction and affect battery performance. However, too little binder content would cause the electrode sheet to have low peeling strength and powder to fall off easily, affecting battery performance.
[0195] The binder used in Example 9 is applied in the absence of an inorganic solid electrolyte. The binder is applied in a liquid electrolyte lithium battery system and can still show a good discharge specific capacity.
[0196] The batteries prepared using Examples 10-12 all showed acceptable specific capacity due to the different binders.
[0197] The batteries prepared using Comparative Examples 1, 2, 3, 5 and 7 all have poor battery performance due to the poor mechanical properties of the electrode sheets: the poly(ethylene-vinyl acetate) formed in Comparative Example 1 has strong plasticity and poor adhesion; the polyamino-type binder formed in Comparative Example 2 has poor film formation under solvent-free conditions and low temperature conditions (the processing temperature needs to be greater than 180°C), and Comparative Example 5 has high plasticity due to its high polyethylene content, and also has poor adhesion. Comparative Examples 1, 2 and 3 will all cause the powder to fall off easily due to the adhesion problem of the binder, thereby reducing the battery capacity.
[0198] Comparative Example 7 uses a traditional adhesive to prepare the dry method of this application. It has poor bonding effect with the current collector and a relatively large interface resistance, resulting in poor battery performance. This shows that traditional dry electrode PTFE and adhesives that are not within the scope of protection of the claims of this application cannot achieve the bonding effect of this application or simplify the process flow.
[0199] The above description is merely a preferred embodiment of the present application and is not intended to limit the present application in any other manner. Any person skilled in the art may utilize the above disclosed technical content to modify or modify the present application into equivalent embodiments with equivalent variations. However, any simple modifications, equivalent variations, and modifications to the above embodiments that do not depart from the technical content of the present application and are based on the technical essence of the present application shall still fall within the scope of protection of the present application.
Claims
1. A binder for a dry electrode, wherein: The binder comprises units containing an alkylene group, units containing an acrylate group, and units containing an isocyanate group or a urethane group.
2. The adhesive according to claim 1, wherein Calculated by mass percentage in the binder, the units containing alkylene groups account for 5-60%, the units containing acrylate groups account for 10-65%, and the units containing isocyanate or urethane groups account for 5-40%.
3. The adhesive according to claim 1 or 2, wherein The binder is prepared by polymerizing a first monomer, a second monomer and a third monomer, wherein the first monomer contains an alkylene group, the second monomer contains an acrylate group and / or an acrylate group containing a hydroxyl group, and the third monomer contains an isocyanate group or a carbamate group.
4. The binder according to any one of claims 1 to 3, wherein The weight average molecular weight of the binder is 1000-200000Da.
5. The adhesive according to claim 2, wherein: Calculated by mass percentage in the binder, the unit containing isocyanate or urethane group accounts for 10-30%.
6. A composition for preparing an electrode plate, comprising the binder, active material, conductive agent and electrolyte according to any one of claims 1 to 5.
7. The composition according to claim 6, wherein In parts by weight, the binder is 0.1-10 parts, preferably 2-5 parts; The active material is 50-100 parts; the electrolyte is 0-50 parts; and the conductive agent is 0-10 parts.
8. An electrode plate, comprising coating the composition according to claim 6 or 7 on a current collector.
9. A method for preparing an electrode sheet, wherein: The method comprises: Mixing an active material, an electrolyte, a conductive agent, and a binder according to any one of claims 1 to 5 to obtain a mixture; The mixture is coated on the surface of the current collector.
10. The method according to claim 9, wherein: In parts by weight, the active material is 50-100 parts, the electrolyte is 0-50 parts, the conductive agent is 0-10 parts, and the binder is 0.1-10 parts.
11. The method according to claim 9 or 10, wherein: The coating thickness is 1-1000 μm.
12. The method according to any one of claims 9 to 11, wherein: The mixture is coated on the surface of the current collector by one or more methods selected from hot roller pressing, hot flat pressing and hot isostatic pressing. Preferably, the temperature is 25-80°C.
13. A battery comprising the electrode sheet according to claim 8 or the electrode sheet prepared by the method according to any one of claims 9 to 12.
14. Use of the binder according to any one of claims 1 to 5 in the preparation of lithium ion batteries.
Citation Information
Patent Citations
Binder treatment method, binder, negative electrode material, negative electrode plate and solid-state battery
CN115799515A
Dry electrode binder and preparation method and application thereof
CN117003952A
Binder for positive electrode of dry electrode as well as preparation method and application of binder
CN117946319A
Binder composition for lithium secondary battery electrode, electrode for lithium secondary battery, and lithium secondary battery and manufacturing method thereof
JP2005044681A
Fabrication of lithium battery dry electrodes
US20220173369A1
Cited By
Lithium iron phosphate dry-method electrode plate and preparation method thereof
CN119864369A
Dry-method membrane preparation method, dry-method electrode pole piece, preparation method of dry-method electrode pole piece and battery
CN120149337A