Rubber mixture and tire
The sulfur-crosslinkable rubber mixture with biologically renewable terpene resin and rice husk ash silica addresses the balance of tire performance and sustainability by enhancing dynamic stiffness and elongation, leading to better handling and durability with reduced abrasion.
Patent Information
- Application Number
- PCT/EP2024/056555
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-12
- Publication Date
- 2024-10-03
AI Technical Summary
Current tire rubber compounds face challenges in balancing wet grip, braking, handling, rolling resistance, winter properties, abrasion, and tear resistance, while also needing to transition to more sustainable and environmentally friendly materials to reduce fossil raw material dependence and greenhouse gas emissions.
A sulfur-crosslinkable rubber mixture for tire treads comprising diene rubber, 5-70 phr terpene resin based on over 95% biologically renewable raw materials, and 5-250 phr silica made from rice husk ash, which enhances dynamic stiffness, tensile strength, and elongation properties, improving handling and structural durability.
The combination of biologically renewable terpene resin and rice husk ash silica in the rubber mixture significantly increases dynamic storage modulus, tensile strength, and elongation, resulting in improved handling behavior, structural durability, and reduced abrasion, while promoting sustainability.
Smart Images

Figure IMGF000015_0001
Abstract
Description
[0001] Description
[0002] Rubber compound and tires
[0003] The invention relates to a sulfur-crosslinkable rubber mixture, in particular for the tread of pneumatic vehicle tires.
[0004] The invention further relates to a pneumatic vehicle tire having at least one component consisting of such a sulfur-vulcanized rubber mixture.
[0005] Since the driving characteristics of a tire, especially a pneumatic tire, depend to a large extent on the rubber composition of the tread, particularly stringent requirements are placed on the composition of the tread compound. Conflicting objectives exist between most of the well-known tire properties, such as wet grip, braking, handling, rolling resistance, winter performance, abrasion, and tear resistance. Numerous attempts have already been made to positively influence tire properties by varying the polymer components, fillers, and other additives in the tread compound.
[0006] In addition to the aforementioned objectives regarding compound and vulcanizate properties, today's efforts are aimed at using the most sustainable and environmentally friendly materials possible in rubber compounds for vehicle tires, reducing dependence on fossil raw materials, and minimizing greenhouse gas emissions. One approach to sustainable products internally involves recycling old, no longer needed products, such as old tires, with the recycled material being used in the production of new tires. Another way to improve product sustainability is to use substances from renewable raw materials as additives for rubber compounds.
[0007] Such additives made from renewable raw materials include vegetable oils, resins based on renewable raw materials, and rice husk silica. The latter is silica produced from bio-based sodium silicate from rice husk ash.
[0008] EP 3 802 152 B1 discloses rubber compounds for tire treads with a good property profile, which contain silica produced from rice husk ash and AMS resin (alpha-methyl-styrene resin).
[0009] The invention is based on the object of providing sustainable rubber compounds for the treads of pneumatic vehicle tires, which are characterized by improved dynamic stiffness and improved tensile-elongation behavior and thus by improved handling behavior and better structural durability in the tire.
[0010] This object is achieved according to the invention by a sulfur-crosslinkable rubber mixture, in particular for the tread of pneumatic vehicle tires, which contains at least the following components:
[0011] - at least one diene rubber,
[0012] - 5 to 70 phr (parts by weight, based on 100 parts by weight of the total rubber in the mixture) of at least one terpene resin based on more than 95% of bio-renewable raw materials and
[0013] - 5 to 250 phr silica made from rice husk ash.
[0014] Surprisingly, it has been found that the special combination of at least one terpene resin based on more than 95% biorenewable raw materials with silica produced from rice husk ash in the specified amounts in diene rubber compounds leads to an increased dynamic storage modulus and thus increased stiffness, while simultaneously improving tensile properties, such as tensile strength and elongation at break, and thus improved structural durability. When the rubber compound according to the invention is used in the treads of pneumatic vehicle tires, this leads to improved handling behavior and better structural durability. In addition to the improved sustainability due to the additives used, the rubber compound according to the invention is also characterized by improved abrasion behavior, i.e., reduced abrasion.
[0015] The term phr (parts per hundred parts of rubber by weight) used in this document is the standard quantity used in the rubber industry for compound formulations. The dosage of the parts by weight of the individual substances is always based on 100 parts by weight of the total mass of all solid rubbers present in the compound.
[0016] In the context of the present invention, the term “a terpene resin based on more than 95% biologically renewable raw materials” is to be understood as meaning a terpene resin which is materially produced from renewable raw materials as a source, with plant sources being particularly preferred.
[0017] For the purposes of the present invention, the term "silica produced from rice husk ash" refers to silica, also known as silicic acid, obtained from the inorganic combustion residues (ash) of rice husks / rice hulls. The term "silica produced from rice husk ash" is also known to those skilled in the art as "rice husk ash silica" (RHAS).
[0018] According to the invention, the rubber mixture contains at least one diene rubber. Diene rubbers are rubbers produced by polymerization or copolymerization of dienes and / or cycloalkenes and thus contain C=C double bonds either in the main chain or in the side groups.
[0019] The diene rubber(s) is / are preferably selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), epoxidized polyisoprene (ENR), butadiene rubber (BR), butadiene-isoprene rubber, styrene-butadiene rubber (SBR), in particular solution-polymerized styrene-butadiene rubber (SSBR) and emulsion-polymerized styrene-butadiene rubber (ESBR), styrene-isoprene rubber, liquid rubbers with a molecular weight Mw of greater than 20,000 g / mol, halobutyl rubber, polynorbornene, isoprene-isobutylene copolymer, ethylene-propylene-diene rubber, nitrile rubber, chloroprene rubber, Acrylate rubber, fluororubber, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrogenated acrylonitrile-butadiene rubber and hydrogenated styrene-butadiene rubber.
[0020] In particular, nitrile rubber, hydrogenated acrylonitrile-butadiene rubber, chloroprene rubber, butyl rubber, halobutyl rubber, or ethylene-propylene-diene rubber are used in the manufacture of technical rubber articles, such as belts, straps, and hoses, and / or shoe soles. The preferred blend compositions for these rubbers are those known to those skilled in the art—specific with regard to fillers, plasticizers, vulcanization systems, and additives.
[0021] According to a particularly preferred embodiment of the invention, the diene rubber(s) is / are selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution-polymerized styrene-butadiene rubber (SSBR), and emulsion-polymerized styrene-butadiene rubber (ESBR). Such a rubber mixture is particularly suitable for the tread of vehicle tires. Natural polyisoprene is understood to be rubber that can be obtained by harvesting sources such as rubber trees (Hevea brasiliensis) or non-rubber tree sources (such as guayule or dandelion (e.g. Taraxacum koksaghyz)). Natural polyisoprene (NR) is understood to mean non-synthetic polyisoprene.
[0022] The rubber mixture according to the invention contains 5 to 70 phr, preferably 20 to 60 phr, particularly preferably 30 to 50 phr, of at least one terpene resin based on more than 95% biorenewable raw materials. Several different terpene resins can also be used in the mixture. Preferably, the terpene resin is based 100% on biorenewable raw materials. Terpene resins based on more than 95% biorenewable raw materials can be obtained, for example, from raw materials obtained from the production of fragrances from orange peels. However, the terpene resin is preferably based on by-products obtained from the pulp production of softwoods. Such by-products are commercially available in large quantities and can be refined on an industrial scale into terpene resins.
[0023] According to a preferred embodiment of the invention, the terpene resin is not based on limonene.
[0024] The terpene resin is preferably based on α- and β-pinene. Such terpene resins can be produced from byproducts resulting from the pulp production of softwoods.
[0025] The terpene resin, which is based on more than 95% biorenewable raw materials, preferably has an average molecular weight (Mw) according to GPC of 800 to 1500 g / mol. Such terpene resins are easy to process and exhibit good tensile properties.
[0026] According to a preferred embodiment of the invention, the terpene resin has a softening point of 100 to 140 °C, preferably 110 to 130 °C.
[0027] For good braking performance of the tire whose tread consists of the rubber mixture according to the invention, the terpene resin has a glass transition temperature Tg according to DSC of 50 to 100 °C, preferably 50 to 80 °C.
[0028] Terpene resins that can be used according to the invention include, for example, those of the type Sylvatraxx® 8115 and Sylvatraxx® 8125 from Kraton Chemicals SAS. These are based 100% on biorenewable raw materials and not on limonene. The rubber mixture according to the invention contains 5 to 250 phr, preferably 20 to
[0029] 200 phr, particularly preferably 40 to 170 phr, silica produced from rice husk ash.
[0030] Preferably, the silica made from rice husk ash contained in the rubber mixture has a nitrogen surface area (BET surface area) (according to DIN ISO 9277 and DIN 66132) of 35 to 400 m 2 / g, preferably from 75 to 320 m 2 / g and particularly preferably from 120 to 235 m 2 / g, and a CTAB surface area (according to ASTM D 3765) of 30 to 400 m 2 / g, preferably from 70 to 300 m 2 / g and particularly preferably from 110 to 230 m 2 / g, on.
[0031] A suitable silica made from rice husk ash with a BET surface area of 155 m 2 / g and a CTAB surface area of 156 to 157 m 2 / g is available, for example, under the trade name "Precipitated Silica K160" from FengHai (PanJin) Rice Biotechnology Co., Ltd.
[0032] In addition to the silica produced from rice husk ash, the rubber mixture may contain other silicas known to those skilled in the art for use in rubber mixtures.
[0033] To improve processability and to bond the silica to the diene rubber in silicic acid-containing mixtures, at least one silane coupling agent is preferably used in the rubber mixture in amounts of 1-15 parts by weight (parts by weight, based on 100 parts by weight of silica / silica). The silane coupling agents can also be used in mixtures.
[0034] The term phf (parts per hundred parts of filler by weight) used in this document is the quantity commonly used in the rubber industry for coupling agents for polar fillers. In the context of the present application, phf refers to the silica present, meaning that other fillers that may be present, such as carbon black, are not included in the calculation of the amount of silane coupling agent. The silane coupling agents react with the surface silanol groups of the silica or other polar groups during mixing of the rubber or rubber mixture (in situ) or even before the filler is added to the rubber in the sense of pretreatment (premodification). Silane coupling agents that can be used are all silane coupling agents known to the person skilled in the art for use in rubber mixtures.Such coupling agents known from the prior art are bifunctional organosilanes which have at least one alkoxy, cycloalkoxy or phenoxy group as a leaving group on the silicon atom and which have as another functionality a group which, optionally after cleavage, can enter into a chemical reaction with the double bonds of the polymer. The latter group can, for example, be the following chemical groups: -SCN, -SH, -NH2 or -Sx- (where x = 2-8). Thus, silane coupling agents which can be used include, for example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane or 3,3'-bis(triethoxysilylpropyl)polysulfides having 2 to 8 sulfur atoms, such as e.g. B. 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfide or mixtures of the sulfides with 1 to 8 sulfur atoms with different contents of the various sulfides can be used.TESPT can also be added, for example, as a mixture with carbon black (trade name X50S from Degussa). Blocked mercaptosilanes, such as those known from WO 99 / 09036, can also be used as silane coupling agents. Silanes such as those described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1, and WO 2008 / 083244 A1 can also be used. Examples of suitable silanes include those marketed under the name NXT® in various versions by Momentive, USA, or those marketed under the name VP Si 363 by Evonik Industries. So-called “silated core polysulfides” (SCP, polysulfides with a silylated core) can also be used, which are described, for example, in US 20080161477 A1 and EP 2 114 961 B1.
[0035] Preferably, at least one silane coupling agent in the rubber mixture is 3,3'-bis(triethoxysilylpropyl) disulfide (TESPD). The rubber mixture may contain other fillers, such as carbon blacks, aluminosilicates, chalk, starch, magnesium oxide, titanium dioxide, rubber gels, carbon nanotubes, graphite, graphene, or so-called "carbon-silica dual-phase fillers," in conventional amounts, whereby the fillers can be used in combination.
[0036] If the rubber mixture contains carbon black, all types of carbon black known to those skilled in the art can be used. However, preference is given to using a carbon black that has an iodine adsorption number according to ASTM D 1510 of 30 to 180 g / kg, preferably 30 to 130 kg / g, and a DBP number according to ASTM D 2414 of 80 to 200 m 1 / 100 g, preferably 100 to 200 m 1 / 100 g, particularly preferably 100 to 180 ml / 100 g. This achieves particularly good rolling resistance indicators for use in vehicle tires, along with good other tire properties.
[0037] The rubber mixture according to the invention may further contain various plasticizers. These are preferably present in the mixture in amounts of 5 to 50 phr, particularly preferably 5 to 30 phr.
[0038] The rubber mixture may additionally contain at least one plasticizer, which is preferably selected from the group consisting of plasticizers from renewable raw materials such as rapeseed oil or sunflower oil, mineral oils, phosphoric acid esters such as tri-(2-ethylhexyl) phosphate, and liquid polymers having a weight average molecular weight distribution Mw according to GPC of 60,000 g / mol or less.
[0039] When using mineral oil, it is preferably selected from the group consisting of DAE (Distilled Aromatic Extracts), RAE (Residual Aromatic Extract), TDAE (Treated Distilled Aromatic Extracts), MES (Mild Extracted Solvents), white oils and naphthenic oils, with RAE being particularly preferred.
[0040] According to an advantageous development of the invention, a vegetable oil is used as the plasticizer. This is advantageous from an ecological and economic perspective and offers advantageous properties in tires. It is particularly preferred if the vegetable oil is rapeseed oil.
[0041] A liquid polymer, for example a liquid diene polymer such as liquid polybutadiene, can also be used as a plasticizer. The liquid polymer is preferably well compatible with the common rubber types of a tread compound and exhibits a low tendency to diffusion.
[0042] Furthermore, the rubber mixture can contain customary additives in customary parts by weight, which are preferably added in at least one basic mixing stage during its production. These additives include a) ageing inhibitors, such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ), b) activators, such as zinc oxide and fatty acids (e.g. stearic acid) or zinc complexes such as zinc ethylhexanoate, c) waxes, d) mastication aids, such as B. 2,2'-dibenzamidodiphenyl disulfide (DBD), and e) processing aids, such as fatty acid salts, such as zinc soaps, and fatty acid esters and their derivatives.
[0043] The proportion of the total amount of other additives is 3 to 150 phr, preferably 3 to 100 phr and particularly preferably 5 to 80 phr.
[0044] The vulcanization of the rubber compound is carried out in the presence of sulfur and / or sulfur donors using vulcanization accelerators, whereby some vulcanization accelerators can also act as sulfur donors. The accelerator is selected from the group consisting of thiazole accelerators and / or mercapto accelerators and / or sulfenamide accelerators and / or thiocarbamate accelerators and / or thiuram accelerators and / or thiophosphate accelerators and / or thiourea accelerators and / or xanthate accelerators and / or guanidine accelerators.
[0045] Preference is given to using a sulfenamide accelerator selected from the group consisting of N-cyclohexyl-2-benzothiazolesufenamide (CBS) and / or N,N-dicyclohexylbenzothiazole-2-sulfenamide (DCBS) and / or benzothiazyl-2-sulfenemorpholide (MBS) and / or N-tert-butyl-2-benzothiazylsulfenamide (TBBS).
[0046] The rubber compound may also contain vulcanization retarders.
[0047] Any sulfur-donating substance known to the person skilled in the art can be used as the sulfur-donating substance. If the rubber mixture contains a sulfur-donating substance, it is preferably selected from the group consisting of, for example, thiuram disulfides, such as tetrabenzylthiuram disulfide (TBzTD), tetramethylthiuram disulfide (TMTD) or tetraethylthiuram disulfide (TETD), thiuram tetrasulfides, such as, for example,
[0048] Dipentamethylenethiuram tetrasulfide (DPTT), dithiophosphates such as DipDis (bis-(diisopropyl)thiophosphoryl disulfide), bis(O,O-2-ethylhexylthiophosphoryl)polysulfide (e.g. Rhenocure SDT 50®, Rheinchemie GmbH), zinc dichloryldithiophosphate (e.g. Rhenocure ZDT / S®, Rheinchemie GmbH) or zinc alkyldithiophosphate, and 1,6-bis(N,N-dibenzylthiocarbamoyldithio)hexane and diarylpolysulfides and dialkylpolysulfides.
[0049] Other network-forming systems, such as those available under the trade names Vulkuren®, Duralink®, or Perkalink®, or network-forming systems as described in WO 2010 / 049216 A2, can also be used in the rubber compound. The latter system contains a vulcanizing agent that crosslinks with a functionality greater than four and at least one vulcanization accelerator.
[0050] During the final mixing stage, at least one vulcanizing agent selected from the group consisting of sulfur, sulfur donor, vulcanization accelerator, and vulcanizing agents that crosslink with a functionality greater than four is preferably added to the rubber mixture during its production. This allows the mixed final mixture to be vulcanized to produce a sulfur-crosslinked rubber mixture for use in rubber products, particularly pneumatic vehicle tires.
[0051] The terms “vulcanized” and “crosslinked” are used synonymously in the context of the present invention.
[0052] The rubber compound is produced according to the process commonly used in the rubber industry, in which a base compound containing all components except the vulcanization system (sulfur and vulcanization-influencing substances) is first prepared in one or more mixing stages. The finished compound is created by adding the vulcanization system in a final mixing stage. The finished compound is further processed, for example, by an extrusion process, and formed into the appropriate shape. Further processing then takes place by vulcanization, with sulfur crosslinking occurring due to the vulcanization system added within the scope of the present invention.
[0053] The rubber compound can be used for a wide variety of rubber products. It can be used in various components of pneumatic vehicle tires. It is preferably used for the production of pneumatic vehicle tires, such as car, van, truck, or two-wheeler tires, where the rubber compound forms at least the part of the tread that comes into contact with the road surface.
[0054] In a pneumatic vehicle tire, the tread can consist of a single compound designed according to the invention. However, pneumatic vehicle tires today often have a tread with a so-called cap / base construction. The term "cap" refers to the part of the tread that comes into contact with the road surface and is arranged radially on the outside (upper tread section or tread cap). The term "base" refers to the part of the tread that is arranged radially on the inside and thus does not come into contact with the road surface during driving or only at the end of the tire's life (lower tread section or tread base). In a pneumatic vehicle tire with such a cap / base construction, at least the rubber compound for the cap is designed according to claim 1.
[0055] The pneumatic vehicle tire according to the invention can also have a tread consisting of different tread compounds arranged side by side and / or one below the other (multi-component tread).
[0056] During the production of the pneumatic vehicle tire, the mixture is formed as a ready-mixed compound into the shape of a tread, preferably at least into the shape of a tread cap, prior to vulcanization and is applied during the production of the green vehicle tire as known in the art. The tread, preferably at least the tread cap, can also be wound onto a green tire in the form of a narrow strip of rubber compound.
[0057] The invention encompasses all advantageous embodiments, which are reflected, inter alia, in the patent claims. In particular, the invention also encompasses embodiments that result from the combination of different features, for example, components of the rubber mixture, with varying degrees of preference for these features, so that a combination of a first feature designated as "preferred" or described within the context of an advantageous embodiment with another feature designated, for example, as "particularly preferred" is also encompassed by the invention.
[0058] The invention will now be explained in more detail using comparative and exemplary embodiments, which are summarized in Table 1.
[0059] The comparison mixtures are marked with V, the mixture according to the invention is marked with E.
[0060] The compound was manufactured according to standard rubber industry procedures under standard conditions in three stages in a laboratory mixer. In the first mixing stage (basic mixing stage), all components except the vulcanization system (sulfur and vulcanization-influencing substances) were mixed. In the second mixing stage, the base mixture was thoroughly mixed again. The final mixture was created by adding the vulcanization system in the third stage (final mixing stage), which was mixed at 90 to 120 °C.
[0061] Furthermore, test specimens were produced from all mixtures by vulcanization under pressure at 160 °C for 20 minutes and material properties typical for the rubber industry were determined using these test specimens using the test methods specified below:
[0062] - Shore A hardness at room temperature according to ISO 868
[0063] - Rebound resilience at room temperature and 70 °C according to ISO 4662
[0064] - Stress value at 300% elongation (M300) at room temperature according to ISO 37
[0065] - Tensile strength at room temperature according to ISO 37
[0066] - Elongation at break at room temperature according to ISO 37
[0067] - Fracture energy density at room temperature determined in the tensile test, where the fracture energy density is the work required until fracture, related to the volume of the sample, according to ISO 37
[0068] - Average dynamic storage modulus (E'average) at 55 °C over the strain sweep from dynamic mechanical measurement at a frequency of 10 Hz according to ISO 4664-1
[0069] - Abrasion at room temperature according to DIN / ISO 4649
[0070] The dynamic storage modulus (E'average) correlates with stiffness and thus with handling behavior. A high dynamic storage modulus E'(average) indicates greater stiffness and thus better handling performance. Tensile properties, such as tensile strength and elongation at break, correlate with structural durability. Table 1 a Sprintan® SLR-3402, Trinseo, functionalized, solution-polymerized styrene-butadiene copolymer with functionalization for the polymer / silica and polymer / carbon black interaction, T g = -62 °C b LBR-302, Kuraray, liquid polybutadiene, T g = -85 °C
[0071] C ZEOSIL® 1165 MP, Solvay SA, BET surface area = 155 m 2 / g (measured with nitrogen), CTAB surface area = 156-157 m 2 / G; dPrecipitated Silica K160, FengHai (PanJin) Rice Biotechnology Co., Ltd, silica from rice husk ash, BET surface area = 155 m 2 / g (measured with nitrogen), CTAB surface area = 156-157 m 2 / G e Sylvatraxx® 4401 , Kraton Chemicals SAS, Alpha-Methyl-Styrene resin, softening point = 85 °C (according to ASTM E 28), T g = 45 °C f Sylvatraxx® 8115, Kraton Chemicals SAS, non-limonene-based terpene resin, softening point = 115 °C (according to ASTM E 28), T g = 66 °C
[0072] 9 3, 3'-Bis(triethoxysilylpropyl) disulfide (TESPD)
[0073] The data in Table 1 shows that the combined presence of the terpene resin, which is based on more than 95% biorenewable raw materials, with silica produced from rice husk ash in Compound 4(E) improves, i.e. increases, the tensile properties (stress value, tensile strength, elongation at break, and fracture energy density). Surprisingly, this improves, i.e., increases, the tensile properties (stress value, tensile strength, elongation at break, and fracture energy density). This effect far exceeds the additive effect of the individual measures (sole replacement of the silica with RHAS 3(V) and sole replacement of the alpha-methyl-styrene resin with terpene resin 2(V)). Compound 4(E) therefore exhibits high structural durability. The dynamic storage modulus E' (medium) is also significantly improved, i.e., increased, in Compound 4(E), which leads to better handling behavior in the treads of pneumatic vehicle tires.
[0074] The abrasion of the mixture according to the invention is also low, so that the mixture has a good property profile of durability, handling and abrasion with high sustainability.
Claims
Patent claims 1. Sulphur-crosslinkable rubber mixture, in particular for the tread of pneumatic vehicle tires, containing at least the following components: - at least one diene rubber, - 5 to 70 phr (parts by weight, based on 100 parts by weight of the total rubber in the mixture) of at least one terpene resin based on more than 95% of bio-renewable raw materials and - 5 to 250 phr silica made from rice husk ash.
2. Sulphur-crosslinkable rubber mixture according to claim 1, characterized in that it contains 20 to 60 phr, preferably 30 to 50 phr, of at least one terpene resin based to more than 95% on biologically renewable raw materials.
3. Sulphur-crosslinkable rubber mixture according to claim 1 or 2, characterized in that the terpene resin is based 100% on biologically renewable raw materials.
4. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the terpene resin is not based on limonene.
5. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the terpene resin is based on α- and β-pinene.
6. Sulfur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the terpene resin has an average molecular weight Mw according to GPC of 800 to 1500 g / mol.
7. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the terpene resin has a softening point of 100 to 140 °C, preferably 110 to 130 °C.
8. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that the terpene resin has a glass transition temperature Tg according to DSC of 50 to 100 °C, preferably 50 to 80 °C.
9. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that it contains 20 to 200 phr, preferably 40 to 170 phr, of silica produced from rice husk ash.
10. Sulphur-crosslinkable rubber mixture according to at least one of the preceding claims, characterized in that it contains 1 - 15 phf (parts by weight, based on 100 parts by weight of silica) of at least one silane coupling agent.
11. Pneumatic vehicle tire with at least one component consisting of a sulfur-vulcanized rubber mixture according to one of claims 1 to 10.
12. Pneumatic vehicle tire according to claim 11 having a tread whose part at least coming into contact with the road surface consists of a sulfur-vulcanized rubber mixture according to one of claims 1 to 10.
Citation Information
Patent Citations
Silated core polysulfides, their preparation and use in filled elastomer compositions
EP2114961B1
Tyres for vehicles and elastomeric compositions for tyres comprising particular silicas from rice husk ash
EP3802152B1
Silated core polysulfides, their preparation and use in filled elastomer compositions
US20080161477A1
Blocked mercaptosilane coupling agents for filled rubbers
WO1999009036A1
Tire compositions and components containing free-flowing filler compositions
WO2008083241A2